Gating transistor material, phase change memory chip, memory device and electronic device
By doping Ge-S materials with Te or Sn elements, a specific type of gate material is prepared, which solves the problems of leakage current and toxic elements in existing phase change memories and achieves low leakage current and appropriate threshold voltage. and high thermal stability phase change memory chips.
Patent Information
- Application Number
- PCT/CN2024/088633
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-31
AI Technical Summary
In existing phase change memories, GeAsSiSe or GeAsSiTe materials contain toxic As element, which poses safety risks, and there is leakage current during read, erase, and write operations, which affects the stability and life of the phase change memory cells.
By doping Ge-S based materials with Te element or Sn element, a (GexS1-x)1-yMy or [(GexS1-x)1-yMy]1-zNz type gate material is prepared to maintain the bidirectional threshold. switching characteristics, reducing leakage current and threshold voltage, while improving thermal stability to ensure the safety and performance of the material.
A gate material with low leakage current, appropriate threshold voltage, strong thermal stability and long cycle life has been realized, which avoids the safety hazards of toxic elements and improves the reliability and storage density of phase change memory chips.
Smart Images

Figure CN2024088633_31102024_PF_FP_ABST
Abstract
Description
Gate tube materials, phase change memory chips, storage devices and electronic devices
[0001] This application claims priority to Chinese patent application No. 202310491385.5 filed on April 28, 2023, entitled “Gate tube material and method for obtaining same, phase change memory chip, storage device and electronic device”, the entire contents of which are incorporated herein by reference. Technical Field
[0002] The present disclosure relates to the field of semiconductor storage technology, and in particular to gate tube materials, phase change memory chips, storage devices, and electronic devices. Background Art
[0003] Phase Change Memory (PCM) has great potential in terms of high storage density and fast operation speed. PCM consists of multiple phase change memory cells. Phase change memory cells have leakage current during read, erase, and write operations. To prevent the leakage current from adversely affecting adjacent phase change memory cells, a gate transistor unit that acts as a switch is configured for each phase change memory cell.
[0004] The gate tube unit includes a gate layer made of a gate tube material. For example, the related art provides some gate tube materials, including GeAsSiSe material, GeAsSiTe material, and the like.
[0005] However, the GeAsSiSe material or the GeAsSiTe material includes the toxic As element, which poses a safety hazard.
[0006] Public content
[0007] In view of this, the present disclosure provides a gate tube material, a phase change memory chip, a storage device and an electronic device, which can solve the above technical problems.
[0008] Specifically, the following technical solutions are included:
[0009] On the one hand, a gate tube material is provided, the chemical formula of the gate tube material is (Ge x S 1-x ) 1-y M y , M element is selected from Te element or Sn element; wherein, 0.2≤x≤0.7, 0<y≤0.4, and x and y are both atomic percentages.
[0010] The gate material provided in the embodiments of the present disclosure achieves at least low leakage current, suitable threshold voltage, and strong thermal stability by doping a Ge-S-based material with a first doping element M and limiting the type and atomic percentage of the first doping element M. This ensures that the gate material maintains bidirectional threshold switching (OTS) characteristics. The synergistic combination of these elements ensures that the gate material exhibits at least the following advantages: low leakage current, suitable threshold voltage, and strong thermal stability. Furthermore, the first doping element M is non-toxic, environmentally friendly, and poses no safety risks.
[0011] In some possible implementations, the M element is Te; the value ranges of x and y are as follows: 0.312≤x≤0.649, 0<y≤0.377.
[0012] Under this condition, the gate tube material can not only maintain low leakage current and appropriate threshold voltage, but also further enhance its thermal stability.
[0013] In some possible implementations, the M element is Sn; the value ranges of x and y are as follows: 0.312≤x≤0.649, 0<y≤0.08.
[0014] Under this condition, the gate tube material can not only maintain low leakage current and appropriate threshold voltage, but also further enhance its thermal stability.
[0015] On the other hand, another gate material is provided, wherein the chemical formula of the gate material is [(Ge x S 1-x ) 1-y M y ] 1-z N z ;
[0016] The M element and the N element are different, and the M element and the N element are respectively selected from one of the Te element, the Sn element, the C element, and the Si element; wherein 0.2≤x≤0.7, 0<y≤0.4, 0≤z≤0.4, and x, y, and z are all atomic percentages.
[0017] The gate material provided by the embodiments of the present disclosure is achieved by doping a Ge-S material with a first doping element M and a second doping element N. The types and atomic percentages of the first doping element M and the second doping element N are limited, so that the gate material maintains bidirectional threshold switching characteristics (i.e., OTS characteristics). The synergistic combination of these elements results in the gate material having at least the advantages of low leakage current, appropriate threshold voltage, and strong thermal stability. Furthermore, both the first doping element M and the second doping element N are non-toxic, environmentally friendly, and pose no safety risks.
[0018] In some possible implementations, the M element is Te; the value ranges of x, y, and z are as follows: 0.312≤x≤0.649, 0<y≤0.377, 0.02≤z≤0.2.
[0019] Under this condition, the gate tube material can not only maintain low leakage current and appropriate threshold voltage, but also further enhance its thermal stability.
[0020] Furthermore, the N element is a C element or a Si element; the value range of z is 0.1≤z≤0.2, which can further improve the thermal stability of the gate tube material.
[0021] Furthermore, the N element is Sn element; the value range of z is 0.02≤z≤0.08, which can further improve the thermal stability of the gate tube material.
[0022] In some possible implementations, the M element is Sn; the value ranges of x, y, and z are as follows: 0.312≤x≤0.649, 0<y≤0.08, 0.02≤z≤0.2.
[0023] Under this condition, the gate tube material can not only maintain low leakage current and appropriate threshold voltage, but also further enhance its thermal stability.
[0024] Furthermore, the N element is a C element or a Si element; the value range of z is 0.1≤z≤0.2, which can further improve the thermal stability of the gate tube material.
[0025] Furthermore, the N element is Te element; the value range of z is 0.02≤z≤0.2, which can further improve the thermal stability of the gate tube material.
[0026] In some possible implementations, the gate tube material is obtained by the following method:
[0027] Analyze whether the band gap values of multiple Ge-SM ternary structure models or Ge-SMN quaternary structure models meet the band gap threshold conditions;
[0028] The gate tube material is obtained according to the percentage of elements corresponding to the Ge-SM ternary structure model or the Ge-SMN quaternary structure model that meets the energy band gap threshold condition.
[0029] In some possible implementations, the gate tube material is also obtained by the following method:
[0030] Analyzing whether the mean square displacement value of the Ge-SM ternary structure model or the Ge-SMN quaternary structure model that meets the energy band gap threshold condition meets the mean square displacement threshold condition;
[0031] The gate tube material is obtained according to the percentage of elements corresponding to the Ge-SM ternary structure model or the Ge-SMN quaternary structure model that meets the mean square displacement threshold condition.
[0032] On the other hand, a phase change memory chip is provided, wherein the phase change memory chip includes a plurality of memory sub-units, each of the memory sub-units includes a gate tube unit and a phase change memory unit connected in series;
[0033] Each of the gate tube units includes a gate layer, and the gate layer is made of any of the above-mentioned gate tube materials.
[0034] Phase-change memory chips, also known as phase-change memories, are configured with a gate transistor unit for each phase-change memory cell. Using the gate transistor unit as a switching device for the phase-change memory cell effectively suppresses leakage current generated during the operation of the phase-change memory chip. The phase-change memory chip provided by the disclosed embodiments utilizes the aforementioned gate transistor materials, resulting in advantages such as low threshold voltage, low leakage current, strong thermal stability, and long cycle life.
[0035] In some possible implementations, the gate tube unit and the phase change memory unit are integrated.
[0036] In some possible implementations, the gate tube unit and the phase change memory unit are independent of each other.
[0037] On the other hand, a storage device is provided, which includes a controller and at least one phase-change memory chip, the phase-change memory chip being as described above, and the controller being configured to store data in the phase-change memory chip.
[0038] The storage device (also referred to as a memory) may be configured to store various types of data, which may be contact data, phone book data, messages, pictures, videos, etc., or may be instructional data.
[0039] On the other hand, an electronic device is provided, which includes a processor and the above-mentioned storage device, and the processor is used to store data generated by the electronic device in the storage device.
[0040] The electronic devices include but are not limited to: computers, mobile phones, music playing devices, digital broadcasting devices, messaging devices, game control devices, medical devices, fitness equipment, personal digital assistants, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] FIG1 is a schematic structural diagram of a memory sub-unit in which a gating layer and a phase-change memory unit with a confined structure are integrated, provided by an embodiment of the present disclosure;
[0042] FIG2 is a schematic structural diagram of an exemplary gate tube unit provided in an embodiment of the present disclosure;
[0043] FIG3 is a schematic diagram of the structure of an exemplary storage device provided by an embodiment of the present disclosure;
[0044] FIG4 is a flowchart of obtaining an exemplary gate tube material according to an embodiment of the present disclosure;
[0045] FIG5 is a flowchart of obtaining another exemplary gate tube material according to an embodiment of the present disclosure;
[0046] FIG6 is a graph showing a band gap test of GeS5 according to an embodiment of the present disclosure;
[0047] FIG7 is a graph showing a band gap test of GeS2 according to an embodiment of the present disclosure;
[0048] FIG8 is a diagram of Ge provided in an embodiment of the present disclosure. 38 S 62 Band gap test diagram;
[0049] FIG9 is a graph showing a band gap test of GeS according to an embodiment of the present disclosure;
[0050] FIG10 is a graph showing a band gap test of Ge2S according to an embodiment of the present disclosure;
[0051] FIG11 is a diagram showing a fitting curve of the energy band gap in a Ge-S binary compound as a function of Ge content provided by an embodiment of the present disclosure;
[0052] FIG12 is a graph showing the band gap of a Ge-S-Te ternary compound with a Te doping percentage of 14% provided by an embodiment of the present disclosure;
[0053] FIG13 is a graph showing the band gap of a Ge-S-Te ternary compound with a Te doping percentage of 30% provided by an embodiment of the present disclosure;
[0054] FIG14 is a graph showing the energy band gap of a Ge-S-Te ternary compound with a Te doping percentage of 40% provided by an embodiment of the present disclosure;
[0055] FIG15 is a diagram showing a fitting curve of the energy band gap in the Ge-S-Te ternary compound according to an embodiment of the present disclosure as a function of Te content;
[0056] FIG16 is a partial wave density of states test diagram of Ge2S provided by an embodiment of the present disclosure;
[0057] FIG17 is a partial wave state density test diagram of a Ge-S-Te ternary compound with a Te doping percentage of 14% provided by an embodiment of the present disclosure;
[0058] FIG18 is a partial wave state density test diagram of a Ge-S-Te ternary compound with a Te doping percentage of 30% provided by an embodiment of the present disclosure;
[0059] FIG19 is a partial wave state density test diagram of a Ge-S-Te ternary compound with a Te doping percentage of 40% provided by an embodiment of the present disclosure;
[0060] FIG20 is a graph showing mean square displacement of elements in a Ge2S binary compound at 600K provided by an embodiment of the present disclosure;
[0061] FIG21 is a graph showing the mean square displacement of each element in a Ge-S-Te ternary compound with a Te doping percentage of 14% at 600K provided by an embodiment of the present disclosure;
[0062] FIG22 is a graph showing the mean square displacement of each element in a Ge-S-Te ternary compound with a Te doping percentage of 30% at 600K provided by an embodiment of the present disclosure;
[0063] FIG23 is a graph showing the mean square displacement of each element in a Ge-S-Te ternary compound with a Te doping percentage of 40% at 600K provided by an embodiment of the present disclosure;
[0064] FIG24 is a graph showing the energy band gap of a Ge-S-Sn ternary compound with a Sn doping percentage of 5% provided by an embodiment of the present disclosure;
[0065] FIG25 is a graph showing the energy band gap of a Ge-S-Sn ternary compound with an 8% Sn doping percentage provided by an embodiment of the present disclosure;
[0066] FIG26 is a graph showing the energy band gap of a Ge-S-Sn ternary compound with a Sn doping percentage of 10% provided by an embodiment of the present disclosure;
[0067] FIG27 is a graph showing mean square displacement of each element in a Ge-S-Sn ternary compound with a Sn doping percentage of 5% at 600K provided by an embodiment of the present disclosure;
[0068] FIG28 is a graph showing mean square displacement of each element in a Ge-S-Sn ternary compound with an 8% Sn doping percentage at 600K provided by an embodiment of the present disclosure;
[0069] FIG29 is a graph showing mean square displacement of each element in a Ge-S-Sn ternary compound with an 8% Sn doping percentage at 600K provided by an embodiment of the present disclosure;
[0070] FIG30 is a graph showing the energy band gap of a Ge-S-Te-Si quaternary compound with a Si doping percentage of 10% provided by an embodiment of the present disclosure;
[0071] FIG31 is a graph showing the mean square displacement of each element in a Ge-S-Te-Si quaternary compound with a Si doping percentage of 10% at 600K provided by an embodiment of the present disclosure;
[0072] FIG32 is a graph showing the energy band gap of a Ge-S-Sn-Si quaternary compound with a Si doping percentage of 10% provided by an embodiment of the present disclosure;
[0073] FIG33 is a graph showing the mean square displacement of each element in the Ge-S-Sn-Si quaternary compound with a Si doping percentage of 10% at 600K provided in an embodiment of the present disclosure.
[0074] In the above-mentioned band gap test diagrams, the horizontal axis Energy (ev) represents the band gap, with the unit being ev; the vertical axis IPR is the Inverse Participation Ratio, which represents the degree of localization of each electronic state in the system.
[0075] In the above mean square displacement test diagrams, the horizontal axis Time is time, the unit is picoseconds; the vertical axis MSD is the mean square displacement value, which represents the square value of the atomic diffusion movement displacement after time t compared with the initial time τ.
[0076] In the above partial wave state density test diagrams, the horizontal axis Energy (ev) represents the band gap, the unit is ev, and the vertical axis PDOS is the number of electronic states occupied by a certain element in each unit.
[0077] The reference numerals represent:
[0078] 1. gating layer; 2. phase change layer; 3. first top electrode; 4. first bottom electrode; 5. middle electrode;
[0079] 6. First insulating medium; 7. First substrate;
[0080] 8. Second top electrode;
[0081] 9. Second bottom electrode; 10. Second insulating medium; 11. Second substrate. DETAILED DESCRIPTION
[0082] To make the technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be described in further detail below with reference to the accompanying drawings.
[0083] Phase Change Memory (PCM) is a solid-state semiconductor non-volatile memory, also known as a phase change memory chip. It uses phase change material as the storage medium. Phase change material can undergo reversible transformation between crystalline and amorphous states. By utilizing the difference in high resistivity and low resistivity of the phase change material in the amorphous and crystalline states, phase change memory can store data "0" and "1".
[0084] The phase change memory includes multiple phase change memory cells, which include read, erase, and write operations. There is leakage current in the phase change memory cell during the read, erase, and write operations. In order to prevent the leakage current from affecting adjacent phase change memory cells and causing problems such as misreading and misoperation, a selection tube unit that acts as a switch is configured for each phase change memory cell.
[0085] Ovonic Threshold Switching (OTS) type gate transistor unit has the advantages of high on-state current and low leakage current and is widely used in phase change memory.
[0086] The operating principle of the OTS-type gate transistor unit is as follows: When the applied voltage or current is less than the threshold voltage or threshold current, the gate transistor unit maintains high resistance and is in the off state, which can effectively suppress leakage current. When the applied voltage or current is greater than the threshold voltage or threshold current, the gate transistor unit quickly changes to low resistance and is in the on state, thus enabling the corresponding phase-change memory unit in series to perform read, write, and erase operations.
[0087] As can be seen, when performing read, write, and erase operations on a phase-change memory cell, the gate transistor unit needs to be turned on and off. Therefore, the number of cycles of the gate transistor unit needs to be at least three orders of magnitude higher than that of the phase-change memory unit. The cycle life of the gate transistor unit directly affects the cycle life of the phase-change memory. The cycle life referred to here refers to the number of cycles that each component can perform before failure, when repeatedly setting the phase-change memory to 0 or 1.
[0088] The gate tube unit includes a gate layer made of a gate tube material. For example, related art provides some gate tube materials, including GeAsSiSe material, GeAsSiTe material, etc. However, GeAsSiSe material or GeAsSiTe material contains As element, which is toxic and poses a safety hazard.
[0089] On the one hand, the embodiment of the present disclosure provides a gate tube material, which is a ternary compound, and the chemical formula of the gate tube material is (Ge x S 1-x ) 1-yM y , M element is selected from Te element or Sn element; wherein, 0.2≤x≤0.7, 0<y≤0.4, and x and y are both atomic percentages.
[0090] The gate material provided in the embodiments of the present disclosure achieves this by doping a Ge-S material with a first doping element M, with the type and atomic percentage of the first doping element M being specified. This ensures that the gate material maintains bidirectional threshold switching (OTS) characteristics. The synergistic effect of these elements also provides the gate material with at least the following advantages: low leakage current, appropriate threshold voltage, strong thermal stability, long cycle life, and high fatigue resistance. Furthermore, the first doping element M is non-toxic, environmentally friendly, and poses no safety risks.
[0091] In some examples, the M element is Te, and the ranges of x and y are as follows: 0.312≤x≤0.649, 0<y≤0.377. That is, the chemical formula of the gate tube material is (Ge x S 1-x ) 1-y Te y , where 0.312≤x≤0.649, 0<y≤0.377.
[0092] When the M element is Te, by further narrowing the value range of x and y, on the one hand, it is beneficial to keep the threshold voltage of the gate tube material at a low level to prevent the threshold voltage from being too large, which would make the phase change memory difficult to operate. On the other hand, it is more beneficial to reduce the leakage current of the gate tube material and improve its thermal stability.
[0093] For the chemical formula (Ge x S 1-x ) 1-y Te y For the gate tube material, the value of x includes but is not limited to: 0.38, 0.43, 0.47, 0.5, 0.53, 0.55, etc. The value of y includes but is not limited to: 0.10, 0.13, 0.16, 0.19, 0.22, etc.
[0094] When Ge, S, and Te are combined in the atomic percentages shown above, the resulting gate material exhibits enhanced thermal stability, enabling gate devices fabricated from these materials to withstand higher operating currents and temperatures, significantly improving their reliability. For example, when gate devices fabricated from these materials through back-end processing can withstand ambient temperatures of 400°C for at least 15 minutes without experiencing issues such as element drift and segregation caused by high temperatures.
[0095] In other examples, the M element is Sn, and the value ranges of x and y are as follows: 0.312≤x≤0.649, 0<y≤0.08. That is, the chemical formula of the gate tube material is (Ge x S 1-x ) 1-y Sn y , where 0.312≤x≤0.649, 0<y≤0.08.
[0096] When the M element is Sn, by further narrowing the value range of x and y, on the one hand, it is beneficial to keep the threshold voltage of the gate tube material at a low level, preventing the threshold voltage from being too large and causing the phase change memory to be difficult to operate. On the other hand, it is more beneficial to reduce the leakage current of the gate tube material and improve its thermal stability.
[0097] For the chemical formula (Ge x S 1-x ) 1-y Sn y For the gate tube material, the value of x includes but is not limited to: 0.38, 0.43, 0.47, 0.5, 0.53, 0.55, etc.; the value of y includes but is not limited to: 0.03, 0.04, 0.05, 0.06, 0.07, etc.
[0098] When Ge, S, and Sn are combined in the atomic percentages shown above, the resulting gate material exhibits enhanced thermal stability, enabling gate devices fabricated from these materials to withstand higher operating currents and temperatures, significantly improving their reliability. For example, when gate devices fabricated from these materials through back-end processing can withstand ambient temperatures of 400°C for at least 15 minutes without experiencing issues such as element drift and segregation caused by high temperatures.
[0099] On the other hand, the embodiment of the present disclosure provides another gate tube material, which is a quaternary compound, and the chemical formula of the gate tube material is [(Ge x S 1-x ) 1-y M y ] 1-z N z ; The M element and the N element are different, and the M element and the N element are respectively selected from one of the Te element, the Sn element, the C element, and the Si element; wherein, 0.2≤x≤0.7, 0<y≤0.4, 0≤z≤0.4, and x, y, and z are all atomic percentages.
[0100] The gate tube material in the form of the quaternary compound provided in the embodiment of the present disclosure is obtained by further doping the gate tube material in the form of the ternary compound with the element N.
[0101] By simultaneously doping the Ge-S material with a first doping element, M, and a second doping element, N, and by limiting the types and atomic percentages of the first doping element, M, and N, the gate material maintains bidirectional threshold switching characteristics (OTS). The synergistic effect of these elements also imparts at least the following advantages: low leakage current, appropriate threshold voltage, strong thermal stability, long cycle life, and high fatigue resistance. Furthermore, the first doping element, M, and the second doping element, N, are non-toxic, environmentally friendly, and pose no safety risks.
[0102] In some examples, the M element is Te; the value ranges of x, y, and z are as follows: 0.312≤x≤0.649, 0<y≤0.377, 0.02≤z≤0.2.
[0103] That is, the chemical formula of the gate tube material is [(Ge x S 1-x ) 1-y Te y ] 1-z N z , N element is one of Sn element, C element, and Si element, wherein 0.312≤x≤0.649, 0<y≤0.377, and 0.02≤z≤0.2.
[0104] When the M element is Te, by further narrowing the value range of x, y and z, on the one hand, it is beneficial to keep the threshold voltage of the gate tube material at a low level to prevent the threshold voltage from being too large, which makes the phase change memory difficult to operate. On the other hand, it is more beneficial to reduce the leakage current of the gate tube material and improve its thermal stability.
[0105] Based on the above example, one type of gate tube material is that the M element is Te, the N element is C or Si, and the value range of z is 0.1≤z≤0.2. In other words, the chemical formula of the gate tube material is [(Ge x S 1-x ) 1-y Te y ] 1-z C z Or [(Ge x S 1-x ) 1-y Te y ] 1-z Si zWherein, 0.312≤x≤0.649, 0<y≤0.377, 0.1≤z≤0.2. Furthermore, when the N element is Si, the value range of z is 0.1≤z≤0.184, which can further improve the thermal stability of the gate tube material.
[0106] For the chemical formula [(Ge x S 1-x ) 1-y Te y ] 1-z C z Or [(Ge x S 1-x ) 1-y Te y ] 1-z Si z For the gate tube material, the value of x includes but is not limited to: 0.38, 0.43, 0.47, 0.5, 0.53, 0.55, etc.; the value of y includes but is not limited to: 0.10, 0.13, 0.16, 0.19, 0.22, etc.; the value of z includes but is not limited to: 0.1, 0.12, 0.14, 0.16, etc.
[0107] When Ge, S, Te, and Si (or C) are combined in the atomic percentages shown above, the resulting gate material exhibits enhanced thermal stability, enabling gate devices fabricated from these materials to withstand higher operating currents and temperatures, significantly improving their reliability. For example, when gate devices fabricated from these materials through back-end processing can withstand ambient temperatures of 400°C for at least 15 minutes without experiencing issues such as element drift and segregation caused by high temperatures.
[0108] Based on the above example, another type of gate tube material is that the M element is Te and the N element is Sn; the value range of z is 0.02≤z≤0.08. In other words, the chemical formula of the gate tube material is [(Ge x S 1-x ) 1-y Te y ] 1-z Sn z ; Among them, 0.312≤x≤0.649, 0<y≤0.377, 0.02≤z≤0.08.
[0109] For the chemical formula [(Ge x S 1-x ) 1-y Te y ] 1-z Sn zFor the gate tube material, the value of x includes but is not limited to: 0.38, 0.43, 0.47, 0.5, 0.53, 0.55, etc.; the value of y includes but is not limited to: 0.10, 0.13, 0.16, 0.19, 0.22, etc.; the value of z includes but is not limited to: 0.04, 0.05, 0.06, 0.07, 0.08, etc.
[0110] When Ge, S, Te, and Sn are combined in the atomic percentages shown above, the resulting gate material exhibits enhanced thermal stability, enabling gate devices fabricated from these materials to withstand higher operating currents and temperatures, significantly improving their reliability. For example, when gate devices fabricated from these materials through back-end processing can withstand ambient temperatures of 400°C for at least 15 minutes without experiencing issues such as element drift and segregation caused by high temperatures.
[0111] In some examples, the M element is Sn; the value ranges of x, y, and z are as follows: 0.312≤x≤0.649, 0<y≤0.08, 0.02≤z≤0.2. In other words, the chemical formula of the gate tube material is [(Ge x S 1-x ) 1-y Sn y ] 1-z N z , N element is one of Te element, C element, and Si element, wherein 0.312≤x≤0.649, 0<y≤0.08, and 0.02≤z≤0.2.
[0112] When the M element is Sn, by further narrowing the value range of x, y and z, on the one hand, it is beneficial to keep the threshold voltage of the gate tube material at a low level to prevent the threshold voltage from being too large, which makes the phase change memory difficult to operate. On the other hand, it is more beneficial to reduce the leakage current of the gate tube material and improve its thermal stability.
[0113] Based on the above example, one type of gate tube material is that the M element is Sn, the N element is C or Si, and the value range of z is 0.1≤z≤0.2. In other words, the chemical formula of the gate tube material is [(Ge x S 1-x ) 1-y Sn y ] 1-z C z Or [(Ge x S 1-x ) 1-y Sn y ] 1-z Siz Wherein, 0.312≤x≤0.649, 0<y≤0.08, 0.1≤z≤0.2. Furthermore, when the N element is Si, the value range of z is 0.1≤z≤0.184, which can further improve the thermal stability of the gate tube material.
[0114] For the chemical formula [(Ge x S 1-x ) 1-y Sn y ] 1-z C z Or [(Ge x S 1-x ) 1-y Sn y ] 1-z Si z For the gate tube material, the value of x includes but is not limited to: 0.38, 0.43, 0.47, 0.5, 0.53, 0.55, etc.; the value of y includes but is not limited to: 0.03, 0.04, 0.05, 0.06, 0.07, etc.; the value of z includes but is not limited to: 0.10, 0.12, 0.14, 0.16, etc.
[0115] When Ge, S, Sn, and Si (or C) are combined in the atomic percentages shown above, the resulting gate material exhibits enhanced thermal stability, enabling gate devices fabricated from these materials to withstand higher operating currents and temperatures, significantly improving their reliability. For example, when gate devices fabricated from these materials through back-end processing can withstand ambient temperatures of 400°C for at least 15 minutes without experiencing issues such as element drift and segregation caused by high temperatures.
[0116] Based on the above example, another type of gate tube material is that the M element is Sn element, the N element is Te element, and the value range of z is 0.02≤z≤0.2. That is, the chemical formula of the gate tube material is [(Ge x S 1-x ) 1-y Sn y ] 1-z Te z ; Among them, 0.312≤x≤0.649, 0<y≤0.08, 0.02≤z≤0.2.
[0117] For the chemical formula [(Ge x S 1-x ) 1-y Sn y ] 1-z Te zFor the gate tube material, the value of x includes but is not limited to: 0.38, 0.43, 0.47, 0.5, 0.53, 0.55, etc.; the value of y includes but is not limited to: 0.03, 0.04, 0.05, 0.06, 0.07, etc.; the value of z includes but is not limited to: 0.05, 0.06, 0.08, 0.10, 0.12, 0.14, 0.16, etc.
[0118] When Ge, S, Sn, and Te are combined in the atomic percentages shown above, the resulting gate material exhibits enhanced thermal stability, enabling gate devices fabricated from these materials to withstand higher operating currents and temperatures, significantly improving their reliability. For example, when gate devices fabricated from these materials through back-end processing can withstand ambient temperatures of 400°C for at least 15 minutes without experiencing issues such as element drift and segregation caused by high temperatures.
[0119] For the various types of gate tube materials provided in the embodiments of the present disclosure, their existence forms include but are not limited to the following: alloy form, compound form such as ternary compound or quaternary compound, mixture form of a mixture of a single substance and a single substance, mixture form of a mixture of a single substance and a compound, or a combination of the above forms.
[0120] For example, the gate material in the form of a ternary compound can be Ge - The mixture of S binary compound or alloy and M single substance is in the form of a mixture. In this case, the atomic percentage of each element is determined according to the chemical formula of the gate tube material. - The S binary compound is mixed evenly with the doping element, and then the gate layer is prepared. The gate tube material in the form of a quaternary compound can be Ge - The mixture of SM ternary compound or alloy and N single substance is in the form of a mixture. In this case, the atomic percentage of each element is determined according to the chemical formula of the gate tube material, and a certain ratio of Ge - The SM ternary compound and the doping element are mixed uniformly, and then the gating layer is prepared.
[0121] In summary, the gate tube material provided by the embodiment of the present disclosure has the advantages of low leakage current, appropriate threshold voltage, and strong thermal stability. The gate tube material is suitable for compatibility with complementary metal oxide semiconductor (CMOS) back-end processes.
[0122] The gate tube material provided in the embodiment of the present disclosure can be used to prepare an OTS type gate tube unit, which has all the advantages of the gate tube material, making it not only compatible with CMOS back-end processes, but also capable of matching storage class memory (SCM).
[0123] In some possible implementations, the various types of gate tube materials mentioned above are obtained by the following methods:
[0124] Analyze whether the band gap values of multiple Ge-SM ternary structure models or Ge-SMN quaternary structure models meet the band gap threshold conditions. Obtain the gate tube material based on the element percentages corresponding to the Ge-SM ternary structure models or Ge-SMN quaternary structure models that meet the band gap threshold conditions.
[0125] Based on the relationship between the band gap of a gate material and its gating performance, the disclosed embodiments screen the band gaps of simulated Ge-SM ternary and Ge-SMN quaternary structural models, thereby obtaining Ge-SM ternary and Ge-SMN quaternary structural models that meet the band gap threshold conditions. Furthermore, gate materials in the form of ternary and quaternary compounds are obtained that meet the required leakage current, threshold voltage, and thermal stability. This method for obtaining gate materials has at least the advantages of simple operation, accurate and reliable screening results, time and labor savings, and low cost, and is of great significance for the efficient development of simple and environmentally friendly gate materials.
[0126] After determining the Ge-SM ternary structure model and the Ge-SMN quaternary structure model that meet the band gap threshold conditions based on the band gap of the gate tube material, the following method can be used to further screen out gate tube materials with stronger thermal stability from these Ge-SM ternary structure models and Ge-SMN quaternary structure models.
[0127] In other words, the method for obtaining the various types of gate tube materials described above further includes analyzing whether the mean square displacement value of a Ge-SM ternary structure model or a Ge-SMN quaternary structure model that satisfies the band gap threshold condition satisfies the mean square displacement threshold condition. The gate tube material is obtained based on the percentage content of the elements corresponding to the Ge-SM ternary structure model or the Ge-SMN quaternary structure model that satisfies the mean square displacement threshold condition.
[0128] By further analyzing the mean square displacement values of the Ge-SM ternary structure model or the Ge-SMN quaternary structure model, the thermal stability of the ternary Ge-SM gate tube material and the quaternary Ge-SMN gate tube material can be further accurately predicted, thereby further improving the thermal stability of the final obtained ternary Ge-SM gate tube material and the quaternary Ge-SMN gate tube material.
[0129] The methods for obtaining the above-mentioned various types of gate tube materials will be further described in the following sections.
[0130] In another aspect, embodiments of the present disclosure further provide a phase-change memory chip comprising a plurality of memory subunits, each of which comprises a gate transistor unit and a phase-change memory unit connected in series. Each gate transistor unit comprises a gate layer made of any of the aforementioned gate transistor materials.
[0131] Phase-change memory chips, also known as phase-change memories, are configured with a gate transistor unit for each phase-change memory cell. Using the gate transistor unit as a switching device for the phase-change memory cell effectively suppresses leakage current generated during the operation of the phase-change memory chip. The phase-change memory chip provided by the disclosed embodiments utilizes the aforementioned gate transistor materials, resulting in advantages such as low threshold voltage, low leakage current, strong thermal stability, and long cycle life.
[0132] Among them, the threshold voltage is appropriate, which means that the value of the threshold voltage makes the value of the leakage current within the expected range, the threshold voltage will not be too low so that the leakage current is too high, and the value of the threshold voltage will not be too high so that the leakage current is too low. In the embodiment of the present disclosure, it is expected that the threshold voltage is appropriate and the power consumption of the corresponding phase change memory chip is as low as possible.
[0133] In some examples, the structure of the phase change memory chip involved in the embodiments of the present disclosure can be a 1S1R (One Selector One Resistor) structure (one selection tube unit controls one phase change memory unit) or a 1SnR (One Selector n Resistor) structure (one selection tube unit controls multiple phase change memory units at the same time).
[0134] In some examples, the gate tube unit may further include a buffer layer, which is stacked on one surface or two opposite surfaces of the gate layer. The buffer layer can effectively prevent element migration or segregation of the gate tube material in the direction of the electric field, reduce the diffusion between the gate tube material and the electrode or the phase change layer, and further improve the thermal stability of the gate tube unit.
[0135] The thickness of the gating layer can be determined according to the size of the operating voltage or operating current corresponding to the gating tube unit. In some examples, the thickness of the gating layer can be 5nm~100nm, for example, 5nm~50nm, 5nm~40nm, 5nm~30nm, 10nm~25nm, etc., which includes but is not limited to: 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, 20nm, 21nm, 22nm, 23nm, 24nm, 25nm, etc.
[0136] For the phase-change memory chip provided by the embodiment of the present disclosure, in its memory subunit, on the one hand, the gate tube unit can be integrated with the phase-change memory unit, and on the other hand, the gate tube unit can also be arranged independently of the phase-change memory unit.
[0137] In the embodiments of the present disclosure, the structure of the phase change memory cell includes but is not limited to a confined structure, a T-shaped structure, a U-shaped trench structure, an L-shaped structure, and the like.
[0138] In some implementations, the gate tube unit is integrated with the phase change memory unit, that is, the gate layer of the gate tube unit and the phase change layer of the phase change memory unit are arranged in the same layer structure unit and share the top electrode and the bottom electrode.
[0139] FIG1 illustrates the structure of a memory sub-unit in which a gating layer and a confined-structure phase-change memory cell are integrated. The memory sub-unit includes a gating layer 1, a phase-change layer 2, a first top electrode 3, a first bottom electrode 4, an intermediate electrode 5, a first insulating dielectric 6, and a first substrate 7. The gating layer 1, the intermediate electrode 5, and the phase-change layer 2 are stacked in sequence and integrally connected between the first top electrode 3 and the first bottom electrode 4. The first bottom electrode 4 is located on the first substrate 7, and the first insulating dielectric 6 covers the sides of the gating layer 1, the intermediate electrode, the phase-change layer 2, the first top electrode 3, and the first bottom electrode 4.
[0140] The arrangement order of the gate layer 1, the intermediate electrode 5 and the phase change layer 2 includes but is not limited to the following:
[0141] As an example, along the top-down direction, the first top electrode 3, the phase change layer 2, the intermediate electrode 5, the gating layer 1, the first bottom electrode 4 and the first substrate 7 are stacked in sequence.
[0142] As another example, along the top-down direction, the first top electrode 3, the gating layer 1, the intermediate electrode 5, the phase change layer 2, the first bottom electrode 4 and the first substrate 7 are stacked in sequence.
[0143] In some examples, the thickness of the first top electrode 3 may be 50 nm to 100 nm, including but not limited to 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, etc.
[0144] In some examples, the thickness of the first bottom electrode 4 can be 100 nm to 150 nm, including but not limited to: 100 nm, 105 nm, 110 nm, 115 nm, 120 nm, 125 nm, 130 nm, 135 nm, 140 nm, 145 nm, 150 nm, etc.
[0145] In other implementations, the gate tube unit and the phase change memory unit are independent of each other, that is, the gate tube unit and the phase change memory unit are separate from each other, the gate tube unit itself has a top electrode and a bottom electrode, and the phase change memory unit itself has another top electrode and another bottom electrode. The electrodes of the gate tube unit and the electrodes of the phase change memory unit can be connected in series by means such as wires, such as copper interconnects.
[0146] Regarding the structure of the gate transistor unit independent of the phase-change memory unit, please refer to Figure 2. The gate transistor unit includes a gate layer 1, a second top electrode 8, a second bottom electrode 9, a second insulating medium 10, and a second substrate 11. The second top electrode 8, the gate layer 1, the second bottom electrode 9, and the second substrate 11 are stacked in sequence from top to bottom; the second insulating medium 10 is configured to provide insulation isolation for the gate transistor unit. For example, the second insulating medium 10 covers the sides of the gate layer 1, the second top electrode 8, and the second bottom electrode 9.
[0147] The gate tube unit may further include a buffer layer, which is used to isolate the gate layer 1 and the electrode, thereby effectively preventing element segregation and drift in the gate layer.
[0148] For the phase change memory unit independent of the gate tube unit, its structure includes but is not limited to: a confined structure, a T-shaped structure, a U-shaped groove structure, an L-shaped structure, etc.
[0149] The structure of an independent phase change memory unit can be seen above. For example, it may include a first top electrode 3, a phase change layer 2, a first bottom electrode 4 and a first substrate 7. The first top electrode 3, the phase change layer 2, the first bottom electrode 4 and the first substrate 7 are stacked in sequence from top to bottom.
[0150] The phase change layer of the phase change memory cell involved in the embodiments of the present disclosure may include alternatingly stacked phase change material layers and template layers. For example, the number of cycles of alternating stacking of the phase change material layers and the template layers is 2 to 100. In some examples, the phase change material layer is provided with two or more layers, so that the phase change film can undergo a layered phase change, thereby achieving multi-level storage capabilities, which helps to improve the data storage density of the phase change memory chip.
[0151] The phase change material used in the phase change material layer may be, for example, a Ge-Te binary compound, a Sb-Te binary compound (e.g., Sb2Te3), a Bi-Te binary compound, a Ge-Sb-Te ternary compound, a Ti-Sb-Te ternary compound, a Ga-Sb binary compound, or Sb. The template material used in the template layer may be, for example, TiTe2.
[0152] As for the first substrate and the second substrate mentioned above, both can be semiconductor substrates, for example, including but not limited to: silicon dioxide, silicon carbide, silicon wafer, sapphire, diamond, etc.
[0153] When used to prepare a phase change memory unit or a gate tube unit, an organic solvent such as ethanol and / or acetone can be used to clean the surface of the first substrate or the second substrate to remove impurities on the substrate surface. After cleaning, the first substrate or the second substrate can be placed in an oven at 50°C to 100°C for drying.
[0154] The electrodes mentioned above include a first top electrode, a first bottom electrode, a second top electrode, and a second bottom electrode, all of which are inert metals.
[0155] Exemplarily, the electrode materials used for the first top electrode and the first bottom electrode include but are not limited to the following: titanium tungsten (TiW), tungsten (W), aluminum (Al), titanium nitride (TiN), titanium (Ti), tantalum (Ta), silver (Ag), platinum (Pt), carbon (C), copper (Cu), ruthenium (Ru), gold (Au), cobalt (Co), chromium (Cr), nickel (Ni), iridium (Ir), palladium (Pd), rhodium (Rh), etc.
[0156] Exemplarily, the electrode materials used for the second top electrode and the second bottom electrode include but are not limited to at least one of the following: Pt (platinum), Ti (titanium), W (tungsten), Au (gold), Ru (ruthenium), Al (aluminum), TiW (titanium tungsten), TiN (titanium nitride), TaN (tantalum nitride), IrO2 (iridium dioxide), ITO (indium tin oxide), and IZO (indium zinc oxide).
[0157] In the embodiment of the present disclosure, the insulating materials used for the first insulating medium and the second insulating medium include but are not limited to silicon dioxide (SiO2), silicon nitride (Si3N4), etc.
[0158] In some examples, the phase-change memory chip provided by the embodiments of the present disclosure is a memory-level phase-change memory chip.
[0159] The phase change memory chip provided in the embodiments of the present disclosure can be used as a separate memory, or can be used together with a dynamic random access memory as a hybrid memory.
[0160] In another aspect, embodiments of the present disclosure further provide a method for fabricating a phase-change memory chip, wherein the phase-change memory chip is as described above. All layers in the phase-change memory chip, other than the substrate, such as the gate layer, buffer layer, phase-change layer, top electrode, and bottom electrode, can be formed using a thin film deposition process.
[0161] The thin film deposition processes mentioned above include but are not limited to the following: evaporation, sputtering, atomic layer deposition, chemical vapor deposition, pulsed laser deposition, molecular beam epitaxy, metal compound vapor deposition, etc.
[0162] For example, the gate layer can be prepared using gate tube materials by evaporation, sputtering, atomic layer deposition, chemical vapor deposition, pulsed laser deposition, molecular beam epitaxy, metal compound vapor deposition, etc.
[0163] The prepared gating layer can realize instantaneous conversion between high and low resistance states under the operation of an electrical signal, and can instantaneously return to a high resistance state when the electrical signal is removed.
[0164] The magnetron sputtering parameters corresponding to each layer are determined according to the specific layer. Taking the preparation of the gating layer as an example, some applicable magnetron sputtering parameters are as follows: the background vacuum degree is 10 -3 Pa~10 -5 Pa; sputtering gas pressure is 0.3 Pa to 0.8 Pa; substrate temperature is 50°C to 400°C; sputtering power is 5 W to 50 W; sputtering gas includes but is not limited to at least one of argon, krypton, xenon, neon, and nitrogen; for example, argon Ar is used as the sputtering gas. The magnetron sputtering method can be DC magnetron sputtering or radio frequency magnetron sputtering.
[0165] Taking the preparation of the gating layer as an example, the gating tube material used can be in the form of an alloy, a multi-component compound, a mixture of a single substance and a single substance, or a mixture of a single substance and a compound, or a combination of the above. When the gating layer is prepared using a magnetron sputtering process, an alloy target, a compound target, a single substance target, or any combination thereof can be used for co-sputtering to ensure that the gating layer has a desired chemical composition.
[0166] On the other hand, an embodiment of the present disclosure further provides a storage device, as shown in FIG3 , which includes a controller 100 and any one of the above-mentioned phase change memory chips 200, wherein the controller 100 is used to store data in the phase change memory chip 200, wherein the controller 100 reads and writes data stored in the storage device and interacts with an external interface.
[0167] The storage device (also referred to as a memory) may be configured to store various types of data, which may be contact data, phone book data, messages, pictures, videos, etc., or may be instructional data.
[0168] The storage devices involved in the embodiments of the present disclosure can be configured into various types, for example, including but not limited to: memory, hard disk, magnetic disk, optical disk, etc.
[0169] On the other hand, an embodiment of the present disclosure further provides an electronic device, which includes a processor and the above-mentioned storage device, and the processor is used to store data generated by the electronic device in the storage device.
[0170] In some examples, the electronic device includes, but is not limited to, computers, mobile phones, music playing devices, digital broadcasting devices, messaging devices, game control devices, medical devices, fitness equipment, personal digital assistants, and the like.
[0171] The embodiment of the present disclosure further provides an exemplary description of a method for obtaining a gate tube material. Referring to FIG4 , the method for obtaining a gate tube material includes the following steps:
[0172] Step S1: constructing a plurality of Ge-S binary structure models, wherein the atomic percentages of Ge elements in the plurality of Ge-S binary structure models are different from each other.
[0173] Step S2: Analyze the energy band gap values E1 of multiple Ge-S binary structure models to determine the atomic percentage range of the Ge element that meets the first threshold condition.
[0174] Step S3: construct multiple Ge-SM ternary structure models, wherein the atomic percentage of the Ge element in the multiple Ge-SM ternary structure models is the same and satisfies the first threshold condition, and the atomic percentage of the M element is different from each other, and the M element is selected from one of the Te element and the Sn element.
[0175] Step S4: Analyze the energy band gap values E2 of multiple Ge-SM ternary structure models to determine the atomic percentage range of the M element that meets the second threshold condition.
[0176] Step S5: Based on the atomic percentage range of the Ge element that meets the first threshold condition and the atomic percentage range of the M element that meets the second threshold condition, determine the preliminary screening chemical formula of the Ge-SM ternary compound, and obtain the gating tube material according to the preliminary screening chemical formula of the Ge-SM ternary compound and the preliminary screening chemical formula of the Ge-SMN quaternary compound.
[0177] Furthermore, referring to FIG5 , the embodiment of the present disclosure further provides another method for obtaining a gate tube material, the method for obtaining a gate tube material comprising:
[0178] Step S1: constructing a plurality of Ge-S binary structure models, wherein the atomic percentages of Ge elements in the plurality of Ge-S binary structure models are different from each other.
[0179] Step S2: Analyze the energy band gap values E1 of multiple Ge-S binary structure models to determine the atomic percentage range of the Ge element that meets the first threshold condition.
[0180] Step S3: construct multiple Ge-SM ternary structure models, wherein the atomic percentage of the Ge element in the multiple Ge-SM ternary structure models is the same and satisfies the first threshold condition, and the atomic percentage of the M element is different from each other, and the M element is selected from one of the Te element and the Sn element.
[0181] Step S4: Analyze the energy band gap values E2 of multiple Ge-SM ternary structure models to determine the atomic percentage range of the M element that meets the second threshold condition.
[0182] Step S5: Based on the atomic percentage range of the Ge element that meets the first threshold condition and the atomic percentage range of the M element that meets the second threshold condition, determine the preliminary screening chemical formula of the Ge-SM ternary compound, and obtain the gating tube material according to the preliminary screening chemical formula of the Ge-SM ternary compound and the preliminary screening chemical formula of the Ge-SMN quaternary compound.
[0183] Step S6: construct multiple Ge-SMN quaternary structure models, wherein the atomic percentage of the Ge element in the multiple Ge-SMN quaternary structure models is the same and satisfies the first threshold condition, the atomic percentage of the M element is the same and satisfies the second threshold condition, and the atomic percentage of the N element is different from each other, and the N element is selected from one of the Te element, Sn element, C element, and Si element.
[0184] Step S7: Analyze the energy band gap values E3 of the multiple Ge-SMN quaternary structure models to determine the atomic percentage range of the N element that meets the third threshold condition.
[0185] Step S8: Determine the preliminary screening chemical formula of the Ge-SMN quaternary compound based on the atomic percentage range of the Ge element that meets the first threshold condition, the atomic percentage range of the M element that meets the second threshold condition, and the atomic percentage range of the N element that meets the third threshold condition.
[0186] Step S9: Obtain the gate tube material according to the preliminary screening chemical formula of the Ge-SM ternary compound and the preliminary screening chemical formula of the Ge-SMN quaternary compound.
[0187] In step S1 , the multiple Ge-S binary structure models constructed are all amorphous structure models thereof, and the atomic percentage of the Ge element in the multiple Ge-S binary structure models constructed can be gradually increased from small to large.
[0188] The atomic percentage gradient D1 between the current Ge-S binary structure model and the previous Ge-S binary structure model, and the atomic percentage gradient between the current Ge-S binary structure model and the next Ge-S binary structure model are defined as D2. The D1 value and the D2 value can be the same or different. For example, the D1 value can be greater than the D2 value, or the D1 value can be less than the D2 value.
[0189] The number of the multiple Ge-S binary structure models constructed is at least two, for example, can be three, four, five, six, seven, eight or more.
[0190] The more Ge-S binary structure models constructed, the more reliable the calculation results will be, but the calculation workload will also increase accordingly.
[0191] In the multiple Ge-S binary structure models constructed, the lower limit of the atomic percentage of Ge can be 0.15-0.25, including but not limited to: 0.155, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, etc. The upper limit of the atomic percentage of Ge can be 0.65-0.75, including but not limited to: 0.655, 0.66, 0.67, 0.68, 0.69, 0.7, 0.71, 0.72, 0.73, 0.74, 0.75, etc.
[0192] For example, five Ge-S binary structure models can be constructed, with the atomic percentages of Ge elements being 0.167, 0.333, 0.38, 0.5, and 0.667, respectively.
[0193] For step S2, the band gap values E1 of multiple Ge-S binary structure models are analyzed to determine whether the band gap values E1 of these Ge-S binary structure models meet the first threshold condition respectively, and the Ge-S binary structure models that meet the first threshold condition are screened out and the atomic percentage range of the Ge element that meets the first threshold condition is determined based on the atomic percentage of the corresponding Ge element.
[0194] In some examples, band gap values E1 for multiple Ge-S binary structure models are obtained. Based on the atomic percentages of Ge and the band gap values E1 in the multiple Ge-S binary structure models, a linear fit is performed on the functional relationship between the atomic percentage of Ge and the band gap value E1 to obtain a fitted function that shows how the band gap value E1 varies with the atomic percentage of Ge. Based on a first threshold condition, the fitted function is used to determine a lower limit and an upper limit of the atomic percentage of Ge that meet the first threshold condition, thereby determining a satisfactory atomic percentage range of Ge.
[0195] For step S3, the method of constructing multiple Ge-SM ternary structure models can refer to the above method of constructing multiple Ge-S binary structure models, including the design method of the atomic percentage of the M element can refer to the above design method of the atomic percentage of the Ge element.
[0196] Unlike constructing a Ge-S binary structure model, in constructing a Ge-SM ternary structure model, it is first necessary to determine the atomic percentage of the Ge element, wherein the atomic percentage of the Ge element must at least meet the first threshold condition. Furthermore, the atomic percentage of the selected Ge element can be 40%-60%, which includes but is not limited to 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, etc.
[0197] For step S4, the band gap values E2 of multiple Ge-SM ternary structure models are analyzed, and it is determined whether the band gap values E2 of these Ge-SM ternary structure models meet the second threshold condition. The Ge-SM ternary structure models that meet the second threshold condition are screened out and the atomic percentage range of the M element that meets the second threshold condition is determined based on the atomic percentage of the corresponding M element.
[0198] In some examples, band gap values E2 for multiple Ge-SM ternary structure models are obtained. Based on the atomic percentages of the M element and the band gap values E2 in the multiple Ge-SM ternary structure models, a linear fit is performed on the functional relationship between the atomic percentage of the M element and the band gap value E2 to obtain a fitting function that shows how the band gap value E2 varies with the atomic percentage of the M element. Based on a second threshold condition, the fitting function is used to determine a lower limit and an upper limit of the atomic percentage of the M element that meet the second threshold condition, thereby determining a satisfactory atomic percentage range of the M element.
[0199] For step S6, the method of constructing multiple Ge-SMN quaternary structure models can refer to the above method of constructing multiple Ge-S binary structure models, including the design method of the atomic percentage of the N element can refer to the above design method of the atomic percentage of the Ge element.
[0200] Unlike constructing a Ge-S binary structure model, constructing a Ge-SMN quaternary structure model first requires determining the atomic percentage of the Ge element and the atomic percentage of the M element. The atomic percentage of the Ge element must at least meet a first threshold condition. Furthermore, the selected atomic percentage of the Ge element can be 40%-60%, including but not limited to 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, etc. The atomic percentage of the M element is close to the median of the atomic percentage range of the M element because the band gap value of the corresponding Ge-SMN ternary structure model is larger at this point.
[0201] For example, when the M element is Te, the atomic percentage range of the Te element is expected to be less than or equal to 0.377. Then, in the constructed Ge-SMN quaternary structure model, the atomic percentage of the selected Te element can be 0.1-0.2, which includes but is not limited to 0.1, 0.12, 0.13, 0.14, 0.15, 0.16, 0.18, etc.
[0202] When the M element is Sn, the atomic percentage range of the Sn element is expected to be less than or equal to 0.08. Then, in the constructed Ge-SMN quaternary structure model, the atomic percentage of the selected Sn element can be 0.03-0.06, which includes but is not limited to 0.03, 0.04, 0.05, 0.06, etc.
[0203] For step S7, the band gap values E3 of multiple Ge-SMN quaternary structure models are analyzed, and it is determined whether the band gap values E3 of these Ge-SMN quaternary structure models meet the third threshold condition. The Ge-SMN quaternary structure models that meet the third threshold condition are screened out and the atomic percentage range of the N element that meets the third threshold condition is determined based on the atomic percentage of the corresponding N element.
[0204] In some examples, band gap values E3 are obtained for multiple Ge-SMN quaternary structure models. Based on the atomic percentages of N and the band gap values E3 in the multiple Ge-SMN quaternary structure models, a linear fit is performed on the functional relationship between the atomic percentage of N and the band gap E3 to obtain a fitting function that shows how the band gap E3 varies with the atomic percentage of N. Based on a third threshold condition, the fitting function is used to determine a lower limit and an upper limit of the atomic percentage of N that meet the third threshold condition, thereby determining a satisfactory atomic percentage range of N.
[0205] The embodiment of the present disclosure sets the first threshold condition, the second threshold condition and the third threshold condition related to the gating performance according to the relationship between the energy band gap value of the gating tube material and its gating performance, and designs the gating tube material based on this.
[0206] By constructing a Ge-S binary structure model and analyzing whether its energy band gap value E1 satisfies the first threshold condition, those Ge-S binary structure models that satisfy the first threshold condition are screened out, and then according to the atomic percentage of each Ge element in these Ge-S binary structure models, the atomic percentage range of the Ge element that satisfies the first threshold condition is determined. Subsequently, by constructing a Ge-SM ternary structure model and analyzing whether its energy band gap value E2 satisfies the second threshold condition, those Ge-SM ternary structure models that satisfy the second threshold condition are screened out, and then according to the atomic percentage of each M element in these Ge-SM ternary structure models, the atomic percentage range of the M element that satisfies the second threshold condition is determined. Under the premise that the atomic percentage range x of the Ge element and the atomic percentage range y of the M element are determined respectively, the preliminary screening chemical formula of the Ge-SM ternary compound (Ge x S 1-x ) 1-y M y The gate tube material is also determined accordingly, thereby obtaining the gate tube material in the form of a ternary compound.
[0207] Furthermore, by constructing a Ge-SMN quaternary structure model and analyzing whether its band gap value E3 satisfies the third threshold condition, those Ge-SMN quaternary structure models that meet the third threshold condition are screened out, and then according to the atomic percentage of each N element in these Ge-SMN quaternary structure models, the atomic percentage range of the N element that meets the third threshold condition is determined. Under the premise that the atomic percentage range x of the Ge element, the atomic percentage range y of the M element, and the atomic percentage range z of the N element are determined, the initial screening chemical formula of the Ge-SMN quaternary compound (Ge x S 1-x ) 1-y-z M y N z The gate tube material is also determined accordingly, thereby obtaining the quaternary compound form.
[0208] As can be seen, the disclosed embodiments screen the band gaps of simulated Ge-SM ternary structure models and Ge-SMN quaternary structure models based on the relationship between the band gap of the gate tube material and its gating performance, thereby obtaining Ge-SM ternary structure models and Ge-SMN quaternary structure models that meet the threshold conditions, and further obtaining gate tube materials in the form of ternary compounds and quaternary compounds. The gate tube material acquisition method provided by the disclosed embodiments has at least the advantages of simple operation, accurate and reliable screening results, time and labor saving, and low cost, and is of great significance for the efficient development of simple and environmentally friendly gate tube materials.
[0209] In the embodiment of the present disclosure, the energy band gap values of multiple Ge-S binary structure models are defined as E1, wherein the first threshold condition includes enabling the energy band gap value E1 to satisfy, 1.4ev≤E1≤2.4ev; the energy band gap values of multiple Ge-SM ternary structure models are defined as E2, wherein the second threshold condition includes enabling the energy band gap value E2 to satisfy, 1.4ev≤E2≤2.4ev; the energy band gap values of multiple Ge-SMN quaternary structure models are defined as E3, wherein the third threshold condition includes enabling the energy band gap value E3 to satisfy, 1.4ev≤E3≤2.4ev.
[0210] The inventors have found that when the energy band gap value of the gate tube material is higher than 2.4eV, the threshold voltage of the gate tube material will be too large, making the phase change memory device difficult to operate; when the energy band gap value of the gate tube material is less than 1.4eV, the leakage current of the gate tube material will be too large.
[0211] Therefore, it is expected that the energy band gap value range of the gate tube material is 1.4ev≤E1≤2.4ev. It can be seen that by limiting the first threshold condition, the second threshold condition and the third threshold condition as above, it can be ensured that the gate tube material in the form of a ternary compound and the gate tube material in the form of a quaternary compound have the advantages of low leakage current, appropriate threshold voltage, strong thermal stability, etc.
[0212] In some examples, multiple Ge-S binary structure models, multiple Ge-SM ternary structure models, and multiple Ge-SMN quaternary structure models are constructed based on first-principles molecular dynamics.
[0213] First-principles molecular dynamics is an algorithm that directly solves the Schrödinger equation based on the principles of interaction between atomic nuclei and electrons and their basic laws of motion, using the principles of quantum mechanics. Based on specific requirements, after some approximate processing, it includes density functional theory (DFT), which can calculate and predict parameters such as the crystal structure, band structure, density of states, and optical properties of materials.
[0214] Based on first-principles molecular dynamics, the disclosed embodiments can construct multiple Ge-S binary structural models, multiple Ge-SM ternary structural models, and multiple Ge-SMN quaternary structural models to accurately simulate binary Ge-S gating tube materials, ternary Ge-SM gating tube materials, and quaternary Ge-SMN gating tube materials. Furthermore, based on first-principles molecular dynamics, parameters such as the band structure (including band gap) and density of states of these structural models can be calculated, thereby effectively predicting the gating performance of these structural models.
[0215] The Vienna Ab initio Simulation Package (VASP) is a computer program for atomic-scale materials simulations based on first principles that can perform electronic structure calculations and quantum mechanical molecular dynamics.
[0216] The disclosed embodiments can utilize VASP software to construct and analyze Ge-S binary structure models, Ge-SM ternary structure models, and Ge-SMN quaternary structure models to obtain the mutual relationships, electronic structures, energy band structures, thermal stability, etc. between atoms within the materials to which these structure models belong, and then screen out the desired Ge-S-based gate tube doping elements and the range of doping concentrations of these doping elements through calculation, thereby achieving accurate prediction of ternary Ge-SM gate tube materials and quaternary Ge-SMN gate tube materials. The predicted ternary Ge-SM gate tube materials and quaternary Ge-SMN gate tube materials have the advantages of being environmentally friendly (non-toxic), having low leakage current, having a suitable threshold voltage, and having good thermal stability, and meet the requirements of high-performance gate tubes.
[0217] In some examples, VASP software was used to construct amorphous Ge-S binary structure model, Ge-SM ternary structure model, and Ge-SMN quaternary structure model respectively through the melt quenching method.
[0218] In some implementations, with respect to step S9, obtaining the gate tube material according to the preliminary screening chemical formula of the Ge-SM ternary compound and the preliminary screening chemical formula of the Ge-SMN quaternary compound may further include:
[0219] Step S91 : testing the mean square displacement of multiple Ge-SM ternary structure models satisfying the primary screening chemical formula of the Ge-SM ternary compound at a set temperature to obtain multiple first mean square displacement values.
[0220] Step S92: Compare the multiple first mean square displacement values with the mean square displacement threshold condition to select multiple Ge-SM ternary structure models that meet the mean square displacement threshold condition. In other words, compare the first mean square displacement value corresponding to each element in the multiple Ge-SM ternary structure models with the mean square displacement threshold condition.
[0221] Step S93: Determine the second screening chemical formula of the Ge-SM ternary compound based on the multiple Ge-SM ternary structure models that meet the mean square displacement threshold condition.
[0222] Step S94 , testing the mean square displacement of multiple Ge-SMN quaternary structure models satisfying the primary screening chemical formula of the Ge-SMN quaternary compound at a set temperature to obtain multiple second mean square displacement values.
[0223] Step S95: Compare the multiple second mean square displacement values with the mean square displacement threshold condition to select multiple Ge-SMN quaternary structure models that meet the mean square displacement threshold condition. In other words, compare the second mean square displacement value corresponding to each element in the multiple Ge-SMN quaternary structures with the mean square displacement threshold condition.
[0224] Step S96: Determine the two-sieve chemical formula of the Ge-SMN quaternary compound based on the multiple Ge-SMN quaternary structure models that meet the mean square displacement threshold condition.
[0225] Step S97 : Obtain the gate tube material according to the two-sieve chemical formula of the Ge-SM ternary compound and the two-sieve chemical formula of the Ge-SMN quaternary compound.
[0226] Among them, steps S91 to S93 are performed in sequence, and steps S94 to S96 are performed in sequence. The execution order of steps S91 to S93 and the execution order of steps S94 to S96 are not prioritized, and the two can be executed in any order.
[0227] The mean square displacement of a particular atom at a set temperature characterizes the atom's mobility at the set temperature. A larger mean square displacement indicates a stronger atom's mobility. Conversely, a smaller mean square displacement indicates a weaker atom's mobility, i.e., a more stable atom. In this application, it is desirable that the mean square displacement of an atom at a set temperature be as small as possible.
[0228] After obtaining the preliminary screening chemical formula of the Ge-SM ternary compound and the preliminary screening chemical formula of the Ge-SMN quaternary compound based on the energy band gap, the mean square displacement of each atom at a set temperature in the structural model corresponding to these preliminary screening chemical formulas is further compared with the mean square displacement threshold condition to determine the motion state of each atom at a set temperature. Expectedly, the motion state of each atom is inactive and does not exhibit large-scale movement, which indicates that the corresponding Ge-SM ternary structural model or Ge-SMN quaternary structural model has stronger thermal stability. It can be seen that through the above-mentioned two screening steps, the thermal stability of the ternary Ge-SM gate tube material and the quaternary Ge-SMN gate tube material can be further accurately predicted, thereby ensuring that the final obtained ternary Ge-SM gate tube material and the quaternary Ge-SMN gate tube material have the advantages of being environmentally friendly, having low leakage current, having a suitable threshold voltage, and having good thermal stability.
[0229] The mean square displacement threshold condition is determined based on the actual requirements for the thermal stability of the gate tube material. For example, the mean square displacement curve of an undoped Ge-S binary compound under the same conditions can be used as a judgment benchmark, and the mean square displacement threshold condition is set so that the difference between the mean square displacement curve and the judgment benchmark is less than or equal to the set threshold.
[0230] The mean square displacement is measured at a set temperature, which is the temperature tolerable for the gate tube material. In some examples, the set temperature may be 550K-650K, including but not limited to 550K, 560K, 570K, 580K, 590K, 600K, 610K, 620K, 630K, 640K, and 650K.
[0231] According to the above-mentioned method for obtaining the gate tube material, the following is a more detailed description with some examples:
[0232] Step S11, based on first principle molecular dynamics, five Ge-S binary structure models are constructed using VASP software, wherein the atomic percentages of Ge element in these five Ge-S binary structure models are 16.7%, 33.3%, 38%, 50% and 66.7%, respectively, and the chemical formulas of the corresponding five Ge-S binary structure models are GeS5, GeS2, Ge 38 S 62 , GeS and Ge2S.
[0233] Step S21, using VASP software to calculate the band gap values E1 of the five Ge-S binary structure models, which are: 2.94 eV (see Figure 6), 2.33 eV (see Figure 7), 2.22 eV (see Figure 8), 2.172 eV (see Figure 9) and 1.32 eV (see Figure 10).
[0234] According to the atomic percentage of Ge element and the band gap value E1 in these five Ge-S binary structure models, a linear fit is performed on the functional relationship between the atomic percentage of Ge element and the band gap value E1 to obtain a fitting function of the band gap value E1 changing with the atomic percentage of Ge element (see Figure 11).
[0235] The first threshold condition is set to include satisfying the energy band gap value E1, 1.4ev≤E1≤2.4ev. The fitting function is used to determine the lower and upper atomic percentage limits of the Ge element that satisfy the first threshold condition, and then the atomic percentage range of the Ge element that meets the requirements is determined to be 31.2%-64.9%, that is, it is determined that in the Ge-S binary compound, the value range of x is 31.2%≤x≤64.9%.
[0236] It can be seen that for the Ge-S binary system, when the atomic percentage of the Ge element is controlled within 31.2%≤x≤64.9%, it is beneficial to obtain a gate tube material with low leakage current and low threshold voltage.
[0237] Step S31: Based on first-principles molecular dynamics, three Ge-SM ternary structure models are constructed using VASP software. The atomic percentages of the Ge element in these three Ge-SM ternary structure models are the same and meet the first threshold condition, and the atomic percentages of the M element are different from each other, and the M element is selected from Te or Sn.
[0238] As an example, the atomic percentage of Ge element in the three Ge-SM ternary structure models is set to 33.3%, and M element is Te element, that is, to construct three (GeS2) 1-y Te y Ternary structure model, these three (GeS2) 1-y Te y The atomic weight percentages (ie, y values) of the Te element in the ternary structure model are 14%, 30%, and 40%, respectively.
[0239] Step S41: Calculate these three (GeS2) using VASP software 1-y Te y The band gap values E2 of the ternary structure model are: 1.86eV (see Figure 12), 1.47eV (see Figure 13), and 1.18eV (see Figure 14), among which the band gap value of GeS2 without Te element is 2.33eV.
[0240] According to these three (GeS2) 1-y Te y The atomic percentage of Te element and the band gap value E2 in the ternary structure model, a linear fit is performed on the functional relationship between the atomic percentage of Te element and the band gap value E2, and a fitting function of the band gap value E2 changing with the atomic percentage of Te element is obtained (see Figure 15).
[0241] Step S51: The second threshold condition is set to include the energy band gap value E2 satisfying 1.4 eV ≤ E2 ≤ 2.4 eV. The fitting function is used to determine the lower and upper atomic percentage limits of the Te element that satisfy the second threshold condition, and then the atomic percentage range of the Te element that meets the requirements is determined to be 0% < y ≤ 37.7%. In this way, the primary screening chemical formula of the Ge-SM ternary compound is determined to be (GeS2) 1-y Te y , where 0.2≤x≤0.7, 0<y≤0.377.
[0242] This example tests the (GeS2) binary structure model and the three (GeS2) 1-y Te yFigures 16-19 show the partial wave density of states for each element in the ternary structure model. It can be seen that the incorporation of Te at different doping concentrations significantly contributes to the mid-gap states of the Ge-S-Te ternary system, which are related to the gating characteristics of the gate tube. This indicates that the incorporation of Te has a positive effect on the gating characteristics of the gate tube material system.
[0243] In order to further verify whether the atomic percentage range of Te element is 0%<y≤37.7%, and whether it meets the thermal stability requirements of the gate tube material, the (GeS2) binary structure model and the above three (GeS2) 1-y Te y The mean square displacement of the ternary structure model (the atomic weight percentage of Te element is 14%, 30% and 40% respectively) at 600K was tested.
[0244] The test results are shown in Figures 20 to 23. As shown in Figure 23, when the atomic weight percentage of Te element is 40%, the (GeS2) 1-y Te y The movement ability of each atom in the ternary structure model system is in a strong motion state, which is undesirable. As shown in Figures 21 and 22, when the atomic weight percentage of Te element is 14% and 30% respectively, the atomic weight percentage of Te element (GeS2) is 14% and 30% respectively. 1-y Te y The motion of each atom in the ternary structure model system remains in a weak motion state, without showing large-scale movement. It can be seen that the acquisition of 0%<y≤37.7% is accurate and reliable.
[0245] Based on the above (GeS2) 1-y Te y The analysis of the ternary structure model shows that for the band gap, as the doping concentration of Te element increases, (GeS2) 1-y Te y The band gap value E2 of the ternary structure model gradually decreases. Since the band gap of the undoped pure GeS2 binary structure model is relatively large, the threshold voltage V th It will be too high, and the operation will consume a lot of power. The doping of Te elements can reduce the band gap, thereby reducing the threshold voltage V th .
[0246] However, when the atomic percentage of Te element is 40%, it will lead to (GeS2) 1-y Te yThe band gap of the ternary structure model is too small (less than the lower limit of 1.4 eV), which will lead to a high leakage current, making the leakage serious. In addition, the atomic mobility in this system is strong, which is not conducive to the thermal stability of the gate tube device. Therefore, the atomic percentage of Te element of 40% will be excluded. Finally, the doping concentration of Te element is determined to be 0<y≤37.7% through band gap fitting. It can be determined that the second screening chemical formula of Ge-SM ternary compound is the same as its primary screening chemical formula, both of which are (GeS2) 1- y Te y , where 0.2≤x≤0.7, 0<y≤0.377.
[0247] As another example, the atomic percentage of Ge element in the three Ge-SM ternary structure models is set to 33.3%, and M element is Sn element, that is, to construct three (GeS2) 1-y Sn y Ternary structure model, these three (GeS2) 1-y Sn y The atomic weight percentages (ie, y values) of Sn elements in the ternary structure model are 5%, 8%, and 10%, respectively.
[0248] Step S41: Calculate these three (GeS2) using VASP software 1-y Sn y The band gap values E2 of the ternary structure model are: 2.09eV (see Figure 24), 2.02eV (see Figure 25), and 2.17eV (see Figure 26), among which the band gap value of GeS2 without Sn doping is 2.33eV.
[0249] According to these three (GeS2) 1-y Sn y The atomic percentage of Sn element and the energy band gap value E2 in the ternary structure model are linearly fitted to the functional relationship between the atomic percentage of Sn element and the energy band gap value E2, and a fitting function of the energy band gap value E2 changing with the atomic percentage of Sn element is obtained.
[0250] Step S51: Set the second threshold condition to include the band gap value E2 satisfying 1.4 eV ≤ E2 ≤ 2.4 eV. The fitting function is used to determine the lower and upper atomic percentage limits of the Sn element that meet the first threshold condition, and further determine that the atomic percentage range of the Sn element that meets the requirements is 0% < y ≤ 12.5%. In this way, the preliminary screening chemical formula of the Ge-SM ternary compound is determined to be (GeS2) 1-y Sn y , where 0.2≤x≤0.7, 0<y≤0.125.
[0251] Considering the Sn element doping, (GeS2) 1-y Sn y The difference between the band gap values of the ternary structure model and the Ge-S binary structure model is small. Further analysis of the three (GeS2) 1-y Sn y The mean square displacement of the ternary structural model (the atomic weight percentage of Sn element is 5%, 8% and 10% respectively) at 600K was tested.
[0252] The test results are shown in Figures 27 to 29. As shown in Figure 29, when the atomic weight percentage of Sn element is 10%, the Sn content (GeS2) is 10%. 1-y Sn y The movement ability of each atom in the ternary structure model system is in a strong motion state, and when the atomic weight percentage of Sn element is 5% and 8%, the atomic weight percentage of Sn element (GeS2) is 5%. 1-y Sn y The motion of each atom in the ternary structure model system remains in a weak motion state, without large-scale movement. Therefore, y needs to be further controlled within 8% to ensure the thermal stability of the gate device.
[0253] It can be seen that the atomic percentage range of Sn element that finally meets the requirements is further screened to 0%<y≤8%. In this way, the second screening chemical formula of Ge-SM ternary compound is determined to be (GeS2) 1-y Sn y , where 0.2≤x≤0.7, 0<y≤0.08.
[0254] Based on the above (GeS2) 1-y Sn y Analysis of the ternary structure model shows that Sn doping contributes little to the band gap, only slightly reducing it. However, when the Sn doping concentration exceeds 8%, the atomic mobility in this system is strong, which is detrimental to the thermal stability of the gate device. Therefore, the case where the atomic percentage of Sn exceeds 8% is excluded, and the final Sn doping concentration is determined to be 0 < y ≤ 8% through band gap fitting.
[0255] Furthermore, the gate tube material in the form of a quaternary compound is further constructed. Some specific examples include but are not limited to the following:
[0256] Step S61: Based on first-principles molecular dynamics, multiple Ge-SMN quaternary structure models are constructed using VASP software. The atomic percentage of the Ge element in the multiple Ge-SMN quaternary structure models is the same and satisfies the first threshold condition, and the atomic percentage of the M element is the same and satisfies the second threshold condition. The M element is selected from Te or Sn, and the N element is selected from Si or C.
[0257] As an example, six Ge-S-Te-Si quaternary structure models are constructed. In these six Ge-S-Te-Si quaternary structure models, the atomic percentage of Ge element is set to 50%, and the atomic percentage of Te element is set to 14%. That is to say, six [(Ge 0.5 S 0.5 ) 0.86 Te 0.14 ] 1-z Si z The quaternary structure model, these six [(Ge 0.5 S 0.5 ) 0.86 Te 0.14 ] 1-z Si z The atomic weight percentages (ie, z values) of the Si element in the quaternary structure model are 5%, 10%, 15%, 20%, 30% and 40%, respectively.
[0258] Step S71, use VASP software to calculate these six [(Ge 0.5 S 0.5 ) 0.86 Te 0.14 ] 1-z Si z The band gap values E3 for the quaternary structure model are: 1.39 eV (5% doping), 1.479 eV (10% doping, see Figure 30), 1.433 eV (15% doping), 0.51 eV (20% doping), 0.42 eV (30% doping), and 0.427 eV (40% doping). It can be seen that as the Si doping level increases, the band gap value E3 decreases, which in turn leads to an increase in leakage current.
[0259] According to these six (GeS) 1-0.14-z Te 0.14 Si z The atomic percentage of Si element and the energy band gap value E3 in the quaternary structure model are linearly fitted to the functional relationship between the atomic percentage of Si element and the energy band gap value E3 to obtain a fitting function of the energy band gap value E3 changing with the atomic percentage of Si element.
[0260] Step S81, set the third threshold condition to include the energy band gap value E3 meeting 1.4ev≤E2≤2.4ev, and determine the lower and upper atomic percentage limits of the Si element that meet the second threshold condition by the fitting function, and then determine that the atomic percentage range of the Si element that meets the requirements is 10%≤z≤19.1%. In this way, the primary screening chemical formula of the Ge-SMN quaternary compound is determined to be [(Ge x S 1-x ) 1-y Te y ] 1-z Si z , among which, 0.2≤x≤0.7, 0<y≤0.377, 0.1≤z≤0.191.
[0261] In order to further verify whether the atomic percentage range of Si element is 0.1≤z≤0.191, whether it meets the thermal stability requirements of the gate tube material, two of them [(Ge 0.5 S 0.5 ) 0.86 Te 0.14 ] 1-z Si z The mean square displacement of the quaternary structure model (the atomic weight percentage of Si element is 10% and 15% respectively) at 600K was tested. The test results show that when the atomic weight percentage of Si element is 10% and 15% respectively, the [(Ge 0.5 S 0.5 ) 0.86 Te 0.14 ] 1-z Si z The motion of each atom in the quaternary structure model system remains in a weak state, without large-scale movement. Therefore, the acquisition of 0.1≤z≤0.191 is accurate and reliable.
[0262] 31 shows examples of Si elements with an atomic weight percentage of 10% [(Ge 0.5 S 0.5 ) 0.86 Te 0.14 ] 0.9 Si 0.1 The schematic diagram of the mean square displacement of the four atoms in the quaternary structure model at 600K shows that the mobility of Si atoms is the lowest. Therefore, the doping of Si elements can effectively increase the stability of the gate tube material system. This is because Si atoms can form a tetrahedron structure in the gate tube material system. The tetrahedron plays a role in increasing the stability of the amorphous structure in the amorphous system. Therefore, the incorporation of Si improves the thermal stability of the gate tube material and reduces the device misreading caused by the gate tube drift.
[0263] As another example, four Ge-S-Sn-Si quaternary structure models are constructed. In these four Ge-S-Sn-Si quaternary structure models, the atomic percentage of the Ge element is set to 50%, and the atomic percentage of the Sn element is set to 5%. That is to say, four [(Ge 0.5 S 0.5 ) 0.95 Sn 0.05 ] 1-z Si z Quaternary structure model, these four [(Ge 0.5 S 0.5 ) 0.95 Sn 0.05 ] 1-z Si z The atomic weight percentages (ie, z values) of the Si element in the quaternary structure model are 5%, 10%, 15%, and 20%, respectively.
[0264] Step S71, use VASP software to calculate the four [(Ge 0.5 S 0.5 ) 0.95 Sn 0.05 ] 1-z Si z The band gap values E3 of the quaternary structure model are: 1.35eV (doping amount is 5%), 1.439eV (doping amount is 10%, see Figure 32), 1.412eV (doping amount is 15%), and 0.198eV (doping amount is 20%).
[0265] According to these four 0.5 S 0.5 ) 0.95 Sn 0.05 ] 1-z Si z The atomic percentage of Si element and the energy band gap value E3 in the quaternary structure model are linearly fitted to the functional relationship between the atomic percentage of Si element and the energy band gap value E3 to obtain a fitting function of the energy band gap value E3 changing with the atomic percentage of Si element.
[0266] Step S81, set the third threshold condition to include the energy band gap value E3 meeting 1.4ev≤E2≤2.4ev, and determine the lower and upper atomic percentage limits of the Si element that meet the second threshold condition by the fitting function, and then determine that the atomic percentage range of the Si element that meets the requirements is 10%≤z≤18.4%. In this way, the primary screening chemical formula of the Ge-SMN quaternary compound is determined to be [(Ge x S 1-x ) 1-y Sn y ]1-z Si z , where 0.2≤x≤0.7, 0<y≤0.377, 0.1≤z≤0.184.
[0267] In order to further verify whether the atomic percentage range of Si element is 0.1≤z≤0.184, whether it meets the thermal stability requirements of the gate tube material, two of them [(Ge 0.5 S 0.5 ) 0.95 Sn 0.05 ] 1-z Si z The mean square displacement of the quaternary structure model (the atomic weight percentage of Si element is 10% and 15% respectively) at 600K was tested. The test results show that when the atomic weight percentage of Si element is 10% and 15% respectively, the [(Ge 0.5 S 0.5 ) 0.95 Sn 0.05 ] 1-z Si z The motion of each atom in the quaternary structure model system remains in a weak state, without large-scale movement. Therefore, the acquisition of 0.1≤z≤0.184 is accurate and reliable.
[0268] 33 shows examples of Si elements with an atomic weight percentage of 10% [(Ge 0.5 S 0.5 ) 0.95 Sn 0.05 ] 0.9 Si 0.1 The schematic diagram of the mean square displacement of the four atoms in the quaternary structure model at 600K shows that the mobility of Si atoms is the lowest. Therefore, the doping of Si elements can effectively increase the stability of the gate tube material system. This is because Si atoms can form a tetrahedron structure in the gate tube material system. The tetrahedron plays a role in increasing the stability of the amorphous structure in the amorphous system. Therefore, the incorporation of Si improves the thermal stability of the gate tube material and reduces the device misreading caused by the gate tube drift.
[0269] In summary, x S 1-x ) 1-y Te y ] 1-z Si z The quaternary structure model and [(Ge x S 1-x ) 1-y Sn y ] 1-z Si zIn obtaining the atomic percentage of Si element in the quaternary structure model, the upper limit value of z can be 0.191 and 0.184, and the minimum value is selected as the upper limit value, that is, 0.1≤z≤0.184 is more beneficial to improving the performance of the gate tube.
[0270] The above description is only for the purpose of facilitating those skilled in the art to understand the technical solutions of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present disclosure shall be included in the scope of protection of the present disclosure.
Claims
1. A gate tube material, wherein: The chemical formula of the gate tube material is (Ge x S 1-x ) 1-y M y , the M element is selected from Te element or Sn element; Wherein, 0.2≤x≤0.7, 0<y≤0.4, and x and y are both atomic percentages.
2. The gate tube material according to claim 1, wherein: The M element is Te element; The value ranges of x and y are as follows: 0.312≤x≤0.649, 0<y≤0.
377.
3. The gate tube material according to claim 1, wherein: The M element is Sn element; The value ranges of x and y are as follows: 0.312≤x≤0.649, 0<y≤0.
08.
4. A gate tube material, wherein: The chemical formula of the gate tube material is [(Ge x S 1-x ) 1-y M y ] 1-z N z ; The M element and the N element are different, and the M element and the N element are respectively selected from one of the Te element, the Sn element, the C element, and the Si element; Among them, 0.2≤x≤0.7, 0<y≤0.4, 0≤z≤0.4, and x, y, and z are all atomic percentages.
5. The gate tube material according to claim 4, wherein: The M element is Te element; The value ranges of x, y and z are as follows: 0.312≤x≤0.649, 0<y≤0.377, 0.02≤z≤0.
2.
6. The gate tube material according to claim 5, wherein: The N element is a C element or a Si element; The value range of z is 0.1≤z≤0.
2.
7. The gate tube material according to claim 5, wherein: The N element is Sn element; The value range of z is 0.02≤z≤0.
08.
8. The gate tube material according to claim 4, wherein: The M element is Sn element; The value ranges of x, y and z are as follows: 0.312≤x≤0.649, 0<y≤0.08, 0.02≤z≤0.
2.
9. The gate tube material according to claim 8, wherein: The N element is a C element or a Si element; The value range of z is 0.1≤z≤0.
2.
10. The gate tube material according to claim 8, wherein: The N element is Te element; The value range of z is 0.02≤z≤0.
2.
11. The gate tube material according to any one of claims 1 to 10, wherein: The gate tube material is obtained by the following method: Analyze whether the band gap values of multiple Ge-SM ternary structure models or Ge-SMN quaternary structure models meet the band gap threshold conditions; The gate tube material is obtained according to the percentage of elements corresponding to the Ge-SM ternary structure model or the Ge-SMN quaternary structure model that meets the energy band gap threshold condition.
12. The gate tube material according to claim 11, wherein: The gate tube material is also obtained by the following method: Analyzing whether the mean square displacement value of the Ge-SM ternary structure model or the Ge-SMN quaternary structure model that meets the energy band gap threshold condition meets the mean square displacement threshold condition; The gate tube material is obtained according to the percentage of elements corresponding to the Ge-SM ternary structure model or the Ge-SMN quaternary structure model that meets the mean square displacement threshold condition.
13. A phase change memory chip, wherein: The phase-change memory chip comprises a plurality of memory sub-units, each of which comprises a gate tube unit and a phase-change memory unit connected in series; Each of the gate tube units comprises a gate layer, and the gate layer is prepared by using the gate tube material according to any one of claims 1-12.
14. The phase change memory chip according to claim 13, wherein: The gate tube unit is integrated with the phase change memory unit.
15. The phase change memory chip according to claim 13, wherein: The gate tube unit and the phase change memory unit are independent of each other.
16. A storage device, wherein: The storage device includes a controller and at least one phase-change memory chip, wherein the phase-change memory chip is as described in any one of claims 13 to 15, and the controller is used to store data in the phase-change memory chip.
17. An electronic device, wherein: The electronic device comprises a processor and the storage device according to claim 16, wherein the processor is used to store data generated by the electronic device in the storage device.
Citation Information
Patent Citations
High refractivity filber waveguides and its application
CN1539090A
Current Compliance Layers and Memory Arrays Comprising Thereof
US20180198064A1
Photo-conductive coating containing Ge, S, and Pb or Sn
US3966470A