Positive electrode active material, positive electrode, battery and electric device
By coating the surface of the ternary cathode material with a carbon-nitrogen coating layer and adjusting the single crystal particle size and nitrogen percentage, the problem of poor cycle performance of the ternary cathode material is solved, and the battery's excellent cycle performance and service life are improved.
Patent Information
- Application Number
- PCT/CN2024/088962
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-23
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
The cycle performance of ternary cathode materials is poor and cannot meet the requirements for improved battery cycle performance.
By coating the surface of the ternary cathode material with a carbon-nitrogen coating layer, the single crystal particle size and the mass percentage of nitrogen in the carbon-nitrogen coating layer are adjusted to meet a specific liquid retention relationship to improve the cycle performance of the cathode and battery. .
It significantly improves the cycle performance and service life of the cathode and battery, avoids the occurrence of side reactions, and enhances the liquid retention effect and long-term cycle stability.
Smart Images

Figure CN2024088962_31102024_PF_FP_ABST
Abstract
Description
Positive electrode active material, positive electrode, battery and electrical equipment
[0001] This disclosure claims priority to the Chinese patent application filed with the China Patent Office on April 23, 2023, with application number 202310466529.1 and application name “Positive Electrode Active Materials, Positive Electrodes, Batteries and Electrical Equipment,” the entire contents of which are incorporated by reference into this disclosure. Technical Field
[0002] The present disclosure relates to the field of battery technology, and in particular to positive electrode active materials, positive electrodes, batteries, and electrical equipment. Background Art
[0003] Ternary cathode materials are widely used in batteries due to their high energy density. However, battery performance requirements are becoming increasingly stringent, such as the need to improve battery cycle performance. However, the cycle performance of ternary cathode materials is relatively poor and cannot meet the requirements for improved battery cycle performance. Therefore, research and development of new ternary cathode materials is needed.
[0004] Summary of the Invention
[0005] In view of this, the present disclosure provides a positive electrode active material, a positive electrode, a battery and an electrical device. The particle size of the single crystal particles in the positive electrode active material, the mass percentage of the nitrogen element in the carbon-nitrogen coating layer and the liquid retention amount satisfy a certain relationship, which is beneficial to improving the cycle performance of the positive electrode and the battery, thereby increasing the service life of the battery.
[0006] In a first aspect, the present disclosure provides a positive electrode active material, comprising a ternary positive electrode material and a carbon-nitrogen coating layer covering the ternary positive electrode material, wherein the particle size of the single crystal particles of the ternary positive electrode material is X μm, the mass percentage of nitrogen in the carbon-nitrogen coating layer is Y, and the liquid retention capacity of the positive electrode active material is Q g / cm 3 , the X, the Y and the Q satisfy: -0.05≤Q+0.01(X 2 -100×Y 2 )-0.026(3X-10Y)≤0.05.
[0007] Optionally, X is 1-10.
[0008] Optionally, the Y is 0.01% to 50%.
[0009] Optionally, X is 3.5 to 4.5, and Y is 9% to 15%.
[0010] Optionally, the Q is greater than or equal to 0.1.
[0011] Optionally, the thickness of the carbon-nitrogen coating layer is less than or equal to 1 μm.
[0012] Optionally, the mass percentage of carbon element in the positive electrode active material is 0.1% to 2%.
[0013] Optionally, the ternary cathode material includes Li α Ni β Co γ M 1-β-γ O2, wherein 0.98≤α≤1.02, 0<β<1, 0<γ<1, and the M is selected from at least one of Al, Mg, Ga, Ti, Cr, Cu, Zn, Mo and Mn.
[0014] Optionally, the form of the nitrogen element in the carbon-nitrogen coating layer includes at least one of pyridinic nitrogen, pyrrolic nitrogen, graphitized nitrogen and nitrogen oxide.
[0015] The single crystal particle size, mass percentage of nitrogen in the carbon-nitrogen coating layer, and liquid retention in the positive electrode active material provided by the present disclosure satisfy a certain relationship, thereby helping to improve the cycle performance of the positive electrode active material and facilitating the use of the positive electrode active material.
[0016] In a second aspect, the present disclosure provides a positive electrode, comprising a positive electrode current collector and a positive electrode active material layer disposed on a surface of the positive electrode current collector, wherein the positive electrode active material layer comprises the positive electrode active material according to the first aspect.
[0017] The positive electrode provided by the present disclosure has excellent cycle performance, which is beneficial to the use of the positive electrode.
[0018] In a third aspect, the present disclosure provides a battery comprising a negative electrode and the positive electrode described in the second aspect.
[0019] The battery provided by the present disclosure has good cycle performance and good safety, and is conducive to long-term use.
[0020] In a fourth aspect, the present disclosure provides an electrical device comprising the battery described in the third aspect.
[0021] The battery in the electrical equipment provided by the present disclosure has excellent electrochemical performance, thereby improving the performance and service life of the electrical equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the embodiments or the description of the prior art. The specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0023] FIG1 is a schematic cross-sectional view of a positive electrode active material provided in one embodiment of the present disclosure.
[0024] FIG2 is a cross-sectional view of a positive electrode provided in one embodiment of the present disclosure.
[0025] FIG3 is an electron microscope image of the positive electrode active material prepared in Example 1.
[0026] FIG4 is a schematic structural diagram of a battery provided in an embodiment of the present disclosure.
[0027] FIG5 is a schematic structural diagram of an electrical device provided in an embodiment of the present disclosure. DETAILED DESCRIPTION
[0028] The following will be combined with the accompanying drawings in the embodiments of the present disclosure to clearly and completely describe the technical solutions in the embodiments of the present disclosure. Obviously, the embodiments described are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without making any creative efforts shall fall within the scope of protection of the present disclosure.
[0029] Please refer to Figure 1, which is a cross-sectional schematic diagram of a positive electrode active material provided in one embodiment of the present disclosure, wherein the positive electrode active material 10 includes a ternary positive electrode material 11 and a carbon-nitrogen coating layer 12 coating the ternary positive electrode material 11. The particle size of the single crystal particles of the ternary positive electrode material 11 is X μm, the mass percentage of nitrogen in the carbon-nitrogen coating layer 12 is Y, and the liquid retention capacity of the positive electrode active material 10 is Q g / cm 3 , X, Y and Q satisfy: -0.05≤Q+0.01(X 2 -100×Y 2 )-0.026(3X-10Y)≤0.05.
[0030] The positive electrode active material provided by the present invention adopts a carbon-nitrogen coating layer to coat the ternary positive electrode material. Compared with the uncoated ternary positive electrode material, the coating of the carbon-nitrogen coating layer can avoid contact between the electrolyte and the ternary positive electrode material, thereby avoiding the occurrence of side reactions and ensuring the performance of the ternary positive electrode material. In addition, compared with the carbon coating layer, the carbon-nitrogen coating layer can make the originally neutral interface electronegative, and can generate electrostatic adsorption with the positively charged lithium salt in the electrolyte, thereby improving the liquid retention effect of the positive electrode active material. In addition, the provision of the carbon-nitrogen coating layer can further avoid direct contact between the ternary positive electrode material and the electrolyte, thereby improving the long-term cycle stability of the ternary positive electrode material, and further improving the cycle stability of the positive electrode active material. At the same time, the particle size of the single crystal particles of the ternary positive electrode material, the mass percentage of the nitrogen element in the carbon-nitrogen coating layer and the liquid retention amount of the positive electrode active material satisfy -0.05≤Q+0.01(X 2 -100×Y 2)-0.026(3X-10Y)≤0.05, the cycle performance of the positive electrode and the battery can be improved. That is to say, the present invention obtains a positive electrode and a battery with excellent cycle performance by setting the particle size of the single crystal particles of the ternary positive electrode material, the mass percentage of the nitrogen element in the carbon-nitrogen coating layer, and the liquid retention amount of the positive electrode active material, which is beneficial to improving the use of the positive electrode and the battery.
[0031] In the present disclosure, the particle size of the single crystal particles of the ternary positive electrode material is X, in μm, wherein the particle size of the single crystal particles of the ternary positive electrode material is measured by an electron microscope spectrometer (in μm), and the average value of the particle size of at least 200 single crystal particles of the ternary positive electrode material is taken as X. The carbon-nitrogen coating layer contains carbon and nitrogen elements, and the mass percentage of the nitrogen element is Y, that is, the mass percentage of the carbon element in the carbon-nitrogen coating layer is not 0, and the mass percentage of the nitrogen element is not 0 (Y is not 0), and the mass percentages of the carbon element and the nitrogen element in the carbon-nitrogen coating layer are measured by an energy spectrometer. The liquid retention value of the positive electrode active material is Q, in g / cm 3 The positive electrode active material is mixed with a binder and a conductive agent to form a positive electrode slurry. The positive electrode slurry is coated on an aluminum foil current collector to form a positive electrode active material layer (volume V1). After drying at 25°C and 1.5MPa, the overall mass is measured as M0. The slurry is placed in a LiPF6 electrolyte (wherein the lithium salt concentration is 1 mol / L and the solvents are ethylene carbonate and dimethyl carbonate). After standing for 3 hours, the slurry is removed and the mass M1 is measured. The liquid retention value Q = (M1-M0) / V1.
[0032] It can be understood that the ternary positive electrode material in the present disclosure may include single crystal particles, and may also include secondary particles formed by the aggregation of single crystal particles. In the present disclosure, the particle size of the single crystal particles of the ternary positive electrode material is Xμm. In one embodiment of the present disclosure, X is 1 to 10. When the particle size of the single crystal particles of the ternary positive electrode material is 1μm to 10μm, the single crystal particles of the ternary positive electrode material can avoid agglomeration and have a suitable specific surface area, which helps to improve the liquid retention capacity of the positive electrode active material and is also beneficial to the deintercalation of lithium. In addition, the preparation difficulty and preparation cost are low, which is beneficial to the improvement of the performance and use of the positive electrode active material. Specifically, X can be, but is not limited to, 1, 1.5, 1.7, 2, 2.2, 2.5, 3, 3.4, 3.5, 3.6, 3.9, 4, 4.2, 4.5, 4.6, 5, 5.5, 5.8, 6, 6.1, 6.5, 7, 7.5, 7.6, 8, 8.3, 8.5, 9, 9.5, 9.9, or 10. In one embodiment of the present disclosure, X can be 1 to 8. In another embodiment of the present disclosure, X can be 2 to 8. In another embodiment of the present disclosure, X can be 3 to 7. In another embodiment of the present disclosure, X can be 3 to 6. In another embodiment of the present disclosure, X can be 3 to 5, which is beneficial for the preparation of the positive electrode active material and the deintercalation of lithium, and can also increase the liquid retention of the positive electrode active material and improve the rate performance of the positive electrode and the battery. In another embodiment of the present disclosure, X can be 3 to 4.5. In another embodiment of the present disclosure, X can be 3.5 to 4.5. Compared to single crystal particles of ternary cathode materials with other particle sizes, the single crystal particles of the ternary cathode materials disclosed herein can have a particle size of 3.5 μm to 4.5 μm, which improves the particle packing effect of the cathode material, namely, provides suitable compaction and liquid-retaining spaces between the particles, thereby further improving the electrochemical performance of the cathode material. In another embodiment of the present disclosure, X can be 3.5 to 4.
[0033] In one embodiment of the present disclosure, the ternary cathode material includes Li α Ni β Co γ M 1-β-γ O2, wherein 0.98≤α≤1.02, 0<β<1, 0<γ<1, M is selected from at least one of Al, Mg, Ga, Ti, Cr, Cu, Zn, Mo and Mn. The above-mentioned ternary positive electrode material has a higher energy density than iron phosphate (LiFePO4) and also meets the life working condition requirements of power battery level. Specifically, the ternary positive electrode material can include but is not limited to Li α Ni β Co γ Al 1-β-γ O2、Li α Ni β Co γ Mg 1-β-γO2、Li α Ni β Co γ Ga 1-β-γ O2、Li α Ni β Co γ Ti 1-β-γ O2、Li α Ni β Co γ Cr 1-β-γ O2、Li α Ni β Co γ Cu 1-β-γ O2、Li α Ni β Co γ Zn 1-β-γ O2、Li α Ni β Co γ Mo 1-β-γ O2 and Li α Ni β Co γ Mn 1-β-γ At least one of O2.
[0034] In the related art, when the positive electrode active material directly adopts the ternary positive electrode material, the ternary positive electrode material is in full contact with the electrolyte, resulting in side reactions between the electrolyte and the ternary positive electrode material, reducing the performance of the positive electrode active material and affecting the service life of the battery. In the present disclosure, a carbon-nitrogen coating layer is coated on the surface of the ternary positive electrode material, thereby avoiding the ternary positive electrode material from being in full contact with the electrolyte during use, thereby reducing or even avoiding the occurrence of side reactions, improving the performance of the ternary positive electrode material, and thus increasing the service life of the positive electrode active material, which is more conducive to its use in the positive electrode and battery; at the same time, compared with the coating of the carbon coating layer, the use of the carbon-nitrogen coating layer can better improve the liquid retention capacity of the positive electrode active material, thereby improving the cycle performance and service life of the positive electrode and the battery.
[0035] In the present disclosure, the mass percentage of nitrogen in the carbon-nitrogen coating layer is Y. In one embodiment of the present disclosure, Y is 0.01% to 50%. When the mass percentage of nitrogen in the carbon-nitrogen coating layer is 0.01% to 50%, it can produce a strong electrostatic adsorption effect, which helps to improve the liquid retention capacity of the positive electrode active material. At the same time, it also improves the coating stability of the carbon-nitrogen coating layer and improves the structural reliability of the positive electrode active material, thereby helping to improve the performance of the positive electrode and the battery. Specifically, Y can be, but is not limited to, 0.01%, 0.03%, 0.05%, 0.09%, 0.1%, 0.35%, 0.5%, 0.7%, 1%, 5%, 8%, 10%, 12%, 14%, 15%, 19%, 20%, 22%, 25%, 27%, 30%, 31%, 35%, 36%, 40%, 43%, 45%, 47% or 50%, etc. In one embodiment of the present disclosure, Y may be 1% to 45%. In another embodiment of the present disclosure, Y may be 2% to 35%. In yet another embodiment of the present disclosure, Y may be 5% to 30%. In yet another embodiment of the present disclosure, Y may be 5% to 25%. In yet another embodiment of the present disclosure, Y may be 5% to 20%, which is beneficial for the long-term and stable coating of the carbon-nitrogen coating layer on the ternary positive electrode material, and is also beneficial for improving the liquid retention capacity of the positive electrode active material, improving the solid-liquid mass transfer efficiency, and improving the cycle performance and service life of the positive electrode and battery. In yet another embodiment of the present disclosure, Y may be 5% to 15%. In yet another embodiment of the present disclosure, Y may be 9% to 15%, thereby further improving the performance of the positive electrode active material. In yet another embodiment of the present disclosure, Y may be 10% to 15%.
[0036] In one embodiment of the present disclosure, X is 3.5 to 4.5, and Y is 9% to 15%. This is beneficial to improving the effective and long-term coating of the carbon-nitrogen coating layer on the ternary positive electrode material, and is beneficial to further improving the liquid retention of the positive electrode active material, thereby helping to further improve the solid-liquid mass transfer efficiency, cycle performance, etc. of the positive electrode and the battery. In one embodiment of the present disclosure, X is 3.5 to 4.5, and Y is 10% to 15%. In another embodiment of the present disclosure, X is 3.5 to 4.2, and Y is 9% to 15%. In yet another embodiment of the present disclosure, X is 3.5 to 4, and Y is 10% to 15%. The above selection allows the ternary positive electrode material and the carbon-nitrogen coating layer to further cooperate with each other, so that the positive electrode active material has a higher liquid retention capacity, further improving the cycle performance of the positive electrode and the battery. In a specific embodiment, X can be 3.9 and Y is 12%, further improving the cycle performance of the positive electrode and the battery.
[0037] In the present disclosure, the carbon-nitrogen coating layer contains carbon elements, which can improve the electron transport capacity of the ternary positive electrode material, accelerate the deintercalation of lithium ions, and improve the rate performance of the positive electrode active material. In one embodiment of the present disclosure, the mass percentage of carbon elements in the positive electrode active material is 0.1% to 2%. The above content can not only ensure the improvement of the rate performance of the positive electrode active material, but also further increase the content of the ternary positive electrode material in the positive electrode active material, thereby improving the electrochemical performance of the positive electrode active material. Specifically, the mass percentage of carbon elements in the positive electrode active material can be, but is not limited to, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.2%, 1.5%, 1.8%, 1.9% or 2%. In one embodiment, the mass percentage of carbon elements in the positive electrode active material can be 0.5% to 2%. In another embodiment, the mass percentage of carbon elements in the positive electrode active material can be 1% to 2%. In another embodiment, the mass percentage of carbon in the positive electrode active material may be 1% to 1.5%.
[0038] In one embodiment of the present disclosure, the form of nitrogen in the carbon-nitrogen coating layer may include at least one of pyridinic nitrogen, pyrrolic nitrogen, graphitized nitrogen and nitrogen oxide, thereby ensuring the stable presence of nitrogen in the carbon-nitrogen coating layer. In one embodiment of the present disclosure, the form of carbon in the carbon-nitrogen coating layer may include at least one of graphene, amorphous carbon, graphite, acetylene black and carbon nanotubes. In one embodiment of the present disclosure, the number of graphene layers may be 1 to 100 layers. Specifically, the number of graphene layers may be, but is not limited to, 3 to 90 layers, 10 to 80 layers, or 15 to 75 layers, etc.
[0039] In one embodiment of the present disclosure, the thickness of the carbon-nitrogen coating layer is less than or equal to 1 μm. The above thickness not only ensures the coating of the carbon-nitrogen coating layer on the ternary positive electrode material and prevents the ternary positive electrode material from contacting the electrolyte, but also ensures the performance of the ternary positive electrode material in the positive electrode active material. Specifically, the thickness of the carbon-nitrogen coating layer may be, but is not limited to, 10 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm or 1 μm, etc. In one embodiment of the present disclosure, the thickness of the carbon-nitrogen coating layer may be 10 nm to 1 μm. In another embodiment of the present disclosure, the thickness of the carbon-nitrogen coating layer may be 100 nm to 900 nm. In another embodiment of the present disclosure, the thickness of the carbon-nitrogen coating layer may be 400 nm to 800 nm.
[0040] In one embodiment of the present disclosure, the carbon-nitrogen coating rate of the positive electrode active material may be greater than or equal to 50%. It can be understood that the coating rate is the ratio of the area of the ternary positive electrode material covered by the carbon-nitrogen coating layer to the entire surface area of the ternary positive electrode material. Specifically, the carbon-nitrogen coating rate of the positive electrode active material may be, but is not limited to, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or 90%, etc. In one embodiment of the present disclosure, the carbon-nitrogen coating rate of the positive electrode active material may be 50% to 90%. In another embodiment of the present disclosure, the carbon-nitrogen coating rate of the positive electrode active material may be 60% to 80%.
[0041] In the present disclosure, the carbon-nitrogen coating layer may be a non-porous structure or a porous structure. In one embodiment of the present disclosure, the carbon-nitrogen coating layer has a porous structure, which may include at least one of micropores and mesopores. Among them, a pore structure with a pore diameter less than 2nm is micropores, and a pore structure with a pore diameter between 2nm and 50nm is mesopores.
[0042] In one embodiment of the present disclosure, the carbon-nitrogen coating layer may further contain oxygen. Specifically, the oxygen content in the carbon-nitrogen coating layer may be, but is not limited to, less than or equal to 0.05%, 0.1%, 0.5%, 0.8%, 1%, 2%, or 3%. In another embodiment of the present disclosure, the sum of the mass percentages of carbon and nitrogen in the carbon-nitrogen coating layer is 1. In other words, the carbon-nitrogen coating layer may not contain other impurity elements.
[0043] In the present disclosure, the particle size X of the single crystal particles of the ternary positive electrode material, the mass percentage Y of the nitrogen element in the carbon-nitrogen coating layer and the liquid retention amount Q of the positive electrode active material satisfy -0.05≤Q+0.01(X 2 -100×Y 2 )-0.026(3X-10Y)≤0.05, which can improve the cycle performance of the positive electrode and the battery; wherein the liquid retention amount of the positive electrode active material can be selected as needed. In one embodiment of the present disclosure, the liquid retention amount of the positive electrode active material can be greater than 0.07g / cm 3 , that is, Q is greater than 0.07. In another embodiment of the present disclosure, the liquid retention capacity of the positive electrode active material can be greater than 0.11 g / cm 3 , that is, Q is greater than 0.11, the positive electrode active material has a high liquid retention capacity, which is beneficial to improving the performance of the positive electrode active material and the battery. In another embodiment of the present disclosure, the liquid retention capacity of the positive electrode active material can be greater than or equal to 0.13g / cm 3 , which is beneficial to improving the energy density of the positive electrode and the battery, and improving the performance of the positive electrode and the battery. Specifically, the liquid retention capacity of the positive electrode active material can be but is not limited to greater than or equal to 0.13g / cm 3 , greater than or equal to 0.14g / cm 3, greater than or equal to 0.15g / cm 3 , greater than or equal to 0.155g / cm 3 or greater than or equal to 0.16 g / cm 3 In one embodiment of the present disclosure, the liquid retention capacity of the positive electrode active material can be greater than 0.07 g / cm 3 And less than 0.25g / cm 3 In one embodiment, the liquid retention capacity of the positive electrode active material can be greater than 0.11 g / cm 3 And less than 0.2g / cm 3 , which is beneficial to improving the liquid retention capacity of the positive electrode active material without increasing the difficulty of preparing the positive electrode and the battery too much, and is helpful to improve the performance of the positive electrode and the battery. In another embodiment, the liquid retention capacity of the positive electrode active material can be greater than 0.11g / cm 3 And less than 0.18g / cm 3 .
[0044] The present disclosure also provides a method for preparing a positive electrode active material, comprising mixing a ternary positive electrode material with a carbon source and a nitrogen source, and forming a carbon-nitrogen coating layer on the surface of the ternary positive electrode material after heating to obtain the positive electrode active material in any of the above embodiments.
[0045] In one embodiment of the present disclosure, a lithium source, a nickel source, a cobalt source, and a raw material containing an element M can be mixed and reacted to obtain a ternary positive electrode material. M is selected from at least one of Al, Mg, Ga, Ti, Cr, Cu, Zn, Mo, and Mn. Specifically, the lithium source can include at least one of lithium hydroxide, lithium chloride, lithium bromide, lithium sulfate, lithium nitrate, lithium chlorate, lithium formate, and lithium acetate, such as LiOH·H2O; the nickel source can include at least one of nickel sulfate, nickel chloride, nickel nitrate, nickel oxalate, and nickel acetate; the cobalt source can include at least one of cobalt sulfate, cobalt chloride, cobalt nitrate, cobalt oxalate, and cobalt acetate; and the raw material containing the element M can include at least one of sulfate, chloride, nitrate, oxalate, and acetate. The amounts of the lithium source, nickel source, cobalt source, and raw material containing the element M are selected based on the content of each element in the ternary positive electrode material. In one embodiment of the present disclosure, a lithium source, a nickel source, a cobalt source, and a raw material containing an M element can be added to water and stirred for more than 1 hour to form a mixed solution; the mixed solution is placed in a hydrothermal kettle (such as a 500ml polytetrafluoroethylene hydrothermal kettle), sealed and placed in an oven for reaction, and then vacuum dried to obtain a ternary positive electrode material. In one embodiment, the reaction temperature can be 100°C to 200°C, and the reaction time can be 10h to 24h. Specifically, the reaction temperature can be, but is not limited to, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, and the reaction time can be, but is not limited to, 10h, 12h, 15h, 18h, 20h, 22h or 24h, etc. In one embodiment, the reaction temperature can be 100°C to 150°C, and the reaction time can be 15h to 24h. In a specific embodiment, the reaction temperature may be 200° C., and the reaction time may be 10 h.
[0046] In one embodiment of the present disclosure, the ternary cathode material can be mixed with a carbon source, and then a nitrogen source is introduced, and the cathode active material is obtained after heating. Wherein, the carbon source includes at least one of glucose, sucrose, citric acid and epoxy resin, and the nitrogen source can be, but is not limited to, ammonia. When the nitrogen source is introduced, an inert gas and a reducing gas, such as argon, hydrogen, etc., can also be passed through. In one embodiment, the ratio of the amount of inert gas, reducing gas and ammonia introduced can be (70-90): (1-10): (9-20). Specifically, the ratio of the amount of inert gas, reducing gas and ammonia introduced can be, but is not limited to, 70:10:20, 75:8:17, 80:5:15, 83:5:12, 85:4:11, 88:3:9 or 90:1:9. In a specific embodiment, the ratio of the amount of argon, hydrogen and ammonia introduced can be, but is not limited to, 80:5:15. The addition of a carbon source or nitrogen source during the above preparation process may introduce oxygen, or the oxygen contained in the carbon source or nitrogen source itself may not be removed during the above preparation process, thereby causing the carbon-nitrogen coating in the positive electrode active material to contain oxygen. In one embodiment of the present disclosure, heating includes a heating stage and a holding stage. The heating rate of the heating stage can be 1°C / min to 10°C / min, the temperature of the holding stage can be 500°C to 800°C, and the holding time of the holding stage can be 0.5h to 5h, thereby improving the performance and preparation efficiency of the positive electrode active material. Specifically, the heating rate in the heating stage may be, but is not limited to, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, or 10°C / min, and the temperature in the holding stage may be, but is not limited to, 500°C, 510°C, 520°C, 530°C, 550°C, 580°C, 600°C, 620°C, 650°C, 700°C, 750°C, or 800°C. In one embodiment of the present disclosure, the temperature in the holding stage may be 500°C-700°C, 520°C-700°C, or 550°C-650°C. In one embodiment of the present disclosure, heating includes a heating stage and a holding stage. The heating rate in the heating stage may be 3°C / min-8°C / min, the temperature in the holding stage may be 600°C-800°C, and the holding time in the holding stage may be 1 hour-4 hours. In one embodiment, the heating process includes a heating phase and a holding phase. The heating rate in the heating phase may be 5°C / min, the temperature in the holding phase may be 800°C, and the holding time in the holding phase may be 2 hours. The heating phase may start from, but is not limited to, room temperature. Specifically, the room temperature may be, but is not limited to, 25°C.
[0047] Refer to Figure 2, which is a cross-sectional view of a positive electrode provided in one embodiment of the present disclosure. Positive electrode 100 includes a positive electrode current collector 20 and a positive electrode active material layer 30 disposed on the surface of positive electrode current collector 20. Positive electrode active material layer 30 is made of the positive electrode active material of any of the above-mentioned embodiments. The positive electrode active material provided in the present disclosure has a high liquid retention capacity, thereby providing the positive electrode with excellent cycle performance, which is beneficial for the use of the positive electrode.
[0048] In the present disclosure, the positive electrode current collector is independently selected from metal foil or alloy foil. Metal foil includes copper, titanium, aluminum, platinum, iridium, ruthenium, nickel, tungsten, tantalum, gold, or silver foil. Alloy foil includes stainless steel or an alloy containing at least one of copper, titanium, aluminum, platinum, iridium, ruthenium, nickel, tungsten, tantalum, gold, and silver. For example, the positive electrode current collector can be aluminum foil. The thickness and surface roughness of the positive electrode current collector in the present disclosure can be adjusted according to actual needs.
[0049] In the present disclosure, the positive electrode active material layer may further include at least one of a binder and a conductive agent. Specifically, the binder may include at least one of fluorine-containing resin, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, polyolefin, styrene-butadiene rubber, etc.; the conductive agent may include at least one of conductive carbon black (such as acetylene black, Ketjen black), carbon nanotubes, carbon fiber, and graphite. In one embodiment of the present disclosure, the mass percentage of the binder in the positive electrode active material layer may be 0.01% to 10%, and the mass percentage of the conductive agent in the positive electrode active material layer may be 0.1% to 20%. Specifically, the mass percentage of the binder in the positive electrode active material layer may be, but is not limited to, 0.01%, 0.1%, 0.5%, 1%, 3%, 5%, 8%, or 10%, and the mass percentage of the conductive agent in the positive electrode active material layer may be, but is not limited to, 0.01%, 0.1%, 0.5%, 1%, 3%, 5%, 8%, 10%, 13%, 15%, or 17%, etc.
[0050] In the present disclosure, the carbon-nitrogen coating layer (12) defines a receiving space (120), and a plurality of single crystal particles of the ternary positive electrode material (11) are received in the space (120).
[0051] As shown in Figure 4, the present disclosure provides a battery 104, comprising a negative electrode 102 and a positive electrode 100 according to any of the above embodiments. The battery 104 provided by the present disclosure has good cycle performance and good safety, and is suitable for long-term use.
[0052] In one embodiment of the present disclosure, the battery 104 further includes an electrolyte 108. In one embodiment of the present disclosure, at least a portion of the positive electrode is immersed in the electrolyte 108, and at least a portion of the negative electrode is immersed in the electrolyte 108, thereby ensuring normal operation of the battery. In one embodiment of the present disclosure, the electrolyte 108 includes a lithium salt and an organic solvent. Specifically, the lithium salt may include, but is not limited to, at least one of lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium perchlorate, lithium hexafluoroborate, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, LiC(CF3SO3)2, and LiN(C4F9SO2)(CF3SO3); the organic solvent may include, but is not limited to, at least one of an ether-based solvent, a nitrile-based solvent, a cyanate-based solvent, a fluoroester-based solvent, a tetrazole-based solvent, a fluorosulfonyl solvent, a chlorosulfonyl solvent, a nitro solvent, a carbonate-based solvent, a dicarbonate-based solvent, a nitrate-based solvent, a fluoroamide-based solvent, a diketone-based solvent, an azole-based solvent, and a triazine-based solvent. For example, the organic solvent may include, but is not limited to, at least one of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl methyl carbonate, and dimethyl carbonate.
[0053] As shown in Figure 5, the present disclosure provides an electric device 106 comprising a battery 104 according to any of the aforementioned embodiments. The battery 104 in the electric device 106 provided herein has excellent electrochemical properties, thereby improving the performance and service life of the electric device 106. Specifically, the electric device 106 may be a vehicle, electronic device, energy storage system, etc., and the battery 104 may be provided in the electric device 106 in the form of a single cell, a battery module, a battery pack, or the like.
[0054] The effects of the technical solution of the present disclosure are further illustrated below through the examples and comparative examples provided in the present disclosure.
[0055] In Example 1, NiSO4, CoSO4, MnSO4 and LiOH·H2O were mixed and dissolved in water, and LiNi was prepared by hydrothermal reaction. 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.8 Co 0.1 Mn 0.1 The particle size of O2 single crystal particles is 4μm. 0.8 Co 0.1 Mn 0.1 O2 and glucose were mixed, and the temperature was raised from room temperature (25°C) to 650°C at a heating rate of 5°C / min in an atmosphere containing argon, hydrogen, and ammonia (the ratio of the amount of argon, hydrogen, and ammonia was 80:5:15). The positive electrode active material was sintered at 650°C to obtain a positive electrode active material. The positive electrode active material includes LiNi coated with a carbon nitrogen coating layer. 0.8 Co 0.1 Mn 0.1O2, the mass percentage of nitrogen in the carbon-nitrogen coating layer is 10%, wherein FIG3 is an electron microscope image of the positive electrode active material prepared in Example 1.
[0056] Example 2 is similar to Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3 μm.
[0057] Example 3 is similar to Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3.5 μm.
[0058] Example 4 is similar to Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 4.5 μm.
[0059] Example 5 is similar to Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 5 μm.
[0060] Example 6 is substantially the same as Example 1, except that the sintering temperature is 500° C. and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 20%.
[0061] Example 7 is similar to Example 6, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3 μm.
[0062] Example 8 is similar to Example 6, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3.5 μm.
[0063] Example 9 is similar to Example 6, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 4.5 μm.
[0064] Example 10 is similar to Example 6, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 5 μm.
[0065] Example 11 is substantially the same as Example 1, except that the sintering temperature is 700° C. and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 5%.
[0066] Example 12 is similar to Example 11, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3 μm.
[0067] Example 13 is similar to Example 11, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3.5 μm.
[0068] Example 14 is similar to Example 11, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 4.5 μm.
[0069] Example 15 is similar to Example 11, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 5 μm.
[0070] Example 16 is substantially the same as Example 1, except that the sintering temperature is 550° C. and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 15%.
[0071] Example 17 is similar to Example 16, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3 μm.
[0072] Example 18 is similar to Example 16, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3.5 μm.
[0073] Example 19 is similar to Example 16, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 4.5 μm.
[0074] Example 20 is similar to Example 16, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 5 μm.
[0075] Example 21 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 2 μm.
[0076] Example 22 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 7 μm, and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 30%.
[0077] Example 23 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3.9 μm, and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 12%.
[0078] Example 24 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 O2 single crystal particles and Al(NO3)3 powder were mixed evenly according to the element ratio and then pre-sintered in a muffle furnace at 500℃ for 5h. Al-doped LiNi was then prepared by solid-phase spherical reaction at 750℃. 0.8 Co 0.1 Mn 0.095 Al 0.005 O2 single crystal particles (particle size 4μm). 0.8 Co 0.1 Mn 0.095 Al 0.005 O2 and glucose were mixed and sintered at 650℃ in an atmosphere containing ammonia to obtain a positive electrode active material. The positive electrode active material includes LiNi coated with a carbon-nitrogen coating layer. 0.8 Co 0.1 Mn 0.095 Al 0.005 O2, the mass percentage of nitrogen in the carbon-nitrogen coating layer is 10%.
[0079] Example 25 is substantially the same as Example 1, except that the mass percentage of nitrogen in the carbon-nitrogen coating layer is 9%.
[0080] Example 26 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 1 μm, the sintering temperature is 520° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 50%.
[0081] Example 27 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 2 μm, the sintering temperature is 535° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 38%.
[0082] Example 28 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 4.5 μm, the sintering temperature is 535° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 33%.
[0083] Example 29 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 8 μm, the sintering temperature is 520° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 49%.
[0084] Example 30 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 8.7 μm, the sintering temperature is 520° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 50%.
[0085] Example 31 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3 μm, the ratio of the introduction of argon, hydrogen and ammonia is 85:5:10, the sintering temperature is 750° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 0.01%.
[0086] Example 32 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 10 μm, the ratio of the introduction of argon, hydrogen and ammonia is 81:6:17, the sintering temperature is 505° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 63%.
[0087] Example 33 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1The particle size of the O2 single crystal particles is 10.1 μm, the ratio of the introduction of argon, hydrogen and ammonia is 77:6:17, the sintering temperature is 505° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 65%.
[0088] Example 34 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 0.8 μm, the sintering temperature is 535° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 35%.
[0089] Example 35 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 2 μm, the ratio of the introduction of argon, hydrogen and ammonia is 85:5:10, the sintering temperature is 505° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 0.005%.
[0090] Comparative Example 1 is similar to Example 1, except that the sintering atmosphere does not contain ammonia, and the positive electrode active material obtained is LiNi coated with a carbon coating layer. 0.8 Co 0.1 Mn 0.1 O2.
[0091] Comparative Example 2 is similar to Comparative Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3 μm.
[0092] Comparative Example 3 is similar to Comparative Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3.5 μm.
[0093] Comparative Example 4 is similar to Comparative Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 4.5 μm.
[0094] Comparative Example 5 is similar to Comparative Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 5 μm.
[0095] Comparative Example 6 is similar to Example 1, except that the carbon-nitrogen coating layer is not prepared. 0.8Co 0.1 Mn 0.1 O2 is directly used as the positive electrode active material.
[0096] Comparative Example 7 is similar to Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 3 μm, the sintering temperature is 530° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 40%.
[0097] Comparative Example 8 is similar to Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 1 μm, the sintering temperature is 550° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 20%.
[0098] Comparative Example 9 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 6 μm, the sintering temperature is 520° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 50%.
[0099] Comparative Example 10 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 10 μm, the sintering temperature is 540° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 30%.
[0100] Comparative Example 11 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 8 μm, the sintering temperature is 500° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 70%.
[0101] Comparative Example 12 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 7 μm, the ratio of the introduction of argon, hydrogen and ammonia is 85:5:10, the sintering temperature is 800° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 0.005%.
[0102] Comparative Example 13 is similar to Example 1, except that LiNi 0.8 Co 0.1 Mn 0.1The particle size of the O2 single crystal particles is 12 μm, the sintering temperature is 650° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 10%.
[0103] Comparative Example 14 is similar to Example 1 except that LiNi 0.8 Co 0.1 Mn 0.1 The particle size of the O2 single crystal particles is 0.05 μm, the sintering temperature is 700° C., and the mass percentage of nitrogen in the carbon-nitrogen coating layer is 5%.
[0104] The following describes the test results of the properties of the positive electrode active materials in the above examples and comparative examples.
[0105] The above-mentioned positive electrode active material was mixed with a binder, PVDF, and a conductive agent, carbon nanotubes, to form a positive electrode slurry. The positive electrode slurry was coated on the surface of an aluminum foil current collector and rolled at 25°C under a pressure of 1.5 MPa to form a positive electrode active material layer. The positive electrode mass M0 and the volume V1 of the positive electrode active material layer were measured. The positive electrode was placed in a LiPF6 electrolyte (wherein the lithium salt concentration was 1 mol / L and the solvents were ethylene carbonate and dimethyl carbonate). After standing for 3 hours, the positive electrode was removed and the mass M1 was measured. The liquid retention capacity Q g / cm was calculated. 3 The results are shown in Table 1, where Q = (M1-M0) / V1, and Q + 0.01 (X 2 -100×Y 2 )-0.026(3X-10Y) (keep four decimal places). The results are shown in the formula value column in Table 1.
[0106] The above-mentioned positive electrode active materials were made into the same standard button-type batteries and then subjected to cycle performance testing, wherein charge and discharge cycles were performed at 2.5V to 4.3V and 0.5C. The capacity retention after 100 cycles is shown in Table 1.
[0107] Table 1 Test results
[0108] As can be seen from Table 1, compared with Comparative Examples 1-6, the positive electrode active materials provided by the present disclosure have a carbon-nitrogen coating layer, and the cycle performance of the battery 104 prepared from these positive electrode active materials is more excellent. Compared with Comparative Examples 7-14, the particle size X of the single crystal particles of the ternary positive electrode material in the positive electrode active materials provided by the present disclosure, the mass percentage Y of the nitrogen element in the carbon-nitrogen coating layer, and the liquid retention capacity Q of the positive electrode active material satisfy -0.05≤Q+0.01(X 2 -100×Y 2)-0.026(3X-10Y)≤0.05, resulting in a battery 104 with improved cycle performance. Compared to Examples 32-35, the battery 104 made with the positive electrode active materials provided in the other examples exhibited improved cycle performance. Therefore, the battery 104 made with the positive electrode active materials provided in the present disclosure exhibits excellent cycle performance, thereby facilitating the use of the battery 104.
[0109] The above description is a preferred embodiment of the present disclosure, but it should not be construed as limiting the scope of the present disclosure. It should be noted that those skilled in the art may make various improvements and modifications without departing from the principles of the present disclosure, and such improvements and modifications are also considered to be within the scope of protection of the present disclosure.
Claims
1. A positive electrode active material (10), characterized in that: The invention comprises a ternary positive electrode material (11) and a carbon-nitrogen coating layer (12) coating the ternary positive electrode material (11), wherein the particle size of the single crystal particles of the ternary positive electrode material (11) is X μm, the mass percentage of the nitrogen element in the carbon-nitrogen coating layer (12) is Y, and the liquid retention capacity of the positive electrode active material (10) is Q g / cm 3 , X, Y and Q satisfy: -0.05≤Q+0.01(X 2 -100×Y 2 )-0.026(3X-10Y)≤0.
05.
2. The positive electrode active material (10) according to claim 1, characterized in that The X is 1-10.
3. The positive electrode active material (10) according to claim 1 or 2, characterized in that: The Y is 0.01% to 50%.
4. The positive electrode active material (10) according to any one of claims 1 to 3, characterized in that The X is 3.5 to 4.5, and the Y is 9% to 15%.
5. The positive electrode active material (10) according to any one of claims 1 to 4, characterized in that The Q is greater than 0.
11.
6. The positive electrode active material (10) according to any one of claims 1 to 5, characterized in that The Q is greater than 0.11 and less than 0.25 g / cm 3 .
7. The positive electrode active material (10) according to any one of claims 1 to 6, characterized in that: The thickness of the carbon-nitrogen coating layer (12) is less than or equal to 1 μm.
8. The positive electrode active material (10) according to any one of claims 1 to 7, characterized in that The thickness of the carbon-nitrogen coating layer (12) is less than or equal to 1 μm and greater than or equal to 10 nm.
9. The positive electrode active material (10) according to any one of claims 1 to 8, characterized in that The mass percentage of carbon element in the positive electrode active material (10) is 0.1% to 2%.
10. The positive electrode active material (10) according to any one of claims 1 to 9, characterized in that The ternary positive electrode material (11) includes Li α Ni β Co γ M 1-β-γ O2, wherein 0.98≤α≤1.02, 0<β<1, 0<γ<1, and M is selected from at least one of Al, Mg, Ga, Ti, Cr, Cu, Zn, Mo and Mn.
11. The positive electrode active material (10) according to any one of claims 1 to 10, characterized in that: The form of the nitrogen element in the carbon-nitrogen coating layer (12) includes at least one of pyridinic nitrogen, pyrrolic nitrogen, graphitized nitrogen and oxidized nitrogen.
12. The positive electrode active material (10) according to any one of claims 1 to 11, characterized in that The carbon-nitrogen coating layer (12) defines a receiving space (120), and a plurality of single crystal particles of the ternary positive electrode material (11) are received in the space (120).
13. A positive electrode (100), characterized in that: The invention comprises a positive electrode current collector (20) and a positive electrode active material layer (30) arranged on the surface of the positive electrode current collector (20), wherein the positive electrode active material layer (30) comprises the positive electrode active material (10) according to any one of claims 1 to 12.
14. A battery (104), characterized in that: It comprises a negative electrode (102) and the positive electrode (100) according to claim 13.
15. The battery (104) according to claim 14, further comprising an electrolyte (108), wherein at least a portion of the positive electrode (100) is immersed in the electrolyte (108), and at least a portion of the negative electrode (102) is immersed in the electrolyte (108).
16. An electrical device (106), characterized in that: Comprising the battery (104) according to claim 14 or 15.
Citation Information
Patent Citations
Ternary positive material preparation method and ternary positive material
CN107579237A
Positive plate of high-power lithium-ion battery and preparation method of positive plate
CN107611339A
N-doped C coated NCA cathode material, lithium ion battery and preparation method
CN108666559A
Nitrogen-doped carbon-coated ternary cathode material and preparation method thereof
CN110783564A
Preparation method of template-method-coated lithium ion battery high-nickel ternary positive electrode material
CN112186167A