Thermal-runaway-preventing material which rapidly absorbs heat, and preparation method therefor
Through the thermal runaway protection material of the laminated structure, combined with the packaging technology of thermal conductive adhesive and flame-retardant graphite thermal conductive film, the problems of low thermal conductivity and easy deformation of materials in the existing technology are solved, achieving efficient heat absorption and modular installation, reducing risk of thermal runaway.
Patent Information
- Application Number
- PCT/CN2024/101971
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-31
AI Technical Summary
Existing technology cannot effectively control the risk of thermal runaway in small electronic components or high-energy batteries. Existing heat-absorbing materials have low thermal conductivity and are easily deformed under high humidity, and cannot be directly used for heat absorption and packaging.
Thermal runaway protection materials using a laminated structure include flame-retardant graphite thermal conductive films, thermal conductive adhesives, high thermal conductivity endothermic materials and edge sealing adhesives. Through adhesive glue and loaded flame-retardant graphite organic tin catalyst composite endothermic materials, combined with thermal conductive adhesive Encapsulated with flame-retardant graphite thermal conductive film to achieve high thermal conductivity and modular installation.
The thermal runaway protection material with high thermal conductivity has been realized, with an endothermic enthalpy value higher than 1200J/g. It can actively absorb heat in the range of 60-400°C, reduce the maximum temperature of thermal runaway, and prevent fire and explosion.
Smart Images

Figure CN2024101971_31102024_PF_FP_ABST
Abstract
Description
A fast-absorbing thermal runaway protection material and its preparation method Technical Field
[0001] The present invention belongs to the technical field of thermal runaway protection materials, and in particular relates to a fast-absorbing thermal runaway protection material and a preparation method thereof. Background Art
[0002] With the rapid development of new energy vehicles and autonomous driving technologies, more and more functional requirements are placed on the electronic control of automobiles, and more and more electronic components are needed. However, the space of the automobile itself is limited. Reducing the size of electronic components and increasing the size and energy density of batteries are the current key research directions.
[0003] However, packaging a large number of electronic components or high-energy batteries in a very small volume also brings the risk of thermal runaway. Thermal runaway refers to a chain reaction phenomenon triggered by various factors, causing devices (such as chips, circuit boards, and batteries) to emit large amounts of heat and harmful gases in a short period of time. In severe cases, it can even cause fires and explosions. These fires or explosions can affect the energy conduction (including heat, electricity, and mechanical energy) of other surrounding cells and ignite the ejected materials, causing the thermal runaway to spread. Therefore, how to effectively control thermal runaway is a very important research direction.
[0004] The three characteristic temperature points of thermal runaway are the self-heating starting temperature T1, the thermal runaway initiation temperature T2, and the thermal runaway maximum temperature T3. Therefore, if endothermic materials can be used to absorb the heat inside the battery or component during the self-heating stage, it is possible to prevent the temperature from rising to the thermal runaway initiation temperature T2, or reduce the thermal runaway maximum temperature T3, thereby preventing the further development of thermal runaway. Endothermic materials are materials prepared by utilizing the property of absorbing heat during chemical or physical changes in phase change, dissolution, and decomposition. By attaching high thermal conductivity endothermic materials to heat-generating electronic devices or batteries to control heat and quickly absorb the heat released by the battery or electronic device, thermal runaway can be effectively alleviated. Therefore, its core lies in the selection of endothermic materials and how to achieve high thermal conductivity and encapsulate the endothermic materials.
[0005] Taking batteries as an example, the existing solutions for dealing with thermal runaway are mainly as follows: (1) Using aerogel to separate each battery pack component. After a single battery pack thermal runaway, the heat can be isolated within a limited range if it is not serious. However, aerogel cannot slow down the process of thermal runaway. When thermal runaway occurs, there is still a possibility of spillover to adjacent battery packs, causing continuous thermal runaway and fire or explosion. (2) Using phase change materials to manage battery heat. Usually, the phase change enthalpy value of phase change materials is only between 200 and 270 J / g, and after packaging, it is usually only between 100 and 200 J / g. Due to the low enthalpy value, phase change materials are usually used to maintain a constant operating temperature (such as 55°C) for the battery to maximize its performance, but cannot solve the problem of thermal runaway. (3) Installing a liquid cooling system on the battery and using a compressor to cool the battery. Due to the power limitation of the on-board compressor, the cooling efficiency of the liquid cooling system is limited and cannot cope with the instantaneous temperature rise. The above solutions for dealing with thermal runaway are of limited effectiveness when the battery is subjected to rapid heating due to squeezing, collision, accidents, etc.
[0006] The heat-absorbing materials that undergo chemical changes between 60 and 400°C and absorb a large amount of heat are mainly inorganic substances and usually exist in the form of powder. Since the powder contains a large amount of air, the thermal conductivity is low and the heat absorption efficiency is very low. It cannot be used directly for heat absorption. In addition, long-term exposure to air will cause the volatilization of crystal water and the volume and shape changes caused by the absorption of water under high humidity, making it impossible to use directly.
[0007] Summary of the Invention
[0008] To address the above technical issues, the present invention provides a rapidly absorbing thermal runaway protection material. This material exhibits excellent strength, vibration resistance, a thermal conductivity greater than 1 W.mK, and a rapid heat absorption rate. It undergoes a chemical reaction between 60°C and 400°C, actively absorbing heat. Once the chemical reaction conditions are met, the heat absorption proceeds spontaneously, resulting in a continuous heat absorption effect (the internal high-conductivity heat-absorbing material has an endothermic enthalpy greater than 1200 J / g). A sufficient amount of this material can reduce the maximum thermal runaway temperature, preventing fires and explosions caused by high temperatures.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions:
[0010] A thermal runaway protection material that absorbs heat quickly has a laminated structure comprising, from bottom to top, a flame-retardant graphite thermal conductive film, a thermal conductive adhesive, a high thermal conductivity heat-absorbing material, a thermal conductive adhesive, and a flame-retardant graphite thermal conductive film; the peripheral sides of the laminated structure are all sealed with edge-sealing adhesive.
[0011] According to the above scheme, the thickness of the thermal conductive adhesive is between 0.02mm and 0.25mm; the thickness of the flame retardant graphite thermal conductive film is between 0.02mm and 0.5mm; the thickness of the high thermal conductivity and heat absorption material is determined according to actual conditions, preferably between 0.5-100mm.
[0012] According to the above scheme, the high thermal conductivity heat-absorbing material comprises, by mass percentage, 80-94% heat-absorbing material, 1-10% heat-conducting material, 0-1% organic tin catalyst loaded with flame-retardant graphite, and 5-10% adhesive. The preparation method is as follows:
[0013] S1: Add adhesive, organic tin catalyst loaded with flame retardant graphite, and thermal conductive material into a mixing kettle, heat to 30-60°C and stir for 2-4 hours;
[0014] S2: slowly add the heat-absorbing material into the above mixing kettle while stirring, and vacuumize to remove bubbles to obtain a mixed glue;
[0015] S3: Pour the mixed glue into a PTFE mold of specified shape and thickness or a mold with a PTFE coating on the surface, and cure it at room temperature for 0.5-48 hours;
[0016] S4: After the curing time is reached, demoulding and grinding the edges to obtain the high thermal conductivity heat absorbing material.
[0017] In the above technical solution, the heat-absorbing material includes but is not limited to sodium acetate trihydrate, ammonium ferric oxalate trihydrate, citric acid monohydrate, citric acid, oxalic acid dihydrate, anhydrous oxalic acid, malonic acid, magnesium sulfate heptahydrate, zinc sulfate heptahydrate, succinic acid, maleic acid, fumaric acid, sodium carbonate decahydrate, calcium chloride hexahydrate, aluminum nitrate nonahydrate, ammonium pentaborate octahydrate, ammonium ferric sulfate dodecahydrate, ferrous chloride tetrahydrate, ammonium oxalate monohydrate, sodium tetraborate decahydrate, sodium tetraborate pentahydrate, aluminum sulfate 18hydrate, ammonium pentaborate, ammonium hydrogen borate tetrahydrate, sodium silicate pentahydrate, hydrated sodium aluminum silicate, potassium aluminum sulfate dodecahydrate, sodium sulfate decahydrate, copper sulfate heptahydrate, ferrous sulfate heptahydrate, cobalt chloride hexahydrate, calcium sulfate dihydrate, etc., a mixture of one or more in any proportion. Preferably, the heat-absorbing material includes but is not limited to a mixture of one or more of oxalic acid dihydrate, anhydrous oxalic acid, ammonium oxalate monohydrate, barium hydroxide octahydrate, sodium acetate trihydrate, boric acid, ammonium pentaborate octahydrate, sodium tetraborate decahydrate, potassium aluminum sulfate dodecahydrate, sodium sulfate decahydrate, calcium sulfate dihydrate, etc. in any proportion, and the mixture preferably has a mesh size between 100 and 500 meshes.
[0018] In the above technical solution, the thermally conductive material is a mixture of one or more carbon-based thermally conductive materials such as carbon nanotubes, flame-retardant graphite, expanded graphite and graphene in any proportion.
[0019] In the above technical solution, the flame-retardant graphite-loaded organotin catalyst is prepared as follows: flame-retardant graphite and dibutyltin diacetate are added to a reactor in a mass ratio of 1:1 to 2:1, followed by the addition of cyclohexane (30-100% by mass of the total mass of the flame-retardant graphite and dibutyltin diacetate), stirred at 50°C for 2-3 hours, and dried in a constant-temperature drying oven at 80-90°C for 24 hours to obtain the flame-retardant graphite-loaded organotin catalyst. The flame-retardant graphite is preferably flake graphite. Flame-retardant graphite itself has excellent thermal conductivity, and the addition of the flame-retardant graphite-loaded organotin catalyst can also enhance the material's thermal conductivity.
[0020] In the above technical solution, the adhesive is a low-viscosity adhesive with a viscosity range of 5 to 200 mPa.s (25°C), preferably the LPA low-viscosity potting adhesive produced by Wuhan Changyingtong Optoelectronics Technology Co., Ltd. This adhesive has low viscosity, low density, and strong penetration ability. It contains a special wetting and dispersing agent, which has excellent wettability on the surface of the heat-absorbing material. Only 5 to 10% of the total mass of the adhesive is required to achieve a high solid content of the heat-absorbing material, and the operation time is long. The curing time can be adjusted according to the addition amount of flame-retardant graphite-supported organotin catalyst to meet different application requirements.
[0021] In the above technical solution, the high-thermal-conductivity endothermic material absorbs heat through a chemical reaction at high temperatures. For example, the endothermic material decomposes to produce water, carbon dioxide, and other substances. This chemical reaction actively absorbs a large amount of heat. The generated carbon dioxide isolates combustible materials from contact with air, thus preventing fire.
[0022] In the above technical solution, the thermally conductive adhesive is preferably SE4450 double-component thermally conductive adhesive produced by Dow Chemical, which has a thermal conductivity greater than 1W / mK and a thickness between 0.02 mm and 0.2 mm.
[0023] In the above technical solution, the thickness of the flame-retardant graphite thermal conductive film is between 0.02 mm and 0.5 mm. It is a thermal conductive film prepared using flame-retardant graphite composite plastic particles. The thermal conductivity of the plastic particles is greater than 1W / mK, and the flame retardant grade reaches UL94-V0 level. Suitable plastics include but are not limited to one or more of polyamide, polyvinyl chloride, polycarbonate, polyphenylene sulfide, polyetheretherketone, polybutylene succinate, polyethylene terephthalate, polypropylene, etc.
[0024] In the above technical solution, the edge sealing glue is preferably CM102 curing glue produced by Wuhan Changyingtong Optoelectronic Technology Co., Ltd., which has very good adhesion to high thermal conductivity heat-absorbing materials, thermal conductive glue, and flame-retardant graphite thermal conductive film, and has good edge sealing effect.
[0025] In the above technical solution, the preparation method of the thermal runaway protection material for rapid heat absorption is as follows: a layer of thermal conductive adhesive is brushed on the upper and lower surfaces of the high thermal conductivity heat-absorbing material, and then the surface of the thermal conductive adhesive is covered with a flame-retardant graphite thermal conductive film, and both are flattened using a mold, placed at room temperature for 0.5 to 48 hours and cut into a specified size, and then the side is brushed with edge sealing glue, and placed at room temperature for 1 to 48 hours to obtain the high thermal conductivity heat-absorbing material. The preparation method of the thermal runaway protection material for rapid heat absorption is actually also a method for achieving high thermal conductivity and modular packaging of heat-absorbing materials. First, the powder heat-absorbing material and the heat-conducting material and the organic tin catalyst loaded with flame-retardant graphite are compounded and preliminarily packaged by an adhesive, and then further laminated and packaged and edge-sealed in combination with the thermal conductive adhesive and the flame-retardant graphite thermal conductive film, thereby achieving the high thermal conductivity and packaging effect of the heat-absorbing material described in the present invention, making a fast-absorbing thermal runaway protection block or sheet, and the size can be controlled according to demand to achieve modular installation.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The overall high thermal conductivity of the thermal runaway protection material of the present invention makes the heat absorption process fast and effective. The size can also be tailored according to customer needs to achieve modular installation.
[0028] 2. Since most of the heat-absorbing materials are powders with low thermal conductivity, and long-term exposure to the air will cause the volatilization of crystal water and the volume and shape changes caused by the absorption of moisture under high humidity, they cannot be used directly. The fast heat-absorbing thermal runaway protection material described in the present invention first combines the powdered high absorption enthalpy heat-absorbing material and the thermal conductive material and the organic tin catalyst loaded with flame-retardant graphite with an adhesive. The adhesive replaces the air on the surface of the powder, thereby achieving stable packaging of the heat-absorbing material and preventing the problem of absorbing and volatilizing moisture in the exposed air; then, the thermal conductive adhesive and the flame-retardant graphite thermal conductive film are combined to further achieve modular packaging, and the size is controlled according to demand, thereby obtaining a fast heat-absorbing thermal runaway protection material that can achieve modular installation of heat-absorbing materials.
[0029] 3. The thermal runaway protection material of the present invention has a very high endothermic enthalpy. It is a material that will undergo a chemical reaction and actively absorb heat between 60-400°C. After the chemical conditions are met, the endothermic reaction will proceed spontaneously, forming a continuous endothermic effect (the endothermic enthalpy of the internal high thermal conductivity endothermic material is greater than 1200 J / g). A sufficient amount of thermal runaway protection material can reduce the maximum thermal runaway temperature and control the heat generation to below the thermal runaway triggering temperature T2, thereby preventing fire and explosion caused by subsequent continued temperature increase. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a schematic diagram of the structure of a fast-absorbing thermal runaway protection material, which consists of four parts: 1-high thermal conductivity heat-absorbing material, 2-thermal conductive adhesive, 3-flame-retardant graphite thermal conductive film, and 4-edge sealing adhesive.
[0031] FIG2 is a schematic diagram of a test platform for testing the thermal runaway effect of thermal runaway protection materials. DETAILED DESCRIPTION
[0032] In order to better understand the present invention, the present invention is further described below through specific embodiments, but it is not intended to limit the present invention.
[0033] Some of the special raw materials used in the following examples are shown in Table 1.
[0034] Table 1
[0035] The mesh size of the heat absorbing materials involved below is between 100-500 mesh.
[0036] The flame-retardant graphite-loaded organic tin catalyst and high thermal conductivity heat-absorbing material used in the present invention are specifically prepared as follows:
[0037] 1. Preparation method of flame-retardant graphite-loaded organic tin catalyst C-1
[0038] 50 g of flame retardant graphite and 55 g of dibutyltin diacetate were added to a reactor, and 50 g of cyclohexane was added. The mixture was stirred at 50° C. for 2 hours, and dried in a constant temperature drying oven at 90° C. for 24 hours to obtain catalyst C-1.
[0039] 2. Preparation method of high thermal conductivity heat absorbing material G-1
[0040] S1: Add 80g LPA-1 adhesive, 5g flame-retardant graphite-loaded organotin catalyst C-1, and 50g carbon nanotubes into a mixing kettle, heat to 40-50°C, and stir for 2.5 hours;
[0041] S2: Slowly add 300g of the endothermic material potassium aluminum sulfate dodecahydrate and 565g of calcium chloride hexahydrate into the above mixing kettle while stirring, and vacuumize to remove bubbles to obtain a mixed glue;
[0042] S3: Pour the mixed glue into a PTFE mold with a specified length of 30 cm, width of 30 cm and thickness of 2 mm, and cure it at room temperature for 5-8 hours;
[0043] S4: After the curing time is reached, the mold is demoulded to obtain the high thermal conductivity heat-absorbing material G-1. The endothermic enthalpy at 50-300° C. is tested to be 1330 J / g.
[0044] In the above steps, the raw materials of the high thermal conductivity heat-absorbing material are calculated by mass percentage as follows: 86.5% heat-absorbing material, 5% heat-conducting carbon nanotubes, 0.5% organic tin catalyst loaded with flame-retardant graphite, and 8% adhesive.
[0045] 3. Preparation method of high thermal conductivity heat absorbing material G-2
[0046] S1: Add 70g of LPA-1 adhesive, 2g of flame-retardant graphite-loaded organotin catalyst C-1, and 30g of flame-retardant graphite into a mixing kettle, heat to 30-40°C, and stir for 3.5 hours.
[0047] S2: Slowly add 300g of silicic acid and 598g of calcium chloride hexahydrate, an endothermic material, into the above mixing kettle while stirring, and vacuumize to remove bubbles to obtain a mixed glue.
[0048] S3: Pour the mixed glue into a PTFE mold with a specified length of 30 cm, width of 30 cm and thickness of 2 mm, and cure it at room temperature for 12-24 hours.
[0049] S4: After the curing time is reached, the high thermal conductivity heat absorbing material G-2 is demoulded to obtain the heat absorbing material G-2. The heat absorption enthalpy at 50-300° C. is tested to be 1440 J / g.
[0050] In the above steps, the raw materials of the high thermal conductivity heat-absorbing material are as follows by mass percentage: heat-absorbing material 89.8%, heat-conducting material flame-retardant graphite 3%, organic tin catalyst loaded with flame-retardant graphite 0.2%, and adhesive 7%.
[0051] 4. Preparation method of high thermal conductivity heat absorbing material G-3
[0052] S1: Add 95g LPA-1 adhesive, 30g graphene, and 10g carbon nanotubes into a mixing kettle, heat to 45-55°C, and stir for 4 hours;
[0053] S2: Slowly add 665g of sodium acetate trihydrate and 200g of potassium aluminum sulfate dodecahydrate into the above mixing kettle while stirring, and vacuumize to remove bubbles to obtain a mixed glue;
[0054] S3: Pour the mixed glue into a PTFE mold with a specified length of 30 cm, width of 30 cm and thickness of 2 mm, and cure it at room temperature for 24-48 hours;
[0055] S4: After the curing time is reached, the high thermal conductivity heat absorbing material G-3 is demoulded to obtain the heat absorbing material G-3. The heat absorption enthalpy at 50-300° C. is tested to be 1226 J / g.
[0056] In the above steps, the raw materials of the high thermal conductivity heat-absorbing material are as follows by mass percentage: heat-absorbing material 86.5%, heat-conducting material (graphene and carbon nanotubes) 4%, and adhesive 9.5%.
[0057] Example 1
[0058] A thermal runaway protection material with rapid heat absorption, as shown in Figure 1, has a laminated structure, which, from bottom to top, comprises 0.2mm flame-retardant graphite thermal conductive film, 0.21mm SE4450 thermal conductive adhesive, 2mm high thermal conductivity heat-absorbing material G-1, 0.21mm SE4450 thermal conductive adhesive, and 0.2mm flame-retardant graphite thermal conductive film;
[0059] The preparation method of the above-mentioned fast heat-absorbing thermal runaway protection material is as follows: SE4450 thermal conductive adhesive is brushed on both the upper and lower surfaces of the high thermal conductivity heat-absorbing material G-1, and then the surface of the SE4450 thermal conductive adhesive is covered with a flame-retardant graphite thermal conductive film. It is flattened using a mold, left at room temperature for 24 hours, and then cut into a specified length of 23 cm and a width of 16 cm. Then, edge sealing glue is brushed on the side. After leaving it at room temperature for 1 hour, the thermal runaway protection material A is obtained. The average thickness is 2.82 mm. The thermal conductivity coefficient, enthalpy value and density of the internal high thermal conductivity heat-absorbing material are shown in Table 2.
[0060] Example 2
[0061] A thermal runaway protection material that absorbs heat quickly, which has a laminated structure consisting of, from bottom to top, 0.2mm flame-retardant graphite thermal conductive film, 0.115mm SE4450 thermal conductive adhesive, 2mm high thermal conductivity heat-absorbing material G-1, 0.115mm SE4450 thermal conductive adhesive, and 0.2mm flame-retardant graphite thermal conductive film;
[0062] The preparation method of the above-mentioned fast heat-absorbing thermal runaway protection material is as follows: SE4450 thermal conductive adhesive is brushed on the upper and lower surfaces of the high thermal conductivity heat-absorbing material G-2, and then the surface of the SE4450 thermal conductive adhesive is covered with a flame-retardant graphite thermal conductive film. It is flattened using a mold, and after being left at room temperature for 24 hours, it is cut into a specified length of 23 cm and a width of 16 cm. Then, edge sealing glue is brushed on the side. After being left at room temperature for 1 hour, the thermal runaway protection material B is obtained. The average thickness is 2.63 mm. The thermal conductivity coefficient, enthalpy value and density of the internal high thermal conductivity heat-absorbing material are shown in Table 2.
[0063] Example 3
[0064] A thermal runaway protection material that absorbs heat quickly, which has a laminated structure consisting of, from bottom to top, 0.2mm flame-retardant graphite thermal conductive film, 0.17mm SE4450 thermal conductive adhesive, 2mm high thermal conductivity heat-absorbing material G-1, 0.17mm SE4450 thermal conductive adhesive, and 0.2mm flame-retardant graphite thermal conductive film;
[0065] The preparation method of the above-mentioned fast heat-absorbing thermal runaway protection material is as follows: SE4450 thermal conductive adhesive is brushed on the upper and lower surfaces of the high thermal conductivity heat-absorbing material G-3, and then the surface of the SE4450 thermal conductive adhesive is covered with a flame-retardant graphite thermal conductive film. It is flattened using a mold, and after being left at room temperature for 24 hours, it is cut into a specified length of 23 cm and a width of 16 cm. Then, edge sealing glue is brushed on the side. After being left at room temperature for 1 hour, the thermal runaway protection material C is obtained. The average thickness is 2.74 mm. The thermal conductivity coefficient, enthalpy value and density of the internal high thermal conductivity heat-absorbing material are shown in Table 2.
[0066] Performance Characterization
[0067] In order to test the thermal runaway effect of the fast-absorbing thermal runaway protective material of the present invention, a test platform was built. A heating plate with a power of 500W was clamped in the center of two soft-pack lithium iron phosphate batteries with an outer size of 227*160*7.25mm, a standard voltage of 3.3V, and a fully charged capacity of 20AH. The two batteries were connected to a signal acquisition device to collect the voltage and surface temperature of the two batteries. Then, the three thermal runaway protective materials prepared in the embodiment with a size of 230*160mm were respectively attached to the two outer surfaces of the battery, and a blank sample without thermal runaway protective material was made. Its structure is shown in Figure 2.
[0068] The test steps are as follows: Power the heating plate to the battery, set the heating plate temperature power to 100%, and collect the battery voltage and temperature. When the collected battery voltage reaches 0V, heating is stopped and the battery temperature is collected again until the battery temperature drops below 50°C, at which point data collection stops. The results are shown in Table 3.
[0069] Table 2 Performance test of the embodiment
[0070] Note: ① Thermal conductivity refers to ISO 22007-2 test
[0071] ② Differential scanning calorimetry test
[0072] ③ Density = weight / volume
[0073] Table 3 Application test of the embodiment
[0074] Note: This temperature is the highest battery temperature during the entire test.
[0075] Through testing, it can be seen that the blank sample (Comparative Example 1) without the use of thermal runaway protection material is completely thermally runaway after 360S of heating on the heating plate, and the maximum temperature of the battery reaches 262°C. The sample using aerogel (Comparative Example 2) has a faster internal temperature rise due to the heat insulation effect of aerogel, and it is completely thermally runaway in 320S, and the maximum temperature also reaches 310°C. The samples using the thermal runaway protection materials A / B / C of the present invention endured nearly twice as much heating time as the blank samples, and the maximum temperature of the battery during the entire test process was 138°C, 143°C, and 160°C, respectively, which is more than 100°C lower than the temperature of the blank sample. This fully demonstrates that the thermal runaway protection material of the present invention has a significant effect on thermal runaway control.
[0076] The above are merely specific application examples of the present invention and do not constitute any limitation on the scope of protection of the present invention. In addition to the above embodiments, the present invention may also have other implementations. Any technical solution formed by equivalent replacement or equivalent transformation falls within the scope of protection claimed by the present invention.
Claims
1. A thermal runaway protection material that absorbs heat quickly. It is characterized in that It is a laminated structure, which includes, from bottom to top, a flame retardant graphite thermal conductive film, a thermal conductive adhesive, a high thermal conductivity heat absorbing material, a thermal conductive adhesive and a flame retardant graphite thermal conductive film; wherein the high thermal conductivity heat absorbing material comprises, by mass percentage: 80-94% heat absorbing material, 1-10% thermal conductive material, 0-1% organic tin catalyst loaded with flame retardant graphite and 5-10% adhesive; the endothermic enthalpy of the endothermic material is greater than 1200 J / g, and it is a material that undergoes a chemical reaction between 60 and 400° C. and actively absorbs heat. After the chemical reaction conditions are met, the endothermic reaction will spontaneously proceed to form a continuous endothermic effect; the thermal conductive material is a carbon-based thermal conductive material.
2. A thermal runaway protection material with rapid heat absorption according to claim 1, It is characterized in that The thickness of the thermal conductive adhesive is between 0.02 mm and 0.25 mm; the thickness of the flame retardant graphite thermal conductive film is between 0.02 mm and 0.5 mm.
3. A fast heat absorbing thermal runaway protection material according to claim 1 or 2, Features The peripheral sides of the laminated structure are all sealed with edge sealing glue; the thermal runaway protection material is a block or a sheet.
4. The thermal runaway protection material having rapid heat absorption according to claim 1, Features The thickness of the high thermal conductivity heat absorbing material is between 0.5 and 100 mm.
5. The thermal runaway protection material with rapid heat absorption according to claim 1, It is characterized in that The method for preparing the high thermal conductivity heat absorbing material comprises the following steps: S1: Add adhesive, organic tin catalyst loaded with flame-retardant graphite, and carbon-based thermal conductive material into a mixing kettle, raise the temperature to 30-60° C. and stir for 2-4 hours; S2: slowly add the heat absorbing material into the above mixing kettle, stir while adding, and vacuumize to remove bubbles to obtain a mixed glue; S3: pouring the mixed glue into a mold of specified shape and thickness, curing at room temperature for 0.5 to 48 hours, and demolding to obtain the high thermal conductivity heat absorbing material; In the above steps, the raw materials of the high thermal conductivity heat-absorbing material are calculated by mass percentage as follows: 80-94% heat-absorbing material, 1-10% heat-conducting material, 0-1% organic tin catalyst loaded with flame-retardant graphite, and 5-10% adhesive.
6. A thermal runaway protection material having rapid heat absorption according to claim 1 or 5, It is characterized in that The heat absorbing material includes, but is not limited to, a mixture of one or more of sodium acetate trihydrate, ammonium ferric oxalate trihydrate, citric acid monohydrate, citric acid, oxalic acid dihydrate, anhydrous oxalic acid, barium hydroxide octahydrate, malonic acid, magnesium sulfate heptahydrate, zinc sulfate heptahydrate, succinic acid, maleic acid, fumaric acid, sodium carbonate decahydrate, calcium chloride hexahydrate, aluminum nitrate nonahydrate, boric acid, ammonium pentaborate octahydrate, ammonium ferric sulfate dodecahydrate, ferrous chloride tetrahydrate, ammonium oxalate monohydrate, sodium tetraborate decahydrate, sodium tetraborate pentahydrate, aluminum sulfate octahydrate, ammonium pentaborate, ammonium hydrogen borate tetrahydrate, sodium silicate pentahydrate, sodium aluminum silicate hydrate, potassium aluminum sulfate dodecahydrate, sodium sulfate decahydrate, copper sulfate heptahydrate, ferrous sulfate heptahydrate, cobalt chloride hexahydrate, and calcium sulfate dihydrate in any proportion; The carbon-based thermal conductive material is a mixture of one or more of carbon nanotubes, expanded graphite, flame-retardant graphite and graphene in any proportion; The organic tin catalyst loaded with flame retardant graphite comprises flame retardant graphite and dibutyltin diacetate, and the mass ratio of the two is 1:1 to 2:
1.
7. A thermal runaway protection material according to claim 1 or 5, It is characterized in that The preparation method of the organic tin catalyst loaded with flame retardant graphite is as follows: flame retardant graphite and dibutyltin diacetate are added into a reactor at a mass ratio of 1:1 to 2:1, and then cyclohexane with a total mass of 30-100% of the flame retardant graphite and dibutyltin diacetate is added, stirring is maintained at 40-60° C. for 2-3 hours, and after drying, the organic tin catalyst loaded with flame retardant graphite is obtained.
8. A thermal runaway protection material according to claim 1 or 2, It is characterized in that The flame retardant graphite thermal conductive film is a thermal conductive film made of flame retardant graphite composite plastic particles, with a thermal conductivity of >1W / mK, a flame retardant grade of UL94-V0, and a thickness of 0.02mm to 0.5mm; the thermal conductivity of the thermal conductive adhesive is >1W / mK, and a thickness of 0.02mm to 0.2mm.
9. The method for preparing the fast endothermic thermal runaway protection material according to claim 1 or 2, It is characterized in that A layer of thermal conductive adhesive is applied to the upper and lower surfaces of the high thermal conductivity heat absorbing material respectively, and then the surface of the thermal conductive adhesive is covered with a flame retardant graphite thermal conductive film, which is flattened using a mold, cured at room temperature, and cut into a specified size, and then edge sealing glue is applied to the side, and after drying, the thermal runaway protection material is obtained.
10. Achieve high thermal conductivity and modular packaging methods for heat absorbing materials, Features: The steps include: S1: Add adhesive, organic tin catalyst loaded with flame-retardant graphite, and carbon-based thermal conductive material into a mixing kettle, raise the temperature to 30-60° C. and stir for 2-4 hours; S2: slowly add the heat-absorbing material into the above-mentioned mixing kettle, stir while adding, and vacuumize to remove bubbles to obtain a mixed glue; the heat-absorbing enthalpy of the heat-absorbing material is greater than 1200 J / g, and the heat-absorbing material is a material that undergoes a chemical reaction between 60 and 400° C. and actively absorbs heat. After the chemical reaction conditions are met, the heat absorption reaction will proceed spontaneously, forming a continuous heat absorption effect; S3: pouring the mixed glue into a mold of a specified shape and thickness, curing at room temperature, and demolding to obtain the high thermal conductivity endothermic material; wherein the high thermal conductivity endothermic material comprises, by mass percentage: 80-94% endothermic material, 1-10% carbon-based thermal conductive material, 0-1% organic tin catalyst loaded with flame retardant graphite, and 5-10% adhesive; S4, brushing a layer of thermal conductive adhesive on the upper and lower surfaces of the high thermal conductivity heat absorbing material respectively, and then covering the surfaces of the upper and lower layers of thermal conductive adhesive with a flame retardant graphite thermal conductive film, and flattening them with a mold, and cutting them into a specified size after curing at room temperature, to obtain a laminated structure of flame retardant graphite thermal conductive film, thermal conductive adhesive, high thermal conductivity heat absorbing material, thermal conductive adhesive and flame retardant graphite thermal conductive film from bottom to top; S5, applying edge sealing glue on the side of the laminated structure, and after drying, obtaining a packaged thermal runaway protection material block or sheet; S6. Prepare the packaged thermal runaway protection material block or sheet into the required size and directly fit it to the heat-generating component to achieve modular packaging of the high thermal conductivity heat-absorbing material around the heat-generating component.
Citation Information
Patent Citations
Novel heat conduction material structure
CN204160826U
Semiconductor heat dissipation device
CN212138205U
Heat absorption and conduction film for solar device
CN215473585U
Novel high-efficiency graphene insulating heat-conducting film
CN217124164U
Insulating panel for construction
KR1020230062960A
Cited By
Fireproof thermal insulation material for new energy automobile battery and preparation method of fireproof thermal insulation material
CN120118519A