Transparent substrate provided with a functional stack of thin layers
The use of substoichiometric or doped tungsten oxide layers in a multi-layer silver-based stack on a glass substrate addresses the balance of solar factor and selectivity in solar control glazing, enhancing energy performance and light transmission while maintaining neutral colors.
Patent Information
- Application Number
- PCT/EP2024/061102
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-31
AI Technical Summary
Existing functional stacks for solar control glazing in residential applications fail to achieve a balance between low solar factor and high selectivity, often resulting in either low light transmission or inadequate energy performance.
A transparent glass substrate with a functional stack comprising multiple silver-based metallic layers and tungsten oxide layers, where the tungsten oxide layers are substoichiometric or doped, strategically positioned between dielectric modules to enhance selectivity and reduce solar factor, while maintaining neutral color and high light transmission.
The solution achieves a solar factor reduction of at least 2% and an increase in light transmission by 1-2% compared to conventional stacks, with selectivity values up to 2.0, while preserving neutral colors and allowing for efficient energy performance in residential applications.
Smart Images

Figure EP2024061102_31102024_PF_FP_ABST
Abstract
Description
Transparent substrate with a functional stack of thin layers
[0001] The invention relates to a transparent glass substrate provided with a functional stack of thin layers with several metallic functional layers. Technical background
[0002] Functional stacks of thin layers are commonly used to provide thermal insulation and / or solar protection functions to glazing. These glazings can be used in buildings or vehicles. Their primary benefit is that they reduce air conditioning efforts by preventing excessive overheating (so-called "solar control" glazing) and / or by reducing the amount of energy dissipated to the outside (so-called "low-emissivity" glazing).
[0003] A particularly used type of functional stack of thin layers comprises a metallic functional layer, in particular based on silver, allowing the reflection of part of the electromagnetic radiation, in particular infrared radiation.
[0004] The metallic functional layer is generally arranged between two dielectric assemblies, also called dielectric modules, in order to neutralize the optical effects of reflection and refraction in the visible range. These dielectric modules may comprise one or more thin dielectric layers of the nitride type, for example silicon or aluminum nitride, and / or of the oxide type, for example silicon, zinc, tin oxide.
[0005] Solar control features are required for glazing that is likely to be exposed to high levels of sunlight. The ability of a glazing to limit the amount of light energy transmitted is defined by the solar factor, g, which is the ratio of the total energy transmitted through the glazed surface or glazing to the interior to the incident solar energy. The lower the value of the solar factor, g, the better the protection against solar radiation.
[0006] JP H0812378 A [NISSAN MOTOR] 16.01.1996 describes a "solar control" functional stack comprising a tungsten oxide layer disposed between two dielectric layers. The stack makes it possible to reduce the surface electrical resistance and increase the transparency to radio waves compared to stacks comprising a metallic functional layer, in particular based on silver.
[0007] JP 2010180449 A [SUMITOMO METAL MINING CO [JP]] 19.08.2010 discloses a tungsten oxide-based layer deposited by sputtering using a tungsten oxide target comprising chemical elements selected from hydrogen, alkali, alkaline earth, and rare earth. The layer has a "solar control" function due to its strong absorption of near-infrared radiation.
[0008] EP 3686312 A1 [SUMITOMO METAL MINING CO [JP]] 29.07.2020 describes a layer based on cesium-doped tungsten oxide, and a method for depositing such a layer by cathode sputtering. The layer has transparency to radio waves and a "solar control" function thanks, in particular, to its strong absorption of infrared radiation.
[0009] EP 847965 A1 [SAINT-GOBAIN VITRAGE [FR]] 17.06.1998 describes an example with a layer of tungsten oxide WO3, in the third dielectric module of a two-layer silver stack and compares this example with two other examples comprising, instead of the layer of tungsten oxide WO3, a layer of zinc oxide ZnO or a layer of tin oxide SnO2. There is no doubt that these layers are all dielectric in nature due to the stable stoichiometry of the material composing them; if the atomic proportion between the elements in a layer were to be changed, this would profoundly modify the nature and the role of the layer in the optical definition of the stack and this would profoundly modify the stack.
[0010] US 4782216 [WOODARD [US]] 01.11.1988 describes two examples of two-layer silver stacks, each with a stoichiometric tungsten oxide layer, WO3, in two dielectric modules.
[0011] For certain applications, for example in the building and construction markets, it is desirable for glazing incorporating a substrate carrying a functional stack to have a low visible light transmission, TL, of the order of 50% or 60% or medium of the order of 70%, or high of the order of 75%, in order to ensure comfortable natural illumination of interior spaces.
[0012] A functional stack is considered suitable for such applications when it meets a triple requirement: adequate light transmission, a low solar factor value and a high selectivity value. A functional stack is therefore suitable when it has a high selectivity value, s, defined as the ratio of light transmission to solar factor, and a low solar factor, for a given light transmission.
[0013] State-of-the-art solutions consisting of using only infrared radiation-absorbing layers as functional layers in the functional stack are not suitable because they have too low a light transmission or too low a selectivity, incompatible for example with applications in the residential market.
[0014] There therefore remains a need for a functional stack suitable for “solar control” applications in a residential market, i.e. presenting high selectivity and suitable overall energy performance, particularly concerning the solar factor. Solution to the technical problem
[0015] According to a first aspect of the invention, a glass substrate is provided, provided with a functional stack of thin layers on at least one of its faces, said functional stack comprising, starting from the substrate, at least two metallic functional layers, preferably each based on silver, each located between two dielectric modules of thin layers and forming a succession comprising a first dielectric module, a first metallic functional layer, a second dielectric module, a second metallic functional layer and a last dielectric module, and in which at least one of the dielectric modules of thin layers comprises a layer of tungsten oxide having a physical thickness of between 5 nm and 50 nm, and: - the tungsten oxide comprising at least one doping element selected from the chemical elements of group 1 according to the IUPAC nomenclature, or - the tungsten oxide being sub-stoichiometrically pure, WOx,with x preferably between 2.55 and 2.98.,
[0016] Said stack may comprise only two metal functional layers, preferably each based on silver or may comprise only three metal functional layers, preferably each based on silver. Even if a stack configuration with several metal functional layers is more complex to design and costs more than a stack configuration with a single metal functional layer, these disadvantages are compensated by the surprising effects obtained, in particular such high selectivity and such low solar factor.
[0017] According to the configurations:- said functional stack comprises a single layer of tungsten oxide and said layer of tungsten oxide is preferably located in said first dielectric module or in said last dielectric module; or- said functional stack comprises two layers of tungsten oxide and said layers of tungsten oxide are preferably located for one in said first dielectric module and for the other in said last dielectric module; or- said functional stack comprises as many layers of tungsten oxide as there are dielectric modules and each dielectric module comprises a layer of tungsten oxide.
[0018] Preferably, the tungsten oxide layer(s) is (or are not) in contact with a metallic functional layer (i.e. there is interposition of at least one layer made of a material different from the other two); this makes it possible to achieve an optical separation between the functions of, on the one hand, the metallic functional layer, which reflects infrared rays, and, on the other hand, the tungsten oxide layer.
[0019] The optical refractive index of the tungsten oxide layer(s) preferably decreases monotonically with wavelength from a maximum value greater than 2.4 at 350 nm to a minimum value between 600 nm and 900 nm such that the difference between the maximum value and the minimum value is greater than 0.8, preferably greater than 1.0, or even greater than 1.4.
[0020] The optical extinction coefficient of the tungsten oxide layer(s) is preferably less than 0.2 at 500 nm and less than 2.0 at 1200 nm.
[0021] The (at least one, or all) tungsten oxide layer(s) of the stack may (or may) not include a dopant.
[0022] The tungsten oxide layer(s) may be pure substoichiometric tungsten oxide, WOx, with x preferably between 2.55 and 2.98, or even between 2.55 and 2.95 or 2.6 and 2.95.
[0023] If several layers of tungsten oxide 120a, 160a, 200a are present in the stack, they may be of the same composition or of different compositions:- one layer may comprise at least one dopant selected from the chemical elements of group 1 according to the IUPAC nomenclature and another layer may be made of pure sub-stoichiometric tungsten oxide, WOx, with x preferably between 2.55 and 2.98; or- several layers may comprise at least one dopant selected from the chemical elements of group 1, the dopants not being identical; or- several layers may be made of pure sub-stoichiometric tungsten oxide, WOx, with different values of x, preferably between 2.55 and 2.98.
[0024] The tungsten oxide layer(s) may comprise a doping element, or several doping elements, preferably in a proportion such that the molar ratio of said element to tungsten, or the sum of the molar ratios of each element to tungsten, is between 0.01 and 0.4, preferably between 0.01 and 0.2, or even between 0.01 and 0.1.
[0025] The tungsten oxide layer(s) preferably comprises at least one doping element selected from hydrogen, lithium, sodium, potassium and cesium.
[0026] The tungsten oxide layer(s) preferably comprises cesium as a doping element, and the molar ratio of cesium to tungsten is between 0.01 and 0.2, preferably between 0.01 and 0.1. Preferably, cesium is then the sole doping element.
[0027] The physical thickness of the tungsten oxide layer(s) is (or are), preferably, between 5 nm and 30 nm, preferably between 5 nm and 20 nm or between 9 nm and 25 nm, or even between 12 nm and 20 nm.
[0028] Said functional stack of layers preferably further comprises at least one blocking overlayer, preferably based on a nickel and chromium alloy, located above and in contact with a metallic functional layer and / or at least one metallic blocking underlayer, preferably based on a nickel and chromium alloy, located below and in contact with a metallic functional layer.
[0029] The functional stack of layers preferably further comprises an oxide-based contact layer, made of titanium oxide, located above and in contact with the metal functional layer furthest from the substrate, said oxide-based contact layer preferably having a physical thickness of at least 5.0 nm, in particular between 5.0 and 35.0 nm.
[0030] The functional stack of layers preferably comprises a layer with a refractive index greater than 2.15 at 550 nm, said layer being included in the last dielectric module.
[0031] According to a second aspect of the invention, there is provided a glazing comprising a transparent substrate according to the first aspect of the invention.
[0032] According to a third aspect of the invention, there is provided a method for manufacturing a transparent substrate according to the first aspect of the invention. Advantages of the invention
[0033] A first advantage of the invention is that it provides a suitable "solar control" functional stack, particularly for applications in the building and construction markets. The functional stack satisfies the triple requirement of adequate light transmission, a low solar factor value, and high selectivity.
[0034] By way of examples, a transparent substrate provided with a functional stack in accordance with the first aspect of the invention may, compared to a conventional functional stack, have a solar factor value lower by at least 2%, or even at least 4%, and an equivalent light transmission, or even higher by at least 1%, or even at least 2%.
[0035] It is possible to achieve a selectivity of at least 1.9, or even at least 2.0 with double glazing incorporating a stack according to the invention comprising only two metallic functional layers and at least one layer based on tungsten oxide.
[0036] A second advantage is that the tungsten oxide layer(s) do not affect, or at least very little, the color of the stack compared to a conventional functional stack. The color specifications are therefore always met when such a layer is introduced into an existing functional stack.
[0037] Another advantage of the invention is that the tungsten oxide layer(s) can be deposited by a magnetron sputtering method, in particular using a tungsten oxide target. Since functional stacks of thin layers are generally deposited by a magnetron sputtering method, existing methods can be more easily adapted.
[0038] is a schematic representation of a first embodiment of the first aspect of the invention;is a representation of the evolution of the optical extinction coefficient as a function of the wavelength W, in nanometers, of an example with a layer of cesium-doped tungsten oxide and of an example with a layer of sub-stoichiometric and pure tungsten oxide;is a representation of the evolution of the optical refractive index as a function of the wavelength W, in nanometers, of an example with a layer of cesium-doped tungsten oxide and of an example with a layer of sub-stoichiometric and pure tungsten oxide;is a schematic representation of a first embodiment of a glazing according to the second aspect of the invention;is a schematic representation of a second embodiment of a glazing according to the second aspect of the invention;is a graphical representation of selectivity versus light transmission for a CE counterexample, an E1 example, and an E2 example;is a graphical representation of selectivity versus light transmission for the CE counterexample, an E13' example, an E13''' example, and the E1 example;is a graphical representation of selectivity versus light transmission for the CE counterexample, the E13' example, an E15' example, an E16' example, and the E1 example; andis a graphical representation of selectivity versus light transmission for the CE counterexample, an E24' example, an E25' example, an E26' example, and the E2 example.; Detailed description of embodiments
[0039] It uses the following definitions and conventions.
[0040] The term "above" or "below" respectively, qualifying the position of a layer or set of layers and defined relative to the position of another layer or set, means that said layer or set of layers is closer to, or further away from, the substrate. These two terms, "above" and "below", do not mean that the layer or set of layers that they qualify and the other layer or set in relation to which they are defined are in contact. They do not exclude the presence of other intermediate layers between these two layers. The expression "in contact" is explicitly used to indicate that no other layer is arranged between them.
[0041] Without any precision or qualification, the term "thickness" used for a layer corresponds to the physical, real or geometric thickness of said layer. It is expressed in nanometers.
[0042] The expression "dielectric module" designates one or more layers in contact with each other forming a set of globally dielectric layers, that is to say that it does not have the functions of a metallic functional layer. If the dielectric module comprises several layers, these may themselves be dielectric. The physical, real or geometric thickness of a dielectric module of layers corresponds to the sum of the physical, real or geometric thicknesses of each of the layers that constitute it.
[0043] In the present description, the expressions "a layer of" or "a layer based on", used to qualify a material or a layer as to what it contains, are used equivalently. They mean that the mass fraction of the constituent that it comprises is at least 50%, in particular at least 70%, preferably at least 90%. In particular, the presence of minority or doping elements is not excluded.
[0044] By the term "transparent", used to describe a substrate, means that the substrate is preferably colorless, non-opaque and non-translucent in order to minimize light absorption and thus maintain maximum light transmission in the visible electromagnetic spectrum.
[0045] The luminous transmission, TL, in the visible spectrum, the solar factor, g, and the selectivity, s, the internal reflection, Rint, and the external reflection, Rext, in the visible spectrum, as well as their methods of measurement and / or calculation are defined in the standards EN 410, ISO 9050 and ISO 10292.
[0046] According to the IUPAC nomenclature, Group 1 of the chemical elements includes hydrogen and the alkali elements, i.e., lithium, sodium, potassium, rubidium, cesium, and francium.
[0047] The expressions "optical refractive index" and "optical extinction coefficient" mean the optical refractive index, n, and the optical extinction coefficient, k, as defined in the technical field, in particular according to the Forouhi & Bloomer model described in the work Forouhi & Bloomer, Handbook of Optical Constants of Solids II, Palik, ED (ed.), Academic Press, 1991, Chapter 7.
[0048] According to a first aspect of the invention, with reference to the, there is provided a transparent glass substrate 10, provided with a functional stack 14 of thin layers on at least one of its faces 11, said functional stack 14 comprising, starting from the substrate 10: at least two metallic functional layers 140, 180 each placed between two dielectric modules 120, 160, 200 of thin layers, and in which at least one of the dielectric modules 120, 160, 200 of thin layers comprises a layer of tungsten oxide 120a, 160a, 200a, and: - either the tungsten oxide comprises at least one doping element selected from the chemical elements of group 1 according to the IUPAC nomenclature; - or the tungsten oxide of the layer(s) of tungsten oxide 120a, 160a, 200a is a pure substoichiometric tungsten oxide, WO x, with x preferably between 2.55 and 2.98, or even between 2.55 and 2.95 or between 2.6 and 2.95; A value of x between 2.99 and 3.02 will be considered as generating a pure stoichiometric tungsten oxide, WO3.
[0049] This layer of tungsten oxide 120a, 160a, 200a (and preferably each layer of tungsten oxide 120a, 160a, 200a) has a physical thickness of between 5 nm and 50 nm: below 5 nm, the effect of such a layer on the optical definition of the stack is not sufficiently notable; it may be difficult, industrially, to deposit more than 50 nm of pure doped or sub-stoichiometric tungsten oxide.
[0050] Surprisingly, a tungsten oxide layer of pure substoichiometric tungsten oxide, WO x, with a thickness between 5 and 50 nm, presents unexpected optical characteristics, particularly in terms of the evolution of the optical extinction coefficient and refractive index as a function of the wavelength of the electromagnetic radiation. These characteristics, combined with the presence of several metallic functional layers, have a synergistic effect on increasing selectivity.
[0051] Surprisingly, a tungsten oxide layer comprising a doping element selected from the group 1 elements according to the IUPAC nomenclature and with a thickness between 5 and 50 nm exhibits unexpected optical characteristics, particularly in terms of the evolution of the optical extinction coefficient and refractive index as a function of the wavelength of the electromagnetic radiation. These characteristics, combined with the presence of several metallic functional layers, have a synergistic effect on increasing selectivity.
[0052] As illustrative and explanatory examples, to which however the present invention should not be considered as inextricably linked, the evolutions of the optical extinction coefficient, k, and of the optical refractive index, n, are represented on theandrespectively, on the one hand for a layer C1 of cesium-doped tungsten oxide and on the other hand for a layer C2 of pure sub-stoichiometric tungsten oxide, WO x , these layers being deposited by cathodic sputtering on a soda-lime-silica glass substrate according to two different deposition conditions.
[0053] On this set, the C1 and C2 layers were deposited on a soda-lime-silica glass substrate on which a first silicon nitride-based layer with a thickness of approximately 5 nm was previously deposited. They were then covered with a second silicon nitride-based layer with a thickness of approximately 5 nm. In other words, each C1 and C2 layer is encapsulated between two silicon nitride-based layers.
[0054] The encapsulation of layers C1 and C2 by two silicon nitride-based layers serves to prevent the degradation of layers C1 and C2 from excessive oxidation and / or excessive diffusion of oxygen into their structure. Instead of silicon nitride, it is possible to use any other suitable type of nitride such as, for example, zirconium nitride.
[0055] The C1 layer was deposited in an atmosphere comprising 20% oxygen at a pressure of 4 mTorr. The resulting stack comprising the C1 layer was annealed at 650°C for 10 min after deposition. The molar ratio of cesium to tungsten is approximately 0.05-0.06.
[0056] The C2 layer was deposited from a tungsten metal target, under an atmosphere comprising 60% dioxygen and at a pressure of 12 mTorr. The resulting stack comprising the C2 layer was annealed at 650°C for 10 min after deposition. The C2 layer is thus a layer of pure substoichiometric tungsten oxide, WO x , with an x of about 2.9.
[0057] The extinction coefficient and refractive index were calculated by modeling from experimental measurements. The measurements were obtained using a Perkin Elmer Lambda 900 spectrophotometer and a VASE M-2000XI JA Wollam ellisopmeter.
[0058] With reference to the, regardless of the C1 or C2 layer, the extinction coefficient decreases monotonically from a value less than 1 at 300 nm to reach a minimum level less than 0.1 for C1 and less than 0.05 for C2 between about 400 nm and 550 nm, then increases monotonically to reach a value greater than 1.2 around 1200 nm for C1 and a value greater than 0.5 around 1200 nm for C2. The C1 and C2 layers have strong absorption in the near infrared and some transparency in the visible region of the electromagnetic spectrum. The C2 layer has absorption in the visible light spectrum and in the near infrared which are lower than those of the C1 layer.
[0059] With reference to the, for the C1 layer, the optical refractive index decreases monotonically from a value close to 3 at 300 nm to reach a minimum level of less than 1.8, or even 1.6 between approximately 800 nm and 1100 nm, then increases monotonically to reach a value greater than 1.8, or even 2 around 1300-1400 nm. For the C2 layer, the optical refractive index decreases monotonically from a value close to 3 at 300 nm to reach a small level at a value close to 1.6 between approximately 900 nm and 1100 nm, then decreases monotonically again to reach a value of approximately 1.45 around 1300 nm.
[0060] According to other preferred embodiments, the optical refractive index of the tungsten oxide layer 120a, 160a, 200a decreases monotonically with wavelength from a maximum value greater than 2.4 at 350 nm to a minimum value between 600 nm and 900 nm such that the difference between the maximum value and the minimum value is greater than 0.8, preferably 1.0, or even 1.4.
[0061] In other words, the value of the optical refractive index decreases monotonically by at least 0.8, preferably by at least 1.0, or even at least 1.4 between a maximum value greater than 2.4 at 350 nm and a minimum value between 600 nm and 900 nm. For example, the optical refractive index value may decrease monotonically by at least 0.8, preferably by at least 1.0, or even at least 1.4 between a maximum value greater than 2.4 at 350 nm and a minimum value less than 2.3 between 600 nm and 900 nm, in particular between 800 nm and 900 nm.
[0062] Although not particularly required to achieve the effects of the present invention, these optical refractive index values may nevertheless be advantageous in meeting color specifications for applications in the building and construction markets. In particular, they allow neutral colors to be obtained.
[0063] According to certain additional preferred embodiments, the optical extinction coefficient of the tungsten oxide layer 120a, 160a, 200a may be less than 0.2, or even 0.1 at 500 nm and less than 2, or even 1.5 at 1200 nm. The selectivity can thus be favorably further increased.
[0064] The optical extinction coefficient and the optical diffraction index may vary if one or more doping elements are included in the tungsten oxide layer and according to the nature and quantity of the doping element(s) selected from the elements of group 1 according to the IUPAC nomenclature. In particular, they may exhibit behaviors different from those described previously in the context of the illustrative and explanatory examples of set. However, it is currently difficult to establish a general behavior law for the optical extinction coefficient and the refractive index according to the nature and / or quantity of the doping element(s).
[0065] According to certain particular embodiments, the tungsten oxide layer does not comprise any doping element and is made of pure substoichiometric tungsten oxide, WOx, with x preferably between 2.55 and 2.98 or between 2.55 and 2.95 or between 2.6 and 2.95.
[0066] According to certain particular embodiments, the tungsten oxide layer comprises the doping element X or the doping elements X1, X2,… in a proportion such that the molar ratio, X / W of said element on the tungsten, W, or the sum of the molar ratios of each element on the tungsten (X1+X2+…) / W is between 0.01 and 0.4, preferably between 0.01 and 0.2, or even between 0.01 and 0.1. It has been found that these molar ratio values can advantageously make it possible to obtain the optical extinction coefficient and refractive index values described in the preceding embodiments while limiting the quantity of doping elements. In addition, a saving on the exploitation of mineral resources for the doping elements can possibly result, as well as a reduction in costs.
[0067] In some embodiments, the tungsten oxide layer comprises at least one doping element selected from hydrogen, lithium, sodium, potassium and cesium. Among the group 1 elements, these particular elements can provide the most optimal optical extinction coefficient and refractive index values for the desired technical effects.
[0068] In particularly preferred embodiments, the tungsten oxide layer comprises cesium as a doping element, and the molar ratio of cesium to tungsten is between 0.01 and 0.2, preferably between 0.01 and 0.1. These embodiments provide the best performance in terms of increased selectivity, preservation of neutral colors, and cost savings.
[0069] What is most important in the context of the invention is that the absorption in the visible range of the material of the tungsten oxide layer(s) is as low as possible in the visible range (wavelength of 380 to 780 nm) in order to maximize the gain in selectivity.
[0070] The transparent substrate 10 may preferably be flat and may be of an organic or inorganic nature, rigid or flexible. In particular, it may be a mineral glass, for example a soda-lime-silica glass.
[0071] Examples of organic substrates that can be advantageously used for implementing the invention may be polymeric materials such as polyethylenes, polyesters, polyacrylates, polycarbonates, polyurethanes, polyamides. These polymers may be fluorinated polymers.
[0072] Examples of mineral substrates that can be advantageously used in the invention may be mineral or glass-ceramic glass sheets. The glass may preferably be a soda-lime-silica, borosilicate, aluminosilicate or alumino-borosilicate type glass. According to a preferred embodiment of the invention, the substrate 10 is a soda-lime-silica mineral glass sheet.
[0073] The presence of the tungsten oxide layer 120a, 160a, 200a in each dielectric module 120, 160, 200 allows for the greatest reductions in solar factor and the greatest increases in light transmission.
[0074] According to certain advantageous embodiments, the physical thickness of the tungsten oxide layer(s) 120a, 160a, 200a may be between 2 nm and 50 nm, in particular between 5 nm and 30 nm, preferably between 5 nm and 20 nm. These thickness ranges are sufficient to obtain the remarkable advantages of the first aspect of the invention.
[0075] Illustrates a structure of a stack 14 with several functional layers according to the invention deposited on a face 11 of a transparent glass substrate 10. This diagram illustrates the positions of different layers relative to each other when these layers are present.
[0076] In this structure, the functional layers 140, 180 are in particular based on silver or a metal alloy containing silver, and are each arranged between two anti-reflection modules: the underlying anti-reflection module 120 located below the first functional layer 140 in the direction of the substrate 10 and the intermediate anti-reflection module 160 arranged above the first functional layer 140 opposite the substrate 10 and under the second functional layer 180. An overlying anti-reflection module 200 is arranged above the second functional layer 180 opposite the substrate 10.
[0077] These anti-reflective modules 120, 160, 200 each comprise at least one dielectric layer 124, 126, 129; 162, 164, 166, 168, 169; 202, 203, 204, 206.
[0078] A terminal protective layer 300, furthest from face 11, can complete the stack.
[0079] For the illustrated two-functional layer stack structure, the first functional layer 140 is located indirectly on the underlying anti-reflective module 120 and indirectly under the intermediate anti-reflective module 160: there is an under-blocking layer 130 located between the underlying anti-reflective module 120 and the first functional layer 140 and an over-blocking layer 150 located between the first functional layer 140 and the intermediate anti-reflective module 160.
[0080] For the illustrated two-functional layer stack structure, the second functional layer 180 is located indirectly on the underlying intermediate anti-reflective module 160 and indirectly under the anti-reflective module 200: there is an under-blocking layer 170 located between the underlying anti-reflective module 160 and the second functional layer 180 and an over-blocking layer 190 located between the second functional layer 180 and the anti-reflective module 200.
[0081] Each metal functional layer 140, 180 has the function of reflecting infrared radiation and / or a portion of solar radiation. It may be of any suitable metal, for example gold-based or silver-based. The thickness of each metal functional layer 140, 180 may typically be between 2 nm and 25 nm, preferably between 10 nm and 20 nm.
[0082] According to preferred embodiments, each metal functional layer 140, 180 is a silver-based layer.
[0083] The dielectric modules may comprise one or more layers of oxides and / or nitrides of metallic elements and / or metallic alloys, such as, for example, zinc oxide, mixed zinc and tin oxide, silicon nitride, silicon oxide, zirconium nitride, titanium oxide, tin oxide, and silicon oxynitride.
[0084] The methods for depositing thin layers on substrates, in particular glass substrates, are well-known methods in the industry. For example, the deposition of a stack of thin layers on a glass substrate is carried out by successively depositing each thin layer of said stack by passing the glass substrate through a succession of deposition cells adapted to deposit a given thin layer.
[0085] Deposition cells can use deposition methods such as magnetic field-assisted sputtering (also called magnetron sputtering), ion beam-assisted deposition (IBAD), evaporation, chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), low-pressure chemical vapor deposition (LPCVD), etc.
[0086] The magnetic field-assisted sputtering deposition process is particularly used. The conditions for deposition of layers are widely documented in the literature, for example in patent applications WO2012 / 093238 A1 and WO2017 / 00602 A1.
[0087] A second aspect of the invention relates to glazing, in particular single, double or triple glazing, comprising a transparent substrate according to any of the embodiments described.
[0088] A monolithic glazing unit comprises a single substrate, in particular a sheet of mineral glass. It may be a single glazing unit. When the substrate according to the invention is used as a monolithic glazing unit, the functional stack of thin layers is preferably deposited on the face of the substrate facing the interior of the room of the building on the walls of which the glazing unit is installed. In such a configuration, it may be advantageous to protect the first layer and possibly the stack of thin layers against physical or chemical damage using a suitable means.
[0089] A multiple glazing unit comprises at least two substrates, in particular mineral glass sheets, parallel and separated by a layer of insulating gas. Most multiple glazing units are double or triple glazing units, i.e. they comprise two or three panes respectively. When the substrate according to the invention is used as an element of a multiple glazing unit, the functional stack of thin layers is preferably deposited on the face of the glass sheet facing inwards in contact with the insulating gas. This arrangement has the advantage of protecting the stack from chemical or physical damage from the external environment.
[0090] Such a stack of thin layers 14 can be used in a laminated window providing a separation between an exterior space and an interior space. This laminated window consists of two glass substrates, which are held together by an interlayer sheet of plastic material.
[0091] Such a stack of thin layers 14 can also be used in a multiple glazing unit 100 providing a separation between an exterior space ES and an interior space IS; this glazing unit can have a double glazing structure, as illustrated in ou: this glazing unit is then made up of two glass substrates 10, 30, which are held together by a frame structure 90 and which are separated from each other by an interposed gas layer 15.
[0092] In this case, the incident direction of sunlight entering the building is illustrated by the double arrow, top or left.
[0093] According to a first embodiment, illustrated in, the stack 14 of thin layers is positioned on face 2 (on the outermost sheet of the building considering the incident direction of the sunlight entering the building and on its face facing the gas blade), that is to say on an inner face 11 of the substrate 10 in contact with the interposed gas blade 15, the other face 9 of the substrate 10 being in contact with the outer space ES. The substrate 30, not carrying a stack in, has a face 29 in contact with the interposed gas blade 15, the other face 31 of the substrate 30 being in contact with the inner space IS; this substrate 30 may comprise a stack of thin layers on one of its faces or both of its faces.
[0094] According to a second embodiment, illustrated in, the stack 14 of thin layers is positioned on face 3 (on the innermost sheet of the building considering the incident direction of the sunlight entering the building and on its face facing the gas blade), that is to say on an inner face 11 of the substrate 10 in contact with the interposed gas blade 15, the other face 9 of the substrate 10 being in contact with the inner space IS. The substrate 30, not carrying a stack, has a face 29 in contact with the interposed gas blade 15, the other face 31 of the substrate 30 being in contact with the outer space ES.
[0095] However, it can also be considered that in this double glazing structure, one of the substrates has a laminated structure.
[0096] According to a third aspect of the invention, there is provided a method of manufacturing a transparent substrate according to the first aspect of the invention, such that the tungsten oxide layer is deposited by a magnetron sputtering method using a tungsten or tungsten oxide target, the material constituting said target being optionally doped using a chemical element chosen from the chemical elements of group 1 according to the IUPAC nomenclature.
[0097] When a pure tungsten metal target or a pure tungsten oxide target is used, it can allow the deposition of a pure substoichiometric tungsten oxide layer, WO x , with x preferably between 2.55 and 2.98, or even between 2.55 and 2.95 or between 2.6 and 2.95.
[0098] An advantage of using a ceramic target (i.e., with oxygen) over a metal target, especially for rotating targets, is that the ceramic target is lighter; thus, it is easier to control the process using this ceramic target.
[0099] When a ceramic or metallic target is used, it may in particular contain one or more doping elements in a proportion as described for the doped tungsten oxide layer in certain embodiments of the first aspect of the invention.
[0100] The tungsten layer(s) may be deposited by sputtering using the aforementioned target under an atmosphere comprising 0% to 50%, preferably 5% to 25% of dioxygen under a pressure of between 1 and 15 mTorr, preferably 3 to 10 mTorr. Preferably, the deposition is carried out cold, i.e. at a temperature below 100°C, in particular between 20°C and 60°C, for the substrate.
[0101] All the embodiments described, whether they relate to the first or second aspect of the invention, can be combined with each other without any particular modification or adaptation. In the event that technical incompatibilities appear during the implementation of one of these combinations, it is within the reach of those skilled in the art to be able to resolve them using their knowledge without this requiring undue effort, in particular by implementing a research program. Examples
[0102] The characteristics and advantages of the invention are illustrated by the examples and counter-examples described below.
[0103] In the following examples, the functional metal layers 140, 180 are silver (Ag) layers. The blocking layers 130, 150, 170, 190 are nickel and chromium alloy (NiCr) metal layers. The dielectric modules 120, 160, 200 comprise barrier layers, smoothing layers or wetting layers. The barrier layers are based on silicon nitride, doped with aluminum (Si3N4:Al), based on silicon nitride and zirconium. The smoothing layers are based on mixed oxide of zinc and tin (SnZnOx). The wetting layers are made of zinc oxide (ZnO).
[0104] NameContentStoichiometryIndex(at 550 nm)CWOCaesium-doped tungsten oxideCs / W = 0.052.20 for C1WOxSubstoichiometric tungsten oxideWO 2,92.45 for C2WO3Stoichiometric tungsten oxideWO32.75SiNAluminum-doped silicon nitrideSi3N4:Al2.07SiZrN17Silicon zirconium nitrideSi x’ Zr y’ N z’ withy / (y + x) = 0.172.20ZnOOzinc oxideZnO2.00SnZnOOzinc tin oxideSn e Zn f O2.00TiOxTitanium oxide-TiO2or close2.20NiCrNickel-Chromium alloyNi 0,8 Cr 0,2 -AgAg-
[0105] The deposition conditions of the layers, which were deposited by sputtering (so-called “magnetron cathode sputtering”), are summarized in Table 2.
[0106] Target layer used Deposition pressure Gas SiNSi:Al at 92:8 wt% 3.2-6.10 -3 mbarAr / (Ar + N2) at 55%SiZrN17Si:Zr:Al at 78:17:5% at.2.10 -3 mbarAr / (Ar + N2) at 45%ZnOZn:Al at 98:2% by weight1.8.10 -3 mbarAr / (Ar + O2) at 63%SnZnOZn:Sn at 64:36% at.2.10 -3 mbarAr / (Ar + O2) at 50%WO3W2.10 -3 mbarAr / (Ar + O2) at 20%TiOxTiO22.10 -3mbarAr / (Ar + O2) at 95%NiCrNi:Cr at 80:20% at.2-3.10 -3 mbarAr at 100%AgAg8.10 -3 mbarAr at 100%
[0107] at. = atomic
[0108] In the following odd-numbered example composition presentation tables, the first two columns indicate the layer or module number, with reference to the, and the third column indicates the material for these layers. For these examples, the tables detail the complete contents of the stacks starting from surface 11 of substrate 10, with a thickness of 6 mm, in the order indicated (the materials and physical thicknesses are in nanometers and the substrate carrying the stack, made of clear glass, is in the last line, at the bottom of the tables). In the following, the samples whose names begin with "CE" correspond to counter-examples; E1, E2, E13', E13''', E24', E24'', E'15, E16', E25', E26' each correspond to a series of examples.In each series of examples or counter-examples, when the name ends with "a", the aim is to obtain a light transmission in double glazing of around 50%; when the name ends with "b", the aim is to obtain a light transmission in double glazing of around 60%; when the name ends with "c", the aim is to obtain a light transmission in double glazing of around 70%; when the name ends with "d", the aim is to obtain a light transmission in double glazing of around 75%. In each series of examples, when the name includes a "1" this means that the C1 layer was used and when the name includes a "2" this means that the C2 layer was used.
[0109] To achieve the low light transmission in double glazing of 50%, or sometimes even to achieve the low light transmission in double glazing of 60%, a metallic absorbent layer 125 is provided in the first dielectric module, between two nitride-based dielectric layers, as taught by international patent application No. WO 02 / 48065.
[0110] In a first series of examples E1a, E1b and E1c, the presence of the tungsten oxide layer C1 is tested in the first dielectric module 120 and the third dielectric module 200.
[0111] Counterexamples CEa, CEb, CEc do not have any tungsten oxide or tungsten oxide based layer. Counterexamples CE'c and CE''c both have a dielectric layer 205 of stoichiometric tungsten oxide, WO3, in the third dielectric module 200.Tab. 3 CEaE1aCEbE1bCEcE1cCE'cCE''c300TiOx 11111111206SiN 335341734323235200200aCWO-27-12-5--205WO3------25202ZnO 5555555-190NiCr0,70,70,70,70,70,70,70,7180Ag15,715,615,316,515,116,015,215,2170NiCr0,20,2------169ZnO55555555140168SnZnO 1010101010101010164SiN6575677366716666162ZnO 55555555150NiCr0,70,70,70,70,70,70,70,7140Ag13,816,112,915,812,514,312,312,5130NiCr112,80,51.0-1.01,1129ZnO 55555555120aCWO-17-21-15--120126SiN 186------125NiCr2,20.5------124SiN 55325265242810glass
[0112] In the tables presenting the properties of the examples and counter-examples below, bearing even numbers, the solar factor, g, the selectivity, s, the light transmission, TL, the light reflection on the inner face, Rint, and on the outer face, Rext, as well as the color in transmission, in reflection on the inner face and in reflection on the outer face, were measured for each substrate of the examples and counter-examples assembled in a double glazing, as illustrated in the. The second glass substrate 30 is a soda-calcium silico mineral glass with a thickness of 4 mm. The thickness of the interlayer blade 15 composed of air with 90% argon is 16 mm. The stack 14 is arranged on face 2, i.e. on face 11 of the substrate 10.
[0113] The term "color", used to describe a transparent substrate with a stack, means the color as defined in the CIE 1976 L*a*b* color space according to ISO 11664, in particular with a D65 illuminant and a visual field of 2° or 10° for the reference observer. It is measured in accordance with said standard. The measurements of the color parameters a* and b*, in transmission (a*T, b*T), in external reflection (a*Rext, b*Rext) and in internal reflection (a*Rint, b*Rint) are grouped together.
[0114] The luminous transmission in the visible spectrum, TL, the solar factor, g, and the selectivity, s, and the internal reflection, Rint, and the external reflection, Rext, in the visible spectrum are defined, measured and calculated in accordance with the standards EN 410, ISO 9050 and / or ISO 10292.
[0115] Tab. 4 CEaE1aCEbE1bCEcE1cCE'cCE''cTL49,049,059,059,469,069,069,969,0g26,023,631,629,037,735,937,837,7s1,8812,0731 ,8662,0471,8281,9241,8261,829a*T-6,9-8,8-5,8-7,2-4,1-5,4-4,1-4,2b*T-2,20,0-2,4-1,5-0,3-1,2-0,3-0,9Rext18,01 7,416,716,515,014,515,015,0a*Rext-1,1-1,0-1,0-2,1-1,0-1,0-1,3-1,5b*Rext-4,2-10,0-6,5-7,7-7,8-5,8-8,1-6,6Ri nt20,621,716,418,414,415,214,314,4a*Rint-0,4-6,00,0-6,1-0,9-2,1-1,00,0b*Rint-5,0-4,8-5,0-5,0-5,0-5,0-5,04,8
[0116] Tab. 4 shows that the three examples E1a, E1b and E1c according to the invention have a light transmission TL similar to that of, respectively, the counterexamples CEa, CEb and CEc and a solar factor, g, better (lower) than those of the counterexamples CEa, CEb and CEc. The counterexamples CE'c and CE''c have a light transmission TL similar to that of example E1c and counterexample CEc and a solar factor, g, similar to that of counterexample CEc and worse (higher) than that of example E1c.
[0117] Tab. 4 shows that the three examples E1a, E1b and E1c according to the invention allow a gain (increase) in selectivity, s, compared, respectively, to the counter-examples CEa, CEb, CEc, CE'c and CE''c. This gain illustrates the synergistic effect of the combination of the tungsten oxide-based layer C1 with the first and third dielectric modules. A dielectric layer 205 of stoichiometric tungsten oxide, WO3, in the third dielectric module 200 does not allow an increase in selectivity.
[0118] External and internal reflections are also low; they are less than 22%.
[0119] In a second series of examples E2a, E2b, E2c and E2d of substrate according to the first aspect of the invention the presence of the tungsten oxide layer C2 is tested in the first dielectric module 120 and in the third dielectric module 200. These examples are compared respectively to the same counter-examples CEa, CEb and CEc as previously and a counter-example CEd is added.
[0120] Tab. 5 CEaE2aCEbE2bCEcE2cCEdE2d300TiOx 11111111206SiN 3353453453520200200aWO x -18-16-21-9202ZnO 55555555190NiCr0,70,70,70,70,70,70,70,7180Ag15,719,915,322,21 5,116,714,919,0170NiCr0.20.2-0.2----169ZnO55555555140168SnZnO 1010101010101010164SiN6568677266726775162ZnO 55555555150NiCr0,70,70,70,70,70,70,70,7140Ag13,815,512,913,512,514,512,511,7130NiCr112,80,21,00.6--129ZnO 55555555120aWO x -24-25-1723120126SiN 1814-10----125NiCr2,22.9-1.4----124SiN 5532526520610glass 6 mm6 mm6 mm6 mm6 mm6 mm6 mm6 mm
[0121] Table 6 presents properties of these examples and counterexamples.
[0122] Tab. 6 CEaE2aCEbE2bCEcE2cCEdE2dTL49,049,059,059,069,069,074,074,0g26,023,231,627,537,734,440,838,1s1,8812,1131, 8662,1461,8282,0061,8131,944a*T-6,9-9,0-5,8-6,6-4,1-4,9-3,1-4,0b*T-2,2-3,3-2,40,5-0,3-1,01,91,0Rext18,08, 716,713,415,015,015,414,1a*Rext-1,1-2,9-1,0-1,8-1,0-1,0-0,9-3,0b*Rext-4,20,0-6,50,1-7,8-4,2-9,5-5,9Rint2 0,615,916,418,014,415,415,114.8a*Rint-0.4-1.00,00.0-0.9-3.8-2.7-0.1b*Rint-5.0-5.0-5.0-5.5-5.0-1.3-7.0-4.4
[0123] Tab. 6 shows that the four examples E2a, E2b, E2c and E2d according to the invention have a light transmission TL similar to that of the counter-examples CEa, CEb, CEc and CEd respectively and a solar factor, g, better (lower) than those of the counter-examples CEa, CEb, CEc and CEd.
[0124] Tab. 6 shows that the four examples E2a, E2b, E2c and E2d according to the invention allow a gain (increase) in selectivity, s, compared, respectively, to the counter-examples CEa, CEb, CEc and CEd. This gain illustrates the synergistic effect of the combination of the tungsten oxide-based C2 layer with the first and third dielectric modules.
[0125] External and internal reflections are also low; they are less than 20%.
[0126] The selectivities of examples E1a, E1b and E1c according to the invention, of examples E2a, E2b, E2c and E2d according to the invention and of counterexamples CEa, CEb, CEc and CEd are summarized and show that the selectivity of the examples is always higher than that of the counterexamples for a similar light transmission.
[0127] In a third series of examples E13'a, E13'''a, E13'b, E13'''b, E13'c, and E13'''c of substrate according to the first aspect of the invention the presence of the tungsten oxide layer C1 is tested in the first dielectric module 120 only for the examples having "'" in their name and in the third dielectric module 200 only for the examples having a "'''" in their name. These examples are compared respectively to the same counter-examples CEa, CEb and CEc as previously (for the properties only).
[0128] Tab. 7 E13'aE13'''aE13'bE13'''bE13'cE13'''c300TiOx 111111206SiN 34193473517200200aCWO-14-2016202ZnO 555555190NiCr0,70,70,70,70,70,7180Ag16,216,416,413,816,014,5170NiCr0,20,20,20,2--169ZnO555555140168SnZnO 101010101010164SiN676571717170162ZnO 555555150NiCr0,70,70,70,70,70,7140Ag14,812,915,314,614,613,5130NiCr--0,90,900129ZnO 555555120aCWO9-22-16-120126SiN 931----125NiCr1,82,4----124SiN 55531102510glass 6 mm6 mm6 mm6 mm6 mm6 mm
[0129] Table 8 presents properties of these examples and compares them to the preceding counterexamples.
[0130] Tab. 8 CEaE13'aE13'''aCEbE13'bE13'''bCEcE13'cE13'''cTL49,049,449,159 ,060,060,069,069,069,0g26,025,925,231,630,530,837,735,936,6s1 ,8811,9081,9501,8661,9681,9501,8281,9211,886a*T-6.9-7.5-9.0-5 .8-6.7-6.3-4.1-5.2-4.8b*T-2.2-3.1-3.0-2.4-3.0-1.5-0.3-1.3-0.5R ext18,018,010,616,716,516,815,015,014,6a*Rext-1,1-1,0-3,0-1,0 -1.0-0.3-1.0-1.1-1.0b*Rext-4.20.0-7.6-6.5-1.1-11.5-7.8-4.2-10, 0Rint20,620,516,016,418,119,014,415,716,3a*Rint-0.4-0.7-6.00, 0-1.5-7.5-0.9-1.6-5.2b*Rint-5.0-5.1-5.0-5.0-6.20.8-5.0-5.0-0.2
[0131] Tab. 8 shows that the six examples E13'a, E13'''a, E13'b, E13'''b, E13'c, and E13'''c according to the invention have a light transmission TL similar to that of the counterexamples CEa, CEb and CEc respectively and a solar factor, g, better (lower) than those of the counterexamples CEa, CEb and CEc.
[0132] External and internal reflections are also low; they are less than 22%.
[0133] Comparing the properties of examples E13'a, E13'''a, E13'b, E13'''b, E13'c, and E13'''c according to the invention with, respectively as a function of the light transmission range, those of examples E1a, E1b and E1c according to the invention shows that the effect of the tungsten oxide-based layer is greater (lower solar factor) or similar when the first and third dielectric modules both comprise this tungsten oxide-based layer.
[0134] The selectivities of examples E1a, E1b and E1c according to the invention, examples E13'a, E13'b and E13'c according to the invention, examples E13'''a, E13'''b and E13'''c according to the invention and counter-examples CEa, CEb and CEc are summarized and show that the selectivity of the examples is always higher than that of the counter-examples for a similar light transmission and that this selectivity is higher or similar (for the light transmission of 70%) when the first and third dielectric modules each comprise a tungsten oxide-based layer.
[0135] In a fourth series of examples, two examples, E24'c and E24''c of substrate according to the first aspect of the invention test the presence of the tungsten oxide layer C2 in the first dielectric module 120 for example E24'c and in the three dielectric modules 120, 160 and 200 for example E24''c. These examples are compared to the same example E2c as previously.
[0136] Tab. 9 E24'cE2cE24''c300TiOx 111206SiN 3457200200aWO x -2119202ZnO 555190NiCr0,70,70,7180Ag15,616,716,3170NiCr---169ZnO555140168SnZnO 101010166SiN--22160aWO x --15164SiN707229162ZnO 555150NiCr0,70,70,7140Ag16,114,514,2130NiCr0,90,60,5129ZnO 555120120aWO x 131719124SiN 105510glass 6 mm6 mm6 mm
[0137] Table 10 presents properties of these examples and counterexamples.
[0138] Tab. 10 CEcE24'cE2cE24''cTL69,069,069,069,0g37,736,234,433,4s1,8281,9052,0062,065a*T-4,1-4,5-4,9-5,5b*T-0,3-0,6-1,0-0,5Rext15,0 15,015,015.0a*Rext-1.0-1.0-1.0-2.9b*Rext-7.8-4.0-4.2-5.0Rint14,414,815,415.3a*Rint-0.9-1.6-3.8-5.3b*Rint-5.0-5.0-1.3-4.1
[0139] Tab. 10 shows that the three examples E24'c, E2c and E24''c according to the invention allow a gain (increase) in selectivity, s, compared, respectively, to the counter-example CEc without tungsten oxide-based layer.
[0140] Tab. 10 shows that for a similar light transmission TL of the order of 70%, the solar factor, g, is better (lower) when each dielectric module has one (and only one) tungsten oxide-based layer (example E24''c). The selectivity is slightly higher (although in practice very close), when a tungsten oxide-based layer is provided in the first and last dielectric module (example E2c).
[0141] Comparison of the properties of examples E24''c and E24c according to the invention shows that the effect of the tungsten oxide-based layer is greater (lower solar factor) when all three dielectric modules comprise a tungsten oxide-based layer compared to a configuration in which only the first dielectric module comprises a tungsten oxide-based layer.
[0142] External and internal reflections are also low; they are less than 20%.
[0143] In another series of examples E15'a, E16'a, E15'b, E16'b, E15'c, and E16'c of substrate according to the first aspect of the invention the presence of the tungsten oxide layer C1 is tested in the first dielectric module 120 for all these examples with in addition:- for the series E15': a high refractive index dielectric layer based on nitride 204 in the third dielectric module 200; and- for the series E16': a contact layer based on oxide 203 in the third dielectric module 200. These examples are compared to the same examples E13'a, E13'b and E13'c as previously (for the properties).
[0144] Tab. 11 E15'aE16'aE15'bE16'bE15'cE16'c300TiOx 111111206SiN 6555510204SiZr17N21-23-24-200200aCWO------203TiOx-24-24-20202ZnO 5-5-5-190NiCr0.7-0.7-0.7-180Ag18,819,317,818,817,018,1170NiCr0.20.2----169ZnO555555140168SnZnO 101010101010164SiN696971717171162ZnO 555555150NiCr0,70,70,70,70,70,7140Ag14,715,315,314,414,516,7130NiCr1,01,01,33,0--129ZnO 555555120aCWO151324191616120126SiN 931----125NiCr1.81.7----124SiN 7655101010glass 6 mm6 mm6 mm6 mm6 mm6 mm
[0145] Table 12 presents properties of these examples and compares them to the preceding counterexamples.
[0146] Tab. 12 E13'aE15'aE16'aE13'bE15'bE16'bE13'cE15'cE16'cTL49,449,949,860 ,059,259,669,069,069,0g25,924,824,730,529,329,235,935,334.8s1 ,9082,0152,0131,9682,0242,0401,9211,9521,983a*T-7,5-8,3-6,9-6 .7-6.6-5.6-5.2-5.1-5.2b*T-3.1-1.7-2.9-3.0-2.3-2.2-1.3-0.9-1.4 Rext18,015,517,916,516,316,215,015,015,0a*Rext-1,0-2,3-3,0-1, 0-2.3-3.0-1.1-1.0-1.0b*Rext0.00.00.0-1.1-2.1-2.2-4.2-4.0-4.0R int20,518,520,318,118,016,415,715,715,6a*Rint-0.7-0.5-2.7-1.5 -3.0-2.3-1.6-2.1-1.3b*Rint-5.1-5.0-5.0-6.2-5.7-5.6-5.0-2.8-3.9
[0147] Tab. 12 shows that the six examples E15'a, E16'a, E15'b, E16'b, E15'c, and E16'c according to the invention have a light transmission TL similar to that of the counterexamples CEa, CEb, and CEc, respectively, and a solar factor, g, better (lower) than those of the counterexamples CEa, CEb, and CEc.
[0148] Tab. 12 shows that the six examples E15'a, E16'a, E15'b, E16'b, E15'c, and E16'c according to the invention allow a gain (increase) in selectivity, s, compared, respectively, to examples E13'a, E13'b and E13'c. This gain illustrates the synergistic effect of the combination of the tungsten oxide-based layer C1 in the first dielectric module with in the third dielectric module: a high refractive index dielectric layer based on nitride 204 or a contact layer based on oxide 203.
[0149] External and internal reflections are also low; they are less than 22%.
[0150] The selectivities of examples E1a, E1b and E1c according to the invention, examples E13'a, E13'b and E13'c according to the invention, examples E15'a, E16'a, E15'b, E16'b, E15'c, and E16'c according to the invention and counter-examples CEa, CEb and CEc are summarized and show that the selectivity of the examples is always higher than that of the counter-examples for a similar light transmission and that this selectivity is higher or similar for the low light transmissions of 50% and 60% when the first and third dielectric modules each comprise a tungsten oxide-based layer. For medium or high light transmissions (70% or more), it may be preferable to provide a single tungsten oxide-based layer in the first dielectric module; a nitride-based high refractive index dielectric layer or an oxide-based contact layer in the third dielectric module can help achieve high selectivity.
[0151] Examples E25'a, E25'b and E25'c according to the invention and examples E26'a, E26'b and E26'c according to the invention were made in a similar manner, respectively one by one to examples E15'a, E15'b, E15'c E16'a, E16'b, and E16'c according to the invention by replacing only layer C1 with layer C2; examples E25'd and E26'd were further designed for double glazing configurations having a light transmission of approximately 75%. Examples E24'a, E24'b and E24'd according to the invention were produced in a similar manner, respectively one by one to examples E2a, E2b and E2d according to the invention using a single layer C2, in the first dielectric module (i.e. without a layer in the third dielectric module), as for example E24'c presented above.
[0152] The selectivities of examples E2a, E2b, E2c and E2d according to the invention are summarized, of examples E24'a, E24'b, E24'c, and E24'd according to the invention, of examples E25'a, E25'b, E25'c, and E25'd according to the invention, of examples E26'a, E26'b, E26'c and E26'd according to the invention and of counter-examples CEa, CEb, CEc and CEd. This shows that the selectivity of the examples is always higher than that of the counter-examples for a similar light transmission. This further shows that this selectivity is higher or similar when the first and third dielectric modules each comprise a tungsten oxide-based layer for the low light transmissions of 50% and 60% or for the average light transmission of 70%.For high light transmissions (more than 70%), it may be preferable to provide a single tungsten oxide-based layer in the first dielectric module; a high refractive index nitride-based dielectric layer or an oxide-based contact layer in the third dielectric module may help achieve high selectivity.
[0153] These examples very clearly illustrate the advantages of the substrates of the invention, namely that they have a reduced solar factor, higher selectivity, and have a neutral color, both in transmission and for reflections.
Claims
Glass substrate (10) provided with a functional stack (14) of thin layers on at least one of its faces (11), said functional stack (14) comprising, starting from the substrate (10) at least two metallic functional layers (140, 180), preferably each based on silver, each located between two dielectric modules (120, 160, 200) of thin layers and forming a succession comprising a first dielectric module (120), a first metallic functional layer (140), a second dielectric module (160), a second metallic functional layer (180) and a last dielectric module (200), and in which at least one of the dielectric modules (120, 160, 200) of thin layers comprises a layer of tungsten oxide (120a, 160a, 200a) having a physical thickness of between 5 nm and 50 nm, and tungsten oxide:- comprising at least one doping element selected from the chemical elements of group 1 according to the IUPAC nomenclature,or- being pure substoichiometric, WOx, with x preferably between 2.55 and 2.98., Substrate (10) according to claim 1, such that said functional stack (14) comprises a single layer of tungsten oxide (120a, 160a, 200a) and said layer of tungsten oxide (120a, 160a, 200a) is preferably located in said first dielectric module (120) or in said last dielectric module (200). Substrate (10) according to claim 1, such that said functional stack (14) comprises two tungsten oxide layers (120a, 160a, 200a) and said tungsten oxide layers (120a, 160a, 200a) are preferably located for one in said first dielectric module (120) and for the other in said last dielectric module (200). Substrate (10) according to claim 1, such that said functional stack (14) comprises as many tungsten oxide layers (120a, 160a, 200a) as dielectric modules (120, 160, 200) and each dielectric module (120, 160, 200) comprises a tungsten oxide layer (120a, 160a, 200a). Substrate (10) according to any one of claims 1 to 4, such that the tungsten oxide layer(s) (120a, 160a, 200a) is not (or are not) in contact with a metallic functional layer (140, 180). Substrate (10) according to any one of claims 1 to 5, such that the optical refractive index of the tungsten oxide layer(s) (120a, 160a, 200a) decreases monotonically with wavelength from a maximum value greater than 2.4 at 350 nm to a minimum value between 600 nm and 900 nm so that the difference between the maximum value and the minimum value is greater than 0.8, preferably greater than 1.0, or even greater than 1.
4. Substrate (10) according to any one of claims 1 to 6, such that the optical extinction coefficient of the tungsten oxide layer(s) (120a, 160a, 200a) is less than 0.2 at 500 nm and less than 2.0 at 1200 nm. Substrate (10) according to any one of claims 1 to 7, such that the tungsten oxide layer(s) (120a, 160a, 200a) is (or are) made of pure sub-stoichiometric tungsten oxide, WOx, with x between 2.55 and 2.
95. Substrate (10) according to any one of claims 1 to 7, such that the tungsten oxide layer(s) (120a, 160a, 200a) comprises (comprise) a doping element, or several doping elements, in a proportion such that the molar ratio of said element to tungsten, or the sum of the molar ratios of each element to tungsten, is between 0.01 and 0.4, preferably between 0.01 and 0.2, or even between 0.01 and 0.
1. Substrate (10) according to any one of claims 1 to 7, 9, such that the tungsten oxide layer(s) (120a, 160a, 200a) comprises (comprise) at least one doping element selected from hydrogen, lithium, sodium, potassium and cesium. Substrate according to claim 10, such that the tungsten oxide layer(s) (120a, 160a, 200a) comprises cesium as doping element, and the molar ratio of cesium to tungsten is between 0.01 and 0.2, preferably between 0.01 and 0.
1. Substrate (10) according to any one of claims 1 to 11, such that the physical thickness of the tungsten oxide layer(s) (120a, 160a, 200a) is (or are) between 5 nm and 30 nm, preferably between 5 nm and 20 nm or between 9 nm and 25 nm, or even between 12 nm and 20 nm. Substrate (10) according to any one of claims 1 to 12, such that said functional stack (14) of layers further comprises at least one blocking overlayer (150, 190), preferably based on a nickel and chromium alloy, located above and in contact with a metallic functional layer (140, 180) and / or at least one metallic blocking underlayer (130, 170), preferably based on a nickel and chromium alloy, located below and in contact with a metallic functional layer (140, 180). Substrate (10) according to any one of claims 1 to 13, such that the functional stack of layers further comprises an oxide-based contact layer (203), made of titanium oxide, located above and in contact with the metal functional layer (180) furthest from the substrate, said oxide-based contact layer (203) preferably having a physical thickness of at least 5.0 nm, in particular between 5.0 and 35.0 nm. Substrate (10) according to any one of claims 1 to 14, such that the functional stack (14) of layers comprises a layer with a refractive index greater than 2.15 at 550 nm, said layer being included in the last dielectric module (200). Glazing comprising at least two transparent substrates, one of the substrates being a substrate according to any one of claims 1 to 15 arranged so that the functional stack of layers is located on face two and / or face three of said glazing. Method for manufacturing a transparent substrate according to any one of claims 1 to 15, such that the tungsten oxide layer(s) (120a, 160a, 200a) is (or are) deposited by a magnetron cathode sputtering method using a tungsten or tungsten oxide target, the material constituting said target being optionally doped using a chemical element chosen from the chemical elements of group 1 according to the IUPAC nomenclature.
Citation Information
Patent Citations
Glazing comprising a substrate furnished with a multiplicity of thin layers providing thermal insulation and / or solar protection
EP0847965A1
Cesium tungsten oxide film and method for manufacturing same
EP3686312A1
Heat ray cut-off glass and its production
JP1996012378A
Target material of composite tungsten oxide, and method for manufacturing the same
JP2010180449A
Glazing provided with a stack of thin layers for solar protection and / or heat insulation
WO2002048065A1