Arc welded joint and method for manufacturing same
Pulse welding with periodic short-circuit transitions and high Ar shielding gas addresses the instability and corrosion issues in conventional arc welding, achieving stable penetration and enhanced corrosion resistance for automotive suspension members, resulting in stronger and more durable welded joints.
Patent Information
- Application Number
- PCT/JP2024/001190
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-01-18
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional arc welding techniques face challenges in achieving stable penetration depth and corrosion resistance due to slag adhesion, oxidation of steel components, and instability in the welding process, which leads to reduced strength and increased corrosion in welded joints, particularly in automotive suspension members.
The use of pulse welding with periodic short-circuit transitions and a shielding gas with a high Ar content to reduce slag formation, combined with specific current waveform parameters, achieves stable penetration and excellent corrosion resistance by minimizing oxidation and slag adhesion, thereby enhancing the strength and durability of welded joints.
This approach results in arc welded joints with low and stable penetration depth, excellent corrosion resistance, and improved strength, while maintaining the existing welding equipment and avoiding the need for specialized setups, thus addressing the limitations of previous methods.
Smart Images

Figure JP2024001190_31102024_PF_FP_ABST
Abstract
Description
Arc welded joint and manufacturing method thereof
[0001] The present invention relates to an arc-welded joint that has a small amount of slag adhesion, a stable penetration depth, and excellent weld joint strength and corrosion resistance of the weld, and a method for producing the same.
[0002] In recent years, there has been a growing need for automobiles to simultaneously increase the strength and rigidity of components used in the body to improve the safety and reliability of the vehicle body, and to reduce the weight of components to improve fuel economy. As a result, the use of high-strength steel plates has led to the reduction in the thickness of component steel plates. Meanwhile, among the various components used in automobiles, thicker steel plates are used for suspension components (e.g., lower arms) compared to the body from the perspective of component strength and rigidity. Therefore, if the strength of the steel plates used in suspension components can be increased and the thickness of the steel plates can be reduced, further weight reduction of the vehicle body is possible. This will achieve improved fuel economy while maintaining the strength and rigidity of the components.
[0003] Generally, components used in corrosive environments undergo rust prevention treatments such as chemical conversion coating and electrodeposition coating after welding to ensure corrosion resistance. However, over time, rust and corrosion may be observed at the weld and its vicinity. As described above, corrosion that occurs in components with electrodeposition coating tends to occur at the weld and, over time, expands over a wide area at and around the weld, accompanied by paint blistering, and progresses in the thickness direction. As corrosion progresses in this manner, the thickness of the weld and its vicinity decreases, resulting in a decrease in the strength of the weld and, ultimately, the strength of the component. In other words, if corrosion occurs and progresses in a component that is subjected to a load at the weld (e.g., an automobile suspension component), it may lead to the destruction of the component.
[0004] When performing electrodeposition coating, a chemical conversion treatment (e.g., zinc phosphate treatment) is performed on the base steel sheet and weld metal as a pretreatment to improve adhesion between the electrodeposition coating and the base steel sheet and weld metal, followed by electrodeposition coating. Zinc phosphate treatment, a widely used example of a chemical conversion treatment, is a technique that grows zinc phosphate crystals on the surface of the base steel sheet and weld metal to improve the adhesion of the coating film during electrodeposition coating. However, with conventional techniques, even on components that have been chemically treated prior to electrodeposition coating, blistering frequently occurs over time in a wide area at and around the weld. In other words, the technique of performing the above-mentioned chemical conversion treatment as a pretreatment and then electrodeposition coating makes it difficult to completely prevent corrosion originating from the weld.
[0005] Furthermore, when arc welding is performed on a member using a steel sheet having a plated layer, the plated layer evaporates at the welded portion exposed to high heat from the arc plasma (hereinafter referred to as "arc"), which is the heat source, and the non-plated portion is locally exposed. Therefore, a significant improvement in corrosion resistance that would justify the use of a steel sheet having a costly plated layer cannot be expected.
[0006] As explained above, various manufacturing technologies have been developed to improve the corrosion resistance of components, but each has advantages and disadvantages. From the perspective of improving corrosion resistance while suppressing increases in manufacturing costs, technologies that can more effectively prevent the occurrence and progression of corrosion originating from welds are being studied.
[0007] The following are known as the starting points for corrosion at welds: (a) slag adhering to welds (mainly the surface of the weld bead), (b) welding fumes adhering to welds, and (c) oxides formed on the surface of steel sheets exposed to high temperatures during welding. Even when components with the above-mentioned deposits (a) and (b) or oxides (c) present at welds are subjected to chemical conversion treatment, these deposits and products form the starting point for areas that are not covered by the chemical conversion treatment layer consisting of zinc phosphate crystals. Applying electrodeposition coating to such areas results in insufficient coating film formation and poor coating adhesion, significantly reducing corrosion resistance and causing a reduction in plate thickness due to the initiation and progression of corrosion. The following technologies have been investigated to prevent the formation of the above-mentioned deposits (a) and (b) and oxides (c).
[0008] For example, Patent Document 1 discloses a technique in which, after arc welding and before electrodeposition coating, the weld and its vicinity are sprayed or immersed in a non-oxidizing acidic solution with a pH of 2 or less and a liquid temperature of 30 to 90° C. This technique removes the above-mentioned (a) slag, (b) welding fumes, and (c) oxides by dissolving the weld bead and base steel plate in the non-oxidizing solution.
[0009] However, the technology disclosed in Patent Document 1 requires washing away the acidic solution before electrodeposition coating, which complicates the manufacturing process of the component. Furthermore, because the component formed into a desired shape is made by overlapping and joining steel plates of various shapes, the acidic solution remaining in the gaps between the overlapping plates can cause severe corrosion. Furthermore, since a large amount of acidic solution is used, the manufacturing equipment is exposed to a corrosive environment, making it prone to corrosion and breakdowns. It is also necessary to prevent the dispersion of fumes to ensure the safety of workers.
[0010] Patent Document 2 discloses a technique for improving the corrosion resistance of a welded portion and its vicinity after painting by reducing the total Si content of a welding wire and a base material used in arc welding and increasing the total Mn content of the welding wire and the base material.
[0011] However, if the Si content is reduced in order to suppress slag generation, a decrease in the strength of the steel sheet is unavoidable. In other words, the technology disclosed in Patent Document 2 requires the use of thick steel sheets to ensure the strength of the members, making it difficult to achieve a reduction in the weight of the vehicle body.
[0012] Patent Document 3 discloses a technology for forming a sufficient chemical conversion coating layer even on weld beads containing slag, welding fumes, and oxides by adjusting the components of the treatment solution used in the chemical conversion coating. Specifically, the formation of the chemical conversion coating layer is facilitated by performing surface treatment using a surface conditioning solution containing zinc phosphate colloid. Furthermore, by performing chemical conversion treatment using a zinc phosphate treatment solution with an F content of 100 ppm by mass or more, slag, welding fumes, and oxides are dissolved and removed, improving the adhesion of the coating film formed by electrodeposition coating.
[0013] However, the technology disclosed in Patent Document 3 uses a zinc phosphate treatment solution containing fluorine, which is designated as a toxic substance, and therefore, when the waste liquid is discharged outside the factory, the fluorine content must be reduced to a level that satisfies environmental standards, which requires a large-scale waste liquid treatment facility in addition to the component manufacturing facility.
[0014] JP-A-9-20994 JP-A-8-33997 Patent No. 5549615
[0015] The present invention has been made in consideration of these problems, and has an object to provide an arc welded joint that has a small amount of slag adhesion, a stable penetration depth, and excellent weld joint strength and corrosion resistance of the weld, and a method for manufacturing the same.
[0016] The inventors have discovered that the most effective way to improve the corrosion resistance of the weld and stably obtain a welded joint with a stable penetration depth is to reduce the amount of slag that adheres to the weld and to achieve periodic short-circuiting transfer using pulse welding.
[0017] To reduce the amount of slag generated at the weld, it is important to suppress the oxidation of elements such as Si, Mn, and Ti contained in the steel sheet and welding wire. Using a shielding gas with a reduced oxidizing gas content suppresses the oxidation of these elements, thereby reducing the amount of slag generated. However, gas-shielded arc welding, which uses a high Ar gas ratio in the shielding gas, increases the arc spread. As a result, the heat flux to the base metal decreases, resulting in a shallow weld penetration depth. Furthermore, after the oxide film on the steel sheet surface is removed by cleaning, the cathode spot creeps along the steel sheet surface, making the arc unstable. As a result, the penetration depth becomes unstable. Therefore, the inventors have discovered a technology that uses pulse welding to reduce the creep of the cathode spot and achieve periodic short-circuit transfer that is less affected by arc wobble. By using a pulse current waveform, the inventors have discovered a technology that reduces slag deposition, achieves stable penetration, and obtains weld joints with excellent weld strength and corrosion resistance.
[0018] The present invention is based on the above findings, and its gist is as follows: [1] An arc welded joint manufactured by lap fillet arc welding to join a corner made of two steel plates, the arc welded joint having an upper plate, a lower plate, and a weld that joins the upper plate and the lower plate and penetrates into the upper plate and the lower plate, 1 and the thickness of the lower plate t 2 are each 5.0 mm or less, and the thickness t 2 The penetration depth d, which is the distance from the boundary between the upper plate and the lower plate in the cross section of the weld to the underside of the weld bead, satisfies the following formula (1), and the bead surface area S of the weld bead surface BEAD and the bead surface area S BEAD The slag surface area S is the area of the region covered by the slag. SLAG The slag coverage area ratio S is calculated using the following formula (2) RATIO 0.20≦d / t 2 ≦0.80 (1) In formula (1), t 2 (mm): thickness of lower plate, d (mm): penetration depth. RATIO =S SLAG / SBEAD × 100 (2) In equation (2), S BEAD (mm 2 ): bead surface area, S SLAG (mm 2 ): slag surface area, S, which is the area of the region covered by the slag RATIO [2] A method for manufacturing an arc welded joint according to the above [1], wherein the arc welding method is pulse welding in which a pulse peak current and a pulse base current are periodically repeated, and the average welding current I AVE is 100 A or more and 320 A or less, and the pulse peak current I p is 400 A or more and 600 A or less, and the pulse peak time T p [3] In the pulse welding, the pulse peak current I is 1.5 ms or more and 3.5 ms or less, and Ar gas having a volume percentage of 98% or more is used as a shielding gas during welding, and droplet transfer is achieved by a short circuit between the welding wire and the base metal. p , pulse base current I b , the pulse peak time T p , the rise time T from the pulse base current to the pulse peak current up , the fall time T from the pulse peak current to the pulse base current down , the arc voltage V, and the welding speed W satisfy the following formula (3). p × (T p +T up +T down )-(I p -I b ) × (T up +T down ) / 2) / (T p +T up +T down )×V / W / 1000≦14.4...(3) I p (A): Pulse peak current, I b (A): Pulse base current, T p (ms): Pulse peak time, T up (ms): Rise time, T down(ms): Fall time, V (V): Arc voltage, W (cm / s): Welding speed
[0019] According to the present invention, it is possible to obtain a welded joint with excellent strength by providing stable penetration, and a welded joint with excellent corrosion resistance by suppressing slag generation. Moreover, the above effects can be obtained without specially modifying the welding equipment used in conventional carbon dioxide welding, MAG welding using a mixed gas of inert gas and active gas, or MIG welding using a gas mainly composed of inert gas.
[0020]
[0023] Figure 1 is a schematic diagram showing an example of a welded joint produced by arc welding. Figures 2(a) and 2(b) are schematic diagrams showing droplet transfer by conventional arc welding. Figures 3(a) and 3(b) are schematic diagrams showing short-circuiting transfer according to the present invention. Figure 4 is a schematic diagram explaining penetration depth and throat thickness in a cross section of a weld. Figure 5 is a schematic diagram showing a pulse current waveform in arc welding according to the present invention. Figure 6 is a schematic diagram showing bead area and slag-covered area in a weld bead. Figure 7 is a schematic diagram showing corrosion resistance testing of a weld bead.
[0021] The present invention will be described in detail below with reference to the drawings. Fig. 1 is a schematic diagram showing an example of a welded joint produced by arc welding, illustrating an embodiment of the present invention. In this example, fillet arc welding of a lap joint joining a corner made of two steel plates is shown as a representative example, but the shape of the welded joint and the welding position are not limited in the present invention.
[0022] In the present invention, as shown in FIG. 1 , for example, a welding voltage is applied from a welding power source (not shown) to a welding wire 1 continuously fed from the welding torch 2 through the center thereof to a base metal 3 (more specifically, a weld line consisting of, for example, a corner of a stepped portion formed by stacking two base metals 3) as the anode, and the base metal 3 as the cathode. A contact tip is attached to the welding torch 2 and serves as a power supply and feed guide for the welding wire 1. A portion of the Ar shielding gas (not shown) supplied from the welding torch 2 is ionized and converted into plasma, forming an arc 5B between the welding wire 1 and the base metal 3. The portion of the Ar shielding gas that does not ionize and flows from the welding torch 2 to the base metal 3 serves to insulate the arc 5B and the molten pool (not shown in FIG. 1 ) formed by melting the base metal 3 from the outside air. Heat input from the arc 5B melts the tip of the welding wire 1 into a molten droplet, which is transported to the molten pool by electromagnetic force, gravity, or the like. This phenomenon occurs continuously as the welding torch 2 or the base material 3 moves, causing the molten pool to solidify behind the weld line, forming a weld bead 6. This achieves the joining of at least two steel plates (base materials 3).
[0023] On the other hand, when conventional MIG welding is performed on carbon steel, which is the subject of the present invention, there is a problem that the welding is extremely unstable. MAG welding or MIG welding is a reverse polarity welding in which the electrode (wire) is the anode, so cathode spots are formed starting from areas on the surface of the base steel sheet that have a low work function like oxides and are prone to electron emission. For example, in the case of an aluminum alloy that has a strong oxide film on the surface of the base material, cathode spots are stably formed starting from the oxide film on the weld line, making good welding possible. In contrast, in steel that is less likely to have an oxide film, cathode spots are formed stably starting from the oxide film on the weld line. 2 or CO 2In MIG welding, which does not produce oxides derived from oxidizing agents, the cathode spot is not fixed and moves around the base metal surface vigorously in search of a location with a low work function. As a result, heat input to the base metal is not stable, resulting in a welded joint with an insufficient penetration depth or a large variation in penetration depth. Furthermore, the instability of the welding process can reduce the shielding effect of the Ar shielding gas, which prevents oxidizing gases from entering the molten pool, and can increase the generation of slag.
[0024] To address this issue, the inventors observed arc behavior in welding experiments and concluded that the main cause of the aforementioned problems of insufficient penetration, unstable penetration, and increased slag generation in MIG welding of carbon steel is unstable droplet transfer. Figures 2(a) and 2(b) show schematic diagrams illustrating droplet transfer during conventional MIG welding. In conventional MIG welding, droplet transfer occurs in two ways: as shown in Figure 2(a), the welding wire 1 melts and is continuously transported to the molten pool 8 from a long, thin liquid column; and as shown in Figure 2(b), large droplets 7 form at the tip of the welding wire 1 and are transported to the molten pool 8 by falling or short-circuiting. Regularly detaching droplets 7 from the tip of the welding wire 1 is considered effective in suppressing this unstable droplet transfer. However, when using Ar shielding gas, the electromagnetic pinch force acting on the welding wire 1 is weak, making droplet 7 detachment difficult. Therefore, in the present invention, it has been found that an effective means for stabilizing droplet transfer is to complete joining by so-called periodic short-circuit transfer, in which the non-short-circuit state of Figure 3(a) and the short-circuit state of Figure 3(b) are regularly repeated between the tip of the welding wire 1 and the base metal 3, and droplets 7 are transferred to the base metal 3 during the short-circuit state. Furthermore, as a result of further welding experiments, it has been found that by limiting the pulse peak current and pulse peak time of the pulse current waveform, it is possible to control the penetration depth of the cross section of the weld as shown in Figure 4 to a predetermined value, and a predetermined weld joint strength can be obtained.
[0025] 4 is a schematic diagram illustrating the penetration depth and throat thickness in the cross section of the weld. The arc welded joint has an upper plate 20, a lower plate 21, and a weld bead 6 that joins the upper plate 20 and the lower plate 21 and penetrates into the upper plate 20 and the lower plate 21. The penetration depth 23 refers to the distance from the boundary 24 between the upper plate 20 and the lower plate 21 in the cross section of the weld to the underside of the weld bead 6. The thickness t of the lower plate 2 is number 22.
[0026] Lower plate thickness t 2 and the penetration depth d satisfies formula (1) 0.20 ≦ d / t 2 ≦ 0.80 (1) In formula (1), t 2 (mm): thickness of lower plate, d (mm): penetration depth. 2 If d / t is less than 0.20, poor penetration of the welded portion occurs, and the strength of the welded joint decreases. 2 is 0.20 or more. 2 is preferably 0.25 or more. 2 is more preferably 0.30 or more. 2 is more preferably 0.32 or more, and most preferably 0.35 or more. 2 If d / t exceeds 0.80, excessive heat input during welding increases the area of the weld heat affected zone, causing a decrease in the strength of the welded joint. In addition, the welding distortion increases, and the required strength of the welded joint may not be obtained. 2 The value of d / t must be 0.80 or less. 2 is preferably 0.75 or less. 2 is more preferably 0.70 or less. 2 More preferably, d / t is 0.68 or less. 2 is most preferably 0.65 or less.
[0027] Upper plate thickness t 1 and the thickness of the lower plate t 2 is 5.0 mm or less Upper plate thickness t 1 and the thickness of the lower plate t 2If the thickness t of the upper plate is larger than 5.0 mm, the penetration will be too small due to the diffusion of heat input, and the throat thickness 25 shown in FIG. 4 will be small, and the cross-sectional area (throat thickness x weld length) that bears the external load will be too small, leading to a decrease in the strength of the welded joint. 1 and the thickness of the lower plate t 2 The thickness of the upper plate t shall be 5.0 mm or less. 1 and the thickness of the lower plate t 2 The thickness t of the upper plate is preferably 4.8 mm or less, more preferably 4.5 mm or less, even more preferably 4.2 mm or less, and most preferably 4.0 mm or less. There is no particular limit to the lower limit, but 1 and the thickness of the lower plate t 2 is preferably 0.5 mm or more, more preferably 0.8 mm or more, even more preferably 1.0 mm or more, and most preferably 1.2 mm or more. Note that the weld length refers to the length of the weld bead 6 in the weld line direction 11 shown in FIG. 6.
[0028] Slag coverage area ratio S RATIO is 15% or less of the bead surface area S of the weld bead surface BEAD and the bead surface area S BEAD The slag surface area S is the area of the region covered by the slag. SLAG The slag coverage area ratio S is calculated using the following formula (2) RATIO If the slag coverage area ratio S exceeds 15%, rust and corrosion will occur from the slag over a wide area of the weld, and the strength of the welded joint may decrease due to a decrease in plate thickness. RATIO The slag coverage area ratio S is 15% or less. RATIO is preferably 14% or less. RATIO The slag coverage area ratio S is more preferably 12% or less. RATIO The slag coverage area ratio S is more preferably 10% or less. RATIO is most preferably 8% or less. The lower limit is not particularly limited, and may be 0%. RATIO =S SLAG / S BEAD × 100 (2) In equation (2), S BEAD (mm 2 ): bead surface area, S SLAG (mm 2 ): slag surface area, S, which is the area of the region covered by the slag RATIO (%): indicates the slag coverage area ratio.
[0029] Next, a method for manufacturing an arc welded joint will be described.
[0030] Average welding current I AVE Pulse welding is performed when the pulse peak current (I p ) and pulse base current (I b ) is periodically repeated. AVE is the time average of the welding current which changes periodically as shown by the pulse waveform in Figure 5. AVE In pulse welding where the average welding current I is less than 100 A, the instability of the MIG arc cannot be suppressed, and the desired penetration depth cannot be obtained. AVE The average welding current I AVE is preferably 120 A or more. AVE More preferably, the average welding current I is 140 A or more. AVE More preferably, the average welding current I is 160 A or more. AVE is most preferably 180 A or more. AVE In pulse welding where the average welding current I exceeds 320 A, the heat input becomes excessive and burn-through, which is a welding defect, may occur. AVE The average welding current I AVE is preferably 300 A or less. AVE More preferably, the average welding current I is 270 A or less. AVE More preferably, the average welding current I is 260 A or less. AVE is most preferably 250A or less.
[0031] Pulse peak current Ip Pulse peak current I is 400A or more and 600A or less p If the pulse peak current I is less than 400 A, the heat input will be too small, resulting in a decrease in the penetration depth. p The pulse peak current I p is preferably 450 A or more. p is more preferably 470 A or more. p The pulse peak current I is more preferably 490 A or more. p is most preferably 500 A or more. p If the pulse peak current I is greater than 600 A, the instantaneous heat input may become excessive, which may result in burn-through, a welding defect. The occurrence of burn-through, a welding defect, means that the base materials are not properly joined, and a desired arc welded joint cannot be obtained. For this reason, the pulse peak current I p The pulse peak current I p is preferably 590 A or less. p is more preferably 580 A or less. p The pulse peak current I is more preferably 570 A or less. p is most preferably 560A or less.
[0032] The pulse base current (I b If the pulse base current (I) is too small, the arc discharge during the base period becomes unstable, causing deterioration of the bead shape and insufficient penetration. b It is preferable that the pulse base current (I b ) is more preferably 40 A or more. b ) is more preferably 45 A or more. b ) is most preferably 50 A or more. On the other hand, if it is too large, burn-through occurs and the pulse peak current (I p ) and pulse base current (I b) difference cannot be sufficiently ensured, and the effect of pushing down the droplet 7 formed at the tip of the welding wire 1 into the molten pool 8 and short-circuiting it cannot be sufficiently obtained, resulting in unstable welding. b It is preferable that the pulse base current (I b It is more preferable that the pulse base current (I b ) is more preferably 100 A or less. b ) is most preferably 90A or less.
[0033] Pulse peak time T p Pulse peak time T is between 1.5 ms and 3.5 ms p If the pulse peak time T is less than 1.5 ms, the heat input will be too small, as with the pulse peak current, and the penetration depth will decrease. p The pulse peak time T p is preferably 1.8 ms or more. p More preferably, the pulse peak time T is 2.0 ms or more. p is more preferably 2.1 ms or more. p If the pulse peak time T exceeds 3.5 ms, the heat input becomes excessively large and burn-through, which is a welding defect, may occur. p The pulse peak time T p is preferably 3.2 ms or less. p More preferably, the pulse peak time T is 3.0 ms or less. p More preferably, the pulse peak time T is 2.9 ms or less. p More preferably, it is 2.8 ms or less.
[0034] Pulse peak current I p and pulse base current I b , pulse peak time T p , the rise time T from the pulse base current to the pulse peak current up , the fall time T from the pulse peak current to the pulse base currentdown , arc voltage V, and welding speed W satisfy the following formula (3) (preferable condition): 5.8 ≦ (I p × (T p +T up +T down )-(I p -I b ) × (T up +T down ) / 2) / (T p +T up +T down )×V / W / 1000≦14.4...(3) I p (A): Pulse peak current, I b (A): Pulse base current, T p (ms): Pulse peak time, T up (ms): Rise time, T down (ms): Fall time, V (V): Arc voltage, W (cm / s): Welding speed (I p × (T p +T up +T down )-(I p -I b ) × (T up +T down ) / 2) / (T p +T up +T down If (I ) × V / W / 1000 is less than 5.8 kJ / cm, the heat input at the peak time that affects the penetration becomes too small, and the penetration depth 23 decreases. p × (T p +T up +T down )-(I p -I b ) × (T up +T down ) / 2) / (T p +T up +T down ) × V / W / 1000 is preferably 5.8 kJ / cm or more. More preferably, it is 6.5 kJ / cm or more. Even more preferably, it is 7.0 kJ / cm or more. Most preferably, it is 7.5 kJ / cm or more. Furthermore, if it exceeds 14.4 kJ / cm, the heat input becomes too large and burn-through, which is a welding defect, may occur. For this reason, (I p × (Tp +T up +T down )-(I p -I b ) × (T up +T down ) / 2) / (T p +T up +T down ) × V / W / 1000 is preferably 14.4 kJ / cm or less, more preferably 12.8 kJ / cm or less, even more preferably 11.5 kJ / cm or less, and most preferably 10.2 kJ / cm or less.
[0035] Use of 98% or more Ar gas as shielding gas. If the Ar gas ratio of the shielding gas is less than 98% by volume, the chemical reaction between the oxidizing gas in the shielding gas and the alloying elements contained in the molten metal is accelerated, increasing the amount of slag produced, which reduces corrosion resistance. Therefore, the Ar gas ratio of the shielding gas is set to 98% by volume or more. The Ar gas ratio of the shielding gas is preferably 99% by volume or more. There is no particular upper limit, and the Ar gas ratio may be 100%.
[0036] The welding wire 1 used in the present invention is not particularly limited. For example, a solid wire for MAG welding as described in JIS Z 3312 can be used.
[0037] The base material 3 of the present invention is intended to be a steel sheet and a plated steel sheet. The chemical composition of the steel sheet is not particularly limited, but a steel sheet containing, for example, 0.02 to 0.3 mass% C, 0.01 mass% or more Si, 0.5% mass% or more Mn, 0.05 mass% or less P, and 0.05 mass% or less S is preferred. Other alloying elements such as Cu, Ni, Cr, and Ti may also be included. In the above steel sheet, the Si content is preferably 3.0 mass% or less, and the Mn content is preferably 5.0 mass% or less. The lower limit of the P content is not particularly limited, but is preferably 0.0005 mass% or more, and the lower limit of the S content is not particularly limited, but is preferably 0.0005 mass% or more. The plating composition of the plated steel sheet is not particularly limited, but may include, for example, Zn.
[0038] Examples of the present invention will be described below. Two steel plates (with the same thickness) having the chemical compositions shown in Table 1 were stacked together, and fillet welding was performed, for example, using the method shown in Figure 1. Note that the steel plates contained alloy elements such as Fe, Cu, Ni, Cr, and Ti as chemical compositions other than those shown in Table 1. Welding was performed under the welding conditions shown in Table 2. A solid wire for MAG welding as specified in JIS Z 3312 was used as the welding wire.
[0039] The welded steel plates obtained as described above were evaluated for slag coverage area ratio, penetration depth, corrosion resistance of the welded portion, and weld joint strength according to the following test methods.
[0040] (Slag Coverage Area Ratio) Fig. 6 is a schematic diagram showing the bead area and the slag covered area of a weld bead. BEAD and the slag-covered surface area S SLAG is calculated by photographing the surface of the area excluding the bead start and end portions 10 of the weld bead 6 (each 15 mm long) from directly above, and measuring the projected area from the top surface of the weld bead 6 and slag. If the length of the weld bead 6 is less than 130 mm, the entire surface is photographed excluding the bead start and end portions 10. If the length of the weld bead 6 is 130 mm or more, the surface of any portion (100 mm long) excluding the bead start and end portions 10 is photographed. The calculated slag surface area S SLAG The value of the bead surface area S BEAD The slag coverage area ratio S RATIO I asked for S. RATIO A value of 15% or less was considered acceptable.
[0041] (Penetration Depth) The penetration depth d was measured by observing a cross section in the thickness direction perpendicular to the weld line (parallel to the line AA in FIG. 6 ) at five arbitrary points of the weld bead 6 as shown in FIG. 4 in an area excluding the bead start and end portions 10 (each 15 mm long) of the weld bead 6. However, the five arbitrary points were positioned at least 5 mm apart from each other. Here, the weld bead 6 was cut at arbitrary points in the thickness direction perpendicular to the weld line, and the penetration depth 23 of each was determined, and the average value thereof was taken as the "penetration depth d (mm)." d / t 2 (t 2is the thickness of the lower plate) was rated as passing when it was 0.20 or more and 0.80 or less.
[0042] (Corrosion Resistance Evaluation Results) Figure 7 is a schematic diagram showing the corrosion resistance test of a weld bead. First, the arc-welded joint after the corrosion test was immersed in an immersion stripper to remove the electrodeposition coating, and then the corrosion products were removed in accordance with ISO 8407. Next, when the weld bead 6 included bead start and end terminals 10 (each 15 mm long), the surface of the area excluding the bead start and end terminals 10 was photographed, and the photographs were analyzed to determine the maximum corrosion width H in the corroded area 12 from the bead toe in a direction perpendicular to the weld line direction 11. MAX When the length of the weld bead 6 was less than 130 mm, the entire surface was photographed excluding the bead start and end portions 10. When the length of the weld bead 6 was 130 mm or more, the surface of any portion (100 mm long) was photographed excluding the bead start and end portions 10. The corrosion resistance was evaluated by the maximum corrosion width H MAX When the thickness was less than 6.0 mm, it was judged to be excellent and marked with "◯", and when it was 6.0 mm or more, it was judged to have insufficient corrosion resistance and marked with "X".
[0043] (Evaluation Results of Welded Joint Strength) First, a tensile test piece according to JIS Z 2241 was obtained from the welded joint by machining. The tensile test piece was prepared so that the weld was at the center. A tensile test was performed on the prepared tensile test piece at room temperature at a tension speed of 10 mm / min to obtain the joint tensile strength. This value was divided by the tensile strength of the base material (here, simply referred to as the strength ratio) and used as an evaluation parameter for the welded joint strength. In the evaluation of the welded joint strength, a strength ratio of 0.6 or more was judged to be superior and given a rating of "◎", a strength ratio of 0.5 or more but less than 0.6 was judged to be excellent and given a rating of "◯", and a strength ratio of less than 0.5 was judged to be insufficient and given a rating of "×".
[0044] As is clear from Table 2, welding Nos. 1 to 6 and 12 to 17 shown as examples of the invention are S RATIO is 15% or less and d / t 2 The welded joints obtained were excellent in corrosion resistance and strength, with a value of 0.20 or more and 0.80 or less.
[0045] Among these invention examples, welds No. 1 to 4 and 12 to 14 are S RATIO is 15% or less and d / t 2 The welded joints obtained were 0.30 or more and 0.70 or less, and had better corrosion resistance and welded joint strength.
[0046] In contrast, the comparative examples, welding Nos. 7 to 11, were S RATIO is greater than 15%, or d / t 2 was less than 0.20 or more than 0.80, and good welded joints could not be obtained.
[0047] In Table 2, "S RATIO is 15% or less and d / t 2 If the value is 0.30 or more and 0.70 or less and the weld joint strength is "◎", the evaluation is A, and if the value is "S RATIO is 15% or less and d / t 2 is 0.20 or more and less than 0.30 or S RATIO is 15% or less and d / t 2 If the value is greater than 0.70 and less than 0.80 and the weld joint strength is "Good", the evaluation is B. RATIO is greater than 15%, or d / t 2 When the value was less than 0.20 or more than 0.80, or the strength of the welded joint was "x", the evaluation was F. Evaluation F was considered a failure, and evaluations A and B were considered pass.
[0048]
[0049]
[0050] REFERENCE SIGNS LIST 1 welding wire 2 welding torch 3 base metal 5B arc 6 weld bead 7 droplet 8 molten pool 10 start and end of bead 11 weld line direction 12 corrosion area 20 upper plate 21 lower plate 22 plate thickness of lower plate 23 penetration depth 24 boundary between upper and lower plates in cross section of weld 25 throat thickness T up Rise time T p Peak current time T down Fall time T b Pulse base current time T up +Tp +T down +T b Pulse 1 cycle S BEAD Bead surface area S SLAG Slag coated surface area H MAX Maximum corrosion width
Claims
1. An arc welded joint manufactured by lap fillet arc welding to join a corner consisting of two steel plates, the arc welded joint having an upper plate, a lower plate, and a welded portion that joins the upper plate and the lower plate and penetrates into the upper plate and the lower plate, and the plate thickness t of the upper plate 1 and the thickness of the lower plate, t 2 are each 5.0 mm or less, and the plate thickness t 2 The penetration depth d, which is the distance from the boundary between the upper plate and the lower plate in the cross section of the weld to the underside of the weld bead, satisfies the following formula (1), and the bead surface area S of the weld bead surface BEAD and the bead surface area S BEAD The slag surface area S is the area of the region covered by the slag. SLAG The slag coverage area ratio S is calculated using the following formula (2) RATIO 0.20≦d / t 2 ≦0.80 (1) In formula (1), t 2 (mm): thickness of lower plate, d (mm): penetration depth. S RATIO =S SLAG / S BEAD × 100 (2) In formula (2), S BEAD (mm 2 ): bead surface area, S SLAG (mm 2 ): slag surface area, which is the area of the region covered by the slag, S RATIO (%): Slag coverage area ratio.
2. A method for manufacturing an arc welded joint according to claim 1, comprising the steps of: a method for manufacturing an arc welded joint according to claim 1, comprising the steps of: a method for manufacturing an arc welded joint according to claim 1, AVE is 100A or more and 320A or less, and the pulse peak current I p is 400 A or more and 600 A or less, and the pulse peak time T p a welding time of 1.5 ms or more and 3.5 ms or less, Ar gas having a volume percentage of 98% or more is used as a shielding gas during welding, and droplet transfer is achieved by a short circuit between the welding wire and the base metal.
3. In the pulse welding, the pulse peak current I p , pulse base current I b , the pulse peak time T p , the rise time T from the pulse base current to the pulse peak current up , the fall time T from the pulse peak current to the pulse base current down 3. The method for manufacturing an arc welded joint according to claim 2, wherein 5.8≦(I p × (T p +T up +T down ) - (I p -I b ) × (T up +T down ) / 2) / (T p +T up +T down )×V / W / 1000≦14.4...(3) I p (A): Pulse peak current, I b (A): Pulse base current, T p (ms): Pulse peak time, T up (ms): Rise time, T down (ms): Fall time, V (V): Arc voltage, W (cm / s): Welding speed
Citation Information
Patent Citations
Gas shielded metal arc welding method which enhances corrosion resistance after coating of weld zone and near this zone
JP1996033997A
Improvement of corrosion resistance after coating in arc weld zone and its vicinity
JP1997020994A
Method for chemical treatment of steel members, method for manufacturing coated steel members with electrodeposition coating, and coated steel members
JP5549615B2
Gas shield arc-welding method, and welding structure component
JP2017164798A
Arc welded joint and arc welding method
WO2021210335A1