Arc welded joint and manufacturing method therefor
Pulse welding with controlled current waveforms and high Ar shielding gas reduces slag and spatter in arc welded joints, addressing corrosion issues and improving the reliability of welded components.
Patent Information
- Application Number
- PCT/JP2024/001191
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-01-18
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional arc welding techniques face challenges in reducing slag and spatter adhesion, which leads to corrosion issues in welded areas, compromising the strength and reliability of components, especially in automotive suspension members.
The use of pulse welding with a controlled pulse current waveform, specifically decreasing the pulse peak current from start to end and maintaining an average welding current between 100A and 320A, along with a shielding gas composition of 98% or more Ar, to minimize slag and spatter formation and enhance corrosion resistance.
This approach results in arc welded joints with reduced slag and spatter adhesion, improving corrosion resistance without requiring changes to existing welding equipment and processes, thus enhancing the durability and reliability of welded components.
Smart Images

Figure JP2024001191_31102024_PF_FP_ABST
Abstract
Description
Arc welded joint and manufacturing method thereof
[0001] The present invention relates to an arc-welded joint that has reduced amounts of slag and spatter adhesion and is excellent in corrosion resistance, and to a method for manufacturing the same.
[0002] In recent years, there has been a growing need for automobiles to simultaneously increase the strength and rigidity of components used in the body to improve the safety and reliability of the vehicle body, and to reduce the weight of components to improve fuel economy. As a result, the use of high-strength steel plates has led to the reduction in the thickness of component steel plates. Meanwhile, among the various components used in automobiles, thicker steel plates are used for suspension components (e.g., lower arms) compared to the body from the perspective of component strength and rigidity. Therefore, if the strength of the steel plates used in suspension components can be increased and the thickness of the steel plates can be reduced, further weight reduction of the vehicle body is possible. This will achieve improved fuel economy while maintaining the strength and rigidity of the components.
[0003] Generally, components used in corrosive environments undergo rust prevention treatments such as chemical conversion coating and electrodeposition coating after welding to ensure corrosion resistance. However, over time, rust and corrosion may be observed at the weld and its vicinity. As described above, corrosion that occurs in components with electrodeposition coating tends to occur at the weld and, over time, expands over a wide area at and around the weld, accompanied by paint blistering, and progresses in the thickness direction. As corrosion progresses in this manner, the thickness of the weld and its vicinity decreases, resulting in a decrease in the strength of the weld and, ultimately, the strength of the component. In other words, if corrosion occurs and progresses in a component that is subjected to a load at the weld (e.g., an automobile suspension component), it may lead to the destruction of the component.
[0004] When performing electrodeposition coating, a chemical conversion treatment (e.g., zinc phosphate treatment) is performed on the base steel sheet and weld metal as a pretreatment to improve adhesion between the electrodeposition coating and the base steel sheet and weld metal, followed by electrodeposition coating. Zinc phosphate treatment, a widely used example of a chemical conversion treatment, is a technique that grows zinc phosphate crystals on the surface of the base steel sheet and weld metal to improve the adhesion of the coating film during electrodeposition coating. However, with conventional techniques, even on components that have been chemically treated prior to electrodeposition coating, blistering frequently occurs over time in a wide area at and around the weld. In other words, the technique of performing the above-mentioned chemical conversion treatment as a pretreatment and then electrodeposition coating makes it difficult to completely prevent corrosion originating from the weld.
[0005] Furthermore, when arc welding is performed on a member using a steel sheet having a plated layer, the plated layer evaporates at the welded portion exposed to high heat from the arc plasma (hereinafter referred to as "arc"), which is the heat source, and the non-plated portion is locally exposed. Therefore, a significant improvement in corrosion resistance that would justify the use of a steel sheet having a costly plated layer cannot be expected.
[0006] As explained above, various manufacturing technologies have been developed to improve the corrosion resistance of components, but each has advantages and disadvantages. From the perspective of improving corrosion resistance while suppressing increases in manufacturing costs, technologies that can more effectively prevent the occurrence and progression of corrosion originating from welds are being studied.
[0007] The following are known as the starting points for corrosion at welds: (a) slag adhering to welds (mainly the surface of the weld bead), (b) welding fumes adhering to welds, and (c) oxides formed on the surface of steel sheets exposed to high temperatures during welding. Even when components with the above-mentioned deposits (a) and (b) or oxides (c) present at welds are subjected to chemical conversion treatment, these deposits and products form the starting point for areas that are not covered by the chemical conversion treatment layer consisting of zinc phosphate crystals. Applying electrodeposition coating to such areas results in insufficient coating film formation and poor coating adhesion, significantly reducing corrosion resistance and causing a reduction in plate thickness due to the initiation and progression of corrosion. The following technologies have been investigated to prevent the formation of the above-mentioned deposits (a) and (b) and oxides (c).
[0008] For example, Patent Document 1 discloses a technique in which, after arc welding and before electrodeposition coating, the weld and its vicinity are sprayed or immersed in a non-oxidizing acidic solution with a pH of 2 or less and a liquid temperature of 30 to 90° C. This technique removes the above-mentioned (a) slag, (b) welding fumes, and (c) oxides by dissolving the weld bead and steel plate in the non-oxidizing solution.
[0009] However, the technology disclosed in Patent Document 1 requires washing away the acidic solution before electrodeposition coating, which complicates the manufacturing process of the component. Furthermore, because the component formed into a desired shape is made by overlapping and joining steel plates of various shapes, the acidic solution remaining in the gaps between the overlapping plates can cause severe corrosion. Furthermore, since a large amount of acidic solution is used, the manufacturing equipment is exposed to a corrosive environment, making it prone to corrosion and breakdowns. It is also necessary to prevent the dispersion of fumes to ensure the safety of workers.
[0010] Patent Document 2 discloses a technique for improving the corrosion resistance of a welded portion and its vicinity after painting by reducing the total Si content of a welding wire and a base material used in arc welding and increasing the total Mn content of the welding wire and the base material.
[0011] However, if the Si content is reduced in order to suppress slag generation, a decrease in the strength of the steel sheet is unavoidable. In other words, the technology disclosed in Patent Document 2 requires the use of thick steel sheets to ensure the strength of the members, making it difficult to achieve a reduction in the weight of the vehicle body.
[0012] Patent Document 3 discloses a technology for forming a sufficient chemical conversion coating layer even on weld beads containing slag, welding fumes, and oxides by adjusting the components of the treatment solution used in the chemical conversion coating. Specifically, the formation of the chemical conversion coating layer is facilitated by performing surface treatment using a surface conditioning solution containing zinc phosphate colloid. Furthermore, by performing chemical conversion treatment using a zinc phosphate treatment solution with an F content of 100 ppm by mass or more, slag, welding fumes, and oxides are dissolved and removed, improving the adhesion of the coating film formed by electrodeposition coating.
[0013] However, the technology disclosed in Patent Document 3 uses a zinc phosphate treatment solution containing fluorine, which is designated as a toxic substance, and therefore, when the waste liquid is discharged outside the factory, the fluorine content must be reduced to a level that satisfies environmental standards, which requires a large-scale waste liquid treatment facility in addition to the component manufacturing facility.
[0014] JP-A-9-20994 JP-A-8-33997 Patent No. 5549615
[0015] The present invention has been made in consideration of these problems, and aims to provide an arc welded joint with excellent corrosion resistance in which the amount of slag and spatter adhesion is reduced, and a method for manufacturing the same.
[0016] The inventors considered that in order to improve the corrosion resistance of welds, it is important to reduce the amount of slag that adheres to the welds and to stably obtain welded joints with reduced amounts of spatter adhesion.
[0017] To reduce the amount of slag generated at a weld, it is important to suppress the oxidation of elements such as Si, Mn, and Ti contained in the steel sheet and welding wire. Using a shielding gas with a reduced oxidizing gas content suppresses the oxidation of these elements, thereby reducing the amount of slag generated. However, in gas-shielded arc welding (GAW) using a high Ar gas ratio in the shielding gas, after the oxide film on the steel sheet surface is removed by cleaning, cathode spots creep along the steel sheet surface, resulting in an unstable arc. Therefore, pulse welding is effective in reducing cathode spot creep and achieving periodic short-circuiting transfer that is less affected by arc wobble. However, conventional short-circuiting transfer generates a large amount of spatter, which adheres to the weld bead surface. Therefore, the inventors have discovered the following technology, which uses pulse welding to reduce cathode spot creep and achieve periodic short-circuiting transfer that is less affected by arc wobble, and controls the pulse current waveform to reduce slag deposition and produce a welded joint with reduced spatter deposition.
[0018] Specifically, in the control of the pulse current waveform, the pulse peak current is decreased from the start of the pulse peak to the end of the pulse peak, and the current I at the start of the pulse peak is pstart 300A or more and 600A or less, the current I at the end of the pulse peak pend The inventors have found that by setting the current to be 200 A or more and 450 A or less, an arc welded joint can be obtained in which the amount of spatter adhesion is reduced in the weld spatter affected zone, which includes the weld bead, the weld toe which is the boundary between the base metal and the weld bead, and the periphery thereof.
[0019] The present invention is based on the above findings and is summarized as follows: [1] An arc welded joint manufactured by arc welding, the arc welded joint having a base metal, a weld bead formed by the base metal and welding wire melted by heat input from an arc mixing and solidifying, and a weld heat affected zone, the length in the weld line direction being the length of the weld bead excluding 15 mm at each end of the weld bead, and the length perpendicular to the weld line being 40 mm centered on the center line of the weld bead, the number of spatters generated during welding and adhering to the weld spatter affected zone, with a maximum length of an adhering region of 0.2 mm or more, is 0.50 spatters / cm 2 and the bead surface area S of the weld bead surface is less than or equal to BEAD and the bead surface area S BEAD The slag surface area S is the area of the region covered by the slag. SLAG The slag coverage area ratio S is calculated using the following formula (1) RATIO An arc welded joint in which the difference is 15% or less. RATIO =S SLAG / S BEAD × 100 (1) In the formula (1), S BEAD (mm 2 ): bead surface area, S SLAG (mm 2 ): slag surface area, S, which is the area of the region covered by the slag RATIO [2] A method for manufacturing an arc welded joint according to the above [1], wherein the welding wire and the base material are joined by short-circuiting, and the arc welding method is pulse welding in which a pulse peak current and a base current are periodically repeated, and the average welding current I AVE is 100 A or more and 320 A or less, the pulse peak current decreases from the pulse peak start to the pulse peak end, and the current I at the pulse peak start pstart is 300 A or more and 600 A or less, and the current I at the end of the pulse peak pend[3] In the pulse welding, a pulse peak time T p is 1.0 ms or more and 3.5 ms or less, and the current I at the start of the pulse peak pstart , the current I at the end of the pulse peak pend , the pulse peak time T p The method for manufacturing an arc welded joint according to [2], wherein the following formula (2) is satisfied: 45≦(I pstart -I pend ) / T p ≦210 (2) In formula (2), I pstart (A): Current at the start of the pulse peak, I pend (A): Current at the end of the pulse peak, T p (ms): Indicates the pulse peak time.
[0020] According to the present invention, it is possible to obtain an arc-welded joint with reduced amounts of spatter and slag adhesion and excellent corrosion resistance at the weld. Moreover, the above effects can be obtained without special modifications to the welding equipment used in conventional carbon dioxide gas welding, MAG welding using a mixed gas of inert gas and active gas, or MIG welding using a gas mainly composed of inert gas.
[0021] Fig. 2(a) and Fig. 2(b) are schematic diagrams showing an example of a welded joint produced by arc welding. Fig. 2(a) and Fig. 2(b) are schematic diagrams showing the state of short-circuit transfer according to the present invention. Fig. 2(a) is a schematic diagram showing a pulse current waveform in arc welding according to the present invention. Fig. 2(b) is a schematic diagram showing a range for evaluating spatter in an arc welded joint according to the present invention. Fig. 2(b) is a schematic diagram showing the bead area and slag covered area in a weld bead.
[0022] The present invention will be described in detail below with reference to the drawings. Fig. 1 is a schematic diagram showing an example of a welded joint produced by arc welding, illustrating an example of an embodiment of the present invention. In this example, welding on one base material is shown as a representative example, but the shape of the welded joint and the welding position are not limited in the present invention.
[0023] In the present invention, as shown in FIG. 1 , for example, a welding voltage is applied from a welding power source (not shown) to a welding wire 1 continuously fed from the welding torch 2 through the center of the welding torch 2 to a base metal 3, which serves as the anode, and the base metal 3 serves as the cathode. A contact tip is attached to the welding torch 2 and serves as a power supply and feed guide for the welding wire 1. A portion of the Ar shielding gas (not shown) supplied from the welding torch 2 is ionized and converted into plasma, forming an arc 5B between the welding wire 1 and the base metal 3. The portion of the Ar shielding gas that does not ionize and flows from the welding torch 2 to the base metal 3 serves to insulate the arc 5B and the molten pool (not shown in FIG. 1 ) formed by melting the base metal 3 from the outside air. Heat input from the arc 5B melts the tip of the welding wire 1, forming droplets, which are transported to the molten pool by electromagnetic force, gravity, or the like. This phenomenon occurs continuously as the welding torch 2 or the base material 3 moves, causing the molten pool to solidify behind the weld line, forming a weld bead 6.
[0024] In the present invention, it has been found that pulse welding, in which the non-short-circuit state shown in Fig. 2(a) and the short-circuit state shown in Fig. 2(b) are regularly repeated between the tip of the welding wire 1 and the base material 3, and droplets 7 are transferred to the base material 3 during the short-circuit state, is an effective means for stabilizing droplet transfer. Figure 3 shows a schematic diagram illustrating an example of a pulse current waveform in arc welding according to the present invention. pstart is the current at the start of the pulse peak, I pend is the current at the end of the pulse peak, I B is the base current, T pindicates the pulse peak time. Furthermore, as a result of further welding experiments, it was found that, as shown in Figure 3, by decreasing the pulse peak current from the start of the pulse peak to the end of the pulse peak, an arc welded joint can be obtained in which the amount of spatter deposited in the weld spatter-affected zone, including the weld bead 6, the weld toe, and its periphery, is reduced. This is because the force of the droplets 7 penetrating into the molten pool 8 can be reduced by reducing the downward action of the arc 5B on the droplets 7 just before the end of the pulse peak current, i.e., at the timing of the short-circuit transition, and by reducing the arc pressure 10, the force of the droplets 7 penetrating into the molten pool 8 can be reduced, thereby making it possible to reduce spatter. Figure 3 shows a representative pulse current waveform in which the pulse peak current decreases at a constant rate from the start of the pulse peak to the end of the pulse peak, but the present invention does not limit the process by which the pulse peak current decreases from the start of the pulse peak to the end of the pulse peak. Furthermore, the current I at the start of the pulse peak pstart 300A or more and 600A or less, the current I at the end of the pulse peak pend By setting the current to be 200 A or more and 450 A or less, the above-mentioned effects can be achieved.
[0025] First, the arc welded joint will be described in detail.
[0026] Figure 4 shows a schematic diagram illustrating the range for evaluating spatter in an arc-welded joint according to the present invention. The arc-welded joint includes a base metal 3, a weld bead 6 formed by the solidification of the base metal 3 and welding wire 1 melted by heat input from an arc 5B, and a weld heat-affected zone (HAZ). Large-diameter spatter can be a starting point for corrosion, so reducing it is preferable. It is particularly important to control the number of spatters 22 adhering to the boundary (weld toe) between the base metal 3 and the weld bead 6, where stress concentration occurs when an external force is applied, and its surrounding area. Therefore, the corrosion resistance of the weld can be improved by reducing the number of spatters 22 adhering during welding in the weld spatter-affected zone 21. The length in the weld line direction 23 is the length of the weld bead 6 excluding 15 mm at each end 20 of the weld bead, and the length perpendicular to the weld line is 40 mm centered on the centerline of the weld bead 6. The weld spatter-affected zone 21 always includes the boundary (weld toe) between the base metal 3 and the weld bead 6.
[0027] The number of spatters adhering to the welding spatter-affected area with a maximum length of 0.2 mm or more is 0.50 / cm 2 The number of spatter particles with a maximum length of 0.2 mm or more in the adhesion area is 0.50 / cm 2 If the number of spatter deposits exceeds 0.50 / cm, rust will start to form from the spatter, and corrosion will progress to the weld toe, reducing the corrosion resistance of the weld and resulting in a decrease in the strength of the welded joint due to a decrease in plate thickness. 2 The number of sputter deposits is preferably 0.48 / cm 2 The number of sputter deposits is more preferably 0.45 / cm 2 More preferably, it is 0.42 particles / cm or less. 2 The lower limit is not particularly limited, and is 0 particles / cm 2 The maximum length of the adhesion region refers to the longest linear distance between the ends of the adhesion region that are different from the end of the adhesion region. The upper limit of the maximum length of the adhesion region is not particularly limited, but since there is little possibility that spatters exceeding 5.0 mm are generated, it is preferable to consider a maximum length of the adhesion region of 5.0 mm or less. Here, spatters with a maximum length of the adhesion region of less than 0.2 mm have little effect on corrosion resistance, so there is no limitation.
[0028] Bead surface area S of the weld bead surface BEAD and the bead surface area S BEAD The slag surface area S is the area of the region covered by the slag. SLAG The slag coverage area ratio S is calculated using equation (1) RATIO is 15% or less S RATIO =S SLAG / S BEAD × 100 (1) In the formula (1), S BEAD (mm 2 ): bead surface area, S SLAG (mm 2 ): slag surface area, S, which is the area of the region covered by the slag RATIO (%): indicates the slag coverage area ratio.
[0029] Slag coverage area ratio S RATIO If the slag coverage area ratio S exceeds 15%, rust and corrosion will occur from the slag over a wide area of the weld, and the strength of the welded joint may decrease due to a decrease in plate thickness. RATIO The slag coverage area ratio S is 15% or less. RATIO is preferably 14% or less. RATIO More preferably, the slag coverage area ratio S is 12% or less. RATIO More preferably, the slag coverage area ratio S is 10% or less. RATIO is most preferably 8% or less. The lower limit is not particularly limited, and may be 0%.
[0030] The welded joint of the present invention is intended to have a length of at least more than 30 mm in the weld line direction 23 and a length of 40 mm or more in the direction perpendicular to the weld line. Although there is no particular upper limit to the above, the length of the welded joint in the weld line direction 23 is preferably 500 mm or less. It is preferable that the length be 500 mm or less in the direction perpendicular to the weld line.
[0031] The method for manufacturing an arc welded joint will be described in detail below.
[0032] Arc welding is a method of joining metals by short-circuiting the welding wire and base metal. In arc welding, external disturbances and creeping of the cathode spot can cause droplet transfer to become unstable, resulting in increased spatter generation and deposition, and increased slag generation and deposition. In response to this, periodically short-circuiting the welding wire 1 and base metal 3 can achieve stable droplet transfer, leading to reduced spatter and slag. For this reason, it is necessary to perform arc welding, which joins metals by short-circuiting the welding wire 1 and base metal 3.
[0033] Pulse welding in which the pulse peak current and the base current are periodically repeated, and the average welding current I AVE Average welding current I is 100A or more and 320A or less AVEBy using a pulse current of 100 A or more and 320 A or less, it is possible to easily perform periodic and stable short-circuit transfer control even in arc welding in which the Ar gas ratio of the shielding gas is 98% by volume or more. Therefore, the arc welding of the present invention is pulse welding in which the pulse peak current and the base current are periodically repeated, and the average welding current I AVE The average welding current I must be between 100A and 320A. AVE If the average welding current I is less than 100 A, droplet transfer becomes unstable and periodic short-circuit transfer cannot be achieved, which may result in an increase in the number of spatters generated and attached. AVE The average welding current I AVE is preferably 120 A or more. AVE is more preferably 140 A or more. AVE The average welding current I is more preferably 150 A or more. AVE is most preferably 170 A or more. AVE If the average welding current I exceeds 320 A, the periodic short circuit transfer cannot be maintained, and the number of spatters generated and attached may increase. AVE The average welding current I AVE is preferably 310 A or less. AVE The average welding current I is more preferably 300 A or less. AVE The average welding current I is more preferably 280 A or less. AVE is most preferably 260A or less.
[0034] The pulse peak current decreases from the start of the pulse peak to the end of the pulse peak. Spatter 22 is mainly generated at the timing of the short circuit that occurs just before the end of the pulse peak. If a short circuit occurs when the current is high and the arc pressure 10 is large, the droplets 7 are struck against the molten pool 8, making the spatter 22 more likely to scatter. In response to this, it is possible to suppress the amount of spatter 22 generated and the number of deposits by decreasing the pulse peak current from the start of the pulse peak to the end of the pulse peak and reducing the current and arc pressure 10 during the short circuit. For this reason, the pulse peak current needs to be decreased from the start of the pulse peak to the end of the pulse peak.
[0035] Current I at the start of the pulse peak pstart is 300A or more and 600A or less. The current I at the start of the pulse peak pstart If the current I is less than 300 A, the driving force for pushing the droplet 7 down to the molten pool 8 to achieve short-circuit transfer becomes too small, and periodic short-circuit transfer cannot be obtained, which may result in an increase in the number of spatters generated and attached. pstart The current at the start of the pulse peak I pstart is preferably 320 A or more, more preferably 340 A or more, even more preferably 350 A or more, and most preferably 370 A or more. In addition, the current I pstart When the current I exceeds 600 A, the driving force for pushing the droplet 7 down into the molten pool 8 to achieve short-circuit transfer becomes excessive, and the number of spatters generated and attached during short-circuiting increases. pstart The current at the start of the pulse peak, I pstart is preferably 590 A or less. The current I at the start of the pulse peak pstart is more preferably 580 A or less. The current I at the start of the pulse peak pstart The current I at the start of the pulse peak is more preferably 570 A or less. pstart is most preferably 560A or less.
[0036] Current at the end of the pulse peak I pendis 200A or more and 450A or less, and the current I at the end of the pulse peak pend If the current I is less than 200 A, the droplet transfer becomes unstable and periodic short-circuit transfer cannot be achieved, which may result in an increase in the number of spatters and adhesions. pend The current at the end of the pulse peak, I pend is preferably 230 A or more. The current I at the end of the pulse peak pend is more preferably 250 A or more. The current I at the end of the pulse peak pend is more preferably 270 A or more. In addition, the current I pend When the current I exceeds 450 A, the current is high and the arc pressure I is large, so the number of spatters generated and attached at the time of short circuit increases. pend The current at the end of the pulse peak should be 450 A or less. pend is preferably 420A or less. pend is more preferably 400 A or less. pend is more preferably 380A or less.
[0037] Pulse peak time T p is 1.0 ms or more and 3.5 ms or less (optimal conditions) Pulse peak time T p If the pulse peak time T is less than 1.0 ms, the time required to push the droplet 7 down into the molten pool 8 to achieve short-circuit transfer becomes too short, and periodic short-circuit transfer cannot be obtained, which may result in an increase in the number of spatters generated and attached. p The pulse peak time Tp is preferably 1.0 ms or more. The pulse peak time T p More preferably, the pulse peak time T p is most preferably 1.6 ms or more. p If the pulse peak time T exceeds 3.5 ms, the time required to push the droplet 7 down into the molten pool 8 to achieve short-circuit transfer becomes too long, and the short-circuit cannot be achieved at the intended timing, resulting in an increase in the number of spatters generated and attached during the short-circuit.p It is preferable that the pulse peak time T p It is more preferable that the pulse peak time T p The pulse peak time T is more preferably 3.0 ms or less. p is most preferably 2.8 ms or less.
[0038] Peak start current I pstart and the current at the end of the pulse peak I pend , pulse peak time T P satisfies the following formula (2) (favorable condition) 45≦(I pstart -I pend ) / T p ≦210 (2) In formula (2), I pstart (A): Current at the start of the pulse peak, I pend (A): Current at the end of the pulse peak, T p (ms): indicates the pulse peak time. PSTART -I pend ) / T p When the current is less than 45 A / ms or more than 210 A / ms, the stable growth of the droplets 7 necessary for short circuit transfer control and the pressing action of the droplets 7 against the molten pool 8 during short circuit cannot be achieved at the same time, which may cause an increase in the number of spatters and adhesions. pstart -I pend ) / T p It is preferable that the current is 45 A / ms or more. pstart -I pend ) / T p It is more preferable that the current is 60 A / ms or more. pstart -I pend ) / T p More preferably, it is 100 A / ms or more. pstart -I pend ) / T p is most preferably 120 A or more. pstart -I pend ) / T p It is preferable that the current is 210 A / ms or less. pstart -I pend ) / T pIt is more preferable that the current is 190 A / ms or less. pstart -I pend ) / T p More preferably, it is 180 A / ms or less. pstart -I pend ) / T p is most preferably 170 A / ms or less.
[0039] The base current I B is not particularly limited, but if it is too small, the arc discharge in the base period becomes unstable, causing deterioration of the bead shape and insufficient penetration. Therefore, the base current I B is preferably 30 A or more, and more preferably 45 A or more. B If the wire is too large, burn-through may occur, so it is preferably 120 A or less, and more preferably 110 A or less.
[0040] Use of 98% or more Ar gas as shielding gas. If the Ar gas ratio of the shielding gas is less than 98% by volume, the chemical reaction between the oxidizing gas in the shielding gas and the alloying elements contained in the molten metal is accelerated, increasing the amount of slag produced, which reduces corrosion resistance. Therefore, the Ar gas ratio of the shielding gas is set to 98% by volume or more. The Ar gas ratio of the shielding gas is preferably 99% by volume or more. There is no particular upper limit, and the Ar gas ratio may be 100%.
[0041] Furthermore, the present invention can achieve its effects regardless of the shape of the welded joint, such as bead-on-plate welding, butt welding, or fillet welding, or the welding position, such as downward welding or horizontal welding.
[0042] The average frequency (short-circuit frequency) F (Hz) of short-circuiting transfer affects the volume of the droplet 7 at the wire end, and is not particularly limited, but is preferably in the range of 20 Hz to 200 Hz. That is, the average frequency (short-circuit frequency) F (Hz) of short-circuiting transfer is preferably 20 Hz or more, more preferably 30 Hz or more, and even more preferably 40 Hz or more. Furthermore, if the average frequency (short-circuit frequency) F (Hz) of short-circuiting transfer is excessively high, the weld pool 8 is disturbed by re-ignition of the arc 5B due to the short circuit, resulting in an unstable weld bead shape. Therefore, the average frequency (short-circuit frequency) F (Hz) of short-circuiting transfer is preferably 200 Hz or less, more preferably 180 Hz or less, even more preferably 170 Hz or less, and most preferably 150 Hz or less. The average frequency (short-circuit frequency) F (Hz) of short-circuiting transfer can be measured, for example, by monitoring the arc voltage during welding with an oscilloscope, counting the number of times it becomes zero, and dividing the count by the monitoring time to determine the number of counts per second (s). If the monitoring time is too short, the variation in the count number will be large, so it is preferably 0.5 seconds or more. It is more preferable that the monitoring time be 0.8 seconds or more. It is even more preferable that the monitoring time be 1.0 seconds or more. Although there is no particular upper limit, as the volume of measurement data increases, the counting process takes a long time, reducing workability. Therefore, it is preferable that the monitoring time be 3.0 seconds or less. It is more preferable that the monitoring time be 2.8 seconds or less. It is even more preferable that the monitoring time be 2.5 seconds or less.
[0043] The welding wire 1 used in the present invention is not particularly limited. For example, a solid wire for MAG welding as described in JIS Z 3312 can be used.
[0044] The base material 3 of the present invention is intended to be a steel sheet and a plated steel sheet. The chemical composition of the steel sheet is not particularly limited, but a steel sheet containing, for example, 0.02 to 0.3 mass% C, 0.01 mass% or more Si, 0.5% mass% or more Mn, 0.05 mass% or less P, and 0.05 mass% or less S is preferred. Other alloying elements such as Cu, Ni, Cr, and Ti may also be included. In the above steel sheet, the Si content is preferably 3.0 mass% or less, and the Mn content is preferably 5.0 mass% or less. The lower limit of the P content is not particularly limited, but is preferably 0.0005 mass% or more, and the lower limit of the S content is not particularly limited, but is preferably 0.0005 mass% or more. The plating composition of the plated steel sheet is not particularly limited, but may include, for example, Zn.
[0045] Examples of the present invention will be described below. Steel plates (thickness: 2.6 mm) having the components shown in Table 1 were used, and arc welding was carried out by the method shown in Figure 1, for example. Note that the steel plates contained alloy elements such as Fe, Cu, Ni, Cr, and Ti as components other than those shown in Table 1. Welding was carried out under the welding conditions shown in Table 2. The welding wire 1 used in the present invention is not particularly limited. For example, a solid wire for MAG welding as specified in JIS Z 3312 can be used.
[0046] The welded steel plates obtained as described above were evaluated for the number of spatter deposits, the slag coverage area ratio, and the corrosion resistance of the welds according to the following test methods.
[0047] (Number of spatter deposits) Figure 4 is a schematic diagram showing the measurement range for the number of spatter deposits. The number of spatter deposits was measured by photographing the surface of the area excluding the weld bead start and end terminals 20 (each 15 mm long) and analyzing the photographs. When the length of the weld bead 6 was less than 130 mm, the entire surface excluding the weld bead start and end terminals 20 was photographed. When the length of the weld bead 6 was 130 mm or more, the surface of any portion (100 mm long) excluding the weld bead start and end terminals 20 was photographed. The measurement range was the weld spatter affected zone 21. Specifically, the weld spatter affected zone 21 was a range whose length in the weld line direction 23 was the length of the weld bead 6 excluding each 15 mm of the weld bead start and end terminals 20 and whose length in the direction perpendicular to the weld line was 40 mm centered on the centerline of the weld bead 6. The number of spatter deposits 22 deposited in this range and whose maximum length of the deposition area was 0.2 mm or more was counted. The spatter deposit count was 0.50 spatter deposits / cm. 2 The following were considered successful:
[0048] (Slag Coverage Area Ratio) Fig. 5 is a schematic diagram showing the bead area and the slag covered area of a weld bead. BEAD and the slag-covered surface area S SLAG is calculated by photographing the surface of the area of the weld bead 6 excluding the start and end portions 20 (each 15 mm long) from directly above, and measuring the projected area from the top of the weld bead 6 and slag. If the length of the weld bead 6 is less than 130 mm, the entire surface is photographed excluding the start and end portions 20 of the weld bead. If the length of the weld bead 6 is 130 mm or more, the surface of any portion (100 mm long) excluding the start and end portions 20 of the weld bead is photographed. The calculated slag surface area S SLAG The value of the bead surface area S BEAD The slag coverage area ratio S RATIO I asked for S. RATIO A value of 15% or less was considered acceptable.
[0049] (Evaluation of corrosion resistance of welded joints) First, the arc-welded joints after the corrosion test were immersed in an immersion stripper to remove the electrodeposition coating, and then the corrosion products were removed in accordance with ISO 8407. Next, when the weld bead 6 included the weld bead start and end portions 20 (each 15 mm long), the surface of the area excluding the weld bead start and end portions 20 was photographed, and the photographs were analyzed to determine the maximum corrosion width H from the bead toe in the direction perpendicular to the weld line. MAX When the length of the weld bead 6 was less than 130 mm, the entire surface was photographed, excluding the start and end portions 20 of the weld bead. When the length of the weld bead 6 was 130 mm or more, the surface of any portion (100 mm long) was photographed, excluding the start and end portions 20 of the weld bead. The corrosion resistance was evaluated based on the maximum corrosion width H MAX When the maximum corrosion width H is less than 6.0 mm, it is judged to be excellent in corrosion resistance and is marked with "○". MAX When the maximum corrosion width H is less than 4.5 mm, it is judged to be more excellent in corrosion resistance and is marked with "◎", and when it is 6.0 mm or more, it is judged to be poor in corrosion resistance and is marked with "×". MAX The maximum corrosion width H MAX The maximum corrosion width H MAX A value of 6.0 mm or more was evaluated as "×", "◯" and "◎" indicated that the target was achieved, and "×" indicated that the target was not achieved.
[0050] As is clear from Table 2, welds No. 1 to 7 and 15 to 21 shown as examples of the invention are S RATIO is 15% or less and the number of spatter deposits is 0.50 / cm 2 The results were as follows: a welded joint with excellent corrosion resistance was obtained.
[0051] Among these invention examples, welds No. 1 to 5, 16, 19, and 20 are S RATIO is 15% or less and the number of spatter deposits is 0.45 / cm 2 The welded joint shape was superior in corrosion resistance.
[0052] In contrast, the comparative welding Nos. 8 to 14 and 22 were S RATIO is greater than 15%, or the number of spatter deposits is 0.50 / cm 2 No larger, better corrosion resistant weld joints were obtained.
[0053] In Table 2, "S RATIO is 15% or less and the number of spatter deposits is 0.45 / cm 2 In the following, "corrosion resistance" is evaluated as "A" and "S" is evaluated as " RATIO is 15% or less and the number of spatter deposits is 0.45 / cm 2 Larger than 0.50 pieces / cm 2 If the corrosion resistance is "0" or less, the evaluation is B. RATIO is greater than 15%, or the number of sputter deposits is 0.50 / cm 2 If the corrosion resistance was greater than 100%, or the corrosion resistance was x, the evaluation was F. Evaluation F was determined as a failure, and evaluations A and B were determined as passing.
[0054]
[0055]
[0056] REFERENCE SIGNS LIST 1 welding wire 2 welding torch 3 base metal 5B arc 6 weld bead 7 droplet 8 molten pool 10 arc pressure 20 weld bead start and end portions 21 weld spatter affected area 22 spatter 23 weld line direction T P Pulse peak current time I PSTART Current at the start of the pulse peak I PEND Current at the end of the pulse peak I B Base current S BEAD Bead surface area S SLAG Slag Coverage Surface Area
Claims
1. An arc welded joint manufactured by arc welding, the arc welded joint having a base material, a weld bead formed by mixing and solidifying the base material and welding wire melted by heat input from an arc, and a weld heat affected zone, the length in the weld line direction being the length of the weld bead excluding 15 mm each at the start and end of the weld bead, and the length in the direction perpendicular to the weld line being 40 mm centered on the center line of the weld bead, the number of spatters generated during welding and adhering to the weld spatter affected zone, with a maximum length of the adhering area being 0.2 mm or more, is 0.50 spatters / cm 2 and the bead surface area S of the weld bead surface BEAD and the bead surface area S BEAD The slag surface area S is the area of the region covered by the slag. SLAG The slag coverage area ratio S is calculated using the following formula (1) RATIO An arc welded joint, in which the difference is 15% or less. RATIO =S SLAG / S BEAD × 100 (1) In formula (1), S BEAD (mm 2 ): bead surface area, S SLAG (mm 2 ): slag surface area, which is the area of the region covered by the slag, S RATIO (%): Slag coverage area ratio.
2. A method for manufacturing an arc welded joint according to claim 1, comprising the steps of: short-circuiting a welding wire and a base metal to form a joint; and pulse welding in which a pulse peak current and a base current are periodically repeated, and an average welding current I AVE is 100 A or more and 320 A or less, the pulse peak current decreases from the start of the pulse peak to the end of the pulse peak, and the current I pstart is 300A or more and 600A or less, and the current I at the end of the pulse peak pend a current flow rate of 200 A or more and 450 A or less, and Ar gas having a volume percentage of 98% or more is used as a shielding gas during welding.
3. In the pulse welding, the pulse peak time T p is 1.0 ms or more and 3.5 ms or less, and the current I pstart , the current I at the end of the pulse peak pend , the pulse peak time T p The method for manufacturing an arc welded joint according to claim 2, wherein the following formula (2) is satisfied: 45≦(I pstart -I pend ) / T p ≦210 (2) In formula (2), I pstart (A): Current at the start of the pulse peak, I pend (A): Current at the end of the pulse peak, T p (ms): Indicates the pulse peak time.
Citation Information
Patent Citations
Gas shielded metal arc welding method which enhances corrosion resistance after coating of weld zone and near this zone
JP1996033997A
Improvement of corrosion resistance after coating in arc weld zone and its vicinity
JP1997020994A
Method for chemical treatment of steel members, method for manufacturing coated steel members with electrodeposition coating, and coated steel members
JP5549615B2
Pulsed MIG welding method
JP2005262250A
Welding power source
JP2014136225A