Positive electrode active material and lithium ion secondary battery
The development of a Li-containing oxide with a minimized T#2 type structure in the O2 type structure addresses capacity limitations in lithium ion secondary batteries, enhancing energy storage through a targeted manufacturing process.
Patent Information
- Application Number
- PCT/JP2024/009926
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional positive electrode active materials with an O2 type structure for lithium ion secondary batteries have limitations in capacity due to the presence of a significant T#2 type structure, which affects their performance.
A Li-containing oxide with an O2 type structure, containing elements like Mn, Ni, Co, and O, is developed, where the X-ray diffraction peak intensity ratio from the T#2 structure to the O2 structure is minimized to enhance capacity, achieved through a specific manufacturing method involving ion-exchange and firing processes.
The Li-containing oxide with a reduced T#2 type structure exhibits improved capacity and performance as a positive electrode active material in lithium ion secondary batteries, leading to increased energy storage capabilities.
Smart Images

Figure JP2024009926_31102024_PF_FP_ABST
Abstract
Description
Positive electrode active material and lithium ion secondary battery
[0001] The present application discloses a positive electrode active material and a lithium ion secondary battery.
[0002] Positive electrode active materials having an O2-type structure are known. As disclosed in Patent Document 1, a positive electrode active material having an O2-type structure is obtained by ion-exchanging at least a portion of Na in a sodium-containing oxide having a P2-type structure with Li.
[0003] JP 2011-170994 A
[0004] Conventional positive electrode active materials having an O2-type structure have room for improvement in terms of capacity.
[0005] The present application discloses the following aspects as means for solving the above problems: <Aspect 1> A positive electrode active material, comprising a Li-containing oxide, the Li-containing oxide having an O2-type structure, the Li-containing oxide containing at least one element selected from Mn, Ni, and Co, Li, and O as constituent elements, and an X-ray diffraction pattern of the Li-containing oxide having a refractive index of 0≦I 1 / I 2 ≦0.30, 1 is the X-ray diffraction peak intensity derived from the (002) plane of the T#2 type structure, 2 is an X-ray diffraction peak intensity derived from the (002) plane of the O2 type structure. <Aspect 2> The cathode active material of aspect 1, wherein the Li-containing oxide is Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2(where 0<a≦1.00, 0≦b≦0.20, x+y+z=1, and 0≦p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.) <Aspect 3> The cathode active material of Aspect 1 or 2, wherein the Li-containing oxide contains at least Li, Mn, Ni, Co, and O as constituent elements. <Aspect 4> A lithium ion secondary battery, comprising a cathode active material layer, an electrolyte layer, and an anode active material layer, wherein the cathode active material layer contains the cathode active material of any of Aspects 1 to 3.
[0006] The positive electrode active material of the present disclosure has an O2 type structure and has a large capacity.
[0007] 1 shows an example of the flow of a method for producing a Li-containing oxide having an O2-type structure. 2 shows a schematic diagram of an example of the configuration of a lithium ion secondary battery. 3 shows the X-ray diffraction patterns of Examples 1 and 2 and Comparative Examples 1 and 2. 1 / I 2 The relationship between the capacitance and the power consumption is shown.
[0008] 1. Positive Electrode Active Material The positive electrode active material according to the embodiment includes a Li-containing oxide. The Li-containing oxide has an O2-type structure. The Li-containing oxide includes, as constituent elements, at least one element selected from Mn, Ni, and Co, Li, and O. The X-ray diffraction pattern of the Li-containing oxide has a refractive index of 0≦I 1 / I 2 ≦0.30. 1 is the X-ray diffraction peak intensity derived from the (002) plane of the T#2 type structure, and 2 is the X-ray diffraction peak intensity derived from the (002) plane of the O2 type structure.
[0009] 1.1 Crystal Structure The Li-containing oxide according to the embodiment has at least an O2-type structure (belonging to space group P63mc) as a crystal structure. The Li-containing oxide according to the embodiment has an O2-type structure and may have a crystal structure other than the O2-type structure. Examples of crystal structures other than the O2-type structure include a T#2-type structure (belonging to space group Cmca) formed when Li is deintercalated from an O2-type structure, and an O6-type structure (belonging to space group R-3m, with a c-axis length of 2.5 nm to 3.5 nm, typically 2.9 nm to 3.0 nm, and different from the O3-type structure also belonging to space group R-3m). However, as will be described later, the Li-containing oxide according to the embodiment has a small amount of the T#2-type structure. The Li-containing oxide according to the embodiment may have an O2-type structure as a main phase, or may have a crystal structure other than the O2-type structure (for example, an O6-type structure) as a main phase. However, the crystal structure serving as the main phase of the Li-containing oxide according to the embodiment may change depending on the charge / discharge state.
[0010] 1.1.1 X-ray diffraction peak intensity The X-ray diffraction pattern of the Li-containing oxide according to the embodiment has a peak intensity of 0≦I 1 / I 2 ≦0.30. 1 is the X-ray diffraction peak intensity derived from the (002) plane of the T#2 type structure, and 2 is the X-ray diffraction peak intensity derived from the (002) plane of the O2 type structure.
[0011] In conventional O2-type positive electrode active materials, a T#2-type structure is inevitably generated along with the O2-type structure, and the X-ray diffraction peak intensity derived from the T#2 structure is large. In the prior art, sufficient consideration has not been given to reducing this T#2-type structure. In contrast, the Li-containing oxide according to the embodiment employs the synthesis conditions described below, thereby reducing the X-ray diffraction peak intensity I derived from the O2-type structure. 2 is the X-ray diffraction peak intensity I 1Here, according to the findings of the present inventors, in the X-ray diffraction pattern of a Li-containing oxide, the lower the X-ray diffraction peak derived from the T#2 type structure is relative to the X-ray diffraction peak derived from the O2 type structure, the greater the capacity as a positive electrode active material.
[0012] In the X-ray diffraction pattern of the Li-containing oxide according to the embodiment, the X-ray diffraction peak intensity I 1 and the X-ray diffraction peak intensity I originating from the (002) plane of the O2 type structure. 2 Relative to I 1 / I 2 However, 0≦I 1 / I 2 The X-ray diffraction pattern satisfies 0≦I≦0.30. 1 / I 2 ≦0.27, 0≦I 1 / I 2 ≦0.25, 0≦I 1 / I 2 ≦0.23, 0≦I 1 / I 2 ≦0.20, 0≦I 1 / I 2 ≦0.17, 0≦I 1 / I 2 ≦0.15, 0≦I 1 / I 2 ≦0.13, 0≦I 1 / I 2 ≦0.10, 0≦I 1 / I 2 ≦0.05, 0≦I 1 / I 2 ≦0.01, or I 1 / I 2 = 0 may be satisfied.
[0013] 1.1.2 Method for Measuring X-ray Diffraction Peak Intensity In the present application, the terms "X-ray diffraction pattern of a Li-containing oxide" and "X-ray diffraction peak intensity" refer to those obtained under the following conditions. That is, an X-ray diffraction pattern is obtained by performing 2θ / θ scanning on a Li-containing oxide using an X-ray diffractometer (Rigaku, fully automatic multipurpose X-ray diffractometer SmartLab) with CuKα as the radiation source, a tube voltage of 45 kV, a tube current of 200 mA, a step width of 0.02°, and a scan speed of 1° / min. In the X-ray diffraction pattern, an X-ray diffraction peak derived from the (002) plane of the T#2 structure and an X-ray diffraction peak derived from the (002) plane of the O2 structure are identified, and the background value near the peaks is subtracted from the X-ray diffraction pattern. The above I is then calculated from the intensity of each X-ray diffraction peak. 1 / I 2 can be obtained.
[0014] 1.1.3 Crystallites The Li-containing oxide according to one embodiment may be a single crystal consisting of one crystallite, or a polycrystal having multiple crystallites. For example, the surface of the Li-containing oxide according to one embodiment may be composed of multiple crystallites. In other words, the Li-containing oxide may have a structure in which multiple crystallites are connected to each other on its surface. When the surface of the Li-containing oxide is composed of multiple crystallites, grain boundaries are present on the surface. Here, the grain boundaries may serve as inlets and outlets for intercalation. That is, when the Li-containing oxide is polycrystalline having multiple crystallites, the effects of increasing the number of inlets and outlets for intercalation, reducing reaction resistance, shortening the migration distance of lithium ions, reducing diffusion resistance, and reducing the absolute amount of expansion and contraction during charge and discharge, making cracking less likely, can be expected. The crystallite size may be large or small, but it is believed that smaller crystallite sizes result in more grain boundaries, making the above-mentioned advantageous effects more likely to be exhibited. For example, when the diameter of the crystallites constituting the Li-containing oxide is less than 1 μm, higher performance is likely to be obtained. The "crystallite" and "crystallite diameter" can be determined by observing the surface of the Li-containing oxide using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, when the surface of the Li-containing oxide is observed and a single closed region surrounded by a grain boundary is observed, the region is considered to be a "crystallite." The maximum Feret diameter of the crystallite is determined and considered to be the "crystallite diameter." If the Li-containing oxide is composed of a single crystal, the particle itself can be considered to be a single crystallite, and the maximum Feret diameter of the particle is the "crystallite diameter." Alternatively, the crystallite diameter can be determined by EBSD or XRD. For example, the crystallite diameter can be determined based on the Scherrer equation from the half-width of the diffraction line of the XRD pattern. When the crystallite diameter of a Li-containing oxide determined by any of these methods is less than 1 μm, higher performance is likely to be exhibited. The crystallites constituting the lithium-containing oxide may have a first surface exposed on the surface of the oxide, and the first surface may be planar. That is, the surface of the lithium-containing oxide may have a structure in which a plurality of planes are connected.As described below, when producing a Na-containing oxide that is a raw material for a Li-containing oxide, crystallites having a planar first surface can be easily obtained by growing the crystallites on the surface of the particles until one crystallite and another crystallite are connected to each other.
[0015] 1.2 Chemical Composition The Li-containing oxide according to one embodiment contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Li, and O. When the Li-containing oxide contains, as constituent elements, at least Li, Mn, one or both of Ni and Co, and O, in particular, when the Li-containing oxide contains, as constituent elements, at least Li, Mn, Ni, Co, and O, higher performance is likely to be obtained.
[0016] In one embodiment, the Li-containing oxide having an O2 structure is Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2(wherein 0<a≦1.00, 0≦b≦0.20, x+y+z=1, and 0≦p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.) When the Li-containing oxide has such a chemical composition, the O2-type structure is easily maintained. In the above chemical composition, a is greater than 0, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, or 0.70 or less. In the above chemical composition, b may be 0 or more, 0.01 or more, 0.02 or more, or 0.03 or more, and may be 0.20 or less, 0.15 or less, or 0.10 or less. Also, x may be 0 or more, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. Also, y may be 0 or more, 0.10 or more, or 0.20 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. Furthermore, z is 0 or more, and may be 0.10 or more, 0.20 or more, or 0.30 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. Element M has a small contribution to charge and discharge. In this regard, in the above chemical composition, when p + q + r is less than 0.17, high charge and discharge capacity is easily ensured. p + q + r may be 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, or 0.10 or less. On the other hand, the inclusion of element M makes it easy to stabilize the O2-type structure. In the above chemical composition, p+q+r is 0 or more, and may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more.The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.
[0017] 1.3 Shape As described below, a Li-containing oxide having an O2-type structure can be obtained by substituting Li for Na in a Na-containing oxide having a P2-type structure. Here, the P2-type structure is a hexagonal crystal system with a large diffusion coefficient of Na ions, and crystals are likely to grow in a specific direction. In particular, when at least one of Mn, Ni, and Co is included as a transition metal element constituting the P2-type structure, plate-like crystals are likely to grow in a specific direction. Therefore, a Na-containing oxide having a P2-type structure typically becomes a plate-like particle with a large aspect ratio, in which the crystal growth direction is biased in a specific direction. The Li-containing oxide according to one embodiment may be obtained based on such plate-like Na-containing oxide particles, or, as described below, may be obtained based on spherical Na-containing oxide particles. That is, the shape of the Li-containing oxide may be either a plate-like particle or a spherical particle. When the Li-containing oxide is a spherical particle, the reaction resistance decreases due to a reduction in crystallite size, and the diffusion resistance inside the particle is likely to decrease. Furthermore, when applied to secondary batteries, etc., it is believed that the degree of curvature is reduced by spheroidization, and the lithium ion conduction resistance is reduced. As a result, for example, rate characteristics are improved and the reversible capacity is likely to increase. In this application, "spherical particles" refers to particles having a circularity of 0.80 or more. The circularity of the particles may be 0.81 or more, 0.82 or more, 0.83 or more, 0.84 or more, 0.85 or more, 0.86 or more, 0.87 or more, 0.88 or more, 0.89 or more, or 0.90 or more. The circularity of the particles is 4πS / L 2 where S is the orthogonal projected area of the particle, and L is the perimeter of the orthogonal projected image of the particle. The circularity of a particle can be determined by observing the appearance of the particle using a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an optical microscope. When the particle consists of more than 100 particles, the circularity is measured, for example, as an average value as follows.
[0018] (1) First, the particle size distribution of the particles is measured. Specifically, the particle diameter (D10) at 10% of the cumulative value in the volume-based particle size distribution and the particle diameter (D90) at 90% of the cumulative value are determined by laser diffraction / scattering. (2) The appearance of the particles whose particle size distribution has been measured is observed using an image of an SEM, TEM, or optical microscope, and 100 particles having a circle-equivalent diameter (the diameter of a circle having the same area as the orthogonal projection area of the particle) equal to or greater than the D10 and equal to or less than the D90 determined in (1) are randomly selected from the images. (3) The circularity of each of the extracted particles is determined by image processing, and the average value is regarded as the "circularity of the particle."
[0019] The Li-containing oxide according to one embodiment may be a solid particle, a hollow particle, or a particle having voids. The size of the Li-containing oxide particles is not particularly limited, but a smaller size is considered to be advantageous. For example, the average particle diameter (D50) of the Li-containing oxide particles may be 0.1 μm or more and 10 μm or less, 1.0 μm or more and 8.0 μm or less, or 2.0 μm or more and 6.0 μm or less. The average particle diameter (D50) is the particle diameter (D50, median diameter) at 50% cumulative volume in a particle size distribution determined by a laser diffraction / scattering method.
[0020] 1.4 Others As described above, the cathode active material according to the embodiment has a large capacity due to the inclusion of the specific Li-containing oxide. The cathode active material according to the embodiment may consist solely of the Li-containing oxide, or may contain the Li-containing oxide together with other cathode active materials (other cathode active materials). From the viewpoint of further enhancing the above-described effects, the proportion of the other cathode active materials in the entire cathode active material may be small. For example, the content of the Li-containing oxide may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less, where the entire cathode active material is taken as 100% by mass.
[0021] 2. Method for Producing Positive Electrode Active Material The Li-containing oxide according to the above embodiment can be produced, for example, by the following method. As shown in Figure 1, a method for producing a Li-containing oxide having an O2-type structure according to one embodiment includes: S1: obtaining a precursor containing at least one element selected from Mn, Ni, and Co; S2: coating the surface of the precursor with a Na source to obtain a composite; S3: calcining the composite to obtain a Na-containing oxide having a P2-type structure; and S4: ion-exchanging at least a portion of the Na in the Na-containing oxide with Li to obtain a Li-containing oxide having an O2-type structure. Here, S3 includes the following steps: S3-1: subjecting the composite to pre-baking at a temperature of 300°C or higher and lower than 700°C for 2 hours or longer and 10 hours or shorter; S3-2: following the pre-baking, subjecting the composite to main baking at a temperature of 700°C or higher and 1100°C or lower for 30 minutes or longer and 48 hours or shorter; and S3-3: following the main baking, subjecting the composite to a temperature T 1 from a temperature T below 100°C 2 and rapidly cooling the material until the temperature reaches a temperature of 1000.degree.
[0022] 2.1 S1 In S1, a precursor containing at least one element selected from Mn, Ni, and Co is obtained. The precursor may contain at least Mn and one or both of Ni and Co, or may contain at least Mn, Ni, and Co. The precursor may be a salt containing at least one element selected from Mn, Ni, and Co. For example, the precursor may be at least one of carbonate, sulfate, nitrate, and acetate. Alternatively, the precursor may be a compound other than a salt. For example, the precursor may be a hydroxide. The precursor may be a hydrate. The precursor may be a combination of multiple compounds. The precursor may have various shapes. For example, the precursor may be particulate, or may be spherical as described below. The particle size of the precursor particles is not particularly limited.
[0023] In step S1, a precipitate as the precursor may be obtained by coprecipitation using an ion source capable of forming a precipitate in an aqueous solution with transition metal ions and a transition metal compound containing at least one element selected from Mn, Ni, and Co. This facilitates the production of spherical particles as the precursor. The "ion source capable of forming a precipitate in an aqueous solution with transition metal ions" may be, for example, at least one selected from sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide, and sodium oxide. The transition metal compound may be the above salt or hydroxide containing at least one element selected from Mn, Ni, and Co. Specifically, in step S1, the ion source and the transition metal compound may be prepared as separate solutions, and then the respective solutions may be added dropwise and mixed to obtain the precipitate as the precursor. In this case, water may be used as the solvent. Various sodium compounds may be used as bases, and aqueous ammonia or the like may be added to adjust the basicity. In the case of the coprecipitation method, for example, an aqueous solution of the transition metal compound and an aqueous solution of sodium carbonate are prepared, and the respective aqueous solutions are added dropwise and mixed to obtain the precipitate as the precursor. Alternatively, the precursor can be obtained by a sol-gel method, and in particular, by a coprecipitation method, spherical particles can be easily obtained as the precursor.
[0024] In step S1, the precursor may contain element M. Element M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. These elements M have the function of stabilizing, for example, the P2-type structure or the O2-type structure. The method for obtaining a precursor containing element M is not particularly limited. When obtaining a precursor by coprecipitation in step S1, for example, an aqueous solution of a transition metal compound containing at least one of Mn, Ni, and Co, an aqueous solution of sodium carbonate, and an aqueous solution of a compound of element M are prepared, and the respective aqueous solutions are added dropwise and mixed to obtain a precursor containing element M together with at least one element of Mn, Ni, and Co. Alternatively, in the manufacturing method of the present disclosure, element M may not be added in step S1, and element M may be doped during the Na-doping calcination in steps S2 and S3 described below.
[0025] 2.2 S2 In S2, the surface of the precursor obtained in S1 is coated with a Na source to obtain a composite. The Na source may be a salt containing Na, such as a carbonate or a nitrate, or a compound other than a salt, such as sodium oxide or sodium hydroxide. In S2, the amount of Na source coated on the surface of the precursor may be determined taking into account the amount of Na lost during the subsequent calcination.
[0026] In S2, the coverage of the Na source with respect to the surface of the precursor is not particularly limited. For example, in S2, the composite may be obtained by coating 40 area% or more, 50 area% or more, 60 area% or more, or 70 area% or more of the surface of the precursor with the Na source. Here, when the precursor obtained in S1 is a spherical particle and the composite obtained in S2 is obtained by coating 40 area% or more of the surface of the precursor with the Na source, the Na-containing oxide having a P2-type structure is likely to become spherical particles in S3 described below. If the coverage of the Na source is small, when the composite is fired, P2-type crystals are likely to grow on the surface of the composite, and the Na-containing oxide is likely to become plate-like. If the coverage of the Na source is large, when the composite is fired, the crystallites of the P2-type crystals are likely to become small, and the Na-containing oxide is likely to become spherical particles corresponding to the shape of the precursor.
[0027] In S2, the method for coating the surface of the precursor with the Na source is not particularly limited. As described above, when 40% or more of the area of the precursor surface is to be coated with the Na source, various methods can be used. For example, a tumbling fluidized coating method or a spray drying method can be used. That is, a coating solution in which a Na source is dissolved is prepared, and the coating solution is brought into contact with the surface of the precursor, and the precursor is dried at the same time as or after the contact. By adjusting the coating conditions (temperature, time, number of times, etc.), it is possible to coat 40% or more of the area of the precursor surface with the Na source.
[0028] In S2, the precursor may be coated with an M source together with the Na source. For example, in S2, the composite may be obtained by mixing the precursor obtained in S1 with a Na source and an M source containing at least one element M selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. The M source may be, for example, a salt containing the element M, such as a carbonate or a sulfate, or a compound other than a salt, such as an oxide or a hydroxide. The amount of the M source relative to the precursor may be determined depending on the chemical composition of the Na-containing oxide after firing.
[0029] 2.3 S3 In S3, the composite obtained in S2 is fired to obtain a Na-containing oxide having a P2-type structure. S3 includes the above S3-1, S3-2, and S3-3.
[0030] 2.3.1 S3-1 In S3-1, the composite is pre-fired at a temperature of 300°C or higher and lower than 700°C for 2 hours to 10 hours. In S3-1, the composite may be optionally shaped and then pre-fired. The pre-fired temperature is lower than that of the main firing. If the pre-fired temperature in S3-1 is insufficient, the P2 phase may not be sufficiently formed in the finally obtained Na-containing oxide. In S3-1, the pre-fired temperature is 300°C or higher and lower than 700°C, and the pre-fired time is 2 hours to 10 hours, so that the composite can be sufficiently pre-fired, the heat uniformity is improved, and the Na-containing oxide obtained through S3-2 and S3-3 described below becomes appropriate, and the Li-containing oxide having an O2-type structure obtained through S4 becomes the above-mentioned I phase. 1 / I 2 The pre-firing temperature may be 400°C or higher and lower than 700°C, 450°C or higher and lower than 700°C, 500°C or higher and lower than 700°C, 550°C or higher and lower than 700°C, or 550°C or higher and lower than 650°C. The pre-firing time may be 2 hours or higher and lower than 8 hours, 3 hours or higher and lower than 8 hours, 4 hours or higher and lower than 8 hours, 5 hours or higher and lower than 8 hours, or 5 hours or higher and lower than 7 hours. The pre-firing atmosphere is not particularly limited, and may be, for example, an oxygen-containing atmosphere.
[0031] 2.3.2 S3-2 In S3-2, following the pre-firing, the composite is subjected to main firing at a temperature of 700°C to 1100°C for 30 minutes to 10 hours. In S3-2, the main firing temperature of the composite is 700°C to 1100°C, preferably 800°C to 1000°C. If the main firing temperature is too low, the P2 phase will not be formed, while if the main firing temperature is too high, an O3 phase or the like will likely form instead of the P2 phase. The temperature rise conditions from the pre-firing temperature to the main firing temperature are not particularly limited. The main firing time is not particularly limited and may be, for example, 30 minutes to 48 hours. However, the shape of the Na-containing oxide can be controlled by the main firing time. As described above, in the method of the present disclosure, if the coverage of the Na source in the composite is 40 area% or more, P2-type crystals with small crystallites are likely to form on the surface of the composite when the composite is fired. In the method of the present disclosure, P2 type crystals are grown along the surface of the particles so as to connect one P2 type crystallite to another, thereby making the shape of the Na-containing oxide correspond to the shape of the precursor. For example, if the precursor is a spherical particle, the Na-containing oxide can also be a spherical particle. If the firing time is too short, the P2 phase is not sufficiently generated. On the other hand, if the firing time is too long, the P2 phase grows excessively, resulting in plate-like particles rather than spherical ones. As far as the inventors have confirmed, spherical particles of Na-containing oxide are easily obtained when the firing time is 30 minutes or more and 3 hours or less. The Na-containing oxide obtained after firing may have a structure in which multiple crystallites are present on the surface and the crystallites are connected to each other.
[0032] 2.3.3 S3-3 In S3-3, following the main sintering, the composite is heated to a temperature T 1 from a temperature T below 100°C 2 The pre-baking and main baking are carried out, for example, in a heating furnace. In step S3-3, for example, after the main baking of the composite in the heating furnace, the composite is baked at an arbitrary temperature T 1 Cool to the temperature T 1After that, the fired product is removed from the heating furnace and heated to an arbitrary temperature T 2 Rapid cooling is performed outside the furnace until the temperature T 1 is any temperature above 200°C, and may be any temperature above 250°C. 2 is any temperature below 100°C, may be any temperature below 50°C, or may be the cooling end temperature. 1 From temperature T 2 In a predetermined temperature range between the temperatures above 200°C and 200°C, moisture is likely to penetrate between the layers of the P2 type structure due to atomic vibrations, molecular motion, etc. When the composite (Na-containing oxide having a P2 type structure) is cooled after the sintering, it is thought that the amount of moisture that penetrates between the layers of the P2 type structure can be reduced by shortening the time it takes to reach this temperature range where moisture is likely to penetrate (i.e., by performing high-speed cooling). In this regard, in step S3-3, when the composite after the sintering is cooled, it is possible to reduce the amount of moisture that penetrates between the layers of the P2 type structure by setting the temperature to an arbitrary temperature T 1 Any temperature T below 100°C 2 For example, by cooling in a dry atmosphere outside the furnace, the temperature T 1 From temperature T 2 The cooling rate during the cooling process is high (for example, 20°C / min or more) until the temperature reaches 100°C, which makes it difficult for moisture to penetrate between the layers of the P2 type structure, and it is possible to suppress the collapse of the P2 type structure. As a result, Na can be efficiently ion-exchanged with Li in S4, and the Li-containing oxide having an O2 type structure obtained through S4 can be obtained by the above-mentioned I 1 / I 2 It is likely to satisfy the above.
[0033] By the above method, it is possible to produce a Na-containing oxide having a P2 type structure and a predetermined chemical composition. The Na-containing oxide contains, as constituent elements, at least one transition metal element selected from Mn, Ni, and Co, Na, and O. In particular, when the constituent elements contain at least Na, Mn, at least one of Ni and Co, and O, and especially when the constituent elements contain at least Na, Mn, Ni, Co, and O, the performance of the positive electrode active material particles is likely to be further improved. The Na-containing oxide contains Na c Mn x-p Niy-q Co z-r M p+q+r O 2 The Na-containing oxide may have a chemical composition represented by the formula: where 0<c≦1.00, x+y+z=1, and 0≦p+q+r<0.17. M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. When the Na-containing oxide has such a chemical composition, the P2 structure is more easily maintained. In the above chemical composition, c may be greater than 0, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, or 0.70 or less. x is 0 or more, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. y is 0 or more, 0.10 or more, or 0.20 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. z is 0 or more, 0.10 or more, 0.20 or more, or 0.30 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. The element M has a small contribution to charge and discharge. In this regard, in the above chemical composition, when p + q + r is less than 0.17, a high charge and discharge capacity is easily ensured. p + q + r may be 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, or 0.10 or less. On the other hand, the inclusion of the element M makes it easy to stabilize the P2 type structure and the O2 type structure. In the above chemical composition, p + q + r is 0 or more, and may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.
[0034] 2.4 S4 In S4, at least a portion of the Na in the Na-containing oxide obtained in S3 is ion-exchanged with Li to obtain a Li-containing oxide having an O2-type structure. Ion exchange can be performed, for example, using an aqueous solution containing lithium halide or using a mixture of lithium halide and other lithium salts (e.g., molten salt). Of the two methods, the method using molten salt is preferred from the viewpoint that the P2-type structure is easily broken by the penetration of water and from the viewpoint of crystallinity. That is, by mixing the Na-containing oxide having the P2-type structure with the molten salt and heating the mixture to a temperature equal to or higher than the melting point of the molten salt, at least a portion of the Na in the Na-containing oxide can be ion-exchanged with Li.
[0035] The lithium halide constituting the molten salt is preferably at least one of lithium chloride, lithium bromide, and lithium iodide. The other lithium salt constituting the molten salt is preferably lithium nitrate. By using the molten salt, the melting point becomes lower than when lithium halide or other lithium salt is used alone, and ion exchange can be performed at a lower temperature.
[0036] The temperature for ion exchange may be, for example, equal to or higher than the melting point of the molten salt and equal to or lower than 600°C, 500°C, 400°C, or 300°C. If the temperature for ion exchange is too high, the stable O3 structure is likely to be formed rather than the O2 structure. On the other hand, from the viewpoint of shortening the time required for ion exchange, it is preferable that the temperature for ion exchange is as high as possible.
[0037] 3. Lithium-ion secondary battery The positive electrode active material according to the embodiment includes the specific Li-containing oxide described above. The positive electrode active material according to the embodiment can be used, for example, as the positive electrode active material of a lithium-ion secondary battery. FIG. 2 schematically shows the configuration of a lithium-ion secondary battery according to an embodiment. As shown in FIG. 2, a lithium-ion secondary battery 100 according to an embodiment has a positive electrode active material layer 10, an electrolyte layer 20, and a negative electrode active material layer 30. Here, the positive electrode active material layer 10 includes the positive electrode active material according to the embodiment described above.
[0038] 3.1 Positive Electrode Active Material Layer The positive electrode active material layer 10 includes at least the positive electrode active material according to the above embodiment and may further include, optionally, an electrolyte, a conductive additive, a binder, and the like. Furthermore, the positive electrode active material layer 10 may also include various other additives. The respective contents of the positive electrode active material, electrolyte, conductive additive, binder, and the like in the positive electrode active material layer 10 may be appropriately determined depending on the desired battery performance. For example, the content of the positive electrode active material may be 40% by mass or more, 50% by mass or more, or 60% by mass or more, or 100% by mass or less, or 90% by mass or less, where the entire positive electrode active material layer 10 (total solid content) is taken as 100% by mass. The shape of the positive electrode active material layer 10 is not particularly limited, and may be, for example, a sheet-like positive electrode active material layer 10 having a substantially flat surface. The thickness of the positive electrode active material layer 10 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and 2 mm or less or 1 mm or less.
[0039] 3.1.1 Positive Electrode Active Material The positive electrode active material is as described above. That is, the positive electrode active material includes a Li-containing oxide, which has an O2-type structure and contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Li, and O. 1 / I 2 As described above, the positive electrode active material may be composed solely of the Li-containing oxide, or may contain the Li-containing oxide and other positive electrode active materials (other positive electrode active materials). From the viewpoint of further enhancing the effects of the technology of the present disclosure, the proportion of the other positive electrode active materials in the entire positive electrode active material may be small. For example, when the entire positive electrode active material is taken as 100 mass%, the content of the Li-containing oxide may be 50 mass% to 100 mass%, 60 mass% to 100 mass%, 70 mass% to 100 mass%, 80 mass% to 100 mass%, 90 mass% to 100 mass%, 95 mass% to 100 mass%, or 99 mass% to 100 mass%.
[0040] The other positive electrode active material may be any of those known as positive electrode active materials for lithium-ion secondary batteries. The other positive electrode active material may be, for example, at least one selected from various lithium compounds other than the above-mentioned Li-containing oxides, elemental sulfur, sulfur compounds, etc. The lithium compound as the other positive electrode active material may be a Li-containing oxide containing at least one element M, Li, and O. The element M may be, for example, at least one selected from Mn, Ni, Co, Al, Mg, Ca, Sc, V, Cr, Cu, Zn, Ga, Ge, Y, Zr, Sn, Sb, W, Pb, Bi, Fe, and Ti, or at least one selected from the group consisting of Mn, Ni, Co, Al, Fe, and Ti. More specifically, the Li-containing oxides as other positive electrode active materials include lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium nickel manganese oxide, lithium cobalt manganese oxide, and lithium nickel cobalt manganese oxide (Li 1±α Ni x Co y Mn z O 2±δ (For example, 0<x<1, 0<y<1, 0<z<1, x+y+z=1)), spinel-based lithium compounds (Li 1+x Mn 2-x-y M y O 4 (wherein M is one or more selected from Al, Mg, Co, Fe, Ni, and Zn)), lithium nickel cobalt aluminate (e.g., Li 1±α Ni p Co q Al r O 2±δ (e.g., p+q+r=1), lithium titanate, lithium metal phosphate (LiMPO 4and the like, where M is one or more selected from Fe, Mn, Co, and Ni). In particular, when the other positive electrode active material contains, as constituent elements, at least one of Ni, Co, and Mn, and a Li-containing oxide containing Li and O, the performance of the secondary battery is more likely to be improved. Alternatively, when the other positive electrode active material contains, as constituent elements, at least one of Ni, Co, and Al, and a Li-containing oxide containing Li and O, the performance of the secondary battery is also more likely to be improved. Only one type of other positive electrode active material may be used alone, or two or more types may be used in combination. The shape of the other positive electrode active material may be any shape commonly used for positive electrode active materials in secondary batteries. The other positive electrode active material may be, for example, particulate. The other positive electrode active material may be solid or may have voids, for example, porous or hollow. The other positive electrode active material may be primary particles or secondary particles formed by aggregation of a plurality of primary particles. The average particle diameter D50 of the other positive electrode active material may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less.
[0041] 3.1.2 Protective Layer An ion-conductive protective layer may be formed on the surface of the positive electrode active material. That is, the positive electrode active material layer 10 may include a composite of the positive electrode active material and the protective layer, and at least a portion of the surface of the positive electrode active material in the composite may be covered with the protective layer. This may, for example, more easily suppress reactions between the positive electrode active material and other battery materials (such as the sulfide solid electrolyte described below). The ion-conductive protective layer may include various ion-conductive compounds. The ion-conductive compound may be, for example, at least one selected from ion-conductive oxides and ion-conductive halides.
[0042] The ion-conductive oxide may contain, for example, at least one element selected from B, C, Al, Si, P, S, Ti, La, Zr, Nb, Mo, Zn, and W, Li, and O. The ion-conductive oxide may be an oxynitride containing N. More specifically, the ion-conductive oxide may contain Li 3 BO 3 , LiBO 2 , Li 2 CO 3 , LiAlO 2 , Li 4 SiO 4 , Li 2 SiO 3 , Li 3 P.O. 4 , Li 2 SO 4 , Li 2 TiO 3 , Li 4 Ti 5 O 12 , Li 2 Ti 2 O 5 , Li 2 ZrO 3 , LiNbO 3 , Li 2 MoO 4 , Li 2 WO 4 , LiPON, Li 2 O-LaO 2 , Li 2 O-ZnO 2 The ion-conductive oxide may be one in which some elements are substituted with various doping elements.
[0043] The ion-conductive halide may be, for example, at least one of the various compounds exemplified as the halide solid electrolyte described below. The ion-conductive halide may include, for example, at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb, and Sm, at least one halogen element selected from the group consisting of Cl, Br, I, and F, and Li. The ion-conductive halide may include at least one element selected from the group consisting of Ti, Al, Gd, Ca, Zr, and Y, at least one element selected from the group consisting of Cl, Br, I, and F, and Li. The ion-conductive halide may also include at least one element selected from the group consisting of Ti and Al, at least one element selected from the group consisting of Cl, Br, I, and F, and Li. The ion-conductive halide may be, for example, a complex halide of Li, Ti, Al, and F.
[0044] The coverage (area ratio) of the protective layer with respect to the surface of the positive electrode active material may be, for example, 70% or more, 80% or more, or 90% or more. The thickness of the protective layer may be, for example, 0.1 nm or more or 1 nm or more, and may be 100 nm or less or 20 nm or less.
[0045] 3.1.2 Electrolyte The positive electrode active material layer 10 may contain an electrolyte. The electrolyte that may be contained in the positive electrode active material layer 10 may be a solid electrolyte, a liquid electrolyte, or a combination thereof.
[0046] 3.1.2.1 Solid Electrolyte As the solid electrolyte, any known solid electrolyte for lithium-ion secondary batteries may be used. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, inorganic solid electrolytes have excellent ionic conductivity and heat resistance. Examples of inorganic solid electrolytes include oxide solid electrolytes, sulfide solid electrolytes, and ionically bonded inorganic solid electrolytes. Among inorganic solid electrolytes, sulfide solid electrolytes, and sulfide solid electrolytes containing at least Li, S, and P as constituent elements, exhibit high performance. Alternatively, among inorganic solid electrolytes, ionically bonded solid electrolytes, and solid electrolytes containing at least Li, Y, and a halogen (at least one of Cl, Br, I, and F) as constituent elements exhibit high performance. The solid electrolyte may be amorphous or crystalline. The solid electrolyte may be particulate. The average particle diameter (D50) of the solid electrolyte may be, for example, 10 nm or more and 10 μm or less. The ionic conductivity of the solid electrolyte at 25° C. may be, for example, 1×10 -5 S / cm or more, 1×10 -4 S / cm or more, or 1 x 10 -3 The solid electrolyte may have a viscosity of 0.15 S / cm or more. One type of solid electrolyte may be used alone, or two or more types may be used in combination.
[0047] The oxide solid electrolyte is lithium lanthanum zirconate, LiPON, Li 1+X Al X Ge 2-X (P.O. 4 ) 3 , Li—SiO-based glass, Li—Al—S—O-based glass, etc. Furthermore, when an oxide solid electrolyte is combined with a liquid electrolyte, ionic conductivity can be improved.
[0048] The sulfide solid electrolyte may be a glass-based sulfide solid electrolyte (sulfide glass), a glass-ceramic-based sulfide solid electrolyte, or a crystalline sulfide solid electrolyte. The sulfide glass is amorphous. The sulfide glass may have a glass transition temperature (Tg). In addition, when the sulfide solid electrolyte has a crystalline phase, examples of the crystalline phase include a Thio-LISICON-type crystalline phase, an LGPS-type crystalline phase, and an Argyrodite-type crystalline phase. The sulfide solid electrolyte may be particulate. The average particle diameter (D50) of the sulfide solid electrolyte may be, for example, 10 nm or more and 100 μm or less.
[0049] The sulfide solid electrolyte may contain, for example, Li, X (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S. The sulfide solid electrolyte may further contain at least one of O and a halogen element. The sulfide solid electrolyte may contain S as a main anion element.
[0050] The sulfide solid electrolyte is, for example, Li 2 S-P 2 S 5 , Li 2 S-P 2 S 5 - LiI, Li 2 S-P 2 S 5 -GeS 2 , Li 2 S-P 2 S 5 -Li 2 O, Li 2 S-P 2 S 5 -Li 2 O-LiI, Li 2 S-P 2 S 5 -LiI-LiBr, Li 2 S-SiS 2 , Li 2 S-SiS 2 - LiI, Li 2 S-SiS 2 - LiBr, Li 2 S-SiS2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S-B 2 S 3 , Li 2 S-P 2 S 5 -ZmSn (where m and n are positive numbers, and Z is Ge, Zn, or Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 P.O. 4 , Li 2 S-SiS 2 -Li x MO y (where x and y are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga, and In).
[0051] The composition of the sulfide solid electrolyte is not particularly limited, but may be, for example, xLi 2 S・(100-x)P 2 S 5 (70≦x≦80), yLiI・zLiBr・(100−y−z)(xLi 2 S·(1−x)P 2 S 5 ) (0.7≦x≦0.8, 0≦y≦30, 0≦z≦30) or the like. Alternatively, the sulfide solid electrolyte may be represented by the general formula: Li 4-x Ge 1-x P x S 4(0<x<1). In the above general formula, at least a portion of Ge may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, at least a portion of P may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, at least a portion of Li may be substituted with at least one of Na, K, Mg, Ca, and Zn. In the above general formula, at least a portion of S may be substituted with a halogen (at least one of F, Cl, Br, and I). Alternatively, the sulfide solid electrolyte may be Li 7-a P.S. 6-a X a (X is at least one of Cl, Br, and I, and a is a number of 0 or more and 2 or less). a may be 0 or greater than 0. In the latter case, a may be 0.1 or greater, 0.5 or greater, or 1 or greater. Also, a may be 1.8 or less, or 1.5 or less.
[0052] The ionically bonded solid electrolyte may contain, for example, at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb, and Sm. These elements can generate cations in water. The ionically bonded solid electrolyte material may further contain, for example, at least one halogen element selected from the group consisting of Cl, Br, I, and F. These elements can generate anions in water. The ionically bonded solid electrolyte may contain at least one element selected from the group consisting of Gd, Ca, Zr, and Y, at least one element selected from the group consisting of Cl, Br, I, and F, and Li. The ionically bonded solid electrolyte may also contain Li and Y, and at least one element selected from the group consisting of Cl, Br, I, and F. More specifically, the ionic solid electrolyte may contain Li, Y, Cl, and Br, or may contain Li, Ca, Y, Gd, Cl, and Br, or may contain Li, Zr, Y, and Cl. 3 YBr 2 Cl 4 , Li 2.8 Ca 0.1 Y 0.5 Gd 0.5 Br 2 Cl 4 , and Li 2.5 Y 0.5 Zr 0.5 Cl 6 It may be at least one of the following.
[0053] The ionically bonded solid electrolyte may be a halide solid electrolyte. The halide solid electrolyte has excellent ion conductivity. Examples of the halide solid electrolyte include those represented by the formula (A): Li α M β X γ...(A) where α, β, and γ are each independently greater than 0, M is at least one element selected from the group consisting of metal elements and metalloid elements other than Li, and X is at least one element selected from the group consisting of Cl, Br, and I. The "metalloid element" may be at least one element selected from the group consisting of B, Si, Ge, As, Sb, and Te. The "metal element" may include (i) all elements contained in Groups 1 to 12 of the periodic table (excluding hydrogen) and (ii) all elements contained in Groups 13 to 16 of the periodic table (excluding B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se). The metal element may form an inorganic compound with a halide ion to become a cation.
[0054] In formula (A), M may contain Y (i.e., yttrium). The halide solid electrolyte containing Y is Li a Me b Y c X 6 (where a+mb+3c=6, c>0, Me is at least one selected from the group consisting of metal elements and metalloid elements other than Li and Y, and m is the valence of Me). Me may be, for example, at least one selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb.
[0055] The halide solid electrolyte has the formula (A1): Li 6-3d Y d X 6 In formula (A1), X is one or more elements selected from the group consisting of Cl, Br, and I. d may satisfy the relationship 0<d<2, or d=1. The halide solid electrolyte may have a composition represented by formula (A2): Li 3-3δ Y 1+δ Cl 6 In formula (A2), 0<δ≦0.15 may be satisfied. The halide solid electrolyte may have a composition represented by formula (A3): Li3-3δ Y 1+δ Br 6 In formula (A3), 0<δ≦0.25 may be satisfied. The halide solid electrolyte may have a composition represented by formula (A4): Li 3-3δ+a Y 1+δ-a Me a Cl 6-x-y Br x I y In formula (A4), Me may be at least one selected from the group consisting of Mg, Ca, Sr, Ba, and Zn. In formula (A4), for example, -1<δ<2, 0<a<3, 0<(3-3δ+a), 0<(1+δ-a), 0≦x≦6, 0≦y≦6, and (x+y)≦6 are satisfied. The halide solid electrolyte may have a composition represented by formula (A5): Li 3-3δ Y 1+δ-a Me a Cl 6-x-y Br x I y In formula (A5), Me may be at least one selected from the group consisting of Al, Sc, Ga, and Bi. In formula (A5), -1<δ<1, 0<a<2, 0<(1+δ-a), 0≦x≦6, 0≦y≦6, and (x+y)≦6 may be satisfied. The halide solid electrolyte may have a composition represented by formula (A6): Li 3-3δ-a Y 1+δ-a Me a Cl 6-x-y Br x I y In formula (A6), Me may be at least one selected from the group consisting of Zr, Hf, and Ti. In formula (A6), -1<δ<1, 0<a<1.5, 0<(3-3δ-a), 0<(1+δ-a), 0≦x≦6, 0≦y≦6, and (x+y)≦6 may be satisfied. The halide solid electrolyte may have a composition represented by formula (A7): Li 3-3δ-2a Y 1+δ-a Me a Cl 6-x-y Br x I yIn formula (A7), Me may be at least one element selected from the group consisting of Ta and Nb. In formula (A7), -1<δ<1, 0<a<1.2, 0<(3-3δ-2a), 0<(1+δ-a), 0≦x≦6, 0≦y≦6, and (x+y)≦6 may be satisfied.
[0056] The ionic solid electrolyte may be a complex hydride solid electrolyte. The complex hydride solid electrolyte may be composed of Li ions and complex ions containing H. The complex ions containing H may have, for example, an element M containing at least one of a nonmetallic element, a semimetallic element, and a metallic element, and H bonded to the element M. Furthermore, the complex ions containing H may have the element M as a central element and H surrounding the element M bonded to each other via a covalent bond. Furthermore, the complex ions containing H may be (M m H n ) α- In this case, m is any positive number, and n and α can take any positive number depending on m and the valence of element M. Element M may be any nonmetallic element or metallic element capable of forming a complex ion. For example, element M may contain at least one of B, C, and N as a nonmetallic element, or may contain B. Furthermore, for example, element M may contain at least one of Al, Ni, and Fe as a metallic element. In particular, when the complex ion contains B or when it contains C and B, higher ionic conductivity is likely to be ensured. Specific examples of complex ions containing H include (CB 9 H 10 ) - , (CB 11 H 12 ) - , (B 10 H 10 ) 2- , (B 12 H 12 ) 2- , (BH 4 ) - , (NH 2 ) - , (AlH 4 ) - , and combinations thereof. In particular, (CB9 H 10 ) - , (CB 11 H 12 ) - In other words, the complex hydride solid electrolyte may contain Li, C, B, and H.
[0057] 3.1.2.2 Liquid Electrolyte The liquid electrolyte (electrolyte solution) is a liquid containing lithium ions as carrier ions. The electrolyte solution may be an aqueous electrolyte solution or a non-aqueous electrolyte solution. The composition of the electrolyte solution may be the same as known compositions of electrolyte solutions for lithium ion secondary batteries. The electrolyte solution may be one in which a lithium salt is dissolved in water or a non-aqueous solvent. Examples of non-aqueous solvents include various carbonate-based solvents. Examples of lithium salts include lithium amide salts and LiPF 6 etc.
[0058] 3.1.3 Conductive Aids Examples of conductive aids that can be contained in the positive electrode active material layer 10 include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, titanium, aluminum, and stainless steel. The conductive aid may be, for example, particulate or fibrous, and its size is not particularly limited. Only one type of conductive aid may be used alone, or two or more types may be used in combination.
[0059] 3.1.4 Binder Examples of binders that can be contained in the positive electrode active material layer 10 include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.
[0060] 3.1.5 Others The positive electrode active material layer 10 may contain various additives in addition to the above components, such as a dispersant and a lubricant.
[0061] 3.2 Electrolyte Layer The electrolyte layer 20 is disposed between the positive electrode active material layer 10 and the negative electrode active material layer 30. The electrolyte layer 20 contains at least an electrolyte. The electrolyte layer 20 may contain at least one of a solid electrolyte and an electrolytic solution, and may further contain a binder or the like. The contents of the electrolyte and binder or the like in the electrolyte layer 20 are not particularly limited. Alternatively, the electrolyte layer 20 may include a separator or the like that holds the electrolytic solution and prevents contact between the positive electrode active material layer 10 and the negative electrode active material layer 30. The thickness of the electrolyte layer 20 is not particularly limited and may be, for example, 0.1 μm or more or 1 μm or more, or 2 mm or less or 1 mm or less.
[0062] The electrolyte layer 20 may consist of one layer or multiple layers. For example, the electrolyte layer 20 may include a first layer disposed on the positive electrode active material layer 10 side and a second layer disposed on the negative electrode active material layer 30 side, and the first layer may include a first electrolyte and the second layer may include a second electrolyte. The first electrolyte and the second electrolyte may be different from each other. The first electrolyte and the second electrolyte may each be at least one selected from the oxide solid electrolyte, sulfide solid electrolyte, and ionically bonded solid electrolyte described above. For example, the first layer may include an ionically bonded solid electrolyte, and the second layer may include at least one of an ionically bonded solid electrolyte and a sulfide solid electrolyte.
[0063] The electrolyte contained in the electrolyte layer 20 may be appropriately selected from the examples (solid electrolytes and / or liquid electrolytes) of the electrolytes that can be contained in the cathode active material layer 10 described above. The binder that can be contained in the electrolyte layer 20 may also be appropriately selected from the examples of the binders that can be contained in the cathode active material layer described above. Each of the electrolytes and binders may be used alone or in combination of two or more. The separator may be any separator commonly used in lithium ion secondary batteries, such as those made of resins such as polyethylene (PE), polypropylene (PP), polyester, and polyamide. The separator may have a single-layer structure or a multi-layer structure. Examples of multi-layer separators include a two-layer structure of PE / PP, or a three-layer structure of PP / PE / PP or PE / PP / PE. The separator may be made of a nonwoven fabric such as a cellulose nonwoven fabric, a resin nonwoven fabric, or a glass fiber nonwoven fabric.
[0064] 3.3 Negative Electrode Active Material Layer The negative electrode active material layer 30 contains at least a negative electrode active material. The negative electrode active material layer 30 may also optionally contain an electrolyte, a conductive additive, a binder, various additives, and the like. The content of each component in the negative electrode active material layer 30 may be appropriately determined depending on the desired battery performance. For example, the total solid content of the negative electrode active material layer 30 is taken as 100% by mass, and the content of the negative electrode active material may be 40% by mass or more, 50% by mass or more, 60% by mass or more, or 70% by mass or more, or may be 100% by mass or less, less than 100% by mass, 95% by mass or less, or 90% by mass or less. Alternatively, the total content of the negative electrode active material layer 30 may be 85% by volume or more, 90% by volume or more, or 95% by volume or more, and the remainder may be voids or other components. The shape of the negative electrode active material layer 30 is not particularly limited, and may be, for example, a substantially flat sheet. The thickness of the negative electrode active material layer 30 is not particularly limited, and may be, for example, 0.1 μm or more, 1 μm or more, 10 μm or more, or 30 μm or more, or may be 2 mm or less, 1 mm or less, 500 μm or less, or 100 μm or less.
[0065] 3.3.1 Negative Electrode Active Material Any known negative electrode active material for lithium ion secondary batteries can be used as the negative electrode active material. Among known active materials, various materials can be used whose potential for absorbing and releasing lithium ions (charge / discharge potential) is lower than that of the above-mentioned positive electrode active material. Examples of such materials include silicon-based active materials such as Si, Si alloys, and silicon oxide; carbon-based active materials such as graphite and hard carbon; various oxide-based active materials such as lithium titanate; metallic lithium and lithium alloys. In particular, when the negative electrode active material layer 30 contains Si as the negative electrode active material, the performance of the lithium ion secondary battery 100 is likely to be improved. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination. The shape of the negative electrode active material may be any shape commonly used for negative electrode active materials in secondary batteries. For example, the negative electrode active material may be particulate. The negative electrode active material particles may be primary particles or secondary particles formed by agglomeration of multiple primary particles. The average particle diameter (D50) of the negative electrode active material particles may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. Alternatively, the negative electrode active material may be in the form of a sheet (foil or film) such as a lithium foil. That is, the negative electrode active material layer 30 may be made of a sheet of negative electrode active material.
[0066] 3.3.2 Others Examples of electrolytes that can be contained in the negative electrode active material layer 30 include the above-mentioned solid electrolytes, electrolytic solutions, and combinations thereof. The conductive additives that can be contained in the negative electrode active material layer 30 may be appropriately selected from, for example, the conductive additives that can be contained in the above-mentioned positive electrode active material layer. The binders that can be contained in the negative electrode active material layer 30 may be appropriately selected from, for example, the binders that can be contained in the above-mentioned positive electrode active material layer. Each of the electrolytes, conductive additives, and binders may be used alone or in combination of two or more.
[0067] 3.4 Positive Electrode Current Collector As shown in FIG. 2 , the lithium-ion secondary battery 100 may include a positive electrode current collector 40 in contact with the positive electrode active material layer 10. Any common positive electrode current collector for secondary batteries can be used as the positive electrode current collector 40. The positive electrode current collector 40 may have at least one shape selected from foil, plate, mesh, punched metal, and foam. The positive electrode current collector 40 may be made of metal foil or metal mesh. Metal foil is particularly advantageous in terms of ease of handling. The positive electrode current collector 40 may be made of multiple foils. Examples of metals constituting the positive electrode current collector 40 include at least one selected from Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, V, Mg, Pb, Ge, In, Sn, Zr, and stainless steel. In particular, from the viewpoint of ensuring oxidation resistance, the positive electrode current collector 40 may contain Al. The positive electrode current collector 40 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. For example, the positive electrode current collector 40 may have a carbon coating layer. Furthermore, the positive electrode current collector 40 may be a metal foil or a substrate on which the above metal is plated or vapor-deposited. Furthermore, when the positive electrode current collector 40 is made of multiple sheets of metal foil, some kind of layer may be present between the multiple sheets of metal foil. The thickness of the positive electrode current collector 40 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.
[0068] 3.5 Negative Electrode Current Collector As shown in FIG. 2 , the lithium-ion secondary battery 100 may include a negative electrode current collector 50 in contact with the negative electrode active material layer 30. Any of the negative electrode current collectors commonly used for secondary batteries can be used as the negative electrode current collector 50. The negative electrode current collector 50 may be in the form of a foil, plate, mesh, punched metal, foam, or the like. The negative electrode current collector 50 may be a metal foil or metal mesh, or a carbon sheet. Metal foil is particularly advantageous in terms of ease of handling. The negative electrode current collector 50 may be composed of multiple foils or sheets. Examples of metals constituting the negative electrode current collector 50 include at least one selected from Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, V, Mg, Pb, Ge, In, Sn, Zr, and stainless steel. In particular, from the viewpoint of ensuring reduction resistance and being less likely to alloy with lithium, the negative electrode current collector 50 may contain at least one metal selected from Cu, Ni, and stainless steel. The negative electrode current collector 50 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. For example, the negative electrode current collector 50 may have a carbon coating layer. The negative electrode current collector 50 may be an aluminum foil having a carbon coating layer. The negative electrode current collector 50 may also be a metal foil or a substrate plated or vapor-deposited with the above metal. Furthermore, when the negative electrode current collector 50 is made of multiple sheets of metal foil, some kind of layer may be present between the multiple sheets of metal foil. The thickness of the negative electrode current collector 50 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.
[0069] 3.6 Other Configurations In addition to the above configurations, the lithium ion secondary battery 100 may have general configurations for secondary batteries. For example, tabs, terminals, etc. The lithium ion secondary battery 100 may have each of the above configurations housed inside an exterior body. Any known exterior body for a battery can be used as the exterior body. Furthermore, multiple secondary batteries 100 may be electrically connected and stacked in any desired manner to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. Examples of shapes of the lithium ion secondary battery 100 include a coin type, a laminate type, a cylindrical type, and a prismatic type.
[0070] The lithium-ion secondary battery 100 can be manufactured by applying known methods, except for using the specific positive electrode active material described above. For example, it can be manufactured as follows. However, the manufacturing method of the lithium-ion secondary battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding. (1) A positive electrode layer slurry is obtained by dispersing a positive electrode active material and the like that constitute the positive electrode active material layer in a solvent. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The positive electrode layer slurry is applied to the surface of a positive electrode current collector using a doctor blade or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode current collector, thereby forming a positive electrode. (2) A negative electrode layer slurry is obtained by dispersing a negative electrode active material and the like that constitute the negative electrode active material layer in a solvent. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The negative electrode layer slurry is applied to the surface of a negative electrode current collector using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector, thereby forming a negative electrode. (3) The layers are stacked so that the electrolyte layer (solid electrolyte layer or separator) is sandwiched between the negative electrode and positive electrode to obtain a laminate having a negative electrode current collector, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer, and a positive electrode current collector in this order. Other components such as terminals are attached to the laminate as needed. (4) The laminate is housed in a battery case. In the case of an electrolyte battery, the battery case is filled with an electrolyte, and the laminate is immersed in the electrolyte and sealed in the battery case to form a secondary battery. In the case of an electrolyte battery, the electrolyte may be impregnated into the negative electrode active material layer, separator, and positive electrode active material layer at the above step (3).
[0071] 4. Method for Increasing the Capacity of a Lithium-Ion Secondary Battery The technology of the present disclosure also has an aspect as a method for increasing the capacity of a lithium-ion secondary battery. That is, the method for increasing the capacity of a lithium-ion secondary battery of the present disclosure is characterized by using the above-described positive electrode active material of the present disclosure in a positive electrode active material layer of the lithium-ion secondary battery.
[0072] 5. Vehicle Having a Lithium-Ion Secondary Battery As described above, the positive electrode active material of the present disclosure has a large capacity and is suitable as a positive electrode active material for a lithium-ion secondary battery. Such a high-capacity lithium-ion secondary battery can be suitably used in at least one type of vehicle selected from, for example, a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), and an electric vehicle (BEV). That is, the technology of the present disclosure also has an aspect of a vehicle having a lithium-ion secondary battery, the lithium-ion secondary battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, and the positive electrode active material layer containing the positive electrode active material of the present disclosure.
[0073] As described above, one embodiment of the positive electrode active material and the lithium ion secondary battery, etc., has been described, but the technology of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist thereof. Hereinafter, the technology of the present disclosure will be described in more detail with reference to examples, but the technology of the present disclosure is not limited to the following examples.
[0074] 1. Preparation of Positive Electrode Active Material 1.1 Example 1 1.1.1 Preparation of Precursor (1) MnSO 4 ・5H 2 O, NiSO 4 ・6H 2 O, CoSO 4 ・7H 2 The first solution was prepared by weighing out the desired composition ratio of O and dissolving it in distilled water to a concentration of 1.2 mol / L. 2 CO 3The second solution was obtained by dissolving the first solution in distilled water to a concentration of 1.2 mol / L. (2) 1000 mL of pure water was placed in a reaction vessel (with a baffle), and 500 mL of the first solution and 500 mL of the second solution were added dropwise at a rate of approximately 4 mL / min. (3) After the addition was completed, the mixture was stirred at room temperature for 1 hour at a stirring speed of 150 rpm to obtain a product. (4) The product was washed with pure water, subjected to solid-liquid separation using a centrifuge, and the precipitate was recovered. (5) The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and then separated into coarse particles and fine particles by air classification. Both the coarse particles and the fine particles were composite salts containing Mn, Ni, and Co. The coarse particles were spherical particles with an average particle diameter D50 of 3.8 μm and a circularity of 0.86. The fine particles were spherical particles having an average particle diameter D50 of 1.4 μm and a circularity of 0.80. In Example 1, the above-mentioned coarse particles were used as precursor particles.
[0075] 1.1.2 Preparation of the complex (1) Na to 1150 g / L 2 CO 3 After weighing the sodium hydroxide and distilled water, stir the solution using a stirrer until it is completely dissolved. 2 CO 3 (2) The above Na 2 CO 3 The aqueous solution and the precursor particles are mixed together to form a mixture having a composition of Na after calcination, which will be described later. 0.7 Mn 0.5 Ni 0.2 Co 0.3 O 2 (3) The above slurry was air-dried by spray drying to obtain a composite. Specifically, a DL410 spray dryer was used, with a slurry delivery rate of 30 mL / min, an inlet temperature of 200°C, and a circulating air volume of 0.8 m 3 The above slurry was dried by air flow under the conditions of a spray rate of 0.3 MPa at a spraying pressure of 0.3 MPa to form a Na 2 CO 3 In the composite, 77% of the surface area of the precursor particles was covered with Na. 2 CO 3It was covered with
[0076] 1.1.3 Firing of the Composite The composite was placed in an alumina crucible and fired in an air atmosphere to obtain a Na-containing oxide having a P2-type structure. The firing conditions were as follows (1) to (7): (1) The alumina crucible containing the composite was placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace was increased from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature inside the heating furnace was maintained at 600°C for 360 minutes to perform pre-firing. (4) After pre-firing, the temperature inside the heating furnace was increased from 600°C to 900°C in 100 minutes. (5) The temperature inside the heating furnace was maintained at 900°C for 60 minutes to perform main firing. (6) After main firing, the temperature inside the heating furnace was decreased from 900°C to 250°C in 120 minutes. (7) At 250°C, the alumina crucible is removed from the heating furnace and allowed to cool outside the furnace in a dry atmosphere until it reaches 25°C in 10 minutes.
[0077] The fired product after being allowed to cool was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles A having a P2 type structure.
[0078] 1.1.4 Ion exchange (1) LiNO 3 and LiCl were weighed out to a molar ratio of 50:50, and mixed with the P2-type particles A at a molar ratio 10 times the minimum Li amount required for ion exchange to obtain a mixture. (2) Using an alumina crucible, ion exchange was performed at 280°C for 1 hour in an air atmosphere to obtain a product containing a Li-containing oxide. (3) The salt remaining in the product was washed with pure water, and solid-liquid separation was performed by vacuum filtration to obtain a precipitate. (4) The obtained precipitate was dried at 120°C overnight to obtain the positive electrode active material of Example 1.
[0079] 1.2 Example 2 1.2.1 Preparation of Precursor Coarse particles and fine particles were obtained in the same manner as in Example 1, and the fine particles were used as precursor particles.
[0080] 1.2.2 Preparation of Composite A composite was obtained by spray drying in the same manner as in Example 1, except that fine particles were used as precursor particles. In the composite, 73% by area of the surface of the precursor particles was Na 2 CO 3 It was covered with
[0081] 1.2.3 Firing of the Composite The composite was placed in an alumina crucible and fired in an air atmosphere to obtain a Na-containing oxide having a P2-type structure. The firing conditions were as follows (1) to (7): (1) The alumina crucible containing the composite was placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace was increased from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature inside the heating furnace was maintained at 600°C for 360 minutes to perform pre-firing. (4) After pre-firing, the temperature inside the heating furnace was increased from 600°C to 1000°C in 160 minutes. (5) The temperature inside the heating furnace was maintained at 1000°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature inside the heating furnace was decreased from 1000°C to 250°C in 160 minutes. (7) At 250°C, the alumina crucible is removed from the heating furnace and allowed to cool outside the furnace in a dry atmosphere until it reaches 25°C in 10 minutes.
[0082] The fired product after being allowed to cool was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles B having a P2 type structure.
[0083] 1.2.4 Ion Exchange Ion exchange was carried out under the same conditions as in Example 1, except that the Na-containing oxide particles B were used instead of the Na-containing oxide particles A, to obtain a positive electrode active material according to Example 2.
[0084] 1.3 Comparative Example 1 1.3.1 Preparation of Precursor Particles As in Example 2, fine particles were used as precursor particles.
[0085] 1.3.2 Preparation of the composite Precursor particles and Na 2 CO 3 And Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 O 2 The precursor and Na were weighed to have the following composition. 2 CO 3 The composite was obtained by mixing the above in a mortar. In the composite, 24% by area of the surface of the precursor particles was Na 2 CO 3 It was covered with
[0086] 1.3.3 Firing of the Composite The composite was placed in an alumina crucible and fired in an air atmosphere to obtain a Na-containing oxide having a P2 structure. The firing conditions were as follows (1) to (7): (1) The alumina crucible containing the composite was placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace was increased from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature inside the heating furnace was maintained at 600°C for 360 minutes to perform pre-firing. (4) After pre-firing, the temperature inside the heating furnace was increased from 600°C to 950°C in 120 minutes. (5) The temperature inside the heating furnace was maintained at 950°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature inside the heating furnace was decreased from 950°C to 250°C in 140 minutes. (7) At 250°C, the alumina crucible is removed from the heating furnace and allowed to cool outside the furnace in a dry atmosphere until it reaches 25°C in 10 minutes.
[0087] The fired product after being allowed to cool was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles C having a P2 type structure.
[0088] 1.3.4 Ion Exchange Ion exchange was carried out under the same conditions as in Example 1, except that the Na-containing oxide particles C were used instead of the Na-containing oxide particles A, to obtain a positive electrode active material according to Comparative Example 1.
[0089] 1.4 Comparative Example 2 1.4.1 Preparation of Precursor Particles As in Example 1, coarse particles were used as precursor particles.
[0090] 1.4.2 Preparation of Composite A composite was obtained in the same manner as in Comparative Example 1, except that coarse particles were used as precursor particles. In this composite, 26% by area of the surface of the precursor particles was Na 2 CO 3 It was covered with
[0091] The composite was placed in an alumina crucible and fired under air conditions to obtain a Na-containing oxide having a P2 structure.
[0092] The fired product after being allowed to cool was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles D having a P2 type structure.
[0093] 1.4.4 Ion Exchange Ion exchange was carried out under the same conditions as in Example 1, except that the Na-containing oxide particles D were used instead of the Na-containing oxide particles A, to obtain a positive electrode active material according to Comparative Example 2.
[0094] 2. Evaluation of Positive Electrode Active Material 2.1 Elemental Analysis Elemental analysis was performed to identify the chemical composition of each of the positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 and 2. The results are shown in Table 1 below.
[0095] 2.2 Identification of Crystal Structure by X-ray Diffraction Measurement For each of the positive electrode active materials of Examples 1-2 and Comparative Examples 1-2, X-ray diffraction measurements using CuKα as a radiation source were performed to obtain X-ray diffraction patterns. FIG. 3 shows the X-ray diffraction patterns for each of Examples 1-2 and Comparative Examples 1-2. As shown in FIG. 3, it can be seen that all of the positive electrode active materials of Examples 1-2 and Comparative Examples 1-2 have an O2-type structure. Also, as shown in FIG. 3, it can be seen that the positive electrode active materials of Examples 1-2, compared to the positive electrode active materials of Comparative Examples 1-2, have a lower X-ray diffraction peak intensity derived from the (002) plane of the T#2 structure relative to the X-ray diffraction peak intensity derived from the (002) plane of the O2-type structure. Table 1 below shows the X-ray diffraction peak intensity I derived from the (002) plane of the T#2 structure for each of Examples 1-2 and Comparative Examples 1-2. 1 and the X-ray diffraction peak intensity I originating from the (002) plane of the O2 type structure. 2 Relative to I 1 / I 2 Shows.
[0096] 3. Preparation of Evaluation Cells Coin cells were prepared using the positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 and 2. The coin cell preparation procedure was as follows: (1) The positive electrode active material, acetylene black (AB) as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder were weighed out in a mass ratio of positive electrode active material:AB:PVdF = 85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode composite slurry. The positive electrode composite slurry was applied to aluminum foil and vacuum dried overnight at 120°C to obtain a positive electrode, which was a laminate of a positive electrode active material layer and a positive electrode current collector. (2) An electrolyte solution was prepared by dissolving LiPF6 at a concentration of 1 M in a mixed solvent of trifluoropropylene carbonate (TFPC) and trifluoroethyl methyl carbonate (TFEMC) in a ratio of 30 vol% to 70 vol%. (3) A metallic lithium foil was prepared as the negative electrode. (4) A coin cell (CR2032) was fabricated using the positive electrode, the electrolyte, and the negative electrode.
[0097] 4. Evaluation of Charge / Discharge Characteristics Each coin cell was charged / discharged at 0.1 C (1 C = 220 mA / g) in a voltage range of 2.0 to 4.8 V in a thermostatic chamber maintained at 25° C., and the capacity was measured. The results are shown in Table 1 below.
[0098] 5. Evaluation Results For each of Examples 1 and 2 and Comparative Examples 1 and 2, the chemical composition of the positive electrode active material and the I identified from the X-ray diffraction pattern were 1 / I 2 and the capacity of the evaluation cell. 1 / I 2 The relationship between the voltage and capacity is shown.
[0099]
[0100] As is clear from the results shown in Table 1 and FIG. 1 / I 2 The positive electrode active materials according to Examples 1 and 2, in which I is 0.30 or less, 1 / I 2The positive electrode active material according to Comparative Examples 1 and 2 has a larger capacity than the positive electrode active materials according to Comparative Examples 1 and 2, in which the X-ray diffraction peak intensity derived from the O2-type structure is higher and the X-ray diffraction peak intensity derived from the T#2 structure is lower, so that the capacity of the positive electrode active material increases.
[0101] 6. Supplementary Information Although the above examples illustrate the case where a precursor is obtained by coprecipitation, the precursor can also be obtained by other methods. Furthermore, the above examples illustrate the case where a composite is obtained by coating the surface of a precursor with a Na source by spray drying, but the composite can also be obtained by other methods. Furthermore, the above examples illustrate the Na-containing oxide having a P2-type structure and the Li-containing oxide having an O2-type structure as having a predetermined chemical composition, but the chemical compositions of the Na-containing oxide and the Li-containing oxide are not limited thereto. Furthermore, the Na-containing oxide and the Li-containing oxide may be doped with an element M other than Mn, Ni, and Co. The element M is as described in the embodiment.
[0102] 7. Summary As described above, in a positive electrode active material containing a Li-containing oxide, if the Li-containing oxide satisfies the following requirements (1) to (3), it can be said that the capacity of the positive electrode active material is large. (1) The Li-containing oxide has an O2-type structure. (2) The Li-containing oxide contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Li, and O. (3) The X-ray diffraction pattern of the Li-containing oxide has a refractive index within the range of 0≦I 1 / I 2 ≦0.30. 1 is the X-ray diffraction peak intensity derived from the (002) plane of the T#2 type structure, and 2 is the X-ray diffraction peak intensity originating from the (002) plane of the O2 type structure.
[0103] 100 Lithium ion secondary battery 10 Positive electrode active material layer 20 Electrolyte layer 30 Negative electrode active material layer 40 Positive electrode current collector 50 Negative electrode current collector
Claims
1. A positive electrode active material comprising a Li-containing oxide, the Li-containing oxide having an O2 type structure, the Li-containing oxide containing at least one element selected from Mn, Ni, and Co, Li, and O as constituent elements, and an X-ray diffraction pattern of the Li-containing oxide having an X-ray diffraction index of 0≦I 1 / I 2 ≦0.30, 1 is the X-ray diffraction peak intensity derived from the (002) plane of the T#2 type structure, 2 is the X-ray diffraction peak intensity derived from the (002) plane of the O2 type structure.
2. The positive electrode active material according to claim 1, wherein the Li-containing oxide is Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0<a≦1.00, 0≦b≦0.20, x+y+z=1, and 0≦p+q+r<0.17, and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W).
3. A positive electrode active material according to claim 1 or 2, wherein the Li-containing oxide contains at least Li, Mn, Ni, Co and O as constituent elements.
4. A lithium ion secondary battery comprising a positive electrode active material layer, an electrolyte layer and a negative electrode active material layer, the positive electrode active material layer containing the positive electrode active material according to any one of claims 1 to 3.
Citation Information
Patent Citations
Non-aqueous electrolyte secondary battery and method of manufacturing the same
JP2011170994A
Non-aqueous electrolyte secondary battery
JP2011228273A
Nonaqueous electrolyte secondary battery and method for manufacturing the same
JP2012094487A
Positive electrode active material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery
JP2015176644A
Method for producing positive electrode active material and method for manufacturing lithium ion battery
JP2021068555A