Method and apparatus for joining metal materials
The pressure-controlled side voltage welding method addresses the limitations of conventional joining techniques by using a controlled current and pressure to efficiently join large metal structures, enhancing joint strength and practicality for industrial use.
Patent Information
- Application Number
- PCT/JP2024/010359
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional metal joining methods, such as mechanical joining and fusion welding, face challenges in achieving strong joints, especially for large structures like construction machines, automobiles, and aircraft, where mechanical joining restricts design freedom and fusion welding struggles to ensure joint strength and is impractical for large-scale applications due to high current requirements.
A pressure-controlled side voltage welding method where a current is passed in a direction intersecting the applied pressure to heat and join metal materials, using a bonding apparatus with a pressure mechanism, heating mechanism, and control unit to manage the joining process, allowing for efficient joining of large structures with improved joint strength.
This method enables strong and efficient joining of large structures by controlling the joining temperature and current distribution, reducing the need for high currents and improving joint strength, making it suitable for industrial applications like construction machines and aircraft.
Smart Images

Figure JP2024010359_31102024_PF_FP_ABST
Abstract
Description
Method and apparatus for joining metal materials
[0001] The present disclosure relates to a method and apparatus for joining metal materials.
[0002] Conventionally, metal materials are generally joined by mechanical joining using rivets or the like, or fusion welding such as arc welding or laser welding. However, mechanical joining results in an increased size of the joint and reduces the degree of freedom in designing the metal material. Furthermore, fusion welding makes it difficult to ensure the strength of the joint. To address these problems, a new solid-state joining method has been proposed, as described in, for example, Patent Document 1 below.
[0003] Special table 2019-181360 publication
[0004] In the pressure-controlled voltage welding method, which is a solid-state welding method described in Patent Document 1, a current is passed through the entire pair of workpieces to which a butt pressure is applied. This causes the pair of workpieces to be heated. When at least one of the workpieces can no longer withstand the pressure, it deforms, and the newly formed surfaces come into sufficient contact with each other, thereby achieving welding of the workpieces.
[0005] The pressure-controlled voltage welding method described above has the advantage that the welding temperature can be controlled by the butt pressure. However, the larger the area of the interface between the materials to be welded (the welded interface), the larger the current value required to heat the materials to be welded. For this reason, applying the pressure-controlled voltage welding method to large structures (e.g., construction machinery, automobiles, aircraft, etc.) (especially in industrial production) is not practical.
[0006] An object of one aspect of the present disclosure is to provide a method for joining metal materials that is also suitable for joining large structures, and a joining device that makes it possible to realize the joining method.
[0007] A method for joining metal materials according to one aspect of the present disclosure includes a preparation step of stacking a first material to be joined containing a first metal and a second material to be joined containing a second metal in a predetermined direction; a heating step of heating at least one of the joining interface between the first material to be joined and the second material to be joined, a first portion of the first material to be joined that is located near the joining interface, and a second portion of the second material to be joined that is located near the joining interface; and a joining step of applying pressure along a predetermined direction toward the joining interface to join the first material to the second material to be joined, wherein in the heating step, a current is passed through at least one of the joining interface, the first portion, and the second portion in an intersecting direction that intersects the predetermined direction.
[0008] A joining device according to another aspect of the present disclosure includes a pressure mechanism that abuts a first workpiece to be joined, which includes a first metal, against a second workpiece to be joined, which includes a second metal, to form a joining interface, and applies pressure to the joining interface in a predetermined direction; a heating mechanism that heats at least one of the joining interface, a first portion of the first workpiece to be joined that is located near the joining interface, and a second portion of the second workpiece to be joined that is located near the joining interface; and a control unit that controls the pressure mechanism and the heating mechanism, wherein the heating mechanism passes an electric current through at least one of the joining interface, the first portion, and the second portion in a direction that intersects the predetermined direction.
[0009] According to one aspect of the present disclosure, it is possible to provide a method for joining metal materials that is also suitable for joining large structures, and a joining device that makes it possible to realize the joining method.
[0010] FIG. 1 is a schematic diagram of a joining apparatus according to an embodiment. FIG. 2(a) is a schematic cross-sectional view showing a first workpiece and a second workpiece before joining, and FIG. 2(b) is a schematic cross-sectional view showing a metal joined body. FIG. 3 is a schematic cross-sectional view of a first part of a heating mechanism. FIG. 4(a) is a plan view of a main part included in an electrode unit, and FIG. 4(b) is a side view of the main part included in the electrode unit. FIG. 5 is a flowchart of a joining method. FIGS. 6(a) and 6(b) are schematic cross-sectional views for explaining the joining method. FIGS. 7(a) and 7(b) are schematic cross-sectional views for explaining the joining method. FIG. 8(a) is a schematic cross-sectional view for explaining a direct current heating method in a reference example, FIG. 8(b) is a schematic perspective view showing a first workpiece used in the reference example, FIG. 8(c) is a schematic cross-sectional view for explaining a direct current heating method in an embodiment, and FIG. 8(d) is a schematic perspective view showing a first workpiece used in an embodiment. 9(a) is a schematic perspective view when side current is applied to the first workpiece, and FIG. 9(b) is a schematic cross-sectional view when side current is applied to the first workpiece. FIG. 10 is a schematic view for explaining a method for measuring thermal emissivity using a thermal imaging camera. FIG. 11 is a view showing a metal bonded body of Example 1. FIG. 12(a) is an electron microscope photograph, and FIG. 12(b) is an enlarged cross-sectional view of the area surrounded by a white square frame shown in FIG. 12(a). FIG. 13(a) is a graph showing the distribution of Vickers hardness in Example 1 and Comparative Example 1, and FIG. 13(b) is a graph in which the area surrounded by the dashed line in FIG. 13(a) is normalized. FIG. 14 is a graph showing measurement results of the maximum tensile strength of joints formed in the metal bonded bodies of Example 1 and Comparative Example 1.
[0011] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. In the following description, identical elements or elements having the same functions will be designated by the same reference numerals, and redundant explanations will be omitted. In this specification, the term "same" and similar words are not limited to "completely identical." Furthermore, since the drawings are intended to conceptually explain the embodiments, the dimensions and ratios of the depicted components may differ from the actual dimensions.
[0012] (1) Overview of the joining method for metal materials In the joining method according to this embodiment, a butt pressure is applied to a pair of workpieces, as in the pressure-controlled voltage welding method described in Patent Document 1. Furthermore, electrical heating is performed on at least one of the workpieces. The joining method according to this embodiment differs significantly from the solid-state joining method in that a current flows in at least one of the workpieces in a direction intersecting the direction in which the butt pressure is applied. Hereinafter, the joining method according to this embodiment may also be referred to as a pressure-controlled side voltage welding method.
[0013] As a specific example, the method for joining metal materials according to this embodiment includes a preparation step of stacking a first material to be joined containing a first metal and a second material to be joined containing a second metal in a predetermined direction; a heating step of heating at least one of the interface to be joined between the first material to be joined and the second material to be joined, a first portion of the first material to be joined that is located near the interface to be joined, and a second portion of the second material to be joined that is located near the interface to be joined; and a joining step of applying pressure along a predetermined direction toward the interface to be joined to join the first material to the second material to be joined, wherein in the heating step, a current is passed through at least one of the interface to be joined, the first portion, and the second portion in an intersecting direction that intersects with the predetermined direction.
[0014] (2) Bonding Apparatus An example of a bonding apparatus used to carry out the bonding method according to this embodiment will be described below with reference to Fig. 1 etc. Fig. 1 is a schematic diagram of the bonding apparatus according to this embodiment. The bonding apparatus 10 shown in Fig. 1 is an apparatus for bonding a first workpiece 2 and a second workpiece 3 by a pressure-controlled side-applied voltage bonding method.
[0015] 2(a) and 2(b), the first and second workpieces 2 and 3 to be joined by the joining apparatus 10 and the metal joined body, which is a joined body of the first and second workpieces 2 and 3, will be described in detail. FIG. 2(a) is a schematic cross-sectional view showing the first and second workpieces 2 and 3 before joining, and FIG. 2(b) is a schematic cross-sectional view showing the metal joined body. As shown in FIG. 2(a), the first and second workpieces 2 and 3 are each a member (metal material) having a metal phase that can be metallurgically joined. A joining interface 4 is formed between the first and second workpieces 2 and 3. The joining interface 4 corresponds to the abutment surface of the second workpiece 3 against the first workpiece 2 and the abutment surface of the first workpiece 2 against the second workpiece 3. Hereinafter, the overlapping direction of the first and second workpieces 2 and 3 will be referred to as the predetermined direction (butt direction). In this embodiment, the predetermined direction corresponds to the up-down direction, but the up-down direction is not limited to the vertical direction. Note that each of the first material to be joined 2 and the second material to be joined 3 may have room temperature strength sufficient to withstand pressure (details of which will be described later) applied during the manufacturing of the metal bonded body. In this case, deformation at unintended locations during the manufacturing of the metal bonded body can be prevented.
[0016] The first and second workpieces 2 and 3 may each be a bulk material containing a single metal or multiple metals. In the latter case, at least one of the first and second workpieces 2 and 3 may be an alloy bulk material. The first and second workpieces 2 and 3 may contain the same or different materials. The first and second workpieces 2 and 3 may contain metals such as iron, titanium, aluminum, copper, magnesium, chromium, zinc, nickel, molybdenum, and cobalt. The metal (first metal) contained in the first workpiece 2 is not limited to the base material of the first workpiece 2. For example, the metal may be a metal contained in a plating applied to the first workpiece 2. Similarly, the metal (second metal) contained in the second workpiece 3 is not limited to the base material of the second workpiece 3. When at least one of the first material to be joined 2 and the second material to be joined 3 is an alloy, the alloy is, for example, a titanium alloy, a steel such as a high-tensile steel plate, a stainless steel, an aluminum alloy, a copper alloy, a magnesium alloy, etc. In this embodiment, the first material to be joined 2 is a copper bulk material, and the second material to be joined 3 is an aluminum bulk material. Therefore, the high-temperature strength of the metal (first metal) contained in the first material to be joined 2 is higher than the high-temperature strength of the metal (second metal) contained in the second material to be joined 3. The high-temperature strength of a metal is the strength at the desired joining temperature.
[0017] The shapes and sizes of the first and second workpieces 2 and 3 are not particularly limited, and may be bulk materials such as plates, sheets, rods, and square bars. The shapes of the first and second workpieces 2 and 3 may be the same or different. In this embodiment, the shapes of the first and second workpieces 2 and 3 are both cylindrical. The sizes of the first and second workpieces 2 and 3 may be the same or different. For example, the cross-sectional area of the first and second workpieces 2 perpendicular to the stacking direction may be the same as or different from the cross-sectional area of the second workpieces 3 perpendicular to the stacking direction.
[0018] As shown in FIG. 2B , in the metal bonded body 1 of the first and second workpieces 2 and 3, the first and second workpieces 2 and 3 are integrated by a bonded portion 5. The bonded portion 5 has a bonded surface 6 located between the first and second workpieces 2 and 3, and a burr portion 7 located outside the bonded surface 6 when viewed from a predetermined direction. The bonded portion 5 corresponds to a portion that contributes to the bonding of the first and second workpieces 2 and 3. The bonded portion 5 may include an intermetallic compound layer containing the first metal and the second metal. The thickness of the intermetallic compound layer in the bonded portion 5 is, for example, 1 μm or less. In this case, the adverse effect of the intermetallic compound layer on the bonding strength can be effectively reduced. The thickness of the intermetallic compound layer may be 500 nm or less, 300 nm or less, 200 nm or less, or 100 nm or less. The burr portion 7 is a portion where the burr has cooled. The flash portion 7 may contain a liquid-phase cooled material. In this case, the flash portion 7 contains melting marks resulting from the liquid phase.
[0019] Returning to Fig. 1 , the bonding apparatus 10 has a pressure mechanism 20, a heating mechanism 30, a control unit 50, and a power source 60. The pressure mechanism 20 is a mechanism that brings the first material to be bonded 2 into contact with the second material to be bonded 3 to form a bonded interface 4, and applies a pressure P (see Fig. 2(a) and (b)) to the bonded interface 4 in a predetermined direction. The pressure mechanism 20 is, for example, an electric servo press, a hydraulic press, or a pneumatic press. From the viewpoint of applying a high pressure to the bonded interface 4, the pressure mechanism 20 may be an electric servo press. The pressure mechanism 20 has a first fixing unit 21 and a second fixing unit 22.
[0020] The first fixing portion 21 is a base portion that fixes the first workpiece 2. Therefore, when the joining device 10 is in use, the first workpiece 2 is fixed on the first fixing portion 21. Although not shown, the first fixing portion 21 may be provided with a structure (claw, arm, etc.) for fixing the first workpiece 2. The second fixing portion 22 is a portion that fixes the second workpiece 3 and is located above the first fixing portion 21. Therefore, when the joining device 10 is in use, the second workpiece 3 is fixed to the bottom of the second fixing portion 22. Although not shown, the second fixing portion 22 may be provided with a structure (claw, arm, etc.) for fixing the second workpiece 3. At least one of the first fixing portion 21 and the second fixing portion 22 is controlled to be movable along a predetermined direction. When the first fixing portion 21 and the second fixing portion 22 approach each other, pressure P can be applied to the joined interface 4 in a predetermined direction. The movement of at least one of the first fixing portion 21 and the second fixing portion 22 is controlled by, for example, the control unit 50 .
[0021] The heating mechanism 30 is a mechanism that heats at least one of the interface 4 to be joined, the first portion 2a of the first material 2 to be joined that is located near the interface 4 to be joined, and the second portion 3a of the second material 3 to be joined that is located near the interface 4 to be joined. The heating mechanism 30 passes a current through at least one of the interface 4 to be joined, the first portion 2a, and the second portion 3a in accordance with the control of the control unit 50 and the power supply from the power source 60. The heating mechanism 30 is, for example, a heating device that uses direct resistance heating. The heating mechanism 30 has a first portion 31 and a second portion 32.
[0022] FIG. 3 is a schematic cross-sectional view of the first portion 31 of the heating mechanism 30. The first portion 31 includes a drive mechanism 33, a rail 34, and an electrode unit 35. The drive mechanism 33 is a mechanism for moving the electrode unit 35 toward the pressure mechanism 20 and away from the pressure mechanism 20, and includes a pump 33a and a cylinder 33b. The pump 33a is a component that controls the movement of the cylinder 33b, such as an air pump or a hydraulic pump. The cylinder 33b is a columnar component that moves back and forth in response to the operation of the pump 33a. The movement speed of the cylinder 33b controlled by the pump 33a is, for example, 50 mm / sec or more and 500 mm / sec or less. The electrode unit 35 is fixed to a stage 33b1 located at the tip of the cylinder 33b. Therefore, the electrode unit 35 moves in response to the operation of the cylinder 33b. In this embodiment, the electrode unit 35 moves back and forth (linearly) in response to the cylinder 33b moving back and forth in a horizontal direction perpendicular to the predetermined direction. The position of the cylinder 33b in a predetermined direction (vertical direction) is changeable, thereby making it possible to change the path (current path) of the current flowing from the heating mechanism 30 into the first workpiece 2 and / or the second workpiece 3.
[0023] The rail 34 is a member that restricts the left-right movement of the cylinder 33b and extends in one horizontal direction. By providing the rail 34, the cylinder 33b and the electrode unit 35 are able to move back and forth in the one direction. The rail 34 may or may not contact the cylinder 33b. The rail 34 may or may not contact the pressure mechanism 20.
[0024] The electrode portion 35 is a conductive member (side electrode) for passing current through at least one of the interface 4, the first portion 2a, and the second portion 3a, and is fixed to the tip of the cylinder 33b. Therefore, the electrode portion 35 is movable in accordance with the movement of the cylinder 33b. The electrode portion 35 includes a base portion 35a, a main portion 35b, and a connecting portion 35c (e.g., a fastening member such as a nut or bolt) connecting the base portion 35a and the main portion 35b. The base portion 35a is fixed to the cylinder 33b and may be, for example, a conductive metal or alloy part. From the viewpoint of heat dissipation of the electrode portion 35, the base portion 35a may be made of a copper plate or the like. A tip portion 35a1 of the base portion 35a is located closer to the pressurizing mechanism 20 than the cylinder 33b in the horizontal direction and is thinner than the other portions of the base portion 35a. The tip portion 35a1 is provided with a hole 35a2 through which the connecting portion 35c can communicate, and the main portion 35b is placed on the hole 35a2. The main portion 35b abuts against the portion of the base 35a that is connected to the tip portion 35a1, so that the main portion 35b can be stably placed on the tip portion 35a1. The tip portion 35a1 does not overlap the cylinder 33b, but this is not a limitation.
[0025] The main portion 35b is a component of the electrode portion 35 that comes into contact with the first material 2 and / or the second material 3, and is, for example, a conductive metal or alloy component. Therefore, the main portion 35b (particularly the main portion 42 described below) can also be referred to as an electrode for the first material 2, the second material 3, and the interface 4 to be joined. From the standpoint of heat dissipation, the main portion 35b may be made of a copper plate or the like. The main portion 35b is configured to be removable from the electrode portion 35 by releasing the connection between the base portion 35a and the main portion 35b by the connecting portion 35c. This facilitates dealing with damage or wear of the main portion 35b and replacing it with an electrode component that matches the shapes of the first material 2 and the second material 3 to be joined.
[0026] FIG. 4A is a plan view of the main portion 35b included in the electrode portion 35, and FIG. 4B is a side view of the main portion 35b included in the electrode portion 35. As shown in FIGS. 4A and 4B, the main portion 35b has a base end 41 and a main portion 42. The base end 41 is provided with a hole 41a through which the connecting portion 35c can communicate. The width W1 of the base end 41 is adjusted depending on the shape of the workpiece, but is, for example, 50 mm or more. From the viewpoint of thermal durability during current application, the thickness T1 of the base end 41 is, for example, 3 mm or more. The main portion 42 extends horizontally from the base end 41 toward the pressure mechanism 20 and has a substantially trapezoidal shape in a plan view. The width of the main portion 42 narrows as it approaches the pressure mechanism 20. Therefore, the width of the main portion 42 increases as it moves away from the first workpiece 2, the second workpiece 3, and the interface 4 to be joined. This suppresses interference of the main portion 35b with the pressure mechanism 20 and the like, and also reduces the likelihood of damage to the main portion 42 due to excessive heating. The maximum width of the main portion 42 is the same as the width W1 of the base end 41. The minimum width W2 of the main portion 42 is, for example, equal to or greater than the diameter of the first workpiece 2 and the second workpiece 3, and equal to or less than half the width W1. From the viewpoint of heat dissipation from the main portion 35b, the length L2 of the main portion 42 is, for example, equal to or greater than twice the length L1 of the base end 41.
[0027] The thickness T2 of the tip portion 42a included in the main portion 42 is thinner than the thickness T1 of the base portion 41, and is, for example, 2 mm or less. This makes it possible to restrict the current path of the main portion 42 so that the current density is highest at the first workpiece 2, the second workpiece 3, or the interface 4 to be joined. By implementing this restriction, Joule heating in the main portion 35b can be suppressed. The length L3 of the tip portion 42a is not particularly limited, but is, for example, 1 / 5 or less of the length L2 of the main portion 42. A recess 42b into which the first workpiece 2 or the second workpiece 3 can be fitted is provided on the tip surface of the tip portion 42a. The thickness of the main portion 42 other than the tip portion 42a is the same as the thickness T1 of the base portion 41.
[0028] The first portion 31 and the second portion 32 have the same configuration. Therefore, although not shown, the second portion 32 also has a drive mechanism corresponding to the drive mechanism 33, a rail corresponding to the rail 34, and an electrode portion 35A corresponding to the electrode portion 35 (see FIG. 6A, etc.). Therefore, in this embodiment, the heating mechanism 30 has a pair of electrodes (electrode portions 35, 35A) and a movement mechanism (the drive mechanism 33 and the above-mentioned drive mechanism) that moves the pair of electrodes in the horizontal direction. The first portion 31 and the second portion 32 are linked to each other. For example, the electrode portion 35 of the first portion 31 and the electrode portion 35A of the second portion 32 move toward the first workpiece 2 at the same time and move away from the first workpiece 2 at the same time.
[0029] The control unit 50 is a device that controls the pressure mechanism 20, the heating mechanism 30, and the power supply 60, and is composed of, for example, a servo press controller, an operation panel, a display device, a PC including a CPU (Central Processing Unit), a ROM (Read Only Memory), a RAM (Random Access Memory), etc. Through control by the control unit 50, for example, the pressure application by the pressure mechanism 20, the movement timing of each electrode unit in the heating mechanism 30, and the timing of current application are synchronized. The PC included in the control unit 50 stores, for example, a program that controls the pressure mechanism 20, the heating mechanism 30, and the power supply 60 to perform the pressure-controlled side voltage connection method.
[0030] The power supply 60 is a device used for heating at least one of the first workpiece 2, the second workpiece 3, and the welded interface 4 by the heating mechanism 30, and is, for example, a DC inverter welding power supply. The output of the power supply 60 is adjusted as appropriate depending on the shapes of the first workpiece 2 and the second workpiece 3, etc.
[0031] (3) Details of the method for joining metal materials Next, the details of the method for joining metal materials according to this embodiment will be described with reference to Figures 5 to 7. Figure 5 is a flowchart of the joining method. Figures 6(a) and 6(b) and Figures 7(a) and 7(b) are schematic cross-sectional views for explaining the joining method. In the following, a joining apparatus 10 is used, but the joining apparatus 10 does not necessarily have to be used in the method for joining metal materials according to this embodiment.
[0032] First, the first workpiece 2 and the second workpiece 3 are stacked in a predetermined direction (step ST1). In step ST1, as shown in Fig. 6(a), the first workpiece 2 is fixed to the first fixing part 21, and the second workpiece 3 is fixed to the second fixing part 22, and then the second fixing part 22 is moved toward the first fixing part 21. This brings the second workpiece 3 into contact with the first workpiece 2. This completes the preparation for carrying out the method for joining metal materials. For this reason, in this specification, step ST1 is also referred to as a preparation step.
[0033] Next, pressure is applied to the first and second workpieces 2 and 3 toward the bonded interface 4 and along the lamination direction (step ST2, load application). The pressure in step ST2 is not a small pressure for maintaining the bonded interface 4, but a value that varies depending on the yield stress of the first and second workpieces 2 and 3. That is, the pressure varies appropriately depending on the materials of the first and second workpieces 2 and 3. The pressure in step ST2 and the pressures in steps ST2 and thereafter may be the same or different. In this embodiment, the pressure is constant, for example, around 100 MPa, but is not limited to this. For example, when bonding copper and aluminum materials, the pressure is 80 MPa or more, 85 MPa or more, or 90 MPa or more, and 120 MPa or less, 110 MPa or less, or 105 MPa or less.
[0034] Next, the electrode portions 35, 35A are brought close to the first workpiece 2 and the second workpiece 3 (step ST3, inserting side electrodes). In step ST3, the electrode portions 35, 35A are moved so as to be inserted between the first fixing portion 21 and the second fixing portion 22. This brings the electrode portions 35, 35A into contact with at least one of the first workpiece 2, the second workpiece 3, and the interface 4 to be joined. In step ST3 of this embodiment, as shown in FIG. 6B, the electrode portions 35, 35A are brought into contact with the first workpiece 2 so as to be separated from the interface 4 to be joined. At this time, the distance from the electrode portions 35, 35A to the interface 4 along the predetermined direction is, for example, 1 mm or more and 3 mm or less.
[0035] Next, current is passed through the electrode portions 35, 35A via at least one of the first workpiece 2, the second workpiece 3, and the interface 4 to be joined (step ST4, start of current flow). In step ST4, current is passed through the electrode portions 35, 35A to heat at least one of the interface 4 to be joined, the first portion 2a of the first workpiece 2 located near the interface 4 to be joined, and the second portion 3a of the second workpiece 3 located near the interface 4 to be joined. This causes a current to flow in a direction intersecting the predetermined direction through at least one of the interface 4 to be joined, the first portion 2a, and the second portion 3a, thereby locally heating the interface 4 to be joined (electrical heating). For this reason, in this specification, step ST4 is also referred to as a heating step.
[0036] From the viewpoints of suppressing HAZ softening and taking into account the strength difference between the workpieces, in step ST4, a metal material with high high-temperature strength may be locally heated. Taking these viewpoints into account, in step ST4 of this embodiment, as shown in FIG. 7A, current is passed through the electrodes 35, 35A via the first workpiece 2. This allows at least the first workpiece 2 (particularly the first portion 2a) to be heated. In this case, the contact resistance of the first workpiece 2 allows the first portion 2a to be selectively heated in a short time. The vicinity of the first portion 2a (e.g., the interface 4 to be joined, the second portion 3a, etc.) is also heated by thermal conduction. The current density applied to the first workpiece 2 and the second workpiece 3 is adjusted depending on the materials contained in the first workpiece 2 and the second workpiece 3. For example, when joining a copper material and an aluminum material, the current density is 50 A / mm 2 or more, and 2 The higher the resistance of the materials to be joined, the lower the current density.
[0037] In step ST4, at least the first portion 2a is heated to a bonding temperature determined according to the pressure. In other words, in the heating step, the bonding temperature between the first material 2 and the second material 3 is determined by the pressure already applied to the first material 2 and the second material 3. The mechanism for determining the pressure and the bonding temperature between the first material 2 and the second material 3 is as described in, for example, Republished Patent Publication WO2019 / 181360.
[0038] In step ST4, at least the first workpiece 2 is heated, thereby forming a softened region (not shown) in the first portion 2a and / or its vicinity. The softened region is a solid-phase region that is softer than both the first workpiece 2 and the second workpiece 3 at room temperature and exhibits fluidity. The softened region may contain a small amount of liquid phase resulting from melting the first workpiece 2 and / or the second workpiece 3. The yield stress of the softened region is smaller than both the yield stress of the first workpiece 2 and the yield stress of the second workpiece 3 at room temperature. The softened region may be formed, for example, from a portion of the first workpiece 2 located near the interface 4 to be joined, or from the contact point between the first workpiece 2 and the second workpiece 3 to be joined. In this embodiment, because the first workpiece 2 is energized, the softened region tends to be formed from a portion of the first workpiece 2 located near the interface 4 to be joined.
[0039] In step ST4, the pressure may be set so that a liquid phase (not shown) containing at least one of the first metal contained in the first workpiece 2 and the second metal contained in the second workpiece 3 is generated near the bonded interface 4. Optimizing the pressure (i.e., the bonding temperature) can control the amount of liquid phase generated and the discharge behavior of the liquid phase. This can also suppress defects at the bonded interface 4 and the heat-affected zone. Therefore, the setting of the pressure in this bonding method is important. This liquid phase may be the liquid first metal, the liquid second metal, or a melt such as a eutectic of the first and second metals. If the liquid phase corresponds to a eutectic melt, in step ST4, electrical heating is performed to the eutectic temperature of the first and second metals. The liquid phase is generated, for example, in the softened region or at a location adjacent to the softened region. The fluidity of the liquid phase is significantly higher than that of the softened region. Therefore, in the joining step described below, the liquid phase tends to be preferentially pushed out from between the first workpiece 2 and the second workpiece 3 to be joined.
[0040] Next, after the current supply to the electrodes 35, 35A is stopped, the electrodes 35, 35A are moved away from the first workpiece 2 and the second workpiece 3 as shown in FIG. 7B (step ST5, side electrode removal). In step ST5, to prevent damage to the electrodes 35, 35A due to discharge, current supply to the electrodes 35, 35A is stopped before the electrodes 35, 35A are moved. For example, the total length of the first workpiece 2 and the second workpiece 3 along the predetermined direction at the start of step ST2 is used as a reference, and current supply to the electrodes 35, 35A is stopped when the approach allowance (i.e., the amount of reduction in the total length) reaches 0.3 mm. Then, immediately after current supply to the electrodes 35, 35A is stopped, the electrodes 35, 35A are moved. For example, the electrodes 35, 35A are moved 0.01 seconds after current supply to the electrodes 35, 35A is stopped. This makes it possible to prevent damage to the electrode portions 35, 35A that occurs when the first workpiece 2 and the second workpiece 3 are joined.
[0041] Next, the moving speed of the first workpiece 2 and the second workpiece 3 is increased (step ST6, moving speed UP). Then, pressure is applied toward the joining interface 4 in a predetermined direction to join the first workpiece 2 and the second workpiece 3 to each other. When the power supply to the electrodes 35, 35A is stopped in step ST5, the temperature of the first portion 2a and the like decreases. Depending on the degree of temperature decrease, the joining force between the first workpiece 2 and the second workpiece 3 may become insufficient. To avoid this problem, the moving speed is increased in step ST6, so that the first workpiece 2 and the second workpiece 3 are joined before the temperatures of the heated first workpiece 2 and / or second workpiece 3 completely decrease. As a result, the newly formed surfaces of the first workpiece 2 and the second workpiece 3 come into good contact with each other, and the butt-joining of the first workpiece 2 and the second workpiece 3 is completed. 2B, a metal bonded body 1 is formed in which the first and second workpieces 2 and 3 are integrated by a bonding portion 5. For this reason, in this specification, step ST6 is also referred to as a bonding process. Note that this bonding method is performed within a few seconds or within one second, for example, depending on the heating rate and other factors.
[0042] If a softened region has been formed by step ST5, in step ST6, pressure is applied in the lamination direction toward the bonded interface 4 to deform the softened region, thereby bonding the first and second workpieces 2 and 3 to each other. Therefore, the bonding process begins during the heating process. When the bonded interface 4 and its vicinity are further deformed, at least a portion of the softened region (if a liquid phase is included, at least a portion of the liquid phase) is extruded from between the first and second workpieces 2 and 3 as a burr. At this time, if impurities, oxide coatings, etc. are present at or near the bonded interface 4, the impurities, etc. are mixed into the liquid phase and are extruded from between the first and second workpieces 2 and 3 (e.g., the bonded interface 4). Therefore, the impurities, oxide coatings, etc. tend to be concentrated in the burr. As a result, the newly formed surfaces of the first material 2 to be joined and the second material 3 to be joined come into good contact with each other, and a butt joining (solid-state joining) is performed between the first material 2 to be joined and the second material 3 to be joined. In other words, the joining portion between the first material 2 to be joined and the second material 3 to be joined is less likely to have an area that adversely affects the joining strength between the first material 2 to be joined and the second material 3 to be joined.
[0043] When the maximum tensile strength (first maximum tensile strength) of the first workpiece 2 is greater than the maximum tensile strength (second maximum tensile strength) of the second workpiece 3 in the butt-joint direction, the maximum tensile strength of the weld 5 of the metal welded body 1 can be set to 85% or more, 90% or more, or 95% or more of the second maximum tensile strength. Satisfying this parameter indicates that the joining strength of the first workpiece 2 and the second workpiece 3 at the weld 5 is good. When ordinary fusion welding is used, this is about 60%, and when friction stir welding is used, this is about 70%. The above-mentioned maximum tensile strength is measured, for example, by the method described in the examples below.
[0044] In the above-described method for joining metal materials, joining parameters other than pressure and joining temperature (e.g., joining time and contact allowance) are appropriately set depending on the material, shape, size, etc. of the materials to be joined. Similarly, the timing for releasing the pressure is also appropriately set. Note that the pressure applied to the joining interface 4 may be increased at the end of the joining process in order to remove burrs and to bring the newly formed surfaces into stronger contact.
[0045] The effects achieved by the joining apparatus 10 according to the present embodiment and the method for joining metal materials using the joining apparatus 10 described above will be described with reference to FIGS. 8(a) to 8(d). FIG. 8(a) is a schematic cross-sectional view illustrating the electric heating method in a reference example, and FIG. 8(b) is a schematic perspective view showing the first workpiece to be joined used in the reference example. FIG. 8(c) is a schematic cross-sectional view illustrating the electric heating method in this embodiment, and FIG. 8(d) is a schematic perspective view showing the first workpiece to be joined used in this embodiment. The first workpiece to be joined 2 and the second workpiece to be joined 3 shown in FIGS. 8(a) to 8(d) are each a rectangular prism. The butting surfaces of the first workpiece to be joined 2 and the butting surfaces of the second workpiece to be joined 3 each have a square shape with one side measuring 200 mm.
[0046] As shown in (a) of Fig. 8, in the reference example, the first workpiece 2 and the second workpiece 3 are electrically heated by the pressure-controlled voltage welding method described in Patent Document 1. Therefore, a current E1 flows from the second fixing portion 122 to the first fixing portion 121 via the first workpiece 2 and the second workpiece 3. In this case, as shown in (b) of Fig. 8, the area corresponding to the range through which the current E1 flows is 200 mm x 200 mm. Here, for example, if the welding area between the first workpiece 2 and the second workpiece 3 is 200 mm x 200 mm and the first workpiece 2 and the second workpiece 3 are both steel materials for building structures, it is estimated that a current of approximately 1.5 million A is required to join the first workpiece 2 and the second workpiece 3 by the pressure-controlled voltage welding method (applied pressure: 250 MPa). For this reason, the joining device (especially the power source for energizing) used to join large structures using the pressure-controlled voltage joining method becomes so large and expensive that it is difficult to put it into practical use.
[0047] In addition, in the pressure-controlled voltage welding method, the materials to be welded are heated simultaneously. Therefore, if the metallic material contained in the first material to be welded 2 and the metallic material contained in the second material to be welded 3 are different from each other and the curves of the temperature dependence of the strength (deformation resistance) of each metallic material do not intersect, the softer material of the metallic materials will deform first. For this reason, there are cases where a good dissimilar joint cannot be obtained by simply performing the pressure-controlled voltage welding method, so various measures can be taken.
[0048] In contrast, when using the joining apparatus 10 according to this embodiment, as shown in FIG. 8C, current E2 flows from the electrode 35 to the electrode 35A via at least the first workpiece 2. In this case, as shown in FIG. 8D, the area corresponding to the range through which current E2 flows is 200 mm × T2 (mm). For example, if T2 is 2 mm and the first workpiece 2 and the second workpiece 3 are both steel materials for architectural structures, it is estimated that a current of approximately 15,000 A is required to join the first workpiece 2 and the second workpiece 3 using the joining apparatus 10 (applied pressure: 250 MPa). In other words, when the joining apparatus 10 is used, the first workpiece 2 and the second workpiece 3 can be joined with a current approximately 1 / 100 of that required in the above-described reference example. Therefore, the method for joining metal materials using the joining apparatus 10 (pressure-controlled side voltage joining method) makes it possible to join large structures at a reasonable price and with practical equipment.
[0049] In addition, with the pressure-controlled side voltage welding method, when the metallic materials contained in the first workpiece 2 and the second workpiece 3 are different from each other and the curves of the temperature dependence of the strength (deformation resistance) of each metallic material do not intersect, it is possible to carry out local heating so that the harder material of each metallic material becomes hotter. This makes it possible to simultaneously deform the first workpiece 2 and the second workpiece 3, thereby realizing good dissimilar joining.
[0050] Here, with reference to FIGS. 9(a), 9(b), and 9(c), the reason why the temperature of the interface between the workpieces is uniformly increased by side current application using the electrode portions 35, 35A will be explained. FIG. 9(a) is a schematic perspective view of side current application to the first workpiece, and FIG. 9(b) is a schematic cross-sectional view of side current application to the first workpiece. FIG. 10 is a schematic diagram for explaining a method for measuring thermal emissivity using a thermal imaging camera. Hereinafter, side current application will be performed only on the first workpiece 2 having a diameter of 5 mm, as shown in FIGS. 9(a) and 9(b). At this time, the electrode portions 35, 35A are positioned 1 mm below the top surface 2f of the first workpiece 2. This allows the top surface 2f to be heated by thermal conduction. The top surface 2f may correspond to a portion of the interface between the workpieces when the workpieces are actually joined. Here, black paint B is applied to the top surface 2f, and the temperature of the black paint B is measured by a thermal imaging camera C. Since no significant difference was observed in the measured temperature distribution of the black paint B, it can be considered that the temperature of the joined interface is uniformly raised even by side current application.
[0051] When the current value flowing through the electrode portions 35, 35A via the first workpiece 2 was 4000 A, the temperature of the black body paint B was 368°C one second after the start of side current application, and 405°C two seconds after the start of side current application. When the current value was 5000 A, the temperature of the black body paint B was 698°C one second after the start of side current application, and 671°C two seconds after the start of side current application. When the current value was 6000 A, the temperature of the black body paint B was 783°C one second after the start of side current application, and 768°C two seconds after the start of side current application. When the current value was 6000 A and the side current was stopped one second after the start of side current application, the temperature of the black body paint B was about 500°C about 0.1 seconds after the stop. This suggests that there is a possibility that the temperature of the interface to be joined drops sharply after the side current flow performed when joining materials to be joined is stopped.
[0052] In this embodiment, the joining temperature between the first material to be joined 2 and the second material to be joined 3 is determined by the pressure P. This makes it possible to accurately determine the joining temperature between the first material to be joined 2 and the second material to be joined 3.
[0053] In this embodiment, the high-temperature strength of the first metal contained in the first workpiece 2 is higher than the high-temperature strength of the second metal contained in the second workpiece 3, and in step ST4, current may be passed through at least one of the workpiece interface 4 and the first workpiece 2. In this case, the first metal, which is a hard material, is heated to a higher temperature than the second metal, softening the first workpiece 2. This eliminates the difference in strength at the joint 5 between the first workpiece 2 and the second workpiece 3, allowing the first workpiece 2 and the second workpiece 3 to deform simultaneously. In addition, HAZ softening is less likely to occur in the second workpiece 3. Furthermore, at least a portion of the joint surface of the first workpiece 2, which contains the hard first metal, can be made to protrude toward the second workpiece 3.
[0054] In this embodiment, in step ST4, a liquid phase containing at least one of the first metal and the second metal is generated near the bonded interface 4, and in step ST6, at least a part of the liquid phase may be extruded from between the first workpiece 2 and the second workpiece 3. In this case, for example, an oxide film, impurities, etc. that existed between the first workpiece 2 and the second workpiece 3 may be extruded together with the liquid phase. This makes it possible to remove substances that adversely affect the bond strength at the bonded portion 5 (particularly the bonded surface 6) from between the first workpiece 2 and the second workpiece 3. Therefore, the bond strength of the metal bonded body 1 can be improved.
[0055] In this embodiment, the heating mechanism 30 has a pair of electrode parts 35, 35A and a drive mechanism 33 that moves the electrode part 35 in the horizontal direction. In this case, it is possible to easily control the timing of heating (timing of energizing) the first workpiece 2 and / or the second workpiece 3. In addition, since it is possible to prevent interference between the electrode parts 35, 35A and the pressure mechanism 20, the electrode parts 35, 35A are less likely to be damaged.
[0056] In this embodiment, the width of each of the electrode portions 35, 35A may increase in plan view as it gets farther away from the bonded interface 4. In this case, the durability of the electrode portions 35, 35A can be improved.
[0057] The following describes a method for joining metal materials according to a modification of the above embodiment. In the description of the modification, descriptions that overlap with the above embodiment will be omitted, and only differences will be described. In other words, to the extent technically possible, the descriptions of the above embodiment may be used appropriately in the modification.
[0058] In the method for joining metal materials according to the modified example, the first workpiece 2 and the second workpiece 3 are electrically heated not only using the electrodes 35, 35A but also in a manner similar to the pressure-controlled voltage welding method described above. In this case, although not shown, the pressure mechanism includes, in addition to the first and second fixing portions 21 and 22, a current-carrying mechanism that applies current from the first fixing portion 21 to the second fixing portion 22 via the first and second workpieces 2 and 3. In this case, using the current-carrying mechanism, in step ST4, a second current (not shown) is passed through the butt joint interface 4, the first portion 2a, and the second portion 3a in the butt joint direction. This allows the entire first workpiece 2 and the second workpiece 3 to be heated, which is expected to shorten the time required to join the first and second workpieces 2 and 3 and improve the joint strength. Note that the current-carrying mechanism may be supplied with power by a power source different from the power source 60, or may be supplied with power by the power source 60.
[0059] In step ST3 of the above embodiment, as shown in FIG. 6B , the electrode portions 35, 35A are brought into contact with the first workpiece 2 so as to be spaced from the workpiece interface 4. However, in step ST3 of the modified example, the electrode portions 35, 35A may be brought into contact with the second workpiece 3 so as to be spaced from the workpiece interface 4. In this case, the second workpiece 3 can be locally electrically heated. Alternatively, one of the electrode portions 35, 35A may be brought into contact with the first workpiece 2, and the other may be brought into contact with the second workpiece 3. In this case, both the first portion 2a and the second portion 3a can be electrically heated. This allows rapid solid-state joining when the first workpiece 2 and the second workpiece 3 are homogeneously joined. In either case, at least one of the electrode portions 35, 35A may be brought into contact with the second workpiece 3.
[0060] The method and apparatus for joining metallic materials according to the present disclosure are as described in [1] to [9] below, and have been described in detail based on the above-mentioned embodiments. [1] A method for joining metallic materials, comprising: a preparation step of stacking a first material to be joined containing a first metal and a second material to be joined containing a second metal in a predetermined direction; a heating step of heating at least one of an interface to be joined between the first material to be joined and the second material to be joined, a first portion of the first material to be joined located near the interface to be joined, and a second portion of the second material to be joined located near the interface to be joined; and a joining step of applying pressure along the predetermined direction toward the interface to be joined to join the first material to the second material to be joined, wherein in the heating step, a current is passed through at least one of the interface to be joined, the first portion, and the second portion in an intersecting direction that intersects the predetermined direction. [2] The joining method according to [1], in which the joining temperature between the first material to be joined and the second material to be joined is determined by the pressure. [3] The joining method according to [1] or [2], wherein in the heating step, a second current along the predetermined direction is passed through the joined interface, the first portion, and the second portion. [4] The joining method according to any of [1] to [3], wherein the high-temperature strength of the first metal is higher than the high-temperature strength of the second metal, and in the heating step, the current is passed through the joined interface and at least one of the first joined materials. [5] The joining method according to any of [1] to [4], wherein in the heating step, a liquid phase containing at least one of the first metal and the second metal is generated in the vicinity of the joined interface, and in the joining step, at least a part of the liquid phase is pushed out from between the first joined material and the second joined material.[6] A bonding device comprising: a pressure mechanism that abuts a first workpiece containing a first metal against a second workpiece containing a second metal to form a bonded interface and applies pressure to the bonded interface in a predetermined direction; a heating mechanism that heats at least one of the bonded interface, a first portion of the first workpiece material located near the bonded interface, and a second portion of the second workpiece material located near the bonded interface; and a control unit that controls the pressure mechanism and the heating mechanism, wherein the heating mechanism passes a current through at least one of the bonded interface, the first portion, and the second portion along a direction intersecting the predetermined direction. [7] The bonding device described in [6], wherein the heating mechanism has a pair of electrodes and a movement mechanism that moves the pair of electrodes in a horizontal direction perpendicular to the predetermined direction. [8] The bonding device described in [7], wherein the width of each of the pair of electrodes increases as the electrodes are farther from the bonded interface in a plan view. [9] The joining device described in any one of [6] to [8], wherein the pressure mechanism further has a first fixing part that fixes the first workpiece, a second fixing part that fixes the second workpiece, and an electric current mechanism that applies electricity from the first fixing part to the second fixing part via the first workpiece and the second workpiece.
[0061] However, one aspect of the present disclosure is not limited to the above embodiment and the above [1] to [9]. One aspect of the present disclosure can be further modified without departing from the spirit thereof.
[0062] The present disclosure will be explained in more detail by the following examples, but the present disclosure is not limited to these examples.
[0063] Example 1: A 5 mm diameter round bar made of oxygen-free copper (model number: C1020BD-H: >99.9 wt% Cu) was prepared as the first material to be joined, and a 5 mm diameter round bar made of pure aluminum (A1070BD-H14: >99.7 wt% Al) was prepared as the second material to be joined. The length of each round bar was approximately 105 mm to 110 mm. The portion of the first material to be joined to the second material to be joined and the portion of the second material to be joined to the first material to be joined were both degreased with acetone.
[0064] Next, the first and second workpieces were butted together using a servo press (CS-50, manufactured by CORETEC) that was electrically controlled. The applied pressure was 100 MPa, the displacement speed was 15 mm / sec, the protrusion length of the first workpiece (Cu) was 4 mm, and the protrusion length of the second workpiece (Al) was 4 mm. During the butting, a power supply (IS-300A, manufactured by Amada Weld Tech Co., Ltd.) and the heating mechanism 30 described above were used to electrically heat the area of the first workpiece near the interface to be joined (current value: 5500 A). The joining of the first and second workpieces was completed when the total distance between the first and second workpieces reached 6 mm. In Example 1, the time required for joining was approximately 2.2 seconds, and the current flow time was approximately 1.5 seconds. This completes the joining of the first and second workpieces, resulting in the production of the metal joined body shown in FIG. 11 . The liquid phase generated during the joining of the first and second workpieces becomes spherical during the joining and is expelled to the outside of the joining interface as burrs, so that the solid phases of the first and second workpieces are joined at the joining interface.
[0065] Next, to perform electron microscope observation of the joint cross section, Vickers hardness measurement, etc., test pieces measuring 20 mm in length and 1 mm in thickness were prepared from the metal bonded body. First, both ends of the metal bonded body were cut off to the above-mentioned length using a high-speed wet specimen cutter (manufactured by Sakamoto Kogyo, UC62 type). Next, both sides were wet-polished with emery paper (#240) to thin it to the above-mentioned thickness. Next, after wet-polishing using appropriate emery paper (#400 to #4000), mirror polishing was performed using a colloidal silica suspension. The test pieces were obtained in this manner.
[0066] Figure 12(a) is an electron microscope photograph. Figure 12(b) is an enlarged cross-sectional view of the area surrounded by a white square frame in Figure 12(a). Both the photographs shown in Figures 12(a) and 12(b) are the results of observation of a test piece using a field emission scanning electron microscope (JSM-7001FA, manufactured by JEOL Ltd.). As shown in Figure 12(a), a portion of the first bonded material (Cu) located near the second bonded material protrudes toward the second bonded material and in a direction perpendicular to the butt direction. The diameter of the first bonded material at the bonded interface was 7.1 mm. As a result, the diameter of the first bonded material at the interface expanded by approximately 2.1 mm, and the expansion rate of the interface was approximately 196%. As shown in (b) of FIG. 12 , SEM observations confirmed no formation of an intermetallic compound layer (IMC layer) between the first and second bonded materials. Here, thin film samples were prepared from the center and edge of the bonded interface of the metal bonded body using an FIB (Hitachi High-Tech Corporation, FB-2000A) and observed using a TEM (JEOL Ltd., JFM-2100F). The TEM observations confirmed a region (suggested region) approximately 30 nm thick that suggested an IMC layer at the center of the bonded interface, and a suggested region approximately 200 nm to 300 nm thick at the edge of the bonded interface. Therefore, although the formation of the suggested region differs depending on the position of the bonded interface, the thickness of the suggested region near the bonded interface is very thin. Therefore, in Example 1, the adverse effect of the IMC layer on the bond strength of the metal bonded body can be considered to be very limited. When elemental mapping was carried out on the suggested region by TEM-EDS, both Cu and Al phases were confirmed in the suggested region.
[0067] Comparative Example 1: A 3 mm diameter round bar made of pure aluminum (A1070BD-H14: >99.7 wt% Al) was prepared as the first material to be joined, and a 3 mm diameter round bar made of oxygen-free copper (model number: C1020BD-H: >99.9 wt% Cu) was prepared as the second material to be joined. The length of each round bar was approximately 105 mm to 110 mm. The portion of the first material to be joined to the second material and the portion of the second material to be joined to the first material to be joined were each lathe-machined into a tapered shape with a diameter of 2 mm and then degreased with acetone.
[0068] Next, the first and second workpieces were butted together using a servo press (CORETEC, FMS100-B) that was electrically controlled. The applied pressure was 100 MPa, the displacement speed was 10 mm / sec, the protrusion length (length of the protruding portion to be heated) of the first workpiece (Al) was 3 mm, and the protrusion length of the second workpiece (Cu) was 2 mm. During this butting, a power supply (Chuo Seisakusho, HVS4E-160-103) was used to electrically heat the interface between the first and second workpieces along the butting direction (current value: 3000 A). The joining of the first and second workpieces was completed when the total distance between them reached 3.5 mm. In Comparative Example 1, the joining of the first and second workpieces was completed in approximately 0.5 seconds.
[0069] (Hardness Evaluation) The mechanical properties of the joints of Example 1 and Comparative Example 1 were evaluated as follows. Fig. 13(a) is a graph showing the distribution of Vickers hardness of Example 1 and Comparative Example 1. Fig. 13(b) is a graph in which the area surrounded by the dashed line in Fig. 13(a) is normalized. The diameters of the welded materials in Example 1 and Comparative Example 1 are different from each other. In order to accurately compare the HAZ softening behavior, Fig. 13(b) shows values normalized by dividing the actual hardness by the base material hardness.
[0070] As shown in (a) of Figure 13, the hardness of the first bonded material (Cu) near the bonded interface in Example 1 was comparable to that of the Cu base material. This is presumably due to the refinement of crystal grains at the bonded interface and its immediate vicinity, as in the case of homogeneous bonding of copper. The hardness of the first bonded material (Cu) near the bonded interface in Comparative Example 1 was lower than that of the Cu base material. In both Example 1 and Comparative Example 1, a change in hardness due to the occurrence of a HAZ softened portion was confirmed in the first bonded material. However, in both Example 1 and Comparative Example 1, the minimum hardness of the first bonded material was higher than that of the Al base material.
[0071] As shown in Figure 13(b), the second bonded material of Comparative Example 1 tends to soften from the region 1 mm away from the bonded interface toward the bonded interface. The hardness of the softest portion of the second bonded material of Comparative Example 1 was approximately 80% of the hardness of the Al base material. On the other hand, the second bonded material of Example 1 tends to soften gradually from the region 2 mm away from the bonded interface toward the bonded interface. However, the hardness of the softest portion of the second bonded material of Example 1 was approximately 90% of the hardness of the Al base material. Therefore, it can be said that the softening of Al in Example 1 was significantly suppressed compared to Comparative Example 1. This difference is presumably due to the fact that the entire second bonded material (Al) generates heat in Comparative Example 1, while in Example 1, the second bonded material is heated only by heat transfer from the first bonded material. In the second bonded material of Example 1, the bonded interface and its immediate vicinity are heated preferentially, and when this region reaches a temperature at which it can be deformed, it is removed as a burr. For this reason, it is presumed that the final welded portion and its surrounding area in the second welded material were less affected by heat than in Comparative Example 1, and HAZ softening was suppressed.
[0072] (Tensile strength) At room temperature (17°C), the maximum tensile strength of the joints formed in the metal joined bodies of Example 1 and Comparative Example 1 was measured. The measurement results of the maximum tensile strength are shown in Figure 14. The maximum tensile strength is the strength along the lamination direction of the first joined material and the second joined material, and was measured using an autograph testing machine (Shimadzu Autograph AG-10TB, manufactured by Shimadzu Corporation). The distance between the grippers was 80 mm, and the crosshead speed was 1 mm / min.
[0073] 14, the joint efficiency of Example 1 (i.e., the ratio of the maximum tensile strength of the joint to the maximum tensile strength of the second joined material) was 96%. On the other hand, the joint efficiency of Comparative Example 1 was 92%. It is presumed that the difference between Example 1 and Comparative Example 1 is due to whether or not the HAZ softening of the second joined material (Al) was suppressed.
[0074] DESCRIPTION OF SYMBOLS 1...Metal bonded body, 2...First material to be bonded, 2a...First portion, 2f...Top surface, 3...Second material to be bonded, 3a...Second portion, 4...Interface to be bonded, 5...Joint portion, 6...Joint surface, 7...Burr portion, 1 0... Bonding device, 20... Pressure mechanism, 21... First fixing part, 22... Second fixing part, 30... Heating mechanism, 31... First part, 32... Second part, 33... Drive mechanism, 33a... Pump, 33b ...cylinder, 33b1...stage, 34...rail, 35, 35A...electrode portion (electrode), 35a...base portion, 35a1...tip portion, 35a2...hole, 35b...main portion, 35c...connecting portion, 41...base end portion, 41a...hole, 42...main portion, 42a...tip portion, 42b...recess, 50...control portion, 60...power source, B...black body paint, C...thermal imaging camera, E1...current, E2...current.
Claims
1. A method for joining metallic materials, comprising: a preparation step of overlapping a first material to be joined, which contains a first metal, and a second material to be joined, which contains a second metal, in a predetermined direction; a heating step of heating at least one of an interface to be joined between the first material to be joined and the second material to be joined, a first portion of the first material to be joined that is located near the interface to be joined, and a second portion of the second material to be joined that is located near the interface to be joined; and a joining step of applying pressure along the predetermined direction toward the interface to be joined to join the first material to the second material to be joined, wherein in the heating step, a current is passed along a direction that intersects with the predetermined direction to at least one of the interface to be joined, the first portion, and the second portion.
2. The bonding method according to claim 1, wherein the bonding temperature between the first and second materials is determined by the pressure.
3. The bonding method according to claim 1 or 2, wherein in the heating step, a second current is passed through the bonded interface, the first portion, and the second portion along the predetermined direction.
4. The joining method according to claim 1 or 2, wherein the high-temperature strength of the first metal is higher than the high-temperature strength of the second metal, and in the heating step, the electric current is passed through at least one of the joined interface and the first joined material.
5. The joining method according to claim 1 or 2, wherein in the heating step, a liquid phase containing at least one of the first metal and the second metal is generated in the vicinity of the joined interface, and in the joining step, at least a part of the liquid phase is pushed out from between the first joined material and the second joined material.
6. A joining device comprising: a pressure mechanism which brings a first material to be joined, which contains a first metal, into contact with a second material to be joined, which contains a second metal, to form a joining interface, and which applies pressure in a predetermined direction to the joining interface; a heating mechanism which heats at least one of the joining interface, a first portion of the first material to be joined which is located in the vicinity of the joining interface, and a second portion of the second material to be joined which is located in the vicinity of the joining interface; and a control unit which controls the pressure mechanism and the heating mechanism, wherein the heating mechanism passes a current along a direction which intersects with the predetermined direction to at least one of the joining interface, the first portion, and the second portion.
7. The bonding device according to claim 6, wherein the heating mechanism comprises a pair of electrodes and a moving mechanism for moving the pair of electrodes along a horizontal direction perpendicular to the predetermined direction.
8. The bonding apparatus according to claim 7, wherein the width of each of the pair of electrodes in a plan view increases as it gets farther away from the bonded interface.
9. A joining device as described in any one of claims 6 to 8, wherein the pressure mechanism further has a first fixing part that fixes the first workpiece, a second fixing part that fixes the second workpiece, and an electrical current mechanism that passes electrical current from the first fixing part to the second fixing part via the first workpiece and the second workpiece.
Citation Information
Patent Citations
Junction method for hot steel material and its device
JP1987142082A
Method for joining billet in hot rolling
JP1994198308A
Method and device for joining heat resistant alloy
JP1998180463A
Metal material solid-phase bonding method and solid-phase bonding device
WO2019181360A1