Negative electrode material for secondary battery, secondary battery, and method for manufacturing negative electrode material for secondary battery
The composite negative electrode material with a nanoscale active phase dispersed in an amorphous phase of Si, Sn, Ti, Al, or Mg enhances lithium reactivity and utilization, addressing the limitations of existing materials by improving energy density and cycle performance.
Patent Information
- Application Number
- PCT/JP2024/013127
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-31
AI Technical Summary
Current negative electrode materials for secondary batteries, such as lithium-ion batteries, face challenges in achieving high energy density and efficient utilization of active phases due to large irreversible capacity and limited utilization rate, particularly with amorphous materials containing silicon, carbon, and oxygen.
A composite negative electrode material is developed with an active phase dispersed within an amorphous material phase, where the active phase has a particle size of 10 nm or less, and the amorphous phase contains elements like Si, Sn, Ti, Al, or Mg, formed through a method involving organometallic compounds and firing processes to enhance lithium reactivity and conductivity.
This approach significantly increases the utilization rate of the active phase, reduces irreversible capacity, and improves the electrochemical performance by facilitating easier deformation and contact between active phase particles, leading to higher capacity and better cycle characteristics.
Smart Images

Figure JP2024013127_31102024_PF_FP_ABST
Abstract
Description
Negative electrode material for secondary battery, secondary battery, and method for producing negative electrode material for secondary battery CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This disclosure claims the benefit of priority to Japanese Patent Application No. 2023-072353, filed on April 26, 2023, in the Japan Patent Office, the entire contents of which are incorporated herein by reference.
[0002] The present disclosure relates to a negative electrode material for a secondary battery, a secondary battery, and a method for producing a negative electrode material for a secondary battery.
[0003] Non-aqueous electrolyte secondary batteries, especially lithium-ion secondary batteries, have high voltage and high energy density, and are therefore expected to be used in small consumer applications, power storage devices, and power sources for electric vehicles. As higher energy densities are required for batteries, the use of negative electrode materials with high theoretical capacity density is expected.
[0004] Patent Document 1 proposes "a method for producing a porous amorphous material, which comprises impregnating a porous resin with one or more organosilicon compounds selected from crosslinkable silanes and siloxanes, forming a crosslinked product of the organosilicon compounds within the porous resin, and then heating and reacting the crosslinked product in a non-oxidizing gas at a temperature of 1000 to 1350°C to obtain an amorphous material containing silicon, carbon, and oxygen as constituent elements and having oxidation resistance."
[0005] Patent Document 2 proposes "a negative electrode active material for a secondary battery, comprising a composite material including an active phase that reacts with Li and an amorphous material phase, the active phase being dispersed in the amorphous material phase, and the amorphous material phase including Si, O, and C."
[0006] JP 2007-115548 A International Publication No. 2022 / 210512 A
[0007] The amorphous material obtained by the manufacturing method of Patent Document 1 has a large irreversible capacity. Moreover, the negative electrode active material of Patent Document 2 has room for improvement in the utilization rate of the active phase.
[0008] One aspect of the present disclosure relates to a negative electrode material for a secondary battery, comprising a composite material including an active phase that reacts with Li and an amorphous material phase, wherein the active phase is dispersed within the amorphous material phase and has a particle size of 10 nm or less, the amorphous material phase contains elements A, O, and C, and the element A is at least one selected from the group consisting of Si, Sn, Ti, Al, and Mg.
[0009] Another aspect of the present disclosure relates to a secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, wherein the negative electrode contains the above-described negative electrode material for secondary batteries.
[0010] Yet another aspect of the present disclosure relates to a method for producing a negative electrode material for a secondary battery, comprising: a first step of reducing an organometallic compound to obtain an intermediate containing an active phase having a median diameter of 10 nm or less as measured by dynamic light scattering; and a second step of calcining the intermediate to obtain a composite material containing an amorphous material phase and the active phase dispersed within the amorphous material phase, wherein the organometallic compound and the amorphous material phase contain elements A, O, and C, and the element A is at least one selected from the group consisting of Si, Sn, Ti, Al, and Mg.
[0011] The present disclosure allows for increased utilization of the active phase dispersed within the amorphous material phase. While the novel features of the present invention are set forth in the appended claims, the present invention, both as to organization and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.
[0012] 1 is a schematic perspective view of a secondary battery according to an embodiment of the present disclosure, with a portion cut away; FIG. 2 is a particle size distribution of an example of nanosilicon (intermediate) measured by dynamic light scattering; FIG. 3 is an XRD spectrum of an example of nanosilicon (intermediate) (median diameter of 3 nm or less); FIG. 4 is an XRD spectrum of reference crystalline nanosilicon (median diameter of 40 nm); FIG. 5 is an SEM image of an example of a particle of a composite material; FIG. 6 is a cross-sectional STEM-EDX image of an example of a particle of a composite material; and FIG. 7 is a fast Fourier transform (FFT) image of a cross-sectional STEM image of an example of a particle of a composite material.
[0013] Hereinafter, embodiments of the present disclosure will be described using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc. may be exemplified, but other numerical values, materials, etc. may be applied as long as the effects of the present disclosure are obtained. Note that components other than those characteristic of the present disclosure may be components of known secondary batteries. In this specification, when a "range from numerical value A to numerical value B" is mentioned, the range includes numerical value A and numerical value B. In the following description, when a lower limit and an upper limit are exemplified for numerical values of specific physical properties, conditions, etc., any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit.
[0014] The present disclosure encompasses any combination of two or more claims arbitrarily selected from the appended claims, i.e., any combination of two or more claims arbitrarily selected from the appended claims may be combined unless a technical contradiction arises.
[0015] The negative electrode material for a secondary battery according to an embodiment of the present disclosure comprises a composite material including an active phase that reacts with Li and an amorphous material phase. The form of the composite material is not particularly limited, and it may be supplied in a bulk state, a sheet state, a powder containing multiple particles, or the like.
[0016] <Composite Material> The active phase is formed of a material that exhibits capacity through a Faraday reaction with lithium (Li). The active phase is dispersed in an amorphous material phase. The active phase repeatedly expands and contracts with a significant volume change during charging and discharging. In other words, the active phase is a material that expands more than the amorphous material phase when the negative electrode active material absorbs lithium. The active phase may contain a metal element that alloys with lithium.
[0017] The active phase is composed of a material that can electrochemically react reversibly with Li during charge and discharge. The particle diameter of the active phase is 10 nm or less, but may be 5 nm or less, or 3 nm or less. The particle diameter of the active phase may be 1 nm or more. The smaller the particle diameter of the active phase, the more easily a network formed by connections between active phases within the amorphous material phase, which increases the conductivity of lithium ions within the composite material and increases the utilization rate of the active phase (i.e., reactivity with Li). It is believed that the active phase gradually changes its morphology with charge and discharge, forming contact points between active phases. It is believed that the active phase's micro-size of 10 nm or less makes it easier for the active phase to deform or move, or for the active phases to come into contact with each other. This change in morphology reduces the number of isolated active phases within the amorphous material phase, significantly improving the utilization rate.
[0018] When the particle size of the active phase is 10 nm or less, it is generally difficult to observe a sharp peak attributable to the active phase by X-ray diffraction (XRD), so the spectrum (XRD spectrum) of the composite material obtained by X-ray diffraction does not have to have a peak attributable to the active phase. The active phase may be a metal phase (including an intermetallic compound phase), but the spectrum (XRD spectrum) of the composite material obtained by X-ray diffraction does not have to have a peak attributable to the metal phase. For example, a material containing a Si phase having a size sufficiently larger than 10 nm has a peak attributable to the Si phase in the range of 2θ from 25° to 30°. On the other hand, when the active phase is a Si phase and its particle size is 10 nm or less, the spectrum obtained by X-ray diffraction of the composite material does not have to have a peak in the range of 2θ from 25° to 30°.
[0019] If the particle diameter is, for example, 5 nm or more, it may be possible to confirm it using an analytical device such as a high-resolution STEM. In this case, the particle diameter can be calculated as the average of the maximum diameters of any 10 or more active phase particles. On the other hand, the size of the active phase may be too small to be observed with an electron microscope. In such cases, it can be said that this indirectly indicates that the particle diameter of the active phase is, for example, 5 nm or less, or 3 nm or less. In such cases, the presence of the active phase can be confirmed by the electrochemical capacity exhibited by the composite material. The capacity of the composite material depends on the content of the active phase, but if an irreversible capacity of, for example, 100 mAh / g or more is obtained, it is useful as an electrode active material.
[0020] However, the composite material may have a microscopically island-sea structure. In this island-sea structure, the active phase forms tiny islands of 10 nm or less, and the amorphous material phase forms a continuous sea or matrix. When the composite material is a powder, a single particle of the composite material contains multiple island regions dispersed in the sea.
[0021] In some cases, it is possible to measure the particle size of the active phase even if it is very small. In such cases, the maximum diameter of, for example, 100 active phase particles may be measured, and the average of these maximum diameters may be determined as the particle size of the active phase.
[0022] (Amorphous material phase) The amorphous material phase is formed of a material that can exhibit a smaller capacity per unit mass (mAh / g) than the active phase (or a material that does not exhibit a capacity). The amorphous material phase undergoes little or no volume change during charging and discharging. The amorphous material phase relieves stress caused by expansion and contraction of the active phase and suppresses side reactions between the active phase and the electrolyte.
[0023] The amorphous material phase contains element A, O (oxygen element), and C (carbon element). Element A is at least one element selected from the group consisting of Si, Sn, Ti, Al, and Mg. As will be described later, when the amorphous material phase is formed, the active phase can be formed from a portion of element A contained in the raw material of the amorphous material phase.
[0024] The amorphous material phase forms a compound in which A, O, and C are randomly bonded by covalent bonds. The amorphous material phase has, for example, an A-O-C bond (covalent bond). In other words, the amorphous material phase is not a simple mixture or a simple composite of multiple compounds (e.g., SiO, SiC, when A = Si). The amorphous material phase is a phase with an unspecified crystal structure. The amorphous material phase may form a single phase without an interface between different materials, as occurs in composites of two or more materials. When the amorphous material phase contains A, O, and C as essential components and is a phase with an unspecified crystal structure, the composite material not only has high hardness but also elasticity or flexibility that relieves stress caused by the expansion and contraction of the active phase.
[0025] In the cross section of the composite material, it is desirable that the amorphous material phase has substantially no grain boundaries. When the amorphous material phase has a continuous structure that has substantially no grain boundaries, the hardness of the composite material increases, the phenomenon of electrolyte seeping into the grain boundaries is reduced, side reactions involving decomposition of the electrolyte are suppressed, and the material is less likely to deteriorate. In this case, the composite material can be formed as primary particles. However, the amorphous material phase may have a small number of grain boundaries. The state in which the amorphous material phase has substantially no grain boundaries can be confirmed in a cross-sectional SEM image of the composite material. A field of view of 500 nm 2 In a cross-sectional SEM image of the composite material, if the total length of the grain boundaries in the amorphous material phase is 1 nm or less, it can be said that the amorphous material phase does not substantially have grain boundaries. It is desirable to perform similar measurements on 10 arbitrary composite particles and calculate the grain boundary length by averaging the measured values.
[0026] From the viewpoint of reducing irreversible capacity, the amorphous material phase preferably contains element M (cation species). Element M is, for example, at least one element selected from the group consisting of Li, Na, K, Mg, Ca, B, and Al. In particular, the amorphous material phase preferably contains at least Li as element M. When element M contained in the amorphous material phase is an element other than Li, during charging and discharging of a lithium ion secondary battery having a negative electrode containing the composite material, elements other than Li are replaced with Li, and Li ions are irreversibly captured in the amorphous material phase, which may result in a decrease in capacity. When element M contains Li, the above-mentioned capacity decrease can be suppressed.
[0027] The amorphous material phase is represented by the general formula (1): M a AO x N y C z When expressed as above, general formula (1) satisfies, for example, 0<a≦4, 0<x≦3, 0≦y≦1, and 0≦1−0.5x−0.75y≦z. Such a composition is empirically determined from the composition of the amorphous material phase produced by the production method described below. Li may be trapped as irreversible capacity during charge and discharge.
[0028] From the viewpoint of reducing irreversible capacity, it is preferable that the amorphous material phase is already doped with element M (e.g., Li) when the composite material is prepared (before the first charge). That is, it is preferable that 0<a≦4 is satisfied in general formula (1). Furthermore, a in general formula (1) is more preferably 0.1 or more, and even more preferably 1 or more. Furthermore, from the viewpoint that dissolution of the amorphous material phase into water is easily suppressed when M is Li, a in general formula (1) may be 2 or less.
[0029] In general formula (1), the range of z, which indicates the atomic ratio of C to A, may be 0.1≦z≦6, 0.5≦z≦4, or 0.5≦z≦3. By controlling the amount of carbon contained in the amorphous material phase within the above range, A-O-Li bonds are less likely to be formed, the irreversible capacity of the composite material is reduced, and the amorphous material phase itself has capacity, which is advantageous for increasing capacity. In general formula (1), M is preferably Li.
[0030] The composition of the amorphous material phase (quantitative analysis of each element in the composite material) can be analyzed by scanning electron microscope (SEM)-energy dispersive X-ray (EDX) analysis. In SEM-EDX analysis, the cross section of the composite material is observed using an SEM, and elemental mapping analysis is performed using EDX. The observation magnification is preferably 2000 to 20,000 times. Mapping analysis is preferably performed on a region at least 1 μm inward from the peripheral edge of the cross section of the composite material particle. In mapping analysis, the element content (i.e., composition) can be calculated using image analysis software. Similar measurements may be performed on any 10 particles, and the measured values may be averaged to determine the composition. The maximum diameter of the particles to be measured is preferably 5 μm or greater. The cross section of the composite material particle may be formed, for example, by filling the composite material in a thermosetting resin, curing it, and then using a cross-section polisher (CP). Alternatively, the battery may be disassembled, the negative electrode removed, and the negative electrode immersed in a thermosetting resin, curing it, and then formed on the cross section of the negative electrode.
[0031] Desired measurement conditions for cross-sectional SEM-EDX analysis are shown below: Processing equipment: JEOL Ltd., IB-19520CCP (cross-section polisher) Processing conditions: Acceleration voltage 6 kV Current value: 150 to 180 μA Vacuum degree: 5×10 -4 ~2 x 10 -3 Pa measuring device: JEM-F200 (field emission scanning electron microscope) manufactured by JEOL Ltd., JED-2300T (EDX detector) manufactured by JEOL Ltd. Acceleration voltage during analysis: 200 kV
[0032] In the C1s spectrum obtained by X-ray photoelectron spectroscopy (XPS) of the composite material, multiple types of C1s peaks contained in the amorphous material phase are observed. For example, C1s peaks attributable to A-C bonds, A-O-C bonds, C-O bonds, C-C bonds, etc. are observed. The presence of such peaks indicates that the amorphous material phase contains a considerable amount of regions other than oxides. In particular, the C1s peak attributable to C-C bonds is a peak characteristic of the composite material according to the present disclosure, and indicates that the amorphous material phase contains a region composed of carbon. The peak attributable to C-C bonds is observed, for example, around 284.8 eV.
[0033] The composite material may include at least one selected from the group consisting of graphite, hard carbon, and soft carbon dispersed within an amorphous material phase.
[0034] In XPS of composite materials, a powder of the composite material is used as a sample, and analysis is performed from the sample surface along the depth direction of the composite material (10 to 100 nm) to analyze the internal state of the composite material.
[0035] Desirable XPS measurement conditions are as follows: Measurement device: PHI5000 manufactured by ULVAC-PHI, Inc. X-ray used: Monochrome Al-Kα, 25 W, 15 kV Vacuum degree: 5×10 -7 Pa
[0036] The composite material may have voids inside the amorphous material phase. In this case, the active phase may be exposed on the inner wall surface of the voids. The presence of voids facilitates the relaxation of stress caused by the expansion and contraction of the active phase. The voids present in the amorphous material phase can be confirmed in a cross-sectional SEM image of the composite material.
[0037] (Active Phase) The material constituting the active phase may contain element A. The material constituting the active phase may also contain at least one selected from the group consisting of a metal phase and an intermetallic compound phase. In this case, the metal phase or the intermetallic compound phase may contain element A. The active phase may contain one type alone or two or more types in the composite material.
[0038] The element A constituting the active phase may be at least one selected from the group consisting of Si, Sn, Ti, Al, and Mg. Therefore, the metal phase may be at least one selected from the group consisting of Si phase, Sn phase, Ti phase, Al phase, and Mg phase. The intermetallic compound phase may be, for example, CrSi 2 Phase, MnSi 2 phase, FeSi 2 Phase, CoSi 2 phase, NiSi 2 The Si phase and the Sn phase have high capacity, and the Si phase is particularly preferred.
[0039] The active phase or metal phase (including the intermetallic compound phase) may contain an element M (at least one element selected from the group consisting of Li, Na, K, Mg, Ca, B, and Al) that can be contained in the amorphous material phase. For example, when the active phase contains Si, the intermetallic compound may contain M x Si can be formed.
[0040] The content of the active phase in the composite material can be controlled as appropriate. From the viewpoint of increasing capacity, it is desirable that the content of the active phase in the composite material be as high as possible. On the other hand, from the viewpoint of alleviating stress due to expansion and contraction of the active phase and suppressing side reactions between the active phase and the electrolyte, it is necessary for the composite material to contain a certain amount of amorphous material phase. The content of the active phase in the composite material is, for example, 50% by mass or less, or may be 40% by mass or less, or may be 25% by mass or less. The content of the active phase in the composite material may be 5% by mass or more, or may be 10% by mass or more.
[0041] The content of the active phase in the composite material can be controlled by the content of element A. For example, when a composite material containing an active phase is obtained by reducing an organometallic compound containing elements A, O, and C, the content of element A in the composite material may be approximately equal to the content of the active phase, or the content of the active phase may be smaller than the content of element A. Therefore, when the content of the active phase in the composite material is controlled within the above range, the content of element A in the composite material is preferably, for example, 50% by mass or less, and may be 40% by mass or less, or 25% by mass or less. The content of element A in the composite material may be 5% by mass or more, or 10% by mass or more.
[0042] When the active phase contains a Si phase, the content of the Si phase in the composite material can be measured by Si-NMR.
[0043] (Conductive Layer) From the viewpoint of improving conductivity, at least a portion of the surface of the composite material may be covered with a conductive layer. The conductive layer may contain carbon. The thickness of the conductive layer is preferably thin enough not to substantially affect the average particle size of the composite material. The thickness of the conductive layer is, for example, 1 nm or more and 10 nm or less.
[0044] The conductive layer is formed, for example, by mixing the raw materials of the conductive layer with a composite material and firing the mixture to carbonize the raw materials of the conductive layer. Examples of the raw materials for the conductive layer include coal pitch or coal tar pitch, petroleum pitch, and phenolic resin. The mixture of the raw materials for the conductive layer and the composite material is fired, for example, in an inert atmosphere (e.g., an argon or nitrogen atmosphere). The firing temperature is, for example, 450°C or higher and 1000°C or lower. The firing time is, for example, 1 hour or higher and 10 hours or lower.
[0045] (Carbon material) The negative electrode material may contain at least one carbon material selected from the group consisting of graphite (natural graphite or artificial graphite), hard carbon, and soft carbon, in addition to the composite material. The carbon material may be composited with an amorphous material phase.
[0046] The carbon material expands and contracts less during charge and discharge than the active phase, and therefore its use in combination with the composite material facilitates improving the cycle characteristics of the battery. The proportion of the carbon material in the total of the composite material and the carbon material may be, for example, 70% by mass or more and 99% by mass or less, 85% by mass or more and 95% by mass or less, or 90% by mass or more and 95% by mass or less. This facilitates achieving both high capacity and better cycle characteristics.
[0047] [Method for producing a negative electrode material for secondary batteries] Next, an example of a method for producing a negative electrode material for secondary batteries will be described. The method for producing a negative electrode material for secondary batteries comprising a composite material in which an active phase is dispersed in an amorphous material phase in the following example includes a first step and a second step.
[0048] (i) Step 1 Step 1 is a first step in which an organometallic compound is reduced to obtain an intermediate containing an active phase having a particle size of 10 nm or less. The organometallic compound contains elements A, O, and C. Element A is at least one element selected from the group consisting of Si, Sn, Ti, Al, and Mg.
[0049] An organometallic compound has an organic group or a halogen atom bonded to element A. Here, halides of element A that do not contain an organic group are also included in the organometallic compound. The organic group may be an alkyl group, an alkoxy group, a cyclopentadienyl group, or the like. An organometallic compound may be solid, liquid, or gas at room temperature.
[0050] Examples of organometallic compounds containing Si as element A include N-sec-butyl(trimethylsilyl)amine, 1,3-diethyl-1,1,3,3-tetramethyldisilazane, tetramethylsilane, tetraethoxysilane, silicon tetrachloride, silane coupling agents, etc. Among these, silane coupling agents are preferred because they are easy to handle and have a wide variety of options.
[0051] The silane coupling agent has a reactive organic group or functional group and a hydrolyzable group. The reactive organic group or functional group is preferably an epoxy group, a halogenated alkyl group, an amino group, a ureido group, a mercapto group, an isocyanate group, or a polymerizable group. The polymerizable group may be a (meth)acryloyl group, a vinyl group, or the like. The hydrolyzable group is preferably an alkoxy group such as a methoxy group, an ethoxy group, or a propoxy group.
[0052] More specifically, examples of the silane coupling agent include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane (γ-glycidoxypropyltrimethoxysilane), 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-chloropropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane. Examples include silane, N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatopropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane (γ-acryloxypropyltrimethoxysilane), vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, p-styryltrimethoxysilane, etc. Among these, at least one selected from the group consisting of 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane is preferred.
[0053] Examples of organometallic compounds containing Sn as the element A include diisopropyltin, tin acetate, tin octoate, dibutyltin acetate, tetraphenyltin, tetraethyltin, tetramethyltin, dioctyltin oxide, and tin octoate.
[0054] Examples of organometallic compounds containing Ti as element A include bis(t-butylcyclopentadienyl)titanium(IV) dichloride, tetrakis(dimethylamino)titanium(IV), titanium tetrachloride (TiCl), titanium(IV) ethoxide, and titanium coupling agents.
[0055] Examples of organometallic compounds containing Al as the element A include triethylaluminum, diethylchloroaluminum, diethylaluminum ethoxide, triisobutylaluminum, and trihexylaluminum.
[0056] As the organometallic compound containing Mg as the element A, for example, various compounds used as Grignard reagents can be used.
[0057] The method for reducing an organometallic compound is not particularly limited, but an example is a method of reacting it with a reducing agent. Reducing agents include, but are not limited to, hydrogen gas, hydrogen sulfide, sulfur dioxide, hydrogen peroxide, sodium thiosulfate, tin(II) chloride, iron(II) sulfide, organic acids, sugar alcohols, and potassium iodide. Among these, organic acids and sugar alcohols are preferred because of their ease of handling. The organic acid may be a salt. Examples of organic acids include oxalic acid, ascorbic acid, and sodium ascorbate. Examples of sugar alcohols include D-glucose.
[0058] When the organometallic compound can form a solution such as an aqueous solution, a reducing agent can be added to the solution to activate the reducing agent. For example, adding an organic acid to an aqueous solution of a silane coupling agent and stirring the solution causes a reduction reaction to occur, producing nanosilicon with particle sizes of 10 nm or less as an intermediate. When synthesizing the intermediate from a solution, a dispersion of the intermediate is obtained. The intermediate may be separated from the dispersion by techniques such as dialysis, centrifugation, or centrifugal ultrafiltration.
[0059] The particle size of the active phase (e.g., nanosilicon) contained in the intermediate can be measured by dynamic light scattering. In order to disperse an active phase having a particle size of 10 nm or less in the amorphous material phase, the median size of the active phase (e.g., nanosilicon) produced as the intermediate, as measured by dynamic light scattering, is preferably 10 nm or less, and may be 5 nm or less, 3 nm or less, or even less.
[0060] When the active phase or metal phase (including the intermetallic compound phase) contains an element M (at least one element selected from the group consisting of Li, Na, K, Mg, Ca, B, and Al) that can be contained in the amorphous material phase, the compound containing the element M may be doped into the organometallic compound before reduction. The molar ratio of the element M to the element A (M / Si) may be, for example, 0.01 or more and 5 or less, or 0.1 or more and 2 or less.
[0061] Examples of compounds containing element M include salts formed from an anion of carbonic acid or carboxylic acid (formic acid, acetic acid, benzoic acid, etc.) and a cation of element M. When element M is lithium, the compound containing element M may be, for example, at least one selected from the group consisting of lithium carbonate, lithium formate, lithium acetate, and lithium benzoate. When the organometallic compound can form a solution such as an aqueous solution, the compound containing element M may be dissolved in the solution.
[0062] (ii) Second Step: In the second step, an intermediate containing an active phase having a particle size of 10 nm or less is calcined to obtain a composite material containing an amorphous material phase and an active phase dispersed within the amorphous material phase. The amorphous material phase is formed from an organometallic compound. Therefore, the amorphous material phase contains elements A, O, and C.
[0063] The intermediate may be granulated before being calcined. When the intermediate is obtained as a dispersion, it can be easily granulated by spray drying the dispersion. A binder that promotes granulation may be dissolved in the dispersion before spray drying. When the dispersion contains water or a polar solvent such as N-methyl-2-pyrrolidone, a water-soluble resin may be used as the binder. In this case, an intermediate containing the binder is obtained. The binder becomes entangled with the active phase to form particles suitable for granulation by spray drying.
[0064] Examples of water-soluble resins include sugars, polyvinylpyrrolidone, polyvinyl alcohol, water-soluble polyesters, polystyrene sulfonic acid, polyacrylic acid, polymethacrylic acid, polyacrylamide, 2-acrylamido-2-methylpropanesulfonic acid, oxazole-based water-soluble polymers (such as oxazole-2-ethyl-4,5-dihydro homopolymer), and salts thereof (such as alkali metal salts and ammonium salts). Examples of sugars include carboxymethyl cellulose (CMC), methyl cellulose, sucrose, mannitol, sorbitol, xylitol, pentaerythritol, and trimethylolpropane.
[0065] Before calcining the intermediate, the intermediate may be mixed with a polymer. The intermediate to be mixed with the polymer may be an intermediate containing a binder, or may be particles granulated by spray drying or the like. The polymer may be any polymer that is carbonized by calcination. Examples of polymers that can be used include coal pitch or coal tar pitch, petroleum pitch, and phenolic resin.
[0066] The amount of intermediate per 100 parts by mass of polymer may be set appropriately depending on the desired proportion of the active phase of the composite material, but may be, for example, 20 parts by mass or more and 250 parts by mass or less, or 50 parts by mass or more and 200 parts by mass or less.
[0067] Along with the polymer, at least one selected from the group consisting of graphite (natural graphite, artificial graphite), hard carbon, and soft carbon may be mixed with the intermediate.
[0068] The firing may be carried out, for example, at a temperature of 600°C or higher and 1000°C or lower in an inert atmosphere. The inert atmosphere may be a reduced pressure atmosphere or may be a flow of inert gas. The inert gas may be argon, nitrogen, helium, or the like. The firing time may be any time that allows the carbon atoms contained in the polymer to be sufficiently carbonized. The composite material obtained after firing is a solid that does not have fluidity. By pulverizing the composite material, a powdered composite material is produced.
[0069] By firing, water-soluble resins, polymers, compounds containing element M, etc. are decomposed to generate gases, such as CO 2 Gas is produced, which causes voids to form within the amorphous material phase.
[0070] The above is merely one example of a manufacturing method. When active phase particles (hereinafter also referred to as "active particles") having a particle size of 10 nm or less are available, the active particles may be mixed with a water-soluble resin and granulated together with the water-soluble resin.
[0071] [Secondary Battery] A secondary battery according to an embodiment of the present disclosure includes a positive electrode, a negative electrode, and an electrolyte. The negative electrode contains the above-described negative electrode material for a secondary battery.
[0072] (Negative Electrode) The negative electrode includes, for example, a sheet-like negative electrode current collector and a negative electrode mixture layer formed on the negative electrode current collector. The negative electrode mixture layer is a negative electrode mixture formed in the form of a layer or a coating film. The negative electrode mixture contains a negative electrode active material as an essential component and may contain, as optional components, a binder, a conductive additive, a thickener, etc. The negative electrode active material includes a negative electrode material for secondary batteries.
[0073] The negative electrode mixture layer can be formed, for example, by applying a negative electrode slurry, in which the negative electrode mixture is dispersed in a dispersion medium, to the surface of the negative electrode current collector and drying the applied film. The dried coating film may be rolled, if necessary.
[0074] The negative electrode current collector may be a non-porous conductive substrate (such as a metal foil) or a porous conductive substrate (such as a mesh, net, or punched sheet). Examples of the material for the negative electrode current collector include stainless steel, nickel, nickel alloys, copper, and copper alloys.
[0075] Examples of binders include resin materials, such as fluororesins such as polytetrafluoroethylene and polyvinylidene fluoride (PVDF); polyolefin resins such as polyethylene and polypropylene; polyamide resins such as aramid resin; polyimide and polyamideimide; acrylic resins such as polyacrylic acid, polymethyl acrylate, and ethylene-acrylic acid copolymer; vinyl resins such as polyacrylonitrile and polyvinyl acetate; polyvinylpyrrolidone; polyethersulfone; and rubber-like materials such as styrene-butadiene copolymer rubber (SBR). These may be used alone or in combination of two or more.
[0076] Examples of conductive additives include carbon black such as acetylene black, carbon nanotubes (hereinafter also referred to as CNT), metal fibers, carbon fluoride, metal powder, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and organic conductive materials such as phenylene derivatives. These may be used alone or in combination of two or more.
[0077] (Positive Electrode) The positive electrode includes a positive electrode active material capable of electrochemically absorbing and desorbing lithium ions. The positive electrode includes, for example, a positive electrode current collector and a positive electrode mixture layer formed on the surface of the positive electrode current collector. The positive electrode mixture layer can be formed by applying a positive electrode slurry, in which the positive electrode mixture is dispersed in a dispersion medium, to the surface of the positive electrode current collector and drying the applied layer. The dried coating may be rolled as necessary. The positive electrode mixture includes a positive electrode active material as an essential component and may include a binder, a conductive agent, etc. as optional components.
[0078] As the positive electrode active material, for example, a lithium-containing composite oxide can be used. a CoO2, Li a NiO2, Li a MnO2, Li a Co b Ni 1-b O2, Li a Co b M 1-b O c , Li a Ni 1-b Mb O c , Li a Mn2O4, Li a Mn 2-b M b Examples of the lithium-containing lithium ion battery include LiMPO4, LiMPO4, and LiMPO4F (where M is at least one selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B). Here, a = 0 to 1.2, b = 0 to 0.9, and c = 2.0 to 2.3. The value a, which indicates the molar ratio of lithium, increases or decreases with charge and discharge.
[0079] The binder and conductive agent may be the same as those exemplified for the negative electrode. As the conductive agent, graphite such as natural graphite or artificial graphite may be used.
[0080] The shape and thickness of the positive electrode current collector can be selected from the shape and range corresponding to those of the negative electrode current collector. Examples of the material of the positive electrode current collector include stainless steel, aluminum, aluminum alloy, and titanium.
[0081] (Electrolyte) The electrolyte has lithium ion conductivity. The electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.
[0082] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.
[0083] The electrolyte solution contains a solvent and an electrolyte salt. The solvent may be a non-aqueous solvent, or water may be used. In the case of a lithium ion secondary battery, the electrolyte salt contains at least a lithium salt.
[0084] The concentration of the lithium salt in the electrolyte solution is preferably, for example, 0.5 mol / L or more and 2 mol / L or less. By controlling the lithium salt concentration within the above range, an electrolyte solution having excellent ionic conductivity and appropriate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.
[0085] Examples of non-aqueous solvents that can be used include cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, and chain carboxylic acid esters. Examples of cyclic carbonates include propylene carbonate (PC) and ethylene carbonate (EC). Examples of chain carbonates include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of cyclic carboxylic acid esters include γ-butyrolactone (GBL) and γ-valerolactone (GVL). Examples of chain carboxylic acid esters include methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, and propyl propionate. One type of non-aqueous solvent may be used alone, or two or more types may be used in combination.
[0086] Examples of lithium salts include LiClO4, LiBF4, LiPF6, LiAlCl4, LiSbF6, LiSCN, LiCF3SO3, LiCF3CO2, LiAsF6, and LiB 10 Cl 10 , lower aliphatic lithium carboxylate, LiCl, LiBr, LiI, borates, imide salts, etc. The lithium salt may be used alone or in combination of two or more.
[0087] The electrolyte may further contain additives such as vinylene carbonate (VC), fluoroethylene carbonate (FEC), and vinyl ethyl carbonate (VEC).
[0088] (Separator) It is usually desirable to interpose a separator between the positive electrode and the negative electrode. The separator has ion permeability and insulating properties. As the separator, a microporous thin film, a woven fabric, a nonwoven fabric, etc. can be used. As the material of the separator, polyolefin such as polypropylene or polyethylene is preferred.
[0089] An example of the structure of the secondary battery is a structure in which an electrode group in which a positive electrode and a negative electrode are wound with a separator interposed therebetween and an electrolyte solution are housed in an exterior body. A stacked electrode group in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween may also be used. The secondary battery may have, for example, a cylindrical shape, a prismatic shape, a coin shape, a button shape, a sheet shape, or the like.
[0090] An example of a secondary battery according to the present disclosure will be described below with reference to FIG. 1 . The battery includes a bottomed, rectangular battery case 4, and an electrode group 1 and an electrolyte (not shown) housed within the battery case 4. The electrode group 1 includes a strip-shaped negative electrode, a strip-shaped positive electrode, and a separator interposed therebetween. The negative electrode current collector of the negative electrode is electrically connected to a negative electrode terminal 6 provided on a sealing plate 5 via a negative electrode lead 3. The negative electrode terminal 6 is insulated from the sealing plate 5 by a resin gasket 7. The positive electrode current collector of the positive electrode is electrically connected to the back surface of the sealing plate 5 via a positive electrode lead 2. That is, the positive electrode is electrically connected to the battery case 4, which also serves as the positive electrode terminal. The periphery of the sealing plate 5 fits into the open end of the battery case 4, and the fitting is laser-welded. The sealing plate 5 has an electrolyte injection hole that is closed with a seal plug 8 after injection.
[0091] (Additional Notes) The above description discloses the following technologies. (Technology 1) A negative electrode material for a secondary battery, comprising a composite material including an active phase reactive with Li and an amorphous material phase, wherein the active phase is dispersed within the amorphous material phase and has a particle size of 10 nm or less, the amorphous material phase contains elements A, O, and C, and the element A is at least one selected from the group consisting of Si, Sn, Ti, Al, and Mg. (Technology 2) The negative electrode material for a secondary battery according to Technology 1, wherein the particle size is 5 nm or less. (Technology 3) The negative electrode material for a secondary battery according to Technology 1 or 2, wherein a spectrum obtained by X-ray diffraction of the composite material does not have a peak in the 2θ range of 25° to 30°. (Technology 4) The negative electrode material for a secondary battery according to any one of Technology 1 to 3, wherein the amorphous material phase does not have substantial grain boundaries in a cross section of the composite material. (Technology 5) The amorphous material phase is represented by the general formula: M a SiO x N y C z The negative electrode material for a secondary battery according to any one of Techniques 1 to 4, wherein the following relationships are satisfied: 0<a≦4, 0<x≦3, 0≦y≦1, and 0≦1-0.5x-0.75y≦z, and the element M is at least one selected from the group consisting of Li, Na, K, Mg, Ca, B, and Al. (Technology 6) The negative electrode material for a secondary battery according to any one of Techniques 1 to 5, wherein the element M contains at least Li. (Technology 7) The negative electrode material for a secondary battery according to any one of Techniques 1 to 6, wherein the element A contains at least Si. (Technology 8) The negative electrode material for a secondary battery according to any one of Techniques 1 to 7, wherein voids exist in the amorphous material phase. (Technology 9) The negative electrode material for a secondary battery according to any one of Techniques 1 to 8, further comprising a conductive layer covering a surface of the composite material, wherein the conductive layer contains carbon. (Technology 10) The negative electrode material for a secondary battery according to any one of Technologies 1 to 9, wherein the material constituting the active phase includes at least one selected from the group consisting of a metal phase and an intermetallic compound phase. (Technology 11) The metal phase is at least one selected from the group consisting of a Si phase, a Sn phase, a Ti phase, an Al phase, and a Mg phase, and the intermetallic compound phase is CrSi 2 Phase, MnSi2 Phase, FeSi 2 Phase, CoSi 2 Phase, NiSi 2The negative electrode material for secondary batteries according to Technology 10, wherein the metal phase is at least one selected from the group consisting of a LiNiSn phase and a LiNiSn phase. (Technology 12) The negative electrode material for secondary batteries according to Technology 10 or 11, wherein the metal phase further contains at least one selected from the group consisting of Li, Na, K, Mg, Ca, B, and Al. (Technology 13) The negative electrode material for secondary batteries according to any one of Technology 1 to 12, wherein the content of the active phase in the composite material is 50 mass% or less. (Technology 14) The negative electrode material for secondary batteries according to any one of Technology 1 to 13, wherein the content of the active phase in the composite material is 40 mass% or less. (Technology 15) The negative electrode material for secondary batteries according to any one of Technology 1 to 14, wherein at least one selected from the group consisting of graphite, hard carbon, and soft carbon is further dispersed in the amorphous material phase. (Technology 16) A secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, wherein the negative electrode contains the negative electrode material for secondary batteries according to any one of Techniques 1 to 15. (Technology 17) A method for producing a negative electrode material for secondary batteries comprising: a first step of reducing an organometallic compound to obtain an intermediate containing an active phase having a particle size of 10 nm or less; and a second step of firing the intermediate to obtain a composite material containing an amorphous material phase and the active phase dispersed within the amorphous material phase, wherein the organometallic compound and the amorphous material phase contain elements A, O, and C, and the element A is at least one selected from the group consisting of Si, Sn, Ti, Al, and Mg. (Technology 18) A method for producing a negative electrode material for secondary batteries according to Technique 17, further comprising a step of granulating the intermediate before firing the intermediate. (Technology 19) The method for producing an anode material for a secondary battery according to Technology 17 or 18, further comprising a step of mixing the intermediate with a polymer before calcining the intermediate, wherein the polymer is carbonized in the second step. (Technology 20) The method for producing an anode material for a secondary battery according to any one of Technology 17 to 19, wherein the organometallic compound is a silane coupling agent. (Technology 21) The method for producing an anode material for a secondary battery according to Technology 20, wherein the silane coupling agent is at least one selected from the group consisting of 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane.
[0092] [Examples] Hereinafter, the present disclosure will be specifically described based on examples and comparative examples, but the present disclosure is not limited to the following examples.
[0093] Example 1 (Composite Material A) 125 mL of a 0.1 M aqueous solution of sodium ascorbate was added to 400 mL of pure water, and after bubbling with nitrogen for at least 2 hours, 100 mL of 3-aminopropyltrimethoxysilane was added dropwise, and the mixture was stirred at 500 rpm for 20 minutes under a nitrogen atmosphere to produce nanosilicon. The aqueous solution was irradiated with UV light with a wavelength of 365 nm, and the production of nanosilicon (intermediate) was confirmed by confirming green light emission.
[0094] Figure 2 shows the particle size distribution of the produced nanosilicon measured by dynamic light scattering, which shows that the median diameter of the produced nanosilicon is 3 nm or less.
[0095] To the obtained nanosilicon dispersion, 200 g of a CMC aqueous solution with a concentration of 1.8 mass % was added and stirred, and then the mixture was spray-dried (spray flow rate: 0.6 m 3 The mixture was granulated at a temperature of 700°C / min (injection nozzle temperature: 130°C). The obtained granulated powder was vacuum dried overnight at 60°C, and then 9 parts by mass of pitch was mixed with 100 parts by mass of the granulated powder, followed by firing at 700°C for 5 hours in a nitrogen atmosphere. The obtained fired powder was crushed in a mortar, stirred in pure water for 10 minutes, washed, filtered by suction, and vacuum dried overnight at 60°C to obtain composite material A1 (Si / C powder).
[0096] The content of silicon element in the composite material A1 calculated by ICP atomic emission spectrometry was 37 mass %.
[0097] 3A shows the XRD spectrum of composite material A1 (Si / C powder) containing nanosilicon (median diameter 3 nm or less), and FIG. 3B shows the XRD spectrum of reference crystalline nanosilicon (median diameter 40 nm). Composite material A1 exhibits an amorphous spectrum, and it can be seen that the XRD spectrum does not have a silicon crystal peak in the 2θ range of 2θ = 25° to 30°.
[0098] Figure 4 is an SEM image of the obtained particle of composite material A1, Figure 5 is a cross-sectional STEM-EDX image of a particle of composite material A1, and Figure 6 is an FFT image of an example of a particle of composite material A1.
[0099] In the STEM image of Figure 5, an amorphous material phase and spotted voids are observed, but no particles of the active phase (nano silicon) are observed. Also in Figure 6, no spots attributed to the active phase (nano silicon) are observed. However, as will be described later, since composite material A1 exhibits high capacity due to silicon, it is clear that nano silicon particles of 3 nm or less are dispersed within the amorphous material phase.
[0100] [Evaluation 1] A test cell having a negative electrode containing the composite material A1 was prepared according to the following procedure, and the capacity was determined.
[0101] <Preparation of Test Cell> (Preparation of Working Electrode (Negative Electrode)) A negative electrode material, carbon nanotubes (CNT), polyacrylic acid (PAA), styrene-butadiene copolymer rubber (SBR), carboxymethyl cellulose (CMC), and an appropriate amount of water were mixed to prepare a negative electrode slurry. The amounts of CNT, PAA, CMC, and SBR added relative to 100 parts by mass of the negative electrode material were 0.5 parts by mass, 5 parts by mass, 5 parts by mass, and 5 parts by mass, respectively.
[0102] The negative electrode slurry was applied to one side of an electrolytic copper foil as a current collector, and the foil was punched out to a size of 2 cm x 2 cm, followed by drying to form a negative electrode mixture layer, thereby obtaining a negative electrode.
[0103] (Preparation of Counter Electrode) A lithium metal foil was attached to one side of an electrolytic copper foil (current collector), and the foil was punched out into a square having a side length of 2.5 cm to prepare a counter electrode.
[0104] (Preparation of Electrolyte Solution) A mixed solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of EC:EMC:DMC=4:1:15 was obtained. 6 was dissolved in a concentration of 1.3 mol / L to prepare an electrolyte solution.
[0105] (Test Cell Assembly) An electrode assembly was constructed by placing a negative electrode and a counter electrode opposite each other with a separator interposed therebetween. A microporous polyolefin film was used as the separator. The electrode assembly was housed in an exterior body made of an aluminum laminate sheet, and after injecting an electrolyte, the opening of the exterior body was sealed. At this time, a portion of the leads attached to the negative electrode and counter electrode was exposed from the exterior body. In this way, a test cell was obtained.
[0106] <Charge / Discharge Test> The test cell was charged and discharged as follows in a thermostatic chamber at 25° C. The rest time between charge and discharge was 20 minutes.
[0107] (Charging) Constant current charging was performed at 0.1 C (1 C is the current value required to discharge the design capacity in 1 hour) until the cell voltage reached 0.005 V. The rest period thereafter was 20 minutes. Next, constant current charging was performed at 0.01 C until the cell voltage reached 0.005 V. The rest period thereafter was 20 minutes. Furthermore, constant current charging was performed at 0.001 C until the cell voltage reached 0.005 V.
[0108] (Discharge) A constant current discharge was performed at 0.1 C until the cell voltage reached 1 V. The rest period thereafter was 20 minutes. Next, a constant current discharge was performed at 0.01 C until the cell voltage reached 1 V. The rest period thereafter was 20 minutes. Furthermore, a constant current discharge was performed at 0.001 C until the cell voltage reached 1 V.
[0109] From the above charge / discharge cycles, the charge capacity (measured charge capacity) per unit mass of the negative electrode material (composite particles) was determined. The theoretical capacity of Si was set at 4200 mAh / g, and the charge capacity (estimated charge capacity) estimated from the amount of Si contained in composite material A1 was calculated. The measured charge capacity was then divided by the estimated charge capacity to determine the utilization rate of Si contained in the composite material. The evaluation results are shown in Table 1.
[0110]
[0111] Comparative Example 1 Silicon nanoparticles with an average particle size of 40 nm were prepared as the material for the active phase. Polycarbosilane (R1 and R2 in the following formula (B1) are -H and -CH, respectively) was used as an organosilicon polymer. 2 -CH=CH2 100 parts by mass of nanoparticles were mixed with 200 parts by mass of polycarbosilane (a polycarbonate base that is liquid at room temperature) until a uniform slurry was obtained, to obtain a mixture. The obtained mixture was fired in a nitrogen atmosphere at 850°C for 3 hours until the carbon atoms contained in the polycarbosilane were carbonized, to obtain composite material B1. The composition of the amorphous material phase of composite material B1 was measured by TEM-EDX, and it was found to be SiO x C z (x=0.32, z=1.62) The content of nanoparticles (active phase) in composite material B1 was approximately 45% by mass.
[0112] Formula (B1):
[0113]
[0114] Comparative Example 2 Silicon nanoparticles with an average particle size of 40 nm were prepared as the material for the active phase. Polysiloxane (R1 and R2 in formula (B2) are -H and -CH=CH, respectively) was used as an organosilicon polymer. 2 220 parts by mass of polysiloxane (a polysiloxane base that is liquid at room temperature) was mixed with 100 parts by mass of nanoparticles until a uniform slurry was obtained, to obtain a mixture. The obtained mixture was baked in a nitrogen atmosphere at 850°C for 3 hours until the carbon atoms contained in the polysiloxane were carbonized, to obtain composite material B2. The composition of the amorphous material phase of composite material B2 was measured by TEM-EDX, and it was found to be SiO x C z (x=0.82, z=1.21). The content of nanoparticles (active phase) in composite material B2 was approximately 45% by mass.
[0115] Formula (B2):
[0116]
[0117] [Evaluation 2] Test cells were prepared using the negative electrode materials of Comparative Examples 1 and 2 in the same manner as in [Evaluation 1], and charge / discharge was performed to determine the utilization rates of Si contained in composite materials B1 and B2. The evaluation results are shown in Table 1.
[0118] From Table 1, it can be seen that the utilization rate of Si in composite material A1 is extremely high.
[0119] The negative electrode material for secondary batteries according to the present disclosure is useful for secondary batteries used as the main power source for mobile communication devices, portable electronic devices, and the like.
[0120] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.
[0121] 1: electrode group, 2: positive electrode lead, 3: negative electrode lead, 4: battery case, 5: sealing plate, 6: negative electrode terminal, 7: gasket, 8: sealing plug
Claims
1. A negative electrode material for a secondary battery, comprising a composite material including an active phase that reacts with Li and an amorphous material phase, wherein the active phase is dispersed within the amorphous material phase and has a particle diameter of 10 nm or less, the amorphous material phase includes elements A, O, and C, and the element A is at least one selected from the group consisting of Si, Sn, Ti, Al, and Mg.
2. The negative electrode material for a secondary battery according to claim 1, wherein the particle size is 5 nm or less.
3. The negative electrode material for a secondary battery according to claim 1, wherein the spectrum obtained by X-ray diffraction of said composite material does not have a peak attributable to said active phase.
4. The negative electrode material for a secondary battery according to claim 1, wherein the amorphous material phase has substantially no grain boundaries in a cross section of the composite material.
5. The amorphous material phase has the general formula: M a A.O. x N y C z 2. The negative electrode material for secondary batteries according to claim 1, which satisfies the following conditions: 0<a≦4 0<x≦3 0≦y≦1 0≦1-0.5x-0.75y≦z, and the element M is at least one selected from the group consisting of Li, Na, K, Mg, Ca, B and Al.
6. The negative electrode material for a secondary battery according to claim 1, wherein the element A contains at least Si.
7. The negative electrode material for a secondary battery according to claim 5, wherein the element M contains at least Li.
8. The negative electrode material for a secondary battery according to claim 1, wherein voids exist within said amorphous material phase.
9. The negative electrode material for a secondary battery according to claim 1, further comprising a conductive layer covering a surface of the composite material, the conductive layer including carbon.
10. The negative electrode material for a secondary battery according to claim 1, wherein the material constituting the active phase includes at least one selected from the group consisting of a metal phase and an intermetallic compound phase.
11. The metal phase is at least one selected from the group consisting of a Si phase, a Sn phase, a Ti phase, an Al phase and a Mg phase, and the intermetallic compound phase is CrSi 2 Phase, MnSi 2 phase, FeSi 2 Phase, CoSi 2 Phase, NiSi 2 10. The negative electrode material for secondary batteries according to claim 9, which is at least one selected from the group consisting of a LiNiSn phase and a LiNiSn phase.
12. The negative electrode material for a secondary battery according to claim 10, wherein the metal phase further contains at least one element selected from the group consisting of Li, Na, K, Mg, Ca, B and Al.
13. The negative electrode material for a secondary battery according to claim 1, wherein the content of the active phase in the composite material is 50 mass % or less.
14. The negative electrode material for a secondary battery according to claim 1, wherein the content of the active phase in the composite material is 40 mass % or less.
15. The negative electrode material for a secondary battery according to claim 1, wherein at least one selected from the group consisting of graphite, hard carbon and soft carbon is further dispersed within the amorphous material phase.
16. A secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, the negative electrode comprising the negative electrode material for secondary batteries according to claim 1.
17. A method for producing a negative electrode material for a secondary battery, comprising: a first step of reducing an organometallic compound to obtain an intermediate containing an active phase having a median diameter of 10 nm or less as measured by dynamic light scattering; and a second step of sintering the intermediate to obtain a composite material containing an amorphous material phase and the active phase dispersed within the amorphous material phase, wherein the organometallic compound and the amorphous material phase contain elements A, O, and C, and the element A is at least one selected from the group consisting of Si, Sn, Ti, Al, and Mg.
18. The method for producing a negative electrode material for a secondary battery according to claim 17, further comprising a step of granulating the intermediate before firing the intermediate.
19. The method for producing a negative electrode material for a secondary battery according to claim 17, further comprising a step of mixing the intermediate with a polymer before firing the intermediate, and the polymer is carbonized in the second step.
20. The method for producing a negative electrode material for a secondary battery according to claim 17, wherein the organometallic compound is a silane coupling agent.
21. The method for producing a negative electrode material for a secondary battery according to claim 20, wherein the silane coupling agent is at least one selected from the group consisting of 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane.
Citation Information
Patent Citations
Si-C-O AMORPHOUS MATERIAL AND NEGATIVE ELECTRODE FOR LITHIUM SECONDARY BATTERY USING THE MATERIAL
JP2007115548A
Secondary-battery negative-electrode active material, negative electrode, and secondary battery
WO2021157459A1
Active material for battery, composite active material for battery, and secondary battery
WO2022009572A1
Negative electrode active material for secondary batteries and method for producing same
WO2022210512A1
Secondary battery material, negative electrode active material, and secondary battery
WO2023017694A1