Positive electrode active material for nonaqueous electrolyte secondary batteries, nonaqueous electrolyte secondary battery, and method for producing positive electrode active material for nonaqueous electrolyte secondary batteries
The integration of a sulfonic acid compound on the surface of lithium-containing composite oxides with specific Ni and Mn content in non-aqueous electrolyte secondary batteries addresses the compatibility issues of durability and direct current resistance, resulting in enhanced battery performance with improved durability and capacity retention.
Patent Information
- Application Number
- PCT/JP2024/014463
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-10
- Publication Date
- 2024-10-31
AI Technical Summary
Existing non-aqueous electrolyte secondary batteries face challenges in achieving both high durability and low direct current resistance, particularly with single-particulate lithium-containing composite oxides, as previous studies have not adequately addressed the compatibility of suppressing direct current resistance and durability.
A positive electrode active material is developed, comprising lithium-containing composite oxides with a sulfonic acid compound on the surface, specifically composed of single particles with a predetermined average particle size and crystallite size, and containing 70 mol% or more of Ni and Mn, which are synthesized using a method involving metal hydroxides, Li compounds, and sulfonic acid compounds to enhance durability and reduce direct current resistance.
The solution results in a non-aqueous electrolyte secondary battery with improved durability and suppressed direct current resistance, maintaining high capacity retention and efficient charge/discharge characteristics.
Smart Images

Figure JP2024014463_31102024_PF_FP_ABST
Abstract
Description
Positive electrode active material for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and method for manufacturing positive electrode active material for non-aqueous electrolyte secondary battery
[0001] The present disclosure relates to a positive electrode active material for a non-aqueous electrolyte secondary battery, a non-aqueous electrolyte secondary battery, and a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery.
[0002] Lithium-containing composite oxides are used as positive electrode active materials for lithium-ion secondary batteries, which are non-aqueous electrolyte secondary batteries. In recent years, efforts have been made to make lithium-containing composite oxides into single particles in order to improve durability. For example, Patent Document 1 describes a lithium-containing composite oxide having an average particle size of 2 μm to 20 μm and a BET specific surface area of 0.15 m. 2 / g to 1.9m 2 Patent Document 2 discloses single particles of an NCM-based lithium-containing composite oxide (Ni content of 0.3≦Ni≦0.6) having an average particle size of 3 μm to 8 μm and a crystallite size of 1100 Å to 2000 Å.
[0003] Special table publication No. 2018-532236 Publication Patent No. 6850949
[0004] As a result of intensive studies by the present inventors, it has been found that even a lithium-containing composite oxide in the form of a single particle may have poor durability. Furthermore, through further studies, the present inventors have found that a single particle may not be able to achieve both suppression of DC resistance and durability. Patent Documents 1 and 2 do not take into consideration achieving both suppression of DC resistance and durability, and there is still room for improvement.
[0005] An object of the present disclosure is to provide a positive electrode active material that is highly durable and reduces the DC resistance of a battery.
[0006] A positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a lithium-containing composite oxide and a sulfonic acid compound present on a surface of the lithium-containing composite oxide, the lithium-containing composite oxide being composed of single particles having an average particle size of 0.5 μm or more and 5 μm or less, and containing 70 mol % or more of Ni and Mn in total relative to the total molar amount of metal elements excluding Li, and the sulfonic acid compound being represented by general formula I. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)
[0007] A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to one aspect of the present disclosure includes a synthesis step of mixing a metal hydroxide containing 70 mol % or more of Ni and Mn in total with a Li compound, and calcining the mixture to obtain a lithium-containing composite oxide composed of single particles; a washing step of washing the lithium-containing composite oxide with water and dehydrating it to obtain a cake-like composition; a drying step of drying the cake-like composition to obtain a powder-like composition; and an addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition or the powder-like composition.
[0008] A non-aqueous electrolyte secondary battery according to one aspect of the present disclosure is characterized by including a positive electrode containing the above-described positive electrode active material for a non-aqueous electrolyte secondary battery, a negative electrode, and a non-aqueous electrolyte.
[0009] According to the positive electrode active material for a nonaqueous electrolyte secondary battery according to one aspect of the present disclosure, it is possible to provide a nonaqueous electrolyte secondary battery that is highly durable and has reduced direct current resistance.
[0010] 1 is a longitudinal cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment of the present invention;
[0011] In recent years, with the widespread use of non-aqueous electrolyte secondary batteries in automotive applications and power storage applications, there is a demand for non-aqueous electrolyte secondary batteries with high capacity and excellent durability. Furthermore, there is a demand for cost reduction in non-aqueous electrolyte secondary batteries, and a positive electrode active material containing relatively inexpensive Ni and Mn as its main components is preferred. To improve durability, single-particle lithium-containing composite oxides have been investigated as positive electrode active materials, but the properties of the single particles remain largely unknown.
[0012] As a result of intensive studies to solve the above problems, the present inventors have found that it is possible to achieve both high durability and low direct current resistance by having a single particle of a lithium-containing composite oxide containing Ni and Mn as main components, having a predetermined average particle size and crystallite size, and having the surface coated with a predetermined sulfonic acid compound.
[0013] An example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail below. Hereinafter, a cylindrical battery in which a wound electrode assembly is housed in a cylindrical exterior body will be exemplified. However, the electrode assembly is not limited to the wound type and may be a laminated type in which multiple positive electrodes and multiple negative electrodes are alternately stacked one by one with separators interposed therebetween. Furthermore, the exterior body is not limited to a cylindrical shape and may be, for example, a prismatic or coin-shaped body, or may be a battery case made of a laminate sheet including a metal layer and a resin layer. Furthermore, the design of the nonaqueous electrolyte secondary battery according to the present disclosure is not limited to the design of the illustrated nonaqueous electrolyte secondary battery, and known nonaqueous electrolyte secondary battery designs may be applied.
[0014] Fig. 1 is a longitudinal cross-sectional view of a nonaqueous electrolyte secondary battery 10 according to an embodiment. As illustrated in Fig. 1, the nonaqueous electrolyte secondary battery 10 includes an electrode assembly 14, a nonaqueous electrolyte (not shown), and a battery case 15 that accommodates the electrode assembly 14 and the nonaqueous electrolyte. The electrode assembly 14 has a wound structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween. The battery case 15 includes a cylindrical outer can 16 with a bottom and a sealing body 17 that closes the opening of the outer can 16.
[0015] The electrode assembly 14 is composed of a strip-shaped positive electrode 11, a strip-shaped negative electrode 12, two strip-shaped separators 13, a positive electrode tab 20 joined to the positive electrode 11, and a negative electrode tab 21 joined to the negative electrode 12. The negative electrode 12 is disposed, for example, so as to sandwich the positive electrode 11 therebetween.
[0016] The nonaqueous electrolyte secondary battery 10 includes insulating plates 18, 19 disposed above and below the electrode assembly 14. In the example shown in Fig. 1 , a positive electrode tab 20 attached to the positive electrode 11 passes through a through-hole in the insulating plate 18 and extends toward the sealing body 17, while a negative electrode tab 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom of the outer can 16. The positive electrode tab 20 is connected to the underside of a bottom plate 23 of the sealing body 17 by welding or the like, and a cap 27 of the sealing body 17 electrically connected to the bottom plate 23 serves as the positive electrode terminal. The negative electrode tab 21 is connected to the inner bottom surface of the outer can 16 by welding or the like, and the outer can 16 serves as the negative electrode terminal.
[0017] The outer can 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the outer can 16 and the sealing body 17, sealing the internal space of the battery case 15. The outer can 16 has a groove 22 that supports the sealing body 17, formed, for example, by pressing the side surface from the outside. The groove 22 is preferably formed in an annular shape along the circumferential direction of the outer can 16, and supports the sealing body 17 on its upper surface.
[0018] The sealing body 17 has a structure in which, in order from the electrode body 14 side, a bottom plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked. Each member constituting the sealing body 17 has, for example, a disk or ring shape, and each member except for the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0019] The positive electrode 11, negative electrode 12, separator 13, and nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10 will be described in detail below, particularly the positive electrode active material contained in the positive electrode mixture layer 31 that constitutes the positive electrode 11.
[0020] [Positive Electrode] The positive electrode 11 includes, for example, a positive electrode current collector 30 and a positive electrode mixture layer 31 formed on the surface of the positive electrode current collector 30. The positive electrode mixture layer 31 is preferably formed on both sides of the positive electrode current collector 30. The positive electrode current collector 30 may be a foil of a metal, such as aluminum or an aluminum alloy, that is stable within the potential range of the positive electrode 11, or a film having such a metal disposed on the surface. The positive electrode mixture layer 31 may include a positive electrode active material, a conductive agent, and a binder. The thickness of the positive electrode mixture layer 31 is, for example, 10 μm to 150 μm on one side of the positive electrode current collector 30. The positive electrode 11 can be produced, for example, by applying a positive electrode slurry containing a positive electrode active material, a conductive agent, a binder, and the like to the surface of the positive electrode current collector 30, drying the coating, and then rolling the coating to form the positive electrode mixture layer 31 on both sides of the positive electrode current collector 30.
[0021] Examples of the conductive agent contained in the positive electrode mixture layer 31 include carbon-based materials such as carbon black (CB) such as acetylene black (AB) and ketjen black, carbon nanotubes (CNT), graphene, and graphite. These may be used alone or in combination of two or more. The content of the conductive agent in the positive electrode mixture layer 31 is, for example, 0.1 mass % or more and 10 mass % or less with respect to the total mass of the positive electrode mixture layer 31.
[0022] Examples of the binder contained in the positive electrode mixture layer 31 include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, and polyolefin-based resins. These may be used alone or in combination of two or more. The content of the binder in the positive electrode mixture layer 31 is, for example, 0.1% by mass or more and 10% by mass or less with respect to the total mass of the positive electrode mixture layer 31.
[0023] The positive electrode active material contained in the positive electrode mixture layer 31 includes a lithium-containing composite oxide and a sulfonic acid compound present on the surface of the lithium-containing composite oxide. The lithium-containing composite oxide is composed of single particles. The positive electrode active material may include secondary particles formed by agglomeration of single particles in addition to the single particles. This increases the charge density of the positive electrode active material in the positive electrode mixture layer, thereby increasing the capacity of the secondary battery 10. The secondary particles formed by agglomeration of single particles are formed, for example, by agglomeration of 2 to 1000 single particles. The positive electrode active material may also include general primary particles that are not single particles, and secondary particles formed by agglomeration of these primary particles. In addition to the lithium-containing composite oxide, the positive electrode active material may also include LiF, Li 2 S and the like may be contained.
[0024] The proportion of the single particles in the positive electrode active material is preferably 10% or more, more preferably 80% or more, particularly preferably 90% or more, by mass ratio, and may be substantially 100%. Note that the lithium-containing composite oxide may contain secondary particles formed by aggregation of more than 100 primary particles.
[0025] The average particle size of the single particles may be 0.5 μm or more and 5 μm or less, preferably 0.7 μm or more and 4 μm or less. In this specification, the average particle size refers to the volume-based median diameter (D50). D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also called the median diameter. The particle size distribution of the positive electrode active material can be measured, for example, using a laser diffraction particle size distribution measuring device (e.g., MT3000II manufactured by Microtrac-Bell Co., Ltd.) using water as a dispersion medium. If the particle size of the single particles is too large, the battery capacity will decrease and the charge / discharge efficiency will deteriorate. If the particle size of the single particles is too small, secondary aggregation will occur, which will cause battery degradation.
[0026] The BET specific surface area of a single particle is, for example, 0.5 m 2 / g or more 4m 2 / g or less, and preferably 1.0m 2 / g or more 3.5m 2 / g or less. The BET specific surface area of a single particle is 0.5 m 2If the BET specific surface area of the single particle is less than 4 m / g, the contact area between the single particle and the non-aqueous electrolyte will be small, leading to a decrease in capacity. 2 If it exceeds / g, the charge / discharge cycle characteristics may be degraded. Secondary particles have voids within the particles, so even if the particle diameter is large, the specific surface area is relatively large. On the other hand, single particles have no voids within the particles, so the larger the particle diameter, the smaller the BET specific surface area. The particle shapes of secondary particles and single particles vary depending on the production conditions, so the BET specific surface area also varies. The BET specific surface area can be measured, for example, using a Tristar II 3020 (manufactured by Shimadzu Corporation) under the following conditions. Number of measurement points: 11 points (P / P0: 0.05-0.3) Warm Free Space: Measured Equilibration Interval: 5s Analysis Adsorptive: N2 Analysis Bath Temp.: 77.3K (liquefied nitrogen temperature) Cold Free Space: Measured Low Pressure Done: None Analysis method: BET multi-point method
[0027] The BET specific surface area of the lithium-containing composite oxide is A (m 2 / g) and the average particle size of the lithium-containing composite oxide is B (μm), the product AB of A and B preferably satisfies 1.5≦AB≦6, and more preferably satisfies 2≦AB≦5.5. This significantly improves the battery capacity and durability of the secondary battery 10. Secondary particles formed by agglomeration of single particles with small particle sizes may have grain boundary cracks, resulting in a decrease in charge-discharge cycle characteristics. Single particles with large particle sizes may have a decrease in battery capacity. Furthermore, if the BET specific surface area of the single particles is small, the contact area with the non-aqueous electrolyte may be small, resulting in a decrease in battery capacity and deterioration of load characteristics. If the BET specific surface area of the single particles is large, many side reactions such as gas generation may occur in the positive electrode, resulting in a decrease in charge-discharge cycle characteristics. Therefore, by having the product of the average particle size (D50) and the BET specific surface area within the above range, a secondary battery 10 with high capacity, high durability, and suppressed gas generation can be obtained.
[0028] The crystallite size of the single particles is preferably 300 Å or more and 800 Å or less. By having the single particles have the above average particle size and crystallite size, a secondary battery 10 with high capacity and improved durability can be obtained. Here, the crystallite size is calculated from the half-width of the diffraction peak of the (104) plane in the X-ray diffraction pattern by X-ray diffraction using the Scherrer formula shown below. In the formula below, s is the crystallite size, λ is the wavelength of the X-ray, B is the half-width of the diffraction peak of the (104) plane, θ is the diffraction angle (rad), and K is the Scherrer constant. In this embodiment, K is set to 0.9. s = Kλ / B cos θ
[0029] The X-ray diffraction pattern was obtained by powder X-ray diffraction using a powder X-ray diffractometer (Rigaku Corporation, trade name "RINT-TTR", Cu-Kα source) under the following conditions: Measurement range: 15-120° Scan speed: 4° / min Analysis range: 30-120° Background: B-spline Profile function: divided pseudo-Voigt function Constraint conditions: Li(3a) + Ni(3a) = 1 Ni(3a) + Ni(3b) = α (α is the Ni content of each element) ICSD No.: 98-009-4814
[0030] The lithium-containing composite oxide contains 70 mol% or more of Ni and Mn in total relative to the total molar amount of metal elements excluding Li. This makes it possible to obtain a lithium-containing composite oxide with a high capacity at a relatively low cost. The lithium-containing composite oxide may be composed only of Ni and Mn. The content of the metal elements contained in the lithium-containing composite oxide is measured, for example, by inductively coupled plasma (ICP) atomic emission spectroscopy.
[0031] Ni is preferably contained in the largest amount among the metal elements other than Li constituting the lithium-containing composite oxide. The Ni content in the lithium-containing composite oxide is preferably 50 mol% or more, more preferably 70 mol% or more, based on the total molar amount of the metal elements excluding Li. The upper limit of the Ni content may be 95 mol%, and is preferably 90 mol%.
[0032] Mn can stabilize the crystal structure of the lithium-containing composite oxide. The content of Mn in the lithium-containing composite oxide is, for example, 5 mol % to 50 mol % relative to the total molar amount of metal elements excluding Li.
[0033] The lithium-containing composite oxide has the general formula Li a Ni x Mn y M1 z M2 w O 2-b (wherein 0.8≦a≦1.2, 0.5≦x≦0.9, 0.05≦y≦0.5, 0≦z≦0.2, 0≦w≦0.1, 0≦b<0.05, x+y≧0.7, x+y+z+w=1, M1 is at least one element selected from the group consisting of Al and Co, and M2 is at least one element selected from Fe, Ti, Si, Nb, Zr, Mo, and Zn).
[0034] By using single particles, a high capacity retention rate can be maintained even at a high charging potential. In particular, a lithium-containing composite oxide having a Ni content of 80% or less and a high Mn content in its composition can obtain a high capacity by increasing the charging potential, and therefore is preferably composed of single particles that are resistant to high potentials.
[0035] The sulfonic acid compound present on the surface of the lithium-containing composite oxide is represented by the following general formula I. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)
[0036] In general formula I, A is preferably a Group 1 element, more preferably Li. This can further reduce the DC resistance. When A is a Group 1 element, n=1.
[0037] In general formula I, R is preferably an alkyl group. R is more preferably an alkyl group having 5 or less carbon atoms, further preferably an alkyl group having 3 or less carbon atoms, and particularly preferably a methyl group. In addition, in R, some of the hydrogen atoms bonded to the carbon atoms may be substituted with fluorine. However, in R, not all of the hydrogen atoms bonded to the carbon atoms are substituted with fluorine. The smaller the molecular weight of R, the smaller the DC resistance can be.
[0038] Examples of sulfonic acid compounds include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, magnesium methanesulfonate, and lithium fluoromethanesulfonate.
[0039] The amount of the sulfonic acid compound present on the surface of the lithium-containing composite oxide is preferably 0.1 mass % or more and 2 mass % or less, and more preferably 0.25 mass % or more and 1.0 mass % or less, relative to the mass of the lithium-containing composite oxide.
[0040] The presence of the sulfonic acid compound on the surface of the lithium-containing composite oxide can be confirmed by, for example, Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode active material exhibits a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It may have an absorption peak at at least one point in the vicinity.
[0041] In the infrared absorption spectrum obtained by FT-IR, for example, a positive electrode active material containing lithium methanesulfonate has a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It has an absorption peak around 1238 cm -1 , 1175 cm -1 , 1065 cm -1 The peak around 785 cm is an absorption peak due to the SO stretching vibration of lithium methanesulfonate.-1 The peak in the vicinity is an absorption peak due to the C-S stretching vibration derived from lithium methanesulfonate.
[0042] In a positive electrode active material containing a sulfonic acid compound other than lithium methanesulfonate, an absorption peak derived from the sulfonic acid compound contained in the positive electrode active material can be identified, similar to a positive electrode active material containing lithium methanesulfonate. The presence of the sulfonic acid compound on the surface of the lithium-containing composite oxide can also be confirmed by ICP, atomic absorption spectroscopy, X-ray photoelectron spectroscopy (XPS), synchrotron XRD measurement, TOF-SIMS, or the like.
[0043] The average particle diameter of the sulfonic acid compound is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less. By setting the average particle diameter of the sulfonic acid compound to preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less, the sulfonic acid compound can be more uniformly adhered to the entire positive electrode active material powder, and the effect of the sulfonic acid compound can be more significantly exhibited. Here, the average particle diameter of the sulfonic acid compound can be determined by observing the sulfonic acid compound adhered to the surface of the lithium-containing composite oxide with an SEM. Specifically, the outer shapes of 50 randomly selected particles are identified, and the major axis (longest axis) of each of the 50 particles is determined, and the average value thereof is taken as the average particle diameter of the sulfonic acid compound.
[0044] By making a sulfonic acid compound exist on the surface of the lithium-containing composite oxide, Li is + In particular, by coating the surface of a single particle of a lithium-containing composite oxide, which has a small BET specific surface area and is likely to have a high initial DCR, with a sulfonic acid compound, a material with excellent single particle durability and initial DCR can be obtained.
[0045] A metal compound may be present on the surface of the lithium-containing composite oxide. The metal compound contains, for example, one or more metal elements selected from the group consisting of Sr, Ca, W, Zr, rare earth elements, and Al. Examples of the Sr-containing compound include SrO, Sr(OH), and the like. 2 and SrCO3 Examples of compounds containing Ca include CaO and Ca(OH). 2 and CaCO 3 Examples of compounds containing W include WO 3 Examples of the compound containing Al include Al 2 O 3 Examples of compounds containing Zr include ZrO 2 , Zr(OH) 4 , Zr(CO 3 ) 2 and Zr(SO 4 ) 2 ・4H 2 Examples of rare earth-containing compounds include oxides, hydroxides, carbonates, sulfates, nitrates, and phosphates of rare earth elements. The metal compound may contain a plurality of types of these metal elements, and examples thereof include SrAlO 4 , CaAlO 4 The metal compound may further contain Li, and an example thereof is lithium tungstate.
[0046] A nonmetallic compound may be present on the surface of the lithium-containing composite oxide. The nonmetallic compound contains, for example, one or more nonmetallic elements selected from the group consisting of P and B. Examples of the P-containing compound include Li, 3-x H x P.O. 4 (0≦x≦3) can be exemplified. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O 7 Examples include:
[0047] The positive electrode active material may have an alkali content of 150 μmol / g or less, preferably 100 μmol / g or less, as measured by the Walder method. That is, the positive electrode active material may contain a small amount of a water-soluble alkali component that can be titrated with an acid. A small amount of alkali component contained in the positive electrode active material improves the stability of the slurry and improves productivity.
[0048] The positive electrode active material contains an alkaline component in an amount corresponding to the above-mentioned acid consumption amount. Examples of the alkaline component include lithium hydroxide (LiOH) and lithium carbonate (Li 2 CO 3 ) and the like. Lithium carbonate and lithium hydroxide may be present at the interface between each primary particle inside the composite oxide particle and on the surface of secondary particles formed by aggregation of primary particles. These are preferably present substantially uniformly without being unevenly distributed on a part of the surface of the primary particle. By having these present substantially uniformly on the surface of the primary particle, reaction unevenness during charge and discharge is less likely to occur, and a decrease in durability can be suppressed.
[0049] The method for quantifying the alkali content using the Walder method is as follows: (1) 1 g of positive electrode active material is added to 30 ml of pure water and stirred to prepare a suspension in which the active material is dispersed in water. (2) The suspension is filtered, and pure water is added to make a 70 ml volume, obtaining a filtrate containing water-soluble alkali components eluted from the active material. (3) While measuring the pH of the filtrate, hydrochloric acid is added dropwise to the filtrate. The amount of hydrochloric acid consumed (titration amount) X mol / g up to the first inflection point (near pH 8) on the pH curve and the amount of hydrochloric acid consumed Y mol / g up to the second inflection point (near pH 4) are determined. The inflection points are the peak positions of the differential value with respect to the titration amount. (4) The alkali content is the value X-(Y-X), which is obtained from the measured X and Y above.
[0050] The positive electrode mixture layer 31 may contain other positive electrode active materials in addition to the positive electrode active material of the present embodiment described above. Examples of other positive electrode active materials include lithium-containing composite oxides having Ni and Mn contents of 0 mol % or more and less than 70 mol %.
[0051] Next, an example of a method for producing the positive electrode active material according to this embodiment will be described. The method for producing the positive electrode active material includes, for example, a synthesis step, a washing step, a drying step, and an addition step.
[0052] In the synthesis step, a metal hydroxide containing 70 mol % or more of Ni and Mn in total is mixed with a Li compound, and the mixture is fired to obtain a lithium-containing composite oxide composed of single particles.
[0053] The metal hydroxide can be obtained, for example, by adding an alkaline solution such as sodium hydroxide dropwise to a stirred solution of a metal salt containing Ni, Mn, and an optional metal element (Al, Co, etc.) and adjusting the pH to the alkaline side (e.g., 8.5 to 12.5), thereby precipitating (co-precipitating) a composite hydroxide containing Ni, Mn, and the optional metal element. Note that, instead of the metal hydroxide, a metal oxide obtained by heat-treating the metal hydroxide may be used. The particle size of the metal hydroxide is preferably 7 μm or less, since the smaller the particle size, the easier it is for primary particles to grow.
[0054] Examples of Li compounds include Li 2 CO 3 , LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4 , LiOH·H 2 Examples of suitable metal materials include O, LiH, and LiF. The mixing ratio of the metal hydroxide and the Li compound is preferably such that the molar ratio of metal elements excluding Li to Li is in the range of 1:0.8 to 1:1.2, in order to facilitate adjustment of the above-mentioned parameters to the ranges specified above. When mixing the metal oxide and the Li compound, other metal materials may be added as necessary. Here, the other metal materials are oxides containing metal elements other than the metal elements constituting the metal oxide.
[0055] The mixture of metal hydroxide and Li compound, etc., is fired, for example, in an oxygen atmosphere (flowing a gas with an oxygen concentration of 80% or more). The firing conditions may include a temperature rise rate of more than 1.0°C / min and less than 5.5°C / min from 450°C to 680°C, and a maximum temperature of 850°C to 1100°C. The temperature rise rate from over 680°C to the maximum temperature may be, for example, 0.1°C / min to 3.5°C / min. The holding time at the maximum temperature may be 1 hour to 30 hours, preferably 1 hour to 25 hours. This firing process may be a multi-stage firing, and multiple first and second heating rates may be set for each temperature range as long as they are within the above-specified range. The particle size of the single particles can be adjusted by adjusting the firing conditions. For example, the particle size of the single particles can be increased by increasing the maximum temperature.
[0056] In the washing step, the lithium-containing composite oxide obtained in the synthesis step is washed with water and dehydrated to obtain a cake-like composition. The washing and dehydration can be performed by a known method and under known conditions. The washing and dehydration should be performed within a range in which lithium is not eluted from the lithium-containing composite oxide and the battery characteristics are not deteriorated. Since the positive electrode active material according to this embodiment is washed with water, the amount of residual alkaline components is small.
[0057] In the drying step, the cake-like composition obtained in the washing step is dried to obtain a powdery composition. The drying step may be performed under a vacuum atmosphere. Drying conditions are, for example, 150°C to 400°C for 0.5 hours to 15 hours. A heat treatment may be performed after the drying step. The heating temperature is, for example, 100°C to 450°C. The heat treatment may be performed after the crushing step described below.
[0058] The powder composition obtained in the drying step can be crushed to obtain single particles. A jet mill or the like can be used for crushing. Crushing using a jet mill can be performed using, for example, a PJM-80 (manufactured by Nippon Pneumatic Co., Ltd.) under the following conditions: Compressed air consumption: 0.5 Nm 3 / min Supply gas pressure: 0.53 MPa Processing capacity: 2000 g / hour
[0059] In the addition step, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the cake-like composition obtained in the washing step or the powder-like composition obtained in the drying step. This allows the sulfonic acid compound to adhere to the surface of the lithium-containing transition metal composite oxide. It is preferable to add at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition. The sulfonic acid compound may be in either powder or solution form. The sulfonic acid solution is, for example, a methanesulfonic acid solution obtained by dissolving methanesulfonic acid in water. Li compounds remain in the cake-like composition, and these remaining Li compounds are dissolved in the water contained in the cake-like composition. Therefore, even when a sulfonic acid solution is added, a Li-containing sulfonic acid compound is formed. From the viewpoint of more easily achieving the effects of the present application, a Li compound or a Li compound solution may be added to the cake-like composition or the powder-like composition together with the sulfonic acid solution. Alternatively, a mixed solution in which a sulfonic acid solution and a Li compound or a Li compound solution are premixed may be added to the cake-like composition or the powder-like composition. The Li compound is, for example, LiOH, and the Li compound solution is, for example, a LiOH solution obtained by dissolving LiOH in water. The amounts of the Li compound and sulfonic acid solution added to the cake-like composition preferably satisfy the relationship of 0≦Li compound / sulfonic acid≦1.3 in molar ratio. The amount of sulfonic acid compound or sulfonic acid added is preferably 0.1% by mass to 1% by mass, more preferably 0.3% by mass to 0.8% by mass, relative to the mass of the lithium-containing transition metal composite oxide. The concentrations of the sulfonic acid solution and the sulfonic acid compound solution are, for example, 0.5% by mass to 40% by mass. The addition step may be performed during or after the washing step, during or after the drying step, and the timing of the addition can be changed as appropriate.
[0060] A metal compound containing one or more metal elements selected from the group consisting of Sr, Ca, W, Zr, rare earth elements, and Al, and a nonmetallic compound containing one or more nonmetallic elements selected from the group consisting of P and B can be attached to the surface of the lithium-containing composite oxide by adding the raw material of the metal compound or nonmetallic compound during the synthesis process, after the synthesis process, during the washing process, after the washing process, during the drying process, after the drying process, or during the addition process. 2 , Sr(OH) 2 ・8H 2 O, SrO, SrCo 3 , SrSO 4 , Sr(NO 3 ) 2、 SrCl 2 , SrAlO 4 Examples of Ca raw materials include Ca(OH) 2 , CaO, CaCO 3 , CaSO 4 , Ca(NO 3 ) 2、 CaCl 2 , CaAlO 4 The Zr raw material is Zr(OH) 4 , ZrO 2 , Zr(CO 3 ) 2 , Zr(SO 4 ) 2 ・4H 2 Examples of rare earth raw materials include oxides, hydroxides, and carbonates of rare earth elements. Examples of W raw materials include tungsten oxide (WO 3 ), lithium tungstate (Li 2 WO 4 , Li 4 WO 5 , Li 6 W 2 O 9 As the W raw material, a solution containing W may be used. As the Al raw material, Al 2 O 3、 Al(OH) 3、 Al 2 (SO 4 ) 3The P raw material may be Al derived from a lithium-containing composite oxide. 3-x H x P.O. 4 (0≦x≦3) and the like. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O 7 These compounds may be pulverized to appropriately change the particle size, or the water content of the hydrates may be adjusted before use.
[0061] [Negative Electrode] The negative electrode 12 may have, for example, a negative electrode current collector 40 and a negative electrode mixture layer 41 formed on the surface of the negative electrode current collector 40, or a metal Li foil may be used as the negative electrode 12. Alternatively, the negative electrode 12 may have a negative electrode current collector 40, and lithium metal may be deposited on the surface of the negative electrode current collector 40 upon charging. When the negative electrode 12 has a negative electrode mixture layer 41, the negative electrode mixture layer 41 is preferably formed on both sides of the negative electrode current collector 40. The negative electrode current collector 40 may be a foil of a metal that is stable within the potential range of the negative electrode 12, such as copper or a copper alloy, or a film with such a metal disposed on the surface layer. The thickness of the negative electrode current collector 40 is, for example, 5 μm to 30 μm. The negative electrode mixture layer 41 includes, for example, a negative electrode active material and a binder. The thickness of the negative electrode mixture layer 41 is, for example, 10 μm to 150 μm on one side of the negative electrode core. The negative electrode 12 can be produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, and the like to the surface of the negative electrode current collector 40, drying the coating, and then rolling it to form the negative electrode mixture layer 41 on both sides of the negative electrode current collector 40.
[0062] The negative electrode active material contained in the negative electrode mixture layer 41 is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, a carbon material such as graphite is used. The graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, or artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads. Furthermore, as the negative electrode active material, metals that alloy with Li, such as Si and Sn, metal compounds containing Si, Sn, and lithium-titanium composite oxides, may also be used. Furthermore, these may be provided with a carbon coating. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.
[0063] Examples of the binder contained in the negative electrode mixture layer 41 include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.
[0064] [Separator] The separator 13 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a laminated structure. Furthermore, a highly heat-resistant resin layer such as an aramid resin, or a filler layer containing an inorganic compound filler may be provided on the surface of the separator 13.
[0065] [Non-aqueous electrolyte]
[0066] The non-aqueous electrolyte has lithium ion conductivity and may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.
[0067] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms in these solvents are substituted with halogen atoms such as fluorine. Examples of the halogen-substituted compound include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).
[0068] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0069] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, and methyl phenyl ether. and chain ethers such as ethyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0070] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiClO 4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO 2 F 2Examples of the borate salt include lithium bis(oxalato)borate (LiBOB) and lithium difluoro(oxalato)borate (LiDFFOB). Examples of the imide salt include lithium bisfluorosulfonylimide (LiN(FSO 2 ) 2 ), lithium bistrifluoromethanesulfonyl imide (LiN(CF 3 SO 2 ) 2 ), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 )), lithium bispentafluoroethanesulfonyl imide (LiN(C 2 F 5 SO 2 ) 2 Among these, LiPF is preferred from the viewpoint of ionic conductivity, electrochemical stability, etc. 6 The concentration of the lithium salt may be, for example, 4 mol or less, or 3 mol or less, preferably 1.8 mol or less, and more preferably 0.8 to 1.8 mol per liter of the non-aqueous solvent.
[0071] The non-aqueous electrolyte may contain an additive such as an unsaturated carbonate ester, an acid anhydride, a phenol compound, a benzene compound, a nitrile compound, an isocyanate compound, a sultone compound, a sulfate compound, a borate ester compound, a phosphate ester compound, or a phosphite ester compound.
[0072] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate. One type of unsaturated cyclic carbonate may be used alone, or two or more types may be used in combination. Some of the hydrogen atoms in the unsaturated cyclic carbonate may be substituted with fluorine atoms. The acid anhydride may be an anhydride formed by intermolecular condensation of multiple carboxylic acid molecules, but is preferably an acid anhydride of a polycarboxylic acid. Examples of polycarboxylic acid anhydrides include succinic anhydride, maleic anhydride, and phthalic anhydride.
[0073] Examples of phenolic compounds include phenol, hydroxytoluene, etc. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), etc.
[0074] Examples of nitrile compounds include adiponitrile, pimelonitrile, propionitrile, and succinonitrile. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and bisisocyanatomethylcyclohexane (BIMCH). Examples of sultone compounds include propane sultone and propene sultone. Examples of sulfate compounds include ethylene sulfate, ethylene sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tris(trimethylsilyl)borate. Examples of phosphate ester compounds include trimethyl phosphate and tris(trimethylsilyl)phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tris(trimethylsilyl)phosphite.
[0075] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.
[0076] Hereinafter, the present disclosure will be further described with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0077] Example 1-1 [Preparation of Positive Electrode Active Material] LiOH and Ni having an average particle size of 6 μm obtained by coprecipitation method 0.8 Mn 0.2 (OH) 2The powders were mixed so that the molar ratio of Li to the total amount of Ni and Mn was 1.1:1 to obtain a mixture. This mixture was fired under an oxygen stream with an oxygen concentration of 90% or more (a flow rate of 0.15 L / min to 0.2 L / min per 1 L of furnace volume) from room temperature to 650 °C for 5 hours, then fired to 900 °C for 2 hours, and held for 9 hours to obtain a lithium transition metal composite oxide (synthesis step). Water was added to this lithium-containing composite oxide so that the slurry concentration was 1500 g / L, stirred for 15 minutes, and filtered to obtain a cake-like composition (washing step). Powdered lithium methanesulfonate was added to this cake-like composition (addition step). The amount of lithium methanesulfonate added was 0.25 mass% relative to the total mass of the lithium-containing composite oxide. After the addition step, a drying step was performed under conditions of 180 °C in a vacuum atmosphere for 2 hours to obtain secondary particles in which single particles were aggregated. The secondary particles were then crushed in a jet mill to obtain a single-particle cathode active material of Example 1. Fourier transform infrared spectroscopy (FT-IR) confirmed the presence of lithium methanesulfonate on the surface of the cathode active material. The alkali content measured by the Walder method was 80 μmol / g.
[0078] [Preparation of Positive Electrode] The positive electrode active material, acetylene black, and polyvinylidene fluoride were mixed in a mass ratio of 92:5:3, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry was applied to a positive electrode current collector made of aluminum foil, the coating was dried and compressed, and then the positive electrode current collector was cut to a predetermined electrode size to obtain a positive electrode in which a positive electrode mixture layer was disposed on both sides of the positive electrode current collector. Note that an exposed portion was provided in part of the positive electrode, exposing the surface of the positive electrode current collector.
[0079] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0080] [Preparation of Test Cell] A positive electrode lead was attached to the exposed portion of the positive electrode, and a negative electrode lead was attached to the lithium metal foil serving as the negative electrode, and the positive and negative electrodes were spirally wound with a polyolefin separator interposed therebetween to prepare a wound electrode assembly. This electrode assembly was housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was poured into it. The opening of the exterior body was then sealed to obtain a test cell.
[0081] [Evaluation of Initial DCR] The test cell was charged at a constant current of 0.2 C in a temperature environment of 25°C until the cell voltage reached 4.5 V (vs. Li), and then charged at a constant voltage of 4.5 V (vs. Li) until the current reached 0.02 C. After 1 hour, the cell was discharged at a constant current of 0.2 C until the cell voltage reached 2.5 V (vs. Li). This was designated the initial cycle. Thereafter, the test cell was again charged at a constant current of 0.2 C in a temperature environment of 25°C until the capacity reached 50% of the initial discharge capacity at a constant voltage of 4.5 V (vs. Li). The SOC of the secondary battery at this time was 50%. The secondary battery was then left to stand in an open circuit for 1 hour, and then subjected to a constant current discharge at a constant current of 0.5 C for 10 seconds. The open circuit voltage (OCV), the closed circuit voltage (CCV) 10 seconds after discharge, and the current value (I) 10 seconds after discharge were measured. 10s The DC resistance (DCR) was calculated from the OCV-CCV using the following formula, and this value was used as the initial DCR: Initial DCR = (OCV-CCV) / I 10s
[0082] [Evaluation of Capacity Retention Rate] The test cell was charged at a constant current of 0.2 C in an environment of 25°C until the battery voltage reached 4.5 V (vs. Li), and then charged at a constant voltage of 4.5 V (vs. Li) until the current value reached 0.02 C. Thereafter, the test cell was discharged at a constant current of 0.2 C until the battery voltage reached 2.5 V (vs. Li). This cycle of charge and discharge was counted as one cycle, and 30 cycles were performed. The capacity retention rate of the test cell during the charge and discharge cycles was calculated using the following formula: Capacity retention rate = (discharge capacity at 30th cycle / discharge capacity at 1st cycle) x 100
[0083] Example 1-2 A test cell was prepared and evaluated in the same manner as in Example 1-1, except that in the addition step of preparing the positive electrode active material, the amount of lithium methanesulfonate added was 0.5 mass% relative to the total mass of the lithium-containing composite oxide. The alkali amount measured by the Walder method was 82 μmol / g.
[0084] Example 1-3 A test cell was prepared and evaluated in the same manner as in Example 1-1, except that in the addition step of preparing the positive electrode active material, the amount of lithium methanesulfonate added was 1.0 mass% relative to the total mass of the lithium-containing composite oxide. The alkali amount measured by the Walder method was 85 μmol / g.
[0085] Example 1-4 A test cell was prepared and evaluated in the same manner as in Example 1-1, except that in the addition step of preparing the positive electrode active material, the amount of lithium methanesulfonate added was 2.0 mass% relative to the total mass of the lithium-containing composite oxide. The alkali amount measured by the Walder method was 90 μmol / g.
[0086] Example 1-5 A test cell was prepared and evaluated in the same manner as in Example 1-3, except that in the synthesis step of preparing the positive electrode active material, the maximum temperature reached was changed to 850° C. The alkali content measured by the Walder method was 95 μmol / g.
[0087] Example 1-6 A test cell was prepared and evaluated in the same manner as in Example 1-3, except that in the synthesis step of preparing the positive electrode active material, the maximum temperature reached was changed to 950° C. The alkali content measured by the Walder method was 75 μmol / g.
[0088] Example 1-7 A test cell was prepared and evaluated in the same manner as in Example 1-3, except that lithium ethanesulfonate was added instead of lithium methanesulfonate in the addition step of preparing the positive electrode active material. The presence of lithium ethanesulfonate on the surface of the positive electrode active material was confirmed by Fourier transform infrared spectroscopy (FT-IR). The alkali content measured by the Walder method was 80 μmol / g.
[0089] Example 1-8 A test cell was prepared and evaluated in the same manner as in Example 1-3, except that sodium methanesulfonate was added instead of lithium methanesulfonate in the addition step of preparing the positive electrode active material. The presence of sodium methanesulfonate on the surface of the positive electrode active material was confirmed by Fourier transform infrared spectroscopy (FT-IR). The alkali content measured by the Walder method was 82 μmol / g.
[0090] Example 1-9 A test cell was prepared and evaluated in the same manner as in Example 1-1, except that in the addition step of preparing the positive electrode active material, a lithium methanesulfonate solution prepared by dissolving lithium methanesulfonate in pure water was added instead of powdered lithium methanesulfonate, and the amount of lithium methanesulfonate added relative to the total mass of the lithium-containing composite oxide was 1.0 mass%. The concentration of the added lithium methanesulfonate solution was 10 mass%, and the lithium methanesulfonate solution was added so that the amount of lithium methanesulfonate added was as described above. Fourier transform infrared spectroscopy (FT-IR) confirmed the presence of lithium methanesulfonate on the surface of the positive electrode active material. The alkali content measured by the Walder method was 81 μmol / g.
[0091] Example 1-10 A test cell was prepared and evaluated in the same manner as in Example 1-1, except that in the addition step of preparing the positive electrode active material, a methanesulfonic acid solution was added instead of powdered lithium methanesulfonate, and the amount of methanesulfonic acid added relative to the total mass of the lithium-containing composite oxide was 1.0 mass%. The concentration of the added methanesulfonic acid solution was 10 mass%, and the methanesulfonic acid solution was added so that the amount of methanesulfonic acid added was as described above. Fourier transform infrared spectroscopy (FT-IR) confirmed the presence of lithium methanesulfonate on the surface of the positive electrode active material. The alkali content measured by the Walder method was 74 μmol / g.
[0092] Example 1-11 In the addition step of preparing the positive electrode active material, a solution containing methanesulfonic acid and LiOH (hereinafter, methanesulfonic acid + LiOH solution) was added in pure water in a molar ratio of 1:0.5, instead of powdered lithium methanesulfonate. The amount of lithium methanesulfonate added relative to the total mass of the lithium-containing composite oxide was 1.0% by mass. A test cell was prepared and evaluated in the same manner as in Example 1-1. The concentration of the added methanesulfonic acid + LiOH solution was 10% by mass, and the methanesulfonic acid + LiOH solution was added so that the amount of lithium methanesulfonate added was as described above. Fourier transform infrared spectroscopy (FT-IR) confirmed the presence of lithium methanesulfonate on the surface of the positive electrode active material. The amount of alkali measured by the Walder method was 77 μmol / g.
[0093] Example 1-12 A test cell was prepared and evaluated in the same manner as in Example 1-1, except that in the addition step of preparing the positive electrode active material, a methanesulfonic acid + LiOH solution was added in place of powdered methanesulfonate, so that the molar ratio of methanesulfonic acid to LiOH was 1:1. The amount of lithium methanesulfonate added relative to the total mass of the lithium-containing composite oxide was 1.0% by mass. The concentration of the added methanesulfonic acid + LiOH solution was 10% by mass, and the methanesulfonic acid + LiOH solution was added so that the amount of lithium methanesulfonate added was as described above. Fourier transform infrared spectroscopy (FT-IR) confirmed the presence of lithium methanesulfonate on the surface of the positive electrode active material. The alkali content measured by the Walder method was 79 μmol / g.
[0094] Comparative Example 1-1 A test cell was produced and evaluated in the same manner as in Example 1-1, except that the addition step was not carried out in the production of the positive electrode active material.
[0095] <Comparative Example 1-2> A test cell was produced and evaluated in the same manner as in Example 1-1, except that in the addition step of producing a positive electrode active material, a 10 mass % lithium succinate solution was added instead of the methanesulfonic acid solution, and the amount of lithium succinate added relative to the total mass of the lithium-containing composite oxide was 1.0 mass %.
[0096] Comparative Example 1-3 A test cell was produced and evaluated in the same manner as in Example 1-1, except that in the addition step of producing a positive electrode active material, a 10 mass % lithium oxalate solution was added instead of the methanesulfonic acid solution, and the amount of lithium oxalate added relative to the total mass of the lithium-containing composite oxide was 1.0 mass %.
[0097] Comparative Example 1-4 A test cell was prepared and evaluated in the same manner as in Example 1-3, except that in the synthesis step of preparing the positive electrode active material, the maximum temperature reached was changed to 1000° C. The alkali amount measured by the Walder method was 82 μmol / g.
[0098] <Comparative Example 1-5> A test cell was prepared and evaluated in the same manner as in Example 1-3, except that in the synthesis step of preparing the positive electrode active material, the maximum temperature was changed to 750°C, the holding time at the maximum temperature was changed to 3 hours, and the secondary particles were not crushed using a jet mill after the drying step. The positive electrode active material of Comparative Example 1-5 had a secondary particle shape. The alkali content measured by the Walder method was 65 μmol / g.
[0099] Example 2-1 In the synthesis process of the positive electrode active material, the composition of the metal hydroxide was changed to Ni 0.5 Mn 0.5 (OH) 2 A test cell was prepared and evaluated in the same manner as in Example 1-3, except that the temperature was changed to 1000°C, the maximum temperature was changed to 1050°C, and the holding time at the maximum temperature was changed to 10 hours. The alkali content measured by the Walder method was 38 μmol / g.
[0100] Example 2-2 A test cell was prepared and evaluated in the same manner as in Example 2-1, except that in the synthesis step of preparing the positive electrode active material, the maximum temperature reached was changed to 1000° C. The alkali amount measured by the Walder method was 45 μmol / g.
[0101] Comparative Example 2 A test cell was produced and evaluated in the same manner as in Example 2-1, except that the addition step was not carried out in the production of the positive electrode active material.
[0102] The initial DCRs and capacity retention rates of the test cells of the examples and comparative examples are shown separately in Tables 1 and 2. The initial DCRs and capacity retention rates of the test cells of Examples 1-1 to 1-12 and Comparative Examples 1-1 to 1-5 shown in Table 1 are expressed relative to the initial DCRs and capacity retention rates of the test cell of Comparative Example 1-1, each of which is set to 100. Furthermore, the initial DCRs and capacity retention rates of the test cells of Examples 2-1 to 2-2 and Comparative Example 2 shown in Table 2 are expressed relative to the initial DCRs and capacity retention rates of the test cell of Comparative Example 2, each of which is set to 100.
[0103]
[0104]
[0105] In Tables 1 and 2, the test cells of the examples had lower initial DCRs and higher capacity retention rates than the test cells of the comparative examples. By using a positive electrode active material in which a sulfonic acid compound is present on the surface of single particles having a predetermined composition, a nonaqueous electrolyte secondary battery with high durability and reduced DC resistance can be provided.
[0106] The present disclosure will be further described by the following embodiments. Configuration 1: A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium-containing composite oxide and a sulfonic acid compound present on the surface of the lithium-containing composite oxide, wherein the lithium-containing composite oxide is composed of single particles having an average particle size of 0.5 μm or more and 5 μm or less, and contains 70 mol % or more of Ni and Mn in total relative to the total molar amount of metal elements excluding Li, and the sulfonic acid compound is represented by general formula I. (wherein A is a Group 1 element or a Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) Configuration 2: The positive electrode active material for a non-aqueous electrolyte secondary battery according to Configuration 1, wherein the crystallite size of the single particle is 300 Å or more and 800 Å or less. Configuration 3: The BET specific surface area of the lithium-containing composite oxide is A (m 2 / g) and an average particle size of the lithium-containing composite oxide is B (μm), the product AB of A and B satisfies 1.5≦AB≦6. Configuration 4: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, having an alkali content of 150 μmol / g or less as measured by the Walder method. Configuration 5: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein A is a Group 1 element. Configuration 6: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein A is Li. Configuration 7: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 6, wherein R is an alkyl group. Configuration 8: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 6, wherein R is a methyl group. Aspect 9: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Aspects 1 to 8, wherein the amount of the sulfonic acid compound present on the surface of the lithium-containing composite oxide is 0.1% by mass or more and 2% by mass or less, relative to the mass of the lithium-containing composite oxide. Aspect 10: A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, comprising: a synthesis step of mixing a metal hydroxide containing 70 mol % or more of Ni and Mn in total with a Li compound, and firing the mixture to obtain a lithium-containing composite oxide composed of single particles; a washing step of washing the lithium-containing composite oxide with water and dehydrating it to obtain a cake-like composition; a drying step of drying the cake-like composition to obtain a powder-like composition; and an addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition or the powder-like composition. Aspect 11: A non-aqueous electrolyte secondary battery comprising: a positive electrode containing the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Aspects 1 to 9, a negative electrode, and a non-aqueous electrolyte.
[0107] REFERENCE SIGNS LIST 10 Non-aqueous electrolyte secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 15 Battery case, 16 Outer can, 17 Sealing body, 18, 19 Insulating plate, 20 Positive electrode tab, 21 Negative electrode tab, 22 Grooved portion, 23 Bottom plate, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket, 30 Positive electrode current collector, 31 Positive electrode mixture layer, 40 Negative electrode current collector, 41 Negative electrode mixture layer
Claims
1. A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium-containing composite oxide and a sulfonic acid compound present on a surface of the lithium-containing composite oxide, wherein the lithium-containing composite oxide is composed of single particles having an average particle size of 0.5 μm or more and 5 μm or less, and contains Ni and Mn in a total amount of 70 mol % or more based on the total molar amount of metal elements excluding Li, and the sulfonic acid compound is represented by general formula I. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) 2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the crystallite size of said single particle is 300 Å or more and 800 Å or less.
3. The BET specific surface area of the lithium-containing composite oxide is A (m 2 2. The positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1 , wherein, when A is the surface area of the lithium-containing composite oxide, and B is an average particle size of the lithium-containing composite oxide, a product AB of A and B satisfies 1.5≦AB≦6.
4. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, having an alkali content of 150 μmol / g or less as measured by the Walder method.
5. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is a Group 1 element.
6. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is Li.
7. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is an alkyl group.
8. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is a methyl group.
9. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the amount of the sulfonic acid compound present on the surface of the lithium-containing composite oxide is 0.1 mass % or more and 2 mass % or less with respect to the mass of the lithium-containing composite oxide.
10. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, comprising: a synthesis step of mixing a metal hydroxide containing 70 mol % or more of Ni and Mn in total with a Li compound, and calcining the mixture to obtain a lithium-containing composite oxide composed of single particles; a washing step of washing the lithium-containing composite oxide with water and dehydrating it to obtain a cake-like composition; a drying step of drying the cake-like composition to obtain a powder-like composition; and an addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition or the powder-like composition.
11. A non-aqueous electrolyte secondary battery comprising a positive electrode containing the positive electrode active material for non-aqueous electrolyte secondary batteries according to any one of claims 1 to 9, a negative electrode, and a non-aqueous electrolyte.
Citation Information
Patent Citations
Positive electrode active material for secondary battery and secondary battery containing the same
JP2018532236A
Lithium-ion battery positive electrode material, lithium-ion battery, communication device, power device, energy storage device and portable storage device using the same, and use of lithium-ion battery
JP6850949B2
Nickel-cobalt-manganese ternary cathode material precursor for lithium battery and preparation method thereof, and cathode material prepared from nickel-cobalt-manganese ternary cathode material precursor
CN109721109A
Nonaqueous secondary battery
JP2009110943A
Ionic conductive material, core-shell structure containing the same, as well as, electrode formed therewith and metal ion battery