Catalyst liquid and method for producing catalyst liquid

The catalyst liquid, featuring a metal oxo complex and specific transition metal chlorides, addresses the issue of poor demoldability and filling in metathesis reactions, offering enhanced stability and productivity by incorporating norbornene and controlled MoOCl/WOCl amounts, resulting in improved handling and catalytic performance.

WO2024225066A1PCT designated stage expired Publication Date: 2024-10-31RIMTEC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014725
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-11
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing catalyst liquids for metathesis reactions have insufficient demoldability and filling properties, hindering productivity in polymerizable compositions.

Method used

A catalyst liquid containing a metal oxo complex represented by the general formula [M(A(R¹R²R³)] and MoOCl₄ or WOCl₄, with specific amounts of MoOCl₄ or WOCl₄, and a norbornene monomer, produced through a method involving reactions in an aliphatic solvent, enhancing stability and handling properties.

Benefits of technology

The catalyst liquid provides polymerizable compositions with excellent demoldability and filling properties, improving handling and catalytic efficiency without the need for recrystallization steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014725_31102024_PF_FP_ABST
    Figure JP2024014725_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a catalyst liquid which contains a metal oxo complex represented by general formula (1) and MoOCl4 and / or WOCl4, wherein the total content of MoOCl4 and WOCl4 is 0.5-20 parts by weight relative to 100 parts by weight of the metal oxo complex. (In general formula (1), M represents a molybdenum atom or a tungsten atom; A represents a carbon atom, a silicon atom, a germanium atom, a tin atom or a lead atom; R1 to R5 each independently represent a hydrogen atom, an optionally substituted linear or branched alkyl group having 1 to 20 carbon atoms, or an optionally substituted aryl group having 6 to 20 carbon atoms; and R1 to R3 may combine with each other to form a ring.)
Need to check novelty before this filing date? Find Prior Art

Description

Catalyst solution and method for producing catalyst solution

[0001] The present invention relates to a catalyst liquid and a method for producing a catalyst liquid, and more particularly to a catalyst liquid that provides a polymerizable composition that is excellent in demoldability and packing properties, and a method for producing such a catalyst liquid.

[0002] Transition metal carbene complexes, such as ruthenium carbene complexes known as Grubbs' catalysts and molybdenum and tungsten carbene complexes known as Schrock's catalysts, are known as highly active catalysts for metathesis reactions (hereinafter sometimes referred to as "metathesis catalysts") and are widely used.

[0003] Among transition metal carbene complexes, molybdenum carbene complexes and tungsten carbene complexes have extremely high activity as metathesis catalysts, and as disclosed in, for example, Patent Document 1, by appropriately selecting the substituents and ligands on the metal, the metathesis reaction can proceed stereospecifically. Therefore, various studies have been conducted on molybdenum carbene complexes and tungsten carbene complexes.

[0004] For example, Patent Document 1 discloses a method for forming a compound having a molybdenum atom or a tungsten atom with -OA(R 1 R 2 R 3 A represents a carbon atom, a silicon atom, a germanium atom, a tin atom, or a lead atom; R 1 ~R 3 each independently represents a hydrogen atom, an optionally substituted linear or branched alkyl group having 1 to 20 carbon atoms, or an optionally substituted aryl group having 6 to 20 carbon atoms; R 1 ~R 3 may be bonded to each other to form a ring.) and a β-diketone are coordinated. In the technology of Patent Document 1, the metal oxo complex is obtained by isolating it through a recrystallization step, and the isolated metal oxo complex is then dissolved in a solvent to obtain a catalyst solution.

[0005] International Publication No. 2020 / 085306

[0006] However, the technology of Patent Document 1 does not provide sufficient demoldability when a polymerizable composition is produced, and therefore, improvement is desired from the viewpoint of productivity. The present invention has been made in view of such circumstances, and an object of the present invention is to provide a catalyst liquid that provides a polymerizable composition that is excellent in demoldability and filling property.

[0007] The present inventors have conducted research to achieve the above object, and have found that a molybdenum atom or a tungsten atom has a -OA(R 1 R 2 R 3 A represents a carbon atom, a silicon atom, a germanium atom, a tin atom, or a lead atom; R 1 ~R 3 each independently represents a hydrogen atom, an optionally substituted linear or branched alkyl group having 1 to 20 carbon atoms, or an optionally substituted aryl group having 6 to 20 carbon atoms; R 1 ~R 3 may be bonded to each other to form a ring.) and a β-diketone are coordinated with a metal oxo complex. 4 and / or WOCl 4 The present inventors have found that the above object can be achieved by using a catalyst solution containing the above compound, and have thus completed the present invention.

[0008] That is, the present invention provides the following inventions: [1] A metal oxo complex represented by the following general formula (1) and MoOCl 4 and / or WOCl 4 A catalyst solution containing MoOCl relative to 100 parts by weight of the metal oxo complex. 4 and WOCl 4 The total content of the catalyst solution is 0.5 to 20 parts by weight. [In the above general formula (1), M represents a molybdenum atom or a tungsten atom, A represents a carbon atom, a silicon atom, a germanium atom, a tin atom, or a lead atom, and R 1 ~R 5each independently represents a hydrogen atom, an optionally substituted linear or branched alkyl group having 1 to 20 carbon atoms, or an optionally substituted aryl group having 6 to 20 carbon atoms; R 1 ~R 3 may be bonded to each other to form a ring.] [2] The catalyst solution according to [1], further containing a norbornene-based monomer. [3] The catalyst solution according to [1] or [2], wherein A in the general formula (1) is a carbon atom or a silicon atom. [4] In the general formula (1), R 4 and R 5 [5] In the general formula (1), R 1 , R 2 [6] A method for producing the catalyst solution according to any one of [1] to [5], comprising: reacting MoCl in an aliphatic solvent with MoCl 6 and / or WCl 6 is reacted with a ketone compound to give MoOCl 4 and / or WOCl 4 a first step of obtaining a solution containing MoOCl obtained in the first step; 4 and / or WOCl 4 a second step of reacting a compound represented by the following general formula (2) with a solution containing the compound represented by the following general formula (3) to obtain a solution containing the compound represented by the following general formula (3); and a second step of reacting a compound represented by the following general formula (4) with the solution containing the compound represented by the general formula (3) obtained in the second step to obtain a metal oxo complex represented by the general formula (1) and MoOCl 4 and / or WOCl 4 and a third step of obtaining a catalyst solution containing the catalyst. [In the above general formulas (2) to (4), A represents a carbon atom, a silicon atom, a germanium atom, a tin atom, or a lead atom; R 1 ~R 5each independently represents a hydrogen atom, an optionally substituted linear or branched alkyl group having 1 to 20 carbon atoms, or an optionally substituted aryl group having 6 to 20 carbon atoms; R 1 ~R 3 may be bonded to each other to form a ring.

[0009] According to the present invention, it is possible to provide a catalyst solution that gives a polymerizable composition that is excellent in demoldability and filling properties, and a manufacturing method for obtaining such a catalyst solution.

[0010] FIG. 1 shows the results of NMR measurement in Example 1.

[0011] <Catalyst Solution> The catalyst solution of the present invention comprises a metal oxo complex represented by the following general formula (1) and MoOCl 4 and / or WOCl 4 Contains:

[0012] In the general formula (1), M represents a molybdenum atom or a tungsten atom, A represents a carbon atom, a silicon atom, a germanium atom, a tin atom, or a lead atom, and R 1 ~R 5 each independently represents a hydrogen atom, an optionally substituted linear or branched alkyl group having 1 to 20 carbon atoms, or an optionally substituted aryl group having 6 to 20 carbon atoms; R 1 ~R 3 may be bonded to each other to form a ring.

[0013] In the general formula (1), M represents a molybdenum atom or a tungsten atom, which is the central metal of the complex. The central metal of the metal oxo complex used in the present invention may be either a molybdenum atom or a tungsten atom, but a tungsten atom is preferred from the viewpoint of superior catalytic activity.

[0014] The compound represented by the general formula (1) is -OA(R 1 R 2 R 3 The metal oxo complex used in the present invention has a group represented by —OA(R 1 R 2R 3 ) and a β-diketone are coordinated, which is presumably why the metal oxo complex used in the present invention exhibits excellent stability in air. Therefore, the metal oxo complex used in the present invention has excellent handleability.

[0015] In the above general formula (1), A represents a carbon atom, a silicon atom, a germanium atom, a tin atom, or a lead atom, and is preferably a carbon atom or a silicon atom, more preferably a carbon atom, from the viewpoint of further enhancing the stability of the metal oxo complex in air.

[0016] Also, -OA(R 1 R 2 R 3 ) R 1 ~R 3 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 20 carbon atoms which may have a substituent. 1 ~R 3 may be bonded to each other to form a ring. Specific examples of the optionally substituted linear or branched alkyl group having 1 to 20 carbon atoms include, but are not limited to, a methyl group, an ethyl group, an isopropyl group, a t-butyl group, an n-butyl group, a 2,2-dimethylpropyl group, and a 2-methyl-2-phenylethyl group. Specific examples of the optionally substituted aryl group having 6 to 20 carbon atoms include, but are not limited to, a phenyl group, a 4-methylphenyl group, a 2,6-dimethylphenyl group, a 2,6-diisopropylphenyl group, and a mesityl group. R 1 ~R 3 The groups represented by the formula (I) may be the same or different from each other.

[0017] Also, R 1 ~R 3 may be bonded to each other to form a ring, in which case, -OA(R 1 R 2 R 3 ) constituting a group represented by -A(R 1 R 2 R3 ) (wherein A is a carbon atom) include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, a cyclodecyl group, a cycloundecyl group, a cyclododecyl group, a norbornyl group, a bornyl group, an isobornyl group, a decahydronaphthyl group, a tricyclodecanyl group, and an adamantyl group. These groups may have a substituent, and among these, a substituted cyclohexyl group is preferred. Examples of the substituent include a methyl group, an ethyl group, an isopropyl group, a t-butyl group, an n-butyl group, a 2,2-dimethylpropyl group, and a phenyl group. Among these, a methyl group and an isopropyl group are preferred.

[0018] In the compound represented by the general formula (1), R 4 , R 5 is a group that binds to the β-diketone structure as a ligand, and R 4 , R 5 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 20 carbon atoms which may have a substituent. Specific examples of the linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent include, but are not limited to, a methyl group, an ethyl group, an isopropyl group, a t-butyl group, an n-butyl group, a 2,2-dimethylpropyl group, and a 2-methyl-2-phenylethyl group. Specific examples of the aryl group having 6 to 20 carbon atoms which may have a substituent include, but are not limited to, a phenyl group, a 4-methylphenyl group, a 2,6-dimethylphenyl group, a 2,6-diisopropylphenyl group, and a mesityl group. R 4 , R 5 The groups represented by the formula (I) may be the same or different from each other.

[0019] In the metal oxo complex used in the present invention, from the viewpoint of further increasing the solubility in the monomer used to obtain the polymer, R 4 , R 5At least one of R is preferably a methyl group or a t-butyl group. In particular, from the viewpoint of further increasing the solubility in the monomer used to obtain the polymer, R 4 , R 5 are both methyl groups, or R 4 , R 5 More preferably, both of the groups are t-butyl groups.

[0020] In the metal-oxo complex of the present invention, among the compounds represented by the above general formula (1), compounds represented by the following formulas (5) to (15) are preferred, compounds represented by the following formulas (5), (7), (8), (9), (10), (11), (14), and (15) are more preferred, compounds represented by the following formulas (14) and (15) are more preferred, and compounds represented by the following formula (15) are even more preferred.

[0021] The catalyst solution of the present invention contains, in addition to the metal oxo complex represented by the general formula (1), MoOCl 4 and / or WOCl 4 In the catalyst solution of the present invention, MoOCl 4 and / or WOCl 4 The content of MoOCl is 100 parts by weight of the metal oxo complex represented by the general formula (1). 4 and WOCl 4 The total content is 0.5 to 20 parts by weight, preferably 1 to 15 parts by weight, and more preferably 2.5 to 12 parts by weight.

[0022] According to the present invention, the specific amount of MoOCl is added to the metal oxo complex represented by the general formula (1). 4 and / or WOCl 4 By incorporating MoOCl into a catalyst solution, it is possible to obtain not only the excellent stability in air that the metal oxo complex represented by the general formula (1) has, but also excellent demoldability and packing properties when blended into a polymerizable composition. 4 and WOCl 4 If the total content of MoOCl is too small, the demoldability will be insufficient. 4and WOCl 4 If the total content is too high, the catalytic activity will decrease.

[0023] The catalyst solution of the present invention is MoOCl 4 and WOCl 4 The metal oxo complex represented by the general formula (1) may contain either one of these or both of these. However, when the M atom of the metal oxo complex represented by the general formula (1) is a molybdenum atom, MoOCl 4 When the M atom of the metal oxo complex represented by the general formula (1) is a tungsten atom, WOC1 4 It is preferable that the composition contains the following:

[0024] In addition, the specific amount of MoOCl 4 and / or WOCl 4 The method for incorporating MoOCl into the metal oxo complex is not particularly limited. Method (A): Isolating a metal oxo complex represented by the general formula (1) by synthesis, and then adding MoOCl to the isolated metal oxo complex represented by the general formula (1). 4 and / or WOCl 4 Alternatively, method (B): as in the method for producing a catalyst solution of the present invention described below, a method of mixing MoOCl generated in the synthesis process when synthesizing a metal oxo complex represented by the general formula (1) may be used. 4 and / or WOCl 4 By leaving the metal oxo complex represented by the general formula (1) and MoOCl 4 and / or WOCl 4 It may also contain the following.

[0025] <Method for Producing Catalyst Solution> Hereinafter, the method for producing a catalyst solution of the present invention, which is the method for producing a catalyst solution according to the above method (B), will be described. The method for producing a catalyst solution of the present invention comprises: 6 and / or WCl 6 is reacted with a ketone compound to give MoOCl 4 and / or WOCl 4a first step of obtaining a solution containing MoOCl obtained in the first step; 4 and / or WOCl 4 a second step of reacting a compound represented by the following general formula (2) with a solution containing the compound represented by the following general formula (3) to obtain a solution containing the compound represented by the following general formula (3); and a second step of reacting a compound represented by the following general formula (4) with the solution containing the compound represented by the general formula (3) obtained in the second step to obtain a metal oxo complex represented by the general formula (1) and MoOCl 4 and / or WOCl 4 and a third step of obtaining a catalyst solution containing the above.

[0026] (First Step) First, in the first step, MoCl 6 and / or WCl 6 is reacted with a ketone compound (monoketone compound) to obtain MoOCl 4 and / or WOCl 4 A solution containing

[0027] The aliphatic solvent is not particularly limited as long as it does not inhibit the reaction, and examples thereof include linear or branched aliphatic hydrocarbons such as propane, n-butane, isobutane, n-pentane, isopentane, n-hexane, propene, 1-butene, isobutene, trans-2-butene, cis-2-butene, 1-pentene, 2-pentene, 1-hexene, 2-hexene, and n-heptane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; and ether compounds such as tetrahydrofuran and diethyl ether. Of these, linear or branched aliphatic hydrocarbons are preferred, and n-hexane is preferred.

[0028] The ketone compound (monoketone compound) is not particularly limited, but examples thereof include acetone, methyl ethyl ketone, diethyl ketone, diisopropyl ketone, methyl isobutyl ketone, methyl hexyl ketone, diisobutyl ketone, butyl aldehyde, propyl acetate, butyl acetate, amyl acetate, etc. Among these, acetone is preferred.

[0029] In the first step, MoCl 6 and / or WCl 6 When reacting with a ketone compound, a method of mixing them in an aliphatic solvent is exemplified. The reaction temperature is not particularly limited, but is preferably 0 to 100°C, more preferably 25 to 65°C. The reaction time is not particularly limited, but is preferably 1 to 48 hours, more preferably 2 to 24 hours. The reaction atmosphere is preferably an inert gas atmosphere.

[0030] In addition, MoCl in the first step 6 and / or WCl 6 The amount of the ketone compound used is not particularly limited, but may be any of "MoCl 6 and WCl 6 The molar amount of the total of the above: the molar amount of the ketone compound is preferably 1:1 to 1:1.05, more preferably 1:1 to 1:1.03, and even more preferably 1:1 to 1:1.01.

[0031] (Second Step) In the second step, MoOCl obtained in the first step is 4 and / or WOCl 4 A solution containing a compound represented by the following general formula (3) is obtained by reacting a compound represented by the following general formula (2) with a solution containing the above.

[0032] In the above general formulas (2) and (3), R 4 , R 5 each independently represents a hydrogen atom, an optionally substituted linear or branched alkyl group having 1 to 20 carbon atoms, or an optionally substituted aryl group having 6 to 20 carbon atoms, specific examples of which are the same as those in general formula (1) above.

[0033] In the second step, the MoOCl obtained in the first step is 4 and / or WOCl 4 The method for reacting the compound represented by the general formula (2) with the solution containing the compound represented by the general formula (2) is not particularly limited. 4 and / or WOCl 4and a method in which the compound represented by the general formula (2) is added to a solution containing the compound represented by the general formula (2) and then mixed. The reaction temperature is not particularly limited, but is preferably 0 to 100°C, more preferably 25 to 65°C, and the reaction time is not particularly limited, but is preferably 1 to 48 hours, more preferably 2 to 24 hours. The reaction atmosphere is preferably an inert gas atmosphere.

[0034] In the second step, MoOCl 4 and / or WOCl 4 and the compound represented by the general formula (2) are reacted. In the production method of the present invention, the MoOCl 4 and / or WOCl 4 Of these, MoOCl that remains without reacting with the compound represented by the general formula (2) 4 and / or WOCl 4 The amount of MoOCl in the final catalyst solution 4 and / or WOCl 4 The amount is:

[0035] Therefore, in the second step, MoOCl 4 and / or WOCl 4 and the reaction rate of the compound represented by the general formula (2) are taken into consideration, and the MoOCl 4 and / or WOCl 4 MoOCl 4 and / or WOCl 4 The amount of the compound represented by the general formula (2) to be added relative to the amount of MoOCl obtained in the first step can be determined. 4 and / or WOCl 4 MoOCl contained in a solution containing 4 and / or WOCl 4 the molar amount of the compound represented by the general formula (2) above is preferably 1:1 to 1:1.05, more preferably 1:1 to 1:1.03, and even more preferably 1:1 to 1:1.01.

[0036] (Third Step) In the third step, a compound represented by the following general formula (4) is reacted with the solution containing the compound represented by the general formula (3) obtained in the second step to obtain a metal oxo complex represented by the general formula (1) and MoOCl 4 and / or WOCl 4 A catalyst solution containing the above is obtained.

[0037] In the general formula (4), A represents a carbon atom, a silicon atom, a germanium atom, a tin atom, or a lead atom; 1 ~R 3 each independently represents a hydrogen atom, an optionally substituted linear or branched alkyl group having 1 to 20 carbon atoms, or an optionally substituted aryl group having 6 to 20 carbon atoms; R 1 ~R 3 In the above general formula (4), A and R may be bonded to each other to form a ring. 1 ~R 3 Specific examples of are the same as those of the general formula (1).

[0038] In the third step, the method for reacting the compound represented by general formula (4) with the solution containing the compound represented by general formula (3) obtained in the second step is not particularly limited, but examples include a method in which the compound represented by general formula (4) is added to the solution containing the compound represented by general formula (3) obtained in the second step and then mixed. The reaction temperature is not particularly limited, but is preferably 0 to 100°C, more preferably 25 to 60°C, and the reaction time is not particularly limited, but is preferably 1 to 48 hours, more preferably 2 to 24 hours. Furthermore, the reaction atmosphere is preferably an inert gas atmosphere.

[0039] The amount of the compound represented by the general formula (4) used in the third step is not particularly limited, but is preferably 1:1 to 1:1.05, more preferably 1:1 to 1:1.03, and even more preferably 1:1 to 1:1.01, in terms of "molar amount of the compound represented by the general formula (3) obtained in the second step:molar amount of the compound represented by the general formula (4)."

[0040] In the production method of the present invention, the metal oxo complex represented by the general formula (1) obtained in the third step is reacted with MoOCl 4 and / or WOCl 4 The catalyst solution of the present invention can be obtained by distilling off volatile components such as the aliphatic solvent from the solution containing the above. In addition, the solvent may be washed as needed.

[0041] According to the production method of the present invention, there is no need to perform a step of isolating the metal oxo complex represented by the general formula (1) by recrystallization or the like. 4 and / or WOCl 4 By controlling the amount of the compound represented by the general formula (2) used to react with MoOCl in the finally obtained catalyst solution, 4 and / or WOCl 4 The amount of can be suitably controlled within the above-mentioned range, and thereby a catalyst solution that gives a polymerizable composition excellent in demoldability and packing property can be obtained with high production efficiency without requiring an isolation step such as recrystallization.

[0042] However, in the present invention, any method other than the above may be employed as long as it is a method capable of producing the catalyst solution of the present invention. For example, a method for producing the catalyst solution of the present invention by reacting the metal oxo complex represented by the general formula (1) obtained in the third step with MoOCl 4 and / or WOCl 4 The solution containing the compound (I) is subjected to distillation to remove volatile components such as aliphatic solvents, followed by recrystallization to isolate the metal oxo complex represented by the general formula (1). 4 and / or WOCl 4 and mixing may be employed.

[0043] <Application as a Metathesis Catalyst Precursor> The catalyst solution of the present invention contains a metal-oxo complex represented by the general formula (1) above, and is therefore suitable for use as a metathesis catalyst precursor. When the catalyst solution of the present invention is used as a metathesis catalyst precursor, it is typically activated by contacting it with an organometallic compound typically used in metathesis polymerization catalysts, and then used in the activated state for a metathesis polymerization reaction. That is, the catalyst solution of the present invention can be produced by contacting the metal-oxo complex represented by the general formula (1) contained in the catalyst solution of the present invention with an organometallic compound, thereby reacting the metal-oxo complex represented by the general formula (1) with the organometallic compound to form a metathesis polymerization catalyst. In this case, the catalyst solution of the present invention contains the predetermined amount of MoOCl 4 and / or WOCl 4 Since it contains MoOCl 4 and / or WOCl 4 By virtue of this action, when a polymerizable monomer is further added to form a polymerizable composition, it is possible to obtain a polymerizable composition having excellent demolding properties and filling properties.

[0044] Examples of organometallic compounds that can be used as activators include organometallic compounds of metals in Groups 11 to 14 of the Periodic Table. Specific examples include alkylaluminum compounds such as triethylaluminum, triisobutylaluminum, trimethylaluminum, tributylaluminum, trihexylaluminum, and trioctylaluminum; alkylaluminum halide compounds such as ethylaluminum dichloride, diethylaluminum chloride, diisobutylaluminum chloride, ethylaluminum sesquichloride, isobutylaluminum dichloride, and dioctylaluminum iodide; alkylaluminum alkoxide compounds such as diethylaluminum ethoxide; organotin compounds such as tetrabutyltin; organozinc compounds such as diethylzinc; and organomagnesium compounds such as isopropylmagnesium chloride. Among these, alkylaluminum compounds and alkylaluminum halide compounds are preferred, with triethylaluminum, trioctylaluminum, diethylaluminum chloride, and dioctylaluminum iodide being more preferred, and triethylaluminum and diethylaluminum chloride being even more preferred. The organometallic compounds that can be used as activators can be used alone or in combination of two or more.

[0045] When the catalyst solution of the present invention is used as a metathesis catalyst precursor, a norbornene-based monomer can be suitably used as the polymerizable monomer. In this case, it is preferable that the catalyst solution of the present invention contains a norbornene-based monomer in advance. That is, the catalyst solution of the present invention is prepared by mixing a metal oxo complex represented by the general formula (1) and MoOCl 4 and / or WOCl 4and a norbornene-based monomer. The content of the norbornene-based monomer in the catalyst solution of the present invention is preferably 100 to 2,000 parts by weight, more preferably 400 to 1,600 parts by weight, and even more preferably 700 to 1,200 parts by weight, relative to 100 parts by weight of the metal-oxo complex represented by the general formula (1) above. By setting the content of the norbornene-based monomer within the above range, the viscosity of the catalyst solution of the present invention can be set within an appropriate range, and handleability and productivity can be improved.

[0046] The norbornene-based monomer is not particularly limited as long as it is a compound having a norbornene structure, and specific examples thereof include dicyclopentadienes such as dicyclopentadiene and methyldicyclopentadiene; tetracyclo[6.2.1.1] 3,6 .0 2,7 ] dodec-4-ene, 9-ethylidenetetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-phenyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-9-ene-4-carboxylic acid, tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-9-ene-4,5-dicarboxylic anhydride and other tetracyclododecenes; 2-norbornene, 5-ethylidene-2-norbornene, 5-vinyl-2-norbornene, 5-phenyl-2-norbornene, 5-norbornene-2-yl acrylate, 5-norbornene-2-yl methacrylate, 5-norbornene-2-carboxylic acid, 5-norbornene-2,3-dicarboxylic acid, 5-norbornene-2,3-dicarboxylic acid anhydride and other norbornenes; 7-oxa-2-norbornene, 5-ethylidene-7-oxa-2-norbornene and other oxanorbornenes; tetracyclo[9.2.1.0 2,10 .0 3,8]tetradeca-3,5,7,12-tetraene (also known as 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene), pentacyclo[6.5.1.1 3,6 .0 2,7 .0 9,13 ] pentadeca-4,10-diene, pentacyclo[9.2.1.0 2,10 .0 3,8 ] Examples include tetracyclic or higher ring olefins such as pentadeca-5,12-diene and tricyclopentadiene.

[0047] The metathesis polymerization reaction using the catalyst solution of the present invention may be carried out in a solvent or without a solvent. For example, the catalyst solution of the present invention may be used in a mixture of a metal oxo complex represented by the general formula (1) and MoOCl 4 and / or WOCl 4 and a norbornene-based monomer, it is possible to carry out a polymerization reaction without a solvent, such as bulk polymerization.

[0048] The present invention will be described below based on examples, but the present invention is not limited to these examples. Note that "parts" and "%" are by mass unless otherwise specified.

[0049] Example 1 Preparation of Catalyst Solution In a reaction vessel equipped with a stirrer, 488.79 g of hexane and tungsten (VI) chloride (WCl 6140 g (353.05 mmol) of acetylacetone was added to the reaction vessel over a period of 27 minutes, and the mixture was stirred for 1 hour. The temperature of the reaction vessel was then adjusted to 55°C, and 41.01 g (353.05 mmol) of acetone was added continuously over 27 minutes under a nitrogen atmosphere. After the addition of acetone was completed, the temperature of the reaction vessel was maintained at 55°C, and the mixture was stirred for 5 hours. Next, while maintaining the temperature of the reaction vessel at 55°C, 70.70 g (353.05 mmol) of acetylacetone was added continuously over 32 minutes under a nitrogen atmosphere. After the addition of acetylacetone was completed, the temperature of the reaction vessel was maintained at 55°C, and the mixture was stirred for 18 hours. Next, under a nitrogen atmosphere, 110.34 g (353.05 mmol) of L-menthol (2-isopropyl-5-methylcyclohexanol) was added continuously over 36 minutes, and after the addition of L-menthol was completed, the temperature of the reaction vessel was maintained at 55°C, and the mixture was stirred for 26 hours. Next, the resulting reaction liquid was subjected to a distillation operation to remove volatile components including hexane, thereby obtaining a yellowish-brown viscous substance.

[0050] A portion of the resulting viscous substance was then added to hexane to form a hexane suspension. The hexane suspension was then centrifuged to precipitate the insoluble matter, and the supernatant yellow-brown solution was removed. The removed supernatant yellow-brown solution was allowed to stand at room temperature overnight to obtain yellow-brown needle-like crystals. NMR analysis confirmed that the resulting needle-like crystals were the compound represented by formula (15). The NMR analysis results are shown in Figure 1.

[0051] Furthermore, the yellowish-brown viscous substance obtained was 183 When W-NMR measurement was performed, it was found that the ratio of WOC1 to 100 parts of the compound represented by formula (15) in the viscous material was 4 The content was 8.4 parts.

[0052] Next, 99.17 parts of a norbornene-based monomer mixture (RIM-M) consisting of 90% dicyclopentadiene and 10% tricyclopentadiene was added to 0.83 parts of the compound represented by formula (15) in the resulting yellow-brown viscous substance to obtain a catalyst solution. The resulting catalyst solution was stirred for 10 minutes, and then the viscosity of the catalyst solution was measured using a Brookfield viscometer and found to be 2900 mPa s.

[0053] (Preparation of activator solution A) In a reaction vessel under a nitrogen atmosphere, triethylaluminum was added to and mixed with dipropylene glycol dimethyl ether, and the triethylaluminum was dissolved in a norbornene-based monomer mixture (RIM-M) consisting of 90% dicyclopentadiene and 10% tricyclopentadiene so that the triethylaluminum concentration was 0.13%, thereby obtaining activator solution A.

[0054] (Preparation of reaction stock solution B) In a reaction vessel under a nitrogen atmosphere, the catalyst solution obtained above was added to a norbornene-based monomer mixture (RIM-M) consisting of 90% dicyclopentadiene and 10% tricyclopentadiene so that the amount of tungsten was 3.5 mmol / kg, and mixed to obtain reaction stock solution B. In preparing reaction stock solution B, the catalyst solution obtained above was stored under a nitrogen atmosphere for 3 days before use.

[0055] (Polymer Production) A 50 mL container purged with nitrogen was placed under conditions of 30°C. 20 g of the reaction stock solution B prepared above was injected into the container using a glass syringe while the container had been previously purged with nitrogen and kept at 30°C, and then stirred with a stirrer. Next, 0.2 g of the activator solution A prepared above was injected using a glass syringe and mixed for 10 seconds. As the polymerization reaction progressed, the mixture transitioned to a gel state, followed by the generation of white smoke. In this example, the time from the start of mixing of the activator solution A and the reaction stock solution B until the transition to the gel state was defined as the "gelation time," and the time until the generation of white smoke was defined as the "curing time." In Example 1, the gelation time was 15 seconds, and the curing time was 70 seconds. The reaction yielded dicyclopentadiene and tricyclopentadiene polymers. The polymerization was carried out in a manner that would allow the formation of thin-plate polymer portions for evaluation of demoldability.

[0056] The resulting polymer was evaluated for demoldability and filling property according to the following methods. The results are shown in Table 1. (Mold demoldability) Of the resulting polymer, the thin plate-like polymer portion used for demoldability evaluation was subjected to hardness measurement by measuring the demolding time, and the evaluation was based on the following criteria. ◯: Demolding time of A4 size within 5 seconds ×: Demolding time of A4 size more than 5 seconds (Filling property) The filling property of the resulting polymer was evaluated by checking for the presence or absence of unfilled portions, and the evaluation was based on the following criteria. ◯: Filled with no missing portions on the A4 size plate ×: Not filled with missing portions on the A4 size plate

[0057] Example 2 Hexane was added to a portion of the viscous substance obtained in Example 1 to prepare a hexane suspension, and the hexane suspension was then centrifuged to precipitate insoluble matter. The supernatant yellow-brown solution was removed, and the removed supernatant yellow-brown solution was allowed to stand at room temperature overnight to isolate the compound represented by formula (15) as yellow needle-like crystals. 183 W-NMR measurement revealed that WOCl 4Then, under a nitrogen atmosphere, 5 parts of the isolated compound represented by formula (15) and WOC1 were placed in a glass vial. 4 0.15 parts (WOC1 relative to 100 parts of the compound represented by formula (15) 4 (3 parts) was added, and then, while stirring, 45 parts of a norbornene-based monomer mixture (RIM-M) consisting of 90% dicyclopentadiene and 10% tricyclopentadiene was added using a glass syringe to obtain a catalyst solution. The obtained catalyst solution was stirred for 10 minutes, and then the viscosity of the catalyst solution was measured using a Brookfield viscometer, and was found to be 34.6 mPa s.

[0058] Then, a reaction stock solution B was prepared in the same manner as in Example 1, except that the catalyst solution obtained above was used, and a polymer was obtained using the activator solution A obtained in the same manner as in Example 1, and the polymer was evaluated in the same manner. The results are shown in Table 1.

[0059] (Example 3) In the same manner as in Example 2, a compound represented by formula (15) was isolated as yellow needle-like crystals using a portion of the viscous substance obtained in Example 1. The obtained needle-like crystals were 183 W-NMR measurement revealed that WOCl 4 Then, under a nitrogen atmosphere, 4.95 parts of the isolated compound represented by formula (15) and WOC1 4 0.5 parts (WOC1 relative to 100 parts of the compound represented by formula (15) 4 (10.1 parts) of cyclopentadiene (a mixture of 90% dicyclopentadiene and 10% tricyclopentadiene) was added thereto with a glass syringe while stirring, to obtain a catalyst solution. The obtained catalyst solution was stirred for 10 minutes, and then the viscosity of the catalyst solution was measured using a Brookfield viscometer and found to be 3,840 mPa s.

[0060] Then, a reaction stock solution B was prepared in the same manner as in Example 1, except that the catalyst solution obtained above was used, and a polymer was obtained using the activator solution A obtained in the same manner as in Example 1, and the polymer was evaluated in the same manner. The results are shown in Table 1.

[0061] Comparative Example 1 In the same manner as in Example 2, a compound represented by formula (15) was isolated as yellow needle-like crystals using a portion of the viscous substance obtained in Example 1. The obtained needle-like crystals were 183 W-NMR measurement revealed that WOCl 4 The presence of WOC1 was not confirmed. Then, under a nitrogen atmosphere, 2 parts of the isolated compound represented by formula (15) was added to a glass vial, and while stirring, 100 parts of a norbornene-based monomer mixture (RIM-M) consisting of 90% dicyclopentadiene and 10% tricyclopentadiene was added using a glass syringe to obtain a catalyst solution. That is, in Comparative Example 1, the catalyst solution contained WOC1 4 was not included.

[0062] Then, a reaction stock solution B was prepared in the same manner as in Example 1, except that the catalyst solution obtained above was used, and a polymer was obtained using the activator solution A obtained in the same manner as in Example 1, and the polymer was evaluated in the same manner. The results are shown in Table 1.

[0063]

[0064] As is clear from the results in Table 1, the amount of MoOCl per 100 parts by weight of the metal oxo complex represented by the general formula (1) is 4 and / or WOCl 4 It has been confirmed that a catalyst solution containing 0.5 to 20 parts by weight of the above can provide a polymerizable composition having excellent demolding properties and filling properties.

Claims

1. A metal oxo complex represented by the following general formula (1) and MoOCl 4 and / or WOCl 4 A catalyst solution containing MoOCl relative to 100 parts by weight of the metal oxo complex. 4 and WOCl 4 The catalyst solution has a total content of 0.5 to 20 parts by weight. [In the above general formula (1), M represents a molybdenum atom or a tungsten atom, A represents a carbon atom, a silicon atom, a germanium atom, a tin atom or a lead atom, R 1 ~R 5 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 20 carbon atoms which may have a substituent; R 1 ~R 3 may be bonded to each other to form a ring.

2. The catalyst solution according to claim 1, further comprising a norbornene-based monomer.

3. The catalyst solution according to claim 1 or 2, wherein in said general formula (1), A is a carbon atom or a silicon atom.

4. In the general formula (1), R 4 and R 5 4. The catalyst liquid according to claim 1, wherein at least one of the groups is a methyl group or a t-butyl group.

5. In the general formula (1), R 1 , R 2 The catalyst solution according to any one of claims 1 to 4, wherein each of the groups is a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, and which is bonded to each other to form a ring.

6. A method for producing the catalyst solution according to any one of claims 1 to 5, comprising the steps of: 6 and / or WCl 6 is reacted with a ketone compound to give MoOCl 4 and / or WOCl 4 A first step of obtaining a solution containing MoOCl obtained in the first step; 4 and / or WOCl 4 A second step of reacting a compound represented by the following general formula (2) with a solution containing the compound represented by the following general formula (3) to obtain a solution containing the compound represented by the following general formula (3); and a second step of reacting a compound represented by the following general formula (4) with the solution containing the compound represented by the general formula (3) obtained in the second step to obtain a metal oxo complex represented by the general formula (1) and MoOCl. 4 and / or WOCl 4 and a third step of obtaining a catalyst solution containing the catalyst. [In the above general formulas (2) to (4), A represents a carbon atom, a silicon atom, a germanium atom, a tin atom, or a lead atom; R 1 ~R 5 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 20 carbon atoms which may have a substituent; R 1 ~R 3 may be bonded to each other to form a ring.

Citation Information

Patent Citations

  • Molybdenum oxoalkylidene compounds, methods for making them, and their use in metathesis reactions

    JP2021512915A

  • Ring-opening metathesis polymerization (ROMP) of cyclo-olefins with molybdenum catalysts

    US20020111446A1

  • Metal-oxo complex and method for production thereof

    WO2020085306A1