Quartz glass

Quartz glass with controlled tin content and heat treatment processes enables selective transmission of 222 nm UV light while blocking 252 nm UV light, addressing the limitations of existing technologies in sterilization and virus inactivation applications.

WO2024225186A1PCT designated stage expired Publication Date: 2024-10-31TOSOH CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015548
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-14
Filing Date
2024-04-19
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional quartz glass used with KrCl excimer lamps for sterilization and virus inactivation struggles to selectively transmit 222 nm UV light while blocking 252 nm UV light, due to the complexity of dielectric multilayer filters and limited irradiation areas, and existing tin-containing quartz glass suppresses both wavelengths.

Method used

Development of quartz glass with a tin content of 5-150 ppm and a specific extinction coefficient ratio at 252 nm to 222 nm, allowing for 222 nm transmission while suppressing 252 nm transmission, achieved through a heat treatment process involving silica and tin sources under controlled conditions.

Benefits of technology

The resulting quartz glass effectively transmits 222 nm light while minimizing the transmission of 252 nm light, enhancing the effectiveness of sterilization and virus inactivation without the need for optical filters, and maintains high transparency for 222 nm light.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-I000001
    Figure JPOXMLDOC01-APPB-I000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide at least one of: a quartz glass capable of transmitting light of 222 nm while suppressing transmission of light of 252 nm; and a method for producing the same. The quartz glass has a tin content of 5 to 150 ppm. The ratio of the absorption coefficient of the quartz glass at a wavelength of 252 nm to an absorption coefficient at a wavelength of 222 nm is 2.5 or greater.
Need to check novelty before this filing date? Find Prior Art

Description

quartz glass

[0001] The present disclosure relates to fused silica.

[0002] Ultraviolet light with a wavelength of around 222 nm (hereinafter also referred to as "222 nm UV light") has extremely little effect on living organisms, and sterilization and virus inactivation technologies using this light have attracted attention. KrCl excimer lamps, which are widely used as light sources for 222 nm UV light, emit not only 222 nm UV light but also ultraviolet light with a wavelength of around 252 nm (hereinafter also referred to as "252 nm UV light"). Since there are concerns about the effect of 252 nm UV light on living organisms, it is necessary to shield this light in order to sterilize or inactivate viruses using KrCl excimer lamps intended for living organisms.

[0003] For example, Patent Documents 1 and 2 propose sterilization devices equipped with optical filters that block 252 nm UV light. Non-Patent Document 1 discloses that tin-containing quartz glass manufactured by the CVD method or the gas flame method blocks 252 nm UV light.

[0004] Patent No. 6025756 Patent No. 6973603

[0005] Glass Physics and Chemistry, Vol. 28, No. 6, 2002, pp. 379-388.

[0006] In Patent Documents 1 and 2, HfO is deposited on a glass plate. 2 layer and SiO 2An optical filter composed of a dielectric multilayer film consisting of 33 alternating layers has been disclosed. However, manufacturing such an optical filter requires complicated processes. Furthermore, not only is it difficult to form a dielectric multilayer film on a curved surface, but the wavelength range it blocks varies depending on the irradiation angle of light from a KrCl excimer lamp (hereinafter also referred to as "excimer light"). Therefore, excimer light equipped with optical filters such as those disclosed in Patent Documents 1 and 2 has a limited irradiation area effective for sterilization and virus inactivation. Furthermore, as is clear from Figure 1 showing the absorption spectrum, the quartz glass disclosed in Non-Patent Document 1 blocks not only 252 nm UV light but also 222 nm UV light.

[0007] The present disclosure aims to provide at least one of a quartz glass that can transmit 222 nm light while suppressing the transmission of 252 nm light, and a method for manufacturing the same.

[0008] The present invention is as set forth in the claims, and the gist of the present disclosure is as follows. [1] Quartz glass having a tin content of 5 ppm or more and 150 ppm or less, and having a ratio of the absorption coefficient at a wavelength of 252 nm to the absorption coefficient at a wavelength of 222 nm of 2.5 or more. [2] Quartz glass according to [1], which has an internal linear transmittance of 70% or less for light with a wavelength of 252 nm when the thickness is 1 mm. [3] Quartz glass according to [1] or [2], which has an internal linear transmittance of 30% or more for light with a wavelength of 222 nm when the thickness is 1 mm. [4] Quartz glass according to any one of [1] to [3], which has an internal linear transmittance of 222 nm for light with a wavelength of 1 mm that is higher than the internal linear transmittance of 252 nm for light with a thickness of 1 mm. [5] Quartz glass having an absorption coefficient at a wavelength of 252 nm of 30,000 cm -1 [6] The quartz glass according to any one of [1] to [4], wherein the absorption coefficient at a wavelength of 222 nm is 200,000 cm or more. -1[7] A method for producing silica glass according to any one of [1] to [5], which is as follows: [7] A method for producing silica glass according to any one of [1] to [6], which comprises a first heat treatment step of heat treating a raw material composition containing a silica source and a tin source at 20°C or higher and 1900°C or lower under a vacuum of 10 Pa or lower, and a second heat treatment step of heat treating the raw material composition heat treated in the first heat treatment step at 1400°C or higher and 1900°C or lower under a nitrogen atmosphere. [8] A method for producing silica glass according to [7], wherein the silica source is silica powder. [9] A method for producing silica glass according to [7], wherein the silica source is silica powder obtained by hydrolyzing silicon alkoxide.

[0009] The present disclosure makes it possible to provide at least one of quartz glass and a method for manufacturing the same, which does not require an optical filter such as those shown in Patent Documents 1 and 2, and which, compared to conventional tin-containing quartz glass, can transmit 222 nm light while suppressing the transmission of 252 nm light.

[0010] The silica glass according to the present disclosure will be described below by showing an example of an embodiment. The configurations and parameters disclosed herein can be combined in any desired manner, and the upper and lower limits of the values ​​disclosed herein can be combined in any desired manner.

[0011] The silica glass of this embodiment has a tin content of 5 ppm to 150 ppm, and the ratio of the absorption coefficient at a wavelength of 252 nm to the absorption coefficient at a wavelength of 222 nm is 2.5 or greater.

[0012] The quartz glass of this embodiment has a tin content of 5 ppm to 150 ppm, which allows the transmission of 222 nm light while suppressing the transmission of 252 nm light. If the tin content is less than 5 ppm, the transmission of 252 nm light cannot be suppressed. If the tin content is more than 150 ppm, the transmission of not only 252 nm light but also 222 nm light is suppressed.

[0013] In the quartz glass of this embodiment, the tin content may be 5 ppm or more and 150 ppm or less, but from the viewpoint of further improving the balance between the suppression of transmission of light with a wavelength of 252 nm and the transmission of light with a wavelength of 222 nm, it is preferably 10 ppm or more and 120 ppm or less, more preferably 15 ppm or more and 80 ppm or less, even more preferably 15 ppm or more and 50 ppm or less, and even more preferably 15 ppm or more and 30 ppm or less. Note that ppm in this specification means ppm by mass.

[0014] In the quartz glass of this embodiment, the tin content can be measured by ICP atomic emission spectrometry using the following method. Quartz glass is crushed and dissolved in hydrofluoric acid, and then sulfuric acid is added and heated to volatilize the hydrofluoric acid, thereby obtaining a residue for measurement. The residue for measurement is then dissolved in nitric acid to obtain a sample solution. Using a general ICP atomic emission spectrometry analyzer (for example, product name: 5800 ICP-OES, manufactured by Agilent Technologies), the sample solution can be measured by inductively coupled plasma atomic emission spectrometry (ICP-AES) under the following conditions: Frequency: 27 MHz Output: 1.2 kW Observation mode: axial Detector: CCD detector Scanning mode: continuous Sample introduction: cyclone nebulizer The tin content and the content of other metal elements in the quartz glass can be determined from the obtained measured values ​​of tin and other metal elements.

[0015] In the silica glass of this embodiment, tin may be contained in any form such as ions, metal, or compounds (e.g., oxides), but oxides (e.g., SnO 2 ) is preferably contained.

[0016] In the silica glass of this embodiment, the ratio of the absorption coefficient at a wavelength of 252 nm to the absorption coefficient at a wavelength of 222 nm is 2.5 or more. From the viewpoint of further improving the balance between the suppression of transmission of 252 nm light and the transmission of 222 nm light, the silica glass of this embodiment preferably has a ratio of the absorption coefficient at a wavelength of 252 nm to the absorption coefficient at a wavelength of 222 nm of 3.0 or more, more preferably 4.0 or more. In the silica glass of this embodiment, the upper limit of the ratio of the absorption coefficient at a wavelength of 252 nm to the absorption coefficient at a wavelength of 222 nm is not particularly limited, but can be, for example, 20 or less, 10 or less, or 7.0 or less. The ratio of the absorption coefficient at a wavelength of 252 nm to the absorption coefficient at a wavelength of 222 nm may be any combination of the upper and lower limits described above. From the viewpoint of further improving the balance between the suppression of transmission of light at a wavelength of 252 nm and the transmission of light at a wavelength of 222 nm, the ratio is preferably 2.5 or more and 20 or less, more preferably 3.0 or more and 10 or less, and even more preferably 4.0 or more and 7.0 or less.

[0017] The absorption coefficient of the silica glass of this embodiment is an absorption coefficient obtained by correcting and removing the effects of light scattered by bubbles in the silica glass and light reflected at the surface (interface) of the silica glass, and can be calculated from the following formula (1). The absorption coefficient at a wavelength of 252 nm (hereinafter referred to as "α 252nm ") is calculated by dividing the absorption coefficient at a wavelength of 222 nm (hereinafter referred to as "α 222nm ") to get α 222nm α for 252nm The ratio of (hereinafter referred to as "α 252nm / α 222nm The absorption coefficient is a parameter that indicates how much light a medium absorbs when light enters it, and the higher the absorption coefficient, the less light passes through the silica glass.

[0018] -LOG(T i ) = α × d × c (1) In the above formula (1), T i represents the internal linear transmittance [%] of the quartz glass for light of wavelength W (nm), and α represents the absorption coefficient [cm-1 ], d represents the thickness [cm] of the measurement sample, and c represents the tin content [g / g] in the quartz glass.

[0019] Ti in the above formula (1) can be calculated from the following formula (2): i = 100 x T c / T M ...(2) In the above formula (2), T i represents the internal linear transmittance [%] of the quartz glass for light of wavelength W (nm), and T c represents the linear transmittance [%] of the measurement sample for light of wavelength W (nm) corrected for the effect of light scattering by bubbles, and T M represents the theoretical linear transmittance [%] of quartz glass for light of wavelength W (nm) calculated from the following formula (7).

[0020] T in the above formula (2) c can be calculated from the following formula (3): c = T x T M(790-800nm) / T (790-800nm) ...(3) In the above formula (3), T c represents the linear transmittance [%] of the measurement sample for light of wavelength W (nm) corrected for the effect of light scattering by bubbles, T represents the actual linear transmittance [%] of the measurement sample for light of wavelength W (nm), and T M(790-800nm) represents the average value [%] of the theoretical linear transmittance of quartz glass for light with wavelengths of 790 nm to 800 nm, calculated from the following formula (4), and T (790-800nm) represents the average value [%] of the measured linear transmittance of the measurement sample for light with wavelengths of 790 nm to 800 nm.

[0021] T in the above formula (3) can be obtained by measuring the actual linear transmittance [%] of the measurement sample for light of wavelength W (nm) using an ultraviolet-visible spectrophotometer under the conditions described below.

[0022] T in the above formula (3) M(790-800nm) can be calculated from the following formula (4). In the above formula (4), T M(790-800nm)represents the average value [%] of the theoretical linear transmittance of the quartz glass for light with wavelengths of 790 nm to 800 nm, and R represents the surface reflectance [-] of the quartz glass for light with wavelength i (nm) calculated from the following formula (5): Note that, as can be understood from the above formula (4), wavelength i (nm) represents each wavelength in 1 (nm) increments within the wavelength range of 790 (nm) to 800 (nm).

[0023] R in the above formula (4) can be calculated from the following formula (5): R=(1-N) 2 / (1+N) 2 ...(5) In the above formula (5), R represents the surface reflectance [-] of the quartz glass for light of wavelength i (nm), and N represents the refractive index [-] of the quartz glass for light of wavelength i (nm) calculated from the following formula (6) (Malitson's formula).

[0024] N in the above formula (5) can be calculated from the following formula (6): N 2 = 1 + a 1 ×λ 2 / (λ 2 -b 1 ) + a 2 ×λ 2 / (λ 2 -b 2 ) + a 3 ×λ 2 / (λ 2 -b 3 ) (6) In the above formula (6), N represents the refractive index [-] of the silica glass for light of wavelength i (nm), λ represents the wavelength i [nm], and a 1 or a 3 and b 1 ~b 3 are respectively a 1 =0.6961663,a 2 =0.4079426, a 3 =0.8974794,b 1 =0.0684043,b 2 =0.1162414,b 3 = 9.896161.

[0025] T in the above formula (3) (790-800nm)can be determined by measuring a measurement sample with an ultraviolet-visible spectrophotometer under the conditions described below and averaging the measured linear transmittance at each wavelength in 1 nm increments within the wavelength range of 790 nm or more and 800 nm or less.

[0026] T in the above formula (2) M can be calculated from the following equation (7): M = 100 × (1 − R) 2 ...(7) In the above formula (7), T M represents the theoretical linear transmittance [%] of the quartz glass for light of wavelength W (nm), and R represents the surface reflectance [-] of the quartz glass for light of wavelength W (nm) calculated from the following formula (8):

[0027] R in the above formula (7) can be calculated from the following formula (8): R=(1-N) 2 / (1+N) 2 ...(8) In the above formula (8), R represents the surface reflectance [-] of the quartz glass for light of wavelength W (nm), and N represents the refractive index [-] of the quartz glass for light of wavelength W (nm) calculated from the following formula (9):

[0028] N in the above formula (8) can be calculated from the following formula (9): N 2 = 1 + a 1 ×λ 2 / (λ 2 -b 1 ) + a 2 ×λ 2 / (λ 2 -b 2 ) + a 3 ×λ 2 / (λ 2 -b 3 ) (9) In the above formula (9), N represents the refractive index [-] of the silica glass for light of wavelength W (nm), λ represents the wavelength W [nm], and a 1 or a 3 and b 1 ~b 3 are respectively a 1 =0.6961663,a 2 =0.4079426, a3 =0.8974794,b 1 =0.0684043,b 2 =0.1162414,b 3 = 9.896161.

[0029] T and T in the above formula (3) (790-800nm) The following measurement conditions can be used for measuring a measurement sample with a UV-visible spectrophotometer, which is used to calculate the above. In measurement with a UV-visible spectrophotometer, the light transmission direction is the thickness direction of the measurement sample. The UV-visible spectrophotometer used for measurement can be a UV-visible spectrophotometer commonly used in the technical field, for example, the V-770 manufactured by JASCO Corporation. Data acquisition interval: 1 nm Bandwidth: 5.0 nm Response: 0.06 seconds Light source: deuterium lamp, halogen lamp Scanning mode: continuous Scanning speed: 400 nm / min Measurement range: 200 nm to 900 nm

[0030] The measurement sample to be measured using a UV-visible spectrophotometer can be surface-polished quartz glass (quartz glass of this embodiment) with a thickness of 0.1 mm to 5.0 mm. The quartz glass to be used as the measurement sample may be cut to a predetermined thickness or less, and then the surface may be polished to a thickness of 0.1 mm to 5.0 mm. Surface polishing of the quartz glass can be performed using a polishing machine commonly used in the technical field, such as the LaboPol 30 manufactured by Struers. It is preferable to polish the quartz glass surface to a smooth surface with an arithmetic mean roughness Ra of 3 nm or less. Surface polishing of the quartz glass may be performed on at least two surfaces: the surface onto which light to be transmitted through the quartz glass enters (hereinafter also referred to as the "incident surface") and the surface from which light to be transmitted through the quartz glass exits (hereinafter referred to as the "exit surface") in measurement using a UV-visible spectrophotometer. Furthermore, a general surface grinder (for example, product name: PSG-52SA1, manufactured by Okamoto Machine Tool Works, Ltd.) can be used to cut the quartz glass. The arithmetic mean roughness Ra of the quartz glass surface (i.e., the surface of the measurement sample) can be measured using a general surface roughness measuring device (for example, product name: Optical Surface Texture Measuring Instrument ZYGO New View 7100, manufactured by ZYGO Corporation) in accordance with JIS B 0601-2001 under the following conditions: Measurement magnification: Objective lens x 50x, Zoom x 1x, Measurement range: 172 μm x 141 μm

[0031] The silica glass of this embodiment has a tin content of 5 ppm or more and 150 ppm or less, and α 252nm / α 222nm If is 2.5 or more, α 252nm and α 222nm Other configurations such as the above are not particularly limited.

[0032] From the viewpoint of making the transmitted light more suitable for irradiation of a living body, the α of the quartz glass of this embodiment is 252nm is 30,000 cm -1 It is preferable that the viscosity is 40,000 cm or more. -1 More preferably, it is 90,000 cm or more. -1 It is even more preferable that the viscosity is 150,000 cm or more. -1It is particularly preferable that α is equal to or greater than α. 252nm The upper limit of is not particularly limited, but is, for example, 700,000 cm -1 Below, 600000cm -1 Below, 500000cm -1 or less, or 400,000 cm -1 It can be: α 252nm may be any combination of the upper and lower limits described above, but from the viewpoint of making the transmitted light more suitable for irradiation of a living body, 30000 cm -1 More than 700000cm -1 Preferably, it is 40,000 cm or less. -1 More than 600000cm -1 More preferably, it is 90,000 cm or less. -1 More than 500000cm -1 Even more preferably, it is 150,000 cm or less. -1 More than 400000cm -1 It is particularly preferred that:

[0033] From the viewpoint of further improving the sterilization performance and virus inactivation performance of transmitted light, the α of the quartz glass of this embodiment is 222nm is 200,000 cm -1 Preferably, it is 150,000 cm or less. -1 More preferably, it is 100,000 cm or less. -1 Even more preferably, it is 80,000 cm or less. -1 It is particularly preferable that α 222nm The lower limit is not particularly limited, but is, for example, 5000 cm -1 Above, 10000cm -1 Above, 15000cm -1 or more, or 20,000 cm -1 It can be set to more than α 222nm may be any combination of the upper and lower limits described above, but from the viewpoint of further improving the sterilization performance and virus inactivation performance by the transmitted light, it is preferable to use a value of 5000 cm -1 More than 200000cm -1 Preferably, it is 10,000 cm or less.-1 More than 150000cm -1 More preferably, it is 15,000 cm or less. -1 More than 100000cm -1 Even more preferably, it is 20,000 cm or less. -1 More than 80000cm -1 It is particularly preferred that:

[0034] The silica glass of this embodiment has a tin content of 5 ppm or more and 150 ppm or less, and α 252nm / α 222nm As long as the ratio is 2.5 or more, the composition is not particularly limited. For example, the silica glass of this embodiment is a glass containing tin and silica (SiO 2 ), or may be composed of tin and silica (SiO 2 In order to further improve the transmittance of light at 222 nm, the silica glass of this embodiment may contain tin and silica (SiO 2 ) is preferable. In particular, from the viewpoint of further improving the transmission of 222 nm light, the quartz glass of this embodiment preferably does not contain alkali metals, alkaline earth metals, and transition metals (hereinafter collectively referred to as "foreign metal elements"). "Not containing foreign metal elements" means that the content of foreign metal elements in the quartz glass of this embodiment is below the detection limit, and although it depends on the detection capability of the measuring device, it can be exemplified as being 0 ppm or more and 3 ppm or less. The content of foreign metal elements in the quartz glass of this embodiment is more preferably more than 0 ppm and 3 ppm or less, and particularly preferably more than 0 ppm and 2 ppm or less. Furthermore, a foreign metal element content of 0 ppm means that no foreign metal elements are contained.

[0035] The silica glass of this embodiment has a tin content of 5 ppm or more and 150 ppm or less, and α 252nm / α 222nmThe linear transmittance is not particularly limited as long as it is 2.5 or more. From the viewpoint of making the transmitted light more suitable for irradiation of living bodies, the quartz glass of this embodiment preferably has an internal linear transmittance of light with a wavelength of 252 nm at a thickness of 1 mm (hereinafter also referred to as "internal linear transmittance 252 nm") of 70% or less, more preferably 50% or less, and particularly preferably 40% or less. Furthermore, from the viewpoint of further improving the sterilization performance and virus inactivation performance of the transmitted light, the quartz glass of this embodiment preferably has an internal linear transmittance of light with a wavelength of 222 nm at a thickness of 1 mm (hereinafter also referred to as "internal linear transmittance 222 nm") of 30% or more, more preferably 50% or more, and particularly preferably 70% or more.

[0036] In the silica glass of this embodiment, the lower limit of the internal linear transmittance at 252 nm when the thickness is 1 mm is not particularly limited and can be, for example, 0% or more. In the silica glass of this embodiment, the upper limit of the internal linear transmittance at 222 nm when the thickness is 1 mm is not particularly limited and can be, for example, 100% or less.

[0037] The internal linear transmittance of the silica glass of this embodiment is a linear transmittance corrected and removed for the effects of light scattered by bubbles in the silica glass and light reflected at the surface (interface) of the silica glass. In the silica glass of this embodiment, the internal linear transmittance at a thickness of 1 mm is calculated by multiplying the thickness d of the measurement sample (the thickness of the measurement sample measured by an ultraviolet-visible spectrophotometer) by the T calculated by the above formula (2). i It can be calculated from the following equation (10) using T 1mm = (T i / 100) 0.1/d × 100 (10) In the above formula (10), T 1mm represents the internal linear transmittance [%] of light with a wavelength W (nm) of quartz glass when the thickness is 1 mm, and T i represents the internal linear transmittance [%] of the quartz glass for light of wavelength W (nm), and d represents the thickness [cm] of the measurement sample.

[0038] In the silica glass of this embodiment, light with a wavelength of 222 nm is more easily transmitted, and the more the transmission of light with a wavelength of 252 nm is suppressed, the better the balance between the suppression of transmission of 252 nm light and the transmission of 222 nm light is. Therefore, in the silica glass of this embodiment, the internal linear transmittance 222 nm at a thickness of 1 mm is preferably higher than the internal linear transmittance 252 nm at a thickness of 1 mm, more preferably 20% or more higher than the internal linear transmittance 252 nm at a thickness of 1 mm, even more preferably 30% or more higher than the internal linear transmittance 252 nm at a thickness of 1 mm, and particularly preferably 40% or more higher than the internal linear transmittance 252 nm at a thickness of 1 mm. The upper limit of the difference (internal linear transmittance 222 nm - internal linear transmittance 252 nm) obtained by subtracting the internal linear transmittance 252 nm at a thickness of 1 mm from the internal linear transmittance 222 nm at a thickness of 1 mm is not particularly limited, but can be, for example, 80% or less, 70% or less, 60% or less, or 50% or less.

[0039] The form of the silica glass of this embodiment is not particularly limited, but it is preferably a single layer of silica glass, as this does not require a complicated manufacturing process.

[0040] Here, the α of quartz glass 252nm / α 222nm does not change depending only on the content of components (such as tin) contained in the quartz glass, but also on other factors, such as the manufacturing method. Therefore, even if the tin content of the quartz glass is 5 ppm or more and 150 ppm or less, the α of the quartz glass 252nm / α 222nm Therefore, the quartz glass of this embodiment has a tin content of 5 ppm or more and 150 ppm or less, and α 252nm / α 222nm The tin content is 5 ppm or more and 150 ppm or less, and α is 2.5 or more. 252nm / α 222nm An example of a method for producing quartz glass having a σ of 2.5 or more (i.e., the quartz glass of this embodiment) will be described.

[0041] The silica glass of this embodiment can be produced by a production method including a first heat treatment step in which a raw material composition containing a silica source and a tin source is heat-treated at a temperature of 20°C or higher and 1900°C or lower under a vacuum of 10 Pa or lower, and a second heat treatment step in which the raw material composition heat-treated in the first heat treatment step is heat-treated under a nitrogen atmosphere at a temperature of 1400°C or higher and 1900°C or lower.

[0042] The silica source contained in the raw material composition can be, for example, silica powder, which can be one or more selected from the group consisting of commercially available silica powder, silica powder obtained by hydrolysis of silicon alkoxide, and silica powder obtained by hydrolysis of silicon tetrachloride with an oxyhydrogen flame or the like.

[0043] Examples of the tin source contained in the raw material composition include tin compounds. Specific examples of tin compounds include tin oxide (SnO 2 Examples of the tin compound include one or more selected from the group consisting of tin(IV) chloride, tin(IV) hydroxide, and tin(II) sulfate, with tin oxide being preferred. The tin compound is preferably in the form of a powder, from the viewpoint of mixing it more uniformly with the silica source. The content of the tin source in the raw material composition may be an amount that results in a tin content of 5 ppm or more and 150 ppm or less in the quartz glass to be produced, and can be adjusted as appropriate.

[0044] The raw material composition may be a simple mixture of the raw materials (silica source and tin source), or a tin compound-containing silica powder obtained by a sol-gel method may be used. The method for producing a tin compound-containing silica powder is not particularly limited, and may be any method for producing a silica powder by a conventionally known sol-gel method, in which a tin compound is added to a reaction solution in which a sol-gel reaction is carried out.

[0045] An example of a specific method for producing tin-containing silica powder is a method in which a sol-gel reaction is carried out in a reaction solution obtained by mixing at least a tin compound, silicon alkoxide, and water to obtain a tin compound-containing silica gel, the obtained tin compound-containing silica gel is dried to obtain a tin compound-containing dried silica gel, and the obtained tin compound-containing dried silica gel is calcined to produce a tin compound-containing silica powder.

[0046] In the above-described method for producing a tin compound-containing silica powder, the content ratio of silicon alkoxide to water (silicon alkoxide:water) in the reaction solution can be any conventionally known content ratio, but can be, for example, a mass ratio of 10: 1 to 1: 1. The content of the tin compound in the reaction solution can be set appropriately, as long as the tin content in the produced quartz glass is 5 ppm or more and 150 ppm or less.

[0047] In the above-mentioned method for producing a tin compound-containing silica powder, conventionally known drying conditions can be used to dry the tin compound-containing silica gel, for example, drying conditions can be used in the atmosphere at 40°C to 150°C for 1 hour to 10 hours. In addition, in the above-mentioned method for producing a tin compound-containing silica powder, conventionally known firing conditions can be used to calcinate the tin compound-containing dried silica gel, for example, calcination conditions can be used in the atmosphere at 600°C to 1300°C for 1 hour to 10 hours.

[0048] In the above-mentioned method for producing a tin compound-containing silica powder, the reaction solution in which the sol-gel reaction is carried out may contain at least a tin compound, a silicon alkoxide, and water. However, from the viewpoint of promoting the sol-gel reaction, it is preferable that the reaction solution further contains, in addition to these, one or more components selected from the group consisting of an acid, an alkali, and a solvent.

[0049] Examples of acids that can be contained in the reaction solution include one or more selected from the group consisting of hydrochloric acid, nitric acid, and sulfuric acid. At least one of hydrochloric acid and sulfuric acid is preferred, and hydrochloric acid is more preferred. Examples of alkalis that can be contained in the reaction solution include one or more selected from the group consisting of ammonia, methylamine, and dimethylamine, and ammonia is preferred. Examples of solvents that can be contained in the reaction solution include one or more selected from the group consisting of ethanol, methanol, and propanol. The acid content in the reaction solution can be a conventionally known content, but can be, for example, 0.001 mol / L to 1 mol / L, preferably 0.001 mol / L to 0.1 mol / L. The alkali content in the reaction solution can be a conventionally known content, but can be, for example, 0.001 mol / L to 1 mol / L, preferably 0.1 mol / L to 1 mol / L. The content of the solvent in the reaction solution is, for example, 30% by volume or more and 80% by volume or less, and preferably 40% by volume or more and 60% by volume or less, relative to 100% by volume of the reaction solution.

[0050] The raw material composition may be composed only of the silica source and tin source described above, but may also contain one or more components other than the silica source and tin source.

[0051] For the raw material composition, a mixture of the raw materials (the silica source, the tin source, and other components contained as necessary) may be used as is, or a molded product obtained by molding the mixture of the raw materials into a predetermined shape by a method such as compression may be used.

[0052] In the first heat treatment step, the heat treatment of the raw material composition is carried out at a temperature of 20° C. or higher and 1900° C. or lower. The heat treatment temperature of the raw material composition in the first heat treatment step may be 20° C. or higher and 1900° C. or lower, but is preferably 20° C. or higher and 1700° C. or lower, more preferably 20° C. or higher and 1600° C. or lower, even more preferably 1000° C. or higher and 1600° C. or lower, and particularly preferably 1400° C. or higher and 1600° C. or lower.

[0053] In the first heat treatment step, the raw material composition is heat-treated under a vacuum of 10 Pa or less. The pressure during the heat treatment of the raw material composition in the first heat treatment step may be 10 Pa or less, but is preferably 0.1 Pa or more and 10 Pa or less. The pressure during the heat treatment can be adjusted, for example, by degassing the air from a heat treatment container containing the raw material composition.

[0054] The heat treatment time of the raw material composition in the first heat treatment step can be, for example, 10 minutes or more and 300 minutes or less, and preferably 30 minutes or more and 90 minutes or less.

[0055] In the second heat treatment step, the raw material composition heat-treated in the first heat treatment step is heat-treated in a nitrogen atmosphere at 1400°C or higher and 1900°C or lower. The second heat treatment step may be performed on the raw material composition heat-treated in the first heat treatment step under the conditions described above. The timing of the second heat treatment step is not particularly limited, but it is preferably performed immediately after the first heat treatment step. In other words, the heat treatment in the second heat treatment step is preferably performed immediately after the completion of the heat treatment in the first heat treatment step (before the raw material composition heat-treated in the first heat treatment step is cooled).

[0056] In the second heat treatment step, the raw material composition is heat-treated at 1400° C. or higher and 1900° C. or lower. The heat treatment temperature of the raw material composition in the second heat treatment step may be 1400° C. or higher and 1900° C. or lower, preferably 1500° C. or higher and 1800° C. or lower, and more preferably 1700° C. or higher and 1800° C. or lower.

[0057] In the second heat treatment step, the raw material composition is heat-treated in a nitrogen atmosphere. The nitrogen atmosphere is an atmosphere in which the excess space (space excluding the raw material composition) of the container in which the raw material composition is stored is replaced with nitrogen gas, and does not exclude gases other than nitrogen that may be unintentionally mixed in. For example, the nitrogen atmosphere may be created by introducing nitrogen gas into a heat treatment container whose internal pressure is set to 10 Pa or less in the first heat treatment step.

[0058] The pressure during the heat treatment of the raw material composition in the second heat treatment step can be, for example, 100,000 Pa or more and 980,000 Pa or less, and is preferably 100,000 Pa or more and 200,000 Pa or less.

[0059] The heat treatment time of the raw material composition in the second heat treatment step can be, for example, 10 minutes or more and 120 minutes or less, and preferably 10 minutes or more and 90 minutes or less.

[0060] The raw material composition is heat-treated in the second heat treatment step to produce the quartz glass of this embodiment. Note that in the second heat treatment step, the quartz glass obtained by the heat treatment may be left in a nitrogen atmosphere to cool, and the quartz glass cooled in the nitrogen atmosphere may be used as the quartz glass of this embodiment.

[0061] The silica glass of this embodiment can be manufactured by a manufacturing method including the above-described first heat treatment step and second heat treatment step.

[0062] The silica glass of this embodiment described above can transmit 222 nm light while suppressing the transmission of 252 nm light. The reason why the silica glass of this embodiment can transmit 222 nm light while suppressing the transmission of 252 nm light is not clear, but it is thought that the tin content is 5 ppm or more and 150 ppm or less, and that the α 252nm / α 222nm It is presumed that when the SiO 2 content is 2.5 or more, the dispersion state of tin in the quartz glass and the state of the quartz are changed to a state that not only suppresses the transmission of 252 nm UV light but also allows the transmission of 222 nm UV light. Such a quartz glass of the present embodiment can be used, for example, as an optical filter for excimer light.

[0063] The present disclosure will be described below with reference to examples, but the present disclosure is not limited to these examples.

[0064] (Tin Content) Quartz glass was crushed and dissolved in hydrofluoric acid, followed by the addition of sulfuric acid and heating to volatilize the hydrofluoric acid, yielding a residue for measurement. This residue for measurement was dissolved in nitric acid to prepare a sample solution. Using a standard ICP atomic emission spectrometer (product name: 5800 ICP-OES, manufactured by Agilent Technologies), the sample solution was measured by inductively coupled plasma atomic emission spectrometry (ICP-AES) under the following conditions: Frequency: 27 MHz Output: 1.2 kW Observation mode: axial Detector: CCD detector Scanning mode: continuous Sample introduction: cyclone nebulizer The tin content and the content of other metal elements in the quartz glass were determined from the obtained measured values ​​of tin and other metal elements.

[0065] (Measurement Sample) A disk-shaped quartz glass with a diameter of 24 mm and a thickness of 8 mm was prepared, and a measurement sample having a thickness that allowed measurement of the linear transmittance using an ultraviolet-visible spectrophotometer (device name: V-770, manufactured by JASCO Corporation) was prepared. That is, the quartz glass was ground to a thickness of 0.5 mm to 3.5 mm while visually inspecting it using a precision surface grinder (device name: PSG-52SA1, manufactured by Okamoto Machine Tool Works, Ltd.). The ground quartz glass was further polished using a polishing machine (Labopol 30, manufactured by Struers) until it was thinner to a thickness of 0.2 mm, and a measurement sample with an arithmetic mean roughness Ra of 3 nm or less on the surfaces (incident surface and exit surface) was obtained. The arithmetic mean roughness Ra of the measurement sample surface (incident surface and exit surface) was measured using a general surface roughness measuring device (product name: optical surface texture measuring device ZYGO New View 7100, manufactured by ZYGO Corporation) in accordance with JIS B 0601-2001 under the following conditions: Measurement magnification: objective lens × 50, zoom × 1, measurement range: 172 μm × 141 μm

[0066] (Absorption Coefficient) Using an ultraviolet-visible spectrophotometer (device name: V-770, manufactured by JASCO Corporation), the measurement sample was measured under the following conditions, and the measured linear transmittance [%] of the measurement sample for light with a wavelength of 222 nm (T in the above formula (3)), the measured linear transmittance [%] of the measurement sample for light with a wavelength of 252 nm (T in the above formula (3)), and the average value [%] of the measured linear transmittance of the measurement sample for light with wavelengths of 790 nm to 800 nm (T in the above formula (3)) were calculated. (790-800nm) The light transmission direction was the thickness direction of the sample. Data acquisition interval: 1 nm Band width: 5.0 nm Response: 0.06 seconds Light source: deuterium lamp, halogen lamp Scan mode: continuous Scan speed: 400 nm / min Measurement range: 200 nm to 900 nm

[0067] The tin content (c in the above formula (1)), the measured linear transmittance [%] of the measurement sample for light with a wavelength of 222 (nm) (T in the above formula (3)), and the average value [%] of the measured linear transmittance of the measurement sample for light with a wavelength of 790 nm to 800 nm (T in the above formula (3)) were determined by the above method. (790-800nm) ), and the wavelength W (nm) is set to 222 (nm) (i.e., W = 222), the absorption coefficient (α 222nm Similarly, the tin content (c in the above formula (1)), the measured linear transmittance [%] of the measurement sample for light with a wavelength of 252 (nm) (T in the above formula (3)), and the average value [%] of the measured linear transmittance of the measurement sample for light with wavelengths of 790 nm to 800 nm (T in the above formula (3)) were determined by the above method. (790-800nm) ), and the wavelength W (nm) is set to 252 (nm) (i.e., W = 252), and from the above equations (1) to (9), the absorption coefficient (α 252nm ) was calculated. 252nm α 222nmBy dividing by α, the ratio of the absorption coefficient at a wavelength of 252 nm to the absorption coefficient at a wavelength of 222 nm is obtained. 252nm / α 222nm ) was sought.

[0068] (Internal linear transmittance at a thickness of 1 mm) α 222nm Using the internal linear transmittance [%] of the quartz glass for light with a wavelength of 222 nm (Ti in the above formula (10) (the above formula (2))) and the thickness [cm] of the measurement sample (d in the above formula (10)), which were calculated in the calculation process, the internal linear transmittance [%] of the quartz glass for light with a wavelength of 222 nm at a thickness of 1 mm was calculated from the above formula (10). 252nm The internal linear transmittance [%] of the quartz glass for light with a wavelength of 252 nm (Ti in the above formula (10) (the above formula (2))) obtained in the calculation process and the thickness [cm] of the measurement sample (d in the above formula (10)) were used to calculate the internal linear transmittance [%] of the quartz glass for light with a wavelength of 252 nm when the thickness was 1 mm from the above formula (10).

[0069] Example 1 Commercially available silica powder (product name: MKC Silica PS100, manufactured by Mitsubishi Chemical Corporation) was jet milled to have an average particle size D50 (median diameter) of 5 μm or less. 100 g of the silica powder was mixed with tin oxide (SnO) to give a Sn content of 30 ppm (0.003 mass%). 2 ) powder (manufactured by SIGMA-ALDRICH Co.), silica powder and tin oxide (SnO 2 ) was obtained as a mixed powder, which was used as a raw material powder.

[0070] 8.0 g of the obtained raw material powder was filled into a mold with a diameter of 30 mm, and then subjected to pressure of 150 kgf / cm 2 A pressure of 100 kJ / cm was applied for 30 seconds to form a compact. The compact was placed in a carbon container and treated at 1575°C for 60 minutes under a vacuum of 10 Pa or less (below the detection limit). Nitrogen was then introduced at 130 kPa, and the compact was treated in a nitrogen atmosphere at 1775°C for 20 minutes, after which it was allowed to cool naturally overnight in the nitrogen atmosphere to obtain the quartz glass of this example.

[0071] The quartz glass of this example had a tin content of 7.4 ppm and a content of foreign metal elements of 2 ppm or less (below the detection limit). The quartz glass of this example also had an absorption coefficient of 62405 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 250275 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm ) was 4.01, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 65.3%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 89.9%.

[0072] Example 2 SnO was added so that the Sn content of the raw material powder was 50 ppm (0.005 mass%). 2 The quartz glass of this example was obtained in the same manner as in Example 1, except that powder (manufactured by SIGMA-ALDRICH) was mixed.

[0073] The quartz glass of this example had a tin content of 8.9 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). The quartz glass of this example also had an absorption coefficient of 77834 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 324405 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm ) was 4.17, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 51.4%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 85.3%.

[0074] Example 3 SnO was added so that the Sn content of the raw material powder was 70 ppm (0.007 mass%). 2 The quartz glass of this example was obtained in the same manner as in Example 1, except that powder (manufactured by SIGMA-ALDRICH) was mixed.

[0075] The quartz glass of this example had a tin content of 13 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). The quartz glass of this example also had an absorption coefficient of 48927 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 227271 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm) was 4.65, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 50.6%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 86.4%.

[0076] Example 4 SnO was added so that the Sn content of the raw material powder was 100 ppm (0.01 mass%). 2 The quartz glass of this example was obtained in the same manner as in Example 1, except that powder (manufactured by SIGMA-ALDRICH) was mixed.

[0077] The quartz glass of this example had a tin content of 18 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). The quartz glass of this example also had an absorption coefficient of 50243 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 248744 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm ) was 4.95, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 35.7%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 81.2%.

[0078] Example 5 SnO was added so that the Sn content of the raw material powder was 200 ppm (0.02 mass%). 2 The quartz glass of this example was obtained in the same manner as in Example 1, except that powder (manufactured by SIGMA-ALDRICH) was mixed.

[0079] The quartz glass of this example had a tin content of 36 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). The quartz glass of this example also had an absorption coefficient of 73574 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 200252 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm ) was 2.72, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 19.0%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 54.3%.

[0080] Example 6 SnO was added so that the Sn content of the raw material powder was 300 ppm (0.03 mass%). 2The quartz glass of this example was obtained in the same manner as in Example 1, except that powder (manufactured by SIGMA-ALDRICH) was mixed.

[0081] The quartz glass of this example had a tin content of 67 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). The quartz glass of this example also had an absorption coefficient of 52323 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 159016 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm ) was 3.04, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 8.6%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 44.6%.

[0082] Example 7 SnO was added so that the Sn content of the raw material powder was 500 ppm (0.05 mass%). 2 The quartz glass of this example was obtained in the same manner as in Example 1, except that powder (manufactured by SIGMA-ALDRICH) was mixed.

[0083] The quartz glass of this example had a tin content of 100 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). The quartz glass of this example also had an absorption coefficient of 41969 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 135066 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm ) was 3.22, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 4.5%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 38.0%.

[0084] Example 8: 200 mL of ethanol (special grade, Junsei Chemical Co., Ltd.) and 150 mL of tetraethoxysilane (Tokyo Chemical Industry Co., Ltd.) were mixed to obtain an ethanol solution, to which 50 mL of purified water, 1 mL of 2 mol / L hydrochloric acid (Fujifilm Wako Pure Chemical Industries, Ltd.), and 0.0117 g of tin chloride pentahydrate (Fujifilm Wako Pure Chemical Industries, Ltd.) were added. 5 mL of 28% aqueous ammonia solution (Fujifilm Wako Pure Chemical Industries, Ltd.) was further added and mixed to obtain a mixed solution. The obtained mixed solution was dried overnight in air at 120°C and then further calcined in air at 800°C for 1 hour to obtain a tin-containing silica powder. The obtained tin-containing silica powder had an Sn content of 100 ppm (0.01% by mass) relative to the silica powder.

[0085] The quartz glass of this example was obtained in the same manner as in Example 1, except that the obtained tin-containing silica powder was used as the raw material powder and the treatment in a nitrogen atmosphere was performed at 1800°C for 60 minutes.

[0086] The quartz glass of this example had a tin content of 56 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). The quartz glass of this example also had an absorption coefficient of 24205 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 90927 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm ) was 3.76, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 30.7%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 73.2%.

[0087] Comparative Example 1: SnO was added so that the Sn content of the raw material powder was 10 ppm (0.001 mass%). 2 The quartz glass of this comparative example was obtained in the same manner as in Example 1, except that powder (manufactured by SIGMA-ALDRICH) was mixed.

[0088] The quartz glass of this comparative example had a tin content of 3.4 ppm and a content of foreign metal elements of 2 ppm or less (below the detection limit). The quartz glass of this comparative example also had an absorption coefficient of 95318 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 149698 cm -1 , the ratio of extinction coefficients (α 252nm / α222nm ) was 1.57, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 88.9%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 92.8%.

[0089] Comparative Example 2: SnO was added so that the Sn content of the raw material powder was 1000 ppm (0.1 mass%). 2 The quartz glass of this comparative example was obtained in the same manner as in Example 1, except that powder (manufactured by SIGMA-ALDRICH) was mixed.

[0090] The quartz glass of this comparative example had a tin content of 160 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). The quartz glass of this comparative example also had an absorption coefficient of 44609 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 186948 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm ) was 4.19, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 0.1%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 19.3%.

[0091] Comparative example 3 SnO 2 The quartz glass of this comparative example was obtained in the same manner as in Example 1, except that no powder was mixed.

[0092] The quartz glass of this comparative example had a tin content of 0 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). Furthermore, the quartz glass of this comparative example had an internal linear transmittance of 97.3% at a wavelength of 252 nm when the thickness was 1 mm, and an internal linear transmittance of 98.6% at a wavelength of 222 nm when the thickness was 1 mm.

[0093] Comparative Example 4 Commercially available silica powder (product name: MKC Silica PS100, manufactured by Mitsubishi Chemical Corporation) was jet milled to have an average particle size D50 (median diameter) of 5 μm or less. 100 g of the silica powder was mixed with tin oxide (SnO) so that the Sn content was 200 ppm (0.02 mass%). 2 ) powder (manufactured by SIGMA-ALDRICH Co.), silica powder and tin oxide (SnO 2 ) was obtained as a mixed powder, which was used as a raw material powder.

[0094] 8.0 g of the obtained raw material powder was filled into a mold with a diameter of 30 mm, and then subjected to pressure of 150 kgf / cm 2 A pressure of 100 kJ / cm was applied for 30 seconds to form a compact. The compact was placed in a carbon container, nitrogen was introduced at 130 kPa, and the compact was treated in a nitrogen atmosphere at 1575°C for 60 minutes, and then further treated in the nitrogen atmosphere at 1775°C for 20 minutes. The compact was then allowed to cool naturally overnight in the nitrogen atmosphere to obtain the quartz glass of this comparative example.

[0095] The quartz glass of this comparative example had a tin content of 39 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). The quartz glass of this comparative example also had an absorption coefficient of 527569 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 532745 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm ) was 1.01, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 0.8%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 0.9%.

[0096] Comparative Example 5 A tin-containing silica powder was obtained in the same manner as in Example 8. 8.0 g of the obtained raw material powder was filled into a mold having a diameter of 30 mm, and then subjected to a pressure of 150 kgf / cm 2 A pressure of 100 kJ / cm was applied for 30 seconds to form a compact. The compact was placed in a carbon container, nitrogen was introduced at 130 kPa, and the compact was treated in a nitrogen atmosphere at 1575°C for 60 minutes, and then further treated in the nitrogen atmosphere at 1800°C for 20 minutes. The compact was then allowed to cool naturally overnight in the nitrogen atmosphere to obtain the quartz glass of this comparative example.

[0097] The quartz glass of this comparative example had a tin content of 33 ppm and a foreign metal element content of 2 ppm or less (below the detection limit). The quartz glass of this comparative example also had an absorption coefficient of 766237 cm at 222 nm. -1 , the extinction coefficient at 252 nm is 681667 cm -1 , the ratio of extinction coefficients (α 252nm / α 222nm ) was 0.89, the internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm was 0.6%, and the internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm was 0.3%.

[0098] The evaluation results of the examples and comparative examples are shown in Table 1 below.

[0099] As can be seen from Table 1 above, the silica glass of each Example had a lower internal linear transmittance at a wavelength of 252 nm when the thickness was 1 mm than Comparative Example 1, which had a tin content of 3.4 ppm. Furthermore, the silica glass of each Example had a higher internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm than Comparative Example 2, which had a tin content of 160 ppm. Furthermore, the silica glass of each Example had a higher internal linear transmittance at a wavelength of 222 nm when the thickness was 1 mm than the silica glasses of Comparative Examples 4 and 5. From these results, it was understood that the silica glass of each Example was able to transmit 222 nm light while suppressing the transmission of 252 nm light.

[0100] (Test of UV irradiation of fibroblasts with a peak wavelength of 254 nm) Normal human adult skin fibroblasts (manufactured by Kurabo Industries, Ltd.) were placed in a 96-well plate (transparent plate) at 3.3 × 10 3 The cells were seeded at 1000 cells / well and cultured overnight. After overnight culture, a 96-well plate was fixed onto the quartz glass (thickness: 3.0 mm) of each Example and Comparative Example. An ultraviolet irradiation device (device name: Handy UV Lamp, manufactured by AS ONE Corporation) was positioned so that the distance from the bottom of the 96-well plate to the irradiation surface was 50 mm, and ultraviolet light with a peak wavelength of 254 nm (ultraviolet light containing 252 nm light) was irradiated so that the ultraviolet light that passed through the quartz glass was irradiated onto normal human adult skin fibroblasts. The ultraviolet light irradiation was performed in a clean bench with the lid of the 96-well plate removed, and three conditions with different irradiation doses (10 J / cm) were used. 2 , 15 J / cm 2 , or 20 mJ / cm 2 As a control, normal human adult skin fibroblasts were irradiated with ultraviolet light under the same conditions as above, except that the quartz glass was not fixed to the 96-well plate.

[0101] 24 hours after UV irradiation, 10 μL of WST-8 reagent (manufactured by Dojin Chemical Co., Ltd.) was added to each well, and the plates were further cultured at 37°C for 2 hours. After 2 hours of culture, the absorbance at 450 nm was measured using a plate reader (device name: EnSpire, manufactured by PerkinElmer) under the following conditions, and the average value of the absorbance in the four wells (hereinafter also referred to as "measured absorbance") was calculated. FLASH: 100 times Measurement height: 7.5 mm

[0102] The absorbance at 450 nm (hereinafter also referred to as "reference absorbance") when cultured under the same conditions as the control (without quartz glass) except for not irradiating with ultraviolet light was set as a relative cell number of 100, and the relative cell number was calculated using the following formula (I). The results are shown in Tables 2a, 2b, and 2c below. Relative cell number = (measured absorbance / reference absorbance) × 100 (I)

[0103]

[0104] As shown in Tables 2a, 2b, and 2c, the relative cell count when ultraviolet light was irradiated through the quartz glass of Example 4 was 96 or more, whereas the relative cell count when ultraviolet light was irradiated through the quartz glass of Comparative Example 3 was 64 or less. From these results, it was understood that the quartz glass of Example 4 can reduce the impact of ultraviolet light passing through it on living organisms compared to the quartz glass of Comparative Example 3.

[0105] (Test of ultraviolet irradiation of Staphylococcus aureus with a peak wavelength of 222 nm) A medium (hereinafter simply referred to as "medium") was prepared by dissolving high polypeptone (Shiotani MS Co., Ltd.), dry yeast extract (Nacalai Tesque, Inc.), and magnesium sulfate (Fujifilm Wako Pure Chemical Industries, Ltd.) in ultrapure water to have the same composition as NBRC (National Institute of Technology and Evaluation Biotechnology Center) Medium No. 702, and sterilizing it by autoclaving. In this test, this medium was used to culture Staphylococcus aureus.

[0106] Vial-dried Staphylococcus aureus (NBRC12732) was suspended in a medium, to which 15% agar powder (Fujifilm Wako Pure Chemical Industries, Ltd.) was added. The suspension was then spread onto a plate and cultured at room temperature (24°C). Every four days, multiple colonies were scraped from the plate to prepare a bacterial cell suspension, which was then spread onto a new plate for subculture.

[0107] Staphylococcus aureus cultured as described above was inoculated at different concentrations into 50 mL tubes containing 10 mL of medium and incubated overnight at 24°C with shaking. After overnight osmotic incubation, the bacterial cell solution with an OD (optical density) at 600 nm of 1 or less was diluted with medium to obtain a bacterial cell solution with an OD at 600 nm of 0.2. The bacterial cell solution with an OD at 600 nm of 0.2 was further diluted 1000-fold with medium to prepare the test solution. 3 mL / well of agar medium was added to a 12-well plate, and the plate was allowed to dry for 1 hour with the lid open. After drying for 1 hour, 50 μL / well of the test solution was added, and the plate was quickly shaken horizontally to diffuse the test solution throughout the wells before it penetrated the agar.

[0108] Quartz glass (thickness 3.0 mm) from each example and comparative example was placed on the well, and an ultraviolet irradiation device (excimer spot lamp, manufactured by Oak Manufacturing Co., Ltd.) was placed so that the distance from the agar surface to the irradiation surface was 30 mm. Ultraviolet light with a peak wavelength of 222 nm was irradiated so that the ultraviolet light that passed through the quartz glass was irradiated onto Staphylococcus aureus. Ultraviolet light irradiation was performed in a clean bench with the lid of the 12-well plate removed, and two conditions with different irradiation doses (10 J / cm 2 , or 20 mJ / cm 2 As a control, Staphylococcus aureus was irradiated with ultraviolet light under the same conditions as above except that no quartz glass was placed on the 12-well plate.

[0109] After 48 hours had passed since the UV irradiation, the UV irradiation was stopped, the number of colonies in the wells was counted, and the average number of colonies in the three wells (hereinafter also referred to as "measured colony number") was calculated.

[0110] As a reference example, the number of colonies measured without UV irradiation was determined. In this reference example, 1 / 50 of the test solution (1 μL of test solution) added to a 12-well plate by the above-described method was diluted with 99 μL of medium to obtain a total of 100 μL of test solution. This was added to two 90 mm Petri dishes containing 10 mL of agar medium, and cultured for 48 hours. After 48 hours of culture, the number of colonies in the two Petri dishes was counted, and the average value was multiplied by 50 to obtain the number of colonies measured without UV irradiation (the number of colonies measured in the reference example).

[0111] The results are shown in Tables 3a and 3b below.

[0112] As shown in Tables 3a and 3b, the number of colonies measured when ultraviolet light was irradiated through the quartz glass of Example 4 was 0.1 [colonies / well], whereas the number of colonies measured when ultraviolet light was not irradiated (measured colony number in the Reference Example) was 12,700 [colonies / well]. From this result, it was understood that the quartz glass of Example 4 can be sterilized by ultraviolet light passing through it.

Claims

1. Quartz glass having a tin content of 5 ppm or more and 150 ppm or less, and a ratio of the absorption coefficient at a wavelength of 252 nm to the absorption coefficient at a wavelength of 222 nm of 2.5 or more.

2. The quartz glass according to claim 1, which has an internal linear transmittance of 70% or less for light having a wavelength of 252 nm when the thickness is 1 mm.

3. The quartz glass according to claim 1 or 2, which has an internal linear transmittance of 30% or more for light having a wavelength of 222 nm when the thickness is 1 mm.

4. Quartz glass according to any one of claims 1 to 3, in which the internal linear transmittance of light with a wavelength of 222 nm when the thickness is 1 mm is higher than the internal linear transmittance of light with a wavelength of 252 nm when the thickness is 1 mm.

5. The absorption coefficient at a wavelength of 252 nm is 30,000 cm -1 The quartz glass according to any one of claims 1 to 4.

6. The absorption coefficient at a wavelength of 222 nm is 200,000 cm -1 The quartz glass according to any one of claims 1 to 5, wherein:

7. A method for producing quartz glass according to any one of claims 1 to 6, comprising: a first heat treatment step of heat treating a raw material composition containing a silica source and a tin source at 20°C or higher and 1900°C or lower under a vacuum of 10 Pa or lower; and a second heat treatment step of heat treating the raw material composition heat-treated in the first heat treatment step at 1400°C or higher and 1900°C or lower under a nitrogen atmosphere.

8. The method for producing quartz glass according to claim 7, wherein the silica source is silica powder.

9. The method for producing silica glass according to claim 7, wherein the silica source is silica powder obtained by hydrolysis of silicon alkoxide.

Citation Information

Patent Citations

  • Silica glass for EUV lithography optical component containing tio2

    JP2009274947A

  • Inactivation processing device of microorganism and cell activation processing device, as well as inactivation processing method of microorganism and cell activation processing method

    JP2019115525A

  • Excimer lamp and ultraviolet light irradiation device