Glass composition and x-ray radiopaque composition

The glass composition with rubidium and other elements effectively balances high X-ray contrast and low refractive index, addressing the limitations of conventional glass in dental imaging and durability.

WO2024225256A1PCT designated stage expired Publication Date: 2024-10-31GC CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015852
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-23
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional glass compositions face challenges in achieving both high X-ray contrast properties and low refractive index, making it difficult to visualize dental materials effectively while maintaining chemical durability.

Method used

A glass composition incorporating rubidium (Rb) with specific mass content ranges, along with other elements like silicon (Si), cesium (Cs), and potassium (K), which enhances X-ray contrast while controlling refractive index and maintaining chemical durability.

Benefits of technology

The glass composition achieves high X-ray contrast properties with a refractive index of 1.564 or less, ensuring good visualization and chemical durability, suitable for dental applications and potentially other fields like optical elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This glass composition contains rubidium (Rb).
Need to check novelty before this filing date? Find Prior Art

Description

Glass composition and X-ray contrast composition

[0001] The present invention relates to a glass composition and an X-ray contrast composition.

[0002] In the field of dentistry, etc., Cs 2 O, BaO and / or SnO 2 X-ray opaque glasses containing optional fluorine are known (for example, see Patent Document 1).

[0003] Japanese Patent Application Laid-Open No. 2019-131457

[0004] With conventional glasses, the refractive index tends to increase as the X-ray contrast property increases, making it difficult to achieve both high X-ray contrast property and a low refractive index.

[0005] An object of the present invention is to provide a glass composition that can provide a glass that has both high X-ray contrast and a low refractive index.

[0006] A glass composition according to one embodiment of the present invention contains rubidium (Rb).

[0007] According to one aspect of the present invention, it is possible to provide a glass composition that can provide glass that has both high X-ray contrast and a low refractive index.

[0008] Hereinafter, embodiments of the present invention will be described in detail.

[0009] The glass composition according to this embodiment contains rubidium (Rb).

[0010] Rubidium (Rb) has an atomic number (number of electrons) of 37, which is approximately the same as that of strontium (Sr), which has an atomic number (number of electrons) of 38 and exhibits high X-ray contrast properties in glass. Therefore, rubidium (Rb) exhibits high X-ray contrast properties in glass equivalent to those of strontium (Sr).

[0011] Here, X-ray contrast property refers to the property in which the shade of an X-ray image changes depending on the amount of X-ray absorption by the object, such as biological tissue or a material, making it possible to visualize or distinguish the object. In particular, in dental treatment, it is necessary to clearly identify the treatment site after surgery using dental materials, including dental filling materials, and therefore dental materials are required to have X-ray contrast property. In dental materials, the resin matrix is ​​an organic substance and therefore does not have X-ray contrast property, and it is the inorganic filler, such as glass, that provides the X-ray contrast property. Therefore, X-ray contrast property is an important property for dental glass.

[0012] Rubidium (Rb) has an effective ionic radius of 152 pm, which is larger than that of strontium (Sr), which has an effective ionic radius of 118 pm. The larger the effective ionic radius, the lower or sparser the electron density within the atom becomes, so rubidium (Rb) can suppress an increase in the refractive index of glass compared to strontium (Sr).

[0013] Furthermore, rubidium (Rb), with an effective ionic radius of 152 pm, has a smaller effective ionic radius than cesium (Cs), an alkali metal with the same effective ionic radius of 167 pm. For elements of the same group, the smaller the effective ionic radius, the greater the single bond strength between the alkali metal and oxygen, and the greater the chemical stability. Therefore, rubidium (Rb) is less likely to reduce the chemical durability of glass than cesium (Cs). Examples of chemical durability include water resistance.

[0014] Rubidium (Rb) is contained in the glass composition in the form of an oxide of rubidium (Rb) (rubidium oxide (Rb 2 O)).

[0015] The content of rubidium (Rb) is not particularly limited, and is, for example, 3 mass % or more, preferably 5 mass % or more, and more preferably 7 mass % or more, calculated as an oxide. The content of rubidium (Rb) calculated as an oxide is determined based on the content of rubidium oxide (Rb 2 0) in the glass composition.

[0016] The upper limit of the content of rubidium (Rb) calculated as an oxide is not particularly limited, but from the viewpoint of suppressing a decrease in the chemical durability of the glass composition, the content of rubidium (Rb) is preferably 60 mass % or less, more preferably 50 mass % or less, and even more preferably 40 mass % or less.

[0017] In this embodiment, the glass composition contains rubidium (Rb), which can improve the X-ray contrast properties of the resulting glass. Furthermore, the refractive index of the resulting glass increases only slightly while maintaining high X-ray contrast properties, making it easier to control the refractive index. Furthermore, the glass composition contains rubidium (Rb), which makes it less likely that the chemical durability of the resulting glass will be reduced.

[0018] The type of the glass composition of this embodiment is not particularly limited as long as it contains rubidium (Rb), and examples of the glass composition include silicate glass, borate glass, phosphate glass, borosilicate glass, silicophosphate glass, fluorophosphate glass, sulfophosphate glass, soda-lime glass, aluminosilicate glass, and aluminoborosilicate glass.

[0019] Among these, silicate glass, borate glass, and borosilicate glass are preferred as the types of glass composition. Note that the main component of silicate glass is silicon (Si).

[0020] That is, the glass composition of the present embodiment preferably contains silicon (Si). Silicon (Si) is contained in the glass composition in the form of an oxide of silicon (Si) (silicon oxide (SiO 2 )

[0021] The content of silicon (Si) is not particularly limited, and is, for example, preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, calculated as an oxide. The content of silicon (Si) calculated as an oxide is silicon oxide (SiO 2 ) in the glass composition.

[0022] When the content of silicon (Si) calculated as oxide is 10 mass % or more, it becomes possible to adjust the viscosity of the glass composition and also to increase the mechanical strength of the glass composition.

[0023] The upper limit of the content of silicon (Si) calculated as oxide is not particularly limited. However, since an increase in silicon (Si) in the glass composition hardens the glass melt, from the viewpoint of reducing production costs, the upper limit is preferably 90 mass % or less, more preferably 85 mass % or less, and even more preferably 80 mass % or less.

[0024] The glass composition of the present embodiment may further contain cesium (Cs).

[0025] Cesium (Cs) has an atomic number (number of electrons) of 55, which is approximately the same as that of barium (Ba), which has an atomic number (number of electrons) of 56, which exhibits high X-ray contrast properties. Therefore, Cs exhibits high X-ray contrast properties equivalent to those of barium (Ba). Therefore, even when Cs is mixed with rubidium (Rb), the X-ray contrast properties of the resulting glass can be improved.

[0026] Furthermore, cesium (Cs) has an effective ionic radius of 167 pm, which is larger than that of barium (Ba), which has an effective ionic radius of 135 pm (the electron density in the atom is low or sparse), and therefore can suppress an increase in the refractive index compared to barium (Ba). Therefore, even when cesium (Cs) is mixed with rubidium (Rb), an increase in the refractive index of the resulting glass can be suppressed while maintaining high X-ray contrast properties.

[0027] Furthermore, although cesium (Cs) has inferior chemical durability compared to rubidium (Rb), mixing cesium (Cs) with rubidium (Rb) does not cause a decrease in chemical durability due to the inclusion of rubidium (Rb). Therefore, by replacing a portion of rubidium (Rb), which has a relatively expensive raw material cost, with cesium (Cs), which has a relatively inexpensive raw material cost, it is possible to prevent an increase in the manufacturing cost of the glass composition.

[0028] Cesium (Cs) is contained in the glass composition as an oxide of cesium (Cs) (cesium oxide (Cs 2 O).

[0029] When cesium (Cs) is contained, the content of cesium (Cs) is not particularly limited, and is, for example, 3 mass % or more, preferably 5 mass % or more, and more preferably 10 mass % or more in terms of oxide. The content of cesium (Cs) in terms of oxide is cesium oxide (Cs 2 0) in the glass composition.

[0030] When the content of cesium (Cs) in terms of oxide is 3% by mass or more, in combination with rubidium (Rb), the X-ray contrast properties of the obtained glass can be improved and an increase in the refractive index can be suppressed. Note that the upper limit of the content of cesium (Cs) in terms of oxide is not particularly limited, but from the viewpoint of not decreasing the content of rubidium (Rb), it is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.

[0031] The glass composition of this embodiment may further contain potassium (K). Potassium (K) is contained in the glass composition in the form of an oxide of potassium (K). 2 O).

[0032] When potassium (K) is contained, the content of potassium (K) is 1 mass % or more and 15 mass % or less, preferably 3 mass % or more and 12 mass % or less, more preferably 5 mass % or more and 10 mass % or less, calculated as an oxide. 2 0) in the glass composition.

[0033] When potassium (K) is contained, the content of potassium (K) in terms of oxide is 1 mass %, which can lower the melting temperature of the glass composition, making it easier to manufacture or process the glass composition and making it applicable as a material in various fields. Furthermore, the content of potassium (K) in terms of oxide is 15 mass % or less, which can suppress a decrease in the chemical durability of the glass composition.

[0034] The glass composition of this embodiment may further contain sodium (Na). Sodium (Na) is contained in the glass composition in the form of an oxide of sodium (Na) (sodium oxide (Na 2 O).

[0035] When sodium (Na) is contained, the content of sodium (Na) is 1 mass % or more and 15 mass % or less, preferably 1.5 mass % or more and 12 mass % or less, more preferably 2 mass % or more and 10 mass % or less, calculated as an oxide. The content of sodium (Na) calculated as an oxide is sodium oxide (Na 2 0) in the glass composition.

[0036] When sodium (Na) is contained, the content of sodium (Na) in terms of oxide of 1 mass % can lower the melting temperature of the glass composition, facilitating the production or processing of the glass composition and making it applicable as a material in various fields. Furthermore, the content of sodium (Na) in terms of oxide of 15 mass % or less can suppress a decrease in the chemical durability of the glass composition.

[0037] From the viewpoint of reliably suppressing a decrease in the chemical durability of the glass composition, it is preferable that the glass composition of this embodiment does not contain at least one of potassium (K) and sodium (Na). In this specification, "not containing at least one of potassium (K) and sodium (Na)" means that the glass composition does not substantially contain potassium (K) and / or sodium (Na) except for inevitable impurities.

[0038] When potassium (K) is contained in the glass composition as an inevitable impurity, the content of potassium (K) is 0.5 mass % or less, preferably 0.3 mass % or less, and more preferably 0.1 mass % or less, calculated as oxide.

[0039] When sodium (Na) is contained in the glass composition as an inevitable impurity, the content of sodium (Na) is 0.5 mass % or less, preferably 0.3 mass % or less, and more preferably 0.1 mass % or less, calculated as an oxide.

[0040] The glass composition of this embodiment may contain other elements as long as they do not impair the object of the present invention. Examples of other elements include boron (B), fluorine (F), aluminum (Al), zinc (Zn), strontium (Sr), zirconium (Zr), tin (Sn), barium (Ba), lanthanum (La), and gadolinium (Gd), from the viewpoint of improving X-ray contrast or chemical durability. The other elements, except for fluorine (F), may be present as oxides in the glass composition. The content of the other elements is not particularly limited, and they may be contained in the glass composition at any mass.

[0041] Boron (B) is contained in the glass composition in the form of an oxide of boron (B) (boron oxide (B 2 O 3 )

[0042] When boron (B) is contained, the content of boron (B) is not particularly limited, but is preferably 40 mass % or less, more preferably 35 mass % or less, and even more preferably 30 mass % or less, calculated as an oxide. The content of boron (B) calculated as an oxide is the content of boron oxide (B 2 O 3 ) in the glass composition.

[0043] When the content of boron (B) in terms of oxide is 40% by mass or less, the melting point of the glass of the glass composition can be lowered and manufacturing can be facilitated. Note that, when boron (B) is contained, the lower limit of the content of boron (B) in terms of oxide is not particularly limited, but from the viewpoint of the chemical durability and ease of manufacturing of the glass composition, it is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more.

[0044] Fluorine (F) may be present in the glass composition as a fluoride or a fluoride salt.

[0045] When fluorine (F) is contained, the content of fluorine (F) is not particularly limited, but is preferably 6 mass % or less, more preferably 5.5 mass % or less, and even more preferably 5 mass % or less. The content of fluorine (F) indicates the mass content of fluorine (F) as a simple substance in the glass composition.

[0046] The refractive index of the resulting glass can be adjusted by adjusting the fluorine (F) content to 6% by mass or less. The lower limit of the fluorine (F) content when fluorine (F) is contained is not particularly limited, but from the viewpoint of reducing the viscosity of the glass composition and improving the handleability of the glass composition, it is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more.

[0047] Aluminum (Al) is contained in the glass composition in the form of an oxide of aluminum (Al) (aluminum oxide (Al 2 O 3 )

[0048] When aluminum (Al) is contained, the content of aluminum (Al) is not particularly limited, but is preferably 35 mass % or less, more preferably 30 mass % or less, and even more preferably 25 mass % or less, calculated as an oxide. The content of aluminum (Al) calculated as an oxide is determined based on the content of aluminum oxide (Al 2 O 3 ) in the glass composition.

[0049] When the content of aluminum (Al) in terms of oxide is 35% by mass or less, the chemical durability of the glass composition can be improved and devitrification of the glass can be suppressed. Note that, when aluminum (Al) is contained, the lower limit of the content of aluminum (Al) in terms of oxide is not particularly limited, but from the viewpoint of the chemical durability of the glass composition and suppression of devitrification of the glass, it is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more.

[0050] Zinc (Zn) may be present in the glass composition as an oxide of zinc (Zn), zinc oxide (ZnO).

[0051] When zinc (Zn) is contained, the content of zinc (Zn) is not particularly limited, but is preferably 20 mass % or less, more preferably 15 mass % or less, and even more preferably 10 mass % or less, calculated as oxide. The content of zinc (Zn) calculated as oxide indicates the mass content of zinc oxide (ZnO), which is an oxide of zinc (Zn), in the glass composition.

[0052] By setting the content of zinc (Zn) in terms of oxide to 20% by mass or less, it is possible to prevent devitrification and facilitate production without reducing the chemical durability of the resulting glass. Note that, when zinc (Zn) is contained, the lower limit of the content in terms of zinc (Zn) in terms of oxide is not particularly limited, but from the viewpoints of the chemical durability of the glass composition and suppressing devitrification of the glass, it is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more.

[0053] Strontium (Sr) may be present in the glass composition as an oxide of strontium (Sr), such as strontium oxide (SrO).

[0054] When strontium (Sr) is contained, the content of strontium (Sr) is not particularly limited, but is preferably 20 mass % or less, more preferably 15 mass % or less, and even more preferably 10 mass % or less, calculated as oxide. The content of strontium (Sr) calculated as oxide indicates the mass content of strontium oxide (SrO), which is an oxide of strontium (Sr), in the glass composition.

[0055] By setting the content of strontium (Sr) in terms of oxide to 20% by mass or less, it is possible to improve the X-ray contrast property while maintaining a low refractive index of the obtained glass. Note that, when strontium (Sr) is contained, the lower limit of the content of strontium (Sr) in terms of oxide is not particularly limited, but from the viewpoint of improving the X-ray contrast property while maintaining a low refractive index, it is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more.

[0056] Zirconium (Zr) is contained in the glass composition in the form of an oxide of zirconium (ZrO 2)

[0057] When zirconium (Zr) is contained, the content of zirconium (Zr) is not particularly limited, but is preferably 20 mass % or less, more preferably 15 mass % or less, and even more preferably 10 mass % or less, calculated as an oxide. The content of zirconium (Zr) calculated as an oxide is zirconium oxide (ZrO 2 ) in the glass composition.

[0058] By ensuring that the zirconium (Zr) content in terms of oxide is 20% by mass or less, it is possible to improve the X-ray contrast properties of the resulting glass and increase its chemical durability while maintaining the meltability of the glass. Note that, when zirconium (Zr) is contained, the lower limit of the zirconium (Zr) content in terms of oxide is not particularly limited, but from the viewpoint of improving chemical durability while maintaining the X-ray contrast properties, it is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 3% by mass or more.

[0059] Tin (Sn) is contained in the glass composition as an oxide of tin (Sn), such as stannic oxide (SnO 2 )).

[0060] When tin (Sn) is contained, the content of tin (Sn) is not particularly limited, but is preferably 25 mass % or less, more preferably 20 mass % or less, and even more preferably 15 mass % or less, calculated as an oxide. The content of tin (Sn) calculated as an oxide is tin oxide (SnO 2 ) in the glass composition.

[0061] When the content of tin (Sn) in terms of oxide is 25% by mass or less, it is possible to maintain the meltability of the glass, improve the X-ray contrast properties of the obtained glass, and increase chemical durability. Note that, when tin (Sn) is contained, the lower limit of the content of tin (Sn) in terms of oxide is not particularly limited, but from the viewpoint of maintaining the X-ray contrast properties and increasing chemical durability, it is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more.

[0062] Barium (Ba) may be present in the glass composition as an oxide of barium (Ba), barium oxide (BaO).

[0063] When barium (Ba) is contained, the content of barium (Ba) is not particularly limited, but is preferably 30 mass % or less, more preferably 25 mass % or less, and even more preferably 20 mass % or less, calculated as the oxide. The content of barium (Ba) calculated as the oxide indicates the mass content of barium oxide (BaO), which is an oxide of barium (Ba), in the glass composition.

[0064] By setting the content of barium (Ba) in terms of oxide to 30% by mass or less, it is possible to improve the X-ray contrast properties of the obtained glass while suppressing a decrease in chemical durability. Note that, when barium (Ba) is contained, the lower limit of the content of barium (Ba) in terms of oxide is not particularly limited, but from the viewpoint of imparting high X-ray contrast properties, it is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more.

[0065] Lanthanum (La) is contained in the glass composition in the form of an oxide of lanthanum (La) (lanthanum oxide (La 2 O 3 )).

[0066] When lanthanum (La) is contained, the content of lanthanum (La) is not particularly limited, but is preferably 40 mass % or less, more preferably 35 mass % or less, and even more preferably 30 mass % or less, calculated as an oxide. The content of lanthanum (La) calculated as an oxide is lanthanum oxide (La 2 O 3 ) in the glass composition.

[0067] When the content of lanthanum (La) in terms of oxide is 40% by mass or less, the X-ray contrast properties of the obtained glass can be improved and chemical durability can be increased while maintaining the meltability of the glass. Note that, when lanthanum (La) is contained, the lower limit of the content of lanthanum (La) in terms of oxide is not particularly limited, but from the viewpoint of improving chemical durability while maintaining the X-ray contrast properties, it is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more.

[0068] Gadolinium (Gd) is an oxide of gadolinium (Gd) 2 O 3 )

[0069] When gadolinium (Gd) is contained, the content of gadolinium (Gd) is not particularly limited, but is preferably 30 mass % or less, more preferably 25 mass % or less, and even more preferably 20 mass % or less, calculated as an oxide. The content of gadolinium (Gd) calculated as an oxide is gadolinium oxide (Gd 2 O 3 ) in the glass composition.

[0070] By ensuring that the gadolinium (Gd) content in terms of oxide is 30% by mass or less, the X-ray contrast properties of the resulting glass can be improved while maintaining the meltability of the glass. Note that, when gadolinium (Gd) is contained, the lower limit of the gadolinium (Gd) content in terms of oxide is not particularly limited, but from the viewpoint of imparting high X-ray contrast properties, it is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more.

[0071] The glass composition of the present embodiment may contain other unavoidable impurities, such as nickel (Ni).

[0072] The form of the glass composition is not particularly limited, and may be, for example, powder (or powder), plate-like, columnar, thread-like, or fibrous. When the glass composition is in powder form, it becomes easier to blend or mix the components of the glass composition. Furthermore, when the glass composition is in plate-like or columnar form, the glass composition can be used in optical elements. Examples of optical elements include optical lenses, prisms, and optical filters.

[0073] The particle size of the powdered glass composition is not particularly limited, but is preferably 0.01 μm or more and 20 μm or less, more preferably 0.02 μm or more and 10 μm or less, and even more preferably 0.1 μm or more and 1 μm or less in terms of median diameter. Here, the particle size means the average particle size defined by the median diameter.

[0074] When the particle size of the glass composition is 0.01 μm or more, the handling of the glass composition is improved when the glass composition is used as a powder, and when the particle size of the glass composition is 20 μm or less, the mechanical strength of the dental composition obtained when applied to a dental material is improved.

[0075] The glass composition of this embodiment can make the refractive index (nd) of glass containing this composition equal to or less than 1.564. In this specification, the refractive index (nd) means the refractive index at the D line (light having a wavelength of 589 nm).

[0076] When the refractive index (nd) of the glass composition of this embodiment is 1.564 or less, when the glass composition is used as a dental composition, the difference in refractive index between the glass composition and a dental resin is small, and the transparency of the resulting dental composition is high. Note that the lower limit of the refractive index (nd) is not particularly limited, but is preferably 1.40 or more, more preferably 1.45 or more, and even more preferably 1.47 or more, as a practical range.

[0077] The glass composition of this embodiment can provide a glass containing the glass with an X-ray contrast property of 200% or more relative to aluminum. In this specification, the X-ray contrast property refers to the X-ray contrast property measured by the X-ray contrast property test method for dental materials in accordance with ISO 4049:2019.

[0078] In this embodiment, a glass composition exhibiting good X-ray contrast properties can be provided by making the X-ray contrast properties of the glass containing the glass composition 200% or more relative to aluminum. The upper limit of the X-ray contrast properties is not particularly limited, but is preferably 1000% or less, more preferably 900% or less, and even more preferably 800% or less relative to aluminum as a practical range.

[0079] The glass composition of this embodiment is not particularly limited in its use, but since the glass composition exhibits high X-ray contrast properties, it can be used as an X-ray contrast composition containing the glass composition.

[0080] Furthermore, by utilizing its high X-ray contrast property, the glass composition of this embodiment can be used as a dental material or dental composition, such as a dental composite resin, a dental cement, a dental adhesive, a dental temporary sealing material, a dental primer, a dental coating material, a dental hard resin, a resin material for dental cutting, a dental temporary restorative material, a dental filling material, a dentifrice, etc.

[0081] The dental composition of this embodiment provides a glass containing the dental composition with high X-ray contrast and transparency, making it possible to obtain a dental composition that combines good X-ray contrast and excellent aesthetics. Furthermore, the dental composition of this embodiment exhibits good X-ray contrast, making it possible to clearly identify the repaired area in a post-treatment diagnosis or examination using X-ray images.

[0082] Furthermore, the glass composition contained in the dental composition of this embodiment is adjusted to a sufficiently suitable refractive index range, and therefore has a small refractive index difference from dental resins, making it suitable for use in dental materials that require aesthetic appeal (e.g., dental composite resins, dental coating materials, dental hard resins, dental cutting resin materials, etc.).

[0083] Furthermore, the glass composition contained in the dental composition of this embodiment has good chemical durability, and therefore can be suitably used as a general dental material applied in the oral cavity.

[0084] The glass composition of the present embodiment can also be used in fields other than dental materials, such as optical elements such as optical lenses, prisms, and optical filters, ultraviolet and infrared blocking glass, and radiation shielding glass.

[0085] The present invention will be further described below with reference to examples. In the following, numerical values ​​without units are based on mass (% by mass) unless otherwise specified.

[0086] <Glass Preparation> The glasses of Examples 1-1 to 1-3, Examples 2-1 to 2-4, Examples 3-1 to 3-2, Examples 4-1 to 4-6, Comparative Examples 1-1 to 1-3, and Comparative Example 3-1 were prepared with the compositions shown in Tables 1 to 4. A raw material batch obtained by mixing various raw materials was placed in a platinum crucible, and then held in an electric furnace preheated to 1400 to 1500°C for 30 to 60 minutes. The batch was then poured into a carbon mold to obtain a bulk body. Alternatively, the glass was melted in a similar manner, and then the molten glass was dropped into a water tank to obtain granulated glass. The glass was pulverized in an alumina magnetic mortar to obtain glass powder with a median diameter (average particle size) of 20 to 300 μm.

[0087] The refractive index of the obtained glass powder (glass) was measured. The obtained glass bulk was heat-treated in an electric furnace by heating from room temperature to 600°C at a heating rate of 20°C / min, holding at 600°C for 30 minutes, and then slowly cooling to room temperature. The heat-treated glass bulk was sliced ​​to obtain slices.

[0088] <Refractive Index> A liquid having a specific refractive index and the prepared glass powder were mixed in a 1:1 mass ratio and packed into a transparent tube. Next, the transparent tube was held over a white LED, and the color of the light transmitted through the transparent tube was visually observed. The refractive index of the liquid that produced green light through the transparent tube was adopted as the refractive index of the glass powder. Note that if the refractive index of the liquid was lower than that of the glass powder, the color of the light transmitted through the transparent tube was blue. Also, if the refractive index of the liquid was higher than that of the glass powder, the color of the light transmitted through the transparent tube was red or yellow. The refractive index of the glass was evaluated as good if the refractive index was 1.564 or less, and poor if the refractive index exceeded 1.564. The results of the refractive index of the glass are shown in Tables 1 to 4.

[0089] <X-ray contrast property> The X-ray contrast property (% relative to Al) of the obtained glass slices was measured. The X-ray contrast property was measured using the X-ray contrast property test method for dental materials in accordance with ISO 4049:2019. Specifically, the optical density or gray value of a test piece (plate-shaped glass composition) with a thickness Ts (unit: mm) was measured. Next, the thickness Ta (unit: mm) of an aluminum plate exhibiting the same optical density or gray value as the test piece with a thickness Ts was determined. The ratio of Ta to Ts (unit: % relative to Al) was used as the value of X-ray contrast property. The evaluation of X-ray contrast property was judged as good when the ratio relative to aluminum was 200% or more, and poor when the ratio relative to aluminum was less than 200%. The results of the refractive index of the glass are shown in Tables 1 to 4.

[0090] <Water Resistance> 2.0 g of glass powder (median diameter 20 to 300 μm) was weighed. The glass powder was added to a Duran glass bottle (manufactured by SCHOTT, "Duran" is a registered trademark), and then 50 mL of distilled water was added and the bottle was shaken. The bottle was placed in a thermostatic chamber preheated to 98°C and allowed to stand for 1 hour. After removal from the thermostatic chamber, the bottle was allowed to cool to room temperature, and the electrical conductivity of the immersion liquid was measured using an electrical conductivity meter (manufactured by HORIBA, Ltd.). In the water resistance test, the amount of ions eluted from the glass powder into the immersion liquid was measured and evaluated. Note that the smaller the amount of ion elution, i.e., the smaller the evaluation value of water resistance (unit: μS), the better the glass composition was evaluated to exhibit water resistance. Specifically, water resistance was evaluated as good when it was 800 μS or less, and poor when it exceeded 800 μS. The water resistance results are shown in Tables 1, 3, and 4.

[0091]

[0092]

[0093]

[0094]

[0095] As can be seen from Tables 1 to 4, in Examples 1-1 to 1-3, Examples 3-1 to 3-2, and Examples 4-1 to 4-6, the glass compositions containing rubidium (Rb) provided glasses with good refractive indexes, X-ray contrast properties, and water resistance.

[0096] In contrast, in Comparative Examples 1-1 to 1-3 and Comparative Example 3-1, the glass compositions not containing rubidium (Rb) were poor in at least one of the refractive index, X-ray contrast property, and water resistance of the resulting glasses.

[0097] Furthermore, as can be seen from Table 1, Examples 1-2 and 1-3 showed excellent physical properties (low refractive index, high X-ray contrast, and high water resistance) due to the inclusion of Rb, even when Na and Cs were contained.

[0098] Furthermore, Table 2 shows that in Examples 2-1 to 2-4, the X-ray contrast property increased with a slight increase in the refractive index as the Rb content increased. In other words, it was found that by increasing the Rb content, the X-ray contrast property can be improved while suppressing an increase in the refractive index. In other words, it was found that the X-ray contrast property can be adjusted as desired by changing the Rb content.

[0099] Furthermore, Table 3 shows that Examples 3-1 and 3-2 exhibited good water resistance by not containing Na and K. In contrast, Comparative Example 3-1 exhibited poor water resistance when Na was contained. In other words, it was found that the water resistance of a glass composition containing Rb can be further improved by using a composition that does not contain Na and / or K.

[0100] Furthermore, Tables 3 and 4 show that glass compositions containing Rb exhibited excellent physical properties (low refractive index, high X-ray contrast, and high water resistance) due to the inclusion of Rb, even when combined with elements such as F, Zn, Sn, Sr, Zr, Ba, La, and Gd. In particular, in Examples 3-1 to 3-2 and Examples 4-1 to 4-6, the inclusion of Sn, Sr, Zr, Ba, La, and Gd further improved the X-ray contrast. In addition, in Examples 4-1 and 4-6, the inclusion of Sn, Zr, and La improved not only the X-ray contrast but also the water resistance. Furthermore, the inclusion of F and Zn resulted in a glass composition having a low refractive index while exhibiting both good X-ray contrast and sufficient water resistance.

[0101] The above-disclosed embodiments include, for example, the following aspects.

[0102] (Supplementary Note 1) A glass composition containing rubidium (Rb).

[0103] (Appendix 2) The glass composition according to Appendix 1, further comprising silicon (Si).

[0104] (Appendix 3) The glass composition according to appendix 1 or 2, containing cesium (Cs).

[0105] (Appendix 4) The glass composition according to any one of Appendices 1 to 3, which does not contain at least one of potassium (K) and sodium (Na).

[0106] (Appendix 5) An X-ray contrast composition comprising the glass composition according to any one of Appendices 1 to 4.

[0107] (Appendix 6) A dental composition comprising the X-ray contrast composition according to Appendix 5.

[0108] Although the embodiments of the present invention have been described above, the present invention is not limited to the specific embodiments, and various modifications and changes are possible within the scope of the invention described in the claims.

[0109] This application claims priority based on Japanese Patent Application No. 2023-074448, filed on April 28, 2023, the entire contents of which are incorporated herein by reference.

Claims

1. A glass composition comprising rubidium (Rb).

2. The glass composition according to claim 1, further comprising silicon (Si).

3. The glass composition according to claim 1, further comprising cesium (Cs).

4. The glass composition according to claim 1, which does not contain at least one of potassium (K) and sodium (Na).

5. An X-ray contrast composition comprising the glass composition according to any one of claims 1 to 4.

6. A dental composition comprising the X-ray contrast composition according to claim 5.

Citation Information

Patent Citations

  • Radiopaque glass and use thereof

    JP2019131457A

  • Prize purchasing device

    JP2023074448A

  • CAD / CAM engravable lithium disilicate microcrystalline glass for dentistry and preparation method thereof

    CN107698167A

  • Glass composition

    JP1983208151A

  • Colored zirconia ceramics

    JP1987128967A