Polymer flocculant, production method for same, and sludge dewatering method

The use of a cationic copolymer with a RAFT agent in polymer flocculants addresses the inefficiencies of conventional dewatering methods by enhancing sludge dewatering performance and reducing costs through improved molecular weight control and flocculant efficiency.

WO2024225281A1PCT designated stage expired Publication Date: 2024-10-31MT AQUAPOLYMER +1

Patent Information

Application Number
PCT/JP2024/015951
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-23
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional polymer flocculants face challenges in effectively dewatering difficult-to-dewater sludge due to high viscosity and molecular entanglement, leading to inefficient sludge dewatering and increased costs, while existing methods for reducing water content in dehydrated cakes require large amounts of flocculants and have high manufacturing costs.

Method used

A cationic copolymer is developed using a reversible addition-fragmentation chain transfer (RAFT) agent as a control agent, allowing for the production of a polymer flocculant with a specific molecular weight range and structure that enhances dewatering performance by forming strong flocs with low viscosity, reducing the amount of flocculant needed and lowering production costs.

Benefits of technology

The new polymer flocculant achieves high dewatering efficiency with a wide range of addition amounts, resulting in a dehydrated cake with low water content and reduced operational costs, while maintaining excellent filtration performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The present invention provides: (1) a polymer flocculant comprising a cationic copolymer that has a cationic monomer as an essential structural unit thereof, said polymer flocculant being characterized in that the cationic copolymer has, at an end thereof, a structure derived from a degenerative chain transfer mechanism-type control agent; and (2) a polymer flocculant characterized by comprising a block copolymer of a polymer block (A) which is formed by polymerizing a monomer component (a) and a polymer block (B) which is formed by polymerizing a monomer component (b), wherein the polymer block (A) has, at an end thereof, a structure derived from a degenerative chain transfer mechanism-type control agent, the polymer block (A) is non-ionic unit, and the polymer block (B) is a cationic unit.
Need to check novelty before this filing date? Find Prior Art

Description

Polymer flocculant, its manufacturing method, and sludge dewatering method

[0001] The present invention relates to a polymer flocculant, a method for producing the same, and a method for dewatering sludge.

[0002] There is a strong global movement toward carbon neutrality, and sewage treatment and industrial wastewater treatment are no exception. The B-DASH (Breakthrough by Dynamic Approach in Sewage High Technology) project, led by the Ministry of Land, Infrastructure, Transport and Tourism of Japan, is focusing on the development of high-concentration sewage digesters and low-power dehydrators. Digested sludge is classified as difficult-to-dehydrate sludge due to its low organic and fibrous content. If high-concentration digestion reactions are achieved, the digested sludge that emerges as residue will likely also become highly concentrated, making it even more difficult to dehydrate. Furthermore, the development of low-power dehydrators requires the drive unit itself to be less powerful, which necessitates the use of chemicals such as polymer flocculants to reduce the moisture content of the dehydrated sludge.

[0003] Polymer flocculants are used to flocculate, settle and separate suspended solids contained in domestic and industrial wastewater, and are also used as retention aids in the paper industry, and as admixtures and mud-adding agents in civil engineering and construction. Polymer flocculants come in various ionic types: nonionic, anionic, cationic and amphoteric, and the type of ionic flocculant to be used depends on the properties of the water to be treated and the treatment method.

[0004] Among these polymer flocculants, cationic polymer flocculants are often used to flocculate and dewater excess sludge after activated sludge treatment of industrial and domestic wastewater, or as retention aids in the paper industry. Cationic polymer flocculants are also used to dewater digested sludge, which is difficult to dewater. In the former application, branched or cross-linked polymers are used for sludge that is difficult to dewater. Amphoteric polymer flocculants are used to coarsely flocculate suspended particles whose charge has been neutralized by a coagulant, and are particularly suitable for sludge that is difficult to dewater or flocculate.

[0005] Conventional cationic polymer flocculants have high viscosity due to strong intermolecular interactions and strong entanglement of the molecules. Because the entanglement of polymer molecules can be stronger than the interaction between the polymer molecules and sludge, linear polymers tend to have a narrow dosage range when added to sludge, and if the dosage is not appropriate, the moisture content of the dehydrated sludge cake may not decrease.

[0006] Crosslinked polymers are sometimes used as polymer flocculants. Emulsion-type crosslinked polymers maintain their three-dimensional molecular structure, exhibit weak intermolecular interactions, and exhibit low viscosity. Therefore, they react rapidly with sludge, forming strong flocs and potentially reducing the moisture content of the dehydrated cake (Patent Document 1). However, because their molecular weight is lower than that of conventional cationic polymer flocculants, they tend to require larger dosages and therefore are more expensive than conventional cationic polymer flocculants. While a complementary effect can be expected from the combined use of conventional powder-type cationic polymer flocculants and emulsion-type crosslinked polymers, the dissolution equipment required can be different, making operation complicated at some treatment plants. Copolymerization of relatively hydrophobic monomers has also been used to hydrophobically modify powdered polymers, but this results in a large amount of insoluble matter due to poor polymerization, making hydrophobic modification difficult.

[0007] Meanwhile, polymer flocculants have traditionally been available in the form of powders and water-in-oil emulsions. Water-in-oil emulsions have the advantage of being highly soluble and dissolving uniformly in a short time, but they have the disadvantage of being more expensive to produce than powders and having a lower content of the active ingredient in the polymer flocculant, resulting in higher transportation costs.

[0008] Under these circumstances, recent developments have focused on polymer flocculants, which are powders made by drying water-in-oil emulsions containing branched or cross-linked cationic or amphoteric polymers. These polymer flocculants exhibit excellent dewatering performance even for difficult-to-dewater sludge, overcome the drawback of transportation costs, and can be used in existing equipment, such as general-purpose automatic dissolving equipment for powders, which has been widely used for some time.

[0009] For example, Patent Document 2 discloses a method for producing a granular polymer flocculant, in which a water-soluble monomer mixture containing a cationic monomer and 5 to 2,000 ppm of a crosslinking agent is reverse-phase polymerized in a non-aqueous liquid to produce a reverse-phase emulsion of primary polymer particles, at least 90% by weight of which have a particle size of 10 μm or less, and then the reverse-phase emulsion is spray-dried, so that at least 90% by weight of the primary polymer particles have a particle size of 20 μm or more, and its use as a polymer flocculant.

[0010] However, the spray-dried granules of crosslinked polymers described in Patent Document 2 exhibit good performance, with improved filtrate volume (filterability) at optimal dosages compared to linear polymers, but require a large dosage relative to the sludge. There is no mention of a method for reducing the dosage. Furthermore, because the production costs are higher than those of reverse-phase emulsions, they are only used for special, difficult-to-dewater sludge.

[0011] Meanwhile, the present applicant has achieved both low production costs and high performance by using a polymer flocculant containing a crosslinked polymer obtained by radical polymerization of a monomer mixture containing a specific cationic monomer and a (meth)acrylate crosslinkable monomer having 3 to 6 (meth)acryloyl groups per molecule. However, there is still room for improvement in terms of performance (Patent Document 3).

[0012] JP 2016-094584 A, Patent No. 4043517 B, Patent No. 6152108

[0013] The first object of the present invention is to solve the above problems and to provide a high-performance polymer flocculant that has excellent flocculation properties for difficult-to-dewater sludge, has a large floc diameter, is excellent in filtration rate and appearance of filtrate, can be effectively dewatered, and can produce a dewatered cake with a low moisture content, a method for producing the same, and a method for dewatering sludge.The second object of the present invention is to provide a polymer flocculant that has superior dewatering performance compared to conventional polymer flocculants, and a method for producing the same.

[0014] As a result of intensive research, the present inventors have found that the first problem can be solved by using a cationic copolymer obtained by copolymerizing monomer components containing at least a cationic monomer in the presence of an exchange chain transfer mechanism control agent as a polymer flocculant; and that the second problem can be solved by a polymer flocculant produced by using, as an intermediate raw material (macro chain transfer agent), a prepolymer obtained by radical polymerization of monomer component (a) in the presence of an exchange chain transfer mechanism control agent, the prepolymer having a structure derived from the exchange chain transfer mechanism control agent at its terminal, and then subjecting monomer component (b) to living radical polymerization in the presence of this prepolymer, thereby completing the present invention.

[0015] The present invention that solves the first problem is described below.

[0016] [1] A polymeric flocculant containing a cationic copolymer having a cationic monomer as an essential constituent unit, characterized in that the cationic copolymer has a structure derived from an exchange chain transfer mechanism type control agent at its terminal.

[0017] [2] The polymer flocculant according to [1], wherein the structure derived from the exchange chain transfer mechanism type control agent is a structure derived from a reversible addition-fragmentation chain transfer agent (RAFT agent).

[0018] [3] The structure derived from the reversible addition-fragmentation chain transfer agent (RAFT agent) is represented by the following chemical formula (1):

[0019]

[0020] (However, in the chemical formula (1), R 3 and R 4 represents an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted heteroaryl group, or an optionally substituted aralkyl group.

[0021] [4] The polymer flocculant according to any one of [1] to [3], wherein the salt viscosity X (mPa·s) at 25°C of a salt solution obtained by dissolving the cationic copolymer in a 4 mass% sodium chloride aqueous solution at a concentration of 0.5 mass% is 3.0 to 200, and the spinnability Y (mm) at 25°C of a solution obtained by dissolving the cationic copolymer in pure water at a concentration of 1.0 mass% is within the range represented by the following mathematical formula (1): 0≦Y≦0.57X+0.0068X 2 ...Number (1)

[0022] [5] The polymer flocculant according to any one of [1] to [4], wherein the cationic copolymer has an insoluble content of 5.0 mass % or less in a 0.1 mass % aqueous solution.

[0023] [6] The cationic monomer is at least a compound represented by the following chemical formula (2): CH 2 =CR 1 -CO-X-Q-N+R 2a R 2b R 2c ・Z - ...Chemical formula (2) (However, in chemical formula (2), R 1 is a hydrogen atom or a methyl group, R 2a and R 2b are each independently an alkyl group having 1 to 3 carbon atoms or a benzyl group, R 2c represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different. X represents an oxygen atom or NH, Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms, Z - and each represent a counter anion.) The polymer flocculant according to any one of [1] to [5], comprising a cationic monomer represented by the following formula:

[0024] [7] A method for producing a polymer flocculant according to any one of [1] to [6], comprising a step of copolymerizing a monomer component containing a cationic monomer by living radical polymerization in the presence of an exchange chain transfer mechanism type control agent to produce a cationic copolymer.

[0025] [8] The method for producing a polymer flocculant according to [7], wherein the exchange chain transfer mechanism type control agent is a reversible addition-fragmentation chain transfer agent (RAFT agent).

[0026] [9] The reversible addition-fragmentation chain transfer agent (RAFT agent) is represented by the following chemical formula (1):

[0027]

[0028] (However, in the chemical formula (1), R 3 and R 4 represents an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted heteroaryl group, or an optionally substituted aralkyl group.

[0029]

[10] The method for producing a polymer flocculant according to any one of [7] to [9], wherein the copolymerization is polymerization by irradiation with active energy rays.

[0030]

[11] A method for dehydrating sludge, comprising adding the polymer flocculant according to any one of [1] to [6] in an amount of 0.1 to 10,000 ppm relative to the mass of organic sludge, stirring and mixing the sludge, and then dehydrating the sludge using a dehydrator.

[0031] The present invention that solves the second problem is described below.

[0032]

[12] A polymer flocculant comprising a block copolymer of a polymer block (A) formed by polymerizing a monomer component (a) and a polymer block (B) formed by polymerizing a monomer component (b), wherein the polymer block (A) has a structure derived from an exchange chain transfer mechanism type controller at its terminal, and the polymer block (A) is a nonionic unit, and the polymer block (B) is a cationic unit.

[0033]

[13] The polymer flocculant according to

[12] , wherein the salt viscosity of a salt solution obtained by dissolving the block copolymer at a concentration of 0.5% by mass in a 4% by mass aqueous sodium chloride solution at 25°C is 3.0 to 200 mPa s.

[0034]

[14] The polymer flocculant according to

[12] , wherein the block copolymer has an insoluble content of 5.0% by mass or less in a 0.1% by mass aqueous solution.

[0035]

[15] The exchange chain transfer mechanism type regulator is represented by the following chemical formula (1): (However, in the chemical formula (1), R 3 and R 4 represents an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted heteroaryl group, or an optionally substituted aralkyl group.

[0036]

[16] The cationic monomer unit constituting the polymer block (B) is represented by the following chemical formula (2): CH 2 =CR 1 -CO-X-Q-N + R 2a R 2b R 2c ・Z - ...Chemical formula (2) (However, R 1 is a hydrogen atom or a methyl group, R 2a and R 2b are each independently an alkyl group having 1 to 3 carbon atoms or a benzyl group, R 2c represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different. X represents an oxygen atom or NH, Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms, Z - and each represent a counter anion.) The polymer flocculant according to

[12] , comprising a structure derived from one or more cationic monomers represented by the following formula:

[0037]

[17] A method for producing a polymer flocculant according to

[12] , characterized by comprising a step of forming a polymer block (B) by radically polymerizing a monomer component (b) containing at least a cationic monomer in the presence of a prepolymer containing a polymer block (A) having a structure derived from an exchange chain transfer mechanism type control agent at its terminal, thereby producing a block copolymer of the polymer block (A) and the polymer block (B).

[0038]

[18] A method for producing a polymer flocculant according to

[12] , characterized by comprising the following steps (I) and (II): step (I): radically polymerizing a monomer component (a) in the presence of an exchange chain transfer mechanism type controller to produce a prepolymer containing a polymer block (A) having a structure derived from the exchange chain transfer mechanism type controller at its terminal; and step (II): radically polymerizing a monomer component (b) containing at least a cationic monomer in the presence of the prepolymer to form a polymer block (B), thereby producing a block copolymer of the polymer block (A) and the polymer block (B).

[0039]

[19] The method for producing a polymer flocculant according to

[17] , wherein the exchange chain transfer mechanism type control agent is a reversible addition-fragmentation chain transfer agent (RAFT agent).

[0040]

[20] The reversible addition-fragmentation chain transfer agent (RAFT agent) is represented by the following chemical formula (1): (However, in the chemical formula (1), R 3 and R 4 represents an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted heteroaryl group, or an optionally substituted aralkyl group.

[0041]

[21] The method for producing a polymer flocculant according to

[17] , wherein the prepolymer has a weight average molecular weight (Mw) of 1,000 to 300,000 as measured by gel permeation chromatography (GPC).

[0042]

[22] The method for producing a polymer flocculant according to

[17] , wherein the radical polymerization is polymerization by irradiation with active energy rays.

[0043]

[23] The method for producing a polymer flocculant according to

[18] , wherein the radical polymerization in the step (II) is polymerization by irradiation with active energy rays.

[0044]

[24] A method for dewatering sludge, comprising adding the polymer flocculant according to any one of

[12] to

[16] to sludge.

[0045] According to the present invention, a polymer flocculant having high dewaterability for sludge can be produced over a wide range of addition amounts.

[0046] The polymer flocculant and its manufacturing method, as well as the sludge dewatering method of the present invention, are described below. In the following description, it is impossible or almost impractical to directly identify the cationic copolymer, prepolymer, block copolymer, and polymer flocculant by their structure or properties. In some cases, they can only be clearly identified by the process (manufacturing method) for obtaining the composition. In the following description, "(meth)acrylic acid" refers to acrylic acid and / or methacrylic acid, and "(meth)acrylate" refers to acrylate and / or methacrylate. Unless otherwise specified, various physical property values ​​are those at 25°C and atmospheric pressure. A description of a numerical value as x to y means that the value is greater than or equal to x and less than or equal to y. When only y is assigned a unit, it means that x also has the same unit.

[0047] A. First Invention 1. Polymer Flocculant The polymer flocculant of the first invention is a polymer flocculant containing a cationic copolymer having a cationic monomer as an essential structural unit, characterized in that the cationic copolymer has a structure derived from an exchange chain transfer mechanism control agent at its terminal. In other words, this cationic copolymer is a cationic copolymer produced by copolymerizing multiple monomers including at least a cationic monomer by living radical polymerization in the presence of an exchange chain transfer mechanism control agent. Note that while living radical polymerization using an exchange chain transfer mechanism control agent is known, there are no known examples of its application to the production of polymer flocculants, and its effects are also unknown.

[0048] The 0.5% by mass (polymer equivalent) salt viscosity X at 25°C of the cationic copolymer constituting the polymer flocculant of the first invention is preferably 3.0 to 200 mPa·s, more preferably 5.0 to 90 mPa·s, and even more preferably 10 to 85 mPa·s. The 0.5% by mass salt viscosity X is an indicator of the molecular weight of the cationic copolymer. If it is less than 3.0 mPa·s, the molecular weight is too small, which may result in poor sludge coagulation. If it exceeds 200 mPa·s, the molecular weight is too large, which may result in reduced solubility of the cationic copolymer or worsening of sludge coagulation. The 0.5% by mass (polymer equivalent) salt viscosity refers to the salt viscosity at 25°C of a salt solution in which a polymer flocculant is dissolved at a concentration of 0.5% by mass in a 4% by mass aqueous sodium chloride solution. The 0.5% by mass salt viscosity can be controlled by the type and amount of the exchange chain transfer mechanism control agent, the type of monomer, and the polymerization conditions.

[0049] The spinnability Y (mm) at 25°C of an aqueous solution in which the cationic copolymer constituting the polymer flocculant of the first invention is dissolved in pure water at a concentration of 1.0 mass % is determined by the following formula (1): 0≦Y≦0.57X+0.0068X 2 ...Number (1) It is preferable that the range is within the range represented by the following formula: Spinnability is an index of the molecular weight distribution of the cationic copolymer. For the same average molecular weight, the lower the spinnability, the fewer high molecular weight polymers there are, i.e., the narrower the molecular weight distribution. When the spinnability Y is within this range, the molecular weight distribution tends to be sufficiently narrow, and the dewatering effect on sludge per added amount tends to be high. When the spinnability Y deviates from this range, the molecular weight distribution tends to be wide, and the amount added to fully achieve the dewatering effect on sludge tends to be large. The spinnability can be controlled by the type and amount of the exchange chain transfer mechanism control agent.

[0050] The insoluble content of the cationic copolymer constituting the polymer flocculant of the first invention in a 0.1% by mass aqueous solution is preferably 5.0% by mass or less, more preferably 4.0% by mass or less. If the insoluble content is high, the flocculation performance per added amount will be low. The insoluble content can be controlled by the type and amount of the exchange chain transfer mechanism type controller, the type of monomer, and the polymerization conditions.

[0051] Examples of the structure derived from an exchange chain transfer mechanism type control agent include structures derived from a reversible addition-fragmentation chain transfer agent in the RAFT method (hereinafter also referred to as a "RAFT agent"), a control agent in the iodine transfer polymerization method, a control agent in the TERP method, a control agent in the SBRP method, a control agent in the BIRP method, etc. Among these, from the viewpoint of ease of implementation, a structure derived from a RAFT agent is particularly preferred.

[0052] As the RAFT agent, various known RAFT agents such as dithioester compounds, xanthate compounds, trithiocarbonate compounds, and dithiocarbamate compounds can be used. Among these, in terms of excellent polymerization control of (meth)acrylic monomers (particularly (meth)acrylic acid ester compounds), compounds represented by the following chemical formula (1):

[0053]

[0054] (However, in the chemical formula (1), R 3 and R 4 represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a heteroaryl group which may have a substituent, or an aralkyl group which may have a substituent.) The structure derived from the trithiocarbonate compound described above means a structure derived from a trithiocarbonate compound and containing at least a part of the trithiocarbonate compound. The cationic copolymer constituting the polymer flocculant of the present invention has at its terminal a trithiocarbonate structure (hereinafter referred to as a "trithio structure"), an organic group bonded to the trithio structure (i.e., R 3 or R 4 The cationic copolymer constituting the polymer flocculant of the first invention preferably has an organic group bonded to the trithio structure at one end and a composite group of an organic group bonded to the trithio structure and a trithio structure at the other end.

[0055] Specific examples of the trithiocarbonate compound include S,S-dibenzyltrithiocarbonate, bis[4-(2,3-dihydroxypropoxycarbonyl)benzyl]trithiocarbonate, bis[4-(2-hydroxyethoxycarbonyl)benzyl]trithiocarbonate, 1,4-bis(n-dodecylsulfanylthiocarbonylsulfanylmethyl)benzene, 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid, and 4-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}-4-cyanopentanoic acid.

[0056] The cationic copolymer constituting the polymer flocculant of the first invention contains at least a cationic monomer as an essential constituent unit, and may also contain constituent units of a nonionic monomer and an anionic monomer as necessary.

[0057] The cationic monomer may be a compound represented by the following chemical formula (2): 2 =CR 1 -CO-X-Q-N+R 2a R 2b R 2c ・Z - ...Chemical formula (2) (However, in chemical formula (2), R 1 is a hydrogen atom or a methyl group, R 2a and R 2b are each independently an alkyl group having 1 to 3 carbon atoms or a benzyl group, R 2c represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different. X represents an oxygen atom or NH, Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms, Z - and each represent a counter anion.

[0058] Specific examples of the (meth)acrylate monomer represented by the above chemical formula (2) include hydrochlorides and sulfates of dialkylaminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylamino-2-hydroxypropyl (meth)acrylate, and dialkylaminoalkyl (meth)acrylamides such as dimethylaminopropyl (meth)acrylamide. Further examples include quaternary salts of alkyl halide adducts such as methyl chloride of dialkylaminoalkyl (meth)acrylates and dialkylaminoalkyl (meth)acrylamides, benzyl halide adducts such as benzyl chloride, and dialkyl sulfate adducts such as dimethyl sulfate. These (meth)acrylate monomers may be used alone or in combination of two or more. Among these preferred (meth)acrylate monomers, the use of the methyl chloride quaternary salt of dimethylaminoethyl acrylate (DAC) is most preferred, as it has particularly excellent performance as a polymer flocculant and is also excellent in the quality and storage stability of the acrylate monomer. These cationic monomer constituent units may be contained alone or in combination of two or more.

[0059] The cationic copolymer constituting the polymer flocculant of the first invention preferably contains 50 to 100 mol %, more preferably 55 to 95 mol %, and particularly preferably 60 to 90 mol % of the cationic monomer structural unit. If the molar fraction of the cationic monomer structural unit is outside the above range, the flocculation property may decrease.

[0060] The cationic copolymer constituting the polymer flocculant of the first invention is preferably a copolymer of the above-mentioned cationic monomer and nonionic monomer.The nonionic monomer is not particularly limited, but examples thereof include (meth)acrylamide compounds represented by the following chemical formula (4), as well as alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and hydroxyethyl (meth)acrylate, styrene, acrylonitrile, and vinyl acetate.Among these nonionic monomers, those having excellent copolymerizability with cationic monomers, easy to increase the molecular weight required for polymer flocculants, and excellent performance as polymer flocculants are preferred, as represented by the following chemical formula (4): CH 2 =CR 1 -CO-NR 2 R 3 ...Chemical formula (4) (wherein, in the above chemical formula (4), R 1 is a hydrogen atom or a methyl group, and R 2 and R 3 and each independently represent a hydrogen atom or an alkyl group having 1 to 8 carbon atoms.

[0061] Among these (meth)acrylamide compounds, acrylamide (AM) is the most preferred because it is water-soluble and has particularly excellent performance as a polymer flocculant. These nonionic monomer constituent units may be used alone or in combination of two or more.

[0062] The cationic copolymer constituting the polymer flocculant of the first invention preferably contains 0 to 50 mol %, more preferably 5 to 45 mol %, and particularly preferably 10 to 40 mol % of the nonionic monomer structural unit. If the molar fraction of the nonionic monomer structural unit is outside the above range, the polymer flocculant tends to be less effective for sludge with a wide range of properties.

[0063] The cationic copolymer constituting the polymer flocculant of the first aspect of the present invention may contain a structural unit of an anionic monomer. Examples of the anionic monomer include (meth)acrylic acid and salts thereof represented by the following chemical formula (5), as well as vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, maleic acid, and salts thereof. Among these anionic monomers, the following chemical formula (5): CH is preferred because it has excellent copolymerizability with cationic monomers, is easily formed into a high molecular weight required for a polymer flocculant, and has excellent performance as a polymer flocculant. 2 =CR 1 -CO-OM... Chemical formula (5) (wherein, in chemical formula (5), R 1 is a hydrogen atom or a methyl group, and M is a hydrogen atom, an ammonium group, or an alkali metal atom.) Preferred salts of (meth)acrylic acids are those represented by the following formula: and salts thereof. Preferred salts are ammonium salts and alkali metal salts such as sodium salts and potassium salts.

[0064] Among these (meth)acrylic acids and their salts, acrylic acid (AA) and its ammonium salt are most preferred because of their particularly excellent performance as polymer flocculants. These anionic monomer structural units may be used alone or in combination of two or more.

[0065] The cationic copolymer produced in the first aspect of the present invention preferably contains 0 to 50 mol %, more preferably 0 to 40 mol %, and particularly preferably 0 to 30 mol % of the anionic monomer structural unit.

[0066] The form of the polymer flocculant of the first aspect of the present invention is not particularly limited, but it is preferably in powder form from the viewpoint of transportation costs and the like.

[0067] The polymer flocculant of the first invention may contain, in addition to the cationic copolymer, various additives as long as they do not impair the effects of the invention. Examples of additives include binders used during granulation, dyes, pH adjusters, anti-degradants, antioxidants, inorganic flocculants, etc. Examples of pH adjusters and anti-degradants include various acidic substances such as sulfamic acid, and examples of inorganic flocculants include, but are not limited to, aluminum sulfate, polyaluminum chloride, ferric chloride, ferrous sulfate, and polyferric sulfate.

[0068] The polymer flocculant of the first aspect of the present invention preferably contains the cationic copolymer in an amount of 50% by mass or more, more preferably 70% by mass or more, and particularly preferably 90% by mass or more. Naturally, it may contain 100% by mass.

[0069] 2. First Method for Producing Polymer Flocculant The cationic copolymer constituting the first polymer flocculant of the present invention is produced by copolymerizing a plurality of monomers, including at least a cationic monomer, by living radical polymerization in the presence of an exchange chain transfer mechanism control agent. The polymerization method is preferably a method of polymerization by irradiation with active energy rays, particularly photopolymerization. Conventional polymerization conditions may be used.

[0070] The method for producing the cationic copolymer constituting the polymer flocculant of the first aspect of the present invention is described in detail below. First, an aqueous solution of monomers containing the above-mentioned cationic monomer, nonionic monomer, and other monomers is prepared. The monomer concentration in the aqueous solution is preferably 20 to 70% by mass, more preferably 30 to 60% by mass. If the monomer concentration is less than 20% by mass, the polymerization proceeds slowly, resulting in an increase in residual monomer in the product. If the monomer concentration exceeds 70% by mass, the polymerization proceeds rapidly and foaming due to water evaporation may occur, causing equipment problems. Next, the above-mentioned exchange chain transfer mechanism type controller is added to the aqueous monomer solution. The amount of exchange chain transfer mechanism type controller added is preferably 1 to 1,000 ppm, more preferably 3 to 100 ppm, and particularly preferably 5 to 50 ppm, relative to the total mass of the monomer components in the aqueous monomer solution. If the amount is less than 1 ppm, the effect of the exchange chain transfer mechanism type regulator is difficult to exhibit, and if the amount is more than 1,000 ppm, the molecular weight is likely to decrease.

[0071] Thereafter, dissolved oxygen in the aqueous monomer solution is removed using nitrogen gas or the like, and then the polymerization reaction is initiated. The polymerization reaction is initiated by adding a polymerization initiator to the aqueous monomer solution prepared by the above method. The polymerization initiation temperature, i.e., the temperature of the aqueous monomer solution at the start of polymerization, is preferably -5 to 30°C. When the monomer concentration is high, the polymerization initiation temperature is set lower, and when the monomer concentration is low, the polymerization initiation temperature is set higher. As the polymerization initiator, a redox polymerization initiator or a photopolymerization initiator is preferred.

[0072] The redox initiator can be prepared by combining a known oxidizing agent and a known reducing agent. Examples of the oxidizing agent include ammonium persulfate, potassium persulfate, hydrogen peroxide, and tertiary butyl hydroperoxide. Examples of the reducing agent include ferrous sulfate, ferrous ammonium sulfate, sodium hydrogen sulfite, and trimethylamine. The amount of the redox initiator added is preferably 1 to 200 ppm relative to the mass of the aqueous monomer solution, for both the oxidizing agent and the reducing agent. Polymerization can be initiated by adding aqueous solutions of the oxidizing agent and the reducing agent to the aqueous monomer solution immediately before the initiation of polymerization.

[0073] Examples of photopolymerization initiators include benzophenone, anthraquinone, acylphosphine oxide compounds, and azo compounds. The amount of photopolymerization initiator added is preferably 200 to 5,000 ppm relative to the mass of the aqueous monomer solution. Polymerization can be initiated by adding the photopolymerization initiator to the aqueous monomer solution and irradiating it with light containing light of the maximum absorption wavelength of the photopolymerization initiator. Examples of light sources include high-pressure mercury lamps and low-pressure mercury lamps. The light irradiation conditions, such as the wavelength, irradiation intensity, and irradiation time of the light used for photopolymerization, are not particularly limited. The light irradiation conditions may be adjusted appropriately depending on the type and amount of photopolymerization initiator used and the physical properties and performance of the polymer. When the water-soluble azo initiator is used as the photopolymerization initiator, light with a wavelength of around 365 nm is preferred, and the irradiation intensity should be 0.1 to 10.0 mW / cm as measured by a 365 nm UV illuminometer. 2 The irradiation time is preferably 0.1 to 3 hours.

[0074] An azo-based polymerization initiator may be added to the aqueous monomer solution in order to promote polymerization at high temperatures in the latter half of the polymerization reaction.

[0075] Examples of azo polymerization initiators include 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(3,4,5,6-tetrahydropyrimidinyl)propane] dihydrochloride, and Examples of the azobis(2-methyl-N-(2-hydroxyethyl)propane) dihydrochloride include dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanopentanoic acid), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]-propionamide, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], and 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide]. These may be used alone or in combination of two or more.

[0076] The amount of azo polymerization initiator added is preferably 100 ppm or more in total, particularly 200 to 10,000 ppm, based on the mass of the aqueous monomer solution. When the azo polymerization initiator is water-soluble, it may be added directly to the aqueous monomer solution, or the azo polymerization initiator may be prepared as an aqueous solution and then added. When the azo polymerization initiator is water-insoluble, polymerization may be difficult to initiate even when the azo polymerization initiator is added directly to the aqueous monomer solution. In this case, the azo polymerization initiator may be dissolved in a polar organic solvent, such as methanol, which has relatively low chain transfer properties and is easily miscible with water, and then added to the aqueous monomer solution. In addition to the aforementioned monomer and polymerization initiator, a chain transfer agent, a pH adjuster, and the like may also be added to the aqueous monomer solution as needed.

[0077] The polymerization reaction reaches a maximum temperature of 50 to 100°C within 30 minutes to 5 hours after the start of polymerization, and is almost completed. The aqueous solution containing the polymer obtained by the polymerization reaction is in a gel state at room temperature (hereinafter, this may be referred to as a "polymer gel").

[0078] The polymerization reaction can be carried out batchwise in a suitable reaction vessel, or can be carried out continuously by continuously pouring the aqueous monomer solution onto a belt such as a belt conveyor.

[0079] The polymer gel obtained by the above polymerization reaction may be subjected to heat treatment in order to reduce the content of residual monomers such as acrylamide. The heat treatment is carried out by heating the polymer gel in a reaction vessel or on a belt conveyor. Alternatively, the polymer gel is cut into appropriate sizes, sealed and packaged in vinyl bags, and then heated in a heating bath such as a hot water bath. The heat treatment conditions are preferably 70 to 100°C and 1 to 5 hours. The polymer gel after the heat treatment can be dried and pulverized by a known method to obtain a powdered cationic copolymer (polymer flocculant).

[0080] B. Second Invention 3. Polymer Flocculant The polymer flocculant of the second invention is primarily composed of a block copolymer of a polymer block (A) formed by polymerizing a monomer component (a) and a polymer block (B) formed by polymerizing a monomer component (b). The polymer block (A) is a nonionic unit having a structure derived from an exchange chain transfer mechanism control agent at its terminal, and the polymer block (B) is a hydrophilic cationic unit. This block copolymer is a block copolymer of the polymer block (A) and the polymer block (B), produced by radically polymerizing a monomer component (b) containing at least a cationic monomer in the presence of a prepolymer containing the polymer block (A) having a structure derived from an exchange chain transfer mechanism control agent at its terminal to form the polymer block (B).

[0081] The 0.5% by mass (polymer equivalent) salted viscosity at 25°C of the block copolymer constituting the polymer flocculant of the second invention is preferably 3.0 to 200 mPa·s, more preferably 5.0 to 90 mPa·s, and even more preferably 10 to 85 mPa·s. If it is less than 3.0 mPa·s, the molecular weight is small and the coagulation properties are poor. If it exceeds 200 mPa·s, the molecular weight is too large and the coagulation properties are similarly deteriorated. The 0.5% by mass (polymer equivalent) salted viscosity is as described in the first invention.

[0082] The insoluble content of the block copolymer constituting the polymer flocculant of the second invention in a 0.1% by mass aqueous solution is preferably 5.0% by mass or less, more preferably 4.0% by mass or less. If the insoluble content is high, the flocculation performance per added amount will be low.

[0083] (1) Polymer Block (A) The polymer block (A) is a polymer block obtained by radical polymerization of the monomer component (a), and is formed by bonding a structure derived from an exchange chain transfer mechanism inhibitor to its terminal. This polymer block (A) is a polymer block introduced by a prepolymer obtained by radical polymerization of the monomer component (a) in the presence of an exchange chain transfer mechanism inhibitor. That is, the second invention is a block copolymer of a polymer block (A) formed by polymerizing the monomer component (a) and a polymer block (B) formed by polymerizing the monomer component (b), in which the polymer block (A) is a polymer block introduced by a prepolymer obtained by radical polymerization of the monomer component (a) in the presence of an exchange chain transfer mechanism inhibitor. The polymer flocculant can also be characterized as comprising a block copolymer in which the polymer block (A) is a nonionic unit and the polymer block (B) is a cationic unit. This prepolymer will be described below.

[0084] The polymer block (A) has a structure derived from an exchange chain transfer mechanism type controller bonded to its terminal. In the second invention, the structure derived from the exchange chain transfer mechanism type controller is derived from the exchange chain transfer mechanism type controller and contains at least a part of the exchange chain transfer mechanism type controller. In the case of a RAFT agent, the structure derived from the exchange chain transfer mechanism type controller means a dithioester structure, a xanthate structure, a trithiocarbonate structure (hereinafter referred to as a "trithio structure"), a dithiocarbamate compound (collectively referred to as an S-containing structure), and / or an organic group bonded to the S-containing structure. For example, the exchange chain transfer mechanism type controller is represented by the following chemical formula (1):

[0085]

[0086] In this case, the terminal of the polymer block (A) is an organic group (i.e., R 3 or R 4 In other words, the polymer block (A) has an organic group (i.e., R 3 or R 4 The terminal structure of the polymer block (A) may be at least one selected from the group consisting of a trithio structure, a trithio structure, and a composite group of an organic group bonded to the trithio structure and a trithio structure, and may also be a mixture of these. In the case of a RAFT agent, the terminal structure of the polymer block (A) is an organic group bonded to the S-containing structure, or a composite group of an organic group bonded to the S-containing structure and an S-containing structure, and more preferably an organic group bonded to the S-containing structure.

[0087] The exchange chain transfer mechanism type regulator is as explained in the first invention.

[0088] The amount of the exchange chain transfer mechanism type regulator used can be appropriately adjusted depending on the type of the monomer component (a) and the exchange chain transfer mechanism type regulator used, etc. Generally, it is 0.01 to 20 mol %, preferably 0.02 to 10 mol %, and more preferably 0.05 to 5 mol %, based on the total amount of the monomer component (a).

[0089] The monomer component (a) that undergoes radical polymerization in the presence of an exchange chain transfer mechanism control agent may be selected depending on the compatibility with the exchange chain transfer mechanism control agent and the degree of hydrophobicity to be imparted to the final polymer flocculant. The compatibility with the exchange chain transfer mechanism control agent can be selected in consideration of the monomer conversion rate, etc. Specific examples include (meth)acrylic acid alkyl ester compounds, (meth)acrylic acid aliphatic cyclic ester compounds, (meth)acrylic acid aromatic ester compounds, and compounds represented by the following chemical formula (3): CH 2 =CR 1 -C(=O)O-(R 2 O) n -R 3 ...Chemical formula (3) (wherein, R 1 represents a hydrogen atom or a methyl group, R 2 represents a linear or branched alkylene group having 2 to 6 carbon atoms; R 3 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms; and n represents an integer of 1 to 100), styrene-based compounds, maleimide compounds, amide group-containing vinyl compounds, and vinyl-based monomers having a crosslinkable functional group.

[0090] Specific examples of the (meth)acrylic acid alkyl ester compound include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and icosyl (meth)acrylate.

[0091] Specific examples of the aliphatic cyclic ester compound of (meth)acrylic acid include cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentanyl (meth)acrylate.

[0092] Specific examples of aromatic ester compounds of (meth)acrylic acid include phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxymethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, and 3-phenoxypropyl (meth)acrylate.

[0093] Examples of the compound in which n is 1 in the above chemical formula (3) include (meth)acrylic acid alkoxyalkyl ester compounds and (meth)acrylic acid hydroxyalkyl ester compounds.

[0094] The (meth)acrylic acid alkoxyalkyl ester compound has an oxyalkylene structure (for example, an oxyethylene chain, an oxypropylene chain, an oxybutylene chain, etc.). Specific examples of the (meth)acrylic acid alkoxyalkyl ester compound include methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, n-propoxyethyl (meth)acrylate, n-butoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, ethoxypropyl (meth)acrylate, n-propoxypropyl (meth)acrylate, n-butoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxybutyl (meth)acrylate, n-propoxybutyl (meth)acrylate, and n-butoxybutyl (meth)acrylate.

[0095] Specific examples of the (meth)acrylic acid hydroxyalkyl ester compound include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.

[0096] When n in the above chemical formula (3) is 2 or more, the compound represented by the above chemical formula (3) has a polyoxyalkylene structure (for example, a polyoxyethylene chain, a polyoxypropylene chain, a polyoxybutylene chain, etc.). When n is 2 or more, two or more R 2 may be the same or different from each other. Therefore, a compound in which n is 2 or more in the above chemical formula (3) may have different types of polyoxyalkylene structures in one molecule, such as a block structure consisting of polyoxyethylene / polyoxypropylene.

[0097] Specific examples of the compound in which n in the above chemical formula (3) is 2 or more include polyoxyethylene (meth)acrylate, polyoxypropylene (meth)acrylate, polyoxybutylene (meth)acrylate, polyoxyethylene-polyoxypropylene (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, lauroxypolyethylene glycol (meth)acrylate, stearoxypolyethylene glycol (meth)acrylate, octoxypolyethylene glycol polypropylene glycol (meth)acrylate, nonylphenoxypolypropylene glycol (meth)acrylate, and phenoxypolyethylene glycol polypropylene glycol (meth)acrylate.

[0098] Specific examples of the styrene-based compound include styrene, α-methylstyrene, β-methylstyrene, vinylxylene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, p-n-butylstyrene, p-isobutylstyrene, p-t-butylstyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, p-hydroxystyrene, m-hydroxystyrene, o-hydroxystyrene, p-isopropenylphenol, m-isopropenylphenol, o-isopropenylphenol, o-vinylbenzoic acid, m-vinylbenzoic acid, p-vinylbenzoic acid, divinylbenzene, and vinylnaphthalene.

[0099] Specific examples of the maleimide compound include maleimide and N-substituted maleimide compounds. Examples of the N-substituted maleimide compound include N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-ethylmaleimide, N-n-propylmaleimide, N-isopropylmaleimide, N-n-butylmaleimide, N-isobutylmaleimide, N-tert-butylmaleimide, N-pentylmaleimide, N-hexylmaleimide, N-heptylmaleimide, N-octylmaleimide, N-laurylmaleimide, and N-stearylmaleimide; N-cyclopentylmaleimide; N-cycloalkyl-substituted maleimide compounds such as N-cyclohexylmaleimide and N-cycloalkyl-substituted maleimide compounds such as N-phenylmaleimide, N-(4-hydroxyphenyl)maleimide, N-(4-acetylphenyl)maleimide, N-(4-methoxyphenyl)maleimide, N-(4-ethoxyphenyl)maleimide, N-(4-chlorophenyl)maleimide, N-(4-bromophenyl)maleimide, and N-benzylmaleimide.

[0100] Specific examples of amide group-containing vinyl compounds include (meth)acrylamide, (meth)acrylamide derivatives, and N-vinylamide monomers. Of these, specific examples of (meth)acrylamide derivatives include tert-butyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, and (meth)acryloylmorpholine. Specific examples of N-vinylamide monomers include N-vinylacetamide, N-vinylformamide, and N-vinylisobutylamide.

[0101] Regarding the vinyl monomer having a crosslinkable functional group, examples of the crosslinkable functional group include a crosslinkable silyl group, a silanol group, a carboxyl group, a hydroxy group, an epoxy group, an oxazoline group, an isocyanate group, and a polymerizable unsaturated group. Examples of the crosslinkable silyl group include an alkoxysilyl group and a halogenosilyl group. Among these, an alkoxysilyl group is preferred in terms of ease of control of reactivity, and examples thereof include a trimethoxysilyl group, a methyldimethoxysilyl group, a dimethylmethoxysilyl group, a triethoxysilyl group, a methyldiethoxysilyl group, and a dimethylethoxysilyl group.

[0102] Specific examples of vinyl monomers having a crosslinkable functional group include crosslinkable silyl group-containing vinyl compounds, unsaturated carboxylic acids, unsaturated acid anhydrides, hydroxy group-containing vinyl compounds, epoxy group-containing vinyl compounds, primary or secondary amino group-containing vinyl compounds, oxazoline group-containing vinyl compounds, and isocyanate group-containing vinyl compounds.

[0103] Examples of crosslinkable silyl group-containing vinyl compounds include vinyl silanes such as vinyltrimethoxysilane, vinyltriethoxysilane, vinylmethyldimethoxysilane, and vinyldimethylmethoxysilane; alkoxysilyl group-containing (meth)acrylic acid esters such as trimethoxysilylpropyl (meth)acrylate, triethoxysilylpropyl (meth)acrylate, methyldimethoxysilylpropyl (meth)acrylate, and dimethylmethoxysilylpropyl (meth)acrylate; alkoxysilyl group-containing vinyl ethers such as trimethoxysilylpropyl vinyl ether; and alkoxysilyl group-containing vinyl esters such as vinyl trimethoxysilylundecanoate. Crosslinkable silyl group-containing vinyl compounds form a crosslinked structure by dehydration condensation between crosslinkable silyl groups, and are therefore suitable in that they can efficiently carry out the polymerization reaction when producing a polymer and the subsequent crosslinking reaction.

[0104] Examples of unsaturated carboxylic acids include (meth)acrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, citraconic acid, cinnamic acid, and monoalkyl esters of unsaturated dicarboxylic acids (monoalkyl esters of maleic acid, fumaric acid, itaconic acid, citraconic acid, etc.). Examples of unsaturated acid anhydrides include maleic anhydride, itaconic anhydride, citraconic anhydride, etc.

[0105] Examples of the hydroxy group-containing vinyl compound include the above-mentioned (meth)acrylic acid hydroxyalkyl ester compounds, (meth)acrylic acid esters of polyalkylene glycols (for example, polyethylene glycol, polypropylene glycol, etc.); styrene-based compounds such as o-hydroxystyrene, m-hydroxystyrene, and p-hydroxystyrene; and maleimide compounds such as N-(4-hydroxyphenyl)maleimide.

[0106] Examples of epoxy group-containing vinyl compounds include glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclohexylmethyl (meth)acrylate, etc. The vinyl monomer constituting the polymer (PA) may be one or more of the above.

[0107] The polymer block (A) formed by this monomer component (a) constitutes the nonionic unit of the final polymer flocculant and adjusts the affinity of the polymer flocculant for water and sludge. To form a polymer with the cationic polymer block (B), the polymer block (A) is preferably water-soluble, although more hydrophobic than the polymer block (B). Generally, the monomer component (a) is preferably a compound represented by the above chemical formula (3). A preferred commercially available product is Blemmer AME-400 manufactured by NOF Corporation, as described in the Examples.

[0108] The weight-average molecular weight (Mw) of this prepolymer, as measured by gel permeation chromatography (GPC), is preferably 1,000 to 300,000, more preferably 1,000 to 100,000, and particularly preferably 1,200 to 100,000. If it is less than 1,000, the characteristics of the nonionic unit are unlikely to be reflected in the final polymer flocculant. In other words, the effect of modification is diminished. If it exceeds 300,000, it becomes difficult to produce a highly pure prepolymer. Furthermore, separation is likely to occur when used to produce a high-molecular-weight water-soluble polymer.

[0109] The prepolymer preferably has a number average molecular weight (Mn) of 1,000 to 300,000, more preferably 1,000 to 100,000, and particularly preferably 1,200 to 100,000, as measured by gel permeation chromatography (GPC) in terms of polystyrene (hereinafter referred to as pSt).

[0110] The molecular weight distribution (Mw / Mn), which is the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is not particularly limited, but is, for example, 1.00 to 3.00, preferably 1.05 to 2.50, and particularly preferably 1.10 to 1.50. If it is within this range, the quality of the polymer flocculant produced using this prepolymer can be easily stabilized.

[0111] (2) Method for Producing Prepolymer The prepolymer can be produced by polymerizing the monomer component (a) in a known polymerization solvent in the presence of the chain exchange transfer mechanism controller and the polymerization initiator.

[0112] The polymerization solvent used may be, for example, a solvent capable of dissolving the monomer component (a). Examples of the polymerization solvent include organic solvents and water. Examples of the organic solvent include aromatic compounds such as benzene, toluene, xylene, and anisole; ester compounds such as methyl acetate, propyl acetate, and butyl acetate; ketone compounds such as acetone, methyl ethyl ketone, and cyclohexanone; and alcohols such as methanol and ethanol. Considering that the polymerization will be carried out in an aqueous solution in a subsequent step, water is the most preferred polymerization solvent. When using an organic solvent, methanol, ethyl acetate, and acetonitrile are preferred because they are less likely to cause a chain transfer reaction in radical polymerization and have a boiling point of less than 100°C, making water substitution in a subsequent step easy.

[0113] The amount of the polymerization solvent used is preferably 5 to 200 parts by mass, more preferably 10 to 100 parts by mass, per 100 parts by mass of the total amount of the monomer component (a) used in the reaction. When the amount of the polymerization solvent used is 200 parts by mass or less, it is preferable in that a high polymerization rate can be achieved in a short time.

[0114] The radical polymerization initiator used in the polymerization reaction is not particularly limited. For example, persulfates such as potassium persulfate and ammonium persulfate, organic peroxides such as t-butyl hydroperoxide, azo initiators, redox initiators, and photopolymerization initiators can be used as appropriate. Among these, azo initiators are preferred because they are easy to handle and do not easily cause side reactions during radical polymerization. These radical polymerization initiators may be used alone or in combination of two or more.

[0115] Specific examples of the azo-based initiator are as explained in the first aspect of the present invention.

[0116] The amount of polymerization initiator added is not particularly limited and may be adjusted appropriately depending on the type of polymerization initiator and the composition of the monomer component (a). From the viewpoint of obtaining a prepolymer with a narrower molecular weight distribution, the amount is preferably 0.5 mol or less, and more preferably 0.4 mol or less, per mol of the exchange chain transfer mechanism inhibitor. Furthermore, from the viewpoint of stably carrying out the polymerization reaction, the amount is preferably 0.01 mol or more, and more preferably 0.03 mol or more, per mol of the exchange chain transfer mechanism inhibitor. The amount of polymerization initiator used per mol of the exchange chain transfer mechanism inhibitor is preferably 0.01 to 0.5 mol, and more preferably 0.03 to 0.4 mol.

[0117] The polymerization reaction may be carried out in the presence of a chain transfer agent (for example, an alkylthiol compound having 2 to 20 carbon atoms) as needed.

[0118] The reaction temperature during polymerization is not particularly limited, but from the viewpoints of suppressing side reactions during polymerization to obtain a prepolymer with a narrow molecular weight distribution, obtaining a prepolymer with little variation in physical properties between lots, and easing restrictions on the polymerization initiator and solvent that can be used, it is preferably 100°C or lower, more preferably 90°C or lower, and even more preferably 80°C or lower. Furthermore, from the viewpoint of smoothly progressing the polymerization reaction, the reaction temperature is preferably 40°C or higher, more preferably 45°C or higher, and even more preferably 50°C or higher. The reaction time in the polymerization reaction can be appropriately set depending on the monomers used, etc., but is preferably 1 hour to 48 hours, more preferably 2 hours to 24 hours, and even more preferably 2 hours to 12 hours.

[0119] (3) Polymer Block (B) The polymer block (B) is a polymer block formed by radical polymerization of a monomer component (b) containing at least a cationic monomer. By radically polymerizing the monomer component (b) containing at least a cationic monomer in the presence of the prepolymer, a block copolymer of a polymer block (A) derived from the prepolymer and a polymer block (B) is formed. The terminals of the polymer block (B) may have the terminal structure of the prepolymer, i.e., a structure derived from the exchange chain transfer mechanism controller.

[0120] The monomer component (b) for forming the polymer block (B) can be appropriately selected depending on the properties to be imparted to the polymer flocculant and its application. The monomer component (a) constituting the polymer block (A) and the monomer component (b) constituting the polymer block (B) are different (not completely identical) monomer components. Specifically, they contain at least a cationic monomer described below, and can also use a nonionic monomer and an anionic monomer, etc., as necessary.

[0121] The cationic monomer may be a compound represented by the following chemical formula (2): 2 =CR 1 -CO-X-Q-N+R 2a R 2b R 2c ・Z - ...Chemical formula (2) (However, in chemical formula (2), R 1 is a hydrogen atom or a methyl group, R 2a and R 2b are each independently an alkyl group having 1 to 3 carbon atoms or a benzyl group, R 2c represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different. X represents an oxygen atom or NH, Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms, Z - and each represent a counter anion.

[0122] Specific examples of the (meth)acrylate monomer represented by the above chemical formula (2) are as explained in the first invention.

[0123] The polymer block (B) preferably contains 50 to 100 mol %, more preferably 55 to 95 mol %, and particularly preferably 60 to 90 mol % of the cationic monomer unit. If the molar fraction of the cationic monomer is outside the above range, the coagulation property may decrease.

[0124] The high molecular weight water-soluble polymer (polymer flocculant) produced in the second invention may be a copolymer of the above-mentioned cationic monomer and nonionic monomer. The nonionic monomer is not particularly limited, but examples thereof include (meth)acrylamide compounds represented by the following chemical formula (4), as well as alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and hydroxyethyl (meth)acrylate, styrene, acrylonitrile, and vinyl acetate. Among these nonionic monomers, those having excellent copolymerizability with cationic monomers, easy to increase the molecular weight required for polymer flocculants, and excellent performance as polymer flocculants are preferred, as represented by the following chemical formula (4): CH 2 =CR 1 -CO-NR 2 R 3 ...Chemical formula (4) (wherein, in the above chemical formula (4), R 1 is a hydrogen atom or a methyl group, and R 2 and R 3 and each independently represent a hydrogen atom or an alkyl group having 1 to 8 carbon atoms.

[0125] Among these (meth)acrylamide compounds, acrylamide (AM) is most preferred because it is water-soluble and has particularly excellent performance as a polymer flocculant. These nonionic monomers may be used alone or in combination of two or more.

[0126] The polymer block (B) preferably contains 0 to 50 mol %, more preferably 5 to 45 mol %, and particularly preferably 10 to 40 mol % of the nonionic monomer unit. If the molar fraction of the nonionic monomer is outside the above range, it is difficult to exhibit the effect on a wide range of sludge properties.

[0127] Examples of anionic monomers include (meth)acrylic acid and salts thereof represented by the following chemical formula (5), as well as vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, maleic acid, and salts thereof. Among these anionic monomers, the following chemical formula (5): CH 2 =CR 1 -CO-OM... Chemical formula (5) (wherein, in chemical formula (5), R 1 is a hydrogen atom or a methyl group, and M is a hydrogen atom, an ammonium group, or an alkali metal atom.) Preferred salts of (meth)acrylic acids are those represented by the following formula: and salts thereof. Preferred salts are ammonium salts and alkali metal salts such as sodium salts and potassium salts.

[0128] Among these (meth)acrylic acids and their salts, acrylic acid (AA) and its ammonium salts are most preferred because of their particularly excellent performance as polymer flocculants. These anionic monomers may be used alone or in combination of two or more.

[0129] The polymer block (B) preferably contains anionic monomer units in an amount of 0 to 50 mol %, more preferably 0 to 40 mol %, and particularly preferably 0 to 30 mol %.

[0130] 4. Second Method for Producing Polymer Flocculant The second polymer flocculant of the present invention is produced by radically polymerizing the monomer component (b) for forming the polymer block (B) in a solution in the presence of the above-mentioned prepolymer. That is, the polymer is produced by radically polymerizing the monomer component (b) for forming the polymer block (B) using the above-mentioned prepolymer as a macrochain transfer agent. As the radical polymerization method, a method of polymerization by irradiation with active energy rays, particularly photopolymerization, is preferred. Conventional known conditions may be used as the polymerization conditions.

[0131] First, an aqueous monomer solution of monomer component (b) containing a cationic monomer, a nonionic monomer, and other monomers is prepared. The monomer concentration in the aqueous solution is 20 to 70% by mass, preferably 30 to 60% by mass. If the monomer concentration is less than 20% by mass, the polymerization proceeds slowly, resulting in an increase in residual monomer in the product. If the monomer concentration exceeds 70% by mass, the polymerization proceeds rapidly and foaming occurs due to water evaporation, which may cause equipment problems. Next, the above-mentioned prepolymer is added to the aqueous monomer solution. The amount of prepolymer added is preferably 10 to 100,000 ppm, more preferably 100 to 50,000 ppm, based on the total mass of monomer component (b) in the aqueous monomer solution.

[0132] Thereafter, dissolved oxygen in the aqueous monomer solution is removed using nitrogen gas or the like, and then the polymerization reaction is initiated. The polymerization reaction is initiated by adding a polymerization initiator to the aqueous monomer solution prepared by the above method. The polymerization initiation temperature, i.e., the temperature of the aqueous monomer solution at the start of polymerization, is preferably -5 to 30°C. When the monomer concentration is high, the polymerization initiation temperature is set lower, and when the monomer concentration is low, the polymerization initiation temperature is set higher. As the polymerization initiator, a redox polymerization initiator or a photopolymerization initiator is preferred. The type and amount of the redox polymerization initiator or photopolymerization initiator, as well as other conditions, are as explained in the first invention.

[0133] An azo-based polymerization initiator may be added to the aqueous monomer solution in order to promote polymerization at high temperatures in the latter half of the polymerization reaction.

[0134] The type, amount and conditions of addition of the azo polymerization initiator are as explained in the first invention.

[0135] The polymerization reaction reaches a maximum temperature of 50 to 100°C within 30 minutes to 5 hours after the start of polymerization, and is almost completed. The aqueous solution containing the polymer obtained by the polymerization reaction is in a gel state at room temperature (hereinafter, this may be referred to as a "polymer gel").

[0136] The polymerization reaction can be carried out batchwise in a suitable reaction vessel, or can be carried out continuously by continuously pouring the aqueous monomer solution onto a belt such as a belt conveyor.

[0137] The polymer gel obtained by the above polymerization reaction may be subjected to heat treatment in order to reduce the content of residual monomers such as acrylamide. The heat treatment method and conditions are as described in the first invention. The polymer gel after the heat treatment can be dried and pulverized by a known method to obtain the present polymer flocculant in powder form.

[0138] 3. Sludge Dewatering Method The sludge dewatering method of the present invention is characterized by adding at least one polymer flocculant obtained by the production method of the present invention to various sludges and then dewatering them. The sludge to be treated is not particularly limited, but examples include sludge generated in sewage treatment, human waste treatment, and domestic wastewater treatment, as well as sludge generated in various industrial wastewater treatment processes at food factories, meat processing plants, and chemical plants, raw human waste generated in livestock farms such as pig farms and sludge generated in wastewater treatment therefor, and sludge generated in the pulp or paper industry. The type of sludge is also not limited, and primary settling sludge, excess sludge, and mixed sludges thereof, thickened sludge, and digested sludge treated with anaerobically microbial agents can all be treated.

[0139] Specific examples of sludge dewatering methods include the following: An inorganic flocculant or the like is added to the sludge as needed, the pH is adjusted, and then the polymer flocculant of the present invention is added. The sludge is stirred and / or mixed by a known method, allowing the polymer flocculant to act on suspended matter in the sludge to form sludge flocs. The formed sludge flocs are mechanically dehydrated by known means to separate them into treated water and dehydrated cake. The amount of the polymer flocculant of the present invention added is preferably 0.1 to 10,000 ppm by mass of cationic copolymer relative to the mass of sludge. The dewatering apparatus is not particularly limited, but examples include a screw press dehydrator, a belt press dehydrator, a filter press dehydrator, a screw decanter, and a multi-disc dehydrator.

[0140] Examples of the polymer flocculant and sludge dewatering method of the present invention will be specifically described below. The present invention is not limited to these examples. Various analyses and evaluations were carried out by the following methods.

[0141] [0.5% Salt Viscosity] 500 g of pure water was placed in a 500 mL conical beaker, and 20.8 g of accurately weighed first-grade reagent sodium chloride powder was added and dissolved. While stirring with a magnetic stirrer, a powder sample of a cationic copolymer was added, weighed accurately in an amount such that the concentration after dissolution would be 0.5% by mass in terms of solid content. The mixture was stirred at 200 rpm for 4 hours, and then allowed to stand to dissolve sufficiently to prepare a 0.5% by mass solution. The viscosity was measured using a BM-type viscometer manufactured by Tokyo Keiki Inc. at 25°C, 60 rpm, and after 5 minutes.

[0142] [0.1% Insoluble Content] 400 g of pure water was placed in a 500 mL conical beaker, and while stirring with a magnetic stirrer, each powder sample was added in an amount accurately weighed so that the concentration after dissolution would be 0.1% by mass in terms of solid content. After stirring for 2 hours, the mixture was left to stand sufficiently for dissolution to prepare a polymer solution with a concentration of 0.1%. This was then suction-filtered using an 83-mesh filter cloth, and the volume (mL) of the residue on the filter cloth was measured using a measuring cylinder, and the content of insoluble content was calculated from this volume.

[0143] Spinnability in 1.0% Aqueous Solution: 500 g of pure water was placed in a 500 mL conical beaker, and while stirring with a magnetic stirrer, 5.0 g of an accurately weighed powder sample of the cationic copolymer was added. The mixture was stirred at 200 rpm for 4 hours, and then allowed to stand to dissolve, preparing a 1.0% by mass sample solution. The spinnability was measured under the following conditions using a spinnability measuring device (manufactured by Abe Iron Works Co., Ltd., model number ST-300). (Measurement conditions) Diameter of glass bead in contact with liquid: 10 mm, Immersion depth: 27 mm, Descending distance: 300 mm, Apparatus descending speed: 4.8 mm / sec. The time (Tc (seconds)) until the thread broke was measured, with the moment when the lower limit of the glass bead separated from the liquid surface of the sample solution being set as time 0. Measurements were taken at seven different sampling locations, the maximum and minimum values ​​were excluded, and the length of the drawn thread was calculated from the average value of the five measurements using the following formula: Length of drawn thread (mm) = Device descending speed (mm / sec) x Tc (sec)

[0144] [Floc diameter] Evaluated visually.

[0145] [Appearance of filtrate] Visual evaluation was performed according to the following criteria. The ratings "2" and "4" respectively mean intermediate between the ratings "1" and "3" and between the ratings "3" and "5" (the same applies below). 1: A large amount of suspended matter was observed in the filtrate. 3: Suspended matter was observed in the filtrate. 5: No suspended matter was observed in the filtrate, and the filtrate was almost transparent.

[0146] [Strength of flocculated floc] After measuring the filtration rate, the cake was collected and the degree of hand squeezing was evaluated according to the following criteria: 1: Floc cake leaked through the fingers on the first hand squeezing. 3: Floc cake leaked through the fingers on the second hand squeezing. 5: Floc cake did not leak through the fingers on the third hand squeezing, and filtrate was squeezed out.

[0147] [First Invention] [Production of Polymer Flocculant] (Example 1) A stainless steel tray with a Teflon (registered trademark) coated inner surface was used as a reaction vessel, and an aqueous monomer solution was charged therein. The composition of the aqueous monomer solution was: a 78% by mass aqueous solution of dimethylaminoethyl acrylate methyl chloride quaternary salt (hereinafter abbreviated as "DAC") in an amount of 80 mol% based on the total monomers; a 40% by mass aqueous solution of acrylamide (hereinafter abbreviated as "AMD") in an amount of 20 mol% based on the total monomers; 5 ppm of 3-((((1-carboxyethyl)thio)carbonothioyl)thio)propanoic acid as a chain transfer agent; and the remainder being distilled water. The monomer concentration of the aqueous monomer solution was 58% by mass, and the total amount of the aqueous monomer solution was 1,160 g. While maintaining the temperature of this aqueous monomer solution at 5°C, dissolved oxygen was removed with nitrogen. Then, under a nitrogen gas flow, 2,2'-azobis(2-aminodipropane) dihydrochloride was added so that the amount was 300 ppm in terms of solid content relative to the total mass of each monomer. Next, a black light fluorescent lamp manufactured by Toshiba Corporation, which radiates light from 300 to 450 nm with a peak wavelength of 352 nm, was measured at 0.40 mW / cm using a UV meter UIT-150 (UVD-S365) manufactured by Ushio Inc., through a 5 mm thick borosilicate glass (manufactured by Corning Incorporated, product name: Pyrex) as a light-transmitting material. 2 After the start of exposure, the substrate was exposed to light for 20 minutes, and then the exposure intensity was increased to 2.0 mW / cm 2The lamp conditions were changed so that the temperature was 0.5% and the light irradiation was continued for another 40 minutes to obtain a hydrogel. The hydrogel was shredded, dried, and pulverized to obtain a powder sample of the target cationic copolymer (polymer flocculant). The powder sample was measured for its 0.5% salt viscosity and spinnability in a 1.0% aqueous solution. The results are shown in Table 1.

[0148] (Examples 2 to 4, Comparative Examples 1 to 3) Powder samples of cationic copolymers (polymer flocculants) were obtained in the same manner as in Example (1), except that the type and amount of chain transfer agent added were changed. The powder samples were measured for 0.5% salted viscosity and spinnability in a 1.0% aqueous solution. The results are shown in Table 1.

[0149]

[0150] The abbreviations used in Table 1 are as follows: A1: 3-((((1-carboxyethyl)thio)carbonothioyl)thio)propanoic acid A2: S,S-dibenzyltrithiocarbonate A3: Sodium hydrogen sulfite

[0151] Example 1 and Comparative Example 1 had similar 0.5% salted viscosities. This means that the average molecular weights were almost the same. On the other hand, Example 1 used an exchange chain transfer mechanism type controller as the chain transfer agent, and therefore exhibited lower spinnability than Comparative Example 1, which used sodium sulfite as the chain transfer agent. This means that the cationic copolymer of Example 1 had a narrow molecular weight distribution. Example 2 and Comparative Example 2, and Example 3 and Comparative Example 3 also showed similar trends.

[0152] Example 5 A Dewar vessel with a Teflon (registered trademark)-coated interior was used as a reaction vessel, and an aqueous monomer solution was charged therein. The composition of the aqueous monomer solution was as follows: DAC in an amount that was 15 mol% relative to the total monomers; 40% by mass AMD in an amount that was 85 mol% relative to the total monomers; 5 ppm of 3-((((1-carboxyethyl)thio)carbonothioyl)thio)propanoic acid as a chain transfer agent; and the remainder being distilled water. The monomer concentration of the aqueous monomer solution was 30% by mass, and the total amount of the aqueous monomer solution was 1,500 g. While maintaining the temperature of this aqueous monomer solution at 8°C, dissolved oxygen was removed with nitrogen. Thereafter, under a nitrogen stream, copper(II) chloride dihydrate, 2,2'-azobis(2-aminodipropane) dihydrochloride, ammonium peroxodisulfate, and sodium hydrogensulfite were added in specified amounts, calculated as solids relative to the total mass of each monomer. The amounts added are shown in Table 2. The temperature was recorded from the start of polymerization, and the polymerization time was recorded as the time until the temperature no longer rose. After the completion of polymerization, the mixture was allowed to stand for an additional 100 minutes to obtain a hydrogel-like substance. The hydrogel-like substance was shredded, dried, and pulverized to obtain a powder sample of the desired cationic copolymer (polymer flocculant). The powder sample was measured for 0.5% salt viscosity and spinnability in a 1.0% aqueous solution. The results are shown in Table 2.

[0153] (Example 6, Comparative Example 4) A powder sample of a cationic copolymer (polymer flocculant) was obtained in the same manner as in Example (5), except that the monomer concentration and the amount of each additive were changed. The powder sample was measured for 0.5% salt viscosity and spinnability in a 1.0% aqueous solution. The results are shown in Table 2.

[0154]

[0155] The abbreviations used in Table 2 are as follows: B1: Copper(II) chloride dihydrate B2: 2,2'-azobis(2-aminodipropane) dihydrochloride B3: Ammonium peroxodisulfate B4: 3-((((1-carboxyethyl)thio)carbonothioyl)thio)propanoic acid B5: Sodium hydrogen sulfite

[0156] Example 5 and Comparative Example 4 had similar 0.5% salted viscosities. This means that the average molecular weights were almost the same. On the other hand, Example 5 used an exchange chain transfer mechanism type regulator as the chain transfer agent, and therefore had lower spinnability than Comparative Example 4. Example 6 and Example 5 had similar spinnability. This means that the cationic copolymers of Examples 5 and 6 had narrow molecular weight distributions.

[0157] Example 7 A Dewar vessel with a Teflon (registered trademark)-coated interior was used as a reaction vessel, and an aqueous monomer solution was charged therein. The composition of the aqueous monomer solution was as follows: DAC in an amount that was 20 mol% relative to the total monomers; 40% by mass AMD in an amount that was 80 mol% relative to the total monomers; 10 ppm of 3-((((1-carboxyethyl)thio)carbonothioyl)thio)propanoic acid as a chain transfer agent; and the remainder being distilled water. The aqueous monomer solution had a monomer concentration of 30% by mass, and a total volume of 1,500 g. While maintaining the aqueous monomer solution at a temperature of 10°C, dissolved oxygen was removed with nitrogen. Thereafter, under a nitrogen stream, copper(II) chloride dihydrate, 2,2'-azobis(2-aminodipropane) dihydrochloride, ammonium peroxodisulfate, and sodium hydrogensulfite were added in specified amounts, calculated as solids relative to the total mass of each monomer. The amounts added are shown in Table 3. The temperature was recorded from the start of polymerization, and the polymerization time was recorded as the time until the temperature no longer rose. After the completion of polymerization, the mixture was allowed to stand for an additional 100 minutes to obtain a hydrogel-like substance. The hydrogel-like substance was shredded, dried, and pulverized to obtain a powder sample of the desired cationic copolymer (polymer flocculant). The powder sample was measured for 0.5% salt viscosity and spinnability in a 1.0% aqueous solution. The results are shown in Table 3.

[0158] (Examples 8 to 9, Comparative Example 5) A powder sample of a cationic copolymer (polymer flocculant) was obtained in the same manner as in Example 7, except that the monomer concentration and the amount of each additive added were changed. The powder sample was measured for 0.5% salted viscosity and spinnability in a 1.0% aqueous solution. The results are shown in Table 3.

[0159]

[0160] The abbreviations used in Table 3 are as follows: B1: Copper(II) chloride dihydrate B2: 2,2'-azobis(2-aminodipropane) dihydrochloride B3: Ammonium peroxodisulfate B4: 3-((((1-carboxyethyl)thio)carbonothioyl)thio)propanoic acid B5: Sodium hydrogen sulfite

[0161] Example 7 and Comparative Example 5 had similar 0.5% salted viscosities. This means that the average molecular weights were almost the same. On the other hand, Example 8 used an exchange chain transfer mechanism inhibitor as the chain transfer agent, and therefore had lower spinnability than Comparative Example 5. This means that the cationic copolymer of Example 7 had a narrower molecular weight distribution. Examples 8 and 9 had similar 0.5% salted viscosities. This means that the average molecular weights were almost the same. On the other hand, Example 8 had lower spinnability than Example 9 because the concentration of the exchange chain transfer mechanism inhibitor was twice that of Example 9. This means that the cationic copolymer of Example 8 had a narrower molecular weight distribution.

[0162] [Sludge Dehydration Test 1] A sludge dehydration test was carried out using the polymer flocculants produced in Examples 2 and 4 and Comparative Example 2. The sludge used was mixed sludge from sewage treatment plant "G." The physical properties of the sludge were pH = 4.65, TS (total evaporation residue) = 30,600 (ppm), and crude suspended matter (relative to SS (suspended solids)) = 16.4%.

[0163] 200 mL of sludge was collected in a 300 mL beaker, and a predetermined amount of polymer flocculant dissolved at 0.2% by mass was added. The mixture was stirred for 30 seconds in a jar tester to allow for flocculation. The flocculated sludge was poured into a stainless steel sieve with an inner diameter of 75 mm, a depth of 100 mm, and an opening of 80 mesh, and gravity filtered. The volume of the filtrate was measured after 5, 10, 20, and 30 seconds using a measuring cylinder. The liquid volume (mL) after 10 seconds and the observation results are shown in Table 4, and flocculation performance was compared and evaluated. The sludge was also dehydrated for 10 minutes at 1,000 rpm using a laboratory centrifuge, dried overnight in a dryer at 110 °C, and the moisture content of the dehydrated cake was measured. The results are shown in Table 4.

[0164]

[0165] At any addition amount between 100 and 160 ppm, the polymer flocculants of Examples 2 and 4 exhibited superior performance to the polymer flocculant of Comparative Example 2, and it can be seen that the polymer flocculant of the present invention can be used in a wide range of addition amounts.

[0166] [Sludge Dehydration Test 2] A sludge dehydration test was carried out using the polymer flocculants produced in Example 3 and Comparative Example 3. The sludge used was mixed sludge containing digested sludge from sewage treatment plant "O." The physical properties of the sludge were pH = 7.5, TS (total evaporation residue) = 11,300 (ppm), and crude suspended matter (relative to SS (suspended solids)) = 5.4%.

[0167] 200 mL of sludge was collected in a 300 mL beaker, and a predetermined amount of polymer flocculant dissolved at 0.2% by mass was added. The mixture was stirred for 30 seconds in a jar tester to allow for flocculation. The flocculated sludge was poured into a stainless steel sieve with an inner diameter of 75 mm, a depth of 100 mm, and an opening of 80 mesh, and gravity filtered. The volume of the filtrate was measured after 5, 10, 20, and 30 seconds using a measuring cylinder. The liquid volume (mL) after 10 seconds and the observation results are shown in Table 5, and flocculation performance was compared and evaluated. The sludge was dehydrated for 10 minutes at 1,000 rpm using a laboratory centrifuge, dried overnight in a dryer at 110 °C, and the moisture content of the dehydrated cake was measured. The results are shown in Table 5.

[0168]

[0169] At any addition amount between 120 and 180 ppm, the polymer flocculant of Example 3 exhibits superior performance to the polymer flocculant of Comparative Example 3, and it can be seen that the polymer flocculant of the present invention can be used in a wide range of addition amounts.

[0170] [Sludge Dehydration Test 3] A sludge dehydration test was carried out using the polymer flocculants produced in Example 6 and Comparative Example 4. The physical properties of the sludge were pH = 7.22, TS (total evaporation residue) = 9,700 (ppm), and crude suspended matter (relative to SS (suspended solids)) = 73.6%.

[0171] 200 mL of sludge was collected in a 300 mL beaker, a predetermined amount of polymer flocculant dissolved at 0.2% by mass was added, and the mixture was stirred for 30 seconds in a jar tester to allow for flocculation. The flocculated sludge was poured into a stainless steel sieve with an inner diameter of 75 mm, a depth of 100 mm, and an opening of 80 mesh, and gravity filtered. The volume of the filtrate was measured after 5, 10, 20, and 30 seconds using a measuring cylinder. The liquid volume (mL) and observation results after 10 seconds are shown in Table 6, and flocculation performance was compared and evaluated.

[0172]

[0173] At an addition amount of 40 to 60 ppm, the polymer flocculant of Example 6 exhibits superior performance to the polymer flocculant of Comparative Example 4, and it is clear that it can be used over a wide range of addition amounts.

[0174] [Second Invention] [Measurement of Molecular Weight of Polymer] The obtained polymer was subjected to gel permeation chromatography (GPC) measurement under the conditions described below to obtain the number average molecular weight (Mn) and weight average molecular weight (Mw) in pSt terms. The molecular weight distribution (Mw / Mn) was calculated from the obtained values. (GPC Measurement Conditions) Column: TSKgel Super Multipore HZ-M x 4, manufactured by Tosoh Corporation Eluent: THF Column temperature: 40°C Detector: RI Flow rate: 1.0 mL / min Molecular weight calculation method: The molecular weight in pSt terms was calculated based on a calibration curve prepared using a pSt standard substance.

[0175] [Monomer Conversion Rate] In each Production Example, the GPC measurement was carried out before the addition of the initiator and after the reaction was stopped, and the monomer conversion rate was calculated from the ratio of the peak intensities of the monomer components. When drying was carried out during the production process, the GPC measurement was carried out at a stage prior to the drying, and the monomer conversion rate (%) was calculated.

[0176] (Prepolymer Production Example 1) A 500 mL flask equipped with a stirrer and thermometer was charged with 0.254 g of 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid ("BM1429" manufactured by Boron Molecular) as an exchange chain transfer mechanism type controller, 100 g of methoxypolyethylene glycol (n≒9) monoacrylate ("Blemmer AME-400" manufactured by NOF Corp.) as a monomer component, and 65 g of ion-exchanged water as a polymerization medium. The mixture was thoroughly degassed by nitrogen bubbling and then heated to 70°C. 0.014 g of 4,4'-azobis(4-cyanovaleric acid) ("ACVA" manufactured by Otsuka Chemical Co., Ltd.) was then added as an initiator to initiate polymerization. After 5 hours while maintaining the temperature at 70°C, the mixture was cooled to room temperature to terminate the reaction, yielding prepolymer PP1. The obtained prepolymer PP1 had Mn=63,500, Mw=94,500, and Mw / Mn=1.49, and the monomer conversion was 95%.

[0177] (Prepolymer Production Example 2) A 500 mL flask equipped with a stirrer and thermometer was charged with 4-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}-4-cyanopentanoic acid (0.254 g) as an exchange chain transfer mechanism controller, 100 g of methoxypolyethylene glycol (n≒9) monoacrylate (NOF Corp., "Blenmer AME-400") as a monomer component, and 65 g of ion-exchanged water as a polymerization medium. The mixture was thoroughly degassed by nitrogen bubbling and then heated to 70°C. 0.014 g of 4,4'-azobis(4-cyanovaleric acid) (Otsuka Chemical Co., Ltd., "ACVA") was then added as an initiator to initiate polymerization. After 5 hours while maintaining the temperature at 70°C, the mixture was cooled to room temperature to terminate the reaction, yielding prepolymer PP2. The obtained prepolymer PP2 had Mn=58,000, Mw=94,500, and Mw / Mn=1.49, and the monomer conversion was 95%.

[0178] A 500 mL flask equipped with a stirrer and thermometer was charged with 6.34 g of 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid ("BM1429" manufactured by Boron Molecular) as a polymerization inhibitor, 80 g of methoxypolyethylene glycol (n≒9) monoacrylate ("Blemmer AME-400" manufactured by NOF Corp.) as the first monomer, and 65 g of ion-exchanged water as the polymerization medium. After thorough degassing with nitrogen bubbling, the temperature was raised to 70 °C. 0.014 g of 4,4'-azobis(4-cyanovaleric acid) ("ACVA" manufactured by Otsuka Chemical Co., Ltd.) was added as an initiator, and polymerization was initiated. After 3 hours while maintaining the temperature at 70 °C, a small amount was sampled and analyzed by GPC, confirming that the monomer conversion rate was 95%. 20 g of N-isopropylacrylamide was added as the second monomer, and the mixture was allowed to react for another 3 hours, after which the mixture was cooled to room temperature to terminate the reaction. The obtained prepolymer PP3 (block polymer) had Mn=3,300, Mw=4,010, and Mw / Mn=1.22. The conversion of the first monomer was 98%, and the conversion of the second monomer was 95%.

[0179] (Production of polymer flocculant) Hereinafter, examples of polymer flocculants produced using the prepolymers produced in the above production examples will be specifically described. The present invention is not limited to these examples. Various analyses and evaluations were carried out by the following methods.

[0180] [0.5% Salt Viscosity] 500 g of pure water was placed in a 500 mL conical beaker, and 20.8 g of accurately weighed first-grade reagent sodium chloride powder was added and dissolved. While stirring with a magnetic stirrer, a powder sample of a cationic copolymer was added, weighed accurately in an amount such that the concentration after dissolution would be 0.5% by mass in terms of solid content. The mixture was stirred at 200 rpm for 4 hours, and then allowed to stand to dissolve sufficiently to prepare a 0.5% by mass solution. The viscosity was measured using a BM-type viscometer manufactured by Tokyo Keiki Inc. at 25°C, 60 rpm, and after 5 minutes.

[0181] [0.1% Insoluble Content] 400 g of pure water was placed in a 500 mL conical beaker, and while stirring with a magnetic stirrer, each powder sample was added in an amount accurately weighed so that the concentration after dissolution would be 0.1 mass % in terms of solid content. After stirring for 2 hours, the mixture was left to stand sufficiently for dissolution to prepare a polymer solution with a concentration of 0.1%. This was then suction filtered through an 83-mesh filter cloth, and the volume (mL) of the residue on the filter cloth was measured with a measuring cylinder to obtain the insoluble content.

[0182] Example 10 A 78% by mass aqueous solution of dimethylaminoethyl acrylate methyl chloride (hereinafter abbreviated as "DAC"), a 50% by mass aqueous solution of acrylamide (hereinafter abbreviated as "AMD"), and the prepolymer PP1 obtained above were added to a stainless steel reaction vessel, and distilled water was further added to bring the total mass to 1.0 kg, followed by uniform mixing. The amounts of each component are shown in Table 7. The pH of this solution was adjusted to 4, and the solution temperature was adjusted to 5°C while nitrogen gas was bubbled into the solution for 60 minutes. Thereafter, 2,2'-azobis(2-methylpropionamidine) dihydrochloride (hereinafter abbreviated as "NC-32P") was added so that the solid content was 200 ppm relative to the total mass of each monomer. Next, the solution was irradiated with light from above the reaction vessel to polymerize, yielding a hydrous gel-like polymer. A 13 W black light was used for light irradiation. The irradiation intensity was 0.4 mW / cm. 2 The irradiation time was 60 minutes. The resulting hydrogel polymer was removed from the container and shredded. This was dried at 80°C for 5 hours and then pulverized to obtain a powdered polymer. The physical properties of powder sample A1 were evaluated according to the analytical and evaluation methods described above. The results are shown in Table 7.

[0183] Examples 11 and 12 Polymers were produced and evaluated in the same manner as in Example 10, except that the type and amount of prepolymer and the amount of monomer were changed as shown in Table 7. The results are shown in Table 7.

[0184] Comparative Examples 6 and 7 Polymers were produced and evaluated in the same manner as in Examples 10 and 11, except that sodium hydrogen sulfite was used as a chain transfer agent instead of the prepolymer. The results are shown in Table 7.

[0185] Comparative Example 8 A polymer was produced and evaluated in the same manner as in Example 10, except that methoxypolyethylene glycol (n≈9) monoacrylate (NOF Corp., "BLEMMER AME-400") was used instead of the prepolymer. The results are shown in Table 7.

[0186]

[0187] In Comparative Example 8, no prepolymer was used, and a hydrophobic monomer was added to a monomer preparation solution of AMD and DAC to perform polymerization trial, but the insoluble matter was very large at 290 mL, and properties as a flocculant were not obtained.

[0188] (Sludge dewatering test) A sludge dewatering test was carried out using the polymer flocculants produced in Examples 10 to 12 and Comparative Examples 6 and 7. The sludge used was organic sludge from sewage treatment plant "S". The physical properties of the sludge were pH = 5.40, TS = 34,100 (mg / L), and crude suspended solids (relative to SS) = 38.2%.

[0189] 200 mL of sludge was collected in a 300 mL beaker, and a predetermined amount of polymer flocculant dissolved at 0.2% by mass was added. The mixture was stirred for 30 seconds in a jar tester to allow for a flocculation reaction. The flocculated sludge was poured into a stainless steel sieve with an inner diameter of 75 mm, a depth of 100 mm, and an 80-mesh mesh size. Gravity filtration was performed, and the volume of the filtrate was measured after 5, 10, 20, and 30 seconds using a measuring cylinder. The liquid volume (mL) after 10 seconds and the observation results are shown in Table 8, and flocculation performance was compared and evaluated. The moisture content of the dehydrated cake was measured after dehydration for 10 minutes in a laboratory centrifuge at 1000 rpm and overnight drying in a dryer at 110 °C. The results are shown in Table 8. Compared to the comparative example, the example had a larger filtrate volume after 10 seconds and a lower moisture content of the dehydrated cake, demonstrating good flocculation performance.

[0190]

Claims

1. A polymeric flocculant comprising a cationic copolymer having a cationic monomer as an essential constituent unit, characterized in that the cationic copolymer has a structure derived from an exchange chain transfer mechanism type control agent at its terminal.

2. The polymer flocculant according to claim 1, wherein the structure derived from the exchange chain transfer mechanism type control agent is a structure derived from a reversible addition-fragmentation chain transfer agent (RAFT agent).

3. The structure derived from the reversible addition-fragmentation chain transfer agent (RAFT agent) is represented by the following chemical formula (1): (In the chemical formula (1), R 3 and R 4 The polymer flocculant according to claim 2, comprising a structure derived from a trithiocarbonate compound represented by the following formula:

4. The polymer flocculant according to any one of claims 1 to 3, wherein the salt viscosity X (mPa·s) of a salt solution obtained by dissolving the cationic copolymer at a concentration of 0.5% by mass in a 4% by mass aqueous sodium chloride solution at 25°C is 3.0 to 200, and the spinnability Y (mm) of a solution obtained by dissolving the cationic copolymer at a concentration of 1.0% by mass in pure water at 25°C is within the range represented by the following chemical formula (1): 0≦Y≦0.57X+0.0068X 2 ... Number (1) 5. The polymer flocculant according to any one of claims 1 to 3, wherein the cationic copolymer has an insoluble content of 5.0 mass% or less in a 0.1 mass% aqueous solution.

6. The cationic monomer is at least one represented by the following chemical formula (2): CH 2 =CR 1 -CO-X-Q-N+R 2a R 2b R 2c Z - ...Chemical formula (2) (In the chemical formula (2), R 1 is a hydrogen atom or a methyl group, R 2a and R 2b each independently represents an alkyl group having 1 to 3 carbon atoms or a benzyl group; R 2c represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different. X represents an oxygen atom or NH, Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms, Z - The polymer flocculant according to any one of claims 1 to 3, comprising a cationic monomer represented by the following formula:

7. A method for producing a polymer flocculant according to claim 1 or 2, comprising a step of copolymerizing a monomer component containing a cationic monomer by living radical polymerization in the presence of an exchange chain transfer mechanism type control agent to produce a cationic copolymer.

8. The method for producing a polymeric flocculant according to claim 7, wherein the exchange chain transfer mechanism type control agent is a reversible addition-fragmentation chain transfer agent (RAFT agent).

9. The reversible addition-fragmentation chain transfer agent (RAFT agent) is represented by the following chemical formula (1): (In the chemical formula (1), R 3 and R 4 represents an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted heteroaryl group, or an optionally substituted aralkyl group.

10. The method for producing a polymer flocculant according to claim 7, wherein the copolymerization is performed by irradiation with active energy rays.

11. A method for dehydrating sludge, comprising adding the polymer flocculant according to any one of claims 1 to 3 in an amount of 0.1 to 10,000 ppm based on the mass of organic sludge, stirring and mixing the mixture, and then dehydrating the sludge using a dehydrator.

12. A polymer flocculant comprising a block copolymer of a polymer block (A) formed by polymerizing a monomer component (a) and a polymer block (B) formed by polymerizing a monomer component (b), wherein the polymer block (A) has a structure derived from an exchange chain transfer mechanism type control agent at its end, and wherein the polymer block (A) is a nonionic unit and the polymer block (B) is a cationic unit.

13. The polymer flocculant described in claim 12, wherein the salt viscosity of a salt solution obtained by dissolving the block copolymer at a concentration of 0.5% by mass in a sodium chloride aqueous solution at a concentration of 4% by mass is 3.0 to 200 mPa·s at 25°C.

14. The polymer flocculant described in claim 12, wherein the insoluble content in a 0.1 mass % aqueous solution of the block copolymer is 5.0 mass % or less.

15. The exchange chain transfer mechanism type regulator is represented by the following chemical formula (1): (In the chemical formula (1), R 3 and R 4 The polymer flocculant according to claim 12, comprising a trithiocarbonate compound represented by the following formula:

16. The cationic monomer unit constituting the polymer block (B) is represented by the following chemical formula (2): CH 2 =CR 1 -CO-X-Q-N + R 2a R 2b R 2c Z - ...Chemical formula (2) (where R 1 is a hydrogen atom or a methyl group, R 2a and R 2b each independently represents an alkyl group having 1 to 3 carbon atoms or a benzyl group; R 2c represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different. X represents an oxygen atom or NH, Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms, Z - The polymer flocculant according to claim 12, comprising a structure derived from one or more cationic monomers represented by the following formula:

17. A method for producing a polymer flocculant as described in claim 12, characterized in that it comprises a step of forming a polymer block (B) by radically polymerizing a monomer component (b) containing at least a cationic monomer in the presence of a prepolymer containing a polymer block (A) having a structure derived from an exchange chain transfer mechanism type control agent at its end, thereby producing a block copolymer of the polymer block (A) and the polymer block (B).

18. A method for producing a polymer flocculant as described in claim 12, characterized in that it comprises the following steps (I) and (II): step (I): a step of radically polymerizing a monomer component (a) in the presence of a chain transfer mechanism type control agent to produce a prepolymer containing a polymer block (A) having a structure derived from the chain transfer mechanism type control agent at an end thereof, and step (II): a step of radically polymerizing a monomer component (b) containing at least a cationic monomer in the presence of the prepolymer to form a polymer block (B), thereby producing a block copolymer of the polymer block (A) and the polymer block (B).

19. The method for producing a polymeric flocculant according to claim 17, wherein the exchange chain transfer mechanism type control agent is a reversible addition-fragmentation chain transfer agent (RAFT agent).

20. The reversible addition-fragmentation chain transfer agent (RAFT agent) is represented by the following chemical formula (1): (In the chemical formula (1), R 3 and R 4 represents an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted heteroaryl group, or an optionally substituted aralkyl group.

21. The method for producing a polymer flocculant according to claim 17, wherein the prepolymer has a weight average molecular weight (Mw) of 1,000 to 300,000 as measured by gel permeation chromatography (GPC).

22. The method for producing a polymer flocculant according to claim 17, wherein the radical polymerization is polymerization by irradiation with active energy rays.

23. The method for producing a polymer flocculant according to claim 18, wherein the radical polymerization in step (II) is polymerization by irradiation with active energy rays.

24. A method for dewatering sludge, comprising adding a polymer flocculant according to any one of claims 12 to 16 to the sludge.

Citation Information

Patent Citations

  • Block copolymer, viscosity-adjusting agent, and flocculation auxiliary

    JP2010013497A

  • Composition for sludge conditioning

    JP2020081930A

  • Production method of water-soluble polymer

    JP2020117597A

  • Synthetic methods for preparing rheology-modifying polymers and their uses

    JP2021533217A

  • Method for treating suspensions of solid particles in water using amphoteric polymers

    US20220017391A1

Cited By

  • Flocculating agent for oil-based drilling fluid as well as preparation method and application of flocculating agent