Positive electrode active material and secondary battery
The positive electrode active material with specific pore characteristics addresses the balance between adhesion and capacity by ensuring sufficient reaction area and preventing binder intrusion, enhancing battery performance.
Patent Information
- Application Number
- PCT/JP2024/016042
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
The challenge lies in finding a positive electrode active material that balances adhesion between the current collector and the composite layer with battery capacity, as excessive pores allow binder intrusion, reducing adhesion, while few pores limit reaction area and capacity.
A positive electrode active material with pore diameters of 30 nm or more and pore volumes of 0.003 cm³/g, characterized by a peak pore volume distribution at 5 nm or less, ensures sufficient reaction area and suppresses binder intrusion, maintaining adhesion and capacity.
This approach effectively prevents decreases in both adhesion and battery capacity by optimizing pore distribution, allowing for efficient battery performance without increasing binder content.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure 00000016_0000
Abstract
Description
Positive electrode active material and secondary battery
[0001] The present disclosure relates to a positive electrode active material and a secondary battery.
[0002] In recent years, secondary batteries such as lithium-ion secondary batteries have been widely used in applications requiring high capacity, such as automotive applications and power storage applications. The cathode active material, which is the main component of the cathode, has a significant impact on increasing the capacity of the battery, and therefore, much research has been done on the cathode active material.
[0003] For example, Patent Document 1 describes a method in which the average pore diameter measured by mercury intrusion porosimetry is in the range of 0.1 to 1 μm, and the total volume of pores having diameters of 0.01 to 1 μm is 0.01 cm 3 The document discloses a positive electrode in which a positive electrode mixture layer containing a positive electrode active material made of porous particles having a surface roughness of 1 / g or more and a binder is formed on a positive electrode current collector.
[0004] Japanese Patent Application Laid-Open No. 2000-323142
[0005] However, if the positive electrode active material has many pores, the binder may enter the pores of the positive electrode active material during the preparation of the positive electrode, resulting in a decrease in the adhesion (peel strength) between the positive electrode current collector and the positive electrode composite layer. In this case, more binder is required, but the battery capacity may decrease. On the other hand, in a positive electrode active material with few pores, the reaction area is small, resulting in a decrease in battery capacity.
[0006] Therefore, an object of the present disclosure is to provide a positive electrode active material that can suppress a decrease in the adhesion between a positive electrode current collector and a positive electrode mixture layer and a decrease in battery capacity, and a secondary battery that includes the positive electrode active material.
[0007] One aspect of the present disclosure is a positive electrode active material having pores, wherein the pore size distribution obtained by analyzing a nitrogen adsorption isotherm by the BJH method has pores with a pore size of 30 nm or more and a pore volume of 0.003 cm or less. 3 / g or more, and in the pore size distribution obtained by analyzing the nitrogen desorption isotherm by the BJH method, the pore volume peak is at a pore size of 5 nm or less.
[0008] One aspect of the present disclosure is a secondary battery having a positive electrode and a negative electrode, wherein the positive electrode includes a positive electrode mixture layer containing the above-described positive electrode active material.
[0009] According to the present disclosure, it is possible to suppress a decrease in the adhesive strength between the positive electrode current collector and the positive electrode mixture layer and a decrease in battery capacity.
[0010] 1 is a cross-sectional view of a secondary battery according to an embodiment;
[0011] Hereinafter, embodiments of the secondary battery according to the present disclosure will be described in detail with reference to the drawings.
[0012] FIG. 1 is a cross-sectional view of a secondary battery according to an embodiment. The secondary battery 10 shown in FIG. 1 includes a wound electrode assembly 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, an electrolyte, insulating plates 18 and 19 disposed above and below the electrode assembly 14, respectively, and a battery case 15 for accommodating the above components. The battery case 15 is composed of a cylindrical case body 16 with a bottom and a sealing body 17 that closes the opening of the case body 16. Note that, instead of the wound electrode assembly 14, other electrode bodies may be used, such as a laminated electrode body formed by alternately stacking positive and negative electrodes with separators interposed therebetween. Examples of the battery case 15 include a cylindrical, rectangular, coin-shaped, or button-shaped metal case, and a resin case formed by laminating a resin sheet (a so-called laminate type).
[0013] The electrolyte has, for example, ion conductivity (for example, lithium ion conductivity). The electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.
[0014] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. Examples of the non-aqueous solvent include ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and mixed solvents of these. The non-aqueous solvent may contain a halogen-substituted compound (e.g., fluoroethylene carbonate) in which at least a portion of the hydrogen atoms of these solvents are substituted with halogen atoms such as fluorine. Examples of the electrolyte salt include LiPF 6 Lithium salts such as
[0015] Furthermore, examples of the solid electrolyte that can be used include solid or gel-like polymer electrolytes, inorganic solid electrolytes, and the like. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. For example, a polymer material that absorbs a non-aqueous solvent and gels is used as the matrix polymer. Examples of the polymer material include fluororesin, acrylic resin, and polyether resin. For example, the inorganic solid electrolyte can be a material known in all-solid-state lithium ion secondary batteries (e.g., oxide-based solid electrolytes, sulfide-based solid electrolytes, halogen-based solid electrolytes, and the like). While the above-exemplified electrolytes are non-aqueous electrolytes, the electrolyte is not limited to non-aqueous electrolytes and may be an aqueous electrolyte.
[0016] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has, for example, a protruding portion 22, which is a portion of the side surface that protrudes inward and supports the sealing body 17. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.
[0017] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked in this order from the electrode body 14 side. Each component constituting the sealing body 17 has, for example, a disk or ring shape, and all components except for the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. If the internal pressure of the secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 may deform and rupture, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. If the internal pressure further increases, the upper valve body 26 may rupture, and gas may be discharged from the opening of the cap 27.
[0018] In the secondary battery 10 shown in Fig. 1, a positive electrode lead 20 attached to the positive electrode 11 passes through a through-hole in the insulating plate 18 and extends toward the sealing body 17, and a negative electrode lead 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom side of the case body 16. The positive electrode lead 20 is connected by welding or the like to the underside of a filter 23, which is the bottom plate of the sealing body 17, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected by welding or the like to the inner bottom surface of the case body 16, and the case body 16 serves as the negative electrode terminal.
[0019] The positive electrode 11, the negative electrode 12, and the separator 13 will be described in detail below.
[0020] [Positive Electrode] The positive electrode 11 has a positive electrode current collector and a positive electrode composite layer disposed on the positive electrode current collector. The positive electrode composite layer may be formed on both sides of the positive electrode current collector or on one side of the positive electrode current collector. The positive electrode current collector may be a foil of a metal, such as aluminum, that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface. The positive electrode composite layer includes, for example, a porous positive electrode active material, a binder, a conductive material, and the like. The positive electrode 11 can be produced, for example, by applying a positive electrode paste containing a positive electrode active material, a binder, a conductive material, and the like to the surface of the positive electrode current collector, drying the coating, and then rolling it.
[0021] The positive electrode active material of this embodiment may be, for example, a lithium transition metal composite oxide. Examples of metal elements contained in the lithium transition metal composite oxide include Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, and W. Among these, it is preferable to contain at least one of Ni, Co, and Mn. An example of a suitable lithium transition metal composite oxide is represented by the general formula LiMO 2 (M is Ni and X, X is a metal element other than Ni, and the proportion of Ni is 50 mol % to 95 mol % based on the total number of moles of the metal elements excluding Li). Examples of X in the above formula include Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, W, etc.
[0022] The positive electrode active material of this embodiment has a pore size distribution (hereinafter referred to as an adsorption-side pore size distribution) obtained by analyzing a nitrogen adsorption isotherm by the BJH (Barrett-Joyner-Halenda) method, in which the pore size is 30 nm or more and the pore volume is 0.003 cm 3 / g or more, and in the pore size distribution obtained by analyzing the nitrogen desorption isotherm by the BJH method (hereinafter referred to as the desorption-side pore size distribution), the pore volume of the peak in the pore size region of 5 nm or less is 2.00 times or more the pore volume of the peak in the pore size region of more than 5 nm.
[0023] In the adsorption side pore size distribution, the pore size is 30 nm or more and the pore volume is 0.003 cm 3 / g or more, sufficient pores are present in the positive electrode active material. Therefore, the reaction area of the positive electrode active material is sufficiently secured, and a decrease in battery capacity is suppressed. Furthermore, in the desorption-side pore size distribution, the pore volume of the peak in the pore diameter region of 5 nm or less is 2.00 times or more the pore volume of the peak in the pore diameter region of more than 5 nm. Therefore, the diameter of the entrance portion of the pore formed in the positive electrode active material is small, and therefore, the penetration of the binder into the pores of the positive electrode active material during positive electrode fabrication is suppressed. Therefore, even without increasing the amount of binder added, a decrease in the adhesion strength between the positive electrode current collector and the positive electrode mixture layer is suppressed. Furthermore, the suppression of the amount of binder added also contributes to suppressing a decrease in battery capacity.
[0024] The pore size distribution was measured as follows. First, 5 g of particles of the positive electrode active material were subjected to vacuum degassing treatment at 105°C for 8 hours using a vacuum heat treatment device (BELSORP-vacII, manufactured by Microtrac-Bell Corporation). After the treatment, the amount of nitrogen adsorption of the particles of the positive electrode active material at liquid nitrogen temperature (77K) was measured using a measuring device (BELSORP-mini, manufactured by Microtrac-Bell Corporation), and a nitrogen adsorption isotherm and a nitrogen desorption isotherm were prepared. The obtained nitrogen adsorption isotherm and nitrogen desorption isotherm were analyzed by the BJH method, respectively, to determine the pore size distribution in the pore diameter range of 200 nm or less. The BJH method is a technique in which the pore shape is assumed to be cylindrical and analysis is performed based on the relationship between the pore diameter that causes capillary condensation and the relative thickness of nitrogen (Kelvin equation). The pore size distribution is plotted as follows: the horizontal axis represents the pore diameter (nm, logarithmic scale) and the vertical axis represents the log differential pore volume (cm 3 In the present disclosure, the pore volume in the pore size distribution refers to the log differential pore volume.
[0025] In the positive electrode active material of this embodiment, in the adsorption side pore size distribution, the pore size is 30 nm or more and the pore volume is 0.003 cm 3 / g or more, but in order to further suppress the decrease in battery capacity, for example, it is preferable that the pore diameter is 30 nm or more and the pore volume is 0.004 cm 3 The upper limit of the pore volume is not particularly limited, but for example, it is 0.01 cm 3In the adsorption-side pore size distribution, the pore volume peak observed in the region of pore diameters of 30 nm or more may be one or more. In addition, in the adsorption-side pore size distribution, the pore volume observed in the region of pore diameters of 30 nm or more may be 0.003 cm or less. 3 The adsorption-side pore size distribution may have one or more peaks of pore volume at pore diameters of less than 30 nm. In this embodiment, the adsorption-side pore size distribution may have a peak of pore volume at pore diameters of less than 0.002 cm 3 / g or more (i.e., the pore volume value is 0.002 cm 3 / g or less, there is no peak).
[0026] In the positive electrode active material of this embodiment, the pore volume of the peak in the pore diameter region of 5 nm or less in the desorption-side pore diameter distribution may be 2.00 times or more the pore volume of the peak in the pore diameter region of more than 5 nm. However, for example, in order to further suppress a decrease in the adhesion strength between the positive electrode current collector and the positive electrode mixture layer, it is preferable that the pore diameter is 5 nm or less and the pore volume is 0.01 cm. 3 / g or more. The lower limit of the pore diameter at the peak is not particularly limited, but is, for example, 1 nm or more. In the desorption-side pore size distribution, one or more pore volume peaks may be observed in the region where the pore diameter is 5 nm or less. In the desorption-side pore size distribution, the pore volume peak may be present at a pore diameter greater than 5 nm, or the pore volume peak may not be present at a pore diameter greater than 5 nm. In this embodiment, in the desorption-side pore size distribution, the pore volume value is preferably 0.003 cm 3 / g or more (i.e., the pore volume value is 0.003 cm 3 / g or less, there is no peak).
[0027] The positive electrode active material of this embodiment preferably has an average particle size of 1 μm or more and 50 μm or less, and more preferably an average particle size of 10 μm or more and 30 μm or less, for example, in terms of further suppressing a decrease in battery capacity, etc. The average particle size is the volume average particle size D50 at which the volume integrated value becomes 50% in a particle size distribution obtained by a laser diffraction scattering method.
[0028] The positive electrode active material of this embodiment has a 0.1 m 2 / g or more, 5m 2 It is preferable that the BET specific surface area is 0.2 m / g or less. 2 / g or more, 3m 2 / g or less. The BET specific surface area is measured using the BET multipoint method from the nitrogen adsorption isotherm described above. As a measuring device, for example, a BELSORP-mini (manufactured by Microtrac BEL Co., Ltd.) can be used.
[0029] An example of a method for producing a positive electrode active material according to the present embodiment will be described. For example, a metal hydroxide or metal oxide such as Ni, Co, Mn, or Al is mixed with a lithium compound, and the mixture is fired. An example of the lithium compound is Li 2 CO 3 , LiOH, etc. Examples of suitable mixtures of metal hydroxides or metal oxides and lithium compounds include a molar ratio of metal elements Me to Li of, for example, 1:0.95 to 1:1.15, preferably 1:1.05 to 1:1.15. The mixture is calcined, for example, in an oxygen stream, by heating the mixture to a set temperature of 500°C to 800°C at a heating rate of 0.2 to 5.5°C / min. The holding time after heating to the set temperature is preferably 2 to 4 hours. The calcined mixture is then cooled to room temperature at a predetermined temperature drop rate, for example, in an oxygen stream. To obtain a positive electrode active material having the above-mentioned peaks in the adsorption-side pore size distribution and the desorption-side pore size distribution, the temperature drop rate during cooling is important. The temperature drop rate is, for example, 1.2°C / min or less and is appropriately set depending on the composition of the elements constituting the positive electrode active material.
[0030] The positive electrode mixture layer may contain a positive electrode active material that does not have the above-described peaks in the adsorption-side pore size distribution and the desorption-side pore size distribution, as long as the effect of this embodiment is not impaired. The content of the positive electrode active material in this embodiment is, for example, preferably 90 mass% or more, more preferably 95 mass% or more, and even more preferably 100 mass%, based on the total mass of the positive electrode active material.
[0031] Examples of the conductive material contained in the positive electrode mixture layer include carbon materials such as carbon black, acetylene black, ketjen black, graphite, and carbon nanotubes.
[0032] Examples of the binder contained in the positive electrode mixture layer include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, styrene-butadiene rubber (SBR), cellulose derivatives such as carboxymethyl cellulose (CMC) or a salt thereof, and polyethylene oxide (PEO).
[0033] The content of the binder is preferably 0.60% by mass or less relative to the mass of the positive electrode active material, for example, in order to further suppress a decrease in battery capacity. Since the positive electrode mixture layer contains the positive electrode active material of this embodiment, even with the binder content above, a decrease in the adhesion between the positive electrode mixture layer and the positive electrode current collector is suppressed.
[0034] The weight-average molecular weight of the binder is preferably 1,000,000 or more, for example, in order to further suppress a decrease in the adhesion between the positive electrode mixture layer and the positive electrode current collector. The weight-average molecular weight may be measured by a general molecular weight measurement method, and specifically, is a value measured using gel permeation chromatography (GPC).
[0035] [Negative Electrode] The negative electrode 12 has a negative electrode current collector and a negative electrode composite layer disposed on the negative electrode current collector. The negative electrode composite layer may be formed on both sides of the negative electrode current collector or on one side of the negative electrode current collector. The negative electrode current collector may be a foil of a metal such as copper that is stable within the potential range of the negative electrode 12, or a film with such a metal disposed on the surface layer. The negative electrode composite layer contains, for example, a negative electrode active material and a binder. The negative electrode 12 can be produced, for example, by applying a negative electrode paste containing a negative electrode active material and a binder to the surface of the negative electrode current collector, drying the coating, and then rolling it.
[0036] Examples of the negative electrode active material include materials that can reversibly absorb and release lithium ions, such as carbon materials such as natural graphite and artificial graphite, metals such as Si and Sn, alloys, or oxides. Examples of the binder include those similar to those in the case of the positive electrode 11. The negative electrode mixture layer may contain a conductive material. Examples of the conductive material include those similar to those in the case of the positive electrode 11.
[0037] [Separator] The separator 13 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have either a single-layer structure or a laminated structure. A heat-resistant layer or the like may be formed on the surface of the separator.
[0038] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0039] Example 1 Preparation of Negative Electrode 100 parts by mass of graphite powder, 1 part by mass of carboxymethyl cellulose sodium (CMC-Na), and 1 part by mass of a dispersion of styrene butadiene rubber (SBR) were mixed, and an appropriate amount of water was added to prepare a negative electrode composite slurry. Next, the negative electrode composite slurry was applied to both sides of a copper foil with a thickness of 8 μm, and the coating was dried. Then, a negative electrode was prepared by rolling the coating using a roller.
[0040] [Fabrication of Positive Electrode] In the adsorption side pore size distribution, the pore diameter was 38 nm and the pore volume was 0.0042 cm 3 / g, and in the desorption side pore size distribution, the pore volume of the peak in the pore diameter region of 5 nm or less is at least twice the pore volume of the peak in the pore diameter region of more than 5 nm, and 0.9 Co 0.05 Al 0.05 O 2 A lithium transition metal composite oxide represented by the following formula was used as the positive electrode active material.
[0041] 100 parts by mass of the above positive electrode active material, 1 part by mass of acetylene black (AB), and 0.6 parts by mass of binder polyvinylidene fluoride (PVDF) were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode composite slurry. Polyvinylidene fluoride (PVDF) with a weight average molecular weight of 1.2 million was used as the binder. Next, the positive electrode composite slurry was applied to both sides of a 15 μm thick aluminum foil, and the coating was dried. Then, a positive electrode was produced by rolling the coating using a roller.
[0042] [Preparation of non-aqueous electrolyte] 5 parts by mass of vinylene carbonate (VC) was added to 100 parts by mass of a mixed solvent in which ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed at a volume ratio of 3:7, and lithium hexafluorophosphate (LiPF 6 A non-aqueous electrolyte was prepared by dissolving 1.5 mol / L of ammonium hydroxide in water.
[0043] [Fabrication of Secondary Battery] A positive electrode lead was attached to the positive electrode, and a negative electrode lead was attached to the negative electrode. The positive and negative electrodes were then wound with a separator interposed therebetween to fabricate a wound electrode assembly. Insulating plates were placed above and below the electrode assembly, and the electrode assembly was housed in a case body. The negative electrode lead was welded to the bottom of the case body, and the positive electrode lead was welded to a sealing member. After injecting a nonaqueous electrolyte into the case body, the opening of the case body was sealed with a sealing member via a gasket to fabricate a secondary battery.
[0044] Example 2 A secondary battery was fabricated in the same manner as in Example 1, except that in fabricating the positive electrode, PVDF having a weight-average molecular weight of 800,000 was used as the binder.
[0045] Example 3 A secondary battery was fabricated in the same manner as in Example 1, except that the amount of binder used in fabricating the positive electrode was changed to 0.8 parts by mass.
[0046] <Example 4> In the preparation of a positive electrode, the pore diameter was 36 nm and the pore volume was 0.0031 cm in the adsorption side pore diameter distribution. 3 / g, and in the desorption side pore size distribution, the pore volume of the peak in the pore size region of 5 nm or less is 2.0 times or more the pore volume of the peak in the pore size region of more than 5 nm, and 0.9 Co 0.05 Al 0.05 O 2 A secondary battery was fabricated in the same manner as in Example 1, except that a lithium transition metal composite oxide represented by the following formula was used as the positive electrode active material and the amount of the binder was set to 0.8 parts by mass.
[0047] <Comparative Example 1> In the preparation of a positive electrode, the pore diameter was 41 nm and the pore volume was 0.0046 cm in the adsorption side pore diameter distribution. 3 / g, and in the desorption side pore size distribution, there is no pore volume peak at pore diameters of 5 nm or less, and there is a pore volume peak at pore diameters of 10.5 nm, and the composition formula is LiNi 0.9 Co 0.05 Mn 0.05 O 2 A secondary battery was fabricated in the same manner as in Example 1, except that a lithium transition metal composite oxide represented by the following formula was used as the positive electrode active material.
[0048] <Comparative Example 2> In the preparation of a positive electrode, in the adsorption side pore size distribution, there was no peak in the pore volume at pore diameters of 30 nm or more, and the pore diameter was 15 nm and the pore volume was 0.0021 cm 3 / g, and in the desorption side pore size distribution, the pore volume of the peak in the pore diameter region of 5 nm or less is at least twice the pore volume of the peak in the pore diameter region of more than 5 nm, and 0.9 Co 0.05 Mn 0.05 O 2 A secondary battery was fabricated in the same manner as in Example 1, except that a lithium transition metal composite oxide represented by the following formula was used as the positive electrode active material.
[0049] <Comparative Example 3> In the preparation of a positive electrode, the pore diameter was 40 nm and the pore volume was 0.0031 cm in the adsorption side pore diameter distribution. 3 / g, and in the desorption side pore size distribution, there is no pore volume peak at pore diameters of 5 nm or less, and there is a pore volume peak at pore diameters of 8.0 nm, and the composition formula is LiNi0.9 Co 0.05 Mn 0.05 O 2 A secondary battery was fabricated in the same manner as in Example 1, except that a lithium transition metal composite oxide represented by the following formula (I) was used as the positive electrode active material and the amount of the binder was 83 parts by mass.
[0050] [Evaluation of Battery Capacity] The test cells of each Example and Comparative Example were charged at a constant current of 0.5 C in a temperature environment of 25°C until the battery voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current value reached 0.05 C. Thereafter, the test cells were discharged at a constant current of 0.2 C until the battery voltage reached 2.5 V. The discharge capacity at this time was determined as the battery capacity. The results are summarized in Table 1. In Table 1, the battery capacity of Example 1 is set as the reference (100), and the battery capacities of the other Examples and Comparative Examples are expressed relative to each other.
[0051] [Peel Strength Test] The positive electrode composite layer surface of a 100 mm x 25 mm positive electrode was attached to a 120 mm x 30 mm acrylic plate via double-sided tape (Nichiban Co., Ltd., Nicetack NW-20). Using a small benchtop tester (FGS-TV and FGP-5) manufactured by Nidec-Shimpo Corporation, 90° peeling was performed at a measurement temperature of 25 ° C. and a tensile speed of 50 mm / min, and the peel strength between the positive electrode composite layer and the positive electrode current collector (aluminum foil) was measured. The results are shown in Table 1. In Table 1, the peel strength of Example 1 is used as the reference (100), and the peel strengths of the other Examples and Comparative Examples are expressed relatively.
[0052]
[0053] Examples 1, 3, and 4 all exhibited high values for battery capacity and peel strength. Example 2 used a binder with a low weight-average molecular weight, resulting in low peel strength, but still higher than the comparative examples. On the other hand, Comparative Examples 1 and 3 exhibited significantly lower peel strengths than Example 1, and Comparative Example 2 exhibited lower battery capacity than Example 1. These results indicate that in the adsorption-side pore size distribution, pore diameters of 30 nm or more and pore volumes of 0.003 cm3 are the most important. 3 / g or more, and in the desorption-side pore size distribution, the pore volume of the peak in the pore diameter region of 5 nm or less is at least twice the pore volume of the peak in the pore diameter region of more than 5 nm, which can be said to make it possible to suppress a decrease in the adhesion between the positive electrode current collector and the positive electrode mixture layer and a decrease in battery capacity.
[0054] 10 Secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 15 Battery case, 16 Case body, 17 Sealing body, 18, 19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Protruding portion, 23 Filter, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket.
Claims
1. A positive electrode active material having pores, in which the pore size distribution obtained by analyzing the nitrogen adsorption isotherm by the BJH method has a pore size of 30 nm or more and a pore volume of 0.003 cm 3 / g or more, and in a pore size distribution obtained by analyzing a nitrogen desorption isotherm by the BJH method, the pore volume of the peak in a pore size region of 5 nm or less is at least twice the pore volume of the peak in a pore size region of more than 5 nm.
2. A secondary battery having a positive electrode and a negative electrode, the positive electrode comprising a positive electrode mixture layer having the positive electrode active material according to claim 1.
3. The secondary battery according to claim 2, wherein the positive electrode mixture layer contains a binder, and the content of the binder is 0.60 mass % or less with respect to the mass of the positive electrode active material.
4. The secondary battery according to claim 3, wherein the binder has a weight average molecular weight of 1,000,000 or more.
Citation Information
Patent Citations
Positive electrode active material for non-aqueous secondary battery, positive electrode and secondary battery
JP2000323142A
Lithium compound oxide particle for lithium secondary battery positive electrode material, and lithium secondary battery positive electrode using the same, and the lithium secondary battery
JP2005123179A
Conductive composite particle, secondary battery positive electrode arranged by use thereof, and secondary battery
JP2014241229A
Positive electrode material for lithium ion secondary battery, positive electrode for lithium ion secondary battery, and lithium ion secondary battery
JP2015069822A
Lithium metal composite oxide, positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery
JP2024053428A