Display device laminate and display device

The laminate structure for flexible displays optimizes hardness and bending resistance through a polyimide resin base material and functional layers, addressing peeling issues and ensuring durability and replaceability.

WO2024225385A1PCT designated stage expired Publication Date: 2024-10-31DAI NIPPON PRINTING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016274
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-25
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Flexible displays, such as foldable and bendable displays, face challenges in achieving both high hardness and bending resistance, as increasing surface hardness reduces bending resistance, and replaceable laminates struggle with peeling issues when repeatedly bent.

Method used

A laminate structure comprising a first laminated film with a polyimide resin base material and a functional layer, bonded to a second laminated film via a releasable adhesive layer, where the thickness and tensile modulus of both films are optimized to achieve high hardness and bending resistance while allowing for replaceability.

Benefits of technology

The laminate provides excellent hardness and bending resistance, preventing peeling and deformation, and allows for easy replacement of damaged layers, enhancing the durability and usability of flexible displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016274_31102024_PF_FP_ABST
    Figure JP2024016274_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a display device laminate that includes: a first layered film that includes a first resin base material and a first functional layer; a bonding layer that is provided on the surface of the first layered film on the first resin base material side; and a second layered film that is provided on the surface of the bonding layer on the reverse side from the first layered film and includes, in order from the bonding layer side, a second functional layer and a second resin base material. The first layered film and the bonding layer can be peeled from the second layered film, the thickness of the first functional layer is at least 8 μm, the A1 value calculated from A1=E1×h13 / 12 is at least 0.10×10-3 Pa⋅m3 but no more than 0.52×10-3 Pa⋅m3, and the A2 value calculated from A2=E2×h23 / 12 is no more than 0.07×10-3 Pa⋅m3. In the expressions, E1 is the tensile elastic modulus (Pa) of the first layered film, h1 is the thickness (m) of the first layered film, E2 is the tensile elastic modulus (Pa) of the second layered film, and h2 is the thickness (m) of the second layered film.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate for display device and display device

[0001] The present disclosure relates to a laminate for a display device and a display device.

[0002] On the surface of the display device, a laminate including functional layers having various properties such as hard coating properties, abrasion resistance, anti-reflection properties, anti-glare properties, anti-static properties, and anti-fouling properties is disposed.

[0003] In recent years, flexible displays such as foldable displays, slidable displays, rollable displays, and bendable displays have attracted attention, and the development of laminates to be placed on the surfaces of flexible displays has been actively promoted (for example, Patent Documents 1 and 2).

[0004] A laminate disposed on the surface of a flexible display is required to be scratch-resistant. Therefore, a laminate with high surface hardness is used. Furthermore, a flexible display is required to be able to withstand repeated bending without causing display defects, and a laminate disposed on the surface of a flexible display is required to have bending resistance that prevents peeling or cracking when repeatedly bent. However, increasing the surface hardness of the laminate may result in a decrease in bending resistance. Therefore, it is difficult to achieve both high hardness and bending resistance.

[0005] JP 2021-60576 A JP 2021-117334 A

[0006] Recently, flexible displays that support pen input have become more common. However, dents and scratches are easily caused during pen input. Therefore, a replaceable laminate that is placed on the surface of a flexible display is desired.

[0007] A replaceable laminate needs to be able to be attached and removed. However, because a replaceable laminate can be removed, it may lift or peel off when repeatedly bent. Therefore, it is difficult to achieve both replaceability and flex resistance.

[0008] The present disclosure has been made in view of the above-described circumstances, and has as its main object to provide a replaceable laminate for a display device that is excellent in hardness and flex resistance, and a display device including the same.

[0009] One embodiment of the present disclosure provides a laminate film having a first laminate film including a first resin substrate and a first functional layer, a bonding layer disposed on a surface of the first laminate film facing the first resin substrate, and a second laminate film disposed on a surface of the bonding layer opposite the first laminate film, the second laminate film including, in this order from the bonding layer side, a second functional layer and a second resin substrate, the first laminate film and the bonding layer being peelable from the second laminate film, the first functional layer having a thickness of 8 μm or more, and an A1 value calculated by the following formula (1) being 0.10 × 10 -3 P.A.M. 3 That's it, 0.52 x 10 -3 P.A.M. 3 The A2 value calculated by the following formula (2) is 0.07 × 10 -3 P.A.M. 3 A laminate for a display device is provided, where A1=E1×h1. 3 / 12 (1) A2=E2×h2 3 / 12 (2) (In the above formula (1), E1 represents the tensile modulus of elasticity (Pa) of the first laminate film, and h1 represents the thickness (m) of the first laminate film. In the above formula (2), E2 represents the tensile modulus of elasticity (Pa) of the second laminate film, and h2 represents the thickness (m) of the second laminate film.)

[0010] Another embodiment of the present disclosure provides a display device comprising a display panel and the above-described display device laminate arranged on the viewer side of the display panel, wherein the display device laminate is arranged so that the surface on the second laminate film side faces the display panel.

[0011] The present disclosure has an effect of providing a replaceable laminate for a display device that has excellent hardness and flex resistance.

[0012] Fig. 1 is a schematic cross-sectional view illustrating a laminate for a display device according to the present disclosure; Fig. 2 is a schematic cross-sectional view illustrating a display device according to the present disclosure; Fig. 3 is a schematic cross-sectional view illustrating a display device according to the present disclosure; Fig. 4 is a schematic view illustrating a dynamic bending test; Fig. 5 is a schematic cross-sectional view illustrating a display device according to the present disclosure.

[0013] Embodiments of the present disclosure will be described below with reference to the drawings and the like. However, the present disclosure can be implemented in many different forms, and should not be construed as being limited to the description of the embodiments exemplified below. Furthermore, to clarify the explanation, the drawings may show the width, thickness, shape, etc. of each part schematically compared to the actual form, but these are merely examples and do not limit the interpretation of the present disclosure. Furthermore, in this specification and each drawing, elements similar to those described above with reference to the previous drawings are designated by the same reference numerals, and detailed descriptions may be omitted as appropriate.

[0014] In this specification, when describing a mode in which another component is placed on a certain component, the term "above" or "below" is used, unless otherwise specified, to include both a case in which another component is placed directly above or below a certain component so as to be in contact with the component, and a case in which another component is placed above or below a certain component with another component interposed therebetween. Also, in this specification, when describing a mode in which another component is placed on the surface of a certain component, the term "on the surface side" or "on the surface" is used, unless otherwise specified, to include both a case in which another component is placed directly above or below a certain component so as to be in contact with the component, and a case in which another component is placed above or below a certain component with another component interposed therebetween.

[0015] The laminate for a display device and the display device according to the present disclosure will be described in detail below.

[0016] A. Laminate for display device The laminate for display device in the present disclosure comprises a first laminate film having a first resin substrate and a first functional layer, a bonding layer disposed on a surface of the first laminate film facing the first resin substrate, and a second laminate film disposed on a surface of the bonding layer opposite to the first laminate film, the second laminate film having, in this order from the bonding layer side, a second functional layer and a second resin substrate, the first laminate film and the bonding layer being peelable from the second laminate film, the first resin substrate containing a polyimide resin, the first functional layer having a thickness of 8 μm or more, and an A1 value calculated by the following formula (1) being 0.10 × 10 -3 P.A.M. 3 That's it, 0.52 x 10 -3 P.A.M. 3 The A2 value calculated by the following formula (2) is 0.07 × 10 -3 P.A.M. 3 The following is true: A1 = E1 × h1 3 / 12 (1) A2=E2×h2 3 / 12 (2) (In the above formula (1), E1 represents the tensile modulus of elasticity (Pa) of the first laminate film, and h1 represents the thickness (m) of the first laminate film. In the above formula (2), E2 represents the tensile modulus of elasticity (Pa) of the second laminate film, and h2 represents the thickness (m) of the second laminate film.)

[0017] FIG. 1 is a schematic cross-sectional view showing an example of a laminate for a display device according to the present disclosure. As shown in FIG. 1 , the laminate for a display device 1 includes a first laminate film 10 having a first resin substrate 11 and a first functional layer 12, a bonding layer 2 disposed on the surface of the first laminate film 10 facing the first resin substrate 11, and a second laminate film 20 disposed on the surface of the bonding layer 2 opposite the first laminate film 10, the second laminate film 20 including, in order from the bonding layer 2 side, a second functional layer 22 and a second resin substrate 21. The first resin substrate 11 contains a polyimide resin, and the thickness of the first functional layer 12 is equal to or greater than a predetermined value. In the first laminate film 10, the A1 value calculated by the above formula (1) is within a predetermined range. In the second laminate film 20, the A2 value calculated by the above formula (2) is within a predetermined range.

[0018] 2 is a schematic cross-sectional view showing an example of a display device including a laminate for a display device according to the present disclosure. The display device 30 includes a display panel 31 and a laminate for a display device 1 arranged on the viewer's side of the display panel 31. The laminate for a display device 1 is arranged so that the surface on the second laminate film 20 side faces the display panel 31. An adhesive layer 32 is arranged between the display panel 31 and the laminate for a display device 1. The first laminate film 10 and the bonding layer 2 are peelable from the second laminate film 20.

[0019] In the present disclosure, the first laminate film and the bonding layer are peelable from the second laminate film, and therefore, in a display device including the laminate for a display device, if a dent or scratch occurs on the surface of the first laminate film on the first functional layer side, the first laminate film and the bonding layer can be replaced.

[0020] On the other hand, since the first laminate film and the bonding layer can be peeled off from the second laminate film, there is a concern that when the laminate for a display device is repeatedly bent, the bonding layer may become lifted or peeled off, i.e., the bending resistance may be reduced.

[0021] For example, as shown in Figure 3, when a bending moment is applied to a display device 30 equipped with a display device laminate 10 from the display device laminate 10 side of the display device 30, the side of the display device 30 opposite the display device laminate 10 side contracts, and the display device laminate 10 side of the display device 30 expands, but there is a surface between them that does not expand or contract, i.e., a neutral plane NP.

[0022] Similarly, as shown in Figure 4, for example, when a bending moment is applied to a display device 30 equipped with a display device laminate 10 from the side opposite the display device laminate 10 side of the display device 30, the display device laminate 10 side of the display device 30 contracts and the side opposite the display device laminate 10 side of the display device 30 expands, but there is a surface between them that does not expand or contract, i.e., a neutral plane NP.

[0023] Generally, in bending, strain increases in proportion to the distance from the neutral plane. Here, the A2 value is calculated by multiplying the tensile modulus E2 of the second laminate film by the cube of the thickness of the second laminate film divided by 12 (h2 3 / 12). In the present disclosure, since the A2 value is a predetermined value or less, it can be said that the thickness of the second laminate film is relatively thin. When the thickness of the second laminate film is thin, the distance d1 from the neutral plane NP to the interface between the second laminate film 20 and the bonding layer 2 as shown in Figures 3 and 4 is shorter than when the thickness of the second laminate film is thick. Therefore, when the thickness of the second laminate film is thin, the strain at the interface between the second laminate film 20 and the bonding layer 2 can be reduced. This can suppress peeling between the bonding layer and the second laminate film. Therefore, although the first laminate film and the bonding layer can be peeled from the second laminate film, lifting and peeling of the bonding layer when bent can be suppressed. In particular, lifting and peeling of the bonding layer can be suppressed even when the laminate for a display device is repeatedly bent. Therefore, when the A2 value is a predetermined value or less, bending resistance can be improved.

[0024] The A1 value is the tensile modulus E1 of the first laminate film and the cube of the thickness of the first laminate film divided by 12 (h1 3 / 12) and indicates the difficulty of bending the first laminate film. The larger the A1 value, the more difficult the first laminate film is to bend, and the smaller the A1 value, the easier it is to bend. The A1 value also serves as an index of the hardness of the first laminate film. The larger the A1 value, the higher the hardness of the first laminate film, and the smaller the A1 value, the lower the hardness of the first laminate film. In addition, in the above formula (1), the value obtained by dividing the cube of the thickness of the first laminate film by 12 is used, referring to the definition of the second moment of area.

[0025] The A2 value is the tensile modulus E2 of the second laminate film and the cube of the thickness of the second laminate film divided by 12 (h2 3 / 12) and indicates the difficulty of bending the second laminate film. The larger the A2 value, the more difficult it is to bend the second laminate film, and the smaller the A2 value, the easier it is to bend the second laminate film. The A2 value also serves as an index of the hardness of the second laminate film. The larger the A2 value, the higher the hardness of the second laminate film, and the smaller the A2 value, the lower the hardness of the second laminate film. In addition, in the above formula (2), the value obtained by dividing the cube of the thickness of the second laminate film by 12 is used, referring to the definition of the second moment of area.

[0026] Here, the second moment of area I is a value indicating the difficulty of bending, and when the thickness of the film is h and the width of the film is b, I = b × h 3 / 12. As can be seen from this formula, the second moment of area I varies depending on the area of ​​the film. For example, if the area of ​​the film is large, the second moment of area increases, and a large force is required to bend the film. On the other hand, if the area of ​​the film is small, the second moment of area decreases, and a smaller force is required to bend the film. Therefore, in the present disclosure, the above formula (1) which does not include the thickness of the first laminate film and the above formula (2) which does not include the thickness of the second laminate film are adopted so that the value indicating the difficulty of bending does not change depending on the area of ​​the first laminate film and the area of ​​the second laminate film.

[0027] In the present disclosure, when the A1 value is equal to or greater than a predetermined value, the first laminate film is less likely to bend and has high hardness. Furthermore, when the A1 value is within a predetermined range, when the thickness of the first functional layer is equal to or greater than a predetermined value, the surface hardness of the first laminate film can be increased. Therefore, deformation of the first laminate film can be suppressed. Furthermore, when the first resin substrate contains a polyimide-based resin, the first resin substrate can be made more susceptible to elastic deformation and less susceptible to plastic deformation. Therefore, even if the first laminate film is deformed, it is more likely to return to its original shape. Therefore, in a display device including a laminate for a display device, when the surface of the laminate for a display device is pressed, deformation of the first laminate film can be suppressed and the first laminate film can be made more likely to recover from deformation.

[0028] In addition, in the present disclosure, since the A2 value is a predetermined value or less, the second laminate film is easy to bend and has low hardness. Therefore, in a display device including a laminate for a display device, if the bonding layer is deformed when the surface of the laminate for a display device is pressed, the second laminate film is also likely to deform along with the deformation of the bonding layer. As a result, the deformation of the bonding layer can be absorbed by the second laminate film.

[0029] Therefore, when the A1 value is equal to or greater than a predetermined value, and when the A1 value is within a predetermined range, the thickness of the first functional layer is equal to or greater than a predetermined value, the first resin base material contains a polyimide-based resin, and the A2 value is equal to or less than a predetermined value, the hardness can be increased, and therefore the scratch resistance can be improved.

[0030] Here, in the laminate for a display device, the first laminate film and the second laminate film are laminated via a bonding layer. The inventors of the present disclosure have found that in such a laminate for a display device, even if the surface hardness of the first laminate film alone is high, the surface hardness of the entire laminate for a display device may be low. In the present disclosure, since the first laminate film and the bonding layer are peelable from the second laminate film, a non-curing adhesive layer such as a pressure-sensitive adhesive layer or a heat-sensitive adhesive layer is typically used as the bonding layer, rather than a curing adhesive layer. Furthermore, in flexible displays, a non-curing adhesive layer that is softer than the curing adhesive layer is often used as the bonding layer for bending resistance. In this case, the bonding layer is softer than the first laminate film and the second laminate film. Therefore, if a bonding layer is present between the first laminate film and the second laminate film, when the surface of the display device laminate is pressed in a display device, the bonding layer is deformed, and at the same time, the components of the bonding layer migrate from the pressed area, i.e., the area where the pressure is high, to the surrounding area, i.e., the surrounding area where the pressure is low, which may make it difficult for the depression caused by the pressing to return to its original state, leading to a decrease in the surface hardness of the entire display device laminate.

[0031] Therefore, in the present disclosure, the A1 value is set to a predetermined value or more, and when the A1 value is within a predetermined range, the thickness of the first functional layer is set to a predetermined value or more, the first resin base material contains a polyimide-based resin, and the A2 value is set to a predetermined value or less, thereby making it possible to increase the surface hardness of the laminate for a display device as described above.

[0032] Therefore, the present disclosure can provide a laminate for a display device that satisfies all of the requirements of high hardness, bending resistance, and replaceability.

[0033] Furthermore, the laminate for a display device according to the present disclosure has excellent flex resistance and hardness, and therefore can be suitably used in flexible displays such as foldable displays, slidable displays, rollable displays, and bendable displays.

[0034] Hereinafter, each component of the laminate for a display device according to the present disclosure will be described.

[0035] 1. First Laminate Film The first laminate film in the present disclosure is disposed on the surface of the bonding layer opposite to the second laminate film, and has, in this order from the bonding layer side, a first resin substrate and a first functional layer.

[0036] (1) Properties of the First Laminate Film (a) A1 Value Calculated by Formula (1) In the first laminate film of the present disclosure, the A1 value calculated by the following formula (1) is within a predetermined range: A1 = E1 × h1 3 / 12 (1) (In the above formula (1), E1 represents the tensile modulus (Pa) of the first laminate film, and h1 represents the thickness (m) of the first laminate film.)

[0037] The A1 value is 0.10 × 10 -3 P.A.M. 3 or more, 0.14 × 10 -3 P.A.M. 3 or more, and may be 0.17 × 10 -3 P.A.M. 3 On the other hand, the A1 value may be 0.52 × 10 -3 P.A.M. 3 is less than or equal to 0.27 × 10 -3 P.A.M. 3or less, 0.40 × 10 -3 P.A.M. 3 That is, the A1 value may be 0.10×10 -3 P.A.M. 3 More than 0.52 x 10 -3 P.A.M. 3 is less than or equal to 0.14 × 10 -3 P.A.M. 3 More than 0.27 x 10 -3 P.A.M. 3 or less, and may be 0.17 × 10 -3 P.A.M. 3 More than 0.40 x 10 -3 P.A.M. 3 The A1 value may be equal to or less than the predetermined value. When the A1 value is equal to or more than the predetermined value, deformation of the first laminate film can be suppressed when the surface of the laminate for a display device is pressed in a display device including the laminate for a display device. Therefore, scratch resistance can be improved. When the A1 value is equal to or less than the predetermined value, bending resistance is improved.

[0038] Examples of methods for adjusting the A1 value include adjusting the tensile modulus of the first laminate film and adjusting the thickness of the first laminate film. Examples of methods for adjusting the tensile modulus of the first laminate film include adjusting the material of the first resin substrate and adjusting the material of the first functional layer. Examples of methods for adjusting the thickness of the first laminate film include adjusting the thickness of the first resin substrate and the first functional layer. When the first resin substrate contains a polyimide resin and the thickness of the first functional layer is equal to or greater than a predetermined value, the A1 value can be easily adjusted to be within a predetermined range.

[0039] (b) Tensile Modulus of First Laminate Film The tensile modulus of the first laminate film in the present disclosure is not particularly limited as long as it satisfies the above A1 value, but is, for example, 5.3 GPa or more and 6.5 GPa or less.

[0040] The tensile modulus of the first laminate film is measured in accordance with JIS K7127:1999. First, the first laminate film and the bonding layer are peeled off from the laminate for a display device. Next, the bonding layer is wiped off with alcohol or the like to obtain the first laminate film. Next, a rectangular test piece having a width of 10 mm and a length of 200 mm is cut out from the first laminate film. Next, a tensile test is performed using a tensile tester under the following conditions.

[0041] <Tensile test conditions> Gauge distance: 100 mm Initial distance between chucks: 100 mm Tensile speed: 50 mm / min Test environment: temperature 23°C, humidity 50±5% RH

[0042] In the stress-strain curve obtained by the tensile test, the slope of the line connecting the stress at a strain of 0.5% and the stress at a strain of 1% is determined, and this slope is taken as the tensile modulus. The tensile test is performed five times, and the tensile modulus of the first laminate film is taken as the arithmetic mean of three of the five measured values, excluding the minimum and maximum values. A Tensilon universal testing machine can be used as the tensile tester.

[0043] (c) Thickness of the First Laminate Film The thickness of the first laminate film in the present disclosure is appropriately adjusted so as to satisfy the above A1 value and the thickness of the first functional layer described below. The thickness of the first laminate film is, for example, 30 μm or more, or may be 40 μm or more, or 50 μm or more. On the other hand, the thickness of the first laminate film is, for example, 100 μm or less, or may be 90 μm or less, or may be 80 μm or less. That is, the thickness of the first laminate film is, for example, 30 μm or more and 100 μm or less, or may be 40 μm or more and 90 μm or less, or may be 50 μm or more and 80 μm or less. By having the thickness of the first laminate film within the above range, the A1 value can be easily adjusted to be within a predetermined range.

[0044] The thickness of the first laminate film is the arithmetic mean value of thicknesses measured at any 10 locations on a cross section of the laminate for a display device in the thickness direction observed with a scanning transmission electron microscope (STEM). The thickness of the laminate for a display device and the thickness of each layer of the laminate for a display device are measured in the same manner.

[0045] A specific example of a method for taking a cross-sectional photograph of a laminate for a display device will be described. First, the laminate for a display device is cut into a size of 1 mm x 10 mm, and a block is prepared by embedding the laminate for a display device in an embedding resin. Next, using an ultramicrotome equipped with a cryomicrotome, the block is frozen at -60°C to -50°C for 10 to 15 minutes. After that, a uniform slice without holes or the like and having a thickness of 70 nm to 100 nm is cut out. This uniform slice without holes or the like is used as the measurement sample. Next, a cross-sectional photograph of the measurement sample is taken using an STEM. A Leica EM FC6 manufactured by Leica Microsystems can be used as the cryomicrotome. A Leica EM UC6 manufactured by Leica Microsystems can be used as the ultramicrotome. A Hitachi High-Technologies Corporation S-4800 can be used as the scanning transmission electron microscope (STEM). When taking a cross-sectional photograph using the above-mentioned "S-4800," cross-section observation is performed with the detector set to "SE," the acceleration voltage set to "5 kV," and the emission current set to "10 μA."

[0046] The magnification is adjusted appropriately from 100x to 100,000x, preferably 500x to 50,000x, and more preferably 1,000x to 10,000x while adjusting the focus and observing the contrast and brightness to see if each layer can be distinguished. When taking a cross-sectional photograph using the above-mentioned "S-4800," the beam monitor aperture may be set to "3," the objective lens aperture to "3," and the WD to "8 mm."

[0047] Furthermore, when measuring the thickness of a laminate for a display device, it is important that the contrast of the interface between the laminate for a display device and the embedding resin can be observed as clearly as possible when the cross section is observed using an STEM. Furthermore, when measuring the thickness of each layer of a laminate for a display device, it is important that the contrast of the interface between the layer to be measured and other layers or the embedding resin can be observed as clearly as possible when the cross section is observed using an STEM. Therefore, if the interface is difficult to see due to insufficient contrast, a staining treatment using osmium tetroxide, ruthenium tetroxide, phosphotungstic acid, or the like may be performed. The staining treatment makes the interface easier to see.

[0048] Furthermore, the contrast of the interface may be difficult to see at higher magnifications. In such cases, observation is performed at both low and high magnifications. For example, observation is performed at two magnifications, high and low, such as 500x and 10,000x, or 1,000x and 20,000x. Then, as described above, the arithmetic mean value of the thicknesses at 10 arbitrary locations observed at each magnification is calculated, and the arithmetic mean value of the two arithmetic mean values ​​is used as the thickness value.

[0049] (2) First Functional Layer The first functional layer in the present disclosure is disposed on the surface of the first resin substrate opposite to the bonding layer.

[0050] The thickness of the first functional layer is 8 μm or more, preferably 11 μm or more, and more preferably 12 μm or more. Having the thickness of the first functional layer within the above range increases the surface hardness of the display laminate and improves scratch resistance. On the other hand, the upper limit of the thickness of the first functional layer is not particularly limited as long as it satisfies the A1 value, and may be, for example, 20 μm or less, 17 μm or less, or 15 μm or less. Furthermore, having the thickness of the first functional layer within the above range improves bending resistance. Specifically, the thickness of the first functional layer is 8 μm or more and 20 μm or less, or may be 11 μm or more and 17 μm or less, or may be 12 μm or more and 15 μm or less.

[0051] Examples of the first functional layer include a hard coat layer, an anti-reflection layer, an anti-glare layer, and an anti-fouling layer. The first functional layer may be a single layer or may have multiple layers. The first functional layer may be a layer having a single function or may have multiple layers having different functions.

[0052] (a) Hard Coat Layer The hard coat layer is a member for increasing the surface hardness. By providing the hard coat layer, scratch resistance can be improved.

[0053] Here, the "hard coat layer" refers to a member for increasing surface hardness, and specifically refers to a layer that exhibits a hardness of "H" or more when the laminate for a display device according to the present disclosure has a hard coat layer and is subjected to a pencil hardness test specified in JIS K 5600-5-4:1999.

[0054] When the laminate for a display device according to the present disclosure has a hard coat layer, the pencil hardness of the surface of the laminate for a display device on the hard coat layer side is preferably H or more, more preferably 2H or more, and even more preferably 3H or more. The measurement of pencil hardness will be described later.

[0055] The hard coat layer may be a single layer or may have multiple layers.

[0056] Examples of materials for the hard coat layer include organic materials, inorganic materials, and organic-inorganic composite materials. Among these, organic materials are preferred. Specifically, the hard coat layer preferably contains a cured product of a resin composition containing a polymerizable compound. The cured product of the resin composition containing a polymerizable compound can be obtained by polymerizing the polymerizable compound using a polymerization initiator as needed, using a known method.

[0057] The polymerizable compound has at least one polymerizable functional group in the molecule. As the polymerizable compound, for example, at least one of a radical polymerizable compound and a cation polymerizable compound can be used. As the polymerizable compound, a general polymerizable compound used in a hard coat layer can be used.

[0058] The hard coat layer preferably contains inorganic particles or organic particles, more preferably inorganic particles, which can improve the hardness of the hard coat layer. As the inorganic particles and organic particles, general inorganic particles and organic particles used in hard coat layers can be used.

[0059] The hard coat layer may also contain an ultraviolet absorber, which can prevent discoloration and deterioration of the resin substrate due to ultraviolet rays.

[0060] The hard coat layer may also contain an antifouling agent, which can impart antifouling properties to the laminate for a display device.

[0061] The hard coat layer may further contain additives as required. The additives are appropriately selected depending on the function to be imparted to the hard coat layer and are not particularly limited, but examples thereof include inorganic or organic particles for adjusting the refractive index, infrared absorbers, antiglare agents, antistatic agents, colorants, leveling agents, surfactants, lubricants, various sensitizers, flame retardants, adhesion promoters, polymerization inhibitors, antioxidants, light stabilizers, surface modifiers, and spectral transmittance adjusters.

[0062] The thickness of the hard coat layer may be adjusted as needed to obtain the desired surface hardness, and is appropriately adjusted to satisfy the above-mentioned A1 value and the thickness of the first functional layer. When the first functional layer has only a hard coat layer, the thickness of the hard coat layer is the same as the thickness of the first functional layer. Furthermore, the thickness of the hard coat layer is, for example, preferably 5 μm or more, more preferably 9 μm or more, and even more preferably 12 μm or more. By having the thickness of the hard coat layer within the above range, the A1 value can be easily adjusted to fall within a predetermined range. Furthermore, if the thickness of the hard coat layer is within the above range, sufficient hardness as a hard coat layer can be obtained. Meanwhile, the upper limit of the thickness of the hard coat layer is the same as the upper limit of the thickness of the first functional layer.

[0063] The method for forming the hard coat layer is appropriately selected depending on the material of the hard coat layer, and examples thereof include a method of applying a resin composition containing the polymerizable compound or the like onto the first resin substrate and curing it, a vapor deposition method, and a sputtering method.

[0064] (b) Antireflection layer An antireflection layer may be disposed on the surface of the hard coat layer opposite to the first resin substrate. By disposing the antireflection layer, reflection of external light can be suppressed, and visibility can be improved.

[0065] The antireflection layer may be composed of a single layer or multiple layers.

[0066] The antireflection layer may be a general antireflection layer, and examples thereof include a single layer film containing a material having a lower refractive index than the hard coat layer, a multilayer film having a high refractive index layer and a low refractive index layer from the first resin substrate side, a multilayer film in which high refractive index layers and low refractive index layers are alternately stacked from the first resin substrate side, and a multilayer film having a medium refractive index layer, a high refractive index layer, and a low refractive index layer in this order from the first resin substrate side.

[0067] The thickness of the antireflection layer is appropriately adjusted so as to satisfy the above-mentioned A1 value and the thickness of the first functional layer, and is, for example, 90 nm or more and 300 nm or less.

[0068] (c) Antifouling layer An antifouling layer may be disposed on the surface of the hard coat layer opposite to the first resin substrate. When the antireflection layer is disposed on the surface of the hard coat layer opposite to the first resin substrate, the antireflection layer and the antifouling layer may be disposed in this order on the surface of the hard coat layer opposite to the first resin substrate. By disposing the antifouling layer, antifouling properties can be imparted to the laminate for a display device. Materials for general antifouling layers can be used as the material for the antifouling layer.

[0069] The thickness of the antifouling layer is appropriately adjusted so as to satisfy the above-mentioned A1 value and the thickness of the first functional layer. The thickness of the antifouling layer is, for example, 1 nm or more, or may be 2 nm or more, or 3 nm or more. On the other hand, the thickness of the antifouling layer is, for example, 30 nm or less, or may be 20 nm or less, or may be 10 nm or less. Specifically, the thickness of the antifouling layer is, for example, 1 nm or more and 30 nm or less, or may be 2 nm or more and 20 nm or less, or may be 3 nm or more and 10 nm or less. When the thickness of the antifouling layer is within the above range, the antifouling properties and durability can be improved.

[0070] (3) First Resin Substrate The first resin substrate in the present disclosure is a transparent member that supports the first functional layer.

[0071] The first resin substrate contains a polyimide-based resin. Examples of polyimide-based resins include polyimide, polyamideimide, polyetherimide, and polyesterimide. These may be used alone or in combination of two or more.

[0072] The polyimide resin is not particularly limited as long as it has transparency, but among the above, polyimide and polyamideimide are preferably used. As the polyimide and polyamideimide, the polyimide and polyamideimide described in WO 2021 / 060559 are preferably used.

[0073] The first resin substrate may further contain other resins in addition to the polyimide resin. Examples of the other resins include polyamide resins and acrylic resins. Examples of the acrylic resins include polymethyl(meth)acrylate and polyethyl(meth)acrylate.

[0074] The first resin substrate may further contain additives as needed, such as ultraviolet absorbers, light stabilizers, antioxidants, inorganic particles, silica fillers for facilitating winding, surfactants for improving film-forming properties and defoaming properties, and adhesion improvers.

[0075] The thickness of the first resin substrate is appropriately adjusted to satisfy the A1 value. The thickness of the first resin substrate is, for example, 25 μm or more, may be 30 μm or more, or may be 50 μm or more. On the other hand, the thickness of the first resin substrate is, for example, 80 μm or less, may be 75 μm or less, or may be 65 μm or less. That is, the thickness of the first resin substrate is, for example, 25 μm or more and 80 μm or less, may be 30 μm or more and 75 μm or less, or may be 50 μm or more and 65 μm or less.

[0076] (4) Other Functional Layers The first laminate film according to the present disclosure may have other functional layers on the surface of the first resin substrate opposite to the first functional layer. Examples of the other functional layers include a primer layer and a color-adjusting layer.

[0077] (a) Primer layer A primer layer may be disposed on the surface of the first resin substrate opposite to the first functional layer. The primer layer can improve adhesion between the first laminate film and the bonding layer.

[0078] The material for the primer layer is not particularly limited as long as it is a material that can enhance the adhesion between the first laminate film and the bonding layer, and general materials for primer layers can be used.

[0079] The thickness of the primer layer may be any thickness that can enhance the adhesion between the first laminate film and the bonding layer, and is appropriately adjusted to satisfy the above-mentioned A1 value. The thickness of the primer layer may be, for example, 0.05 μm or more, or 0.1 μm or more. On the other hand, the thickness of the primer layer may be, for example, 3 μm or less, or 2 μm or less. Specifically, the thickness of the primer layer may be, for example, 0.05 μm or more and 3 μm or less, or 0.1 μm or more and 2 μm or less.

[0080] (b) Color Adjusting Layer A color adjusting layer may be disposed on the surface of the first resin substrate opposite the first functional layer. The color adjusting layer is a component that adjusts the color of the first laminate film. For example, if the first resin substrate contains a polyimide resin, the material may have a yellowish tint due to its characteristics. By disposing the color adjusting layer, the color of the first laminate film can be made closer to colorless and transparent.

[0081] The color-adjusting layer contains, for example, a resin and a blue colorant, and general resins and blue colorants can be used as the resin and blue colorant.

[0082] The thickness of the color-adjusting layer may be any thickness that allows color adjustment and is appropriately adjusted to satisfy the above-mentioned A1 value. The thickness of the color-adjusting layer is, for example, 0.05 μm or more, or may be 0.1 μm or more, or may be 0.3 μm or more. On the other hand, the thickness of the color-adjusting layer is, for example, 2 μm or less, or may be 1 μm or less, or may be 0.8 μm or less. Specifically, the thickness of the color-adjusting layer is, for example, 0.05 μm or more and 2 μm or less, or may be 0.1 μm or more and 1 μm or less, or may be 0.3 μm or more and 0.8 μm or less.

[0083] 2. Second Laminate Film The second laminate film in the present disclosure is disposed on the surface of the bonding layer opposite to the first laminate film, and has, in this order from the bonding layer side, a second functional layer and a second resin substrate.

[0084] (1) Properties of the Second Laminate Film (a) A2 Value Calculated by Formula (2) In the second laminate film of the present disclosure, the A2 value calculated by the following formula (2) is within a predetermined range: A2 = E2 × h2 3 / 12 (2) (In the above formula (2), E2 represents the tensile modulus (Pa) of the second laminate film, and h2 represents the thickness (m) of the second laminate film.)

[0085] The A2 value is 0.07 × 10 -3 P.A.M. 3 is less than or equal to 0.03 × 10 -3 P.A.M. 3 It may be 0.02 × 10 or less. -3 P.A.M. 3 or less. When the A2 value is a predetermined value or less, as described above, when a display device including the laminate for a display device is bent, the distance from the neutral plane to the interface between the second laminate film and the bonding layer is shortened. Therefore, the strain at the interface between the second laminate film and the bonding layer can be reduced. This can suppress lifting or peeling of the bonding layer when bent, and improve bending resistance. On the other hand, as described above, since the bonding layer is softer than the second laminate film, the lower limit of the A2 value is not particularly limited, and can be, for example, 0.01 × 10 -3 P.A.M. 3 Specifically, the A2 value is 0.01 × 10-3 P.A.M. 3 More than 0.07 x 10 -3 P.A.M. 3 is less than or equal to 0.01 × 10 -3 P.A.M. 3 More than 0.03 x 10 -3 P.A.M. 3 It may be 0.01 × 10 or less, -3 P.A.M. 3 More than 0.02 x 10 -3 P.A.M. 3 It may be the following:

[0086] Examples of methods for adjusting the A2 value include adjusting the tensile modulus of the second laminate film and adjusting the thickness of the second laminate film. Examples of methods for adjusting the tensile modulus of the second laminate film include adjusting the material of the second resin substrate and adjusting the material of the second functional layer. Examples of methods for adjusting the thickness of the second laminate film include adjusting the thickness of the second resin substrate and the second functional layer.

[0087] (b) Tensile Modulus of Second Laminate Film The tensile modulus of the second laminate film in the present disclosure is not particularly limited as long as it satisfies the above A2 value, but is, for example, 4.0 GPa or more and 6.5 GPa or less.

[0088] The tensile modulus of the second laminate film is measured in accordance with JIS K7127:1999. First, the first laminate film and the bonding layer are peeled from the laminate for a display device to obtain a second laminate film. If the laminate for a display device is attached to a display device, the first laminate film and the bonding layer are peeled from the laminate for a display device, and then the second laminate film is peeled from the display device. In many cases, the laminate for a display device is attached via an adhesive layer, so the adhesive layer can be peeled off by heating using a hair dryer or the like. If an adhesive component is attached to the second laminate film, the adhesive component is wiped off with alcohol or the like. Because the tensile modulus of the adhesive component is significantly lower than that of the second laminate film, slight wiping unevenness of the adhesive component does not affect the measurement of the tensile modulus of the second laminate film. Next, a rectangular test piece measuring 10 mm wide and 200 mm long is cut from the second laminate film. A tensile test is then performed using a tensile tester. The conditions for the tensile test are the same as those for the tensile test in the method for measuring the tensile modulus of the first laminate film described above. In the stress-strain curve obtained by the tensile test, the slope of the line connecting the stress at a strain of 0.5% and the stress at a strain of 1% is determined, and this slope is taken as the tensile modulus. The tensile test is performed five times, and the tensile modulus of the second laminate film is taken as the arithmetic mean of three of the five measured values, excluding the minimum and maximum values. A Tensilon universal testing machine can be used as the tensile tester.

[0089] (c) Thickness of the Second Laminate Film The thickness of the second laminate film in the present disclosure is appropriately adjusted to satisfy the A2 value. The thickness of the second laminate film is, for example, preferably 50 μm or less, and may be 40 μm or less, or may be 30 μm or less. When the thickness of the second laminate film is a predetermined value or less, the distance from the neutral plane to the interface between the second laminate film and the bonding layer is shortened when a display device including the display device laminate is bent. This reduces the strain at the interface between the second laminate film and the bonding layer. This prevents the bonding layer from lifting or peeling during bending, improving bending resistance. On the other hand, the lower limit of the thickness of the second laminate film is not particularly limited, but may be, for example, 20 μm or more or 25 μm or more. Specifically, the thickness of the second laminate film is 20 μm or more to 50 μm or less, or may be 20 μm or more to 40 μm or less, or 25 μm or more to 40 μm or less, or 25 μm or more to 30 μm or less.

[0090] (d) Water Contact Angle In the present disclosure, the water contact angle of the surface of the second laminate film on the second functional layer side is, for example, preferably 90° or more, more preferably 94° or more, and even more preferably 98° or more. Having the water contact angle within the above range can suppress adhesive residue when the first laminate film and the bonding layer are peeled off from the second laminate film. Furthermore, in a display device including a laminate for a display device, when the first laminate film and the bonding layer are peeled off from the laminate for a display device to expose the second laminate film, having the water contact angle within the above range can impart antifouling properties to the surface of the second laminate film on the second functional layer side. Meanwhile, the water contact angle is, for example, preferably 113° or less, more preferably 110° or less, and even more preferably 105° or less. Having the water contact angle within the above range can easily adjust the adhesive strength of the bonding layer to the second laminate film to be within a predetermined range. Specifically, the water contact angle is preferably 90° or more and 113° or less, more preferably 94° or more and 110° or less, and even more preferably 98° or more and 105° or less.

[0091] The water contact angle of the surface of the second laminate film on the side of the second functional layer is measured by the θ / 2 method in accordance with the sessile drop method of JIS R3257: 1999. Specifically, 2 μL of pure water is dropped onto the surface of the second laminate film on the side of the second functional layer at a temperature of 20° C. and a humidity of 50±5% RH, and the contact angle is measured 20 seconds after the drop has settled.

[0092] As a method for adjusting the water contact angle of the surface of the second laminate film on the side of the second functional layer, for example, a method of adding an antifouling agent to the second functional layer can be mentioned.

[0093] (2) Second Functional Layer The second functional layer in the present disclosure is disposed between the second resin substrate and the bonding layer.

[0094] The thickness of the second functional layer is appropriately adjusted to satisfy the A2 value. The thickness of the second functional layer is, for example, 2 μm or more, or may be 4 μm or more, or 5 μm or more. On the other hand, the thickness of the second functional layer is, for example, 10 μm or less, or may be 8 μm or less, or may be 6 μm or less. That is, the thickness of the second functional layer is, for example, 2 μm or more and 10 μm or less, or may be 4 μm or more and 8 μm or less, or may be 5 μm or more and 6 μm or less.

[0095] The second functional layer is similar to the first functional layer.

[0096] (3) Second Resin Substrate The second resin substrate in the present disclosure is a transparent member that supports the second functional layer.

[0097] The resin constituting the second resin substrate is not particularly limited as long as it is transparent, and examples thereof include polyimide resins, polyamide resins, polyester resins, cellulose resins, and acrylic resins. Examples of polyimide resins include polyimide, polyamideimide, polyetherimide, and polyesterimide. Examples of polyester resins include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of cellulose resins include triacetyl cellulose (TAC). Examples of acrylic resins include polymethyl(meth)acrylate and polyethyl(meth)acrylate. These resins may be used alone or in combination of two or more.

[0098] The second resin substrate containing at least one of a polyimide resin and a polyamide resin is advantageous in terms of flex resistance, hardness, and transparency, while the second resin substrate containing polyethylene terephthalate, triacetyl cellulose, or an acrylic resin is advantageous in terms of cost.

[0099] When the second resin substrate contains a polyimide-based resin, the same applies as in the first resin substrate containing a polyimide-based resin.

[0100] The second resin base material may further contain additives as needed, which are the same as the additives used in the first resin base material.

[0101] The thickness of the second resin substrate is appropriately adjusted to satisfy the A2 value. The thickness of the second resin substrate is, for example, 20 μm or more, and may be 25 μm or more. On the other hand, the thickness of the second resin substrate is, for example, 48 μm or less, may be 46 μm or less, or may be 35 μm or less. That is, the thickness of the second resin substrate is, for example, 20 μm or more and 48 μm or less, may be 20 μm or more and 46 μm or less, may be 25 μm or more and 46 μm or less, or may be 25 μm or more and 35 μm or less.

[0102] (4) Other Functional Layers The second laminate film according to the present disclosure may have other functional layers on the surface of the second resin substrate opposite to the second functional layer, which are the same as the other functional layers used in the first laminate film.

[0103] 3. Bonding Layer The bonding layer in the present disclosure is a member disposed between the first laminate film and the second laminate film and serves to bond the first laminate film and the second laminate film together. The bonding layer is also peelable from the second laminate film.

[0104] The bonding layer is not particularly limited as long as it can bond the first laminate film and the second laminate film and can be peeled from the second laminate film, and examples thereof include a pressure-sensitive adhesive layer and a heat-sensitive adhesive layer. Of these, a pressure-sensitive adhesive layer is preferred.

[0105] The pressure-sensitive adhesive layer includes a pressure-sensitive adhesive. Examples of the pressure-sensitive adhesive include optically clear adhesives (OCAs). Specific examples include acrylic adhesives, urethane adhesives, and silicone adhesives.

[0106] The heat-sensitive adhesive layer contains a heat-sensitive adhesive such as a heat-sealing agent. Examples of resins contained in the heat-sensitive adhesive include heat-weldable thermoplastic resins. Examples of such thermoplastic resins include, but are not limited to, acrylic resins, vinyl chloride-vinyl acetate copolymers, polyamide resins, polyester resins, polyester urethane resins, chlorinated polypropylene, chlorinated rubber, urethane resins, epoxy resins, styrene resins, polyolefin resins, silicone resins, polyvinyl acetal resins such as polyvinyl butyral (PVB), and polyether urethane resins. These thermoplastic resins may be used alone or in combination of two or more.

[0107] The heat-sensitive adhesive may further contain a curing agent, thereby improving heat resistance and adhesiveness. Examples of the curing agent include an isocyanate-based curing agent, an epoxy-based curing agent, and a melamine-based curing agent. The curing agent may be used alone or in combination of two or more. When the heat-sensitive adhesive contains a curing agent, the heat-sensitive adhesive layer contains a cured product of the heat-sensitive adhesive.

[0108] The heat-sensitive adhesive may also contain additives as needed. Examples of additives include light stabilizers, ultraviolet absorbers, infrared absorbers, antioxidants, plasticizers, coupling agents, antifoaming agents, fillers, inorganic or organic particles for adjusting the refractive index, antistatic agents, colorants such as blue pigments and purple pigments, leveling agents, surfactants, lubricants, various sensitizers, flame retardants, adhesion promoters, polymerization inhibitors, and surface modifiers. These additives can be appropriately selected from commonly used additives. The content of the additives can be appropriately set.

[0109] The thickness of the bonding layer is, for example, 50 μm or less, and may be 30 μm or less. On the other hand, the lower limit of the thickness of the bonding layer is not particularly limited, and may be, for example, 20 μm or more, and may be 25 μm or more. That is, the thickness of the bonding layer may be, for example, 20 μm or more and 50 μm or less, and may be 25 μm or more and 30 μm or less. In the present disclosure, even when the thickness of the bonding layer is relatively thick, the surface hardness of the surface on the first laminate film side of the laminate for a display device can be increased, and scratch resistance can be improved.

[0110] The bonding layer may be, for example, a film-like bonding layer. Alternatively, the bonding layer may be formed by applying an adhesive composition onto the first laminate film or the second laminate film.

[0111] 4. Characteristics of the Laminate for a Display Device (1) Thickness of the Laminate for a Display Device The thickness of the laminate for a display device in the present disclosure is, for example, 110 μm or more, or may be 120 μm or more, or may be 130 μm or more. On the other hand, the thickness of the laminate for a display device is, for example, 180 μm or less, or may be 170 μm or less, or may be 160 μm or less. Specifically, the thickness of the laminate for a display device is 110 μm or more and 180 μm or less, or may be 120 μm or more and 170 μm or less, or may be 130 μm or more and 160 μm or less.

[0112] (2) Peelability In the present disclosure, the first laminate film and the bonding layer are peelable from the second laminate film.

[0113] The phrase "the first laminate film and the bonding layer can be peeled from the second laminate film" means that no adhesive residue is left when the first laminate film and the bonding layer are peeled from the second laminate film. Furthermore, "no adhesive residue" is defined as follows. First, a 180-degree peel test is performed on the display device laminate in accordance with Method 1 of JIS Z0237:2009, and the first laminate film and the bonding layer are peeled from the display device laminate to obtain a second laminate film. Specifically, a test piece measuring 25 mm wide and 200 mm long is cut out from the display device laminate. Next, a 2 kg roller is moved back and forth three times using a pressure-bonding device to attach the second laminate film side of the test piece to a stainless steel plate via a strong adhesive. The test piece is then aged for 24 hours at a temperature of 25°C and a humidity of 50±5% RH. Next, using a tensile tester, the test piece is peeled 180 degrees from the stainless steel plate at a temperature of 25°C, a humidity of 50±5% RH, a peel angle of 180°, and a peel speed of 300 mm / min. At this time, the ends of the first laminate film and the bonding layer previously peeled from the test piece are fixed to the upper chuck of the tensile tester, and the test piece is fixed to the lower chuck. A Tensilon universal testing machine can be used as the tensile tester. Next, after the 180-degree peel test, black tape is applied to the side of the second laminate film opposite the side where the bonding layer was located, and the side where the bonding layer of the second laminate film was located is visually inspected by reflection under a bright room fluorescent lamp of 1300 lux to 1700 lux. Then, an arbitrary 2 cm x 2 cm square area is selected, and the area of ​​the adhesive residue within the area is determined. If the area of ​​the adhesive residue is 1% or less, it is considered that there is no adhesive residue.

[0114] In addition, when the size of the laminate for a display device layer is small and a test piece having a width of 25 mm and a length of 200 mm cannot be prepared, the size of the test piece may be smaller than 25 mm in width and 200 mm in length.

[0115] When the first laminate film and the bonding layer are peeled off from the second laminate film, no adhesive residue is left, which prevents the adhesive residue from becoming foreign matter and causing poor biting when the first laminate film and the bonding layer are replaced.

[0116] In the present disclosure, the adhesive strength of the bonding layer to the second laminate film is, for example, preferably 230 mN / 25 mm or more, more preferably 500 mN / 25 mm or more, and even more preferably 750 mN / 25 mm or more. When the adhesive strength is within the above range, the first laminate film and the bonding layer can be peeled from the second laminate film, but peeling between the second laminate film and the bonding layer when bent can be suppressed. Furthermore, even when the laminate for a display device is repeatedly bent, the peeling can be suppressed. Meanwhile, the adhesive strength of the bonding layer to the second laminate film is, for example, preferably 10,000 mN / 25 mm or less, more preferably 7,700 mN / 25 mm or less, and even more preferably 5,000 mN / 25 mm or less. When the adhesive strength is within the above range, adhesive residue can be suppressed when the first laminate film and the bonding layer are peeled from the second laminate film. Specifically, the adhesive strength of the bonding layer to the second laminate film is preferably 230 mN / 25 mm or more and 10,000 mN / 25 mm or less, more preferably 500 mN / 25 mm or more and 7,700 mN / 25 mm or less, and even more preferably 750 mN / 25 mm or more and 5,000 mN / 25 mm or less.

[0117] The adhesive strength of the bonding layer to the second laminate film is measured in accordance with Method 1 of JIS Z0237:2009. Specifically, first, a test piece 25 mm wide and 200 mm long is cut out from the display device laminate. Next, a 2 kg roller is rolled back and forth three times using a pressure-bonding device to attach the second laminate film side of the test piece to a stainless steel plate via a strong adhesive. The test piece is then aged for 24 hours at a temperature of 25°C and a humidity of 50±5% RH. Next, using a tensile tester, the test piece is peeled 180 degrees from the stainless steel plate at a temperature of 25°C, a humidity of 50±5% RH, a peel angle of 180°, and a peel speed of 300 mm / min, and the adhesive strength is measured. At this time, the ends of the first laminate film and bonding layer previously peeled from the test piece are fixed to the upper chuck of the tensile tester, and the test piece is fixed to the lower chuck. A Tensilon universal testing machine can be used as the tensile tester. In the 180-degree peel test, the measurement value for the first 25 mm length is ignored. After that, the measurement values ​​for a length of 100 mm or more peeled from the stainless steel plate are averaged to obtain the adhesive strength value. The 180-degree peel test is performed five times, and the adhesive strength of the bonding layer to the second laminate film is the arithmetic mean value of the three measurements excluding the maximum and minimum values ​​of the five measurements.

[0118] If the size of the laminate for a display device layer is small and it is not possible to prepare a test piece with a width of 25 mm and a length of 200 mm, the size of the test piece may be smaller than 25 mm in width and 200 mm in length. If the width of the test piece is not 25 mm, the adhesive strength (actual measured value) measured by the 180-degree peel test is converted to a 25 mm width using the following formula: Adhesive strength converted to 25 mm width (N / 25 mm) = Actual measured adhesive strength (N) × 25 (mm) / Width of test piece (mm)

[0119] Methods for adjusting the adhesive strength of the bonding layer to the second laminate film include, for example, adjusting the water contact angle on the surface of the second laminate film on the second functional layer side, adjusting the thickness of the bonding layer, and adjusting the material of the bonding layer. A low water contact angle tends to increase the adhesive strength, while a high water contact angle tends to decrease the adhesive strength. By setting the water contact angle within a predetermined range, the adhesive strength can be easily adjusted to fall within the predetermined range. Furthermore, a thin bonding layer tends to decrease the adhesive strength, while a thick bonding layer tends to increase the adhesive strength.

[0120] (3) Total Light Transmittance The total light transmittance of the laminate for a display device according to the present disclosure is, for example, preferably 85% or more, more preferably 88% or more, and even more preferably 90% or more. Such a high total light transmittance results in good transparency.

[0121] Here, the total light transmittance of the laminate for a display device is measured in accordance with JIS K7361-1: 1997. As a measuring device, a haze meter HM150 manufactured by Murakami Color Research Laboratory can be used.

[0122] (4) Haze The haze of the laminate for a display device according to the present disclosure is, for example, preferably 5% or less, more preferably 2% or less, and even more preferably 1% or less. Such a low haze results in good transparency.

[0123] Here, the haze of the laminate for a display device is measured in accordance with JIS K7136: 2000. As a measuring device, a haze meter HM150 manufactured by Murakami Color Research Laboratory can be used.

[0124] (5) Bending Resistance The laminate for a display device according to the present disclosure has bending resistance. Specifically, when the laminate for a display device is subjected to a dynamic bending test described below, it is preferable that the laminate for a display device does not crack, break, or peel off.

[0125] Here, in the dynamic bending test, "cracking" refers to a phenomenon in which a crack occurs in the laminate for a display device. "Fracture" refers to a phenomenon in which the laminate for a display device completely breaks into two pieces. "Peeling" refers to a phenomenon in which any layer constituting the laminate for a display device peels off or lifts off.

[0126] The dynamic bending test is performed as follows. As shown in FIG. 5( a), in the dynamic bending test, first, a short side 1C of a 20 mm × 100 mm laminate 1 for a display device and a short side 1D opposite the short side 1C are fixed by parallel fixing portions 51, respectively. Also, as shown in FIG. 5( a), the fixing portions 51 are slidable horizontally. Next, as shown in FIG. 5( b), the fixing portions 51 are moved closer to each other to deform the laminate 1 for a display device so as to fold it. Furthermore, as shown in FIG. 5( c), the fixing portions 51 are moved to a position where the distance d between the two opposing short side portions 1C, 1D fixed by the fixing portions 51 of the laminate 1 for a display device becomes a predetermined value, and then the fixing portions 51 are moved in the opposite direction to eliminate the deformation of the laminate 1 for a display device. By moving the fixing portions 51 as shown in FIGS. 5( a) to 5( c), the laminate 1 for a display device can be folded 180°. Furthermore, by conducting a dynamic bending test so that the bent portion 1E of the laminate for a display device 1 does not protrude from the lower end of the fixing portion 51 and controlling the distance d when the fixing portion 51 is closest, it is possible to set the distance d between the two opposing short side portions 1C, 1D of the laminate for a display device 1 to a predetermined value. For example, when the distance d between the two opposing short side portions 1C, 1D is 10 mm, the outer diameter of the bent portion 1E is considered to be 10 mm.

[0127] It is preferable that the laminate for a display device does not crack, break, or peel when a test in which the laminate for a display device 1 is folded 180° so that the distance d between the opposing short sides 1C and 1D of the laminate for a display device is 8 mm is repeated 200,000 times. Furthermore, it is more preferable that the laminate for a display device does not crack, break, or peel when a test in which the laminate for a display device 1 is folded 180° so that the distance d between the opposing short sides 1C and 1D of the laminate for a display device is 10 mm is repeated 200,000 times.

[0128] In the dynamic bending test, it is preferable that the laminate for a display device does not crack or break when the laminate for a display device is folded so that the first laminate film is on the inside.

[0129] (6) Pencil Hardness The pencil hardness of the surface of the laminate for a display device according to the present disclosure on the side of the first functional layer is preferably H or more, more preferably 2H or more, and even more preferably 3H or more.

[0130] Here, the pencil hardness is measured by the pencil hardness test specified in JIS K5600-5-4:1999. Specifically, first, a laminate for a display device is bonded to a 1 mm thick glass plate via an optical adhesive (3M "8146-3", adhesive layer thickness 100 μm) to prepare a test piece. This is because in actual display devices, a laminate for a display device is often bonded to the surface of the display device via an adhesive layer. Next, using a test pencil specified in JIS S6006:2020, a pencil hardness test specified in JIS K5600-5-4:1999 is performed on the surface of the first functional layer side of the laminate for a display device. The measurement conditions are an angle of 45°, a load of 750 g, a speed of 13 mm / s to 15 mm / s, a temperature of 25°C, and a humidity of 50±5% RH.

[0131] In the pencil hardness test, the highest pencil hardness that does not cause dents or scratches is evaluated. When measuring pencil hardness, multiple pencils of different hardness are used, and the pencil hardness test is performed five times for each pencil. If no dents or scratches are caused on the surface of the test piece four or more times out of the five, it is determined that the pencil of that hardness did not cause dents or scratches on the surface of the test piece. Dents and scratches refer to those that are visually observed when the surface of the test piece that has undergone the pencil hardness test is observed through transmission under fluorescent light.

[0132] 5. Uses of the Laminate for a Display Device The laminate for a display device according to the present disclosure can be used as a component arranged on the viewer's side of the display panel in a display device. The laminate for a display device according to the present disclosure can be used in display devices such as smartphones, tablet devices, wearable devices, personal computers, televisions, digital signage, public information displays (PIDs), and in-vehicle displays. In particular, the laminate for a display device according to the present disclosure can be suitably used in flexible displays such as foldable displays, slidable displays, rollable displays, and bendable displays.

[0133] When the laminate for a display device according to the present disclosure is used in a display device, it is arranged so that the surface on the second laminate film side faces the display panel side and the surface on the first laminate film side faces the viewer side.

[0134] The method for disposing the laminate for a display device according to the present disclosure on the surface of the display device is not particularly limited, and examples thereof include a method using an adhesive layer, etc. As the adhesive layer, a known adhesive layer used for adhering laminates for a display device can be used.

[0135] 6. Modifications In the above-described embodiment, an example in which the first resin substrate contains a polyimide-based resin has been described, but the present invention is not limited to this. Any resin may be used for the first resin substrate as long as the A1 value is within a predetermined range and the A2 value is equal to or less than a predetermined value. In particular, it is preferable that the first resin substrate contains a polyester-based resin. Examples of polyester-based resins include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. When the first resin substrate contains a polyester-based resin, the present invention is the same as the above-described embodiment, except that the first resin substrate contains a polyester-based resin instead of a polyimide-based resin.

[0136] B. Display Device A display device according to the present disclosure includes a display panel and the above-described laminate for a display device disposed on the viewer side of the display panel, with the laminate for a display device being disposed so that the surface of the laminate for a display device on the second laminate film side faces the display panel.

[0137] Fig. 6 is a schematic cross-sectional view showing an example of a display device according to the present disclosure. As shown in Fig. 6, a display device 30 includes a display panel 31 and a laminate for a display device 1 arranged on the viewer's side of the display panel 31. The laminate for a display device 1 is arranged so that the surface on the second laminate film 20 side faces the display panel 31. An adhesive layer 32 is arranged between the display panel 31 and the laminate for a display device 1.

[0138] The laminate for a display device is the same as the above-mentioned laminate for a display device.

[0139] The method for disposing the laminate for a display device according to the present disclosure on the surface of a display device is not particularly limited, and examples thereof include a method using an adhesive layer.

[0140] Examples of the display panel in the present disclosure include an organic EL display device and a liquid crystal display device.

[0141] The display device according to the present disclosure may have a touch panel member between the display panel and the laminate for a display device.

[0142] The display device according to the present disclosure is preferably a flexible display such as a foldable display, a slidable display, a rollable display, a bendable display, etc. The display device according to the present disclosure includes the above-described laminate for a display device, and is therefore suitable as a flexible display.

[0143] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any configuration that is substantially identical to the technical idea described in the claims of the present disclosure and that provides similar effects is included within the technical scope of the present disclosure.

[0144] The present disclosure will be further described below with reference to Examples and Comparative Examples. Using the materials listed below, laminates for display devices of Examples 1 to 11 and Comparative Examples 1 to 9 were produced in the combinations shown in Table 1 below.

[0145] [Materials] (1) Composition for Hard Coat Layer Compositions 1 to 3 for hard coat layer were prepared by blending the components so as to obtain the formulations shown below.

[0146] <Hard Coat Layer Composition 1> Urethane acrylate ("EBECRYL8254" manufactured by Daicel Allnex Corporation): 60 parts by mass Silica particles (solid content 20% by mass, solvent MIBK (methyl isobutyl ketone), average primary particle diameter 45 nm): 35 parts by mass (value converted to 100% by mass of solid content) Leveling agent ("KY-1203" manufactured by Shin-Etsu Chemical Co., Ltd., solid content 20% by mass, solvent mixed solvent of MEK (methyl ethyl ketone) and MIBK (methyl isobutyl ketone): 0.5 parts by mass (value converted to 100% by mass of solid content) Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, "Omnirad184" manufactured by IGM Resins B.V.): 4.5 parts by mass Methyl isobutyl ketone (MIBK): 200 parts by mass

[0147] <Hard Coat Layer Composition 2> Urethane acrylate ("EBECRYL8254" manufactured by Daicel-Allnex Corporation): 60 parts by mass Silica particles (solid content 20% by mass, solvent MIBK (methyl isobutyl ketone), average primary particle diameter 45 nm): 35 parts by mass (value calculated based on 100% by mass of solid content) Leveling agent ("F477" manufactured by DIC Corporation): 0.5 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, "Omnirad184" manufactured by IGM Resins B.V.): 4.5 parts by mass Methyl isobutyl ketone (MIBK): 200 parts by mass

[0148] <Hard Coat Layer Composition 3> Urethane acrylate ("EBECRYL8254" manufactured by Daicel Allnex Corporation): 60 parts by mass Silica particles (solid content 20% by mass, solvent MIBK (methyl isobutyl ketone), average primary particle diameter 45 nm): 35 parts by mass (value calculated based on 100% by mass of solid content) Leveling agent ("F477" manufactured by DIC Corporation): 0.02 parts by mass Polymerization initiator (1-hydroxycyclohexyl phenyl ketone, "Omnirad184" manufactured by IGM Resins B.V.): 4.5 parts by mass Methyl isobutyl ketone (MIBK): 200 parts by mass

[0149] The "value converted to 100% by mass of solid content" is a value when the mass of solid content in the solvent-diluted product is taken as 100%.

[0150] (2) Resin substrates Resin substrate 1: 80 μm thick polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) Resin substrate 2: 50 μm thick polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) Resin substrate 3: 30 μm thick polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) Resin substrate 4: 100 μm thick polyethylene terephthalate (PET) film ("Cosmoshine A4360" manufactured by Toyobo Co., Ltd.) Resin substrate 5: 40 μm thick cellulose triacetate (TAC) film ("Konica Minolta TAC KC4UA" manufactured by Konica Minolta, Inc.) Resin substrate 6: 38 μm thick polyethylene terephthalate (PET) film ("Cosmoshine A4360" manufactured by Toyobo Co., Ltd.) Resin substrate 7: 23 μm thick polyethylene terephthalate (PET) film ("Lumirror 23U403" manufactured by Toray Industries, Inc.) Resin substrate 8: 50 μm thick polyethylene terephthalate (PET) film ("Cosmoshine A4360" manufactured by Toyobo Co., Ltd.)

[0151] (3) Bonding layer Adhesive film 1: "8146-1" manufactured by 3M, bonding layer thickness 25 μm, OCA tape with double-sided separate film Adhesive film 2: "NCF-D692" manufactured by Lintec Corporation, bonding layer thickness 15 μm, OCA tape with double-sided separate film Adhesive film 3 (bonding layer thickness 30 μm, two bonding layers of the above adhesive film 2 bonded together)

[0152]

[0153] [Example 1] (1) Preparation of First Laminated Film An 80 μm thick polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) was used as the first resin substrate. The hard coat layer composition 1 was applied to one side of the first resin substrate using a bar coater to form a coating film. The coating film was then heated at 70° C. for 2 minutes to evaporate the solvent in the coating film. Next, using an ultraviolet irradiation device (Fusion UV Systems Japan, light source H bulb), ultraviolet light was irradiated at an integrated light intensity of 300 mJ / cm under conditions of an oxygen concentration of 200 ppm or less. 2 The coating film was completely cured by irradiation, thereby forming a hard coat layer having a thickness of 19 μm as the first functional layer.

[0154] (2) Preparation of second laminate film A second laminate film was prepared in the same manner as the first laminate film, except that a 40 μm thick cellulose triacetate (TAC) film (Konica Minolta TAC KC4UA manufactured by Konica Minolta) was used as the second resin substrate, and the thickness of the hard coat layer, which was the second functional layer, was 12 μm.

[0155] (3) Preparation of Laminate for Display Device The laminate for display device was prepared according to the test application described below. First, a first laminate film and a second laminate film of a size according to the test application were prepared. Next, one of the separate films of the adhesive film 1 was peeled off, and the surface of the bonding layer was attached to the surface of the first resin substrate side of the first laminate film, taking care not to curl. Thereafter, the other separate film of the adhesive film 1 was peeled off, and the surface of the bonding layer was attached to the surface of the second functional layer side of the second laminate film, taking care not to curl. This resulted in a laminate for display device.

[0156] [Example 2] A laminate for a display device was manufactured in the same manner as in Example 1, except that in preparing the second laminate film, a 38 μm thick polyethylene terephthalate (PET) film (Cosmoshine A4360 manufactured by Toyobo Co., Ltd.) was used as the second resin substrate, and the thickness of the second functional layer was 9 μm.

[0157] Example 3 A laminate for a display device was produced in the same manner as in Example 2, except that the adhesive film 2 was used in the production of the laminate for a display device.

[0158] Example 4 A laminate for a display device was produced in the same manner as in Example 2, except that the above-mentioned composition 2 for hard coat layer was used in forming the second functional layer in the second laminate film.

[0159] Example 5 A laminate for a display device was produced in the same manner as in Example 1, except that the thickness of the first functional layer in the first laminate film was set to 15 μm.

[0160] Example 6 A laminate for a display device was produced in the same manner as in Example 5, except that the above-mentioned composition 2 for hard coat layer was used in forming the second functional layer in the second laminate film.

[0161] [Example 7] A laminate for a display device was manufactured in the same manner as in Example 2, except that the thickness of the first functional layer in the first laminate film was 9 μm and the adhesive film 2 was used in the production of the laminate for a display device.

[0162] [Example 8] A laminate for a display device was manufactured in the same manner as in Example 2, except that a 50 μm thick polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) was used as the first resin substrate in the first laminate film, the thickness of the first functional layer was set to 9 μm, and a 23 μm thick polyethylene terephthalate (PET) film ("Lumirror 23U403" manufactured by Toray Industries, Inc.) was used as the second resin substrate in the second laminate film.

[0163] [Example 9] A laminate for a display device was manufactured in the same manner as in Example 1, except that a 50 μm thick polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) was used as the first resin substrate in the first laminate film and the thickness of the first functional layer was 9 μm.

[0164] Example 10 A laminate for a display device was produced in the same manner as in Example 5, except that the adhesive film 3 was used in the production of the laminate for a display device.

[0165] Example 11 A laminate for a display device was produced in the same manner as in Example 8, except that the adhesive film 3 was used in the production of the laminate for a display device.

[0166] Comparative Example 1 A laminate for a display device was produced in the same manner as in Example 2, except that a 50 μm thick polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) was used as the second resin substrate in the second laminate film.

[0167] [Comparative Example 2] A laminate for a display device was produced in the same manner as in Comparative Example 1, except that a polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) having a thickness of 80 μm was used as the second resin substrate in the second laminate film.

[0168] Comparative Example 3 A laminate for a display device was produced in the same manner as in Comparative Example 2, except that the above-mentioned composition 2 for hard coat layer was used in forming the second functional layer in the second laminate film.

[0169] Comparative Example 4 A laminate for a display device was produced in the same manner as in Comparative Example 1, except that the above-mentioned composition 2 for hard coat layer was used in forming the second functional layer in the second laminate film.

[0170] [Comparative Example 5] A laminate for a display device was manufactured in the same manner as in Example 1, except that a 50 μm thick polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) was used as the first resin substrate in the first laminate film, the thickness of the first functional layer was 9 μm, a 50 μm thick polyethylene terephthalate (PET) film ("Cosmoshine A4360" manufactured by Toyobo Co., Ltd.) was used as the second resin substrate in the second laminate film, and the above-mentioned hard coat layer composition 2 was used in forming the second functional layer.

[0171] [Comparative Example 6] A laminate for a display device was manufactured in the same manner as in Comparative Example 4, except that a 50 μm thick polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) was used as the first resin substrate in the first laminate film and the thickness of the first functional layer was 9 μm.

[0172] [Comparative Example 7] A laminate for a display device was produced in the same manner as in Example 3, except that a 30 μm thick polyamideimide film ("CPI" manufactured by Kolon Co., Ltd.) was used as the first resin substrate in the first laminate film, and the above-mentioned hard coat layer composition 2 was used to form the second functional layer in the second laminate film.

[0173] [Comparative Example 8] A laminate for a display device was manufactured in the same manner as in Example 3, except that a 100 μm thick polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., "Cosmoshine A4360") was used as the first resin substrate in the first laminate film, and the above-mentioned hard coat layer composition 2 was used to form the second functional layer in the second laminate film.

[0174] Comparative Example 9 A laminate for a display device was produced in the same manner as in Example 1, except that the following hard coat layer composition 3 was used in forming the second functional layer in the second laminate film.

[0175] [Evaluation] (1) A1 value The tensile modulus of the first laminate film was measured using a Tensilon universal testing machine ("RTC-1310A" manufactured by A&D Co., Ltd.) by the method described above in "A. Laminate for display device 1. First laminate film (1) Properties of the first laminate film." The A1 value was calculated from the tensile modulus and thickness of the first laminate film using the above formula (1).

[0176] (2) A2 Value The tensile modulus of the second laminate film was measured using a Tensilon universal testing machine ("RTC-1310A" manufactured by A&D Co., Ltd.) by the method described above in "A. Laminate for display device 2. First laminate film (1) Properties of second laminate film." The A2 value was calculated from the tensile modulus and thickness of the second laminate film using the above formula (2).

[0177] (3) Water contact angle on the surface of the second functional layer side of the second laminate film Using a contact angle meter "DropMaster 300" manufactured by Kyowa Interface Science Co., Ltd., the water contact angle on the surface of the second functional layer side of the second laminate film was measured using the method described above in "A. Laminate for display device 2. First laminate film (1) Characteristics of the second laminate film."

[0178] (4) Adhesion strength of bonding layer to second laminate film A test piece having a width of 25 mm and a length of 200 mm was cut out from the laminate for a display device using a punching machine so that no lifting or burrs occurred at the edges, and the adhesion strength of the bonding layer to the second laminate film was measured using a Tensilon universal testing machine ("RTC-1310A" manufactured by A&D Co., Ltd.) according to the method described above in "A. Laminate for a display device 2. First laminate film (1) Properties of the second laminate film".

[0179] (5) Bending Resistance The laminate for a display device was subjected to the dynamic bending test described above in "A. Laminate for a display device 4. Properties of the laminate for a display device." In this test, the laminate for a display device was folded so that the first laminate film was on the inside. The evaluation criteria are as follows: A1: When a test in which the laminate for a display device was folded 180° so that the distance d between the opposing short sides of the laminate for a display device was 8 mm was repeated 200,000 times, no cracking, breakage, or peeling occurred. A2: When a test in which the laminate for a display device was folded 180° so that the distance d between the opposing short sides of the laminate for a display device was 10 mm was repeated 200,000 times, no cracking, breakage, or peeling occurred. B: When a test in which the laminate for a display device was folded 180° so that the distance d between the opposing short sides of the laminate for a display device was 10 mm was repeated 200,000 times, cracking, breakage, or peeling occurred.

[0180] (6) Peelability (adhesive residue) A test piece 25 mm wide and 200 mm long was cut out from the laminate for a display device, and the area of ​​the adhesive residue was determined by the method described above in "A. Laminate for a display device 4. Properties of the laminate for a display device." A Tensilon universal testing machine ("RTC-1310A" manufactured by A&D Co., Ltd.) was used as the tensile tester. Black tape manufactured by Yamato Co., Ltd. was used as the black tape.

[0181] (7) Pencil Hardness The pencil hardness of the surface of the first functional layer side of the laminate for a display device was measured using a pencil scratch coating hardness tester manufactured by Toyo Seiki Co., Ltd., according to the method described above in "A. Laminate for a display device 4. Properties of the laminate for a display device." The table below shows the highest pencil hardness that did not cause dents or scratches.

[0182]

[0183] As shown in Table 1, in Examples 1 to 11, the A1 values ​​were within a predetermined range, the A2 values ​​were equal to or less than a predetermined value, the first resin substrate contained a polyimide resin, and the thickness of the first functional layer was equal to or greater than a predetermined value. Therefore, it was confirmed that the films had excellent flex resistance and hardness and were replaceable. On the other hand, in Comparative Examples 1 to 4, the A2 values ​​were large, resulting in poor flex resistance. In Comparative Examples 5 and 6, the A2 values ​​were large, resulting in deformation of the bonding layer located between the first laminate film and the second laminate film during the pencil hardness test, making it difficult for the indentation to recover after the pencil hardness test, and reducing the pencil hardness. In Comparative Example 7, the A1 value was small, resulting in reduced surface hardness. In Comparative Example 8, the PET film used as the first resin substrate was prone to plastic deformation during the pencil hardness test, making it difficult for the indentation to recover after the pencil hardness test, resulting in a significant reduction in pencil hardness. In Comparative Example 9, the water contact angle on the surface of the second functional layer side of the second laminate film was small, resulting in high adhesive strength of the bonding layer to the second laminate film, resulting in adhesive residue.

[0184] As described above, in Examples 1 to 11, the A2 value is equal to or less than a predetermined value, that is, the A2 value is 0.07 × 10 -3 P.A.M. 3 That is, for example, as in Example 1, the A2 value is 0.072 × 10 -3 P.A.M. 3 In the case of , 0.07 × 10 -3 P.A.M. 3 In this specification, the A2 value is expressed as a × 10 -3 When the value of a is rounded to two decimal places, it becomes 0.07 x 10 -3 P.A.M. 3 If it becomes 0.07 x 10 -3 P.A.M. 3 It is understood to be included below.

[0185] The present disclosure provides the following inventions: [1] A laminate film comprising: a first laminate film having a first resin substrate and a first functional layer; a bonding layer disposed on a surface of the first laminate film facing the first resin substrate; and a second laminate film disposed on a surface of the bonding layer opposite the first laminate film, the second laminate film having, in this order from the bonding layer side, a second functional layer and a second resin substrate, wherein the first laminate film and the bonding layer are peelable from the second laminate film; the first functional layer has a thickness of 8 μm or more; and an A1 value calculated by the following formula (1) is 0.10×10 -3 P.A.M. 3 That's it, 0.52 x 10 -3 P.A.M. 3 The A2 value calculated by the following formula (2) is 0.07 × 10 or less. -3 P.A.M. 3 A laminate for a display device, wherein A1=E1×h1. 3 / 12 (1) A2=E2×h2 3 / 12 (2) (In the above formula (1), E1 represents the tensile modulus of elasticity (Pa) of the first laminate film, and h1 represents the thickness (m) of the first laminate film. In the above formula (2), E2 represents the tensile modulus of elasticity (Pa) of the second laminate film, and h2 represents the thickness (m) of the second laminate film.) [2] The laminate for a display device according to [1], wherein the first resin substrate contains a polyimide resin. [3] The laminate for a display device according to [1] or [2], wherein the first functional layer has a thickness of 11 μm or more. [4] The laminate for a display device according to any one of [1] to [3], wherein the second laminate film has a thickness of 50 μm or less. [5] The laminate for a display device according to any one of [1] to [4], wherein the bonding layer has a thickness of 50 μm or less. [6] The laminate for a display device according to any one of [1] to [5], wherein the adhesive strength of the bonding layer to the second laminate film is 230 mN / 25 mm or more and 10,000 mN / 25 mm or less. [7] The laminate for a display device according to any one of [1] to [6], wherein the surface of the second laminate film on the second functional layer side has a water contact angle of 90° or more and 113° or less. [8] The laminate for a display device according to any one of [1] to [7], wherein the second resin substrate contains polyethylene terephthalate, triacetyl cellulose, or an acrylic resin. [9] The laminate for a display device according to any one of [1] to [8], which is used for a foldable display, a slidable display, or a rollable display.

[10] A display device comprising: a display panel; and the laminate for a display device according to any one of [1] to [8], arranged on the viewer side of the display panel, the laminate for a display device being arranged so that the surface on the second laminate film side faces the display panel.

[11] The display device according to

[10] , which is a foldable display, a slidable display, or a rollable display.

[0186] REFERENCE SIGNS LIST 1 laminate for display device 2 bonding layer 10 first laminate film 11 first resin substrate 12 first functional layer 20 second laminate film 21 second resin substrate 22 second functional layer 30 display device 31 display panel 32 adhesive layer

Claims

1. A laminated film having a first resin substrate and a first functional layer; a bonding layer disposed on a surface of the first laminated film facing the first resin substrate; and a second laminated film disposed on a surface of the bonding layer opposite the first laminated film, the second laminated film having, in this order from the bonding layer side, a second functional layer and a second resin substrate, the first laminated film and the bonding layer are peelable from the second laminated film; the first functional layer has a thickness of 8 μm or more; and the A1 value calculated by the following formula (1) is 0.10 × 10 -3 P.A.M. 3 More than that, 0.52 x 10 -3 P.A.M. 3 The A2 value calculated by the following formula (2) is 0.07 × 10 or less. -3 P.A.M. 3 A laminate for a display device, which is: A1=E1×h1 3 / 12 (1) A2=E2×h2 3 / 12 (2) (In the above formula (1), E1 represents the tensile modulus of elasticity (Pa) of the first laminate film, and h1 represents the thickness (m) of the first laminate film. In the above formula (2), E2 represents the tensile modulus of elasticity (Pa) of the second laminate film, and h2 represents the thickness (m) of the second laminate film.) 2. The display laminate according to claim 1, wherein the first resin base material contains a polyimide resin.

3. A laminate for a display device according to claim 1 or 2, wherein the thickness of the first functional layer is 11 μm or more.

4. A laminate for a display device according to claim 1 or 2, wherein the thickness of the second laminate film is 50 μm or less.

5. The laminate for a display device according to claim 1 or 2, wherein the thickness of the bonding layer is 50 μm or less.

6. A laminate for a display device according to claim 1 or 2, wherein the adhesive strength of the bonding layer to the second laminate film is 230 mN / 25 mm or more and 10,000 mN / 25 mm or less.

7. A laminate for a display device according to claim 1 or 2, wherein the water contact angle of the surface of the second laminate film on the side of the second functional layer is 90° or more and 113° or less.

8. A laminate for a display device according to claim 1 or 2, wherein the second resin substrate contains polyethylene terephthalate, triacetyl cellulose or an acrylic resin.

9. The laminate for a display device according to claim 1 or 2, which is used for a foldable display, a slidable display or a rollable display.

10. A display device comprising: a display panel; and a laminate for a display device according to claim 1 or claim 2, arranged on the viewer's side of the display panel, the laminate for a display device being arranged so that the surface of the laminate for a display device on the second laminate film side faces the display panel.

11. The display device according to claim 10, which is a foldable display, a slidable display or a rollable display.

Citation Information

Patent Citations

  • Hard coat film, polarizing plate and liquid crystal display apparatus

    JP2007140229A

  • Laminated sheet and manufacturing method therefor

    JP2021149087A

  • Interchangeable cover lenses for flexible displays

    JP2021523413A

  • Polarization plate with retardation layer and picture display unit including polarization plate with retardation layer

    JP2024089227A

  • Protective cover and display device including the same

    US20180136371A1