Aluminum electrolytic capacitor for liquid immersion cooling, method for cooling aluminum electrolytic capacitor, and method for cooling electronic apparatus
The use of a resin member with a specific solubility parameter distance from the coolant in aluminum electrolytic capacitors addresses the issue of coolant infiltration, ensuring stable performance in liquid immersion cooling systems.
Patent Information
- Application Number
- PCT/JP2024/016450
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Aluminum electrolytic capacitors are difficult to apply to liquid immersion cooling systems using hydrocarbon or silicone oil refrigerants due to coolant infiltration, which causes performance deterioration.
Incorporating a resin member with a Hansen solubility parameter distance of 4.5 or more from the cooling liquid, made from materials like epoxy resin, phenol resin, or (meth)acrylic resin, to prevent coolant infiltration and maintain airtightness.
The resin member effectively suppresses coolant infiltration, maintaining the aluminum electrolytic capacitor's performance and preventing capacitance decrease and equivalent series resistance increase during liquid immersion cooling.
Smart Images

Figure JP2024016450_31102024_PF_FP_ABST
Abstract
Description
Immersion-cooled aluminum electrolytic capacitor, cooling method for aluminum electrolytic capacitor, and cooling method for electronic device
[0001] The present disclosure relates to an immersion-cooled aluminum electrolytic capacitor, a cooling method for an aluminum electrolytic capacitor, and a cooling method for an electronic device.
[0002] There are two types of cooling technologies for electronic devices, such as supercomputers and server equipment, that generate heat during operation: air-cooled systems, which use air to cool the electronic devices, and liquid immersion cooling systems, which immerse the electronic devices in a cooling liquid. Liquid immersion cooling systems use a liquid as a refrigerant, which has higher thermal conductivity than air, so they generally have higher cooling efficiency than air-cooled systems and have been attracting attention in recent years as a technology that contributes to reducing power consumption.
[0003] Known coolants used in immersion cooling systems include fluorine-based insulating refrigerants such as 1,1,1,3,3,3-hexafluoroisopropyl methyl ether and 1,1,2,3,3,3-hexafluoropropyl methyl ether (Patent Document 1). Immersion cooling systems using fluorine-based insulating refrigerants have the advantage of being easy to maintain, including the inspection and repair of electronic devices. Therefore, fluorine-based insulating refrigerants are the most widely used refrigerants for immersion cooling systems today.
[0004] Japanese Patent Application Laid-Open No. 2022-169554
[0005] Although fluorine-based insulating refrigerants are highly convenient as described above, they are expensive and may cause environmental pollution. Therefore, replacement with cheaper cooling liquids other than fluorine-based insulating refrigerants is being considered. Examples of cooling liquids that can replace fluorine-based insulating refrigerants include hydrocarbon-based refrigerants and silicone oil-based refrigerants.
[0006] Here, inexpensive aluminum electrolytic capacitors with large capacitance are widely used in electronic devices. A commonly used aluminum electrolytic capacitor has an aluminum electrolytic capacitor element housed in an outer case, the opening of which is sealed with a sealant. The sealant used in aluminum electrolytic capacitors is often made of rubber, such as ethylene propylene rubber or butyl rubber, or has a rubber member made of rubber, such as ethylene propylene rubber or butyl rubber. However, because rubber is susceptible to organic refrigerants, when an aluminum electrolytic capacitor having such a sealant is subjected to immersion cooling, the coolant may penetrate into the aluminum electrolytic capacitor, causing contact between the aluminum electrolytic capacitor element and the coolant, resulting in performance degradation and other problems. For this reason, aluminum electrolytic capacitors are considered difficult to apply to immersion cooling systems, and no aluminum electrolytic capacitors capable of withstanding immersion cooling using coolants such as hydrocarbon-based refrigerants or silicone oil-based refrigerants have been known to date.
[0007] An object of the present disclosure is to provide an aluminum electrolytic capacitor that can be used in a liquid immersion cooling system that uses a hydrocarbon-based refrigerant and / or a silicone oil-based refrigerant as the coolant.
[0008] As a result of extensive research aimed at solving the above problems, the present inventors have found that by providing a resin member that prevents coolant from seeping into the aluminum electrolytic capacitor, it is possible to provide an aluminum electrolytic capacitor that is highly stable against coolant selected from hydrocarbon-based refrigerants and silicone oil-based refrigerants.
[0009] [1] An aluminum electrolytic capacitor for liquid immersion cooling that is used for cooling in a coolant, comprising an aluminum electrolytic capacitor element and a resin member that prevents the coolant from penetrating into the aluminum electrolytic capacitor, wherein the coolant is one or more refrigerants selected from the group consisting of hydrocarbon-based refrigerants and silicone oil-based refrigerants. [2] The aluminum electrolytic capacitor for liquid immersion cooling according to [1], wherein the resin member is made of a resin material that has a Hansen solubility parameter distance with the coolant of 4.5 or greater. [3] The aluminum electrolytic capacitor for liquid immersion cooling according to [1] or [2], wherein the resin member is made of a resin material containing one or more resins selected from the group consisting of epoxy resin, phenol resin, (meth)acrylic resin, polyamide resin, polycarbonate resin, and polystyrene resin. [4] The aluminum electrolytic capacitor for liquid immersion cooling according to any one of [1] to [3], wherein the resin member comprises a cured product of an epoxy resin composition containing the epoxy resin and one or more curing agents selected from the group consisting of a phenol-based curing agent, an amine-based curing agent, and an acid anhydride-based curing agent. [5] The aluminum electrolytic capacitor for liquid immersion cooling according to any one of [1] to [4], wherein the coolant is one or more selected from the group consisting of a mixture of hydrocarbons having from 15 to 50 carbon atoms and poly-α-olefins. [6] The aluminum electrolytic capacitor for liquid immersion cooling according to any one of [1] to [5], wherein the aluminum electrolytic capacitor element contains one or more electrolytes selected from the group consisting of liquid electrolytes and solid electrolytes. [7] The aluminum electrolytic capacitor for liquid immersion cooling according to any one of [1] to [6], comprising a bottomed cylindrical metal case that houses the aluminum electrolytic capacitor element and a sealing body that seals the opening of the metal case, and the resin member is a member that covers a region of the surface of the sealing body that is surrounded by the opening. [8] A cooling method for an aluminum electrolytic capacitor, comprising an immersion cooling step of immersing the aluminum electrolytic capacitor in a cooling liquid to cool it, wherein the aluminum electrolytic capacitor has an aluminum electrolytic capacitor element and a resin member that suppresses penetration of the cooling liquid into the aluminum electrolytic capacitor, and the cooling liquid is one or more refrigerants selected from the group consisting of hydrocarbon-based refrigerants and silicone oil-based refrigerants.[9] The cooling method for an aluminum electrolytic capacitor according to [8], wherein the aluminum electrolytic capacitor is mounted on an electronic device, and the immersion cooling step is performed by immersing a part or all of the electronic device in the coolant.
[10] A cooling method for an electronic device having an aluminum electrolytic capacitor, comprising: an immersion cooling step of immersing a part or all of the electronic device in a coolant to cool it, the immersion cooling step being performed so that at least the aluminum electrolytic capacitor is immersed in the coolant, the aluminum electrolytic capacitor has an aluminum electrolytic capacitor element and a resin member that prevents the coolant from penetrating into the aluminum electrolytic capacitor, and the coolant is one or more refrigerants selected from the group consisting of hydrocarbon-based refrigerants and silicone oil-based refrigerants.
[0010] According to the present disclosure, an aluminum electrolytic capacitor that can be applied to a liquid immersion cooling system that uses a hydrocarbon-based refrigerant and / or a silicone oil-based refrigerant as the coolant can be provided.
[0011] Fig. 1 is a schematic cross-sectional view of an immersion cooling aluminum electrolytic capacitor according to an embodiment of the present disclosure. Fig. 2 is a schematic cross-sectional view of an immersion cooling aluminum electrolytic capacitor according to an embodiment of the present disclosure. Fig. 3 is a schematic cross-sectional view of an immersion cooling aluminum electrolytic capacitor according to an embodiment of the present disclosure. Fig. 4 is a schematic cross-sectional view of an immersion cooling aluminum electrolytic capacitor according to an embodiment of the present disclosure. Fig. 5 is a graph showing the relationship between the HSP distance between the constituent materials of the test pieces obtained in the examples and a hydrocarbon-based refrigerant, and the swelling ratio in a swelling test.
[0012] The following describes in detail embodiments of the present disclosure. The following description of the components is an example (typical example) of an embodiment of the present disclosure, and the present disclosure is not limited to these contents as long as it does not exceed the gist of the present disclosure.
[0013] 1. Aluminum Electrolytic Capacitor for Immersion Cooling A first embodiment of the present disclosure is an aluminum electrolytic capacitor for immersion cooling (hereinafter, sometimes simply referred to as an "aluminum electrolytic capacitor") that is cooled in a coolant, and includes an aluminum electrolytic capacitor element and a resin member that prevents the coolant from penetrating into the aluminum electrolytic capacitor. When the aluminum electrolytic capacitor according to this embodiment is immersion cooled, one or more refrigerants selected from the group consisting of hydrocarbon-based refrigerants and silicone oil-based refrigerants are used as the coolant.
[0014] 1-1. Aluminum Electrolytic Capacitor Element In this embodiment, a known aluminum electrolytic capacitor element or one similar to a known aluminum electrolytic capacitor element can be used as the aluminum electrolytic capacitor element (hereinafter sometimes simply referred to as "capacitor element"). For example, the aluminum electrolytic capacitor element may be a laminated type or a wound type, but a wound type is preferred.
[0015] When the aluminum electrolytic capacitor element is of a wound type, the aluminum electrolytic capacitor may be of any of a chip type, a lead type, a substrate-supporting type, and a screw terminal type, but is preferably of any of a lead type, a substrate-supporting type, and a screw terminal type.
[0016] In this embodiment, the aluminum electrolytic capacitor element preferably contains one or more electrolytes selected from the group consisting of liquid electrolytes (i.e., electrolytic solutions) and solid electrolytes. Examples of solid electrolytes include conductive polymers and ion-conductive solids. Examples of such aluminum electrolytic capacitor elements include liquid electrolyte-type aluminum electrolytic capacitor elements in which an anode foil and a cathode foil are stacked or wound with a separator impregnated with an electrolytic solution interposed therebetween; conductive polymer-type aluminum solid electrolytic capacitor elements in which an anode foil and a cathode foil are stacked or wound with a separator impregnated with a conductive polymer interposed therebetween; and conductive polymer hybrid-type aluminum electrolytic capacitor elements in which an anode foil and a cathode foil are stacked or wound with a separator impregnated with an electrolytic solution and a conductive polymer interposed therebetween.
[0017] 1-2. Resin Member Conventionally, commonly used aluminum electrolytic capacitors have a metal case housing a capacitor element, the opening of which is sealed with a rubber seal. However, when such an aluminum electrolytic capacitor is subjected to immersion cooling, the seal may swell and / or deteriorate due to the coolant, resulting in the coolant penetrating into the aluminum electrolytic capacitor. Contact between the coolant that has penetrated into the aluminum electrolytic capacitor and the aluminum electrolytic capacitor element can cause problems such as a decrease in capacitance (Cap) and an increase in equivalent series resistance (ESR). In contrast, in this embodiment, the resin member serves as a sealing member that enhances the airtightness of the aluminum electrolytic capacitor, suppressing, and preferably preventing, the ingress of coolant into the aluminum electrolytic capacitor. Furthermore, by enhancing the airtightness of the aluminum electrolytic capacitor, the resin member can also suppress the ingress of oxygen into the aluminum electrolytic capacitor and the leakage of electrolyte out of the aluminum electrolytic capacitor. Therefore, the aluminum electrolytic capacitor according to this embodiment, which includes a resin member, exhibits minimal degradation of characteristics such as capacitance and equivalent series resistance during immersion cooling, allowing it to maintain good performance over a long period of time.
[0018] As mentioned above, a rubber sealant cannot sufficiently prevent the coolant from entering the aluminum electrolytic capacitor, and therefore, in this disclosure, a rubber sealant does not fall under the category of a "resin member."
[0019] The shape, arrangement, and other aspects of the resin member for suppressing the infiltration of coolant into the aluminum electrolytic capacitor are not particularly limited, but a preferred embodiment is one in which the aluminum electrolytic capacitor has a cylindrical metal case with a bottom that houses an aluminum electrolytic capacitor element and a sealing body that seals the opening of the metal case, with the resin member covering the area of the surface of the sealing body that is surrounded by the opening of the metal case; or one in which the aluminum electrolytic capacitor does not have a sealing body and the resin member directly covers the entire aluminum electrolytic capacitor element. Several examples are given below to explain these specific embodiments, but the resin member in this embodiment is not limited to the following examples. Furthermore, the sealing body, terminals, and other components in the following examples are not limited to the illustrative embodiments.
[0020] 1 to 5 are schematic cross-sectional views of an aluminum electrolytic capacitor 10 according to this embodiment. The aluminum electrolytic capacitor 10 shown in Figures 1 to 4 includes a capacitor element 2, a metal case 4 that houses the capacitor element 2, a sealing body 6 that seals the opening of the metal case 4, and a resin member 8 that covers the area of the surface of the sealing body 6 that is surrounded by the opening of the metal case 4. The metal case 4 has horizontal crimped portions 4a and vertical crimped portions 4b, which secure the sealing body 6 in place and also improve airtightness.
[0021] In aluminum electrolytic capacitor 10 shown in FIG. 1, resin member 8 is a resin layer disposed on the surface of sealing body 6 to prevent sealing body 6 from being exposed to the outside, and has through holes for leading out terminals 9.
[0022] 1(a), the sealing body 6 is a sealing rubber disposed between the vertical crimped portion 4b and the capacitor element 2, and in FIG. 1(b), the sealing body 6 is a rubber-clad laminate disposed between the vertical crimped portion 4b and the horizontal crimped portion 4a, and has a rubber layer and a substrate. The rubber forming the sealing rubber and the rubber layer of the rubber-clad laminate is not particularly limited, and rubbers commonly used for sealing rubbers, such as ethylene propylene rubber and butyl rubber, can be used.
[0023] The portions of this aluminum electrolytic capacitor 10 other than the resin member 8 are manufactured by sequentially inserting the capacitor element 2 and the sealing body 6 into a cylindrical metal case 4 having an opening and a bottom, crimping the metal case 4 laterally from the side (drawing), and then crimping the opening edge of the metal case 4 vertically (curling). More specific manufacturing methods include those disclosed in Japanese Patent Application Laid-Open Nos. 2004-119907 and 2002-25870. The resin member 8 can be formed by a resin molding method such as compression molding or potting, or a coating method.
[0024] Although FIG. 1 shows aluminum electrolytic capacitor 10 in which resin member 8 is disposed only on the surface of sealing body 6, from the viewpoint of improving the airtightness of aluminum electrolytic capacitor 10, it is also preferable that resin member 8 be disposed so as to cover not only the surface of sealing body 6 but also a part of metal case 4 (for example, vertical crimping portion 4 b, or vertical crimping portion 4 b and the side surface of metal case 4) or the entire metal case 4.
[0025] The aluminum electrolytic capacitor 10 shown in FIG. 2 is similar to the aluminum electrolytic capacitor 10 shown in FIG. 1 except for the configuration of the resin member 8. The aluminum electrolytic capacitor 10 shown in FIG. 2 has a resin member 8 disposed in a space defined by a sealing body 6, a vertical crimped portion 4b of a metal case 4, and an imaginary end face facing the bottom surface of the metal case 4. The imaginary end face is an imaginary plane parallel or approximately parallel to the bottom surface of the metal case, and is the end face opposite the bottom surface in the axial direction of the metal case (a direction perpendicular to the bottom surface). The resin member 8 in FIG. 2 also has through holes for drawing out terminals 9. Such a resin member 8 can be formed by a resin molding method such as compression molding or potting.
[0026] The aluminum electrolytic capacitor 10 shown in Fig. 3 is similar to the aluminum electrolytic capacitor 10 shown in Fig. 1 except for the aspect of the resin member 8. The aluminum electrolytic capacitor 10 shown in Fig. 3 has a resin member 8 that surrounds a portion of the side surface of the metal case 4 that continues to the space defined by the sealing body 6, the vertical crimped portion 4b of the metal case 4, and the imaginary end face. The resin member 8 in Fig. 3 also has a through hole for drawing out the terminal 9. Such a resin member 8 can be formed by a resin molding method such as insert molding, transfer molding, injection molding, compression molding, or potting.
[0027] In Figure 3, the proportion of the side surface of the metal case 4 that is covered with the resin member 8 is not particularly limited, and it is sufficient that the distance h' from the axial end of the metal case 4 to the end of the resin member 8 on the side surface of the metal case 4 relative to the axial height h of the metal case 4 is set to preferably more than 0% and not more than 80%, more preferably 5% to 50%, and even more preferably 10% to 40%.
[0028] The aluminum electrolytic capacitor 10 shown in Fig. 4 is similar to the aluminum electrolytic capacitor 10 shown in Fig. 1 except for the form of the resin member 8. The aluminum electrolytic capacitor 10 shown in Fig. 4 includes a resin member 8 that completely covers the metal case 4 and the sealing body 6 and has through holes for leading out the terminals 9. Such a resin member 8 can be formed by a resin molding method such as insert molding, transfer molding, injection molding, compression molding, or potting.
[0029] 2 to 4, the sealing body 6 is shown as a sealing rubber disposed between the vertical crimping portion 4b and the capacitor element 2, but the sealing body 6 may also be a rubber-clad laminate disposed between the vertical crimping portion 4b and the horizontal crimping portion 4a, as shown in FIG. 1(b).
[0030] The aluminum electrolytic capacitor 10 shown in FIG. 5 includes a resin member 8 that completely covers the aluminum electrolytic capacitor element 2 and has through holes for extending the terminals 9. The aluminum electrolytic capacitor element 2 in this aluminum electrolytic capacitor 10 is not housed in a metal case, and therefore does not include a sealing member such as a rubber seal or a rubber-clad laminate. Even in this embodiment where the aluminum electrolytic capacitor does not include a sealing member, the resin member can suppress performance degradation of the aluminum electrolytic capacitor due to infiltration of coolant into the aluminum electrolytic capacitor. The aluminum electrolytic capacitor element 2 in FIG. 5 may be wound or laminated. The aluminum electrolytic capacitor 10 shown in FIG. 5 can be manufactured by a resin molding method such as insert molding, transfer molding, injection molding, compression molding, or potting.
[0031] 1 to 5 , the aluminum electrolytic capacitor element 2 is sealed with the resin member 8 and the metal case 4, or with the resin member 8 alone, thereby ensuring airtightness and suppressing not only the intrusion of coolant into the aluminum electrolytic capacitor 10 but also the intrusion of oxygen into the aluminum electrolytic capacitor 10 and the leakage of electrolyte out of the aluminum electrolytic capacitor 10. The resin member 8 suppresses, or preferably prevents, contact between the aluminum electrolytic capacitor element 2 and the coolant, isolating the aluminum electrolytic capacitor element 2 from the coolant. This allows the aluminum electrolytic capacitor 10 to maintain its characteristics, such as capacitance and equivalent series resistance, for a long period of time, even when immersion cooling is performed.
[0032] The aluminum electrolytic capacitor according to this embodiment preferably has the configuration illustrated in Figures 1 to 4. That is, the aluminum electrolytic capacitor according to this embodiment preferably has a cylindrical metal case with a bottom that houses an aluminum electrolytic capacitor element, a sealing body that seals the opening of the metal case, and a resin member that covers the area of the sealing body that is surrounded by the opening.
[0033] Specific embodiments of aluminum electrolytic capacitors having a resin member have been described above with reference to FIGS. 1 to 5 , but the resin member is not limited to the embodiments shown in FIGS. 1 to 5 , and may further cover elements other than the aluminum electrolytic capacitor element, other electronic components, other members, etc., or may be integrated with the resin member of another aluminum electrolytic capacitor.
[0034] An example of an aluminum electrolytic capacitor having such a resin member is a modified example of the one shown in Fig. 4, in which a unit formed by sealing the opening of a metal case containing an aluminum electrolytic capacitor element with a sealing member is placed on a substrate such as a printed circuit board, and the entire unit is covered by the substrate. In this case, the resin member is not only placed in the same position as the resin member shown in Fig. 4, but also covers the entire substrate including the unit, thereby integrally covering the unit and the substrate.
[0035] 1-2-2. Constituent Materials of Resin Members 1-2-2-1. Hansen Solubility Parameter of Constituent Materials of Resin Members The present inventors considered that, in order to suppress the occurrence of defects in aluminum electrolytic capacitors due to immersion cooling, it would be desirable to employ a resin member that is less susceptible to swelling by the coolant. Focusing on the Hansen Solubility Parameter (HSP) as an indicator for selecting a constituent material for the resin member, they found that swelling of the resin member can be sufficiently suppressed by forming the resin member from a resin material whose HSP distance to the coolant is equal to or greater than a predetermined value. Therefore, it is preferable that the constituent material of the resin member have an HSP distance to the coolant that is equal to or greater than a predetermined value.
[0036] HSP is a value obtained by quantifying the solubility of a substance A in another substance B using a multidimensional vector. It is estimated that the shorter the HSP distance between two substances, the higher the solubility of substance A in substance B and the higher its compatibility with substance B.
[0037] The HSP is calculated from the chemical structure using HSP analysis software such as HSPiP (Hansen Solubility Parameters in Practice, Ver. 5.4.05). The HSP is expressed by three components: δD (dispersion term), δP (polarization term), and δH (hydrogen bond term). The units of δD, δP, δH, and Ra are MPa. 1/2 The HSP distance between two compounds is the distance between two points when the respective δD, δP, and δH values are plotted on a three-dimensional orthogonal coordinate system, and can be calculated according to the following formula. In the present disclosure, HSP is a value at 25°C. In addition, in this embodiment, the constituent material of the resin member corresponds to substance B, and the coolant corresponds to substance A.
[0038] HSP distance (Ra) = {4×(δD 1 -δD 2 ) 2 + (δP 1 -δP 2 ) 2 + (δH 1 -δH 2 ) 2} 1/2 In the formula, δD 1 , δP 1 and δH1 are δD, δP, and δH of substance A, respectively. 2 , δP 2 and δH 2 are δD, δP, and δH of material B, respectively.
[0039] If the HSP distance between the constituent material of the resin member and the coolant is a predetermined value or more, swelling of the resin member due to contact with the coolant during immersion cooling is less likely to occur, and as a result, it is thought that problems such as a decrease in Cap and an increase in ESR of aluminum electrolytic capacitors due to immersion cooling can be suppressed.
[0040] Specifically, the HSP distance between the constituent material of the resin member and the coolant is preferably 4.5 or more, more preferably 4.7 or more, even more preferably 7.5 or more, even more preferably 7.7 or more, particularly preferably 13.0 or more, and most preferably 13.4 or more, in order to more effectively suppress swelling of the resin member. The upper limit of the HSP distance between the constituent material of the resin member and the coolant is not particularly limited, but is preferably 50.0 or less, 40.0 or less, 30.0 or less, or 20.0 or less. That is, preferred ranges of the HSP distance between the constituent material of the resin member and the coolant include, for example, 4.5 to 50.0, 4.7 to 50.0, 7.5 to 40.0, 7.7 to 40.0, 13.0 to 30.0, and 13.4 to 20.0.
[0041] 1-2-2-2. Constituent Material of Resin Member The constituent material of the resin member is preferably a cured product of a thermosetting resin, a cured product of a thermosetting resin composition containing a thermosetting resin, a thermoplastic resin, or a thermoplastic resin composition containing a thermoplastic resin. The thermosetting resin composition may contain, in addition to the thermosetting resin, a curing agent, a curing accelerator, an inorganic filler, and other additives. The thermoplastic resin composition may also contain, in addition to the thermoplastic resin, an inorganic filler and other additives.
[0042] Preferred examples of thermosetting resins include epoxy resins, phenolic resins, and polyurethane resins. Among these, from the viewpoint of improving resistance to coolants and airtightness, the thermosetting resin is more preferably one or more selected from the group consisting of epoxy resins and phenolic resins, and particularly preferably an epoxy resin. That is, the resin member is preferably made of a cured product of an epoxy resin, a cured product of a phenolic resin, a cured product of an epoxy resin composition, or a cured product of a phenolic resin composition, more preferably a cured product of an epoxy resin composition or a cured product of a phenolic resin composition, and even more preferably a cured product of an epoxy resin composition containing the epoxy resin described below and optional components such as a curing agent, a curing accelerator, an inorganic filler, and other additives in the amounts described below as needed.
[0043] The epoxy resin may be a compound having two or more epoxy groups per molecule, and the molecular structure, molecular weight, and other properties are not particularly limited. Known epoxy resins can be used. Examples of known epoxy resins include bisphenol-type epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AD epoxy resin, and bisphenol S epoxy resin; hydrogenated versions of the above bisphenol-type epoxy resins; novolac-type epoxy resins such as cresol novolac epoxy resin, phenol novolac epoxy resin, and naphthol novolac epoxy resin; biphenyl-type epoxy resins; and alicyclic epoxy resins such as 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate. The epoxy resin may also be a modified epoxy resin such as a urethane-modified epoxy resin or a silicone-modified epoxy resin.
[0044] Of these, the epoxy resin is preferably a bisphenol type epoxy resin, more preferably a bisphenol A type epoxy resin, from the viewpoint of improving moldability, curability, and airtightness of the aluminum electrolytic capacitor.
[0045] In the field of polymers, the term "epoxy resin" is a concept that includes a monomer having two or more epoxy groups in one molecule, an oligomer of the monomer, a polymer of the monomer, and a mixture of two or more of these compounds. In the present disclosure, "epoxy resin" is also defined as above.
[0046] Examples of the phenolic resin include novolac type phenolic resin and resol type phenolic resin, and novolac type phenolic resin is preferred.
[0047] The thermosetting resins may be used alone or in any combination of two or more in any ratio.
[0048] When a resin member is formed by a molding method such as injection molding (including insert molding), compression molding, or potting, the lower limit of the thermosetting resin content in the thermosetting resin composition is not particularly limited, but is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, from the viewpoint of improving the airtightness of the aluminum electrolytic capacitor. The upper limit of the thermosetting resin content in the thermosetting resin composition is not particularly limited, but is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less, from the viewpoint of improving fluidity and moldability. That is, preferred ranges for the thermosetting resin content in the thermosetting resin composition include 20% by mass or more and 90% by mass or less, 30% by mass or more and 80% by mass or less, and 40% by mass or more and 70% by mass or less.
[0049] When a resin member is formed by a molding method such as transfer molding, the lower limit of the content of the thermosetting resin in the thermosetting resin composition is not particularly limited, but from the viewpoint of fluidity and moldability, it is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 5% by mass or more. Furthermore, the upper limit of the content of the thermosetting resin in the thermosetting resin composition is not particularly limited, but from the viewpoint of further improving the reliability of the aluminum electrolytic capacitor, it is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less. That is, preferred ranges for the content of the thermosetting resin in the thermosetting resin composition include 1% by mass or more and 50% by mass or less, 2% by mass or more and 30% by mass or less, and 5% by mass or more and 20% by mass or less.
[0050] The thermosetting resin composition preferably contains a curing agent. Examples of the curing agent for the epoxy resin include, but are not limited to, phenol-based curing agents, amine-based curing agents, acid anhydride-based curing agents, polyisocyanate-based curing agents, and polythiol-based curing agents. Among these, the curing agent for the epoxy resin is preferably one or more selected from the group consisting of phenol-based curing agents, amine-based curing agents, and acid anhydride-based curing agents, from the viewpoint of improving the airtightness of the aluminum electrolytic capacitor.
[0051] Examples of phenolic curing agents include bisphenol A, bisphenol F, bisphenol AD, bisphenol S, tetrabromobisphenol A, 4,4'-biphenol, 3,3',5,5'-tetramethyl-4,4'-biphenol, catechol, resorcinol, hydroquinone, naphthalenediol, and phenol novolac resin.
[0052] Examples of amine curing agents include ethylenediamine, trimethylenediamine, tetramethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, polyethyleneamine, 1,3-bisaminomethylcyclohexane, 4,4'-methylene-bis(cyclohexylamine), m-phenylenediamine, p-phenylenediamine, m-xylylenediamine, p-xylylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, isophoronediamine, and dicyandiamide.
[0053] Examples of acid anhydride curing agents include maleic anhydride, trimellitic anhydride, pyromellitic anhydride, polyazelaic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, 3-methyl-1,2,3,6-tetrahydrophthalic anhydride, tetrabromophthalic anhydride, 4-methyl-1,2,3,6-tetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, phthalic anhydride, hexahydrophthalic anhydride, 3,6-endomethylene-1,2,3,6-tetrahydrophthalic anhydride, dodecenylsuccinic anhydride, and octenylsuccinic anhydride.
[0054] Examples of polyisocyanate curing agents include aliphatic polyisocyanates such as ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, propylene-1,2-diisocyanate, cyclopentene-1,3-diisocyanate, and isophorone diisocyanate; and aromatic isocyanates such as 1,4-phenylene diisocyanate, naphthalene-1,5-diisocyanate, tolylene-2,4-diisocyanate, tolylene-2,6-diisocyanate, 1,3,5-triisocyanatobenzene, m-xylylene diisocyanate, and diphenylmethane diisocyanate.
[0055] Examples of polythiol curing agents include butanediol bis(3-mercaptopropionate), ethylene glycol bis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris-(3-mercaptopropionyloxyethyl)isocyanurate. and ester group-containing polythiols such as ester acetate; and ether group-containing polythiols such as 2,2-bis[(3-mercaptopropoxy)methyl]-1-butanol, 3-(3-mercapto-propoxy)-2,2-bis-(3-mercapto-propoxymethyl)-propan-1-ol, and 3-{3-(3-mercapto-propoxy)-2,2-bis-[(3-mercaptopropoxy)methyl]propoxy}-propan-1-ol.
[0056] The curing agent for the phenolic resin is not particularly limited, but examples thereof include phenolic resins, epoxy resins, isocyanate-based curing agents, amine-based curing agents such as hexamethylenetetramine (hexamine), and organic acid-based curing agents such as benzenesulfonic acid and paratoluenesulfonic acid. The curing agent for the novolac-type phenolic resin is preferably one or more selected from the group consisting of resole-type phenolic resins, epoxy resins, isocyanate-based curing agents, and amine-based curing agents, and more preferably one or more selected from amine-based curing agents. Furthermore, the curing agent for the resole-type phenolic resin is preferably one or more selected from organic acid-based curing agents.
[0057] The curing agent may be used alone or in any combination of two or more in any ratio.
[0058] When the thermosetting resin composition contains a curing agent, the lower limit of the content of the curing agent in the thermosetting resin composition is not particularly limited, but from the viewpoint of sufficiently curing the thermosetting resin, it is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more. Furthermore, the upper limit of the content of the curing agent in the thermosetting resin composition is not particularly limited, but from the viewpoint of ensuring the fluidity and moldability of the thermosetting resin composition, it is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less. That is, when the thermosetting resin composition contains a curing agent, preferred ranges of the content of the curing agent in the thermosetting resin composition include 1% by mass or more and 30% by mass or less, 5% by mass or more and 20% by mass or less, and 10% by mass or more and 15% by mass or less.
[0059] The thermosetting resin composition preferably contains a curing accelerator (excluding those corresponding to the curing agents described above). Examples of the curing accelerator for epoxy resins include, but are not limited to, phosphorus-based compounds, tertiary amine compounds, and imidazole compounds.
[0060] Examples of phosphorus compounds include triphenylphosphine, tris(2,6-dimethoxyphenyl)phosphine, tris(4-methylphenyl)phosphine, and tetraphenylphosphonium tetraphenylborate.
[0061] Examples of tertiary amine compounds include 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), and 1,5-diazabicyclo[4.3.0]non-5-ene (DBN).
[0062] Examples of the imidazole compound include 2-methylimidazole, 2-phenylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, and 2-ethyl-4-methylimidazole.
[0063] Examples of curing accelerators for phenolic resins include, but are not limited to, alkaline earth metal oxides or hydroxides such as magnesium oxide, calcium hydroxide, and barium hydroxide; and aromatic carboxylic acids such as salicylic acid and benzoic acid.
[0064] The curing accelerator may be used alone or in any combination of two or more in any ratio. The thermosetting resin composition may not contain a curing accelerator.
[0065] When the thermosetting resin composition contains a curing accelerator, the lower limit of the content of the curing accelerator in the thermosetting resin composition is not particularly limited, but from the viewpoint of sufficiently curing the thermosetting resin, it is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 1.0 mass% or more. Furthermore, the upper limit of the content of the curing accelerator in the thermosetting resin composition is not particularly limited, but from the viewpoint of ensuring the fluidity and moldability of the thermosetting resin composition, it is preferably 5.0 mass% or less, more preferably 4.0 mass% or less, and even more preferably 3.0 mass% or less. That is, when the thermosetting resin composition contains a curing accelerator, preferred ranges of the content of the curing accelerator in the thermosetting resin composition include 0.1 mass% or more and 5.0 mass% or less, 0.5 mass% or more and 4.0 mass% or less, and 1.0 mass% or more and 3.0 mass% or less.
[0066] Examples of thermoplastic resins include (meth)acrylic resins, polyamide resins, polycarbonate resins, polystyrene resins, and polyolefin resins such as polyethylene resins and polypropylene resins. In the present disclosure, "(meth)acrylic resin" is a general term for acrylic resins and methacrylic resins, and means "acrylic resin and / or methacrylic resin."
[0067] The resin member preferably includes at least one selected from the group consisting of epoxy resin, phenolic resin, (meth)acrylic resin, polyamide resin, polycarbonate resin, and polystyrene resin, among the thermosetting and thermoplastic resins described above. These resin materials have a large HSP distance with the coolant in this embodiment and are less likely to swell with the coolant. Therefore, by including a resin member made of such a resin material in an aluminum electrolytic capacitor, it is possible to suppress the decrease in Capacitance and the increase in ESR caused by immersion cooling.
[0068] The inorganic filler is not particularly limited, but examples thereof include silica, alumina, kaolin, talc, mica, rock wool, wollastonite, glass powder, glass flakes, glass beads, glass fiber, silicon carbide, silicon nitride, aluminum nitride, carbon black, carbon fiber, graphite, titanium dioxide, calcium carbonate, calcium sulfate, barium carbonate, magnesium carbonate, magnesium sulfate, barium sulfate, cellulose, aramid, and wood.
[0069] The inorganic filler may be used alone or in any combination of two or more in any ratio. The thermosetting resin composition and the thermoplastic resin composition may not contain an inorganic filler.
[0070] When the thermosetting resin composition and the thermoplastic resin composition contain an inorganic filler and are used to form a resin part by a molding method such as injection molding (including insert molding), compression molding, or potting, the lower limit of the inorganic filler content in these compositions is not particularly limited, but is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, from the viewpoint of improving strength. Furthermore, the upper limit of the inorganic filler content in the thermosetting resin composition and the thermoplastic resin composition is not particularly limited, but is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, from the viewpoint of improving flowability, moldability, and airtightness of the aluminum electrolytic capacitor. That is, when the thermosetting resin composition and the thermoplastic resin composition contain an inorganic filler, preferred ranges for the inorganic filler content in these compositions include 20% by mass or more and 80% by mass or less, 30% by mass or more and 70% by mass or less, and 40% by mass or more and 60% by mass or less.
[0071] When the thermosetting resin composition and the thermoplastic resin composition contain an inorganic filler and are used to form a resin part by a molding method such as transfer molding, the lower limit of the inorganic filler content in these compositions is not particularly limited, but is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 75% by mass or more, from the viewpoint of further improving the reliability of the aluminum electrolytic capacitor. Furthermore, the upper limit of the inorganic filler content in the thermosetting resin composition and the thermoplastic resin composition is not particularly limited, but is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, from the viewpoint of improving the flowability, moldability, and airtightness of the aluminum electrolytic capacitor. That is, when the thermosetting resin composition and the thermoplastic resin composition contain an inorganic filler, preferred ranges for the inorganic filler content in these compositions include 50% by mass or more and 95% by mass or less, 60% by mass or more and 90% by mass or less, and 75% by mass or more and 85% by mass or less.
[0072] Other additives (excluding those corresponding to the curing agent, the curing accelerator, and the inorganic filler) include coupling agents, antifoaming agents, flame retardants, pigments, solvents, etc. In this embodiment, when an epoxy resin is used as the thermosetting resin, it is also preferable that the thermosetting resin composition contains an epoxy silane coupling agent such as 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0073] These additives may be used alone or in any combination of two or more in any ratio. The thermosetting resin composition and the thermoplastic resin composition may not contain any other additives.
[0074] When the thermosetting resin composition and the thermoplastic resin composition contain other additives, the content of the other additives in these compositions is not particularly limited, but is preferably 0.01% by mass or more and 10% by mass or less, more preferably 0.05% by mass or more and 5% by mass or less, and even more preferably 1% by mass or more and 3% by mass or less.
[0075] The aluminum electrolytic capacitor according to this embodiment is suitable for use in electronic devices that are immersion cooled using the above-described coolant. By providing an aluminum electrolytic capacitor that can be adapted to immersion cooling using the above-described coolant, the degree of freedom in selecting the coolant increases, making it possible to replace the expensive fluorine-based insulating refrigerants that have been used up to now with less expensive coolants such as hydrocarbon-based refrigerants or silicone oil-based refrigerants.
[0076] Examples of hydrocarbon refrigerants include petroleum hydrocarbons such as paraffinic mineral oil and naphthenic mineral oil, synthetic oils such as poly-α-olefins (PAOs) and artificial petroleum obtained by Fischer-Tropsch synthesis, and bio-oil. Of these, the hydrocarbon refrigerant is preferably one or more selected from the group consisting of petroleum hydrocarbons and synthetic oils, more preferably one or more selected from synthetic oils, even more preferably one or more selected from the group consisting of artificial petroleum and poly-α-olefins obtained by Fischer-Tropsch synthesis, and particularly preferably artificial petroleum or poly-α-olefins obtained by Fischer-Tropsch synthesis.
[0077] The artificial petroleum obtained by Fischer-Tropsch synthesis is preferably a mixture of hydrocarbons having from 15 to 50 carbon atoms, and more preferably a mixture of hydrocarbons having from 18 to 50 carbon atoms. Each hydrocarbon may be a linear hydrocarbon, a branched hydrocarbon, or a cyclic hydrocarbon, but is preferably a linear hydrocarbon or a branched hydrocarbon.
[0078] The poly-α-olefin is preferably a homopolymer or copolymer of an α-olefin having from 2 to 32 carbon atoms, more preferably a homopolymer or copolymer of an α-olefin having from 6 to 16 carbon atoms, even more preferably a homopolymer or copolymer of one or more α-olefins selected from the group consisting of α-octene, 1-decene, 1-dodecene, and 1-tetradecene, and particularly preferably a homopolymer of 1-decene. Furthermore, the poly-α-olefin may be a poly-α-olefin in which the terminal double bonds have been hydrogenated.
[0079] The degree of polymerization of the poly-α-olefin is preferably 2 or more, more preferably 3 or more, and even more preferably 4 or more, and is preferably 10 or less, more preferably 8 or less, and even more preferably 5 or less. That is, preferred ranges of the degree of polymerization of the poly-α-olefin include, for example, from 2 to 10, from 3 to 8, and from 4 to 5.
[0080] The number of carbon atoms in the poly-α-olefin is preferably 10 or more, more preferably 20 or more, and even more preferably 30 or more, and is preferably 80 or less, more preferably 70 or less, and even more preferably 60 or less. That is, preferred ranges for the number of carbon atoms in the poly-α-olefin include, for example, 10 or more and 80 or less, 20 or more and 70 or less, and 30 or more and 60 or less.
[0081] From the viewpoint of reducing the environmental load, the hydrocarbon refrigerant is preferably a fluorine-free hydrocarbon, and more preferably a petroleum-based hydrocarbon. In this disclosure, the term "fluorine-free hydrocarbon" refers to a hydrocarbon that does not contain a fluorine atom as a constituent atom, and does not exclude hydrocarbons that unavoidably contain fluorine or a fluorine-containing compound as an impurity.
[0082] Examples of silicone oil-based refrigerants include polysiloxanes such as polydimethylsiloxane and polymethylphenylsiloxane.
[0083] From the viewpoint of reducing the environmental load, the silicone oil-based refrigerant is preferably a fluorine-free silicone oil. The term "fluorine-free" here has the same meaning as "fluorine-free" in "fluorine-free hydrocarbon."
[0084] The coolant may be used alone or in any combination of two or more kinds in any ratio.
[0085] The coolant is preferably insulating. In order not to impede wireless communication in the gigahertz band, the relative dielectric constant of the coolant is preferably 3.0 or less, and more preferably 2.5 or less.
[0086] 1-4. Evaluation Whether an aluminum electrolytic capacitor can be used for immersion cooling using the above-mentioned coolant can be evaluated by conducting a degradation test on the aluminum electrolytic capacitor in the coolant. Specific test methods are as follows (a) to (c).
[0087] (a) The capacitance (Cap) and equivalent series resistance (ESR) of the aluminum electrolytic capacitor before the degradation test are measured using the following method. (b) The aluminum electrolytic capacitor is immersed in a coolant and heated at 125°C for a certain period of time, after which the Cap and ESR of the aluminum electrolytic capacitor are measured using the following method. (c) The Cap change rate and ESR change ratio are calculated using the following formulas (I) and (II).
[0088] (Method of Measuring Cap) Using an LCR meter ("4284A Precision LCR Meter" manufactured by Agilent Technologies, Inc.), the Cap is measured at a temperature of 20° C. and a frequency of 120 Hz.
[0089] (ESR Measurement Method) Using an LCR meter ("4284A Precision LCR Meter" manufactured by Agilent Technologies, Inc.), ESR is measured at a temperature of 20° C. and a frequency of 100 kHz.
[0090] Cap change rate={(Cap before deterioration test−Cap after deterioration test) / (Cap before deterioration test)}×100 Formula (I)
[0091] ESR change ratio=(ESR after degradation test) / (ESR before degradation test) Formula (II)
[0092] When a degradation test of 135 hours or more is performed, the aluminum electrolytic capacitor according to the present embodiment can be determined to be suitable for liquid immersion cooling if it satisfies the following conditions (A) and / or (B), preferably (A) and (B): (A) The cap change rate of the aluminum electrolytic capacitor according to the present embodiment is smaller than the cap change rate of an aluminum electrolytic capacitor that does not have a resin member; (B) The ESR change ratio of the aluminum electrolytic capacitor according to the present embodiment is smaller than the ESR change ratio of an aluminum electrolytic capacitor that does not have a resin member.
[0093] More specifically, the cap change rate at the time point after 135 hours of heating is preferably 15.0% or less, more preferably 12.0% or less, even more preferably 10.0% or less, and particularly preferably 8.0% or less, and the cap change rate at the time point after 190 hours of heating is preferably 50.0% or less, more preferably 20.0% or less, even more preferably 15.0% or less, and particularly preferably 10.0% or less.
[0094] Furthermore, the ESR change ratio at the time point after 135 hours of heating is preferably 4.0 times or less, more preferably 3.0 times or less, even more preferably 2.0 times or less, and particularly preferably 1.6 times or less, and the ESR change ratio at the time point after 190 hours of heating is preferably 100.0 times or less, more preferably 10.0 times or less, even more preferably 3.0 times or less, and particularly preferably 2.0 times or less.
[0095] 2. Cooling Method for Aluminum Electrolytic Capacitor A second embodiment of the present disclosure is a cooling method for an aluminum electrolytic capacitor according to the first embodiment of the present disclosure, comprising an immersion cooling step of immersing the aluminum electrolytic capacitor in a coolant to cool it. The coolant is one or more selected from the group consisting of a hydrocarbon-based refrigerant and a silicone oil-based refrigerant, and is the same as the coolant described in the first embodiment of the present disclosure.
[0096] In this embodiment, the aluminum electrolytic capacitor may be mounted on an electronic device. When the aluminum electrolytic capacitor is mounted on an electronic device, the immersion cooling process is performed by immersing the aluminum electrolytic capacitor together with the electronic device in a cooling liquid. In this case, the immersion cooling process may be performed by immersing at least a component of the electronic device to which the aluminum electrolytic capacitor is attached in the cooling liquid to cool the aluminum electrolytic capacitor. Therefore, the immersion cooling process may be a process of immersing the entire electronic device in the cooling liquid to cool the aluminum electrolytic capacitor, or a process of immersing a part or all of the electronic device in the cooling liquid so that the component to which the aluminum electrolytic capacitor is attached is immersed in the cooling liquid to cool the aluminum electrolytic capacitor. An example of a component to which the aluminum electrolytic capacitor is attached is a substrate such as a printed circuit board. When the aluminum electrolytic capacitor is mounted on an electronic device, the immersion cooling process may cool not only the aluminum electrolytic capacitor but also the entire electronic device or the entire component to which the aluminum electrolytic capacitor is attached.
[0097] The electronic device to be cooled by the immersion cooling process is not particularly limited as long as it has an aluminum electrolytic capacitor according to the first embodiment of the present disclosure, and examples thereof include supercomputers, servers, and communication devices that have printed circuit boards to which aluminum electrolytic capacitors are attached.
[0098] In the immersion cooling process, an aluminum electrolytic capacitor or an electronic device is immersed in a coolant, and heat generated by the operation of the aluminum electrolytic capacitor or the electronic device is transferred to the coolant, thereby cooling (heat dissipation). The specific method for performing the immersion cooling process is not particularly limited as long as the above-mentioned coolant is used, and the process can be performed using a known immersion cooling system. Known immersion cooling systems include a single-phase immersion cooling system that uses the coolant in a liquid state, and a two-phase immersion cooling system that uses the phase change of the coolant.
[0099] According to the cooling method of this embodiment, the airtightness of the aluminum electrolytic capacitor can be improved by swelling of the sealing body during immersion cooling, and the occurrence of the above-mentioned problems can be suppressed. This makes it possible to immerse the aluminum electrolytic capacitor and an electronic device incorporating the aluminum electrolytic capacitor in liquid immersion cooling using a hydrocarbon-based refrigerant and / or a silicone oil-based refrigerant as the coolant.
[0100] 3. Cooling Method for Electronic Devices A third embodiment of the present disclosure is a cooling method for an electronic device having the aluminum electrolytic capacitor according to the first embodiment of the present disclosure, comprising an immersion cooling step of immersing a part or all of the electronic device in a cooling liquid to cool it. The cooling liquid is at least one selected from the group consisting of a hydrocarbon-based refrigerant and a silicone oil-based refrigerant, and is the same as the cooling liquid described in the description of the first embodiment of the present disclosure. The electronic device is also the same as the electronic device described in the description of the second embodiment of the present disclosure.
[0101] In the immersion cooling process, the electronic device is immersed in the coolant so that at least the aluminum electrolytic capacitor is immersed in the coolant. In other words, the immersion cooling process may be a process of immersing the entire electronic device in the coolant to cool the aluminum electrolytic capacitor, or a process of immersing a part or all of the electronic device in the coolant so that the component to which the aluminum electrolytic capacitor is attached is immersed in the coolant to cool the aluminum electrolytic capacitor. An example of a component to which an aluminum electrolytic capacitor is attached is a substrate such as a printed circuit board. The immersion cooling process can cool the entire electronic device or the entire component to which the aluminum electrolytic capacitor is attached.
[0102] In the immersion cooling process, an electronic device is immersed in a coolant, and heat generated during operation is transferred to the coolant, thereby cooling (heat dissipation). The specific method for performing the immersion cooling process is not particularly limited as long as the above-mentioned coolant is used, and the process can be performed using a known immersion cooling system. Known immersion cooling systems include a single-phase immersion cooling system that uses the coolant in a liquid state, and a two-phase immersion cooling system that uses a phase change of the coolant.
[0103] The cooling method according to the present embodiment can prevent the deterioration of the airtightness of the aluminum electrolytic capacitor due to swelling of the sealing body during immersion cooling, thereby preventing the occurrence of the above-mentioned problems. This makes it possible to perform immersion cooling of an electronic device equipped with an aluminum electrolytic capacitor using a hydrocarbon-based refrigerant and / or a silicone oil-based refrigerant as the coolant.
[0104] The present disclosure will be explained in more detail below using examples, but the present disclosure is not limited to the description of the following examples as long as it does not depart from the gist of the disclosure.
[0105] Comparative Example 1-1: An aluminum electrolytic capacitor element (size: diameter 6.1 mm × height 6.3 mm) was obtained by winding an anode foil and a cathode foil with a separator interposed therebetween and immersing the foil in an electrolytic solution. Aluminum foil having an oxide film on its surface was used as the anode foil, and aluminum foil was used as the cathode foil. The electrolytic solution was prepared by dissolving ethylmethylimidazolinium phthalate in γ-butyrolactone to a concentration of 20% by mass.
[0106] The resulting aluminum electrolytic capacitor element was inserted into an aluminum case, and then a sealing member made of butyl rubber was inserted into the opening of the aluminum case, followed by vertical crimping and horizontal crimping in that order to obtain an aluminum electrolytic capacitor.
[0107] Example 1-1 An epoxy resin composition was prepared by mixing 100 parts by mass of bisphenol A epoxy resin, 11 parts by mass of an amine-based curing agent, and an inorganic filler.
[0108] This epoxy resin composition was applied to the area of the surface of the sealing body of the aluminum electrolytic capacitor obtained in Comparative Example 1-1 that was exposed to the outside through the opening of the aluminum case, and cured at 150°C for 3 minutes to obtain the aluminum electrolytic capacitor shown in Figure 1(a).
[0109] Example 1-2 An epoxy resin composition was prepared in the same manner as in Example 1-1, except that 11 parts by mass of the amine curing agent was changed to 85 parts by mass of an acid anhydride curing agent.
[0110] This epoxy resin composition was applied to the area of the surface of the sealing body of the aluminum electrolytic capacitor obtained in Comparative Example 1-1 that was exposed to the outside through the opening of the aluminum case, and cured at 150°C for 30 minutes to obtain the aluminum electrolytic capacitor shown in Figure 1(a).
[0111] Example 1-3 A powdery epoxy resin composition was prepared in the same manner as in Example 1-1, except that the bisphenol A epoxy resin was changed to a cresol novolac epoxy resin, 11 parts by mass of the amine-based curing agent was changed to 20 parts by mass of a phenol-based curing agent, and 1 part by mass of a curing accelerator was further mixed.
[0112] This epoxy resin composition was placed on the surface of the sealing body of the aluminum electrolytic capacitor obtained in Comparative Example 1-1, in a region exposed to the outside from the opening of the aluminum case, and cured for 60 seconds by compression molding at a mold temperature of 175°C. The cured product was then after-cured at 170°C for 1 hour to obtain the aluminum electrolytic capacitor shown in Figure 1(a).
[0113] Example 1-4 An acrylic resin was heated and melted, and applied to the area of the surface of the sealing body of the aluminum electrolytic capacitor obtained in Comparative Example 1-1 that was exposed to the outside through the opening of the aluminum case, and then cooled to room temperature, thereby obtaining the aluminum electrolytic capacitor shown in FIG. 1( a).
[0114] Example 1-5 Polypropylene resin was heated and melted, and applied to the area of the surface of the sealing body of the aluminum electrolytic capacitor obtained in Comparative Example 1-1 that was exposed to the outside through the opening of the aluminum case, and then cooled to room temperature to obtain the aluminum electrolytic capacitor shown in FIG. 1( a).
[0115] [Evaluation of Suitability for Immersion Cooling] The capacitance (Cap) and equivalent series resistance (ESR) of the aluminum electrolytic capacitors were measured using the following method. The aluminum electrolytic capacitors were immersed in the hydrocarbon-based refrigerants shown in Table 1 and allowed to stand at a temperature of 125°C. The Cap and ESR of the aluminum electrolytic capacitors were measured using the following method at 66 hours, 135 hours, and 190 hours after the start of immersion. The measurement results are shown in Table 1.
[0116] (Method for Measuring Cap) Using an LCR meter ("4284A Precision LCR Meter" manufactured by Agilent Technologies, Inc.), the Cap was measured at a temperature of 20° C. and a frequency of 120 Hz.
[0117] (ESR Measurement Method) ESR was measured at a temperature of 20° C. and a frequency of 100 kHz using an LCR meter ("4284A Precision LCR Meter" manufactured by Agilent Technologies, Inc.).
[0118]
[0119] From Table 1, it can be seen that the aluminum electrolytic capacitor obtained in Comparative Example 1-1 had a large decrease in Cap and a large increase in ESR due to immersion in a hydrocarbon-based refrigerant. This is thought to be because the hydrocarbon-based refrigerant had a negative effect on the airtightness of the aluminum electrolytic capacitor.
[0120] On the other hand, it can be seen that the aluminum electrolytic capacitors obtained in Examples 1-1 to 1-3 show almost no difference in Cap and ESR before and after immersion in a hydrocarbon-based refrigerant. Furthermore, the results of Examples 1-1 to 1-3 show that Cap and ESR can be maintained even after immersion in a hydrocarbon-based refrigerant, regardless of the type of curing agent in the epoxy resin composition.
[0121] As described above, the aluminum electrolytic capacitor of the present disclosure exhibits high airtightness due to the resin member, which is believed to be able to suppress a decrease in Cap and an increase in ESR due to immersion cooling. Therefore, the aluminum electrolytic capacitor of the present disclosure can be applied to an immersion cooling system that uses a hydrocarbon refrigerant and / or a silicone oil refrigerant, particularly a hydrocarbon refrigerant, as the coolant.
[0122] In addition, it can be seen that the aluminum electrolytic capacitors obtained in Examples 1-4 and 1-5 also have small differences in Cap and ESR before and after immersion in a hydrocarbon-based refrigerant, similar to the aluminum electrolytic capacitors obtained in Examples 1-1 to 1-3.
[0123] Furthermore, Table 1 shows that when the resin member is made of a cured product of an epoxy resin composition (Examples 1-1 to 1-3) or an acrylic resin (Example 1-4), the decrease in Cap and the increase in ESR of the aluminum electrolytic capacitor can be efficiently suppressed.
[0124] Furthermore, in evaluating the suitability of the aluminum electrolytic capacitor obtained in Example 1-1 for immersion cooling, a comparison was made between the case where a mixture of hydrocarbons having 18 to 50 carbon atoms was used as the hydrocarbon-based refrigerant and the case where PAOs were used, and it was found that there was not much difference in the Cap change rate and ESR change ratio. This shows that, regardless of which hydrocarbon-based refrigerant was used, the resin member can suppress a decrease in Cap and an increase in ESR of the aluminum electrolytic capacitor.
[0125] [Examples 2-1 to 2-3] Each of the epoxy resin compositions prepared in Examples 1-1 to 1-3 was molded and cured in accordance with JIS K 7154-2:2002 ("Plastics - Injection-molded test specimens for thermosetting resin molding materials - Part 2: Small rectangular plates", published July 31, 2002) to prepare test specimens measuring 60 mm x 60 mm x 1 mm.
[0126] [Examples 2-4 to 2-5] The acrylic resin used in Example 1-4 and the polypropylene resin used in Example 1-5 were each molded in accordance with JIS K 7152-3:2006 ("Plastics - Injection-molded test specimens of thermoplastic materials - Part 3: Small rectangular plates", published February 20, 2006) to prepare test specimens measuring 60 mm x 60 mm x 1 mm.
[0127] Example 2-6: An epoxy resin composition was prepared by mixing 100 parts by mass of phenolic resin, 10 parts by mass of hexamine curing agent, and an inorganic filler. This phenolic resin composition was molded and cured in accordance with JIS K 7154-2:2002 ("Plastics - Injection-molded test pieces for thermosetting resin molding materials - Part 2: Small rectangular plates", published July 31, 2002) to prepare test pieces measuring 60 mm x 60 mm x 1 mm.
[0128] [Example 2-7] A polyamide resin was molded in accordance with JIS K 7152-3:2006 ("Plastics - Injection-molded test specimens of thermoplastic materials - Part 3: Small rectangular plates", published February 20, 2006) to prepare a test specimen measuring 60 mm x 60 mm x 1 mm.
[0129] [Example 2-8] A polycarbonate resin was molded in accordance with JIS K 7152-3:2006 ("Plastics - Injection-molded test specimens of thermoplastic materials - Part 3: Small rectangular plates", published February 20, 2006) to prepare a test specimen measuring 60 mm x 60 mm x 1 mm.
[0130] [Example 2-9] Polystyrene resin was molded in accordance with JIS K 7152-3:2006 ("Plastics - Injection-molded test specimens of thermoplastic materials - Part 3: Small square plates", published February 20, 2006) to prepare test specimens measuring 60 mm x 60 mm x 1 mm.
[0131] Comparative Example 2-1 No. 8 dumbbell test specimens were prepared by molding and processing the butyl rubber that was the constituent material of the sealing bodies used in Examples 1-1 to 1-5 and Comparative Example 1-1 in accordance with JIS K 6250:2019 ("Rubber - General rules for physical testing methods", 8. Collection and preparation of test specimens, published June 20, 2019).
[0132] [Evaluation by Swelling Test] Before the swelling test, the weight of the test specimen was measured. Then, the swelling test was carried out as follows. The test specimen was immersed in 10 mL of a hydrocarbon-based refrigerant (Fischer-Tropsch distillate heavy oil; a mixture of hydrocarbons having 18 to 50 carbon atoms), allowed to stand under a constant temperature condition, and then removed from the hydrocarbon-based refrigerant. The hydrocarbon-based refrigerant adhering to the test specimen was wiped off, and the weight of the test specimen was measured. The heating conditions in the swelling test were 105°C for two weeks for the test specimens obtained in Examples 2-1 to 2-9, and 85°C for one week for the test specimen obtained in Comparative Example 2-1.
[0133] The swelling ratio (weight increase ratio) due to the swelling test was calculated from the weight of the test piece before and after the swelling test according to the following formula. The results are shown in Table 2.
[0134]
[0135] [Calculation of HSP distance] The HSP of the constituent material of the test specimen and the hydrocarbon-based refrigerant (Fischer-Tropsch distillate heavy oil; a mixture of hydrocarbons with 18 to 50 carbon atoms) was calculated using the HSP analysis software "HSPiP (Ver. 5.4.05)". The HSP distance between the constituent material of the test specimen and the hydrocarbon-based refrigerant obtained from these calculated values is shown in Table 2. The relationship between this HSP distance and the swelling ratio is shown in Figure 6.
[0136]
[0137] From Table 2, it was confirmed that the test pieces of Examples 2-1 to 2-9 had smaller swelling ratios than the test piece (Comparative Example 2-1) formed from butyl rubber, which is the constituent material of the sealing bodies of the aluminum electrolytic capacitors of Examples 1-1 to 1-5.
[0138] Furthermore, Table 2 and Figure 6 confirm that there is a correlation between the HSP distance between the constituent material of the test specimen and the hydrocarbon refrigerant and the swelling ratio. Specifically, it was confirmed that if the HSP distance between the constituent material of the test specimen and the hydrocarbon refrigerant is 4.5 or more, the swelling ratio can be suppressed, if it is 7.5 or more, the swelling ratio can be further suppressed, and if it is 13.0 or more, the swelling ratio can be further suppressed. Furthermore, Table 2 shows that there is a correlation between the HSP distance and the Cap change rate and the ESR change rate, and there is also a correlation between the swelling ratio and the Cap change rate and the ESR change rate.
[0139] From these facts, it is considered that even when the constituent materials of the test specimens of Examples 2-6 to 2-9 are used as the materials for the resin members, it is possible to suppress the Cap reduction and ESR increase of the aluminum electrolytic capacitor caused by immersion cooling, as in Examples 1-1 to 1-5.
[0140] 2 Capacitor element 4 Metal case 4a Horizontal crimped portion 4b Vertical crimped portion 6 Sealing body 6a Rubber layer 6b Substrate 8 Resin member 9 Terminal 10 Aluminum electrolytic capacitor
Claims
1. An aluminum electrolytic capacitor for liquid immersion cooling that is cooled in a coolant, comprising an aluminum electrolytic capacitor element and a resin member that prevents the coolant from penetrating into the aluminum electrolytic capacitor, the coolant being one or more refrigerants selected from the group consisting of hydrocarbon-based refrigerants and silicone oil-based refrigerants.
2. The aluminum electrolytic capacitor for liquid immersion cooling according to claim 1, wherein the resin member is made of a resin material having a Hansen solubility parameter distance with the cooling liquid of 4.5 or more.
3. The aluminum electrolytic capacitor for liquid immersion cooling according to claim 1, wherein the resin member is made of a resin material containing one or more resins selected from the group consisting of epoxy resin, phenolic resin, (meth)acrylic resin, polyamide resin, polycarbonate resin, and polystyrene resin.
4. The aluminum electrolytic capacitor for liquid immersion cooling according to claim 2, wherein the resin member comprises a cured product of an epoxy resin composition containing the epoxy resin and one or more curing agents selected from the group consisting of a phenol-based curing agent, an amine-based curing agent, and an acid anhydride-based curing agent.
5. The aluminum electrolytic capacitor for liquid immersion cooling according to claim 1, wherein the cooling liquid is at least one selected from the group consisting of a mixture of hydrocarbons having 15 to 50 carbon atoms and poly-α-olefins.
6. The aluminum electrolytic capacitor for liquid immersion cooling according to claim 1, wherein the aluminum electrolytic capacitor element contains one or more electrolytes selected from the group consisting of liquid electrolytes and solid electrolytes.
7. The aluminum electrolytic capacitor for liquid immersion cooling according to claim 1, comprising a cylindrical metal case with a bottom that houses the aluminum electrolytic capacitor element and a sealing body that seals an opening of the metal case, and the resin member is a member that covers an area of the surface of the sealing body that is surrounded by the opening.
8. A cooling method for an aluminum electrolytic capacitor, comprising: an immersion cooling step of immersing the aluminum electrolytic capacitor in a cooling liquid to cool it, the aluminum electrolytic capacitor having an aluminum electrolytic capacitor element and a resin member that suppresses penetration of the cooling liquid into the aluminum electrolytic capacitor, and the cooling liquid is one or more types selected from the group consisting of a hydrocarbon-based refrigerant and a silicone oil-based refrigerant.
9. The cooling method for an aluminum electrolytic capacitor according to claim 8, wherein the aluminum electrolytic capacitor is mounted on an electronic device, and the liquid immersion cooling step is carried out by immersing a part or the whole of the electronic device in the cooling liquid.
10. A method for cooling an electronic device having an aluminum electrolytic capacitor, comprising: an immersion cooling step of immersing a part or all of the electronic device in a cooling liquid to cool it, the immersion cooling step being performed so that at least the aluminum electrolytic capacitor is immersed in the cooling liquid, the aluminum electrolytic capacitor has an aluminum electrolytic capacitor element and a resin member that suppresses penetration of the cooling liquid into the aluminum electrolytic capacitor, and the cooling liquid is one or more types selected from the group consisting of hydrocarbon-based refrigerants and silicone oil-based refrigerants.
Citation Information
Patent Citations
JP1982061827U
Solid electrolytic capacitor and its manufacture
JP2000114118A
Set battery
JP2001060466A
Electrolytic capacitor
JP2012182326A
Electrolytic capacitor
WO2021193282A1