Dielectric composition with high-temperature stability

The dielectric composition, combining barium titanate with specific auxiliary components, addresses the challenge of maintaining capacitance stability at high temperatures in multilayer ceramic capacitors, achieving X8R standards and controlling sintering temperatures, thereby improving the reliability and voltage stability of these components.

WO2024225690A1PCT designated stage expired Publication Date: 2024-10-31AMOTECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005201
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2024-04-18
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Multilayer ceramic capacitors used in automotive applications face challenges in maintaining capacitance stability at high temperatures, with existing dielectric compositions experiencing significant changes in capacitance and sintering temperature issues, which affect the reliability and voltage stability of these components.

Method used

A dielectric composition based on a barium titanate (BaTiO3) main component, supplemented with auxiliary components such as Yb2O3, BaZrO3, Y2O3, MgCO3, V2O5, MnO2, and SiO2, which helps in achieving the X8R temperature characteristics by controlling the Curie temperature and reducing extreme dielectric constant changes while suppressing the increase in sintering temperature.

Benefits of technology

The proposed dielectric composition effectively maintains capacitance stability within ±15% over a temperature range of -55°C to 150°C, meeting the X8R standard while keeping the sintering temperature within manageable limits, thus enhancing the reliability and voltage stability of multilayer ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005201_31102024_PF_FP_ABST
    Figure KR2024005201_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A dielectric composition comprising a barium titanate-based base material major component and a minor component is disclosed. The dielectric composition comprises at least one minor component from among: a first minor component, which can be oxides or carbonates of Yb; a second minor component, which can be oxides including Ba and Zr; a third minor component, which can be oxides or carbonates of Y; a fourth minor component, which can be oxides or carbonates of Mg; a fifth minor component, which can be oxides or carbonates of V and Mn; and a sixth minor component, which can be oxides or carbonates of Si, wherein the at least one minor component can comprise the first minor component. The present invention satisfies X8R properties specified by EIA standards.
Need to check novelty before this filing date? Find Prior Art

Description

Dielectric composition with high temperature stability

[0001] The present invention relates to a dielectric composition having high temperature stability, and more particularly, to a dielectric composition satisfying X8R characteristics.

[0002] Multilayer ceramic chip capacitors have high capacity and high reliability, but are relatively small in size, so they are widely used in fields such as automobiles and motors that require precision and stability.

[0003] Multilayer ceramic capacitors have various requirements, such as capacity, temperature stability, and voltage stability. In particular, multilayer ceramic capacitors for automotive electronics must not change their capacity (capacitance) even at high temperatures because they operate at high temperatures. In this regard, the Electronic Industries Association (EIA) of the United States stipulates that a multilayer ceramic capacitor satisfies the X8R characteristic when the change in capacitance between -55 and 150 degrees Celsius is within ±15% of the reference capacitance at 25 degrees Celsius.

[0004] The present invention provides a dielectric composition that satisfies the X8R standard.

[0005] A dielectric composition according to embodiments of the present invention includes a barium titanate-based base material main component and a subcomponent, and the subcomponents include a first subcomponent including at least one selected from the group consisting of oxides and carbonates of Yb element, a second subcomponent including at least one selected from the group consisting of oxides including Ba and Zr, a third subcomponent including at least one selected from the group consisting of oxides and carbonates of Y element, a fourth subcomponent including at least one selected from oxides and carbonates of a valence-fixed acceptor element including Mg, a fifth subcomponent including at least one selected from the group consisting of oxides and carbonates of a valence-variable acceptor element including at least one selected from the group consisting of oxides and carbonates of Si element, and a sixth subcomponent including at least one selected from the group consisting of oxides, carbonates, and glasses of Si element. At least one subcomponent is included, and at least one subcomponent includes a first subcomponent, and the content of the Yb element included in the first subcomponent is 0.2 to 6 molar parts with respect to 100 molar parts of the main component of the parent material.

[0006] The dielectric composition of the present invention satisfies the X8R characteristics of the EIA standard.

[0007] FIG. 1 is a perspective view showing a laminated ceramic capacitor according to an embodiment of the present invention.

[0008] FIG. 2 is a perspective view showing a plurality of electrode units of a laminated ceramic capacitor according to an embodiment of the present invention.

[0009] Hereinafter, in order to explain the technical idea of ​​the present invention in detail to an extent that a person of ordinary skill in the art to which the present invention pertains can easily put it into practice, the most preferred embodiment of the present invention will be described with reference to the accompanying drawings. First, when adding reference numerals to components in each drawing, it should be noted that the same components are given the same numerals as much as possible even if they are shown in different drawings. In addition, when describing the present invention, if it is determined that a specific description of a related well-known structure or function may obscure the gist of the present invention, the detailed description thereof will be omitted.

[0010] The present invention relates to a dielectric composition, and electronic components including the dielectric composition include capacitors, inductors, piezoelectric elements, varistors, thermistors, etc., and below, a multilayer ceramic capacitor (MLCC) will be described as an example of the dielectric composition and electronic components.

[0011] Multilayer ceramic capacitors

[0012] FIG. 1 is a perspective view showing a multilayer ceramic capacitor according to an embodiment of the present invention, and FIG. 2 is a perspective view showing a plurality of electrode units of a multilayer ceramic capacitor according to an embodiment of the present invention.

[0013] Referring to FIG. 1, a multilayer ceramic capacitor according to an embodiment of the present invention is configured to include a dielectric (100), a first external electrode (220), and a second external electrode (240).

[0014] The dielectric (100) is composed of a rectangular parallelepiped having a top surface, a bottom surface, a first side surface, a second side surface opposite the first side surface, a third side surface, and a fourth side surface opposite the third side surface. As an example, the first side surface is the left side in the drawing, the second side surface is the right side in the drawing, the third side surface is the front side in the drawing, and the fourth side surface is the back side in the drawing.

[0015] The dielectric (100) may include a plurality of dielectric sheets. The plurality of dielectric sheets may be laminated. Each dielectric sheet may include a dielectric composition and may be formed by sintering the dielectric composition.

[0016] The first external electrode (220) is an electrode disposed on the first side of the dielectric (100). The first external electrode (220) may be formed to extend from the first side of the dielectric (100) to the upper surface, lower surface, third side, and fourth side of the dielectric (100). The second external electrode (240) is an electrode disposed on the second side of the dielectric (100). The second external electrode (240) may be formed to extend from the second side of the dielectric (100) to the upper surface, lower surface, third side, and fourth side of the dielectric (100). The first external electrode (220) and the second external electrode (240) may be formed to face each other at a predetermined distance from each other on the upper surface, lower surface, third side, and fourth side of the dielectric (100).

[0017] Referring to FIG. 2, a laminated ceramic capacitor according to an embodiment of the present invention may further include a plurality of electrode units (300). At this time, the plurality of electrode units (300) are laminated to form a laminate, and this laminate is disposed inside a dielectric (100).

[0018] A plurality of electrode units (300) are stacked vertically in the drawing and placed inside the dielectric (100). Each electrode unit (300) includes a first electrode set (320) and a second electrode set (340), and the first electrode set (320) and the second electrode set (340) are alternately stacked.

[0019] The first electrode set (320) is composed of a plate-shaped conductor formed in a rectangular shape. The first electrode set (320) is arranged inside the dielectric (100) so as to be offset from the first side of the dielectric (100). The first end of the first electrode set (320) is connected to the first external electrode (220) at the first side of the dielectric (100).

[0020] The second electrode set (340) is composed of a plate-shaped conductor formed in a rectangular shape. The second electrode set (340) is arranged inside the dielectric (100) so as to be offset from the second side of the dielectric (100). The first end of the second electrode set (340) is connected to the second external electrode (240) at the second side of the dielectric (100).

[0021] The first electrode set (320) and the second electrode set (340) are respectively distributed and arranged on two adjacent dielectric sheets among the dielectric sheets included in the dielectric (100). The first electrode set (320) and the second electrode set (340) may partially overlap each other with the dielectric sheet (110) therebetween.

[0022] Dielectric composition and method for producing the same

[0023] Hereinafter, a dielectric composition and a manufacturing method thereof according to embodiments of the present invention will be described in detail. The dielectric composition can form the above-described dielectric (100). However, to avoid redundant description, any content that overlaps with the above-described content will be omitted.

[0024] The dielectric composition according to embodiments of the present invention may include a parent material main component including a rare earth element. The parent material main component may be a barium titanate compound including Ba and Ti, and preferably, BaTiO3. In addition, the dielectric composition according to embodiments of the present invention may additionally include an auxiliary component, and the auxiliary component may include the first to sixth auxiliary components.

[0025] The dielectric composition according to embodiments of the present invention may include the auxiliary components of Table 1 per 100 moles of the base material BaTiO3.

[0026] 1st auxiliary ingredient 2nd auxiliary ingredient 3rd auxiliary ingredient 4th auxiliary ingredient 5th auxiliary ingredient 6th auxiliary ingredient Yb2O3BaZrO3Y2O3MgCO3V2O5MnO2Ba 0.6 Ca 0.4 SiO30.1-3.000.1-3.000-1.000.1-2.000.03-2.000.03-2.000.1-5.00

[0027] In order to implement the X8R temperature characteristics, a dielectric composition with rare earth materials (such as Yb2O3) that increase the Curie temperature or a modified base material (BaTiO3) instead of the main component of the base material was used. 1-x Ca x ) A dielectric composition using TiO3, etc. has been developed. Here, in the case of a dielectric composition with Yb2O3, a rare earth material, added, it can meet the X8R standard, which requires that the temperature coefficient of capacitance (TCC) at 150℃ change within the range of +15% to -15% as the Curie temperature increases. However, the dielectric composition with Yb2O3 added has a problem in that the sintering temperature increases as Yb2O3 is added to implement the X8R temperature characteristics. If the sintering temperature becomes excessively high, the heat generation of the MLCC increases, which damages the Ni internal electrode, which may cause connectivity problems of the internal electrode, and there is a problem in that the process becomes complicated. In addition, among the base materials modified by substitution, etc., the widely known one is (Ba) in which Ca is substituted for Ba. 1-x Ca x )TiO3, i.e. BCT, and when these BCTs are used alone or in combination in a dielectric composition, the change in capacity with temperature is small, and at the same time, it can satisfy the X8R standard that the change should be within the range of +15% to -15% as the Curie temperature rises. However, the dielectric composition using BCT as a parent material has the disadvantage of high difficulty in BCT synthesis. When synthesizing BCT, Ca initially substitutes for Ba, but as the amount of Ca added increases, it gradually substitutes for Ti instead of Ba, so Ba(Ti 1-x Ca x )O3, and in this case, the Curie temperature is rather lowered, so it is not suitable for the X8R composition. In addition, BCT has a problem that it is somewhat disadvantageous in implementing capacity because the dielectric constant is low compared to the composition with Yb2O3 added.

[0028] To solve this problem, the dielectric composition according to embodiments of the present invention is characterized by providing a dielectric composition that can suppress a rise in sintering temperature while satisfying the standard of X8R that must change within the range of 15% to -15% by adding Yb2O3 and BaZrO3 to BaTiO3. The dielectric composition according to embodiments of the present invention can suppress a rise in sintering temperature by reducing the amount of Yb2O3 added as BaZrO3 is added to BaTiO3, and at the same time, the overall permittivity is reduced due to BaZrO3, and the change in permittivity according to temperature is reduced, thereby alleviating extreme permittivity changes around the Curie temperature. That is, the dielectric composition according to embodiments of the present invention satisfies the X8R (-55°C to 150°C) characteristic specified in the EIA standard, thereby realizing a dielectric composition with excellent reliability and a multilayer ceramic capacitor including the same.

[0029]

[0030] Hereinafter, each component of the dielectric composition according to embodiments of the present invention will be described in more detail.

[0031] Main ingredient of the parent material

[0032] The dielectric composition according to embodiments of the present invention may include a base material component including Ba and Ti. According to embodiments, the base material component is BaTiO3.

[0033] The above-mentioned parent material main component may be included in a dielectric composition in powder form. The average particle diameter of the parent material main component powder is not particularly limited, but may be 1000 nm or less. Preferably, the average particle diameter of the parent material main component powder may be 200 nm to 350 nm, and more preferably, 250 nm.

[0034] First component

[0035] The dielectric composition according to embodiments of the present invention may include, as a first auxiliary component, at least one selected from the group consisting of oxides and carbonates of the Yb element. Alternatively, the first auxiliary component may include, instead of the Yb element, at least one selected from the group consisting of oxides and carbonates of at least one of other rare earth elements, namely Sc, Lu, and Tm.

[0036] The first auxiliary component may be included in an amount of 0.2 to 6 mol parts per 100 mol parts of the parent material main component. The content of the first auxiliary component may be based on the content of the element included in the first auxiliary component, regardless of the addition form such as oxide or carbonate. For example, the total content of the element included in the first auxiliary component may be 0.2 to 6 mol parts per 100 mol parts of the parent material main component. For example, when the first auxiliary component is Yb2O3, assuming that 2 mol parts of Yb2O3 exist per 100 mol parts of BaTiO3, 4 mol parts of Yb, a metal included in the first auxiliary component, exist. Therefore, in this case, 4 mol parts of Yb are included per 100 mol parts of BaTiO3.

[0037] The first subcomponent may have the effect of shifting the Curie temperature toward a higher temperature and improving the stability of capacitance according to temperature changes. In other words, the first subcomponent serves to prevent a decrease in the reliability of a multilayer ceramic capacitor formed using a dielectric composition according to embodiments of the present invention.

[0038] If the content of the Yb element included in the first subcomponent is less than 0.2 mol parts with respect to 100 mol parts of the main component of the parent material, the effect of improving the temperature coefficient of capacitance (TCC) in the high temperature section may not be significantly observed, and if the content of the Yb element included in the first subcomponent exceeds 6 mol parts with respect to 100 mol parts of the main component of the parent material, the characteristics related to sintering may be deteriorated.

[0039] Second component

[0040] The dielectric composition according to embodiments of the present invention may include at least one selected from the group consisting of oxides containing Ba and Zr as a second auxiliary component. The second auxiliary component is preferably BaZrO3 or a mixture of BaO and ZrO2, but is not limited thereto. In the case of BaZrO3, the ratio of Ba and Zr is not particularly limited, and the molar ratio of Ba to Zr (Ba / Zr) may be 0.5 to 1.5, and preferably, 0.9 to 1.1.

[0041] When a second auxiliary component is added, the overall permittivity may decrease, and the permittivity change according to temperature may become flat. The second auxiliary component may be included in an amount of 0.1 to 3 mol parts per 100 mol parts of the main component of the base material. If the content of the second auxiliary component is less than 0.1 mol parts per 100 mol parts of the main component of the base material, the high-temperature TCC improvement effect may not be significantly exhibited, and if the content of the second auxiliary component exceeds 3 mol parts per 100 mol parts of the main component of the base material, the high-temperature withstand voltage characteristics may deteriorate.

[0042] Third component

[0043] The dielectric composition according to embodiments of the present invention may include, as a third auxiliary component, at least one selected from the group consisting of oxides and carbonates of the Y element. Alternatively, the third auxiliary component may include at least one selected from the group consisting of oxides and carbonates of at least one rare earth element selected from Dy, Ho, Tb, Gd, Eu, and Er instead of the Y element. The third auxiliary component is preferably Y2O3, which is an oxide of Y, but is not limited thereto.

[0044] The third auxiliary component may be contained in an amount of 2 molar parts or less with respect to 100 molar parts of the parent material main component. The content of the third auxiliary component may be based on the content of the element contained in the third auxiliary component, regardless of the addition form such as oxide or carbonate. For example, the total content of the elements contained in the third auxiliary component may be 2 molar parts or less with respect to 100 molar parts of the parent material main component. For example, when the third auxiliary component is Y2O3, assuming that Y2O3 exists in an amount of 0.3 molar parts with respect to 100 molar parts of BaTiO3, Y, a metal contained in the third auxiliary component, exists in an amount of 0.6 molar parts. Therefore, in this case, Y is contained in an amount of 0.6 molar parts with respect to 100 molar parts of BaTiO3.

[0045] The third auxiliary component can help improve the high-temperature TCC and prevent the deterioration of the reliability of the multilayer ceramic capacitor formed from the dielectric composition. If the content of the Y element contained in the third auxiliary component exceeds 2 mol parts per 100 mol parts of the main component of the base material, this effect may be insufficient.

[0046] 4th subsidiary component

[0047] The dielectric composition according to embodiments of the present invention may include at least one of an oxide and a carbonate of a fixed-valence acceptor element including Mg as a fourth component.

[0048] The fourth auxiliary component may be included in an amount of 0.1 to 2 mol parts or less with respect to 100 mol parts of the main component of the parent material. The content of the fourth auxiliary component may be based on the content of the Mg element included in the fourth auxiliary component, regardless of the addition form such as oxide or carbonate. For example, the content of the Mg element included in the fourth auxiliary component may be 0.1 to 2 mol parts or less with respect to 100 mol parts of the main component of the parent material.

[0049] If the content of the fourth component is less than 0.1 mol parts or more than 2 mol parts with respect to 100 mol parts of the main component of the dielectric base material, the dielectric constant may decrease and the high-temperature withstand voltage characteristics may decrease, which is not desirable.

[0050] 5th subsidiary component

[0051] The dielectric composition according to embodiments of the present invention may include at least one selected from the group consisting of oxides and carbonates of atomic variable acceptor elements including at least one of V, Mn, Cr, Fe, Ni, Co, Cu, and Zn as a fifth auxiliary component. The fifth auxiliary component is V2O5 and It is preferable that at least one selected from the group consisting of MnO2, but is not limited thereto.

[0052] The fifth auxiliary component may be included in an amount of 0.03 to 4 molar parts per 100 molar parts of the parent material main component. The content of the fifth auxiliary component may be based on the content of the elements included in the fifth auxiliary component, regardless of the addition form, such as oxide or carbonate. For example, the total content of the elements included in the fifth auxiliary component may be 0.03 to 4 molar parts per 100 molar parts of the parent material main component.

[0053] The fifth auxiliary component can improve the high-temperature withstand voltage characteristics by improving the reduction resistance of the dielectric composition. If the content of the fifth auxiliary component is less than 0.03 parts by mole, the high-temperature withstand voltage may be reduced, and if it exceeds 4 parts by mole, the reliability of the dielectric magnetic composition may be reduced (e.g., a decrease in permittivity, etc.).

[0054] 6th component

[0055] The dielectric composition according to embodiments of the present invention may include, as a sixth auxiliary component, at least one selected from the group consisting of an oxide of Si element, a carbonate of Si element, and a glass containing Si element. Preferably, the sixth auxiliary component is Ba. x Ca 1-x It may include a complex oxide represented by SiO3 (wherein x is 0.3 to 0.8). The x value of the complex oxide may be 0.3 to 0.8. Here, if the x value is too small, the dielectric properties may deteriorate due to a reaction between SiO2 and the main component BaTiO3. Conversely, if the x value is too large, the melting point may increase, which may deteriorate the properties related to plasticity.

[0056] The sixth auxiliary component may be included in an amount of 0.1 to 5 mol parts based on 100 mol parts of the main component of the above-mentioned parent material. If the content of the sixth auxiliary component is less than 0.1 mol parts, the rate of change in capacitance depending on temperature may increase. Conversely, if the content of the sixth auxiliary component exceeds 5 mol parts, problems such as reduced sinterability and density, and formation of secondary phases may occur, which is not preferable.

[0057] Hereinafter, the configuration and effects of the present invention will be described in more detail with specific examples and comparative examples, but these examples are only intended to make the present invention more clearly understood and are not intended to limit the scope of the present invention.

[0058] As a starting material for forming a dielectric layer, the main component BaTiO3 powder is prepared, and as auxiliary components, Yb2O3, BaZrO3, Y2O3, MgCO3, V2O5, MnO2, Ba 0.6 Ca 0.4 SiO3 was prepared respectively. Here, the BaTiO3 mixed solid solution powder, which is the base material powder containing the main component, was manufactured by applying the solid-state method as follows.

[0059] The starting materials are BaCO3 and TiO2. These starting material powders were mixed in a ball mill and calcined at 900-1000℃ to prepare the main component base material powder. After mixing the auxiliary component additive powders with the main component base material powder in the ingredient ratios shown in Table 2, the raw material powder containing the main and auxiliary components was ball milled for a predetermined time (e.g., 20 hours) using zirconia balls as a mixing / dispersing medium and mixing ethanol / toluene with a dispersant and binder.

[0060] The manufactured slurry was molded into a 10㎛ thick sheet using a doctor blade type coater, and Ni internal electrodes were printed on the molded sheet. The upper and lower covers were manufactured by laminating 25 layers of cover sheets, and 21 layers of printed active sheets were pressed and laminated to manufacture a press bar. The press bar was cut into chips of size 3225 (length Х width Х thickness 3.2 mm Х 2.5 mm Х 2.5 mm) using a cutter.

[0061] After the manufactured chip was calcined, it was fired at a temperature of 1150°C to 1350°C for more than 1 hour in a reducing atmosphere (0.1% H2 / 99.9% N2, H2O / H2 / N2 atmosphere), and then heat-treated by reoxidation in a nitrogen (N2) atmosphere at a temperature of 1000°C for more than 2 hours.

[0062] The external electrode was completed by performing a termination process and electrode firing using copper paste on the fired chip.

[0063] For the laminated ceramic capacitor specimens completed as described above, the capacitance (dielectric constant), temperature-dependent capacitance change (TCC), and sintering temperature were measured and evaluated. In addition, room temperature insulation resistance, high-temperature accelerated life, and loss factor were evaluated, but are not described.

[0064] The room temperature capacitance was measured using an LCR meter under conditions of 1 kHz and AC 0.2 V / ㎛. The permittivity of the multilayer ceramic capacitor (MLCC) chip was calculated from the capacitance, dielectric thickness, internal electrode area, and number of layers of the multilayer ceramic capacitor (MLCC) chip.

[0065] The change in capacitance according to temperature was measured in the temperature range of -55℃ to 150℃. In this temperature range, the capacitance change was measured under the conditions of 1kHz and 1Vrms using an LCR-meter. At this time, the change rate (%) of the capacitance at each temperature was measured compared to the capacitance at 25℃. In this specification, the change in capacitance at 150℃ is described. If the change rate of capacitance (Temperature Coefficient of Capacitance, TCC) at 150℃ was within ±15%, it was judged as good, and otherwise, it was judged as bad.

[0066] Table 2 below is a composition table of comparative examples, and Table 3 shows the characteristics of a multilayer ceramic capacitor chip corresponding to the composition specified in Table 2. In Table 2, Comparative Examples 1 to 4 differ from the examples described later in that the second auxiliary component BaZrO3 is not added.

[0067] 100 moles of main ingredient of the parent material, moles of auxiliary ingredient, handmade 1st part ingredient, 2nd part ingredient, 3rd part ingredient, 4th part ingredient, 5th part ingredient, 6th part ingredient, Yb2O3BaZrO3Y2O3MgCO3V2O5MnO2Ba 0.6 Ca 0.4SiO3Comparative Example 11.09001.450.060.132.7Comparative Example 22.18001.450.060.132.7Comparative Example 34.36001.450.060.132.7Comparative Example 45001.450.060.132.7

[0068] Dielectric constant, high temperature TCC (150℃), sintering temperature (℃), characteristic judgment, comparative example 1, 800-19.8, 1, 180X, comparative example 2, 500-19.4, 1, 200X, comparative example 3, 350-13.0, 1, 290O, comparative example 4, 350-10.1, 1, 310O

[0069] Comparative Examples 1 to 4 in Table 2 represent samples in which the content of the third auxiliary component Y was fixed at 0 mol, the content of the fourth auxiliary component Mg was fixed at 1.45 mol, the content of the sum of the fifth auxiliary component (V, Mn) was fixed at 0.25 mol, and the content of the sixth auxiliary component was fixed at 2.7 mol, and the content of the first auxiliary component Yb was changed while no second auxiliary component was added, and Table 3 shows the characteristics of samples corresponding to Comparative Examples 1 to 4 in Table 2. In the range where the content of the first auxiliary component Yb was 4.36 mol or less (Comparative Examples 1 to 2), the high-temperature TCC (150°C) exceeded ±15% and was vulnerable to temperature changes. In the range where the content of the first auxiliary component Yb was 8.72 mol or more (Comparative Examples 3 to 4), the high-temperature TCC satisfied the X8R specification within ±15%. However, as the content of Yb increases, the rate of change in capacity decreases, but there is a problem that the sintering temperature increases, causing damage to the Ni internal electrode. According to the comparative examples of the present invention, when the content of the first auxiliary component Yb is 10 moles or more, a sintering temperature of 1300°C or higher is required.

[0070] To solve this, the dielectric composition according to embodiments of the present invention is characterized by providing a dielectric composition capable of suppressing an increase in sintering temperature while satisfying the criteria of X8R that must vary within a range of 15% to -15% by adding Yb2O3 and BaZrO3 to BaTiO3.

[0071] Table 4 below is a composition table of examples, and Table 5 shows the characteristics of a multilayer ceramic capacitor chip corresponding to the composition specified in Table 4. In Table 4, examples 2 to 6 differ from the comparative examples described above in that the second auxiliary component, BaZrO3, is added.

[0072] 100 moles of main ingredient of the parent material, moles of auxiliary ingredient, handmade 1st part ingredient, 2nd part ingredient, 3rd part ingredient, 4th part ingredient, 5th part ingredient, 6th part ingredient, Yb2O3BaZrO3Y2O3MgCO3V2O5MnO2Ba 0.6 Ca 0.4 SiO3Example 12001.450.060.132.7Example 22101.450.060.132.7Example 321.501.450.060.132.7Example 42201.450.060.132.7Example 52301.450.060.132.7Example 62501.450.060.132.7

[0073] Dielectric constant High temperature TCC (150℃) Sintering temperature (℃) Characteristics Determination Example 1 1500-16.5 1200 X Example 2 1900-11.3 1265 O Example 3 1800-11.1 1250 O Example 4 1800-12.3 1250 O Example 5 1900-12.8 1245 O Example 6 1900-19.7 1235 X

[0074] Examples 1 to 6 in Table 4 show samples in which the content of the second auxiliary component was changed while the content of the first auxiliary component Yb was fixed at 2 mol, the content of the third auxiliary component Y was fixed at 0 mol, the content of the fourth auxiliary component Mg was fixed at 1.45 mol, the content of the sum of the fifth auxiliary component (V, Mn) was fixed at 0.25 mol, and the content of the sixth auxiliary component was fixed at 2.7 mol. Table 5 shows the characteristics of the samples corresponding to Examples 1 to 6 in Table 4. When the content of the second auxiliary component was 0 mol (Example 1), there was a problem that the high temperature TCC (150°C) exceeded ±15% and was vulnerable to temperature changes. In addition, when the content of the second auxiliary component exceeded 3 mol (Example 6), there was a problem that the high temperature TCC (150°C) exceeded ±15% and was vulnerable to temperature changes. In the range where the content of the second auxiliary component exceeds 0 mol (e.g., 0.1 mol or more) and is 3 mol or less (Examples 2 to 5), the high temperature TCC was found to be within ±15%, satisfying the X8R standard. Therefore, the appropriate content range of the second auxiliary component can be said to be 0.1 to 3 mol parts or less with respect to 100 mol parts of the main component of the base material.

[0075] Examples 2 to 5 showed that the high temperature TCC was within ±15% when the second auxiliary component BaZrO3 was added, satisfying the X8R standard while having a sintering temperature within the range of 1245°C to 1265°C. That is, the sintering temperatures of Examples 2 to 5 were lower than the sintering temperatures of Comparative Examples 3 to 4, which were in the range of 1290°C to 1310°C. In this way, it can be seen that the addition of the second auxiliary component BaZrO3 to the dielectric composition can satisfy the X8R standard even without increasing the content of the first auxiliary component Yb2O3, and at the same time, can lower the content of Yb2O3, thereby having the effect of suppressing the increase in sintering temperature.

[0076] 100 moles of main ingredient of the parent material, moles of auxiliary ingredient, handmade 1st part ingredient, 2nd part ingredient, 3rd part ingredient, 4th part ingredient, 5th part ingredient, 6th part ingredient, Yb2O3BaZrO3Y2O3MgCO3V2O5MnO2Ba 0.6 Ca 0.4SiO3Example 701.501.450.060.132.7Example 80.11.501.450.060.132.7Example 921.501.450.060.132.7Example 1031.501.450.060.132.7Example 1141.501.450.060.132.7

[0077] Dielectric constant High temperature TCC (150℃) Sintering temperature (℃) Characteristics Determination Example 7 1900-19.4 1200 X Example 8 1800-11.5 1245 O Example 9 1500-10.9 1250 O Example 10 1400-12.3 1265 O Example 11 1350-19.8 1280 X

[0078] Examples 7 to 11 in Table 6 show samples in which the content of the first auxiliary ingredient was changed while the content of the second auxiliary ingredient was fixed at 1.5 mol, the content of the third auxiliary ingredient Y was fixed at 0 mol, the content of the fourth auxiliary ingredient Mg was fixed at 1.45 mol, the content of the sum of the fifth auxiliary ingredient (V, Mn) was fixed at 0.25 mol, and the content of the sixth auxiliary ingredient was fixed at 2.7 mol. Table 7 shows the characteristics of the samples corresponding to Examples 7 to 11 in Table 6. When the content of the first auxiliary ingredient Yb was 0 mol (Example 7), there was a problem that the high-temperature TCC (150°C) exceeded ±15% and was vulnerable to temperature changes. In addition, when the content of the first auxiliary ingredient Yb exceeded 6 mol (Example 11), there was a problem that the high-temperature TCC (150°C) exceeded ±15% and was vulnerable to temperature changes. In the range where the content of the first auxiliary component Yb exceeds 0 mol (e.g., 0.2 mol or more) and is 6 mol or less (Examples 8 to 10), the high-temperature TCC was found to be within ±15%, satisfying the X8R standard, and the sintering temperature was also found to be lower than that of the comparative examples. Therefore, the appropriate content range of the first auxiliary component Yb can be said to be 0.2 to 6 mol parts in element ratio with respect to 100 mol parts of the main component of the base material.

[0079] 100 moles of main ingredient of the parent material, moles of auxiliary ingredient, handmade 1st part ingredient, 2nd part ingredient, 3rd part ingredient, 4th part ingredient, 5th part ingredient, 6th part ingredient, Yb2O3BaZrO3Y2O3MgCO3V2O5MnO2Ba 0.6 Ca 0.4SiO3Example 1221.50.51.450.060.132.7Example 1321.511.450.060.132.7Example 1421.521.450.060.132.7

[0080] Dielectric constant High temperature TCC (150℃) Sintering temperature (℃) Characteristics Determination Example 12 1800-11.0 1245O Example 13 1800-10.9 1250O Example 14 1500-19.1 1300X

[0081] Examples 12 to 14 in Table 8 show samples in which the content of the third auxiliary component Y was changed while the content of the first auxiliary component Yb was fixed at 2 mol, the content of the second auxiliary component was fixed at 1.5 mol, the content of the fourth auxiliary component Mg was fixed at 1.45 mol, the content of the sum of the fifth auxiliary component (V, Mn) was fixed at 0.25 mol, and the content of the sixth auxiliary component was fixed at 2.7 mol. Table 9 shows the characteristics of the samples corresponding to Examples 12 to 14 in Table 8. When the content of the third auxiliary component Y exceeded 2 mol (Example 14), the high-temperature TCC (150°C) exceeded ±15%, which was a problem in that it was vulnerable to temperature changes. In the range where the content of the third auxiliary component Y was 2 mol or less (Examples 12 to 13), the high-temperature TCC was found to be within ±15%, satisfying the X8R specification, and the sintering temperature was also found to be relatively low. Therefore, the appropriate content range of the third auxiliary component Y can be said to be 2 mol parts or less in element ratio with respect to 100 mol parts of the main component of the parent material.

[0082] The present invention is not limited to the embodiments described above and the accompanying drawings, but is defined by the appended claims. Therefore, it will be apparent to those skilled in the art that various substitutions, modifications, and alterations are possible within the scope of the technical spirit of the present invention as defined in the claims, and such modifications also fall within the scope of the appended claims.

Claims

1. In a dielectric composition containing a main component and a secondary component of a barium titanate-based material, The above auxiliary ingredients are, A first subcomponent comprising at least one selected from the group consisting of oxides and carbonates of the element Yb; A second component comprising at least one selected from the group consisting of oxides comprising Ba and Zr; A third component comprising at least one selected from the group consisting of oxides and carbonates of element Y; A fourth minor component comprising at least one of an oxide and a carbonate of an atomic fixed acceptor element including Mg; A fifth secondary component comprising at least one selected from the group consisting of oxides and carbonates of variable acceptor elements, wherein the atomic number comprises at least one of V, Mn, Cr, Fe, Ni, Co, Cu, and Zn; and A sixth auxiliary component comprising at least one selected from the group consisting of oxides, carbonates and glasses of the Si element; comprising at least one auxiliary component; wherein said at least one subcomponent comprises said first subcomponent, The content of the Yb element included in the first auxiliary component is 0.2 to 6 molar parts per 100 molar parts of the main component of the parent material. Genetic composition.

2. In paragraph 1, wherein said at least one subcomponent further comprises said second subcomponent, The content of the second auxiliary component is 0.1 to 3 mol parts per 100 mol parts of the main component of the parent material. Genetic composition.

3. In paragraph 1, wherein said at least one subcomponent further comprises said third subcomponent, The content of the Y element included in the above third auxiliary component is 2 mol parts or less per 100 mol parts of the main component of the parent material. Genetic composition.

4. In paragraph 1, wherein said at least one subcomponent further comprises said fourth subcomponent, The content of the Mg element included in the fourth auxiliary component is 0.1 to 2 molar parts per 100 molar parts of the main component of the parent material. Genetic composition.

5. In paragraph 1, wherein said at least one subcomponent further comprises said fifth subcomponent, The content of the variable valence acceptor element included in the fifth auxiliary component is 0.03 to 4 mol parts per 100 mol parts of the parent material main component. Genetic composition.

6. In paragraph 1, wherein said at least one subcomponent further comprises said sixth subcomponent, The content of the above sixth auxiliary component is 0.1 to 5 mol parts per 100 mol parts of the main component of the above-mentioned parent material. Genetic composition.

7. In paragraph 6, The above sixth component is Ba x Ca 1-x Comprising a complex oxide represented by SiO3 (wherein x is 0.3 to 0.8), Genetic composition.

8. In a method for producing a genetic composition, Step for preparing the main component of barium titanate-based base material; A step of preparing at least one subcomponent including the first subcomponent, which includes at least one selected from the group consisting of oxides and carbonates of Yb element, a second subcomponent including at least one selected from the group consisting of oxides including Ba and Zr, a third subcomponent including at least one selected from the group consisting of oxides and carbonates of Y element, a fourth subcomponent including at least one selected from oxides and carbonates of a valence-fixed acceptor element including Mg, a fifth subcomponent including at least one selected from the group consisting of oxides and carbonates of a valence-variable acceptor element including at least one selected from the group consisting of oxides and carbonates of Si element, and a sixth subcomponent including at least one selected from the group consisting of oxides, carbonates and glasses of Si element; A step of preparing a mixture comprising the above main component and at least one auxiliary component; and Comprising a step of calcining the above mixture, The content of the Yb element included in the first auxiliary component is 0.2 to 6 molar parts per 100 molar parts of the main component of the parent material. Method for producing a dielectric composition.

9. In paragraph 8, The sintering temperature of the above mixture is 1150℃ or higher. Method for producing a dielectric composition.

Citation Information

Patent Citations

  • Method for manufacturing irreducible dielectric ceramic, irreducible dielectric ceramic, and laminated ceramic capacitor

    JP2004345927A

  • Dielectric ceramic and capacitor

    JP2013049587A

  • Ceramic capacitor dielectric material

    JP2017024969A

  • multilayer ceramic component and method for manufacturing same

    KR1020080052691A

  • Low temperature sintering dielectric composition and multilayer cderamic capacitor

    KR1020160073121A