High-strength aluminum-zinc-magnesium-copper alloy thick plate and method for producing same
The multi-stage homogenization and reheating process for aluminum-zinc-magnesium-copper alloy plates addresses the challenge of achieving high mechanical properties and cost-effective hot rolling at room temperature, resulting in plates with enhanced strength and elongation, and reduced secondary phase fractions.
Patent Information
- Application Number
- PCT/KR2024/005456
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-31
AI Technical Summary
The challenge is to manufacture high-strength aluminum-zinc-magnesium-copper alloy thick plates with improved mechanical properties by reducing secondary phase fractions and enabling hot rolling at room temperature, while avoiding casting defects and high heating costs associated with traditional hot rolling methods.
A multi-stage homogenization treatment process followed by reheating within a specific temperature range, allowing for hot rolling using rolls at room temperature, which minimizes secondary phase formation and enhances mechanical properties through controlled heat treatment and composition optimization.
The method produces high-strength aluminum-zinc-magnesium-copper alloy plates with yield strength of 450 MPa or more, tensile strength of 520 MPa or more, and elongation of 10% or more, while reducing the fraction of secondary phases and enabling cost-effective hot rolling without thermal shock damage.
Smart Images

Figure KR2024005456_31102024_PF_FP_ABST
Abstract
Description
High-strength aluminum-zinc-magnesium-copper alloy thick plate and its manufacturing method
[0001] The technical idea of the present invention relates to a method for manufacturing an aluminum alloy, and more specifically, to a high-strength aluminum-zinc-magnesium-copper alloy thick plate and a method for manufacturing the same.
[0002] Recently, the global trend toward lighter transportation components to improve fuel efficiency has led to a growing demand for lightweight and high-strength materials. Among these, the use of aluminum alloys is rapidly increasing due to their excellent castability, processability, mechanical properties, durability, and recyclability. In particular, 7000 series aluminum alloys, which contain zinc and magnesium as major alloying elements, have been primarily used as aircraft materials. However, due to their high mechanical properties, their application is expanding to automobiles, electronic device cases, and leisure goods.
[0003] However, while 7000 series aluminum alloys increase in strength as the content of additive elements such as zinc, magnesium, and copper increases, the fraction of secondary phases within the cast material increases, making casting defects more likely to occur, and these secondary phases degrade mechanical properties. Therefore, there is a growing demand for thick plates with superior mechanical properties, which feature a reduced fraction of secondary phases and fine grain size.
[0004] Furthermore, hot rolling of mass-produced 7000 series aluminum alloy slabs is typically performed using hot rolling rolls heated to high temperatures. However, heating hot rolling rolls is expensive when producing small quantities of 7000 series aluminum alloy slabs. Therefore, a technology is needed to manufacture aluminum alloy thick plates by hot rolling 7000 series aluminum alloy slabs at room temperature without heating the hot rolling rolls.
[0005] <Prior Art Document> Korean Patent No. 10-0933385
[0006] The technical problem to be achieved by the technical idea of the present invention is to provide a high-strength aluminum-zinc-magnesium-copper alloy thick plate and a method for manufacturing the same, which can perform hot rolling using a hot rolling roll at room temperature, and improve mechanical properties by preventing defects by reducing the secondary phase fraction.
[0007] However, these tasks are exemplary and the technical idea of the present invention is not limited thereto.
[0008] According to one aspect of the present invention, a high-strength aluminum-zinc-magnesium-copper alloy thick plate and a method for manufacturing the same are provided.
[0009] According to one embodiment of the present invention, the method for manufacturing the high-strength aluminum-zinc-magnesium-copper alloy thick plate may include a casting step of melting alloy elements corresponding to an aluminum alloy including 5 wt% to 8 wt% of zinc (Zn), 2 wt% to 3 wt% of magnesium (Mg), 1 wt% to 2 wt% of copper (Cu), and the remainder being aluminum (Al) and other unavoidable impurities, casting the molten metal to form an aluminum alloy cast material; a multi-stage homogenization step of performing a multi-stage homogenization treatment on the aluminum alloy cast material to form an aluminum alloy homogenized material; a reheating step of heating the aluminum alloy homogenized material to a temperature in the range of 300°C to 400°C; and a hot rolling step of hot-rolling the reheated aluminum alloy homogenized material to form an aluminum alloy thick plate.
[0010] According to one embodiment of the present invention, the multi-stage homogenization treatment step may include a step of first homogenizing the aluminum alloy cast material at a temperature ranging from 450°C to 475°C for more than 6 hours but less than 24 hours; and a step of second homogenizing the aluminum alloy cast material subjected to the first homogenization treatment at a temperature ranging from 470°C to 490°C for 1 hour but less than 4 hours.
[0011] According to one embodiment of the present invention, the temperature of the second homogenization treatment step may be higher than the temperature of the first homogenization treatment step.
[0012] According to one embodiment of the present invention, the hot rolling step can be performed using a hot rolling roll at room temperature.
[0013] According to one embodiment of the present invention, the method may further include a solution treatment step of solution treating the aluminum alloy thick plate at a temperature ranging from 420°C to 500°C for 30 minutes to 5 hours.
[0014] According to one embodiment of the present invention, the method may further include an aging treatment step of aging the aluminum alloy thick plate at a temperature ranging from 100°C to 200°C for 5 to 30 hours.
[0015] According to one embodiment of the present invention, the method may further include a solution treatment step of solution treatment of the aluminum alloy thick plate at a temperature ranging from 420°C to 500°C for 30 minutes to 5 hours; and an aging treatment step of aging the aluminum alloy thick plate at a temperature ranging from 100°C to 200°C for 5 hours to 30 hours.
[0016] According to one embodiment of the present invention, the aluminum alloy may further include at least one of 0.3 wt% or less of chromium (Cr), 0.1 wt% or less of titanium (Ti), and 0.1 wt% or less of zirconium (Zr).
[0017] According to one embodiment of the present invention, the aluminum alloy casting material may have an average grain size in the range of 50 μm to 80 μm.
[0018] According to one embodiment of the present invention, the aluminum alloy casting material may have a thickness in a range of 120 mm to 200 mm, and the aluminum alloy thick plate may have a thickness in a range of 25 mm to 40 mm.
[0019] According to one embodiment of the present invention, the high-strength aluminum-zinc-magnesium-copper alloy thick plate contains 5 wt% to 8 wt% of zinc (Zn), 2 wt% to 3 wt% of magnesium (Mg), 1 wt% to 2 wt% of copper (Cu), and the remainder being aluminum (Al) and other unavoidable impurities, and the aluminum-zinc-magnesium-copper alloy thick plate can satisfy a yield strength (YS): 450 MPa or more, a tensile strength (UTS): 520 MPa or more, and an elongation (EL): 10% or more.
[0020] According to one embodiment of the present invention, the aluminum-zinc-magnesium-copper alloy thick plate may have a recrystallized fraction of 50% to 80% by volume.
[0021] According to one embodiment of the present invention, the aluminum-zinc-magnesium-copper alloy thick plate may further include at least one of 0.3 wt% or less of chromium (Cr), 0.1 wt% or less of titanium (Ti), and 0.1 wt% or less of zirconium (Zr).
[0022] According to the technical idea of the present invention, a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate can provide a high-strength aluminum-zinc-magnesium-copper alloy thick plate having excellent mechanical properties by minimizing the fraction of compounds present in a cast material through a multi-stage homogenization treatment, thereby improving the mechanical properties of the thick plate, and controlling the reheating heat treatment temperature to suppress breakage occurring during rolling for hot rolling using a roll at room temperature.
[0023] The effects of the present invention described above are illustrative, and the scope of the present invention is not limited by these effects.
[0024] FIG. 1 is a process flow diagram schematically showing a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to one embodiment of the present invention.
[0025] FIG. 2 is a schematic diagram showing changes in process time and process temperature in a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to one embodiment of the present invention.
[0026] FIGS. 3a to 3c are graphs showing thermodynamic calculation results for aluminum alloy design in a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to one embodiment of the present invention.
[0027] FIG. 4 is an optical microscope photograph showing the microstructure of an aluminum alloy casting manufactured according to a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0028] FIGS. 5a and 5b are differential scanning calorimetry graphs of an aluminum alloy manufactured according to a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0029] FIGS. 6 and 7 are optical microscope photographs showing changes in the microstructure of an aluminum alloy manufactured according to a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention, depending on the homogenization time.
[0030] FIGS. 8a and 8b are graphs showing the compound fraction according to the homogenization time of an aluminum alloy manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0031] FIGS. 9a and 9b are graphs showing the hardness according to the homogenization time of an aluminum alloy manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0032] FIG. 10 is a photograph showing the results of hot rolling according to the reheating temperature of an aluminum alloy manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0033] FIGS. 11a, 11b, and 11c are scanning electron microscope photographs showing cross-sections of aluminum alloy plates manufactured using a method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy plates according to one embodiment of the present invention.
[0034] FIG. 12 is a graph showing the strength and elongation of an aluminum alloy thick plate manufactured using a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0035] FIG. 13 is a graph showing the fatigue characteristics of an aluminum alloy thick plate manufactured using a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0036] FIG. 14 is a graph showing the fracture toughness of an aluminum alloy thick plate manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0037] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. Embodiments of the present invention are provided to more completely explain the technical idea of the present invention to those skilled in the art. The following embodiments may be modified in various different forms, and the scope of the technical idea of the present invention is not limited to the following embodiments. Rather, these embodiments are provided to more faithfully and completely convey the technical idea of the present invention to those skilled in the art. Like reference numerals throughout this specification denote like elements. Furthermore, various elements and areas in the drawings are schematically drawn. Therefore, the technical idea of the present invention is not limited by the relative sizes or intervals drawn in the attached drawings.
[0038] It should be noted that, in this specification, the term "alloy element" is used to refer to other elements added intentionally or unintentionally, excluding aluminum, to an aluminum-zinc-magnesium-copper alloy thick plate. In addition, it should be noted that the term "compound" described herein refers to all types of compounds that are not dissolved in the aluminum matrix but are formed as precipitates or crystallized phases at grain boundaries or within grains, and includes secondary phases commonly referred to in aluminum alloys.
[0039] The technical idea of the present invention is to provide a high-strength aluminum-zinc-magnesium-copper alloy thick plate with excellent mechanical properties and a method for manufacturing the same by enabling hot rolling using a rolling roll at room temperature by controlling the composition range and optimizing the multi-stage homogenization heat treatment and reheating temperature.
[0040] Hereinafter, a high-strength aluminum-zinc-magnesium-copper alloy thick plate, which is one aspect of the present invention, will be described.
[0041] High-strength aluminum-zinc-magnesium-copper alloy thick plate
[0042] A high-strength aluminum-zinc-magnesium-copper alloy thick plate, which is one aspect of the present invention, contains 5 wt% to 8 wt% of zinc (Zn), 2 wt% to 3 wt% of magnesium (Mg), 1 wt% to 2 wt% of copper (Cu), and the remainder being aluminum (Al) and other unavoidable impurities.
[0043] The high-strength aluminum-zinc-magnesium-copper alloy thick plate may further comprise at least one of 0.3 wt% or less of chromium (Cr), 0.1 wt% or less of titanium (Ti), and 0.1 wt% or less of zirconium (Zr). For example, the high-strength aluminum-zinc-magnesium-copper alloy thick plate may further comprise at least one of 0.01 wt% to 0.3 wt% of chromium (Cr), 0.01 wt% to 0.1 wt% of titanium (Ti), and 0.01 wt% to 0.1 wt% of zirconium (Zr).
[0044] Hereinafter, the role and content of each component included in the high-strength aluminum-zinc-magnesium-copper alloy thick plate according to the present invention will be described. Here, the content of the component elements all refers to weight%.
[0045] Zinc (Zn): 5 wt% to 8 wt%
[0046] Zinc is an element that enhances the strength of aluminum-zinc-magnesium-copper alloy plates. When the zinc content is less than 5 wt%, it can be difficult to secure strength. When the zinc content exceeds 8 wt%, the fluidity of the molten metal decreases, resulting in poor castability. Furthermore, segregation can occur in the center of the alloy plate, degrading its mechanical properties. Therefore, zinc is preferably added at 5 to 8 wt% of the total plate weight.
[0047] Magnesium (Mg): 2 wt% to 3 wt%
[0048] Magnesium is a solid-solution strengthening element that, when incorporated into the matrix of aluminum-zinc-magnesium-copper alloy plates, enhances strength and formability. When the magnesium content is less than 2 wt%, it can be difficult to secure strength and improve formability. When the magnesium content exceeds 3 wt%, elongation is significantly reduced, potentially leading to cracking. Therefore, magnesium is preferably added at 2 to 3 wt% of the total plate weight.
[0049] Copper (Cu): 1 wt% to 2 wt%
[0050] Copper is an element that improves the strength and formability of aluminum-zinc-magnesium-copper alloy plates. When the copper content is less than 1 wt%, it can be difficult to secure strength and improve formability. When the copper content exceeds 2 wt%, cracks can form due to segregation during casting. Therefore, it is preferable to add copper at 1 to 2 wt% of the total plate weight.
[0051] Chromium (Cr): 0.3 wt% or less
[0052] Chromium has the effect of suppressing recrystallization and thus refining grains, and can be added as a refiner, for example, in the form of an aluminum master alloy containing chromium, but is not limited to the above-mentioned refiner. When the chromium content is less than 0.01 wt%, the grain refinement effect may not be present. When the chromium content exceeds 0.3 wt%, coarse intermetallic compounds may be formed, which may reduce ductility. Therefore, it is preferable that chromium be added in an amount of 0.5 wt% or less, for example, 0.01 wt% to 0.3 wt%, of the total weight of the thick plate.
[0053] Titanium (Ti): 0.1 wt% or less
[0054] Titanium has the effect of suppressing recrystallization and refining grains, and can be added as a refining agent containing titanium, for example, an aluminum master alloy containing titanium, for example, Al-5Ti-1B, which is an Al-Ti-B grain refining agent, but is not limited to the above-mentioned refining agents. When the titanium content is less than 0.01 wt%, the grain refining effect may not be effective. When the titanium content exceeds 0.1 wt%, coarse intermetallic compounds may be formed, which may reduce ductility. Therefore, titanium is preferably added in an amount of 0.1 wt% or less of the total weight of the thick plate, for example, 0.01 wt% to 0.1 wt%.
[0055] Zirconium (Zr): 0.1 wt% or less
[0056] Zirconium has the effect of suppressing recrystallization and refining grains, and can be added as a refiner, for example, in the form of an aluminum master alloy containing zirconium, but is not limited to the above-mentioned refiner. When the zirconium content is less than 0.01 wt%, the grain refinement effect may not be effective. When the zirconium content exceeds 0.1 wt%, coarse intermetallic compounds may be formed, which may reduce ductility. Therefore, zirconium is preferably added in an amount of 0.1 wt% or less, for example, 0.01 wt% to 0.1 wt%, of the total weight of the thick plate.
[0057] The remaining component of the above aluminum-zinc-magnesium-copper alloy plate is aluminum (Al). However, during the typical manufacturing process, unintended impurities from raw materials or the surrounding environment can inevitably be mixed in, and thus cannot be excluded. Since these impurities are readily apparent to anyone skilled in the art of typical manufacturing, their full content is not specifically discussed in this specification.
[0058] However, the technical idea of the present invention is not limited to the composition of the alloy, and can comprehensively include alloy compositions that can be used as 7000 series aluminum alloy thick plates, such as 7075 series, 7050 series, and 7068 series.
[0059] The high-strength aluminum-zinc-magnesium-copper alloy thick plate manufactured by controlling the specific components of the alloy composition described above and the content range thereof through the manufacturing method described below can have its mechanical properties varied through subsequent hot rolling and heat treatment.
[0060] The above high-strength aluminum-zinc-magnesium-copper alloy thick plate can satisfy, for example, a yield strength (YS): 450 MPa or more, a tensile strength (UTS): 520 MPa or more, and an elongation (EL): 10% or more, and can satisfy, for example, a yield strength (YS): 450 MPa to 650 MPa, a tensile strength (UTS): 520 MPa to 720 MPa, and an elongation (EL): 10% to 16%.
[0061] The above high-strength aluminum-zinc-magnesium-copper alloy thick plate may have a recrystallized fraction of 50 to 80 volume%. The recrystallized fraction may be reduced by the addition of chromium (Cr), zirconium (Zr), etc. It may also be changed by the reduction ratio during hot rolling.
[0062] Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plates
[0063] Below, a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate is described in detail.
[0064] FIG. 1 is a process flow diagram schematically showing a method (S100) for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to one embodiment of the present invention.
[0065] FIG. 2 is a schematic diagram showing changes in process time and process temperature in a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to one embodiment of the present invention.
[0066] Referring to FIGS. 1 and 2, the method for manufacturing the high-strength aluminum-zinc-magnesium-copper alloy thick plate (S100) includes a casting step (S110); a multi-stage homogenization treatment step (S120); a reheating step (S130); a hot rolling step (S140); a solution treatment step (S150); and an aging treatment step (S160).
[0067] The above casting step (S110) is a step of casting after melting the alloy elements constituting the aluminum-zinc-magnesium-copper alloy plate to form a molten metal.
[0068] In the casting step (S110), for example, alloying elements corresponding to an aluminum alloy including 5 wt% to 8 wt% of zinc (Zn), 2 wt% to 3 wt% of magnesium (Mg), 1 wt% to 2 wt% of copper (Cu), and the remainder including aluminum (Al) and other unavoidable impurities may be melted to form a molten metal. In addition, the molten metal may further include at least one of 0.3 wt% or less of chromium (Cr), 0.1 wt% or less of titanium (Ti), and 0.1 wt% or less of zirconium (Zr).
[0069] The above alloying elements can be melted in a graphite crucible using a high-frequency induction melting furnace at a temperature at which the alloying elements are completely melted. This can be done by adding the alloying elements individually, or by adding all or part of the alloying elements in the form of a master alloy. For example, zinc can be added to the aluminum molten metal in its pure elemental state, or in the form of an aluminum-zinc master alloy with a high zinc content. This method can also be applied to other additive elements such as magnesium and copper.
[0070] The above molten metal can be poured into a slab mold and solidified to form an aluminum alloy casting. The aluminum alloy casting can be produced using a DC (direct chilled) continuous casting method, but this is exemplary and the technical concept of the present invention is not limited thereto.
[0071] The above aluminum alloy casting material can be cooled to room temperature in the air. However, this is merely exemplary, and the technical concept of the present invention also includes a case where a subsequent multi-stage homogenization treatment is continuously performed immediately after casting without cooling in the air.
[0072] The above aluminum alloy casting material may have a grain size of 150 μm or less and an average grain size in the range of 50 μm to 80 μm.
[0073] The multi-stage homogenization treatment step (S120) is a step of heating and homogenizing the aluminum alloy cast material to form an aluminum alloy homogenized material. The multi-stage homogenization treatment step (S120) may include a first homogenization treatment step and a second homogenization treatment step.
[0074] In the first homogenization treatment step, the aluminum alloy casting material may be subjected to the first homogenization treatment at a temperature ranging from 450°C to 475°C for more than 6 hours but less than 24 hours. The first homogenization treatment step may be performed for, for example, 9 hours to 12 hours.
[0075] In the second homogenization treatment step, the aluminum alloy casting material that has been subjected to the first homogenization treatment can be subjected to the second homogenization treatment at a temperature ranging from 470°C to 490°C for 1 hour to less than 4 hours. The temperature of the second homogenization treatment step is preferably higher than the temperature of the first homogenization treatment step.
[0076] For example, the first homogenization treatment step may be performed at a temperature of 460°C for 12 hours, and the second homogenization treatment step may be performed at a temperature of 475°C for 2 hours.
[0077] The above homogenization treatment achieves homogenization of the internal structure of the aluminum alloy, and in particular, compounds precipitated during the casting process can be re-incorporated into the aluminum matrix. Furthermore, by performing the above homogenization treatment in multiple stages, the overall time required for the homogenization treatment can be reduced.
[0078] Next, the aluminum alloy homogenized material formed by the above homogenization treatment can be air-cooled to room temperature.
[0079] Optionally, the aluminum alloy homogenizer can be ground to remove surface defects, thereby preventing the occurrence of defects in subsequent hot rolling.
[0080] The above reheating step (S130) is a step of reheating the aluminum alloy homogenized material for hot rolling. The above reheating step (S130) can be performed by heating the aluminum alloy homogenized material and maintaining it at a temperature in the range of 300°C to 400°C for 1 to 4 hours, and for example, can be performed by maintaining it for about 2 hours.
[0081] Conventional hot rolling of aluminum alloys uses hot rolling rolls heated to 200°C or higher, but the present invention has the technical feature of using hot rolling rolls at room temperature. In order to use hot rolling rolls at room temperature like this, the reheating temperature is important. If the reheating temperature is lower than 300°C, the load applied to the hot rolling roll increases, making hot rolling impossible. If the reheating temperature is higher than 400°C, the thermal shock caused by the temperature difference between the aluminum alloy homogenizer and the hot rolling roll may be too large, causing the rolled material to be destroyed during hot rolling.
[0082] The above hot rolling step (S140) is a step of forming an aluminum alloy thick plate by hot rolling the reheated aluminum alloy homogenized material at a temperature ranging from 300°C to 400°C.
[0083] The above hot rolling can be performed using a pair of hot rolling rolls that rotate at a speed of 50 m / min to 70 m / min and have a temperature in the range of room temperature, for example, 0°C to 40°C. When the speed of the hot rolling rolls is less than 50 m / min, it may be difficult to generate shear deformation, which helps improve the formability of the thick plate by applying rolling deformation to the entire thick plate. When the speed of the hot rolling rolls exceeds 70 m / min, deformation may not be induced to the center of the thick plate.
[0084] The above hot rolling can be performed at a reduction ratio ranging from 4% to less than 10%, and can be performed at an average reduction ratio of 7%. When the reduction ratio is less than 4%, the process time and cost may increase because a large number of repeated rollings must be performed. When the reduction ratio is 10% or more, significant cracks may occur in the thick plate, which may deteriorate the surface quality and mechanical properties. The above hot rolling can be performed repeatedly until the desired thickness is obtained.
[0085] The aluminum alloy casting material or the aluminum alloy homogenized material before performing hot rolling may have a thickness in the range of 120 mm to 200 mm (120T to 200T), and the aluminum alloy thick plate formed by performing hot rolling may have a thickness in the range of 25 mm to 40 mm (25T to 40T).
[0086] After performing the above hot rolling step (S140), the aluminum alloy thick plate can be cooled to room temperature by air cooling, for example, to a temperature in the range of 0°C to 40°C.
[0087] In the above-described solution treatment step (S150), the hot-rolled aluminum alloy thick plate is solution treated. The above-described solution treatment step (S150) can be performed by heating the aluminum alloy thick plate and maintaining it at a temperature in the range of, for example, 420°C to 500°C for 30 minutes to 5 hours, and can be performed at, for example, 470°C for 1 hour.
[0088] After performing the above solution treatment step (S150), water cooling quenching may be performed so that the aluminum alloy thick plate can be cooled to room temperature, for example, to a temperature in the range of 0°C to 40°C. By performing the solution treatment, the product phase formed by hot rolling can be decomposed, and the compositional uniformity of the aluminum matrix can be improved. After performing the solution treatment, water cooling quenching may be performed so that the aluminum alloy thick plate can be cooled to room temperature, for example, to a temperature in the range of 0°C to 40°C.
[0089] In the aging treatment step (S160), the solution-treated aluminum alloy thick plate is subjected to aging treatment. The aging treatment step (S160) may be performed by heating the aluminum alloy thick plate and maintaining it at a temperature ranging from 100°C to 200°C for 5 to 30 hours, for example, or at 120°C for 24 hours.
[0090] After performing the above aging treatment, water-cooling quenching may be performed so that the aluminum alloy thick plate may be cooled to room temperature, for example, to a temperature in the range of 0°C to 40°C. Through the aging treatment, solute elements may be extracted from the supersaturated solid solution to form an aging precipitate phase. After performing the above aging treatment, water-cooling quenching may be performed so that the aluminum alloy thick plate may be cooled to room temperature, for example, to a temperature in the range of 0°C to 40°C.
[0091] The above solution treatment step (S150) and the aging treatment step (S160) may be performed sequentially. Alternatively, only the solution treatment step (S150) may be performed, or only the aging treatment step (S160) may be performed.
[0092] Experimental example
[0093] Below, experimental examples of high-strength aluminum-zinc-magnesium-copper alloy thick plates according to the technical concept of the present invention will be described in detail. The following experimental examples serve as examples for explaining the technical concept of the present invention, and the present invention is not limited to the experimental examples described below.
[0094] Table 1 shows the alloy composition of an aluminum alloy manufactured according to a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to one embodiment of the present invention. The alloy composition in Table 1 refers to weight percent, and the remainder includes aluminum (Al) and inevitable impurities.
[0095] Classification Target Composition ZnMgCuCrTiZrFeSi Casting Material Al-5.6Zn-2.5Mg-1.5Cu5.5 2.40 1.40 0.14 0.02 50.05 0.09 0.02 1st Homogenized Fire Material Al-5.6Zn-2.5Mg-1.5Cu5.5 2.40 1.40 0.14 0.02 50.05 0.09 0.02 Example 1 Al-5.6Zn-2 .5Mg-1.5Cu5.552.401.400.140.0250.050.090.02Example 2Al-6.2Zn-2.5Mg-1.5Cu6.202.401.450.190.02500.100.02Example 3Al-7.8Zn-2.5Mg-1.5Cu7.852.551.400.180.02000.090.015
[0096] Table 1 shows the target composition and actual composition of aluminum alloys. The target composition, for example, "Al-5.6Zn-2.5Mg-1.5Cu" means that the alloy contains 5.6 wt% zinc, 2.5 wt% magnesium, and 1.5 wt% copper, with the remainder being aluminum.
[0097] Additionally, Table 1 shows the contents of chromium (Cr), titanium (Ti), and zirconium (Zr) added as refiners. Furthermore, the contents of iron (Fe) and silicon (Si), which were added as unavoidable impurities rather than intentionally, are indicated by underlining.
[0098] The ratio of zinc to magnesium (Zn / Mg) was 2.24 for the cast material, the first homogenizer, and Example 1, 2.48 for Example 2, and 3.12 for Example 3.
[0099] Aluminum alloy castings were manufactured by performing DC continuous casting on the aluminum alloys in Table 1. The castings had dimensions of 350 mm in width, 150 mm in thickness, and 600 mm in length.
[0100] Figures 3a to 3c are graphs showing thermodynamic calculation results for aluminum alloy design in a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to one embodiment of the present invention. Figure 3a is for Example 1, Figure 3b is for Example 2, and Figure 3c is for Example 3.
[0101] Referring to Figures 3a to 3c, the change in phase formed according to temperature when the zinc content is changed is shown. It can be seen that the compound mainly formed in the aluminum alloy is the MgZn2 phase. In addition, Al3Mg2 phase, Al 13 Cr2 phase, and T-(Mg 32 (Al, Zn) 49 ) are formed. According to thermodynamic calculations, as the zinc content increases, the fraction of the total compound formed within the aluminum alloy increases from 6.3 vol% to 7.5 vol%.
[0102] Next, the aluminum alloy casting material was homogenized. The conditions for the homogenization process will be described in detail below.
[0103] Table 2 shows the homogenization treatment conditions of an aluminum alloy manufactured according to a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to one embodiment of the present invention.
[0104] Classification 1st homogenization treatment 2nd homogenization treatment Casting material Not provided Not provided 1st homogenization material 460℃, 12 hours Not provided Example 1 460℃, 12 hours 475℃, 2 hours Example 2 460℃, 12 hours 475℃, 2 hours Example 3 460℃, 12 hours 475℃, 2 hours
[0105] FIG. 4 is an optical microscope photograph showing the microstructure of an aluminum alloy casting manufactured according to a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0106] Referring to Fig. 4, the aluminum alloy casting material had a grain size of about 150 μm or less and a microstructure with an average grain size in the range of 50 μm to 80 μm. In addition, the aluminum alloy casting material had a compound fraction in the range of 3.2% to 3.6% by volume, about 3.4% by volume (vol%).
[0107] When the aluminum alloy casting material is homogenized, partial melting may occur at high temperatures. It is desirable to prevent such partial melting and minimize the fraction of compounds formed by precipitation or crystallization. Since such partial melting is an endothermic reaction, a peak appears in a differential scanning calorimetry (DSC) graph, and thus the homogenization temperature that prevents partial melting can be determined.
[0108] FIGS. 5a and 5b are differential scanning calorimetry graphs of an aluminum alloy manufactured according to a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0109] Referring to Fig. 5a, in the aluminum alloy casting, the starting temperature of the peak indicating partial melting was approximately 477.7°C, the peak temperature was approximately 481.2°C, and the ending temperature was approximately 491.0°C. In addition, it is necessary to consider that the internal temperature deviation of the homogenization treatment furnace is approximately 15°C. Accordingly, since the first homogenization treatment must be controlled below the starting temperature at which the peak begins due to partial melting, approximately 460°C is analyzed as the preferable temperature.
[0110] According to these results, the aluminum alloy casting material was subjected to primary homogenization at 460°C for 12 hours to produce the aluminum alloy primary homogenized material.
[0111] Referring to Fig. 5b, in the aluminum alloy primary homogenization material, the starting temperature of the peak indicating partial melting was approximately 492.8°C, the peak temperature was approximately 499.6°C, and the ending temperature was approximately 503.2°C. In addition, it is necessary to consider that the internal temperature deviation of the homogenization treatment furnace is approximately 15°C. Accordingly, since the secondary homogenization treatment must be controlled below the starting temperature at which the peak begins due to partial melting, approximately 475°C is analyzed as the preferable temperature.
[0112] According to these results, the aluminum alloy primary homogenizer was subjected to secondary homogenization at 475°C for 2 hours to produce an aluminum alloy secondary homogenizer.
[0113] The reason why the peak start temperature of the aluminum alloy primary homogenization material is higher than that of the aluminum alloy casting material is that some of the compounds that cause partial melting are dissolved into the aluminum matrix through the primary homogenization treatment, and thus the content of the compounds is lowered, which is analyzed to be the reason why the start temperature at which partial melting occurs increases.
[0114] The above aluminum alloy secondary homogenizer corresponds to Example 1, and a two-stage multi-stage homogenization treatment was performed. In addition, Examples 2 and 3 differ from Example 1 only in alloy composition, and the homogenization treatment was manufactured by a multi-stage homogenization treatment at the same temperature and time.
[0115] Below, the optimization of the multi-stage homogenization treatment time will be described in detail.
[0116] FIGS. 6 and 7 are optical microscope photographs showing changes in the microstructure of an aluminum alloy manufactured according to a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention, depending on the homogenization time.
[0117] Referring to Fig. 6, the microstructure of the aluminum alloy cast material subjected to the first homogenization treatment at 460°C for varying times of 6 to 48 hours is shown. The aluminum alloy cast material had a compound fraction of approximately 3.4 vol% immediately after casting. As the first homogenization treatment time of the aluminum alloy cast material increased, the compound fraction continued to decrease until 36 hours, while the compound fraction increased again at 48 hours. The compound present at the grain boundary indicated by the white arrow was found when the aluminum alloy cast material was homogenized for 6 hours, but was not found when the homogenization treatment was performed for 12 hours or longer. Therefore, as a result of optimization considering minimizing the compound fraction and minimizing the homogenization treatment time, it is preferable to perform the first homogenization treatment at 460°C for 12 hours.
[0118] Here, the aluminum alloy primary homogenizer is a case where the primary homogenization treatment was performed at 460°C for 12 hours as shown in Fig. 6, and the compound fraction was found to be 1.18% by volume.
[0119] Referring to Fig. 7, the microstructure of the aluminum alloy primary homogenization material is shown when the secondary homogenization treatment is performed for a period of time ranging from 1 hour to 24 hours at 475°C. As the secondary homogenization treatment time of the aluminum alloy cast material increases, the compound fraction continues to decrease up to 24 hours. In particular, it can be seen that the secondary homogenization treatment time for the compound fraction to decrease to 1% by volume or less is 2 hours or more. Therefore, as an optimized result considering the minimization of the compound fraction and the minimization of the homogenization treatment time, it is preferable to perform the secondary homogenization treatment at 475°C for 2 hours.
[0120] When examining the change in the above compound fraction, the compound fraction was 3.42 vol% in the aluminum alloy cast material, and the compound fraction was reduced to 1.18 vol% in the aluminum alloy primary homogenized material subjected to the first homogenization treatment at 460°C for 12 hours, and the compound fraction was reduced to 0.84 vol% in the aluminum alloy primary homogenized material subjected to the second homogenization treatment at 475°C for 2 hours. Therefore, according to the present invention, the compound (secondary phase) fraction can be achieved to be less than 1 vol% in a short period of time.
[0121] Figures 8a and 8b are graphs showing the compound fraction according to the homogenization time of an aluminum alloy manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention. Figure 8a shows a case where the aluminum alloy cast material was first homogenized at 460°C, and Figure 8b shows a case where the aluminum alloy first homogenized material was secondarily homogenized at 475°C.
[0122] Referring to FIGS. 8a and 8b, the results of optimization considering minimizing the compound fraction and minimizing the homogenization treatment time are shown in which the first homogenization treatment was performed at 460°C for 12 hours and the second homogenization treatment was performed at 475°C for 2 hours. This is consistent with the results described above with reference to FIGS. 6 and 7.
[0123] Figures 9a and 9b are graphs showing the hardness according to the homogenization time of an aluminum alloy manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention. Figure 9a shows the case where the aluminum alloy cast material was first homogenized at 460°C, and Figure 9b shows the case where the aluminum alloy first homogenized material was secondarily homogenized at 475°C.
[0124] Table 3 is a table showing the hardness according to the homogenization time of an aluminum alloy manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0125] 1st homogenization treatment2nd homogenization treatmentTime (h)Hardness (Hv)Time (h)Hardness (Hv)095.84 ± 6.611151.24 ± 0.866139.98 ± 2.052153.01 ± 1.3012141.11 ± 1.774153.62 ± 1.1424142.72 ± 2.538154.27 ± 1.1436151.38 ± 1.6012154.30 ± 1.1548150.13 ± 1.7924155.05 ± 0.87
[0126] Referring to FIGS. 9a, 9b, and Table 3, when the aluminum alloy cast material was subjected to the first homogenization treatment at 460°C, the hardness increased rapidly from immediately after casting to 6 hours, and thereafter, the hardness was almost the same. In addition, when the aluminum alloy first homogenized material was subjected to the second homogenization treatment at 475°C, the hardness increased rapidly until 2 hours, and thereafter, the hardness increased gradually. As an optimized result considering such an increase in hardness and minimization of the homogenization treatment time, it can be seen that the first homogenization treatment was performed at 460°C for 12 hours, and the second homogenization treatment was performed at 475°C for 2 hours. This is consistent with the compound fraction results described above with reference to FIGS. 6 to 8.
[0127] Next, the aluminum alloy homogenized material subjected to secondary homogenization was reheated to various temperatures and then hot-rolled using a hot-rolling roll at room temperature to produce an aluminum alloy thick plate having a thickness of approximately 25 mm. Hereinafter, the hot-rolling condition settings will be described in detail.
[0128] FIG. 10 is a photograph showing the results of hot rolling according to the reheating temperature of an aluminum alloy manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0129] Referring to Fig. 10, the hot rolling results of the aluminum alloy secondary homogenizer of Example 1 are shown. The hot rolling was performed using a hot rolling roll at room temperature. When hot rolling was performed by reheating to 350°C and 400°C, the hot rolling of the aluminum alloy secondary homogenizer was successfully performed. On the other hand, when the reheating temperature was 460°C, the aluminum alloy secondary homogenizer was destroyed, making hot rolling impossible.
[0130] When the reheating temperature is 460°C, it is analyzed that the thermal shock caused by the temperature difference between the aluminum alloy secondary homogenizer and the hot rolling roll has a large effect, thereby destroying the aluminum alloy secondary homogenizer. On the other hand, it is analyzed that when the reheating temperature is reduced to 460°C or lower, the temperature difference between the aluminum alloy secondary homogenizer and the hot rolling roll is reduced, thereby reducing the effect of the thermal shock and enabling hot rolling.
[0131] Table 4 is a table showing the hot rolling results according to the reheating temperature of an aluminum alloy manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to one embodiment of the present invention.
[0132] Reheating temperature (℃) 320 340 360 380 400 460 Casting material OOOXXX 1st homogenization material OOOOXX Example 1 OOOOOX
[0133] Referring to Table 4, it can be seen that when hot rolling is performed using a hot rolling roll at room temperature for Example 1 in which secondary homogenization was performed, it is desirable to reheat to a range of 320°C to 400°C. On the other hand, the aluminum alloy primary homogenized material could not be hot rolled above 400°C, and the aluminum alloy cast material could not be hot rolled above 380°C. These results are analyzed to be because, as the homogenization treatment is performed, the fraction of compounds at the grain boundaries decreases and the mechanical properties increase, thereby increasing the resistance to thermal shock generated during hot rolling using a hot rolling roll at room temperature.
[0134] In industrial settings, minimizing the load on hot rolling rolls during hot rolling is crucial to prevent damage to rolling equipment, thus increasing the reheating temperature. To achieve this, multi-stage homogenization, which reduces the compound fraction, is analyzed as a way to reduce the load when hot rolling is performed using hot rolling rolls at room temperature.
[0135] Next, the hot-rolled aluminum alloy thick plates of Examples 1 to 3 were heated and subjected to a solution treatment at 470°C for 1 hour, water-cooled, and then heated again and aged at 120°C for 12 hours, i.e., the examples were subjected to a T6 heat treatment. In this way, the following mechanical properties were measured and microstructures were observed for the aluminum alloy thick plates that had undergone a solution treatment and an aging treatment.
[0136] Figures 11a, 11b, and 11c are scanning electron microscope photographs showing cross-sections of aluminum alloy thick plates manufactured by a method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plates according to one embodiment of the present invention. Figure 11a is for Example 1, Figure 11b is for Example 2, and Figure 11c is for Example 3. “RD” indicates the rolling direction, and “ND” indicates the direction perpendicular to the rolling direction, i.e., the thickness direction.
[0137] Referring to Figs. 11a, 11b, and 11c, the examples showed similar microstructures and did not show a clear tendency for changes in zinc content. The average grain size of the examples ranged from 46.8 μm to 49.1 μm, the kernel average misorientation (KAM) ranged from 1.14 to 1.21, and the recrystallized fraction ranged from 63 vol% to 66 vol%. Here, the recrystallized fraction was defined to include crystals having a GOS (grain orientation spread) value between 0 and 2 degrees when analyzed by EBSD (Electron Backscatter Diffraction).
[0138] FIG. 12 is a graph showing the strength and elongation of an aluminum alloy thick plate manufactured using a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0139] Table 5 is a table showing the strength and elongation of an aluminum alloy thick plate manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to one embodiment of the present invention.
[0140] Classification Yield strength (MPa) Tensile strength (MPa) Elongation (%) Example 1 500 ± 8.5 571 ± 2.7 14.2 ± 0.6 Example 2 545 ± 3.8 608 ± 3.5 13.3 ± 0.5 Example 3 591 ± 4.0 653 ± 2.0 13.1 ± 0.6
[0141] Referring to Fig. 12 and Table 5, the examples exhibited similar behavior in strength-elongation curves. As the zinc content of the examples increased, the yield strength and tensile strength increased, while the elongation tended to decrease.
[0142] FIG. 13 is a graph showing the fatigue characteristics of an aluminum alloy thick plate manufactured using a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0143] In Fig. 13, the fatigue test was performed at an R ratio of 0.1, a fatigue cycle frequency of 30 Hz, and room temperature (25°C). The fatigue stress was 10 7 It was defined as the stress acquired in the cycle. In the above fatigue experiment, 10 4 The time to cycle is 0.09 hours, 10 5 The time to cycle is 0.93 hours, 10 6 The time to cycle is 9.26 hours, and 10 7 The time taken to cycle was 92.59 hours.
[0144] Referring to Figure 13, the examples exhibited similar behavior in the cycle count-fatigue stress curves. In all cases, the maximum stress decreased as the fatigue cycle increased. The fatigue stress of Example 1 was lower than that of the other examples. The fatigue stress tended to increase as the zinc content increased.
[0145] FIG. 14 is a graph showing the fracture toughness of an aluminum alloy thick plate manufactured by a method for manufacturing a high-strength aluminum-zinc-magnesium-copper alloy thick plate according to an embodiment of the present invention.
[0146] Referring to Fig. 14, K Q In the case of Example 1, it is 28.1 MPa m 1 / 2 , in the case of Example 2, 26.7 MPa m 1 / 2 , in the case of Example 3, 23.0 MPa m 1 / 2 Therefore, it can be seen that as the zinc content increases, the fracture toughness of the aluminum alloy thick plate decreases.
[0147] It will be apparent to a person skilled in the art to which the technical idea of the present invention pertains that the technical idea of the present invention described above is not limited to the above-described embodiments and the attached drawings, and that various substitutions, modifications, and changes are possible within a scope that does not depart from the technical idea of the present invention.
Claims
A casting step of forming an aluminum alloy casting material by casting a molten metal formed by melting alloy elements corresponding to an aluminum alloy containing 1.5 to 8 wt% of zinc (Zn), 2 to 3 wt% of magnesium (Mg), 1 to 2 wt% of copper (Cu), and the remainder being aluminum (Al) and other unavoidable impurities; A multi-stage homogenization treatment step of forming an aluminum alloy homogenized material by performing a multi-stage homogenization treatment on the above aluminum alloy casting material; A reheating step of heating the above aluminum alloy homogenizer to a temperature in the range of 300°C to 400°C; and A hot rolling step of hot rolling the reheated aluminum alloy homogenized material to form an aluminum alloy thick plate, Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plate.
2. In paragraph 1, The above multi-stage homogenization treatment step is, A step of first homogenizing the aluminum alloy casting material at a temperature ranging from 450°C to 475°C for more than 6 hours but less than 24 hours; and A step of performing a second homogenization treatment on the aluminum alloy casting material subjected to the first homogenization treatment at a temperature ranging from 470°C to 490°C for 1 hour to less than 4 hours, Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plate.
3. In paragraph 2, The temperature of the above second homogenization treatment step is higher than the temperature of the above first homogenization treatment step. Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plate.
4. In paragraph 1, The above hot rolling step is, Performed using hot rolling rolls at room temperature, Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plate.
5. In paragraph 1, Further comprising a solution treatment step of solution treating the aluminum alloy thick plate at a temperature ranging from 420°C to 500°C for 30 minutes to 5 hours. Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plate.
6. In paragraph 1, Further comprising an aging treatment step of aging the aluminum alloy thick plate at a temperature ranging from 100°C to 200°C for 5 to 30 hours. Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plate.
7. In paragraph 1, A solution treatment step of solution treating the aluminum alloy plate at a temperature ranging from 420°C to 500°C for 30 minutes to 5 hours; and Further comprising an aging treatment step of aging the aluminum alloy thick plate at a temperature ranging from 100°C to 200°C for 5 to 30 hours. Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plate.
8. In paragraph 1, The above aluminum alloy, further comprising at least one of chromium (Cr) of 0.3 wt% or less, titanium (Ti) of 0.1 wt% or less, and zirconium (Zr) of 0.1 wt% or less. Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plate.
9. In paragraph 1, The above aluminum alloy casting material has an average grain size in the range of 50 μm to 80 μm. Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plate.
10. In paragraph 1, The above aluminum alloy casting material has a thickness ranging from 120 mm to 200 mm, The above aluminum alloy plate has a thickness ranging from 25 mm to 40 mm. Method for manufacturing high-strength aluminum-zinc-magnesium-copper alloy thick plate. Contains 11.5 to 8 wt% of zinc (Zn), 2 to 3 wt% of magnesium (Mg), 1 to 2 wt% of copper (Cu), and the remainder being aluminum (Al) and other unavoidable impurities. The above aluminum-zinc-magnesium-copper alloy thick plate satisfies the following: yield strength (YS): 450 MPa or more, tensile strength (UTS): 520 MPa or more, and elongation (EL): 10% or more. High-strength aluminum-zinc-magnesium-copper alloy thick plate.
12. In paragraph 11, The above aluminum-zinc-magnesium-copper alloy plate, Having a recrystallized fraction of 50 to 80 volume%, High-strength aluminum-zinc-magnesium-copper alloy thick plate.
13. In paragraph 11, The above aluminum-zinc-magnesium-copper alloy plate, further comprising at least one of chromium (Cr) of 0.3 wt% or less, titanium (Ti) of 0.1 wt% or less, and zirconium (Zr) of 0.1 wt% or less. High-strength aluminum-zinc-magnesium-copper alloy thick plate.
Citation Information
Patent Citations
Material for airplane stringer with fine crystal grain and its manufacture
JP1981090949A
High-strength, high-toughness al-zn alloy products and methods for making such products
JP2008516079A
Method for manufacturing of al-zn-mg-cu alloy sheet with refined crystal grains
KR1020150047246A
High-strength aluminum alloy plate with superior bake-hardenability and manufacturing method thereof
KR1020170132116A
Tension support for cargo binding belt
KR1020220127972A