Cathode active material, cathode, and lithium secondary battery

The development of high nickel cathode active materials with specific particle structures and compositions in lithium secondary batteries addresses structural deterioration and energy density issues, enhancing battery performance and lifespan by maintaining a stable layered structure.

WO2024225855A1PCT designated stage expired Publication Date: 2024-10-31LG CHEM LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005819
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-29
Filing Date
2024-04-29
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

High nickel cathode active materials in lithium secondary batteries suffer from structural deterioration and cracking during charging and discharging, leading to reduced lifespan and conductivity issues due to volume changes, and existing secondary particles with micron-level primary particles cannot be manufactured for high nickel content due to degradation of the layered structure into a rock salt structure at high heat treatment temperatures.

Method used

A high nickel cathode active material with secondary particles formed from aggregated disk-shaped primary particles of specific size and composition, including lithium, nickel, cobalt, and manganese, which maintains a layered structure even after high heat treatment, improving energy density and lifespan by controlling particle size and structure.

Benefits of technology

The solution enhances the energy density and lifespan of lithium secondary batteries by maintaining a stable layered structure in high nickel content cathode active materials, addressing the issues of structural deterioration and cracking, while also improving rolling density and cell characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005819_31102024_PF_FP_ABST
    Figure KR2024005819_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a cathode active material and, to a cathode active material, a cathode comprising same, and a lithium secondary battery, the cathode active material enabling problems of conventional secondary particles and problems of discrete particles to be solved simultaneously, and comprising: as primary particles, particles such as conventional discrete particles; and secondary particles formed by aggregating a plurality of primary particles, and thus the present invention has cell characteristics such as improved lifespan of a lithium secondary battery and reduced gas generation, and also has excellent density characteristics so as to have improved energy density.
Need to check novelty before this filing date? Find Prior Art

Description

Cathode active material, cathode, and lithium secondary battery

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-00656231, filed April 28, 2023, and Korean Patent Application No. 10-2024-0057122, filed April 29, 2024, the entire contents of which are incorporated herein by reference.

[0003] Technology field

[0004] The present invention relates to a positive electrode active material, a positive electrode including the same, and a lithium secondary battery.

[0005]

[0006] Recently, with the advancement of technology such as electric vehicles, the demand for high-capacity secondary batteries is increasing, and accordingly, research on high-nickel (High Ni) cathode active materials with excellent capacity characteristics is being actively conducted.

[0007] High-nickel cathode active materials, formed by a secondary particle structure composed of aggregated primary particles, undergo structural degradation during charging and discharging of lithium secondary batteries, but also experience relatively large changes in lattice structure constants, i.e., volume changes within the unit cell. These volume changes cause cracks within the cathode active material. Furthermore, cracks can also occur within the cathode active material due to pressure during electrode rolling.

[0008] The cracks in the high nickel positive electrode active material that occur in this way become more severe during the charging and discharging process of the lithium secondary battery, and as a result, they act as voids that cannot be reached by the electrolyte or reduce conductivity, which lowers the life characteristics of the lithium secondary battery or acts as a factor in increasing resistance.

[0009] To minimize cracking in these secondary particle structures, attempts have been made to manufacture single-particle cathode active materials. However, these single-particle cathode active materials suffer from the problem of non-uniform particle sizes, resulting in a large particle size distribution after milling. Furthermore, single-particle cathode active materials have a low specific surface area, making them vulnerable to cell resistance degradation.

[0010] Therefore, there is a need for the development of a cathode active material that can simultaneously solve the problems of conventional secondary particles and single particles.

[0011] Meanwhile, Korean Patent Publication No. 10-1785262 (Patent Document 1) discloses large-diameter secondary particles, which include secondary particles in which primary particles are aggregated, the secondary particles include a nickel-based lithium transition metal oxide, and the average particle size of the primary particles is 3 to 5 μm and the average particle size of the secondary particles is 10 to 20 μm. These large-diameter secondary particles include primary particles with an average particle size on the micron level, thereby improving the rolling density and minimizing cracks caused by rolling, etc., and improving cell characteristics by increasing the specific surface area through the secondary particle structure.

[0012] In order to manufacture a positive electrode active material in the form of secondary particles whose primary particles are on the micron level in size, as disclosed in Patent Document 1, it is necessary to perform heat treatment at a higher temperature than that of secondary particles whose primary particles are on the submicron level of less than 1 ㎛ in size. However, as the heat treatment temperature increases, the layered structure of the lithium-transition metal composite oxide degenerates into a rock salt structure, which causes a decrease in crystallinity and, in turn, a decrease in the performance of the positive electrode active material. In particular, since nickel is most vulnerable to the degeneration of the layered structure of the lithium-transition metal composite oxide into a rock salt structure at high heat treatment temperatures, the degeneration becomes more severe when the nickel content in the lithium-transition metal composite oxide constituting the positive electrode active material increases. Therefore, in the past, as a positive electrode active material in the form of secondary particles with a primary particle size of micron-level, it could only be applied to a mid-nickel (Mid Ni) positive electrode active material in which the content of nickel among the transition metals of the lithium-transition metal composite oxide was 50 mol%, as in Patent Document 1, and it was not possible to manufacture a positive electrode active material in the form of secondary particles with a primary particle size of micron-level for a high-nickel (High Ni) positive electrode active material with excellent capacity characteristics due to the high content of nickel among the transition metals of the lithium-transition metal composite oxide.

[0013]

[0014] The problem to be solved in the present invention is to provide a cathode active material that can simultaneously solve the problems of conventional secondary particles and single particles in a high nickel (High Ni) cathode active material.

[0015] That is, the present invention has been devised to solve the problems of the above-mentioned prior art, and is a high nickel (High Ni) cathode active material having excellent capacity characteristics due to a high content of nickel among transition metals of a lithium transition metal composite oxide, and by implementing a cathode active material in the form of secondary particles having a primary particle size of micron level, it is intended to provide a cathode active material having excellent density characteristics and improving energy density as well as cell characteristics such as improved lifespan and reduced gas generation.

[0016] In addition, the present invention aims to provide a positive electrode and a lithium secondary battery including the positive electrode active material.

[0017]

[0018] To solve the above problem, the present invention provides a cathode active material, a cathode including the same, and a lithium secondary battery.

[0019] (1) The present invention comprises a secondary particle in which a plurality of primary particles are aggregated, and the plurality of primary particles have an average particle size of 1.5 ㎛ or more and 5.0 ㎛ or less as measured from an SEM image, and the particle size of the primary particles is a particle size based on the major axis of the primary particles, and the plurality of primary particles include disk-type primary particles, and the disk-type primary particles are such that, in the primary particles observed from an SEM image of the surface or cross-section of the secondary particles, when two imaginary tangent lines having the greatest number of contact points are drawn for two boundaries of the primary particles existing within an angle of 45° or less with respect to the major axis direction, and one imaginary line crossing the two tangent lines is drawn, the same side angle is 150° or more and 210° or less, the minor axis is 0.3 ㎛ or more, and the aspect ratio (major axis / minor axis) is 1.5 or more. Provides active material.

[0020] (2) The present invention provides a positive electrode active material in the above (1), wherein the plurality of primary particles include three or more disk-type primary particles.

[0021] (3) The present invention provides a positive electrode active material in (1) or (2) above, wherein the disk-shaped primary particles have a short diameter of 0.8 ㎛ or more.

[0022] (4) The present invention provides a positive electrode active material comprising a lithium transition metal composite oxide containing nickel, cobalt, and manganese in any one of the above (1) to (3).

[0023] (5) The present invention provides a positive electrode active material comprising a lithium transition metal composite oxide containing nickel in an amount of 60 mol% or more among the total transition metals, in any one of (1) to (4) above.

[0024] (6) The present invention provides a positive electrode active material comprising a lithium transition metal composite oxide having an average composition represented by the following chemical formula 1, in any one of the above (1) to (5).

[0025] [Chemical Formula 1]

[0026] Li x Ni a Co b Mn c M 1 d O2

[0027] In the above chemical formula 1, M 1 is at least one selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, V, F, P, S and Y, and 0.9≤x≤1.3, 0.6≤a<1.0, 0 <b<0.4, 0<c<0.4, 0≤d≤0.2, a+b+c+d=1이다.

[0028] (7) The present invention provides a positive electrode active material according to any one of the above (1) to (6), wherein the plurality of primary particles include single-crystal primary particles.

[0029] (8) In any one of the above (1) to (7), the secondary particles have an average particle diameter (D) according to a volume cumulative distribution measured using a laser diffraction particle size analyzer. 50 ) provides a positive electrode active material having a particle size of 7.0 ㎛ or more and 20.0 ㎛ or less.

[0030] (9) The present invention provides a positive electrode comprising a positive electrode active material according to any one of (1) to (8).

[0031] (10) The present invention provides a lithium secondary battery including a positive electrode according to the above (9); a negative electrode; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.

[0032]

[0033] The cathode active material of the present invention is a cathode active material that can simultaneously solve the problems of conventional secondary particles and single particles in high nickel (High Ni) cathode active materials, and by implementing a cathode active material in the form of secondary particles whose primary particles are on the micron level in size, it can not only improve cell characteristics such as improved lifespan of a lithium secondary battery and reduced gas generation, but also improve energy density due to excellent density characteristics.

[0034]

[0035] Figure 1 is an SEM image of (A) the positive electrode active material of Example 1, and (B) an SEM image of a cross-section of the positive electrode active material.

[0036] Figure 2 is an SEM image of (A) the positive electrode active material of Example 2, and (B) an SEM image of a cross-section of the positive electrode active material.

[0037] Figure 3 is an SEM image of (A) the positive electrode active material of Example 3, and (B) an SEM image of a cross-section of the positive electrode active material.

[0038] Figure 4 is an SEM image of (A) the positive electrode active material of Example 4, and (B) an SEM image of a cross-section of the positive electrode active material.

[0039] Figure 5 is an SEM image of (A) the positive electrode active material of Example 5, and (B) an SEM image of a cross-section of the positive electrode active material.

[0040] Figure 6 is an SEM image of (A) the positive electrode active material of Example 6, and (B) an SEM image of a cross-section of the positive electrode active material.

[0041] Figure 7 is an SEM image of (A) the positive electrode active material of Example 7, and (B) an SEM image of a cross-section of the positive electrode active material.

[0042] Figure 8 is an SEM image of (A) the positive electrode active material of Example 8, and (B) an SEM image of a cross-section of the positive electrode active material.

[0043] Figure 9 is an SEM image of (A) the positive electrode active material of Example 9, and (B) an SEM image of a cross-section of the positive electrode active material.

[0044] Figure 10 is an SEM image of (A) the positive electrode active material of Example 10, and (B) an SEM image of a cross-section of the positive electrode active material.

[0045] Figure 11 is an SEM image of (A) the positive electrode active material of Example 11, and (B) an SEM image of a cross-section of the positive electrode active material.

[0046] Figure 12 is an SEM image of (A) the positive electrode active material of Comparative Example 1, and (B) an SEM image of a cross-section of the positive electrode active material.

[0047] Figure 13 shows an SEM image of (A) the positive electrode active material of Comparative Example 2, and an SEM image of (B) the cross-section of the positive electrode active material.

[0048] Figure 14 is an SEM image of (A) the positive electrode active material of Comparative Example 3, and (B) an SEM image of a cross-section of the positive electrode active material.

[0049] Figure 15 is an SEM image of (A) the positive electrode active material of Comparative Example 4, and (B) an SEM image of a cross-section of the positive electrode active material.

[0050] Figure 16 is an SEM image of (A) the positive electrode active material of Comparative Example 5, and (B) an SEM image of a cross-section of the positive electrode active material.

[0051] Figure 17 is a segmentation image showing multiple lithium composite transition metal oxides segmented by performing image analysis based on an artificial intelligence model from an SEM image of the positive electrode active material of Example 1.

[0052] Figure 18 is a segmentation image showing multiple lithium composite transition metal oxides segmented by performing image analysis based on an artificial intelligence model from an SEM image of the positive electrode active material of Comparative Example 1.

[0053] Figure 19 is a TEM image of a cross-section of the positive electrode active material of Example 1.

[0054] Figure 20 is a TEM image of a cross-section of the positive electrode active material of Example 2.

[0055] Figure 21 is a TEM image of a cross-section of the positive electrode active material of Example 8.

[0056] Figure 22 is an EBSD pattern image of a cross-section of the positive electrode active material of Example 1.

[0057] Figure 23 is an EBSD pattern image of a cross-section of the positive electrode active material of Example 2.

[0058] Figure 24 is an EBSD pattern image of a cross-section of the positive electrode active material of Example 3.

[0059] Figure 25 is an EBSD pattern image of a cross-section of the positive electrode active material of Example 4.

[0060] Figure 26 is an EBSD pattern image of a cross-section of the positive electrode active material of Example 8.

[0061] Figure 27 is an EBSD pattern image of a cross-section of the positive electrode active material of Example 10.

[0062] Figure 28 is an EBSD pattern image of a cross-section of the positive electrode active material of Example 11.

[0063] Figure 29 is an EBSD pattern image of a cross-section of the positive electrode active material of Comparative Example 3.

[0064] Figure 30 is an EPMA analysis image of the positive electrode active material of Example 1.

[0065] Figure 31 is a graph showing the cumulative volume distribution of the positive electrode active material of Example 1 measured using a laser diffraction particle size analyzer, with the x-axis representing a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis representing a weight distribution in which the y-value increases from bottom to top.

[0066] Figure 32 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 2 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0067] Figure 33 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 3 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0068] Figure 34 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 4 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0069] Figure 35 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 5 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0070] Figure 36 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 6 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0071] Figure 37 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 7 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0072] Figure 38 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 8 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0073] Figure 39 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 9 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0074] Figure 40 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 10 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0075] Figure 41 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 11 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0076] Figure 42 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Comparative Example 1 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0077] Figure 43 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Comparative Example 3 measured using a laser diffraction particle size analyzer, in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0078] Figure 44 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 1 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0079] Figure 45 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 2 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0080] Figure 46 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 3 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0081] Figure 47 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 4 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0082] Figure 48 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 5 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0083] Figure 49 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 6 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0084] Figure 50 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 7 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0085] Figure 51 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 8 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0086] Figure 52 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 9 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0087] Figure 53 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 10 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0088] Figure 54 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Example 11 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0089] Figure 55 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Comparative Example 1 measured using a laser diffraction particle size analyzer, with the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top.

[0090] Figure 56 is a frequency distribution graph showing the volume cumulative distribution of the positive electrode active material of Comparative Example 3 measured using a laser diffraction particle size analyzer, in which the x-axis represents a log scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0091]

[0092] Hereinafter, the present invention will be described in more detail to help understand the present invention.

[0093] The terms or words used in the description and claims of the present invention should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.

[0094]

[0095] In the present invention, the term 'primary particle' means the smallest particle unit that can be distinguished as a single lump when observing the cross-section of a positive electrode active material through a scanning electron microscope (SEM), and may be composed of a single crystal or multiple crystal grains.

[0096] In the present invention, the term "secondary particle" refers to a secondary structure formed by the aggregation of multiple primary particles. The average particle diameter of the secondary particles can be measured using a particle size analyzer.

[0097] In the present invention, the term 'average particle diameter (D 50)' means the particle size at the 50% point of the volume cumulative distribution according to particle size. The above average particle size is calculated by dispersing the powder to be measured in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., S3500 from Microtrac), and measuring the difference in diffraction pattern according to particle size when the particles pass through the laser beam to calculate the particle size distribution, and calculating the particle diameter at the point where it becomes 50% of the volume cumulative distribution according to particle size in the measuring device, thereby obtaining D 50 can be measured.

[0098] In the present invention, the term 'major axis of a primary particle' refers to the length of the longest line segment when a line is drawn passing through two points of the primary particle boundary in a primary particle observed from an SEM image of the surface or cross-section of a secondary particle.

[0099] In the present invention, the term 'shortest diameter of a primary particle' refers to the length of the shortest line segment when a line is drawn passing through two points of the primary particle boundary in a primary particle observed from an SEM image of the surface or cross-section of a secondary particle.

[0100]

[0101] positive electrode active material

[0102] The present invention provides a positive electrode active material.

[0103] According to one embodiment of the present invention, a plurality of primary particles may include secondary particles aggregated together, and the plurality of primary particles may have an average particle size measured from an SEM image of 1.5 μm or more and 5.0 μm or less.

[0104] According to one embodiment of the present invention, the secondary particle is a secondary particle formed by agglomeration of a plurality of primary particles, and may be a secondary particle formed by agglomeration of at least two, specifically at least three or more primary particles.

[0105] According to one embodiment of the present invention, the plurality of primary particles may have an average particle size measured from an SEM image of 1.5 ㎛ or more, 1.6 ㎛ or more, 1.7 ㎛ or more, 1.8 ㎛ or more, 1.9 ㎛ or more, 2.0 ㎛ or more, 2.1 ㎛ or more, 2.2 ㎛ or more, 2.3 ㎛ or more, 2.4 ㎛ or more, or 2.5 ㎛ or more, and further, 5.0 ㎛ or less, 4.9 ㎛ or less, 4.8 ㎛ or less, 4.7 ㎛ or less, 4.6 ㎛ or less, 4.5 ㎛ or less, 4.4 ㎛ or less, 4.3 ㎛ or less, 4.2 ㎛ or less, 4.1 ㎛ or less, 4.0 ㎛ or less, 3.9 ㎛ or less, 3.8 ㎛ or less, 3.7 ㎛ or less, 3.6 ㎛ or less, 3.5 It may be ㎛ or less, 3.4 ㎛ or less, 3.3 ㎛ or less, 3.2 ㎛ or less, 3.1 ㎛ or less, or 3.0 ㎛ or less. Here, when measuring the average particle size for the plurality of primary particles from the SEM image, the particle size of each primary particle may be a particle size based on the major diameter of the primary particle. Within this range, the rolling density of the positive electrode active material can be further improved, and the lifespan of the lithium secondary battery can be further improved.

[0106] According to one embodiment of the present invention, the positive electrode active material may include a lithium transition metal composite oxide containing nickel, cobalt, and manganese. As a specific example, the positive electrode active material may include a lithium transition metal composite oxide containing nickel at 60 mol% or more among the total transition metals. The lithium transition metal composite oxide may be a primary particle, a secondary particle, and the positive electrode active material itself containing these, and as a specific example, the positive electrode active material may include a secondary particle in which a plurality of primary particles composed of the lithium transition metal composite oxide are aggregated.

[0107] According to one embodiment of the present invention, the positive electrode active material may include a lithium transition metal composite oxide having an average composition represented by the following chemical formula 1.

[0108] [Chemical Formula 1]

[0109] Li x Ni a Co b Mn c M 1 d O2

[0110]

[0111] *52 In the above chemical formula 1, M 1 is at least one selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, V, F, P, S and Y, and 0.9≤x≤1.3, 0.6≤a<1.0, 0 <b<0.4, 0<c<0.4, 0≤d≤0.2, a+b+c+d=1이다.

[0112] According to one embodiment of the present invention, in the chemical formula 1, x is a molar ratio of lithium to a transition metal in a lithium transition metal composite oxide, which may be 0.9 or more, 0.95 or more, or 1.0 or more, and may also be 1.1 or less, 1.07 or less, 1.05 or less, or 1.03 or less.

[0113] According to one embodiment of the present invention, in the chemical formula 1, a, b, c and d are nickel (Ni), cobalt (Co), manganese (Mn) and doping element (M) among transition metals, respectively. 1) may be a mole fraction. As a specific example, the above a may be a mole fraction of nickel (Ni) among transition metals, and may be 0.6 or more, 0.7 or more, 0.8 or more, 0.85 or more, 0.88 or more, 0.90 or more, 0.91 or more, 0.92 or more, 0.93 or more, 0.94 or more, 0.95 or more, or 0.96 or more, and may also be less than 1.0, 0.99 or less, 0.98 or less, 0.97 or less, or 0.96 or less. In addition, the above b is a mole fraction of cobalt (Co) among the transition metals, which may be greater than 0, 0.01 or more, 0.02 or more, or 0.03 or more, and may also be less than 0.4, 0.3 or less, 0.2 or less, 0.1 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, or 0.05 or less. The above c is a mole fraction of manganese (Mn) among the transition metals, which may be greater than 0, 0.01 or more, or 0.05 or more, and may also be less than 0.4, 0.3 or less, 0.2 or less, 0.1 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, or 0.05 or less. The above d is a doping element (M) among the transition metals. 1) as a mole fraction of 0, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, 0.10 or more, 0.11 or more, 0.12 or more, 0.13 or more, 0.14 or more, 0.15 or more, 0.16 or more, 0.17 or more, 0.18 or more, or 0.19 or more, and also less than 0.20, 0.19 or less, 0.18 or less, 0.17 or less, 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, 0.10 or less, 0.09 or less, 0.08 or less, It may be 0.07 or less, 0.06 or less, 0.05 or less, 0.04 or less, 0.03 or less, 0.02 or less, or 0.01 or less. When the composition of the lithium transition metal composite oxide is adjusted as above, the capacity can be further improved.

[0114] According to one embodiment of the present invention, the plurality of primary particles may include single-crystal primary particles, in which case the rolling density of the positive electrode active material can be further improved. The single-crystal primary particles refer to primary particles formed of a single crystal.

[0115] According to one embodiment of the present invention, the secondary particles have an average particle diameter (D) according to a volume cumulative distribution measured using a laser diffraction particle size analyzer. 50 ) may be 7.0 ㎛ or more and 20.0 ㎛ or less. As a specific example, the secondary particles may have an average particle diameter (D 50) may be 7.0 ㎛ or more, 7.1 ㎛ or more, 7.2 ㎛ or more, 7.3 ㎛ or more, 7.4 ㎛ or more, 7.5 ㎛ or more, 7.6 ㎛ or more, 7.7 ㎛ or more, 7.8 ㎛ or more, 7.9 ㎛ or more, 8.0 ㎛ or more, 8.1 ㎛ or more, 8.2 ㎛ or more, 8.3 ㎛ or more, 8.4 ㎛ or more, 8.5 ㎛ or more, 8.6 ㎛ or more, 8.7 ㎛ or more, 8.8 ㎛ or more, 8.9 ㎛ or more, or 9.0 ㎛ or more, and also may be 20.0 ㎛ or less, 19.9 ㎛ or less, 19.8 ㎛ or less, 19.7 ㎛ or less, 19.6 ㎛ or less, 19.5 ㎛ or less, 19.4 ㎛ or less, 19.3 ㎛ or less, 19.2 ㎛ or less, 19.1 ㎛ or less, 19.0 ㎛ or less, 18.9 ㎛ or less, 18.8 ㎛ or less, 18.7 ㎛ or less, 18.6 ㎛ or less, 18.5 ㎛ or less, 18.4 ㎛ or less, 18.3 ㎛ or less, 18.2 ㎛ or less, 18.1 ㎛ or less, 18.0 ㎛ or less, 17.9 ㎛ or less, 17.8 ㎛ or less, 17.7 ㎛ or less, 17.6 ㎛ or less, 17.5 ㎛ or less, 17.4 ㎛ or less, 17.3 ㎛ or less, 17.2 ㎛ or less, 17.1 ㎛ or less, 17.0 ㎛ or less, 16.9 ㎛ or less, 16.8 ㎛ or less, 16.7 ㎛ or less, It may be 16.6 ㎛ or less, 16.5 ㎛ or less, 16.4 ㎛ or less, 16.3 ㎛ or less, 16.2 ㎛ or less, 16.1 ㎛ or less, 16.0 ㎛ or less, 15.9 ㎛ or less, 15.8 ㎛ or less, 15.7 ㎛ or less, 15.6 ㎛ or less, 15.5 ㎛ or less, 15.4 ㎛ or less, 15.3 ㎛ or less, 15.2 ㎛ or less, 15.1 ㎛ or less, or 15.0 ㎛ or less. Within this range, the rolling density of the positive electrode active material can be further improved, and the lifespan can be further improved.

[0116] As a specific example, the positive electrode active material is a high nickel positive electrode active material including a lithium transition metal composite oxide containing nickel at 60 mol% or more among the total transition metal, and a plurality of primary particles are formed by agglomeration of primary particles having a particle size of 0.5 ㎛ or more and 5.0 ㎛ or less, such as a conventional single particle, specifically, micron-level primary particles having a particle size of 1.0 ㎛ or more, and more specifically, a plurality of primary particles having an average particle size of 2.0 ㎛ or more and 3.5 ㎛ or less as measured from an SEM image, and having an average particle diameter (D 50 ) may include secondary particles having a particle size of 7.0 ㎛ or more and 20.0 ㎛ or less, and may be expressed as a particle size single particle cluster in the sense that primary particles in the form of single particles are aggregated to form particles in the form of secondary particles.

[0117] As described above in the background technology of the present invention, in order to manufacture a positive electrode active material in the form of secondary particles having a primary particle size of micron level, it is necessary to perform heat treatment at a higher temperature than that of secondary particles having a primary particle size of less than 1 ㎛ in submicron level. However, as the heat treatment temperature increases, the layered structure of the lithium-transition metal composite oxide degenerates into a rock salt structure, which causes a decrease in crystallinity and, in turn, a decrease in the performance of the positive electrode active material. In particular, since nickel is most vulnerable to the degeneration of the layered structure of the lithium-transition metal composite oxide into a rock salt structure at high heat treatment temperatures, the degeneration becomes more severe when the nickel content in the lithium-transition metal composite oxide constituting the positive electrode active material increases. Therefore, in the past, it was only possible to apply the method to mid-nickel cathode active materials in which the nickel content among the transition metals of the lithium-transition metal composite oxide was 50 mol%, as a cathode active material in the form of secondary particles in which the primary particles were on the micron level in size, and it was not possible to manufacture a cathode active material in the form of secondary particles in which the primary particles were on the micron level in size for high-nickel cathode active materials in which the nickel content among the transition metals of the lithium-transition metal composite oxide was high and thus had excellent capacity characteristics.

[0118] However, since the positive electrode active material of the present invention has a high content of nickel among the transition metals of the lithium-transition metal composite oxide, even if the layered structure of the lithium-transition metal composite oxide degenerates into a rock salt structure at a high heat treatment temperature, the above-mentioned problem is solved by recovering the rock salt structure into a layered structure. Specifically, unlike the conventional mid-nickel positive electrode active material, the positive electrode active material of the present invention is a high-nickel positive electrode active material including a lithium-transition metal composite oxide containing nickel at 60 mol% or more of the total transition metal, and while including secondary particles having a size of the primary particles on the micron level, the rock salt structure formed by the high heat treatment temperature is recovered into a layered structure, so that the crystallinity of the lithium-transition metal composite oxide is excellent, and the problems of the conventional secondary particles and the problems of the single particles can be solved at the same time. The positive electrode active material of the present invention can be manufactured by restoring the rock salt structure formed by the high heat treatment temperature as described above into a layered structure, and the method for restoring the rock salt structure into a layered structure is not limited, but according to one embodiment of the present invention, the method for restoring the rock salt structure into a layered structure may be to perform cobalt (Co) coating on a lithium transition metal composite oxide including the rock salt structure formed by the high heat treatment temperature.

[0119] According to one embodiment of the present invention, the plurality of primary particles may include disk-type primary particles, and as a specific example, may include three or more disk-type primary particles, in which case the cell has excellent lifespan and energy density.

[0120] According to one embodiment of the present invention, the disk-shaped primary particle may mean that, in the primary particle observed from an SEM image of the surface or cross-section of the secondary particle, when two virtual tangent lines having the greatest number of contact points are drawn for each of the two boundaries of the primary particle existing within an angle of 45° or less with respect to the major axis direction, and one virtual line crossing the two tangent lines is drawn, the same-sided internal angle is 150° or more and 210° or less, the minor axis of the primary particle is 0.3 ㎛ or more, and the aspect ratio (major axis / minor axis) is 1.5 or more. As a specific example, the disk-shaped primary particle may have a primary particle diameter of 0.3 ㎛ or more, 0.4 ㎛ or more, 0.5 ㎛ or more, 0.6 ㎛ or more, 0.7 ㎛ or more, 0.8 ㎛ or more, 0.9 ㎛ or more, or 1.0 ㎛ or more. Here, when the disk-shaped primary particle has a primary particle diameter of 0.3 ㎛ or more and an aspect ratio (major axis / minor axis) of 1.5 or more, the area ratio of the (003) plane among the crystal planes on the surface of the primary particle may be the largest.

[0121] As a specific example, the positive electrode active material may include secondary particles in which a plurality of primary particles are aggregated, and the plurality of primary particles may have an average particle size of 1.5 ㎛ or more and 5.0 ㎛ or less as measured from an SEM image, and the plurality of primary particles may include disk-type primary particles, and the disk-type primary particles may have, in the primary particles observed from an SEM image of a surface or cross-section of the secondary particles, when two imaginary tangent lines having the greatest number of contact points are drawn for each of two boundaries of the primary particles existing within an angle of 45° or less with respect to the major axis direction, and one imaginary line crossing the two tangent lines is drawn, the coplanar internal angle may be 150° or more and 210° or less, the minor axis of the primary particles may be 0.3 ㎛ or more, and the aspect ratio (major axis / minor axis) may be 1.5 or more. More specifically, the disk type primary particles may have a short diameter of 0.8 ㎛ or more.

[0122] According to one embodiment of the present invention, the disk-shaped primary particle may mean that, in the primary particle observed from the SEM image of the surface or cross-section of the secondary particle, when two imaginary tangent lines having the largest number of contact points are drawn for each of the two boundaries of the primary particle existing within an angle of 45° or less with respect to the major axis direction, and one imaginary line crossing the two tangent lines is drawn, the coplanar internal angle is 150° or more and 210° or less, and the area ratio of the (003) plane among the crystal planes on the surface of the primary particle of the primary particle is the largest. Here, when the area ratio of the (003) plane among the crystal planes on the surface of the primary particle of the disk-shaped primary particle is the largest, the primary particle may have a minor axis of 0.3 ㎛ or more, and an aspect ratio (major axis / minor axis) of 1.5 or more. That is, the largest area ratio of the (003) plane among the crystal planes on the surface of the primary particle can be confirmed from the fact that the primary particle's minor axis is 0.3 ㎛ or more and its aspect ratio (major axis / minor axis) is 1.5 or more.

[0123] According to one embodiment of the present invention, the positive electrode active material is a frequency distribution graph in which the x-axis represents a logarithmic scale for particle diameters in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top, and the peak point at the top of the y-axis of the peak appearing at the mode; and when a triangle is drawn with two points of contact of the frequency distribution curve that touch at the half width (FWHM) of the mode, the internal angle (θ) at the left point of the two points of contact of the frequency distribution curve that touch at the half width L ) and the interior angle (θ) at the right contact point R ) of the difference (θ) L - θ R ) may be greater than or equal to 6 and less than or equal to 20. As a specific example, the interior angle (θ) at the left contact point L ) and the interior angle (θ) at the right contact point R) of the difference (θ) L - θ R ) may be 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, 11 or more, 12 or more, 13 or more, or 14 or more, and may also be 20 or less, 19 or less, 18 or less, 17 or less, 16 or less, or 15 or less. The positive electrode active material may have a ratio (θ) of the inner angle at the left contact point to the inner angle at the right contact point. L / θ R ) may be greater than or equal to 1.100 and less than or equal to 2.000. As a specific example, the ratio of the interior angle at the left contact point to the interior angle at the right contact point (θ L / θ R ) is 1.100 or higher, 1.110 or higher, 1.120 or higher, 1.130 or higher, 1.140 or higher, 1.150 or higher, 1.160 or higher, 1.170 or higher, 1.180 or higher, 1.190 or higher, 1.200 or higher, 1.210 or higher, 1.220 or higher, 1.230 or higher, 1.240 or higher, 1.250 or higher, 1.260 or higher, 1.270 or higher, 1.280 or higher, 1.290 or higher, 1.300 or higher, 1.310 or higher, 1.320 or higher, 1.330 or higher, 1.340 or higher, 1.350 or higher, 1.360 or higher, 1.370 or higher, 1.380 or higher, 1.390 or higher, It may be 1.400 or more, 1.410 or more, 1.420 or more, 1.430 or more, or 1.440 or more, and may also be 1.450 or less, 1.460 or less, 1.470 or less, 1.480 or less, 1.490 or less, 1.500 or less, 1.550 or less, 1.600 or less, 1.650 or less, 1.700 or less, 1.750 or less, 1.800 or less, 1.850 or less, 1.900 or less, 1.950 or less, or 2.000 or less. Here, the frequency distribution graph may be a unimodal distribution graph.

[0124] According to one embodiment of the present invention, the positive active material may exhibit positive skewness in a frequency distribution graph in which the volume cumulative distribution measured using a laser diffraction particle size analyzer is represented by a linear scale for particle diameters in which the x-axis represents the x-value increasing from left to right, and the y-axis represents the weight distribution in which the y-value increasing from bottom to top. Here, the frequency distribution graph may be a unimodal distribution graph.

[0125] According to one embodiment of the present invention, the positive electrode active material has a y-value (P) of the peak point at the top of the y-axis of the peak appearing in the mode according to the volume cumulative distribution. MODE ) to the ratio of skewness values ​​(S) (S / P) MODE ) may be 0.037 or more and 0.150 or less. As a specific example, the positive electrode active material may have a y-value (P) of the peak point at the top of the y-axis of the peak appearing in the mode according to the volume cumulative distribution. MODE ) to the ratio of skewness values ​​(S) (S / P) MODE) is 0.037 or more, 0.038 or more, 0.039 or more, 0.040 or more, 0.041 or more, 0.042 or more, 0.043 or more, 0.044 or more, 0.045 or more, 0.046 or more, 0.047 or more, 0.048 or more, 0.049 or more, 0.050 or more, 0.051 or more, 0.052 or more, 0.053 or more, 0.054 or more, 0.055 or more, 0.056 or more, 0.057 or more, 0.058 or more, 0.059 or more, 0.060 or more, 0.061 or more, 0.062 or more, 0.063 or more, 0.064 or more, 0.065 or more, 0.066 or more, 0.067 or higher, 0.068 or higher, 0.069 or higher, 0.070 or higher, 0.071 or higher, 0.072 or higher, 0.073 or higher, 0.074 or higher, 0.075 or higher, 0.076 or higher, 0.077 or higher, 0.078 or higher, 0.079 or higher, 0.080 or higher, 0.081 or higher, 0.082 or higher, 0.083 or higher, 0.083 or higher, 0.084 or higher, 0.085 or higher, 0.086 or higher, 0.087 or higher, 0.088 or higher, 0.089 or higher, 0.090 or higher, 0.091 or higher, 0.092 or higher, 0.093 or higher, 0.094 or higher, 0.095 or higher, 0.096 It may be 0.097 or more, 0.098 or more, 0.099 or more, or 0.100 or more, and may be 0.150 or less, 0.140 or less, 0.130 or less, 0.120 or less, or 0.110 or less. Here, the skewness value (S) may be calculated from the following equation 3.

[0126] [Formula 3]

[0127]

[0128] According to one embodiment of the present invention, the positive electrode active material has a BET specific surface area of ​​0.20 m as measured through nitrogen adsorption BET specific surface area analysis. 2 / g or more, 0.35 m 2 / g or less. As a specific example, the positive electrode active material has a BET specific surface area of ​​0.20 m measured through nitrogen adsorption BET specific surface area analysis. 2 / g or more, 0.21 m 2 / g or more, 0.22 m 2 / g or more, 0.23 m 2 / g or more, 0.24 m 2 / g or more, 0.25 m 2 / g or more, 0.26 m 2 / g or more, 0.27 m 2 / g or more, 0.28 m 2 / g or more, 0.29 m 2 / g or more, 0.30 m 2 / g or more, or 0.31 m 2 / g or more, and also 0.35 m 2 / g or less, or 0.34 m 2 / g or less. Within this range, the DC resistance can be reduced and the rolling density can be improved.

[0129] According to one embodiment of the present invention, the positive electrode active material has an average particle diameter (D) according to a volume cumulative distribution measured using a laser diffraction particle size analyzer for the secondary particles. 50 ) is 7.0 ㎛ or more and 20.0 ㎛ or less, and the size of the cross-section of the secondary particles observed from the SEM image of the cross-section of the secondary particles is the average particle diameter (D) of the secondary particles 50 ) For the cross-section of a secondary particle having a size within the range, the number of cross-sections of primary particles confirmed within a unit area of ​​5 ㎛ in width and 5 ㎛ in length within the cross-section of the secondary particle may be 1 or more and 100 or less.

[0130] According to one embodiment of the present invention, the size of the cross-section of the secondary particle observed from the SEM image of the cross-section of the secondary particle is the average particle diameter (D) of the secondary particle 50) For the cross-section of a secondary particle having a size within the range, the number of cross-sections of primary particles confirmed within a unit area of ​​5 ㎛ wide x 5 ㎛ long within the cross-section of the secondary particle means the number of cross-sections of all primary particles that include at least a part of the cross-sections of the primary particles in addition to all cross-sections of the primary particles confirmed within the unit area. In addition, the unit area of ​​5 ㎛ wide x 5 ㎛ long within the cross-section of the secondary particle means the unit area at any point within the cross-section of the secondary particle, and the location is not limited as long as it is within the cross-section of the secondary particle.

[0131] According to one embodiment of the present invention, the cathode active material has a cross-section size of the secondary particles, as observed from an SEM image of the cross-section of the secondary particles, equal to the average particle diameter (D) of the secondary particles. 50 ) for the cross-section of the secondary particle having a size within the range, the number of primary particle cross-sections confirmed within a unit area of ​​5 ㎛ in width and 5 ㎛ in length within the cross-section of the secondary particle may be 1 or more and 100 or less, and as a specific example, it may be 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, or 10 or more, and further, it may be 100 or less, 95 or less, 90 or less, 85 or less, 80 or less, 75 or less, 70 or less, 65 or less, 60 or less, 55 or less, 50 or less, 45 or less, 40 or less, 35 or less, 30 or less, or 25 or less. When such a range is satisfied, the positive electrode active material is formed by agglomeration of a plurality of primary particles having a particle size of 0.5 ㎛ or more and 5.0 ㎛ or less, such as a conventional single particle, specifically a micron-level primary particle of 1.0 ㎛ or more, and more specifically a plurality of primary particles having an average particle size of 2.0 ㎛ or more and 3.5 ㎛ or less as measured from an SEM image, and an average particle diameter (D50 ) can indicate that it contains secondary particles with a large particle size of 7.0 ㎛ or more and 20.0 ㎛ or less.

[0132] According to one embodiment of the present invention, the positive electrode active material has an average particle diameter (D) according to a volume cumulative distribution measured using a laser diffraction particle size analyzer for the secondary particles. 50 ) is 7.0 ㎛ or more and 20.0 ㎛ or less, and the size of the cross-section of the secondary particle observed from the backscattered electron diffraction (EBSD) pattern of the SEM image of the cross-section of the secondary particle (measured under the conditions of acceleration voltage 20 kV, WD 16 mm, measurement magnification 5,000 times (width 16 ㎛ * height 16 ㎛), step size 0.025 ㎛) is the average particle diameter (D) of the secondary particle 50 ) For the cross-section of a secondary particle having a size within the range, the number of cross-sections of grains confirmed within a unit area of ​​5 ㎛ in width and 5 ㎛ in length within the cross-section of the secondary particle may be 1 or more and 150 or less.

[0133] According to one embodiment of the present invention, the size of the cross-section of the secondary particle observed from the backscattered electron diffraction (EBSD) pattern of the SEM image of the cross-section of the secondary particle (measured under the conditions of acceleration voltage 20 kV, WD 16 mm, measurement magnification 5,000 times (width 16 ㎛ * height 16 ㎛), step size 0.025 ㎛) is the average particle diameter (D) of the secondary particle 50) For the cross-section of a secondary particle having a size within the range, the number of cross-sections of grains confirmed within a unit area of ​​5 ㎛ in width * 5 ㎛ in length within the cross-section of the secondary particle means the number of cross-sections of all grains that include at least a part of the cross-sections of grains in addition to all cross-sections of grains confirmed within the unit area. In addition, the unit area of ​​5 ㎛ in width * 5 ㎛ in length within the cross-section of the secondary particle means the unit area at any point within the cross-section of the secondary particle, and the location is not limited as long as it is within the cross-section of the secondary particle.

[0134] According to one embodiment of the present invention, the cathode active material has a cross-section size of the secondary particles, which is observed from the backscattered electron diffraction (EBSD) pattern of the SEM image of the cross-section of the secondary particles (measured under the conditions of acceleration voltage 20 kV, WD 16 mm, measurement magnification 5,000 times (width 16 ㎛ * height 16 ㎛), step size 0.025 ㎛). 50) for the cross-section of the secondary particle having a size within the range, the number of cross-sections of grains confirmed within a unit area of ​​5 ㎛ in width * 5 ㎛ in length within the cross-section of the secondary particle may be 1 or more and 150 or less, and as a specific example, it may be 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, or 9 or more, and also, 150 or less, 145 or less, 140 or less, 135 or less, 130 or less, 125 or less, 120 or less, 115 or less, 110 or less, 105 or less, 100 or less, 95 or less, 90 or less, 85 or less, 80 or less, 75 or less, 70 or less, 65 or less, 60 or less, It may be 55 or less, 50 or less, 45 or less, 40 or less, 35 or less, 30 or less, 25 or less, or 20 or less. When such a range is satisfied, the positive electrode active material is formed by agglomeration of a plurality of primary particles having a particle size of 0.5 ㎛ or more and 5.0 ㎛ or less, such as a conventional single particle, specifically a micron-level primary particle of 1.0 ㎛ or more, and more specifically a plurality of primary particles having an average particle size of 2.0 ㎛ or more and 3.5 ㎛ or less as measured from an SEM image, and having an average particle diameter (D 50 ) can indicate that it contains secondary particles with a large particle size of 7.0 ㎛ or more and 20.0 ㎛ or less.

[0135] According to one embodiment of the present invention, the positive electrode active material has a single crystallinity of 0.15 ㎛ calculated from the following equation 1. 3 It could be something like this.

[0136] [Formula 1]

[0137]

[0138] In the above equation 1, radius(grain) is the size of the cross-section of the secondary particle observed from the backscattered electron diffraction (EBSD) pattern of the SEM image of the cross-section of the secondary particle (measured under the conditions of acceleration voltage 20 kV, WD 16 mm, measurement magnification 5,000 times (width 16 ㎛ * height 16 ㎛), step size 0.025 ㎛). 50 ) Among all the cross-sections of grains that can be identified in the cross-section of secondary particles having a size within the range, the area of ​​the cross-section of the grain is 0.196 ㎛. 2 For the cross-section of an ideal grain, n is the radius of the cross-section of the grain assuming that the cross-section of the grain is circular, and n is the number of grains.

[0139] According to one embodiment of the present invention, the positive electrode active material has a single crystallinity of 0.15 ㎛ calculated from the above equation 1. 3 Above, 12.70 ㎛ 3 It may be as follows. As a specific example, the positive electrode active material has a single crystallinity of 0.15 ㎛ calculated from the above equation 1. 3 Above, 0.20 ㎛ 3 Above, 0.25 ㎛ 3 Above, 0.30 ㎛ 3 Above, 0.35 ㎛ 3 Above, 0.40 ㎛ 3 Above, 0.45 ㎛ 3 Above, 0.50 ㎛ 3 Above, 0.55 ㎛ 3 Above, 0.60 ㎛ 3 Above, 0.65 ㎛ 3 Above, 0.70 ㎛ 3 Above, 0.75 ㎛ 3 Above, 0.80 ㎛ 3 Above, 0.85 ㎛ 3 Above, 0.90 ㎛ 3 Above, 0.95 ㎛ 3 Above, 1.00 ㎛ 3 or 1.05 ㎛ 3It may be more than that, and also, the upper limit is not particularly limited, but 20.00 ㎛ 3 Below, 19.00 ㎛ 3 Below, 18.00 ㎛ 3 Below, 17.00 ㎛ 3 Below, 16.00 ㎛ 3 Below, 15.00 ㎛ 3 Below, 14.00 ㎛ 3 Below, 13.00 ㎛ 3 or less, or 12.70 ㎛ 3 It could be as follows:

[0140] According to one embodiment of the present invention, the positive electrode active material may include a lithium transition metal composite oxide including aluminum (Al), yttrium (Y), and zirconium (Zr). As a specific example, the positive electrode active material may include aluminum (Al), yttrium (Y), and zirconium (Zr) as doping elements.

[0141] According to one embodiment of the present invention, the aluminum (Al) may be included in an amount of 500 ppm to 3,000 ppm based on the total weight of the lithium transition metal composite oxide. As a specific example, the aluminum (Al) may be included in an amount of 500 ppm or more, 1,000 ppm or more, or 1,500 ppm or more based on the total weight of the lithium transition metal composite oxide, and may also be included in an amount of 3,000 ppm or less, 2,500 ppm or less, or 2,000 ppm or less based on the total weight of the lithium transition metal composite oxide.

[0142] According to one embodiment of the present invention, the yttrium (Y) may be included in an amount of 100 ppm to 2,000 ppm based on the total weight of the lithium transition metal composite oxide. As a specific example, the yttrium (Y) may be included in an amount of 100 ppm or more, 200 ppm or more, 300 ppm or more, 400 ppm or more, or 500 ppm or more based on the total weight of the lithium transition metal composite oxide, and may also be included in an amount of 2,000 ppm or less, 1,900 ppm or less, 1,800 ppm or less, 1,700 ppm or less, 1,600 ppm or less, or 1,500 ppm or less.

[0143] According to one embodiment of the present invention, the zirconium (Zr) may be included in an amount of 500 ppm to 5,000 ppm based on the total weight of the lithium transition metal composite oxide. As a specific example, the zirconium (Zr) may be included in an amount of 500 ppm or more, 1,000 ppm or more, or 1,500 ppm or more based on the total weight of the lithium transition metal composite oxide, and may also be included in an amount of 5,000 ppm or less, 4,500 ppm or less, 4,000 ppm or less, 3,500 ppm or less, or 3,000 ppm or less.

[0144] According to one embodiment of the present invention, the positive electrode active material may include a lithium transition metal composite oxide having an average composition represented by the following chemical formula 2.

[0145] [Chemical Formula 2]

[0146] Li x [Ni a Co b Mn c Al e Y f Zr g M 2 d ]O 2-y A y

[0147] In the above chemical formula 2, M 2 is at least one selected from the group consisting of B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, V, F, P and S, A is at least one selected from the group consisting of F, Cl, Br, I and S, 0.9≤x≤1.3, 0.6≤a<1.0, 0 <b<0.4, 0<c<0.4, 0≤d≤0.2, 0<e≤0.01, 0<f≤0.0006, 0<g≤0.0005, a+b+c+d+e+f+g=1, 0≤y≤0.2이다.

[0148] According to one embodiment of the present invention, in the chemical formula 2, x is a molar ratio of lithium to a transition metal in a lithium transition metal composite oxide, which may be 0.9 or more, 0.95 or more, or 1.0 or more, and may also be 1.1 or less, 1.07 or less, 1.05 or less, or 1.03 or less.

[0149] According to one embodiment of the present invention, in the chemical formula 2, a, b, c, d, e, f and g are each a transition metal, nickel (Ni), cobalt (Co), manganese (Mn), and a doping element (M). 2), aluminum (Al), yttrium (Y), and zirconium (Zr). As a specific example, the above a is a mole fraction of nickel (Ni) among transition metals, and may be 0.6 or more, 0.7 or more, 0.8 or more, 0.85 or more, 0.88 or more, 0.90 or more, 0.91 or more, 0.92 or more, 0.93 or more, 0.94 or more, 0.95 or more, or 0.96 or more, and may also be less than 1.0, 0.99 or less, 0.98 or less, 0.97 or less, or 0.96 or less. In addition, the above b is a mole fraction of cobalt (Co) among the transition metals, which may be greater than 0, 0.01 or more, 0.02 or more, or 0.03 or more, and may also be less than 0.4, 0.3 or less, 0.2 or less, 0.1 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, or 0.05 or less. The above c is a mole fraction of manganese (Mn) among the transition metals, which may be greater than 0, 0.01 or more, or 0.05 or more, and may also be less than 0.4, 0.3 or less, 0.2 or less, 0.1 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, or 0.05 or less. The above d is a doping element (M) among the transition metals. 2) as a mole fraction of 0, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, 0.10 or more, 0.11 or more, 0.12 or more, 0.13 or more, 0.14 or more, 0.15 or more, 0.16 or more, 0.17 or more, 0.18 or more, or 0.19 or more, and also less than 0.20, 0.19 or less, 0.18 or less, 0.17 or less, 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, 0.10 or less, 0.09 or less, 0.08 or less, It may be 0.07 or less, 0.06 or less, 0.05 or less, 0.04 or less, 0.03 or less, 0.02 or less, or 0.01 or less. The e is a mole fraction of aluminum (Al) among the transition metals, and may be greater than 0, 0.001 or more, 0.002 or more, 0.003 or more, 0.004 or more, or 0.005 or more, and may also be 0.01 or less, 0.009 or less, or 0.008 or less. The f is a mole fraction of yttrium (Y) among the transition metals, and may be greater than 0, 0.0001 or more, 0.0002 or more, or 0.0003 or more, and may also be 0.0006 or less, 0.0005 or less, or 0.0004 or less. The above g is a mole fraction of zirconium (Zr) among transition metals, and may be greater than 0, 0.0001 or more, or 0.0002 or more, and may also be 0.0005 or less, or 0.0004 or less.

[0150] According to one embodiment of the present invention, in the chemical formula 2, y is a molar ratio of the A element substituted for oxygen in the lithium transition metal composite oxide, which may be 0, more than 0, 0.01 or more, 0.02 or more, or 0.03 or more, and may also be 0.2 or less, 0.15 or less, or 0.1 or less.

[0151] According to one embodiment of the present invention, the positive electrode active material is aluminum (Al), zirconium (Zr) and M 3 It may include a lithium transition metal composite oxide including aluminum (Al), zirconium (Zr), and M. As a specific example, the positive electrode active material may include aluminum (Al), zirconium (Zr), and M. 3 It may contain as a doping element.

[0152] According to one embodiment of the present invention, the M 3 It can be a metallic element with an oxidation number of +4 or higher. As a specific example, the above M 3 It may be at least one selected from the group consisting of titanium (Ti), tantalum (Ta), tungsten (W), vanadium (V), molybdenum (Mo), and niobium (Nb).

[0153] According to one embodiment of the present invention, the aluminum (Al) may be included in an amount of 500 ppm to 3,000 ppm based on the total weight of the lithium transition metal composite oxide. As a specific example, the aluminum (Al) may be included in an amount of 500 ppm or more, 1,000 ppm or more, or 1,500 ppm or more based on the total weight of the lithium transition metal composite oxide, and may also be included in an amount of 3,000 ppm or less, 2,500 ppm or less, or 2,000 ppm or less based on the total weight of the lithium transition metal composite oxide.

[0154] According to one embodiment of the present invention, the zirconium (Zr) may be included in an amount of 500 ppm to 3,000 ppm based on the total weight of the lithium transition metal composite oxide. As a specific example, the zirconium (Zr) may be included in an amount of 500 ppm or more, 1,000 ppm or more, or 1,500 ppm or more based on the total weight of the lithium transition metal composite oxide, and may also be included in an amount of 3,000 ppm or less, 2,500 ppm or less, or 2,000 ppm or less based on the total weight of the lithium transition metal composite oxide.

[0155] According to one embodiment of the present invention, the M 3 Silver may be included in an amount of 100 ppm to 2,000 ppm based on the total weight of the lithium transition metal composite oxide. As a specific example, the M 3 Silver may be included in a content of 100 ppm or more, 200 ppm or more, 300 ppm or more, 400 ppm or more, or 500 ppm or more based on the total weight of the lithium transition metal composite oxide, and may also be included in a content of 2,000 ppm or less, 1,900 ppm or less, 1,800 ppm or less, 1,700 ppm or less, 1,600 ppm or less, or 1,500 ppm or less.

[0156] According to one embodiment of the present invention, the positive electrode active material includes a coating formed on at least one of a primary particle surface, a primary particle interface, and a secondary particle surface, and the coating may include at least one coating element selected from the group consisting of cobalt (Co) and boron (B).

[0157] According to one embodiment of the present invention, the coating portion may be an island-shaped coating portion formed on at least one portion of the primary particle surface, the primary particle interface, and the secondary particle surface.

[0158] According to one embodiment of the present invention, the coating portion may be a coating layer formed to surround at least one of a primary particle surface, a primary particle interface, and a secondary particle surface.

[0159] According to one embodiment of the present invention, the coating portion may include at least one coating portion among a coating portion including cobalt (Co), a coating portion including cobalt (Co) and boron (B), and a coating portion including boron (B).

[0160] According to one embodiment of the present invention, the coating portion may include a coating portion in which a coating portion including cobalt (Co), a coating portion including cobalt (Co) and boron (B), and a coating portion including boron (B) are sequentially formed.

[0161] According to one embodiment of the present invention, the coating portion may include cobalt-boron oxide.

[0162] According to one embodiment of the present invention, when the positive electrode active material is formed into a pellet by putting the positive electrode active material into a cylindrical mold having a diameter of 13 mm using an automatic pellet press and applying a force until a force equivalent to 9,000 kgf is reached, the rolling density calculated by the following equation 2 is 3.60 g / cm 3 It could be something like this.

[0163] [Formula 2]

[0164] Rolling density (g / cm) 3 ) = Positive active material weight (g) / Pellet volume (cm 3 )

[0165] According to one embodiment of the present invention, the positive electrode active material has a rolling density of 3.60 g / cm calculated by the above formula 2. 3 It may be more than that, and as a specific example, 3.61 g / cm 3 Above, 3.62 g / cm 3 Above, 3.63 g / cm 3 Above, 3.64 g / cm 3 Above, 3.65 g / cm 3 Above, 3.66 g / cm 3 Above, 3.67 g / cm 3 Above, 3.68 g / cm 3 Above, 3.69 g / cm 3 Above, 3.70 g / cm 3 or 3.71 g / cm 3 It may be more than 10.0 g / cm, and the upper limit is not particularly limited. 3 It could be as follows:

[0166] According to one embodiment of the present invention, the positive electrode active material may be a lithium secondary battery including a positive electrode including the positive electrode active material; a negative electrode; and a separator and an electrolyte interposed between the positive electrode and the negative electrode, wherein the discharge capacity when the lithium secondary battery is charged with a 0.5 C current and then discharged with a 0.1 C current is based on the discharge capacity when the lithium secondary battery is charged with a 0.5 C current and then discharged with a 1.0 C current, which may be 92.0% or more. Here, the lithium secondary battery is for confirming the discharge capacity according to the output characteristics of the positive electrode active material, and components other than the positive electrode active material are not particularly limited as long as they can be used in a lithium secondary battery. As a specific example, the positive electrode active material may have a discharge capacity of 92.0% or more, 92.1% or more, 92.2% or more, 92.3% or more, 92.4% or more, 92.5% or more, 92.6% or more, 92.7% or more, 92.8% or more, 92.9% or more, 93.0% or more, or 93.1% or more, based on the discharge capacity when the lithium secondary battery is charged with a 0.5 C current and then discharged with a 0.1 C current, and the upper limit is not particularly limited, but may be 100% or less.

[0167] According to one embodiment of the present invention, the positive electrode active material may be a lithium secondary battery including a positive electrode including the positive electrode active material; a negative electrode; and a separator and an electrolyte interposed between the positive electrode and the negative electrode, wherein the discharge capacity when the lithium secondary battery is charged with a 0.5 C current and then discharged with a 0.1 C current is based on the discharge capacity when the lithium secondary battery is charged with a 0.5 C current and then discharged with a 2.0 C current, which may be 89.0% or more. Here, the lithium secondary battery is for confirming the discharge capacity according to the output characteristics of the positive electrode active material, and components other than the positive electrode active material are not particularly limited as long as they can be used in the lithium secondary battery. As a specific example, the positive electrode active material may have a discharge capacity of 89.0% or more, 89.1% or more, 89.2% or more, 89.3% or more, 89.4% or more, 89.5% or more, 89.6% or more, 89.7% or more, 89.8% or more, 89.9% or more, 90.0% or more, 90.1% or more, 90.2% or more, 90.3% or more, or 90.4% or more, based on the discharge capacity when the lithium secondary battery is charged with a 0.5 C current and then discharged with a 0.1 C current, and the upper limit is not particularly limited, but may be 100% or less.

[0168] According to one embodiment of the present invention, when the volume value is calculated from the following equation 5 for each of the primary particles observed from the SEM image (measurement magnification 3,000 times) of the surface of the secondary particle, the single particle size (Dv) corresponding to the diameter of the volume at the point where the cumulative volume distribution of the primary particles is 50% 50 ) may be 1.2 ㎛ or more and 3.8 ㎛ or less.

[0169] [Formula 5]

[0170]

[0171] In the above equation 5,

[0172] The radius is the radius of the surface of the primary particle assuming that the surface of the primary particle is circular as observed from the SEM image (measurement magnification 3,000x) of the surface of the secondary particle.

[0173] As a specific example, the above cathode active material has the single particle degree (Dv 50 ) may be 1.2 ㎛ or more, 1.3 ㎛ or more, 1.4 ㎛ or more, 1.5 ㎛ or more, 1.6 ㎛ or more, or 1.65 ㎛ or more, and may also be 3.8 ㎛ or less, 3.7 ㎛ or less, 3.6 ㎛ or less, 3.59 ㎛ or less, 3.58 ㎛ or less, 3.57 ㎛ or less, 3.56 ㎛ or less, or 3.55 ㎛ or less.

[0174]

[0175] Method for manufacturing positive electrode active material

[0176] The present invention provides a method for manufacturing a positive electrode active material.

[0177] According to one embodiment of the present invention, the method for manufacturing the positive electrode active material may be a method for manufacturing the positive electrode active material described above.

[0178] According to one embodiment of the present invention, the method for manufacturing the positive electrode active material may be performed by including a step (S10) of mixing a positive electrode active material precursor including nickel, cobalt, and manganese and a lithium raw material, and performing firing to manufacture a fired product.

[0179] According to one embodiment of the present invention, the step (S10) may be performed by a method such as a method of dividing the temperature range within one firing step and performing firing (one-step method), a method of dividing the firing step into two steps (two-step method), and a method of performing plastic firing before dividing the temperature range within one firing step and performing firing (plastic firing method).

[0180] According to one embodiment of the present invention, the one-step method is a method of sequentially performing firing at two temperature ranges within one firing step, such that a single-stage firing may be performed on a mixture of a positive electrode active material precursor and a lithium raw material, and immediately thereafter, a second-stage firing may be performed by changing the temperature range. At this time, the second-stage firing may be performed at a lower temperature than the single-stage firing, and each firing temperature may be controlled according to the nickel content, and through such temperature control, the shape and size of the primary particles and the average particle diameter of the secondary particles may be controlled.

[0181] According to one embodiment of the present invention, the two-step method is a method that performs the first firing and the second firing separately, and can be performed by performing the first firing on a mixture of a positive electrode active material precursor and a lithium raw material, crushing a first fired product manufactured by the first firing, and then performing the second firing on the crushed product. At this time, the second firing can be performed at a lower temperature than the first firing, and each firing temperature can be controlled according to the nickel content, and through such temperature control, the shape and size of the primary particles and the average particle diameter of the secondary particles can be controlled.

[0182] According to one embodiment of the present invention, the sintering method is a method of performing sintering prior to one-step sintering, wherein sintering is performed on a mixture of a positive electrode active material precursor and a lithium raw material, and the one-step method is performed on the sintered product. At this time, the sintering may be performed at a lower temperature than the one-step sintering, and each sintering temperature may be controlled according to the nickel content, and through such temperature control, the shape and size of the primary particles and the average particle diameter of the secondary particles may be controlled.

[0183] According to one embodiment of the present invention, the positive electrode active material precursor may contain nickel in an amount of 60 mol% or more among the transition metals. As a specific example, the positive electrode active material precursor may be a transition metal hydroxide containing nickel, cobalt, and manganese, and containing nickel in an amount of 60 mol% or more among the transition metals. As a specific example, the transition metal hydroxide may have an average composition represented by the following chemical formula 3.

[0184] [Chemical Formula 3]

[0185] Ni a' Co b' Mn c'( OH)2

[0186] In the above chemical formula 3, 0.6≤a'<1.0, 0 <b'<0.4, 0<c'<0.4, a'+b'+c'=1이다.

[0187] According to one embodiment of the present invention, in the chemical formula 3, a', b', and c' may be mole fractions of nickel (Ni), cobalt (Co), and manganese (Mn), respectively, among transition metals. As a specific example, a' may be a mole fraction of nickel (Ni) among transition metals, and may be 0.6 or more, 0.7 or more, 0.8 or more, 0.85 or more, 0.88 or more, 0.90 or more, 0.91 or more, 0.92 or more, 0.93 or more, 0.94 or more, 0.95 or more, or 0.96 or more, and may also be less than 1.0, 0.99 or less, 0.98 or less, 0.97 or less, or 0.96 or less. In addition, the above b' may be a mole fraction of cobalt (Co) among transition metals, which may be greater than 0, 0.01, 0.02, or 0.03, and may also be less than 0.4, 0.3 or less, 0.2 or less, 0.1 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, or 0.05 or less. The above c' may be a mole fraction of manganese (Mn) among transition metals, which may be greater than 0, 0.01 or more, or 0.05 or more, and may also be less than 0.4, 0.3 or less, 0.2 or less, 0.1 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, or 0.05 or less.

[0188] According to one embodiment of the present invention, the lithium raw material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide or oxyhydroxide, and for example, Li2CO3, LiNO3, LiNO2, LiOH, LiOH H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7 or a mixture thereof.

[0189] According to one embodiment of the present invention, the step (S10) may be performed by further including one or more doping raw materials selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S and Y. The doping raw material may be an acetate, a nitrate, a sulfate, a halide, a sulfide, a hydroxide, an oxide or an oxyhydroxide containing the element, and specific examples thereof include Al2O3, Al(OH)3, Al(NO3)3·9H2O, Al2(SO4)3, Y2O3, It could be ZrO2, etc.

[0190] According to one embodiment of the present invention, the doping raw material may include Al, Y and Zr. In addition, the doping raw material may include Al, Zr and a metal element having an oxidation number of +4 or higher (M 3 ) may be included.

[0191] According to one embodiment of the present invention, when mixing the positive electrode active material precursor and the lithium raw material in the step (S10), the molar ratio (Li / M) of lithium (Li) of the lithium raw material to the transition metal (M) of the positive electrode active material precursor may be 0.9 or more and 1.3 or less. As a specific example, the Li / M may be 0.9 or more, 0.95 or more, or 1.0 or more, and further, 1.1 or less, 1.07 or less, 1.05 or less, or 1.04 or less, and the Li / M may be adjusted depending on the content of nickel in the transition metal.

[0192] According to one embodiment of the present invention, the method for manufacturing the positive electrode active material may further include a step (S20) of coating the positive electrode active material manufactured in step (S10). As a specific example, step (S20) may be performed by including at least one coating raw material selected from the group consisting of Co and B. In addition, step (S20) may be performed by further including an Al coating raw material.

[0193] According to one embodiment of the present invention, the coating of step (S20) may be performed by coating each coating raw material simultaneously, or may be performed sequentially. As a specific example, the coating of step (S20) may be performed by including a step (S21) of mixing Co coating raw material and Al coating raw material into the positive active material and heat-treating them, and a step (S22) of mixing B coating raw material into the coated product manufactured in step (S21) and heat-treating them.

[0194] According to one embodiment of the present invention, the Co coating raw material may be a cobalt hydroxide such as Co(OH)2, the Al coating raw material may be an aluminum hydroxide such as Al(OH)3, and the B coating raw material may be H3BO3.

[0195] According to one embodiment of the present invention, the method for manufacturing the positive electrode active material may include, when performing steps (S10) and (S20), a step of crushing the sintered product after firing, if necessary, and the crushing may be performed without particular limitation using a crushing device capable of crushing the positive electrode active material.

[0196] According to one embodiment of the present invention, the doping raw material and the coating raw material can be introduced by adjusting them to satisfy the doping element content and coating element content of the positive electrode active material described above.

[0197]

[0198] anode

[0199] The present invention provides a positive electrode comprising the positive electrode active material.

[0200] According to one embodiment of the present invention, the positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and the positive electrode active material layer may include the positive electrode active material.

[0201] According to one embodiment of the present invention, the positive electrode current collector may include a highly conductive metal, and is not particularly limited as long as it is easily adhered to by the positive electrode active material layer and does not react within the voltage range of the battery. The positive electrode current collector may be made of, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode current collector may typically have a thickness of 3 ㎛ to 500 ㎛, and fine unevenness may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0202] According to one embodiment of the present invention, the positive electrode active material layer may optionally include a conductive material and a binder, together with the positive electrode active material, as needed. In this case, the positive electrode active material may be included in an amount of 80 wt% to 99 wt%, more specifically 85 wt% to 98.5 wt%, based on the total weight of the positive electrode active material layer, and excellent capacity characteristics may be exhibited within this range.

[0203] According to one embodiment of the present invention, the conductive material is used to provide conductivity to the electrode, and in the battery to be formed, any conductive material that does not cause a chemical change and has electronic conductivity can be used without particular limitation. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive tubes such as carbon nanotubes; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used. The conductive material may be included in an amount of 0.1 wt% to 15 wt% based on the total weight of the positive electrode active material layer.

[0204] According to one embodiment of the present invention, the binder serves to improve adhesion between positive electrode active material particles and adhesion between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylalcohol, polyacrylonitrile, polymethyl methacrylate, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, polyacrylic acid, and polymers in which hydrogens of these are substituted with Li, Na, or Ca, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The above binder may be included in an amount of 0.1 wt% to 15 wt% based on the total weight of the positive electrode active material layer.

[0205] According to one embodiment of the present invention, the positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the positive electrode active material described above is used. Specifically, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer, which is manufactured by dissolving or dispersing the positive electrode active material and optionally a binder, a conductive material, and a dispersant in a solvent as needed, onto a positive electrode current collector, followed by drying and rolling, or by casting the composition for forming a positive electrode active material layer onto a separate support, and then laminating the film obtained by peeling it from the support onto a positive electrode current collector.

[0206] According to one embodiment of the present invention, the solvent may be a solvent generally used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), dimethylformamide (DMF), acetone, or water, and one of these may be used alone or as a mixture of two or more. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, binder, and dispersant in consideration of the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.

[0207]

[0208] lithium secondary battery

[0209] The present invention provides a lithium secondary battery including the positive electrode.

[0210]

[0211] According to one embodiment of the present invention, the lithium secondary battery may include the positive electrode; the negative electrode; a separator interposed between the positive electrode and the negative electrode; and an electrolyte. In addition, the lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0212] According to one embodiment of the present invention, the negative electrode may include a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.

[0213] According to one embodiment of the present invention, the negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 ㎛ to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0214] According to one embodiment of the present invention, the negative electrode active material layer may optionally include a binder and a conductive material together with the negative electrode active material.

[0215] According to one embodiment of the present invention, a compound capable of reversible intercalation and deintercalation of lithium may be used as the negative electrode active material. Specific examples thereof include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, and Al alloy; metallic oxides capable of doping and dedoping lithium, such as SiOβ (0<β<2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more thereof may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical or fibrous shapes, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes. The negative electrode active material may be included in an amount of 80 wt% to 99 wt% based on the total weight of the negative electrode active material layer.

[0216] According to one embodiment of the present invention, the binder of the negative electrode active material layer is a component that assists in bonding between the conductive material, the active material, and the current collector, and is typically added in an amount of 0.1 wt% to 10 wt% based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0217] According to one embodiment of the present invention, the conductive material of the negative electrode active material layer is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10 wt% or less, preferably 5 wt% or less, based on the total weight of the negative electrode active material layer. The conductive material is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; fluorinated carbon; metal powder such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0218] According to one embodiment of the present invention, the negative electrode can be manufactured by applying and drying a composition for forming a negative electrode active material layer, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, on a negative electrode current collector, or by casting the composition for forming a negative electrode active material layer on a separate support, and then laminating the film obtained by peeling it off from the support on a negative electrode current collector.

[0219] According to one embodiment of the present invention, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in lithium secondary batteries can be used without particular limitation, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.

[0220] According to one embodiment of the present invention, the electrolyte may include, but is not limited to, an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, etc. that can be used in the manufacture of a lithium secondary battery. As a specific example, the electrolyte may include an organic solvent and a lithium salt.

[0221] According to one embodiment of the present invention, the organic solvent may be used without particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylenecarbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.

[0222] According to one embodiment of the present invention, the lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the anion of the lithium salt is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - At least one selected from the group consisting of may be used, and the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. It is preferable to use the concentration of the lithium salt within the range of 0.1 M to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0223] According to one embodiment of the present invention, in addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 wt% to 5 wt% based on the total weight of the electrolyte.

[0224]

[0225] A lithium secondary battery including a cathode active material according to the present invention stably exhibits excellent capacity characteristics, output characteristics, and life characteristics, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs) and electric vehicles (EVs).

[0226] There is no particular limitation on the external shape of the lithium secondary battery of the present invention, but it may be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.

[0227] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but can also be preferably used as a unit battery in a medium- to large-sized battery module including a plurality of battery cells.

[0228] Accordingly, according to one embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.

[0229] According to one embodiment of the present invention, the battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0230]

[0231] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0232]

[0233] Examples and Comparative Examples

[0234] Example 1

[0235] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.89 Co 0.03 Mn 0.08 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 10.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.04. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0236] The above mixture was fired under an oxygen atmosphere at 850°C for 6 hours and then at 800°C for 9 hours to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 9.8 ㎛, and LiNi 0.8833Co 0.0298 Mn 0.0794 Al 0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0237] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 740°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8641 Co 0.0491 Mn 0.0777 Al 0.0066 Y 0.0010 Zr 0.0015 It was O2.

[0238] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8602 Co 0.0489 Mn 0.0773 Al 0.0066 Y 0.0010 Zr 0.0015 B 0.0045 It was O2.

[0239]

[0240] Example 2

[0241] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.89 Co 0.03 Mn 0.08 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 10.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.00. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0242] The above mixture was first fired at 850°C for 6 hours under an oxygen atmosphere to obtain a first fired product. Thereafter, the first fired product was subjected to a first firing at room temperature to obtain an average particle diameter (D 50 ) was ground to 9.8 ㎛.

[0243] The above-mentioned pulverized first fired product and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 0.04, and the second fired product was obtained by secondary firing at 800°C for 9 hours under an oxygen atmosphere. The second fired product was pulverized at room temperature to obtain an average particle diameter (D 50 ) is 9.8 ㎛, and LiNi0.8833 Co 0.0298 Mn 0.0794 Al 0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0244] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 740°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8641 Co 0.0491 Mn 0.0777 Al 0.0066 Y 0.0010 Zr 0.0015 It was O2.

[0245] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8602 Co 0.0489 Mn 0.0773 Al 0.0066 Y 0.0010 Zr 0.0015 B 0.0045 It was O2.

[0246]

[0247] Example 3

[0248] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.89 Co 0.03 Mn 0.08 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 10.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.04. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0249] The above mixture was calcined at 550°C for 5 hours under an oxygen atmosphere to obtain a calcined product. Afterwards, the calcined product was calcined at room temperature to obtain an average particle diameter (D 50 ) was ground to 9.8 ㎛.

[0250] The above-mentioned pulverized plastic product was fired at 850°C for 6 hours and then at 800°C for 9 hours in an oxygen atmosphere to obtain a sintered product. The sintered product was pulverized at room temperature to obtain an average particle size (D 50 ) is 9.8 ㎛, and LiNi 0.8833 Co 0.0298 Mn 0.0794 Al 0.0050 Y0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0251] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 740°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8641 Co 0.0491 Mn 0.0777 Al 0.0066 Y 0.0010 Zr 0.0015 It was O2.

[0252] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8602 Co0.0489 Mn 0.0773 Al 0.0066 Y 0.0010 Zr 0.0015 B 0.0045 It was O2.

[0253]

[0254] Example 4

[0255] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.89 Co 0.03 Mn 0.08 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 10.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.04. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0256] The above mixture was fired under an oxygen atmosphere at 880°C for 6 hours and then at 800°C for 9 hours to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 9.8 ㎛, and LiNi 0.8833 Co 0.0298 Mn 0.0794 Al 0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0257] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 740°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8641 Co 0.0491 Mn 0.0777 Al 0.0066 Y 0.0010 Zr 0.0015 It was O2.

[0258] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8602 Co 0.0489 Mn 0.0773 Al 0.0066 Y 0.0010 Zr 0.0015 B 0.0045 It was O2.

[0259]

[0260] Example 5

[0261] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.89 Co 0.03 Mn 0.08 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 10.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.04. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 2,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0262] The above mixture was fired under an oxygen atmosphere at 850°C for 6 hours and then at 800°C for 9 hours to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 9.8 ㎛, and LiNi 0.8824 Co 0.0297 Mn 0.0793 Al 0.0050 Y 0.0021 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0263] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 740°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8632 Co 0.0491 Mn 0.0776 Al 0.0066 Y 0.0020 Zr 0.0015 It was O2.

[0264] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8593 Co 0.0489 Mn 0.0772 Al 0.0066 Y 0.0020 Zr 0.0015 B 0.0045 It was O2.

[0265]

[0266] Example 6

[0267] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.89 Co 0.03 Mn 0.08 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 10.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.04. Here, Al(OH)3 was added in an amount of 2,940 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0268] The above mixture was fired under an oxygen atmosphere at 850°C for 6 hours and then at 800°C for 9 hours to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 9.8 ㎛, and LiNi 0.8789 Co 0.0296 Mn 0.0790 Al 0.0100 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0269] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 740°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8597 Co 0.0490 Mn 0.0773 Al 0.0115 Y 0.0010 Zr 0.0015 It was O2.

[0270] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8559 Co 0.0488 Mn 0.0769 Al 0.0115 Y 0.0010 Zr 0.0014 B 0.0045 It was O2.

[0271]

[0272] Example 7

[0273] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.89 Co 0.03 Mn 0.08 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 10.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.04. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 3,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0274] The above mixture was fired under an oxygen atmosphere at 850°C for 6 hours and then at 800°C for 9 hours to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 9.8 ㎛, and LiNi 0.8815 Co 0.0297 Mn 0.0793 Al 0.0050 Y 0.0010 Zr 0.0035 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0275] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 740°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8623 Co 0.0491 Mn 0.0775 Al 0.0066 Y 0.0010 Zr 0.0035 It was O2.

[0276] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8584 Co 0.0489 Mn 0.0772 Al 0.0066 Y 0.0010 Zr 0.0034 B 0.0045 It was O2.

[0277]

[0278] Example 8

[0279] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.96 Co 0.03 Mn 0.01 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 14.5 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.02. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0280] The above mixture was fired under an oxygen atmosphere at 800°C for 6 hours and then at 760°C for 9 hours to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 14.2 ㎛, and LiNi 0.9528 Co 0.0298 Mn 0.0099 Al 0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0281] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to the metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 700°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 14.5 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.9320 Co 0.0491 Mn 0.0097 Al 0.0067 Y 0.0010 Zr 0.0015 It was O2.

[0282] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50 ) was pulverized to 14.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.9278 Co 0.0489 Mn 0.0097 Al 0.0066 Y 0.0010 Zr 0.0015 B 0.0045 It was O2.

[0283]

[0284] Example 9

[0285] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.96 Co 0.03 Mn 0.01 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 14.5 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 0.98. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0286] The above mixture was first fired at 800°C for 6 hours under an oxygen atmosphere to obtain a first fired product. Thereafter, the first fired product was subjected to a first firing at room temperature to obtain an average particle diameter (D 50 ) was ground to 14.2 ㎛.

[0287]

[0288] *227 The above-mentioned pulverized first fired product and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 0.04, and the second fired product was obtained by firing the product for a second time at 760°C for 9 hours under an oxygen atmosphere. The second fired product was pulverized at room temperature to obtain an average particle diameter (D 50 ) is 14.2 ㎛, and LiNi 0.9528 Co 0.0298 Mn 0.0099 Al 0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0289] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to the metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 700°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 14.5 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.9320 Co 0.0491 Mn 0.0097 Al 0.0067 Y 0.0010 Zr 0.0015 It was O2.

[0290] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50 ) was pulverized to 14.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.9278 Co 0.0489 Mn 0.0097 Al 0.0066 Y 0.0010 Zr 0.0015 B 0.0045 It was O2.

[0291]

[0292] Example 10

[0293] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.96 Co 0.03 Mn 0.01 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 14.5 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.02. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0294] The above mixture was calcined at 550°C for 5 hours under an oxygen atmosphere to obtain a calcined product. Afterwards, the calcined product was calcined at room temperature to obtain an average particle diameter (D 50 ) was ground to 14.2 ㎛.

[0295] The above-mentioned pulverized plastic product was fired at 800°C for 6 hours and then at 760°C for 9 hours in an oxygen atmosphere to obtain a sintered product. The sintered product was pulverized at room temperature to obtain an average particle size (D 50 ) is 14.2 ㎛, and LiNi 0.9528 Co 0.0298 Mn 0.0099 Al 0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0296] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to the metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 700°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 14.5 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.9320 Co 0.0491 Mn 0.0097 Al 0.0067 Y 0.0010 Zr 0.0015 It was O2.

[0297] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50 ) was pulverized to 14.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.9278 Co 0.0489 Mn 0.0097 Al 0.0066 Y 0.0010 Zr 0.0015 B 0.0045 It was O2.

[0298]

[0299] Example 11

[0300] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.96 Co 0.03 Mn 0.01 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 14.5 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.02. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0301] The above mixture was fired under an oxygen atmosphere at 830°C for 6 hours and then at 760°C for 9 hours to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 14.2 ㎛, and LiNi 0.9528 Co 0.0298 Mn 0.0099 Al 0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was manufactured.

[0302] The lithium transition metal oxide in the form of secondary particles manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of secondary particles manufactured above so that the molar ratio of cobalt (Co) to the metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 700°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a first coated product. At room temperature, the first coated product had an average particle diameter (D 50 ) was pulverized to 14.5 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.9320 Co 0.0491 Mn 0.0097 Al 0.0067 Y 0.0010 Zr 0.0015 It was O2.

[0303] To the above-mentioned pulverized first coating product, H3BO3 was added in an amount of 500 ppm based on the total weight of the above-mentioned pulverized first coating product and mixed to prepare a mixture. The mixture was heat-treated at 330°C for 5 hours under an air atmosphere to obtain a second coating product. At room temperature, the second coating product had an average particle diameter (D 50 ) was pulverized to 14.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co, Al, and B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.9278 Co 0.0489 Mn 0.0097 Al 0.0066 Y 0.0010 Zr 0.0015 B 0.0045 It was O2.

[0304]

[0305] Comparative Example 1

[0306] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.87 Co 0.05 Mn 0.08 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 10.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.05. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0307] The above mixture was fired at 780°C for 5 hours under an oxygen atmosphere to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 9.8 ㎛, and LiNi 0.8635 Co 0.0496 Mn 0.0794 Al 0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was prepared. Subsequently, 100 parts by weight of the lithium transition metal oxide in the form of secondary particles prepared above and 100 parts by weight of water were stirred for 5 minutes, and then washed using a filter press. The washed product was dried at 130°C for 4 hours to prepare a dried product.

[0308] To the above-mentioned manufactured dry product, H3BO3 was added in an amount of 1,000 ppm based on the total weight of the lithium transition metal oxide and mixed to prepare a mixture. The mixture was heat-treated at 300°C for 5 hours under an air atmosphere to obtain a coating product. At room temperature, the coating product had an average particle diameter (D 50) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8558 Co 0.0492 Mn 0.0787 Al 0.0049 Y 0.0010 Zr 0.0015 B 0.0089 It was O2.

[0309]

[0310] Comparative Example 2

[0311] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.87 Co 0.05 Mn 0.08 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 12.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.05. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0312] The above mixture was fired at 780°C for 5 hours under an oxygen atmosphere to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 11.8 ㎛, and LiNi 0.8635 Co 0.0496 Mn 0.0794 Al 0.0050 Y 0.0010 Zr 0.0015A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was prepared. Subsequently, 100 parts by weight of the lithium transition metal oxide in the form of secondary particles prepared above and 100 parts by weight of water were stirred for 5 minutes, and then washed using a filter press. The washed product was dried at 130°C for 4 hours to prepare a dried product.

[0313] To the above-mentioned manufactured dry product, H3BO3 was added in an amount of 1,000 ppm based on the total weight of the lithium transition metal oxide and mixed to prepare a mixture. The mixture was heat-treated at 300°C for 5 hours under an air atmosphere to obtain a coating product. At room temperature, the coating product had an average particle diameter (D 50 ) was pulverized to 12.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8558 Co 0.0492 Mn 0.0787 Al 0.0049 Y 0.0010 Zr 0.0015 B 0.0089 It was O2.

[0314]

[0315] Comparative Example 3

[0316] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.94 Co 0.05 Mn 0.01 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50: 14.5 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.02. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0317] The above mixture was fired at 730°C for 5 hours under an oxygen atmosphere to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 14.2 ㎛, and LiNi 0.9330 Co 0.0496 Mn 0.0099 Al 0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was prepared. Subsequently, 100 parts by weight of the lithium transition metal oxide in the form of secondary particles prepared above and 100 parts by weight of water were stirred for 5 minutes, and then washed using a filter press. The washed product was dried at 130°C for 4 hours to prepare a dried product.

[0318] To the above-mentioned manufactured dry product, H3BO3 was added in an amount of 1,000 ppm based on the total weight of the lithium transition metal oxide and mixed to prepare a mixture. The mixture was heat-treated at 300°C for 5 hours under an air atmosphere to obtain a coating product. At room temperature, the coating product had an average particle diameter (D 50 ) was pulverized to 14.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.9246 Co 0.0492 Mn 0.0098 Al 0.0050 Y 0.0010 Zr 0.0015 B0.0089 It was O2.

[0319]

[0320] Comparative Example 4

[0321] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.94 Co 0.05 Mn 0.01 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 10.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.02. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0322] The above mixture was fired at 730°C for 5 hours under an oxygen atmosphere to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 9.8 ㎛, and LiNi 0.9330 Co 0.0496 Mn 0.0099 Al 0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide having a composition represented by O2 and in the form of secondary particles in which primary particles are aggregated was prepared. Subsequently, 100 parts by weight of the lithium transition metal oxide in the form of secondary particles prepared above and 100 parts by weight of water were stirred for 5 minutes, and then washed using a filter press. The washed product was dried at 130°C for 4 hours to prepare a dried product.

[0323] To the above-mentioned manufactured dry product, H3BO3 was added in an amount of 1,000 ppm based on the total weight of the lithium transition metal oxide and mixed to prepare a mixture. The mixture was heat-treated at 300°C for 5 hours under an air atmosphere to obtain a coating product. At room temperature, the coating product had an average particle diameter (D 50 ) was pulverized to 10.2 ㎛, and a positive electrode active material was manufactured in which a coating portion including B was formed on a lithium transition metal oxide in the form of secondary particles in which primary particles were aggregated. The overall composition of the positive electrode active material including the coating portion was LiNi 0.9246 Co 0.0492 Mn 0.0098 Al 0.0050 Y 0.0010 Zr 0.0015 B 0.0089 It was O2.

[0324]

[0325] Comparative Example 5

[0326] Ni is a secondary particle formed by the agglomeration of tens to hundreds of primary particles. 0.89 Co 0.03 Mn 0.08 Transition metal complex hydroxides (D) having a composition represented by (OH)2 50 : 4.2 ㎛) and LiOH were mixed so that the molar ratio of lithium (Li) to transition metal (Ni+Co+Mn) (Li / (Ni+Co+Mn)) was 1.04. Here, Al(OH)3 was added in an amount of 1,470 ppm, Y2O3 in an amount of 1,000 ppm, and ZrO2 in an amount of 1,500 ppm based on the total weight of the transition metal composite hydroxide, and mixed to prepare a mixture.

[0327] The above mixture was fired under an oxygen atmosphere at 930°C for 6 hours and then at 830°C for 9 hours to obtain a fired product. The fired product was pulverized at room temperature to obtain an average particle size (D 50 ) is 3.8 ㎛, and LiNi 0.8833 Co 0.0298 Mn 0.0794 Al0.0050 Y 0.0010 Zr 0.0015 A lithium transition metal oxide in the form of a single particle was prepared, having a composition represented by O2.

[0328] The lithium transition metal oxide in the form of a single particle manufactured above and Al(OH)3 were added in an amount of 500 ppm based on the total weight of the lithium transition metal oxide in the form of a single particle manufactured above so that the molar ratio of cobalt (Co) to the metal (Ni+Co+Mn+Al+Y+Zr) excluding lithium (Co / (Ni+Co+Mn+Al+Y+Zr)) was 0.02, and were uniformly mixed to prepare a mixture. The mixture was heat-treated at 740°C for 3 hours and then at 500°C for 3 hours under an oxygen atmosphere to obtain a coating product. At room temperature, the coating product had an average particle diameter (D 50 ) was pulverized to 3.8 ㎛, and a positive electrode active material was manufactured in which a coating portion including Co and Al was formed on a lithium transition metal oxide in the form of a single particle. The overall composition of the positive electrode active material including the coating portion was LiNi 0.8641 Co 0.0491 Mn 0.0777 Al 0.0066 Y 0.0010 Zr 0.0015 It was O2.

[0329]

[0330] Experimental example

[0331] Experimental Example 1: Particle Analysis 1

[0332] The positive electrode active materials manufactured in Examples 1 to 11 and Comparative Examples 1 to 5 were photographed using a scanning electron microscope (FEI quanta250 FEG), and the SEM images of Examples 1 to 11 are sequentially shown in Figs. 1 to 11 (A), and the SEM images of Comparative Examples 1 to 5 are sequentially shown in Figs. 12 to 16 (A). From the SEM images, the average particle size of the primary particles present in each of the Examples and Comparative Examples was measured, and is shown in Table 1 below.

[0333] And, after ion milling each of the positive electrode active materials manufactured in Examples 1 to 11 and Comparative Examples 1 to 5, they were photographed using a scanning electron microscope, and the SEM images of Examples 1 to 11 are sequentially shown in (B) of Figs. 1 to 11, respectively, and the SEM images of Comparative Examples 1 to 5 are sequentially shown in (B) of Figs. 12 to 16, respectively. In (B) of Figs. 1 to 15, the white squares indicate the size of the cross-section of the secondary particles observed from the SEM images of the cross-sections of the secondary particles photographed for the cross-sections of the positive electrode active materials, where the average particle diameter (D) of the secondary particles 50 ) For the SEM image of the cross-section of the secondary particle having a size within the range, a unit area of ​​5 ㎛ in width and 5 ㎛ in length is set within the cross-section of the secondary particle, and the number of cross-sections of the primary particle confirmed within the unit area is shown in Table 1 below.

[0334] In addition, a segmentation image showing multiple lithium composite transition metal oxides segmented by performing image analysis based on an artificial intelligence model from the SEM image of Example 1 of the present invention is shown in FIG. 17, and a segmentation image of Comparative Example 1 is shown in FIG. 18.

[0335]

[0336] Average particle size of primary particles measured from SEM images (㎛) Number of cross-sections of primary particles in unit area Example 12.513 Example 22.718 Example 32.822 Example 43.210 Example 52.68 Example 62.415 Example 72.611 Example 81.713 Example 91.814 Example 101.924 Example 112.119 Comparative Example 1 < 0.5120 Comparative Example 2 < 0.5161 Comparative Example 3 < 0.5145 Comparative Example 4 < 0.5127 Comparative Example 54.0-

[0337] Experimental Example 2: Particle Analysis 2

[0338] The positive electrode active materials manufactured in Examples 1, 2, and 8 were each subjected to ion milling, and then photographed using a transmission electron microscope (FEI Titan cubed G2 60-300). TEM images of the cross-sections of the primary particles of the positive electrode active materials of Examples 1, 2, and 8 are shown in FIGS. 19 to 21, respectively, in that order.

[0339]

[0340] Referring to FIGS. 1 to 11 and Table 1, in the case of the positive electrode active materials of Examples 1 to 11, it can be confirmed that a plurality of primary particles include aggregated secondary particles, and that the plurality of primary particles have an average particle size of 1.5 μm or more and 5.0 μm or less as measured from an SEM image. In addition, it can be confirmed that the plurality of primary particles include three or more disk-type primary particles. At this time, the disk-type primary particles refer to primary particles in which, when two imaginary tangent lines having the largest number of contact points are drawn for two boundaries of primary particles existing within an angle of 45° or less based on the major axis direction in the primary particle observed from an SEM image of the surface or cross-section of the secondary particle, the imaginary line crossing the two tangent lines is drawn, and the same-sided internal angle is 150° or more and 210° or less. For reference, when drawing virtual yellow tangent lines with the most contact points for each of the two boundary lines of the primary particles existing within an angle of 45° or less based on the major axis direction in red in (B) of FIGS. 1 to 11, one virtual line (not shown) crossing the two yellow tangent lines satisfies the condition that the same internal angle is 150° or more and 210° or less, and the primary particles corresponding to this case are defined as disk-shaped primary particles. In addition, it can be confirmed that the disk-shaped primary particles have a minor axis of 0.3 ㎛ or more and an aspect ratio (major axis / minor axis) of 1.5 or more. In addition, it can be confirmed that the number of cross-sections of the primary particles per unit area is 1 or more and 100 or less. Specifically, it can be confirmed that the number of cross-sections of the primary particles per unit area is 8 or more and 24 or less.

[0341] In addition, referring to FIGS. 1 to 11 and 19 to 21, in the case of the positive electrode active material according to one embodiment of the present invention, it can be confirmed that the area ratio of the (003) plane among the crystal planes on the surface of the primary particle is the largest.

[0342] Meanwhile, in the case of the positive electrode active materials of Comparative Examples 1 to 4, it can be confirmed that the average particle size of the primary particles measured from the SEM image is small, less than 500 nm. In addition, in the case of the positive electrode active material of Comparative Example 5, it can be confirmed that it does not contain the disk-shaped primary particles.

[0343] And, referring to FIGS. 17 and 18, it can be confirmed that the positive electrode active material according to one embodiment of the present invention includes single crystal primary particles.

[0344]

[0345] Experimental Example 3: Particle Analysis 3

[0346] The positive electrode active materials manufactured in Examples 1 to 11 and Comparative Examples 1 to 5 were photographed using a scanning electron microscope equipped with EBSD (FEI quanta250 FEG).

[0347] Among these, the size of the cross-section of the secondary particles observed from the backscattered electron diffraction (EBSD) pattern of the SEM image of the cross-section of the secondary particles photographed for the cross-section of the positive electrode active materials of Examples 1 to 4, 8, 10, 11 and Comparative Example 3 (measured under the conditions of acceleration voltage 20 kV, WD 16 mm, measurement magnification 5,000 times (width 16 ㎛ * height 16 ㎛), step size 0.025 ㎛) is the average particle diameter (D) of the secondary particles. 50) for the EBSD pattern of the cross-section of the secondary particle having a size within the range, a unit area of ​​5 ㎛ in width and 5 ㎛ in length was set in the central region and the outer region within the cross-section of the secondary particle, respectively, and is shown in Fig. 22 (Example 1), Fig. 23 (Example 2), Fig. 24 (Example 3), Fig. 25 (Example 4), Fig. 26 (Example 8), Fig. 27 (Example 10), Fig. 28 (Example 11), and Fig. 29 (Comparative Example 3), and the number of cross-sections of grains confirmed within the unit area and the degree of single crystallinity were calculated according to the following Equation 1 and are shown together in Table 2 below.

[0348] [Formula 1]

[0349]

[0350]

[0351] Number of cross-sections of grains within a unit area of ​​the central region Number of cross-sections of grains within a unit area of ​​the outer region Single crystallinity (㎛) 3 )Example 112140.86Example 2360.90Example 3890.92Example 4660.98Example 5--0.87Example 6--0.87Example 7--0.88Example 812191.09Example 9--1.20Example 10791.57Example 1112131.56Comparative Example 1--0.046Comparative Example 2--0.040Comparative Example 32031800.050Comparative Example 4--0.070Comparative Example 5--3.1

[0352] Referring to Table 2, it can be confirmed that the number of cross-sections of grains per unit area of ​​the positive electrode active materials of Examples 1 to 11 is 1 or more and 150 or less. Specifically, it can be confirmed that the number of cross-sections of grains per unit area is 3 or more and 19 or less. In addition, the single crystallinity is 0.15 ㎛. 3 It can be confirmed that the ideal is 0.86 ㎛. Specifically, the single crystallinity is 0.86 ㎛. 3 Above, 1.57 ㎛ 3 You can see the following.

[0353]

[0354] Experimental Example 4: Particle Analysis 4

[0355] From the SEM image of the positive electrode active material obtained in the above Experimental Example 1, the single particle diameter (Dv) corresponding to the volume diameter at the point where the volume cumulative distribution of the primary particles present in each of the examples and comparative examples is 50% 50 ) were measured and shown in Table 3 below.

[0356] Specifically, the area of ​​each primary particle is measured through the number of pixels corresponding to each of n primary particles observed from the image projected on a two-dimensional plane from the SEM images of the surfaces of the secondary particles photographed on the surfaces of the positive electrode active materials of Examples 1 to 11 and Comparative Examples 1 to 5. Then, assuming that the surface of the primary particle is circular, that is, using the radius of a circle having the same area as the surface area of ​​each of the primary particles, the radius of the surface of the primary particle was derived. Using the radius, the volume value is calculated according to the following Equation 5, and the single particle size (Dv) corresponding to the diameter of the volume at the point where the cumulative volume distribution of the primary particles is 50% 50 ) was calculated and shown in Table 3 below.

[0357] [Formula 5]

[0358]

[0359]

[0360] Discriminant particle size (Dv) 50 ) (㎛) Example 12.23 Example 22.24 Example 32.26 Example 43.51 Example 52.34 Example 62.21 Example 72.33 Example 81.69 Example 91.70 Example 101.72 Example 112.83 Comparative Example 11.05 Comparative Example 21.01 Comparative Example 30.80 Comparative Example 40.87 Comparative Example 53.48

[0361] Referring to Table 3, it can be confirmed that the single particle size of the positive electrode active materials of Examples 1 to 11 is 1.2 ㎛ or more and 3.8 ㎛ or less. Specifically, it can be confirmed that the single particle size is 1.65 ㎛ or more and 3.55 ㎛ or less.

[0362]

[0363] Experimental Example 5: Particle Analysis 5

[0364] For the positive electrode active materials manufactured in Examples 1 to 11 and Comparative Examples 1 to 4, electron spectroscopy chemical analysis (ESCA) was performed using a K-alpha XPS device from Thermo Fisher to analyze the element distribution of the Co and B coating layers present on the surface. For depth profiling, etching was performed at a rate of 0.3 nm / 10 s using an Ar ion source, and the contents (atomic %) of B and Co, respectively, included in the coating layers with a thickness of 0 to 100 nm were measured, and the results are shown in Tables 4 (B coating layer) and 5 (Co coating layer), respectively.

[0365] EPMA cross-sectional analysis was performed to confirm the surface coating characteristics of the positive electrode active material of Example 1. First, the positive electrode active material of Example 1, carbon black conductive agent, and PVDF binder were mixed in a weight ratio of 95:2:3 in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry. The prepared positive electrode slurry was applied to one surface of an aluminum current collector, dried at 130°C, and rolled to an electrode porosity of 20% to prepare a positive electrode. In order to create a flat surface for EPMA cross-sectional analysis, the positive electrode was subjected to Ar-ion milling using a HITACHI IM-5000 equipment at an acceleration voltage of 6 kV to obtain a cross-section of the positive electrode sample. Then, the cross-sectional image of the positive electrode sample was observed using a JEOL JXA-iHP200F equipment at an acceleration voltage of 15 kV and a probe current of 50 nA, and is shown in Fig. 30.

[0366]

[0367] Etching time (s) 0 1 0 3 0 5 0 1 0 2 0 0 3 0 0 5 0 0 1 0 0 2 0 0 3 0 0 0 Example 1 1 0.4 1 0.7 9.4 8.4 6.6 4.3 3.4 2.4 1.6 1.3 1 Example 2 1 1 1 0.8 9.4 8.1 6.5 4.3 3.7 2.8 1.9 1.1 1 Example 3 1 0.4 1 0.8 9.4 8.9 6.7 4.3 3.7 2.4 1.7 1.2 1 Example 4 1 0.4 1 0.2 9.2 6.8 4.8 3.5 2.8 1.8 1.5 1 Example 5 1 0.4 1 0.7 9.9 8.1 6.7 4.5 3.4 2.9 1.1 1.5 1 Example 610.410.19.28.26.14.43.82.81.21.51Example 710.410.89.78.46.2432.41.51.21Example 811.211.29.18.76.84.23.12.91.91.41Example 910.710.79.18.16.44.932.81.71.51Example 1010.710.89.486.44.23.42.51.81.51Example 111111.29.28.76.14.53.72.91.91.51Comparative Example 116.417.515.114.811.88.975.93.52.41.5Comparative Example 21617.514.814.8128.77.85.1321Comparative Example 31616.815.114.811.48.87.55.93.51.91.5Comparative Example 415.416.41514.811.28.775.53.821.1

[0368] Etching time (s) 0 1 0 3 0 5 0 1 0 2 0 0 3 0 0 5 0 0 1 0 0 2 0 0 3 0 0 0 Example 1 1 8 3 4 5 5 4 5 9 4 8 3 9 2 2 1 ... 622.84.25.55.94.83.720.90.70.8Example 71.82.74.55.45.54.93.82.11.10.90.6Example 81.634.55.35.94.53.52.21.310.7Example 91.73.14.25.35.94.83.82.111.10.9Example 1023.14.45.164.93.921.20.90.8Example 111.93.34.55.16.14.942.10.91.10.7Comparative Example 100.10.10.30.30.30.40.80.90.90.6Comparative Example 200.10.20.30.20.40.50.70.80.60.5Comparative Example 30.10.10.20.20.30.50.40.70.70.81.0Comparative Example 40.10.20.10.20.30.30.40.70.70.81.0

[0369] Referring to the SEM images of FIGS. 1 to 11 and Tables 4, 5 and FIG. 30, it can be confirmed that, in the case of the positive electrode active materials of Examples 1 to 11, a coating portion including Co and / or B is formed on the surface of the primary particle, the interface of the primary particle and / or the surface of the secondary particle. In addition, it can be confirmed that the coating portion has both an island shape formed on a portion of the surface of the primary particle, the interface of the primary particle and / or the surface of the secondary particle, and a coating layer shape formed to surround the surface of the primary particle, the interface of the primary particle and / or the surface of the secondary particle.

[0370]

[0371] Experimental Example 6: Volume Cumulative Distribution Analysis

[0372] For the positive electrode active materials manufactured in Examples 1 to 11 and Comparative Examples 1 to 5, D was measured using a particle size analyzer (PSD, Malvern, martersizer 3500). min , D 50 and D max , the mode in the cumulative volume distribution according to the particle size, the y-value (P) of the peak point at the top of the y-axis of the peak appearing in the mode according to the cumulative volume distribution MODE ), θ L , and θ R Measure , θ L - θ R The results were calculated and shown in Table 6.

[0373]

[0374] And, the skewness value (S) is calculated from the following equation 3, and the y-value (P) of the peak point at the top of the y-axis of the peak appearing in the mode according to the volume cumulative distribution MODE ) to the ratio of skewness values ​​(S) (S / P) MODE ) were calculated and shown in Table 6 below.

[0375] [Formula 3]

[0376]

[0377]

[0378] In addition, the volume cumulative distributions of the positive electrode active materials of Examples 1 to 11 and Comparative Examples 1 and 3 measured using a laser diffraction particle size analyzer, and the frequency distribution graphs in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top, are shown in FIG. 31 (Example 1), FIG. 32 (Example 2), FIG. 33 (Example 3), FIG. 34 (Example 4), FIG. 35 (Example 5), FIG. 36 (Example 6), FIG. 37 (Example 7), FIG. 38 (Example 8), FIG. 39 (Example 9), FIG. 40 (Example 10), FIG. 41 (Example 11), FIG. 42 (Comparative Example 1), and FIG. 43 (Comparative Example 3), respectively.

[0379] And, the volume cumulative distribution of the positive electrode active materials of Examples 1 to 11 and Comparative Examples 1 and 3 measured using a laser diffraction particle size analyzer, the x-axis representing a log scale for particle diameter in which the x value increases from left to right, and the y-axis representing a weight distribution in which the y value increases from bottom to top, are shown in frequency distribution graphs in FIG. 44 (Example 1), FIG. 45 (Example 2), FIG. 46 (Example 3), FIG. 47 (Example 4), FIG. 48 (Example 5), FIG. 49 (Example 6), FIG. 50 (Example 7), FIG. 51 (Example 8), FIG. 52 (Example 9), FIG. 53 (Example 10), FIG. 54 (Example 11), FIG. 55 (Comparative Example 1), and FIG. 56 (Comparative Example 3), respectively.

[0380]

[0381] Category D min (㎛)D 50 (㎛)D max (㎛)Mode (㎛)P MODE Skewness value (S)S / P MODE θ L θ R θ L / θ R θ L - θ RExample 12.5211.4762.2312.008.510.9260.10947.98033.1611.44714.819 Example 25.0410.3237.0010.6013.721.0370.07671.68463.0891.1368.595 Example 34.629.8737.009.9212.980.5870.04571.21562.5821.1388.633 Example 43.2710.0652.3310.5012.751.0070.07950.34542.7511.2357.594 Example 55.049.9537.0010.3712.250.7440.06172.13565.4211.1036.714Example 65.5010.6240.3510.6013.321.0170.07672.84265.951.1056.892Example 75.0410.2937.0010.0913.060.7610.05872.75365.0051.1197.748Example 88.4814.0737.0014.2716.420.6580.04071.52164.7571.1046.764Example 98.4814.1337.0014.2716.310.8000.04970.69563.2951.1177.400Example 108.4814.2037.0014.2716.280.7810.04870.53862.8121.1237.726Example 118.4814.2737.0014.2716.300.7550.04670.77463.0041.1237.770Comparative Example 16.549.8526.1610.0916.90.5960.03575.64671.021.0654.626Comparative Example 27.1311.82371214.520.4110.02878.62173.0261.0775.595Comparative example 35.049.953710.3718.010.6530.03672.13570.8601.0181.275Comparative example 45.510.6240.3510.612.011.8250.15272.84268.9521.0563.890Comparative example 52.004.3018.054.4610.360.3250.03153.21524.3602.18528.855

[0382] Referring to Table 6, for the positive electrode active materials of Examples 1 to 11, the D 50 It can be confirmed that this is 7.0 ㎛ or more and 20.0 ㎛ or less. In addition, (θ L - θ R ) can be confirmed to be 6 or more and 20 or less. In addition, it can be confirmed that the volume cumulative distribution measured using a laser diffraction particle size analyzer shows positive skewness in the frequency distribution graph in which the x-axis represents a linear scale for particle diameter in which the x-value increases from left to right, and the y-axis represents a weight distribution in which the y-value increases from bottom to top.

[0383]

[0384] Experimental Example 7: Rolling Density Measurement

[0385] Using an automatic pellet press (Auto Pellet Press, Carver, 3887.4), a cylindrical mold was used to adjust the zero point for thickness on a circular pellet holder having a diameter of 13 mm. Then, 3 g each of the positive electrode active materials manufactured in Examples 1 to 11 and Comparative Examples 1 to 5 was placed on the circular pellet holder, and a force was applied until a force corresponding to 9,000 kgf was reached, and the thickness of the formed pellet was measured. Then, the pellet volume was calculated using the following Equation 4, and the rolling density was calculated using the following Equation 2, and the results are shown in Table 7 below.

[0386] [Formula 4]

[0387] Pellet volume (cm) 3 ) = π(radius of the circular pellet holder) 2 Thickness of X pellet

[0388] [Formula 2]

[0389] Rolling density (g / cm) 3 ) = Positive active material weight (g) / Pellet volume (cm 3 )

[0390]

[0391] Rolled density (g / cm) 3 ) Example 13.67 Example 23.68 Example 33.67 Example 43.69 Example 53.68 Example 63.66 Example 73.69 Example 83.75 Example 93.76 Example 103.74 Example 113.76 Comparative Example 13.27 Comparative Example 23.30 Comparative Example 33.49 Comparative Example 43.46 Comparative Example 53.50

[0392] Referring to Table 7, for the positive electrode active materials of Examples 1 to 11, the rolling density was 3.60 g / cm 3 It can be confirmed that the above is true. Specifically, the rolling density is 3.66 g / cm 3 You can see that it is abnormal.

[0393]

[0394] Experimental Example 8: BET Surface Area Measurement

[0395] The specific surface area was measured using the nitrogen gas adsorption and desorption method. Specifically, after measuring the weight of an empty cell, 3 g each of the positive electrode active materials manufactured in Examples 1 to 11 and Comparative Examples 1 to 5 was taken and pretreated at 130°C for 3 hours. After measuring the weight of the cell after the pretreatment process, a dewar containing liquid nitrogen was prepared and the cell was fastened. The BET specific surface area was measured from the nitrogen gas adsorption amount using a gas adsorption analyzer (Micromeritics TriStarr II) under a nitrogen atmosphere, and the results are shown in Table 8 below.

[0396]

[0397] Specific surface area (m) 2 / g)Embodiment 10.305Embodiment 20.294Embodiment 30.240Embodiment 40.305Embodiment 50.312Embodiment 60.322Embodiment 70.307Embodiment 80.332Embodiment 90.328Embodiment 100.270Embodiment 110.338Comparative Example 10.504Comparative Example 20.592Comparative Example 30.631Comparative Example 40.729Comparative Example 50.748

[0398] Referring to Table 8, for the positive electrode active materials of Examples 1 to 11, the BET specific surface area is 0.20 m 2 / g or more, 0.35 m 2 / g or less. Specifically, the BET surface area is 0.240 m 2 / g or more, 0.338 m 2 You can see that it is below / g.

[0399]

[0400] Experimental Example 9: Manufacturing and Charge-Discharge Evaluation of Coin-Type Half-cells

[0401] A positive electrode slurry was prepared by mixing 95 parts by weight of each of the positive electrode active materials manufactured in Examples 1 to 11 and Comparative Examples 1 to 5, 2 parts by weight of a conductive agent (Denka, FX35), and 3 parts by weight of a binder (KUREHA, KF9709) in an N-methylpyrrolidone (NMP) solvent. The prepared positive electrode slurry was applied to one surface of a 20 μm thick aluminum current collector, and rolled so that the porosity of the positive electrode active material layer became 24% by volume, thereby preparing a positive electrode.

[0402] An electrode assembly was manufactured using a lithium metal electrode as the negative electrode and a porous polyethylene separator interposed between the positive and negative electrodes. This was placed inside a battery case and an electrolyte was injected to manufacture a lithium secondary battery. The electrolyte was prepared by dissolving 1 M LiPF6 in an organic solvent containing ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) in a volume ratio of 3:3:4.

[0403] Using lithium secondary batteries including the positive electrode active materials of Examples 1 to 11 and Comparative Examples 1 to 5 manufactured above, charging was performed in CC / CV mode at 0.1 C constant current at 25°C to 4.25 V (end current 0.05 C), and then discharging was performed in CC mode until 2.5 V, and the charge capacity and discharge capacity were measured, which are shown in Table 9 below. At this time, 1 C = 200 mA / g was set.

[0404] In addition, the manufactured lithium secondary battery was charged in CC / CV mode at 45°C with a constant current of 0.5 C to 4.25 V (end current of 0.05 C), and then discharged in CC mode at a constant current of 1.0 C until it reached 2.5 V. This was repeated 50 times, and the percentage of discharge capacity of the 50th cycle compared to the discharge capacity of the first cycle was used as the capacity retention rate, and is shown together in Table 9 below.

[0405]

[0406] Classification Charge capacity Discharge capacity Efficiency DC resistance High temperature (45 ℃) Capacity retention rate (mAh / g) (mAh / g) (%) (Ω) (%) Example 1 233.6 209.0 89.5 18.5 96.17 Example 2 233.4 208.4 89.3 20.2 96.30 Example 3 233.6 207.1 88.7 20.4 96.93 Example 4 231.1 205.8 89.1 19.4 96.57 Example 5 232.6 207.7 89.3 18.4 95.80 Example 6 231.7 208.7 90.1 18.2 96.20 Example 7 232.0 207.9 89.6 13.2 96.50 Example 8247.9216.587.329.293.67 Example 9247.6216.387.330.294.00 Example 10247.4215.186.930.295.45 Example 11245.9212.486.430.594.92 Comparative Example 1232.4212.191.319.694.90 Comparative Example 2231.1211.791.620.494.50 Comparative Example 3242.6222.891.824.595.20 Comparative Example 4242.9223.492.023.195.30 Comparative Example 5232.3198.685.526.095.00

[0407]

[0408] Experimental Example 10: Evaluation of High-Rate Discharge Capacity

[0409] Using the lithium secondary battery manufactured in the above experimental example 9, the battery was charged in CC / CV mode at 25°C with a constant current of 0.5 C to 4.25 V (end current of 0.05 C), and then discharged in CC mode at a constant current of 0.1 C to 2.5 V, and the discharge capacity was measured. In addition, the discharge capacity was measured while charging in CC / CV mode at 0.5 C constant current at 25 ℃ to 4.25 V (end current 0.05 C) and then discharging in CC mode at 1.0 C constant current until 2.5 V, and the discharge capacity was measured while charging in CC / CV mode at 0.5 C constant current at 25 ℃ to 4.25 V (end current 0.05 C) and then discharging in CC mode at 2.0 C constant current until 2.5 V, and the percentage of the discharge capacity at 0.1 C discharge after 0.5 C charge is shown in Table 10 below.

[0410]

[0411] Distinction (1.0 C discharge capacity) / (0.1 C discharge capacity) Х 100 (%) (2.0 C discharge capacity) / (0.1 C discharge capacity) Х 100 (%) Example 192.7790.64 Example 292.7290.64 Example 392.7090.48 Example 492.6690.44 Example 592.8290.43 Example 692.8590.58 Example 792.8390.64 Example 893.4391.02 Example 993.3890.95 Example 1093.3590.87 Example 1193.0489.78 Comparative Example 187.4786.18 Comparative Example 287.6086.28Comparative example 390.4487.63Comparative example 490.8488.74Comparative example 591.5489.57

[0412] Referring to Tables 9 and 10 above, it can be seen that the batteries including the positive electrode active materials of Examples 1 to 11 have large discharge capacities, high efficiency and high temperature capacity retention, low DC resistance, and excellent rate characteristics. In contrast, the batteries including the positive electrode active materials of Comparative Examples 1 to 4 have poor rate characteristics, and the batteries including the positive electrode active materials of Comparative Example 5 have small discharge capacities and low efficiency.

[0413]

[0414] From these results, it was confirmed that the cathode active material of the present invention is a cathode active material that can simultaneously solve the problems of conventional secondary particles and single particles in high nickel (High Ni) cathode active materials, and by implementing a cathode active material in the form of secondary particles with primary particles of micron size, it can not only improve cell characteristics such as improved lifespan of lithium secondary batteries and reduced gas generation, but also improve energy density due to excellent density characteristics.

Claims

1. Contains secondary particles that are agglomerated from multiple primary particles, The above plurality of primary particles have an average particle size of 1.5 ㎛ or more and 5.0 ㎛ or less as measured from an SEM image, and the particle size of the primary particles is a particle size based on the major diameter of the primary particles. The above plurality of primary particles include disk type primary particles, The above disk-shaped primary particles are, In the case of a primary particle observed from an SEM image of the surface or cross-section of a secondary particle, when two imaginary tangent lines with the greatest number of contact points are drawn for each of the two boundaries of the primary particle existing within an angle of 45° or less based on the major axis direction, and one imaginary line is drawn crossing the two tangent lines, the same internal angle is 150° or more and 210° or less, A positive electrode active material having a minor diameter of 0.3 ㎛ or more and an aspect ratio (major diameter / minor diameter) of 1.5 or more.

2. In paragraph 1, A cathode active material wherein the plurality of primary particles include three or more disk-type primary particles.

3. In paragraph 1, The above disk-shaped primary particle is a positive electrode active material having a diameter of 0.8 ㎛ or more.

4. In paragraph 1, A cathode active material comprising a lithium transition metal composite oxide containing nickel, cobalt and manganese.

5. In paragraph 1, A cathode active material comprising a lithium transition metal composite oxide containing nickel in an amount of 60 mol% or more among the total transition metals.

6. In paragraph 1, A cathode active material comprising a lithium transition metal composite oxide having an average composition represented by the following chemical formula 1: [Chemical Formula 1] Li x Ni a Co b Mr c M 1 d O2 In the above chemical formula 1, M 1 is at least one selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, V, F, P, S and Y, 0.9≤x≤1.3, 0.6≤a<1.0, 0 <b<0.4, 0<c<0.4, 0≤d≤0.2, a+b+c+d=1이다.

7. In paragraph 1, A cathode active material wherein the plurality of primary particles include single crystal primary particles.

8. In paragraph 1, The above secondary particles are measured using a laser diffraction particle size analyzer and have an average particle diameter (D) based on the cumulative volume distribution. 50 ) is a positive electrode active material having a particle size of 7.0 ㎛ or more and 20.0 ㎛ or less.

9. A positive electrode comprising a positive electrode active material according to any one of claims 1 to 8.

10. A lithium secondary battery comprising a positive electrode according to Article 9; a negative electrode; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.

Citation Information

Patent Citations

  • Positive electrode active material, preparing method thereof, positive electrode including the same, and lithium secondary battery employing the positive electrode

    KR101785262B1

  • Positive electrode active material for secondary battery and secondary battery containing the same

    JP2018538663A

  • Method for searching stuff using bluetooth low energy

    KR1020200139441A

  • Method and system for managing cloud access and accounts