Method for producing optical member
The method of forming a fine uneven structure on PMMA surfaces via ion irradiation and depositing a low-refractive-index protective film addresses the heat resistance and reflection issues in PMMA optical components, ensuring high antireflection performance in high-temperature environments.
Patent Information
- Application Number
- PCT/JP2023/030759
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-01
- Filing Date
- 2023-08-25
- Publication Date
- 2024-11-07
AI Technical Summary
Optical components made from polymethyl methacrylate resin (PMMA) face issues with surface reflection and heat resistance due to the difference in coefficients of linear expansion between the PMMA base material and the antireflection film, leading to cracks and reduced light transmittance in high-temperature environments, especially in automotive applications.
A method involving ion irradiation to form a fine uneven structure, such as a moth-eye structure, on the PMMA surface, followed by the deposition of a thin protective film with a refractive index lower than the base material, like silicon oxide, to enhance heat resistance and maintain the antireflection effect.
The method effectively suppresses surface reflection and maintains spectral properties even in high-temperature environments, improving the heat resistance and antireflection performance of optical components.
Smart Images

Figure JP2023030759_07112024_PF_FP_ABST
Abstract
Description
Optical member manufacturing method
[0001] The present disclosure relates to a method for manufacturing optical components, and can be applied to, for example, a method for manufacturing optical components with high anti-reflection properties in a high-temperature environment by forming a protective film on a fine uneven structure formed on the surface of a plastic (synthetic resin) substrate.
[0002] Plastics, which have excellent translucency, are lightweight, have excellent mechanical strength, are easy to process, and can be designed freely, so they are particularly used as an alternative to glass. Plastics are particularly used in the optical field, and in recent years, plastics have been used in a wide range of parts such as automobile headlights.
[0003] Transparent plastics that are currently widely used include thermoplastic polyvinyl chloride (PVC), polystyrene (PS), polycarbonate (PC), polymethyl methacrylate (PMMA), and thermosetting polyethylene glycol bisallyl carbonate (CR39).
[0004] Among these plastics, PMMA is excellent for optical parts in transparency, light weight, ease of processing, and impact resistance, and in particular, has the best light transmittance compared to other resins.
[0005] JP 2019-15826 A
[0006] However, when an anti-reflection film for suppressing surface reflection is formed on the surface of a PMMA base material in order to improve the transmittance of an optical component using polymethyl methacrylate resin (PMMA), the following problems arise.
[0007] For example, in the optical field, such as in consumer projectors, reliability conditions of around 70°C are required, so an anti-reflection film can be formed on the surface of a PMMA substrate by vacuum deposition. On the other hand, lighting systems in the automotive field require reliability conditions of high temperatures of 90 to 100°C (hereinafter, high temperature environments refer to environments of around 90 to 100°C), so there is a problem that the formed anti-reflection film may crack due to the difference in linear expansion coefficient between the substrate and the anti-reflection film.
[0008] Furthermore, while automobile headlights initially used a single lens, there is now a demand for more precise headlights using multiple lenses. When multiple lenses are used, aberration correction is required, which increases the number of lenses, and this also creates the problem of increased surface reflection.
[0009] In view of the above-mentioned problems, the present disclosure aims to provide a method for manufacturing an optical component that has high anti-reflection properties in a high-temperature environment by forming a protective film on a fine uneven structure formed on the surface of a substrate made of a synthetic resin such as polymethyl methacrylate resin, with the aim of having heat resistance in the desired high-temperature environment and preventing loss of light intensity.
[0010] In order to solve such problems, the method for manufacturing an optical component according to the present disclosure is characterized by comprising: (1) a fine uneven structure forming process in which the surface of a substrate is changed by ion irradiation to form a fine uneven structure on the surface of the substrate; and (2) a protective film forming process in which a vapor deposition material is evaporated and deposited on the surface of the substrate to form a protective film on the fine uneven structure formed on the surface of the substrate.
[0011] According to the present disclosure, a protective film can be formed on a fine uneven structure formed on the surface of a synthetic resin substrate, making it possible to manufacture optical components with high anti-reflection properties even in high-temperature environments.
[0012] 1 is a diagram showing the conditions for forming a fine uneven structure in step A and the spectral characteristics of a substrate having a fine uneven structure. FIG. 2 is a diagram showing the conditions for forming a fine uneven structure in step C and the spectral characteristics of a substrate having a fine uneven structure. FIG. 3 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film are formed in the steps of Example 1. FIG. 4 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film are formed in the steps of Example 2. FIG. 5 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film are formed in the steps of Example 3. FIG. 6 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film are formed in the steps of Example 4. FIG. 7 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film are formed in the steps of Example 5. FIG. 8 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure is formed in step A before a high-temperature test and the spectral characteristics of a substrate in a high-temperature environment. FIG. 9 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure is formed in step A before a high-temperature test and the spectral characteristics of a substrate in a high-temperature environment. FIG. 10 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure is formed in step A before a high-temperature test and the spectral characteristics in a high-temperature environment. FIG. 11 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure is formed in step A before a high-temperature test and the spectral characteristics in a high-temperature environment. 10A and 10B are graphs showing the results of comparing the antireflection effect of Example 1 with that of other antireflection films, and are diagrams showing the spectral characteristics of Example 1 and that of other antireflection films.
[0013] (A) Embodiments Hereinafter, embodiments of the optical thin film manufacturing method of the present disclosure will be described in detail with reference to the drawings.
[0014] (A-1) Overview In recent years, there has been an increasing demand for plastic optical components as an alternative to glass-based optical components. For example, a method for preventing surface reflection of an optical lens by forming a fine uneven structure on the surface of a substrate is known.
[0015] One such fine uneven structure is called a moth-eye structure (called moth-eye because it resembles the minute protrusions on the surface of a moth's eye). In the present disclosure, the moth-eye structure is exemplified as an example of a fine uneven structure, but the present disclosure is not limited to the moth-eye structure.
[0016] Conventionally, a method for forming a moth-eye structure on the surface of a plastic substrate includes, for example, molding a fine uneven structure by injection molding using a mold.
[0017] However, this method has the risk of the resin sticking to the mold when the molded product is removed from the mold, destroying the fine uneven structure, making it difficult to adopt as a production method for products.
[0018] Another method is to use ion sputtering. Ion sputtering is a phenomenon caused by ion irradiation, and involves irradiating the surface of a PMMA substrate with ions to modify the surface and change its shape. Conventionally, for example, a vacuum deposition device equipped with a plasma gun is used to irradiate the surface with ions during film formation, activating the evaporated molecules and improving film strength.
[0019] The inventors of the present application confirmed that a moth-eye shape (a shape having a fine uneven structure) is formed on the surface of a PMMA substrate by irradiating the PMMA substrate with ions without forming (laminated) a multilayer film on the substrate surface, and confirmed the anti-reflection effect and spectral characteristics of the PMMA substrate having the moth-eye shape.
[0020] PMMA has a chain structure, and the C-O portion of C-OOCH3 is broken by plasma, forming a moth-eye shape. In fact, using a plasma gun based on this method, it was possible to form a moth-eye shape on the substrate surface by adjusting conditions such as the argon gas flow rate, oxygen flow rate, and ion irradiation power. Moth-eyes could also be formed using another method, a CVD (chemical vapor deposition) device, by plasma discharge, adjusting the argon gas flow rate, oxygen flow rate, and high-frequency power. The formation of a fine uneven structure on the substrate surface confirmed the anti-reflection effect or the spectral characteristic effect of enhancing transparency.
[0021] However, when testing was conducted in the high-temperature environments required in the automotive industry, the spectral characteristics changed, returning to the original lens surface reflection, and the objective could not be achieved. This is thought to be because the moth-eye shape, which is a fine uneven structure, collapses in the high-temperature environment.
[0022] Therefore, the inventors of the present application have conducted extensive research and have proposed that, instead of forming (laminating) a conventional multilayer anti-reflection film on a substrate, a thin protective film be formed on the fine uneven structure (e.g., moth-eye shape) on the surface of a synthetic resin substrate, so that the film (protective film) is thin enough not to generate stress.
[0023] As a result, it was possible to maintain the shape of the fine uneven structure even in a high-temperature environment, improving the heat resistance of the optical component, and confirming the surface anti-reflection function and spectral characteristics.
[0024] The protective film maintains a fine uneven structure and has improved heat resistance. The material for the protective film is preferably silicon oxide, which has a lower refractive index than the synthetic resin of the base material. A high refractive index increases reflection due to optical interference, so a material with an intermediate refractive index is preferred; for example, a material with a refractive index of 1.6 or less is preferable, with 1.65 or less being even more preferable. The optical thickness of the protective film when irradiated with light having a wavelength of 550 nm is preferably λ / 50 to λ / 16.
[0025] The protective film functions as an anti-reflection film that suppresses reflection on the substrate surface and also has spectral properties that separate light wavelengths. Furthermore, the protective film functions as a film that maintains the shape of the fine uneven structure even in a high-temperature environment. In this disclosure, the protective film is exemplified as a silicon oxide (SiO2) film or a silicon oxide mixed (SiOx) film, but is not limited thereto.
[0026] (A-2) Optical Thin Film Manufacturing Method Hereinafter, the optical thin film manufacturing method according to this embodiment will be described.
[0027] In the optical thin film manufacturing method according to this embodiment, a fine uneven structure is formed on the surface of a substrate by ion irradiation, and a protective film is formed on the fine uneven structure on the surface of the substrate.
[0028] (1) Substrate The substrate was a plastic substrate (transparent substrate) made of a highly transparent plastic (synthetic resin). The transparent substrate plastic was a chain-bonded polymethyl methacrylate resin (PMMA) with high transparency.
[0029] The present disclosure utilizes the property of PMMA that the surface of a substrate is changed by ion irradiation, resulting in the formation of a moth-eye pattern on the substrate surface. Therefore, the present disclosure is not limited to PMMA, and a wide range of other synthetic resins can be used as long as they can form a fine uneven structure on their surface by ion irradiation.
[0030] It should be noted that polycarbonate (PC) having a benzene ring and cycloolefin polymer (COP: Cycloolefin Polymer), which is a cyclic compound, do not form a fine uneven structure on the substrate surface by ion irradiation, and it is therefore considered difficult to use these as substrates.
[0031] (2) Material (deposition material) It is desirable that the refractive index of the material be lower than that of the plastic (synthetic resin) used for the substrate. If the refractive index of the synthetic resin used for the substrate is high, there is a risk that reflection will increase due to light interference.
[0032] In this embodiment, the material (evaporation material) is silicon oxide. However, the material (evaporation material) is not limited to silicon oxide, and may be, for example, aluminum oxide, titanium oxide, tantalum oxide, zirconium oxide, or the like.
[0033] (3) Formation Method The methods for forming a protective film on the surface of a substrate are generally: (a) a method in which silicon oxide, which is the material, is evaporated as is, and (b) a method in which hexamethyldisiloxane (HMDS) is subjected to plasma discharge (polymerization) to form a Si+SiO2+SiO mixed film material (hereinafter referred to as "SiOx").
[0034] (3-1) Pre-processing First, when forming a fine uneven structure on a substrate, there may be stains such as burns, fingerprints, and oil on the surface of the substrate, so pure water and neutral detergent are added to an ultrasonic cleaner, and the substrate is placed in the cleaner and ultrasonically cleaned. In addition, because PMMA has a high water absorption rate, it is also desirable to pre-dry the substrate.
[0035] (3-2) Setting the substrate in a vacuum device. After the above-mentioned pre-processing is completed, the substrate is placed in a vacuum device. Here, the exhaust system of the vacuum device is not particularly limited, and for example, a vacuum pump such as a diffusion pump or a turbomolecular pump can be used.
[0036] The apparatus used in the optical thin film formation method is exemplified as a vacuum deposition apparatus equipped with a plasma gun, a chemical vapor deposition apparatus, or both.
[0037] When using a vacuum deposition device equipped with a plasma gun, two processes are considered: "Step A" for forming a fine uneven structure on the surface of the substrate, and "Step B" for forming a protective film on the fine uneven structure on the surface of the substrate.
[0038] Similarly, when a chemical vapor deposition apparatus is used, a "step C" of forming a moth-eye pattern on the surface of the substrate and a "step D" of forming a protective film on the moth-eye pattern on the surface of the substrate can be considered.
[0039] In the following examples (Examples 1 to 5), effective steps from "Step A" to "Step D" can be combined.
[0040] Although details will be described later, depending on the combination of steps, there is a method in which the "moth-eye shape" and the "protective film" are formed using both a vacuum vapor deposition apparatus and a chemical vapor deposition apparatus, and there is also a method in which the "moth-eye shape" and the "protective film" are formed using either a vacuum vapor deposition apparatus or a chemical vapor deposition apparatus.
[0041] In other words, the former method (that is, the method using two devices) can be said to be a method for forming a "moth-eye shape" and a "protective film" in two stages.
[0042] Conversely, the latter method (i.e., the method using one device) can be said to be a method of forming the "moth-eye shape" and the "protective film" in one step. In other words, since the process can be carried out continuously using one device, it is expected to improve the productivity of optical components and enable more efficient manufacturing.
[0043] (3-3) Vacuum deposition equipment equipped with a plasma gun A vacuum deposition equipment equipped with a plasma gun generally comprises a vacuum chamber, a substrate setting section (rack) for setting the substrate inside the vacuum chamber, a deposition source provided with a crucible for setting the material to be used as the deposition material, an electron gun, a plasma gun, a heater for heating the substrate, and a vacuum pump as an exhaust system.
[0044] [Step A] The substrate is placed on a rack with its surface facing the deposition source, and a material serving as a deposition material is placed in a crucible. The vacuum chamber is then depressurized using a vacuum pump, and the substrate is heated using a heater as needed. The material (deposition material) evaporated and sublimated in the vacuum chamber is then irradiated with ions using a plasma gun, causing the surface shape of the substrate to change and forming a finely textured structure on the substrate surface. In other words, a moth-eye shape is formed on the substrate surface. This step is referred to as "Step A." According to Step A, the material is activated by ion irradiation, improving film strength.
[0045] It should be noted that evaporation and sublimation of the deposition material are not essential, and in the following Examples 1 to 5 illustrated in this embodiment, cases in which evaporation and sublimation of the deposition material were not performed are illustrated.
[0046] [Step B] The substrate is placed on a rack with its surface facing the deposition source, and the deposition material is placed in a crucible. The vacuum chamber is then depressurized using a vacuum pump, and the substrate is heated using a heater as needed. This process overlaps with part of Step A.
[0047] Then, in the vacuum chamber, the deposition material is dissolved and evaporated by an electron gun, and the evaporated deposition material is deposited on the surface of the substrate, forming a protective film on the surface of the substrate. This process is called "Process B."
[0048] (3-4) Chemical Vapor Deposition Apparatus (CVD) A chemical vapor deposition apparatus generally includes a reaction chamber, a substrate setting section for setting a substrate in the reaction chamber, a high-frequency power supply, a material supply section for supplying gasified material to the reaction chamber by plasma discharge using high-frequency waves, a supply section for supplying gas (carrier gas) to the reaction chamber, and a vacuum pump as an exhaust system for evacuating the inside of the reaction chamber.
[0049] [Step C] The substrate is placed in the substrate placement section, and the material is placed in the material supply section. The reaction chamber is then evacuated using a vacuum pump, and gas is supplied from the supply section, allowing the gas to flow from the supply section toward the vacuum pump within the reaction chamber. Then, plasma is generated at a high frequency (e.g., 36.56 MHz), and the material supply section supplies the evaporated material into the reaction chamber, forming a fine uneven structure on the substrate surface. This step is called "Step C."
[0050] Here, the type of gas supplied into the reaction chamber by the supply unit may be argon gas, oxygen gas, nitrogen gas, or the like.
[0051] [Step D] The substrate is placed in the substrate placement section, and the material is placed in the material supply section. Next, the reaction chamber is evacuated using a vacuum pump, and gas is supplied from the supply section so that the gas flows from the supply section to the vacuum pump within the reaction chamber. This process overlaps with part of step C.
[0052] Then, in the material supply unit, plasma discharge is generated by high frequency to gasify organic silicon such as hexamethyldisiloxane (HMDS), tetraethoxysilane (TEOS), and triethoxysilane (TRIES), and the gasified material is polymerized by high frequency to form SiOx. The material supply unit then supplies SiOx into the reaction chamber to form a protective film on the surface of the substrate. This process is called "Process D."
[0053] (3-5) Conditions for Forming a Fine Relief Structure on a Substrate Surface The conditions for forming a fine relief structure on a substrate surface in "Step A" and "Step C" will be described with reference to FIGS. 1 and 2.
[0054] FIG. 1A shows the conditions for forming a fine uneven structure by step A, and FIG. 1B shows the results of confirming the transmission characteristics of a substrate having a fine uneven structure under each condition.
[0055] In FIG. 1B, the horizontal axis represents wavelength [nm] and the vertical axis represents transmittance [%]. Light was transmitted through the substrate while changing the wavelength (λ) from 400 nm to 750 nm, and the transmittance at each wavelength was confirmed.
[0056] 1B, the results for condition number 102 were favorable, maintaining a transmittance of approximately 95% to 97% at each wavelength from 400 nm to 750 nm. Therefore, in the following examples and comparative examples, when a fine uneven structure is formed on the surface of a substrate in step A, it is formed under the conditions of condition number 102.
[0057] FIG. 2A shows the conditions for forming a fine uneven structure by step C, and FIG. 1B shows the results of confirming the transmission characteristics of a substrate having a fine uneven structure under each condition.
[0058] 2B, it can be seen that the results for condition number 111 maintain high transmittance at each wavelength from 400 nm to 750 nm, and in particular maintain a transmittance of approximately 90% to 97% for light with wavelengths from 470 nm to 750 nm. Therefore, in the following examples and comparative examples, a fine uneven structure is formed on the surface of a substrate under the condition of condition number 111.
[0059] (A-3) Description of Examples (A-3-1) Example 1 (Process A + Process B) Fig. 3 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film were formed in the process of Example 1. Example 1 is a combination of Process A and Process B.
[0060] In step A, the substrate is placed on the rack of a vacuum deposition device, and the pressure in the vacuum chamber is reduced to 5×10 -3 Ion irradiation was carried out after evacuation to (5E-3) Pa. The vacuum deposition apparatus used was a dome-shaped apparatus with an apparatus diameter (diameter of the vacuum chamber) of 1600φ.
[0061] In step B, the vacuum deposition apparatus used in step A was used. That is, without opening the vacuum chamber, SiO2 as a material was evaporated by an electron gun to form a SiO2 film on the surface of the substrate.
[0062] In Example 1, the optical film thickness of the SiO2 film formed on the surface of the substrate was changed, and the transmittance characteristics were measured by irradiating each sample substrate with light of each wavelength from 400 nm to 750 nm.
[0063] The SiO2 film conditions were such that the optical film thicknesses were λ / 32, λ / 16, λ / 8, λ / 4, λ / 3, and λ / 2 when the wavelength λ of the light irradiated onto the substrate was 550 nm. These six substrates and one without a SiO2 film (uncoated) were used as samples.
[0064] The results in FIG. 3 show that at each wavelength from 400 nm to 750 nm, all of the substrates with optical film thicknesses of λ / 32 to λ / 2 (λ / 32, λ / 16, λ / 8, λ / 4, λ / 3, λ / 2) have a transmittance of approximately 90% or more, and all of the substrates maintain high transmittance.
[0065] In FIG. 3, among the six substrates, each of the substrates with wavelengths from λ / 32 to λ / 3 (λ / 32, λ / 16, λ / 8, λ / 4, λ / 3) maintains a transmittance of approximately 92% or more for light with wavelengths from 470 nm to 750 nm, demonstrating good anti-reflection effects. Furthermore, each of the substrates with wavelengths from λ / 32 to λ / 4 (λ / 32, λ / 16, λ / 8, λ / 4) maintains a transmittance of approximately 95% to 99%, demonstrating high anti-reflection effects.
[0066] Furthermore, it can be seen that among the six base materials, the λ / 3 and λ / 2 base materials tend to have higher transmittance as the wavelength value increases.
[0067] Furthermore, among the six substrates, the substrates with wavelengths from λ / 32 to λ / 3 (λ / 32, λ / 16, λ / 8, λ / 4, λ / 3) all have high transmittance for light with wavelengths from 470 nm to 750 nm, but tend to have high transmittance for wavelengths shorter than 550 nm.
[0068] (A-3-2) Example 2 (Process A + Process D) Fig. 4 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film were formed in the process of Example 2. Example 2 is a combination of Process A and Process D.
[0069] In step A, the substrate was placed on a rack in a vacuum deposition apparatus (dome-shaped, 1600φ), and the air pressure in the vacuum chamber was adjusted to 5×10 -3 The chamber was evacuated to (5E-3) Pa and ion irradiation was carried out.
[0070] In step D, the substrate was reinstalled in the substrate installation section of the chemical vapor deposition apparatus, the pressure in the reaction chamber was evacuated to 0.2 Pa, and a SiOx film was formed on the surface of the substrate by polymerizing hexamethyldisiloxane (HMDS) through plasma discharge. In order to move to step D, the vacuum chamber of the vacuum deposition apparatus was opened, the substrate was removed, and the substrate was then reinstalled in the chemical vapor deposition apparatus.
[0071] In Example 2, the optical film thickness of the SiOx film formed on the surface of the substrate was changed, and the transmittance characteristics were measured by irradiating each sample substrate with light of each wavelength from 400 nm to 750 nm.
[0072] The SiOx film conditions were such that the optical film thicknesses were λ / 32, λ / 16, λ / 8, and λ / 4 when the wavelength λ of the light irradiated onto the substrate was 550 nm. These four substrates and one without a SiO2 film (uncoated) were used as samples.
[0073] The results in FIG. 4 show that at each wavelength from 400 nm to 750 nm, the substrates with optical film thicknesses of λ / 32 to λ / 4 (λ / 32, λ / 16, λ / 8, λ / 4) all had a transmittance of approximately 92% or more, and all substrates maintained a high transmittance.
[0074] Furthermore, among the four substrates, the substrates with λ / 32 to λ / 8 (λ / 32, λ / 16, λ / 8) maintain a transmittance of approximately 94% to 97% for light with wavelengths of 470 nm to 750 nm, and the substrates with λ / 32 and λ / 16 maintain a transmittance of approximately 95% or more for light with wavelengths of 470 nm to 750 nm, demonstrating a high anti-reflection effect.
[0075] Furthermore, among the four substrates, the λ / 32 and λ / 16 substrates have high transmittance for light with wavelengths of 470 nm to 750 nm, but tend to have high transmittance for wavelengths shorter than 550 nm.
[0076] (A-3-3) Example 3 (Step C + Step D) Fig. 5 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film were formed in the steps of Example 3. Example 3 is a combination of Step C and Step D.
[0077] In step C, a substrate was placed in the substrate placement section of the chemical vapor deposition apparatus, the pressure inside the reaction chamber was evacuated to 0.2 Pa, and plasma discharge was performed.
[0078] In step D, the chemical vapor deposition apparatus used in step C was used as it was, and the reaction chamber was not opened, and a SiOx film was formed on the surface of the substrate by polymerizing hexamethyldisiloxane (HMDS) through plasma discharge.
[0079] In Example 3, the optical film thickness of the SiOx film formed on the surface of the substrate was changed, and the transmittance characteristics were measured by irradiating each sample substrate with light of each wavelength from 400 nm to 750 nm.
[0080] The SiOx film conditions were such that the optical film thicknesses were λ / 32, λ / 16, λ / 8, and λ / 4 when the wavelength λ of the light irradiated onto the substrate was 550 nm. These four substrates and one without a SiO2 film (uncoated) were used as samples.
[0081] The results in FIG. 5 show that, at wavelengths of 480 nm to 750 nm used in the measurement, the substrates with optical film thicknesses of λ / 32 to λ / 4 (λ / 32, λ / 16, λ / 8, λ / 4) all had a transmittance of approximately 90% or more, and all substrates maintained high transmittance.
[0082] Furthermore, among the four substrates, the substrates with λ / 32 to λ / 8 (λ / 32, λ / 16, λ / 8) have a transmittance of approximately 93% or more at wavelengths of approximately 520 nm or more, and are found to have a high anti-reflection effect.
[0083] (A-3-4) Example 4 (Step C + Step B) Fig. 6 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film were formed in the steps of Example 4. Example 4 is a combination of Step C and Step B.
[0084] In step C, a substrate was placed in the substrate placement section of the chemical vapor deposition apparatus, the pressure inside the reaction chamber was evacuated to 0.2 Pa, and plasma discharge was performed.
[0085] In step B, the substrate is placed on the rack of a vacuum deposition device (dome-shaped, 1600φ), and the air pressure in the vacuum chamber is increased to 2×10 -3The chamber was evacuated to (2E-3) Pa, and SiO2 as a material was evaporated with an electron gun to form a SiO2 film on the surface of the substrate. To move to step B, the reaction chamber of the chemical vapor deposition apparatus was opened, the substrate was removed, and the substrate was then reset in the vacuum deposition apparatus.
[0086] In Example 4, the optical film thickness of the SiO2 film formed on the surface of the substrate was changed, and the transmittance characteristics were measured by irradiating each sample substrate with light of each wavelength from 400 nm to 750 nm.
[0087] The SiO2 film conditions were such that the optical film thicknesses were λ / 32, λ / 16, λ / 8, λ / 4, λ / 3, and λ / 2 when the wavelength λ of the light irradiated onto the substrate was 550 nm. These six substrates and one without a SiO2 film (uncoated) were used as samples.
[0088] The results in FIG. 6 show that, at wavelengths of approximately 470 nm to 750 nm used in the measurements, the substrates with optical film thicknesses of λ / 32 to λ / 2 (λ / 32, λ / 16, λ / 8, λ / 4, λ / 3, λ / 2) all had a transmittance of approximately 90% or more, and all substrates maintained high transmittance.
[0089] Furthermore, among the four substrates, the substrates with wavelengths from λ / 32 to λ / 3 (λ / 32, λ / 16, λ / 8, λ / 4, λ / 3) have a transmittance of approximately 93% or more at wavelengths of approximately 500 nm or more, and are therefore found to have a high anti-reflection effect.
[0090] (A-3-5) Example 5 (Step A+Step B) FIG. 7 is a diagram showing the spectral characteristics of a substrate on which a fine uneven structure and a protective film were formed in the steps of Example 5.
[0091] Example 5 is a combination of process A and process B, and aluminum oxide was used as the material (evaporation material) for the protective film.
[0092] In step A, the substrate is placed on the rack of a vacuum deposition device, and the pressure in the vacuum chamber is reduced to 5×10 -3 Ion irradiation was carried out after evacuation to (5E-3) Pa. The vacuum deposition apparatus used was a dome-shaped apparatus with an apparatus diameter (diameter of the vacuum chamber) of 1600φ.
[0093] In step B, the vacuum deposition apparatus used in step A was used. That is, without opening the vacuum chamber, Al2O3 as a material was evaporated by an electron gun to form an Al2O3 film on the surface of the substrate.
[0094] In Example 5, the optical film thickness of Al2O3 on the surface of the substrate was changed, and light of each wavelength from 400 nm to 750 nm was irradiated onto each sample substrate to measure the transmission characteristics.
[0095] The Al2O3 film conditions were such that the optical film thicknesses were λ / 32, λ / 16, and λ / 8 when the wavelength λ of the light irradiated onto the substrate was 550 nm. These six substrates and one without an Al2O3 film (uncoated) were used as samples.
[0096] 7, it can be seen that, of the three substrates, the substrates with λ / 32 to λ / 16 (λ / 32, λ / 16) maintained high transmittance of approximately 91% or more for light with wavelengths of 400 nm to 750 nm. In particular, the substrate with λ / 32 maintained high transmittance of approximately 94% or more for light with wavelengths of 400 nm to 750 nm.
[0097] (A-3-6) Comparative Example 1 (Process A) FIG. 8 shows the results of using a substrate on which a fine uneven structure was formed in Process A, showing the spectral characteristics of the substrate before a high-temperature test and the spectral characteristics of the substrate in a high-temperature environment.
[0098] In Comparative Example 1, a fine uneven structure was formed on the surface of the substrate in step A, and the transmittance characteristics of the substrate were measured and confirmed in a high-temperature environment.
[0099] In step A, the substrate is placed on the rack of a vacuum deposition device, and the pressure in the vacuum chamber is reduced to 5×10 -3 The chamber was evacuated to (5E-3) Pa and ion irradiation was carried out.
[0100] In FIG. 8, the dotted line indicates the results of the spectral characteristics of the substrate before the high-temperature test, and the solid line indicates the results of the spectral characteristics of the substrate after the high-temperature test.
[0101] 8, the transmittance of the substrate that underwent the high-temperature test was lower than that of the substrate before the high-temperature test at each wavelength from 400 nm to 750 nm. In other words, it can be seen that the transmittance (spectral characteristics) of the fine uneven structure formed on the substrate surface was reduced by being placed in a high-temperature environment.
[0102] (A-3-7) High-Temperature Test Results for Example 1 (Step A + Step B) Figure 9 shows the results of the spectral characteristics before the high-temperature test and the spectral characteristics in a high-temperature environment using the substrate of Example 1. Here, a SiO2 film with a thickness of λ / 8 was used.
[0103] 9, it can be seen that the transmittance of the substrate after the high-temperature test is almost the same as that of the substrate before the high-temperature test at each wavelength of 400 nm to 750 nm in a high-temperature environment. In other words, it can be seen that the transmittance (spectral characteristics) does not decrease even in a high-temperature environment, and a high anti-reflection effect is achieved.
[0104] Conventionally, when the temperature becomes high, the fine uneven structure on the surface of the substrate is destroyed, resulting in a decrease in the anti-reflection effect and the spectral characteristics (see Comparative Example 1).
[0105] In contrast, as in Example 1, the anti-reflection effect and spectral characteristics can be maintained even at high temperatures by forming a SiO2 film as a protective film on the fine uneven structure on the substrate surface in step B. In other words, even in the targeted high-temperature environment, the protective film prevents the fine uneven structure from collapsing, thereby maintaining the anti-reflection effect and spectral characteristics.
[0106] Furthermore, in Example 1, since the process A and the process B can be carried out consecutively using the same vacuum deposition apparatus, the efficiency of manufacturing optical components can be improved.
[0107] (A-3-8) High-Temperature Test Results for Example 3 (Step C + Step D) Fig. 10 shows the results of the spectral characteristics before the high-temperature test and the spectral characteristics in a high-temperature environment using the substrate of Example 3. Here, a SiOx film with a thickness of λ / 16 was used.
[0108] 10, it can be seen that in a high-temperature environment, the transmittance of the substrate after the high-temperature test is almost the same as that of the substrate before the high-temperature test at each wavelength of approximately 480 nm to 750 nm. In other words, it can be seen that even in a high-temperature environment, the transmittance (spectral characteristics) does not decrease, and a high anti-reflection effect is achieved.
[0109] In Example 3, as in the case of (A-3-7), the anti-reflection effect and spectral characteristics can be maintained even at high temperatures by forming a SiOx film as a protective film on the fine uneven structure on the substrate surface in step D. This is because the protective film prevents the fine uneven structure from collapsing even in the intended high-temperature environment, thereby maintaining the anti-reflection effect and spectral characteristics.
[0110] Furthermore, in Example 3, the same chemical vapor deposition apparatus can be used to carry out Steps C and D consecutively, thereby improving the efficiency of manufacturing optical components.
[0111] (A-3-9) Comparison with other antireflection films Fig. 11 shows the results of comparing the antireflection effects of Example 1 and other antireflection films. Fig. 12 is a diagram showing the spectral characteristics of Example 1 and other antireflection films.
[0112] As shown in FIG. 11, two examples of other antireflection films are a "four-layer antireflection film formed by vacuum deposition" and a "single-layer antireflection film formed by vacuum deposition."
[0113] 11, the test contents included spectral characteristics showing the average transmittance from 450 nm to 650 nm, a high temperature test (90°C), and a high temperature test (100°C). The spectral characteristics were based on the results of the spectral characteristics in FIG.
[0114] The four-layer anti-reflection film, made by vacuum deposition, has an average transmittance of approximately 98% from 450 nm to 650 nm, and has excellent spectral characteristics. In the automotive and optical fields, high-temperature tests (90°C and 100°C) required, microcracks occurred, making the film visually unacceptable, and so it was marked "X."
[0115] The single layer film formed by the vacuum deposition method showed no problem in the high temperature test (90° C.), but cracks occurred in the high temperature test (100° C.), resulting in a grade of "X."
[0116] As shown in Figure 9, Example 1 had an average transmittance of approximately 98% or more from 450 nm to 650 nm. It also showed excellent results with no change in the high temperature test and high temperature / high humidity test. Since Example 1 was manufactured using the same equipment, continuous production is possible, and mass production is also expected.
[0117] (A-4) Effects of the embodiment As described above, according to this embodiment, a protective film can be formed on a fine uneven structure formed on the surface of a synthetic resin substrate, making it possible to manufacture optical components with high anti-reflection properties even in high-temperature environments.
Claims
1. A method for manufacturing an optical member, comprising: a fine concave-convex structure forming step of forming a fine concave-convex structure on the surface of the substrate by changing the surface of the substrate by ion irradiation; and a protective film forming step of evaporating a deposition material and depositing it on the surface of the substrate to form a protective film on the fine concave-convex structure formed on the surface of the substrate.
2. The method for manufacturing an optical component as described in claim 1, characterized in that the fine unevenness structure forming process forms the fine unevenness structure on the surface of the substrate by releasing plasma in a reduced pressure container and irradiating ions in the plasma atmosphere, and the protective film forming process forms a silicon oxide film on the fine unevenness structure on the surface of the substrate by using silicon oxide as the deposition material in the same container as the fine unevenness structure forming process and attaching silicon oxide to the surface of the substrate by vacuum deposition.
3. The method for manufacturing an optical component as described in claim 1, characterized in that the fine unevenness structure forming step forms the fine unevenness structure on the surface of the base material by releasing plasma in a reduced pressure container and irradiating ions in the plasma atmosphere, and the protective film forming step forms a silicon oxide mixed film on the fine unevenness structure on the surface of the base material in the same container as the fine unevenness structure forming step by using an organosilicon compound as the deposition material and gasifying the organosilicon compound by chemical vapor deposition.
4. The method for manufacturing an optical component as described in claim 1, characterized in that the fine unevenness structure forming step forms the fine unevenness structure on the surface of the base material by releasing plasma in a reduced pressure container and irradiating ions in the plasma atmosphere, and the protective film forming step forms a silicon oxide mixed film on the fine unevenness structure on the surface of the base material in a container different from that used for the fine unevenness structure forming step, by using an organosilicon compound as the deposition material and gasifying the organosilicon compound by chemical vapor deposition.
5. The method for manufacturing an optical component as described in claim 1, characterized in that the fine unevenness structure forming process forms the fine unevenness structure on the surface of the substrate by releasing plasma in a reduced pressure container and irradiating ions in the plasma atmosphere, and the protective film forming process forms a silicon oxide film on the fine unevenness structure on the surface of the substrate by using silicon oxide as the deposition material and attaching silicon oxide to the surface of the substrate by vacuum deposition in a container different from that used for the fine unevenness structure forming process.
6. The method for manufacturing an optical component according to claim 1, characterized in that the refractive index of the deposition material is 1.6 or less, and the optical thickness of the protective film when irradiated with light having a wavelength of 550 nm is λ / 50 to λ / 16.
7. The method for manufacturing an optical component according to claim 2 or 5, characterized in that in the protective film forming step, the optical film thickness of the silicon oxide film when irradiated with light having a wavelength of 550 nm is λ / 50 to λ / 3.
8. The method for manufacturing an optical component according to claim 3 or 4, characterized in that in the protective film formation step, the optical film thickness of the silicon oxide mixed film when irradiated with light having a wavelength of 550 nm is λ / 50 to λ / 8.
Citation Information
Patent Citations
Anti-fog coated lens
CN218298561U
Antireflection treatment of transparent substrate
JP1987143846A
Reflection preventing plate
JP1989239501A
Optical functional membrane, optical functional film, antiglare- antireflection film, manufacturing method therefor, polarizing plate, and liquid crystal display device
JP2004341541A
Method for creating nanostructures on plastic surfaces
JP2010511079A