Free-machining copper alloy and production method for free-machining copper alloy
The development of a free-cutting copper alloy with a modified β phase addresses dezincification and stress corrosion issues, reduces Pb content, and maintains strength and machinability, enhancing its performance and regulatory compliance.
Patent Information
- Application Number
- PCT/JP2024/016186
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-05
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-07
AI Technical Summary
Current free-cutting copper alloys face challenges with dezincification corrosion resistance, stress corrosion cracking resistance, and high Pb content, which are exacerbated by the need for reduced Pb content due to regulatory constraints, while maintaining good machinability and strength.
A free-cutting copper alloy with a modified β phase (β1 phase) is developed, characterized by specific compositional ranges and a unique cooling treatment process that enhances dezincification corrosion resistance, stress corrosion cracking resistance, and machinability, while reducing Pb content and maintaining high strength and ductility.
The alloy achieves improved dezincification corrosion resistance, stress corrosion cracking resistance, and machinability, with a significant reduction in Pb content, and maintains a balance of strength and ductility, comparable to conventional free-cutting brass.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Free-machining copper alloy and method for producing free-machining copper alloy
[0001] The present invention relates to a free-cutting copper alloy that has excellent corrosion resistance, particularly excellent dezincification corrosion resistance and stress corrosion cracking resistance, high strength, and a significantly reduced Pb content, and to a method for producing the free-cutting copper alloy.The free-cutting copper alloy can be used for cutting parts such as appliances and parts used in drinking water consumed daily by humans and animals, appliances and parts used in sanitary facilities such as kitchens, baths, and toilets, water meters, musical instruments, tableware, drainage appliances and parts, industrial piping parts, electrical and electronic equipment parts, automobile parts, machine parts, stationery, toys, sliding parts, instrument parts, precision machine parts, medical parts, and parts used in liquids and gases such as hydrogen, including specific parts such as water taps, mixer taps, faucet fittings, stopcocks, valves, joints, valves, shower heads, cocks, gears, shafts, bearings, shafts, sleeves, spindles, sensors, bolts, nuts, flare nuts, pen nibs, insert nuts, cap nuts, nipples, spacers, and screws.The free-cutting copper alloy and a method for producing the free-cutting copper alloy also relate to the free-cutting copper alloy. This application claims priority based on Japanese Patent Application No. 2023-075579 filed in Japan on May 1, 2023, and Japanese Patent Application No. 2023-173342 filed in Japan on October 5, 2023, the contents of which are incorporated herein by reference.
[0002] Traditionally, steel has been used for drinking water and sanitation equipment and parts, water meters, musical instruments, tableware, electrical, home appliance and electronic equipment parts, automobile parts, machine parts, stationery, precision machinery parts, medical parts, and industrial water, wastewater, and equipment and parts related to liquids and gases such as hydrogen, and parts such as water taps, mixer taps, stopcocks, valves, cocks, joints, gears, sensors, nuts and screws, etc., with excellent machinability, antibacterial properties and corrosion resistance. Generally, Cu-Zn-Pb alloys containing 56 to 65 mass% of Cu, 1 to 4 mass% of Pb, and the balance being Zn (so-called free-cutting brass rods, forging brass, and casting brass), which have good properties, or Cu-Sn-Zn-Pb alloys containing 80 to 88 mass% of Cu, 2 to 8 mass% of Sn, 1 to 8 mass% of Pb, and the balance being Zn (so-called bronze castings: gunmetal) have been used.
[0003] However, in recent years, concerns have arisen about the effects of Pb on the human body and the environment, and countries around the world are actively moving toward regulating Pb. For example, in the state of California in the United States, a regulation came into effect in January 2010 limiting the Pb content in drinking water appliances to 0.25 mass% or less. Countries other than the United States are also rapidly moving toward such regulations, and there is a demand for the development of copper alloy materials that comply with the Pb content regulations.
[0004] Furthermore, in other industrial fields such as electrical and electronic equipment, automobiles, and machinery, for example, the European RoHS Directive and ELV Directive allow the Pb content of free-cutting copper alloys to be up to 4 mass% as an exception, but as in the field of drinking water, there is active discussion about strengthening regulations on Pb content, including the elimination of the exception.
[0005] In the midst of this trend toward stricter Pb restrictions on free-cutting copper alloys, there are several options for replacing Pb-containing free-cutting copper alloys, which contain 56-65 mass% Cu, 1-4 mass% Pb, and the balance Zn, particularly free-cutting brass (JIS standard: C3604, ASTM standard: C36000, EN standard: CW614N), which contains 3 mass% Pb and is the most widely used in the world. These options include: (1) replacing Pb with Bi, which has machinability, and in some cases Therefore, (1) a Cu—Zn—Bi alloy or a Cu—Zn—Bi—Se alloy containing Se in addition to Bi, (2) a Cu—Zn alloy containing a high concentration of Zn to increase the amount of β phase and thereby improve machinability, or (3) a Cu—Zn—Si alloy containing a large amount of γ phase and κ phase instead of Pb, which have excellent machinability, and (4) a Cu—Zn—Si—Pb alloy in which the machinability of the β phase is improved by the inclusion of Si, etc. For example, in Patent Document 1, 0.3 to 4 mass%, preferably 1.8 to 3.2 mass%, of Bi is added to a Cu—Zn alloy, and since the β phase has poor dezincification corrosion resistance, the β phase is reduced and the β phase is separated by an α phase, thereby improving machinability and dezincification corrosion resistance.
[0006] However, alloys containing Bi instead of Pb have many problems, including that Bi is inferior to Pb in machinability, may be harmful to the environment and human body like Pb, is a rare metal and therefore presents resource problems, makes copper alloy materials brittle, etc. Furthermore, as shown in Patent Document 1, the β phase of Cu-Zn alloys has traditionally been poor in dezincification corrosion resistance, and as a solution to this problem, it has been essentially necessary to reduce the β phase and perform annealing to separate the β phase with an α phase.
[0007] Furthermore, although Cu-Zn binary alloys containing a large amount of β phase contribute to improving machinability, the β phase has inferior machinability compared to Pb, and is inferior in dezincification corrosion resistance and stress corrosion cracking resistance, so they cannot possibly be a substitute for Pb-containing free-cutting copper alloys. Therefore, Cu-Zn-Si alloys containing Si instead of Pb have been proposed as free-cutting copper alloys, for example, in Patent Documents 2 to 8.
[0008] In Patent Documents 2 to 7, the Cu content is roughly 58 to 65 mass% and the Si content is 0.2 to 1.5 mass%, and it is said that machinability is improved by the presence of Si contained in the β phase and fine P compounds formed from P and Zn, etc., and the area ratios of the β phase and γ phase are specified, and excellent machinability is achieved by the presence of P compounds combined with the inclusion of a small amount of Pb. However, as disclosed in Patent Document 1, it is a well-known fact that the β phase of Cu-Zn alloys has poor dezincification corrosion resistance and further poor stress corrosion cracking resistance. Therefore, Patent Documents 2 to 7 do not disclose specific data related to dezincification corrosion resistance and stress corrosion cracking resistance, and it is presumed that the dezincification corrosion resistance and stress corrosion cracking resistance, which are technical issues with the β phase of conventional Cu-Zn alloys, have not been improved. Patent Document 8 specifies the Cu content at 71.5 to 78.5 mass%, the Si content at 2.0 to 4.5 mass%, and the total area of the γ and κ phases, which are formed from an alloy with high Cu and Si concentrations and have excellent machinability, to achieve excellent machinability with a small Pb content of 0.02 mass% or less. Furthermore, by including Sn and Al in amounts of 0.1 mass% or more, a large amount of γ phase is formed, further improving machinability and corrosion resistance.
[0009] In addition, in Patent Document 9, a Cu-Zn-Sn alloy contains small amounts of Si, Pb, P, or Fe, and 0.5 mass% or less of Pb, and by devising a manufacturing method, Pb-enriched particles are dispersed in the matrix, and the number density of the Pb-enriched particles present in the α phase is increased, thereby obtaining excellent machinability. Patent Document 9 also states that a finish heat treatment at 400 to 600°C is essentially required to improve dezincification corrosion resistance.
[0010] Patent Document 10 relates to a technique for producing a near-net hollow hot forged product using a hollow material in a Cu-Zn-Si-Pb-P alloy, and proposes a copper alloy in which the area ratios of β, γ, and μ phases are limited. Patent Document 11 proposes a copper alloy casting in which Si, Pb, and Sn are selectively contained in a Cu-Zn-Zr-P alloy, and the crystal grains are refined by the action of Zr and P. Patent Document 12 proposes a copper alloy with excellent discoloration resistance in which Si and Pb are selectively contained in a Cu-Zn-Sn-Al alloy, and the area ratios of γ and β phases are limited. Patent Document 13 proposes a copper alloy casting in which Pb is not contained in a Cu-Zn-Si-Sn-Al-P alloy. Patent Document 14 proposes that the apparent Zn content is important for improving corrosion resistance in Cu-Zn-Si-Sn-Al alloys, and proposes copper alloys that substantially contain a large amount of Pb or Bi to improve machinability. Patent Document 15 describes a Cu-Zn-Si alloy containing 65 mass% or more of Cu, a Pb-free copper alloy casting with good castability and mechanical strength, and claims that the machinability is improved by the γ phase, and describes examples containing large amounts of Sn, Al, Mn, Ni, and Sb.
[0011] Japanese Patent Application Laid-Open No. 2002-003967 Japanese Patent Application Laid-Open No. 2021-042461 Japanese Patent Application Laid-Open No. 2021-042459 Japanese Patent Application Laid-Open No. 2021-042460 International Publication No. 2020 / 261666 Japanese Patent Application Laid-Open No. 2021-042462 International Publication No. 2021 / 117528 International Publication No. 2007 / 034571 Japanese Patent Application Laid-Open No. 2016-194123 International Publication No. 2013 / 065830 International Publication No. 2006 / 016630 International Publication No. 2015 / 046421 Japanese Patent Application Laid-Open No. 2010-133006 Japanese Patent Application Laid-Open No. 2018-048398 Special Publication No. 2019-508584
[0012] As shown in Patent Documents 1 to 15, no substantial improvements have been found to date in the dezincification corrosion resistance and stress corrosion cracking resistance of the β phase present in Cu—Zn alloys, which have been major technical challenges for some time. Furthermore, no disclosure has been found of a Cu—Zn alloy that exhibits low cutting resistance and excellent machinability under high-speed cutting conditions of cutting speeds exceeding 100 m / min, even when containing less than 0.2% Pb and Bi, and even when Bi is not required to be included.
[0013] The present invention has been made to solve the problems of the prior art, and an object of the present invention is to provide a free-cutting copper alloy which has excellent hot workability and machinability, and which has good dezincification corrosion resistance and stress corrosion cracking resistance despite containing a large amount of β phase (β1 phase, described below), high strength, a good balance between strength and ductility, and which has a significantly reduced Pb content, and a method for producing the free-cutting copper alloy.
[0014] To solve the above-mentioned problems and achieve the above-mentioned object, the inventors conducted extensive research and discovered the following. In this specification, unless otherwise specified, the β phase includes the β' phase, the γ phase includes the γ' phase, and the α phase includes the α' phase. The β1 phase is a modified β phase and is distinguished from the β phase and the β' phase. The β1 phase is characterized by the observation of grain boundary patterns, i.e., crystal grain boundaries, within the β1 phase when observed under a metallurgical microscope using hydrogen peroxide and aqueous ammonia as an etching solution. The β phase present in common Cu—Zn alloys, Cu—Zn—Bi alloys, Cu—Zn—Si alloys, etc., does not exhibit crystal grain boundaries even when etched with hydrogen peroxide and aqueous ammonia. Therefore, the β phase and the β1 phase can be clearly distinguished. Crystal grain boundaries are sometimes simply referred to as grain boundaries. Hot-worked materials include hot-extruded materials, hot-forged materials, and hot-rolled materials. Cold workability refers to the performance of cold processing such as drawing, wire drawing, rolling, crimping, and bending. Unless otherwise specified, good or excellent machinability refers to low cutting resistance during peripheral cutting using a lathe and good or excellent chip breakability. Conductivity refers to electrical conductivity, thermal conductivity, and electrical conductivity. Cooling rate refers to the average cooling rate within a certain temperature range. One day and night means one day. Actual operation means manufacturing using actual mass production equipment.
[0015] The above-mentioned Patent Document 8 states that the β phase in a Cu-Zn-Si alloy does not contribute much to the machinability of the copper alloy, but rather impairs it. Patent Documents 10, 11, and 12 also significantly limit the amount of β phase. Patent Document 1 states that, as a method for improving the dezincification corrosion resistance of the β phase, a process of annealing at 350 to 550°C is required to reduce the β phase and divide the β phase with the α phase. Patent Document 9 states that, to improve the dezincification corrosion resistance of the β phase, a process of containing more Sn than Si is required, and that the alloy is heated to a temperature of 700 to 850°C, hot extruded, and subjected to a finish heat treatment at 400 to 600°C for 30 minutes or more, with an average cooling rate from 400 to 200°C of 0.2 to 10°C / second.
[0016] On the other hand, Patent Documents 2 to 7 discovered that in Cu-Zn-Si alloys, the inclusion of a certain amount of Si in the β phase significantly improves the machinability of the β phase itself. They then state that the synergistic effects of the three elements—the presence of fine P compounds, a small amount of Pb, and possibly Bi—result in the alloy's excellent machinability. However, to ensure the presence of P compounds, an average cooling rate of approximately 0.1°C / min to approximately 70°C / min is required in the temperature range from approximately 530°C to approximately 450°C after hot working. Patent Documents 2 to 7 do not disclose data related to dezincification corrosion resistance or stress corrosion cracking resistance. Furthermore, they make no mention of modifying the β phase itself. In other words, it is presumed that the β phase present in Cu-Zn-Si alloys does not improve its dezincification corrosion resistance or stress corrosion cracking resistance, nor does it further improve its machinability.
[0017] The inventors further attempted to modify the β phase itself in Cu—Zn—Si alloys. As a result of extensive research, they found that even without the presence of P compounds, the modified β phase, i.e., the β1 phase, further improved machinability, particularly during high-speed cutting, without the essential inclusion of Bi. They also significantly improved the dezincification corrosion resistance and stress corrosion cracking resistance of the β phase, which had long been issues with Cu—Zn alloys. In addition, alloys containing the β1 phase instead of the β phase were able to further increase strength without impairing ductility. This β1 phase can be obtained by first solid-solving a certain amount of Si and P within the β phase, and then maintaining the β phase at 500–670°C and increasing the cooling rate during cooling to room temperature, thereby maintaining the high-temperature metallographic structure at room temperature.
[0018] The β1 phase can be easily distinguished from the β phase of Cu-Zn alloys. The surface is mirror-polished and etched with a mixture of hydrogen peroxide and aqueous ammonia. For etching, an aqueous solution containing 3 mL of 3 vol% hydrogen peroxide and 22 mL of 14 vol% aqueous ammonia is used. When the polished metal surface is immersed in this solution for approximately 2 to 10 seconds at room temperature (approximately 15 to 25°C) and observed under a metallurgical microscope at 200 to 1000 magnifications, grain boundary patterns, i.e., crystal grain boundaries, are visible within the β1 phase, whereas crystal grain boundaries are not observed within the β phase of ordinary Cu-Zn alloys. The use of this etching solution is also disclosed in Patent Documents 2 to 7, 10, and 11, and metal structures are published in those documents.
[0019] To obtain the β1 phase, i.e., to maintain the β phase state at 500-670°C after hot working and bring it down to room temperature, the cooling process after hot working requires that the hot-worked material be cooled at a temperature lower than 670°C but higher than 500°C, and that the cooling be performed at an average cooling rate of more than 300°C / min in the temperature range from the cooling start temperature to 500°C, followed by cooling at an average cooling rate of at least 300°C / min in the temperature range from 500°C to 300°C. In this specification, unless otherwise specified, cooling refers to controlling the cooling rate by water cooling or a similar method, rather than natural cooling. Patent Documents 2 to 7 state that, in order to obtain fine P-containing compounds, the hot-worked material must be cooled at an average cooling rate of at least about 0.1°C / min and not more than about 70°C / min in the temperature range from about 530°C to about 450°C after hot working. In other words, it is clear that the present application and Patent Documents 2 to 7 are heading in opposite directions (teaching opposites). However, for example, if the cooling rate around 520°C after hot working is 60°C / min and the average cooling rate in the temperature range from 520°C to 500°C, which is the cooling treatment start temperature, exceeds 300°C / min, an alloy containing both the β1 phase and P compounds may exist in the present application as well.
[0020] The β1 phase in this application significantly improves the machinability of Cu-Zn-Si alloys, particularly in high-speed cutting, even without the P compounds disclosed in Patent Documents 2 to 7. Furthermore, the synergistic effect of the β1 phase and fine Pb particles or particles containing Pb and Bi reduces cutting resistance and promotes chip fragmentation. More importantly, the dezincification corrosion resistance and stress corrosion cracking resistance, which were previously unresolved issues with the conventional β phase, are significantly improved and resolved by converting the β phase to the β1 phase. Furthermore, the mechanical properties of the alloy retain the high strength of the conventional β phase, while improving ductility, resulting in even higher strength and a better balance between strength and ductility. As a result, we have invented a copper alloy that has machinability comparable to that of conventional free-cutting brass, but has better dezincification corrosion resistance and stress corrosion cracking resistance and higher strength than conventional free-cutting brass.
[0021] A free-cutting copper alloy according to a first aspect of the present invention contains more than 60.5 mass% and less than 65.0 mass% Cu, more than 0.50 mass% and less than 1.20 mass% Si, 0.002 mass% or more and less than 0.20 mass% Pb, and more than 0.01 mass% and less than 0.18 mass% P, and contains, as an optional element, 0.0001 mass% or more and less than 0.20 mass% Bi, with the balance consisting of Zn and inevitable impurities, wherein the total content of Fe, Mn, Co, and Cr among the inevitable impurities is less than 0.40 mass%, and the content of Al is less than 0.30 mass%, the content of Cu is [Cu] mass%, the content of Si is [Si] mass%, When the Pb content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, the relationship of 57.5≦f1=[Cu]−4.6×[Si]+0.5×([Pb]+[Bi])−[P]≦60.5 is satisfied. When Bi is contained, the relationship of 0.003≦f2=[Pb]+[Bi]<0.20 is also satisfied. In addition, when the area ratio of the α phase, the area ratio of the γ phase, and the area ratio of the β1 phase, which is a modified β phase, are (α)%, and (γ)%, respectively, in the constituent phases of the metallographic structure excluding non-metallic inclusions, the following relationships are satisfied: 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, and 27<f6=(β1)×([Si]). 1/2-(γ)×2+([Pb]+[Bi]) 1/2 × 20 + ([P]) 1/2 ×15, and the β1 phase is characterized in that the grain boundaries are observable when etched with a mixed solution of hydrogen peroxide and aqueous ammonia.
[0022] A free-cutting copper alloy according to a second aspect of the present invention comprises 61.2 mass% to 64.8 mass% Cu, 0.65 mass% to 1.10 mass% Si, 0.003 mass% to less than 0.10 mass% Pb, and 0.03 mass% to 0.15 mass% P, and optionally 0.001 mass% to less than 0.10 mass% Bi, with the balance consisting of Zn and inevitable impurities, wherein the total content of Fe, Mn, Co, and Cr among the inevitable impurities is less than 0.30 mass%, and the content of Al is less than 0.15 mass%, the content of Cu is [Cu] mass%, the content of Si is [Si] mass%, When the Pb content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, the relationship of 58.0≦f1=[Cu]−4.6×[Si]+0.5×([Pb]+[Bi])−[P]≦60.2 is satisfied. When Bi is contained, the relationship of 0.004≦f2=[Pb]+[Bi]<0.10 is also satisfied. In addition, when the area ratio of the α phase, the area ratio of the γ phase, and the area ratio of the β1 phase, which is a modified β phase, are (α)%, and (γ)%, respectively, in the constituent phases of the metallographic structure excluding non-metallic inclusions, the following relationships are satisfied: 30≦f3=(α)≦70, 30≦f4=(β1)≦70, 0≦f5=(γ)<1, and 35<f6=(β1)×([Si]). 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 × 20 + ([P]) 1/2 ×15, and the β1 phase is characterized in that the grain boundaries are observable when etched with a mixed solution of hydrogen peroxide and aqueous ammonia.
[0023] The free-cutting copper alloy of embodiment 3 of the present invention contains more than 60.5 mass% and less than 65.0 mass% Cu, more than 0.50 mass% and less than 1.20 mass% Si, 0.002 mass% or more and less than 0.20 mass% Pb, more than 0.01 mass% and less than 0.18 mass% P, and more than 0.05 mass% and less than 0.90 mass% Sn, and optionally contains 0. The alloy contains 0.001 mass% or more and less than 0.20 mass% Bi, with the balance being Zn and inevitable impurities, and among the inevitable impurities, the total content of Fe, Mn, Co, and Cr is less than 0.40 mass%, and the Al content is less than 0.30 mass%, the Cu content is [Cu] mass%, the Si content is [Si] mass%, and the Pb content is [Pb] mass%. mass%, the P content is [P] mass%, the Bi content is [Bi] mass%, and the Sn content is [Sn] mass%, then the relationship of 57.5≦f1=[Cu]−4.6×[Si]+0.5×([Pb]+[Bi])−[P]−[Sn]≦60.5 is satisfied, and the relationship of f0=[Sn] / [Si]<1 is also satisfied, and when Bi is contained, the relationship of 0.00 The relationship of 3≦f2=[Pb]+[Bi]<0.20 is satisfied, and in the constituent phases of the metal structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, then 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, 27<f6=(β1)×([Si]). 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 × 20 + ([P]) 1/2 ×15, and the β1 phase is characterized in that the grain boundaries are observable when etched with a mixed solution of hydrogen peroxide and aqueous ammonia.
[0024] The free-cutting copper alloy of aspect 4 of the present invention contains 61.2 mass% or more and 64.8 mass% or less of Cu, 0.65 mass% or more and 1.10 mass% or less of Si, 0.003 mass% or more and less than 0.10 mass% of Pb, 0.03 mass% or more and 0.15 mass% or less of P, and 0.10 mass% or more and less than 0.50 mass% of Sn, and optionally contains: The alloy contains 0.001 mass% or more and less than 0.10 mass% Bi, with the balance being Zn and inevitable impurities, and among the inevitable impurities, the total content of Fe, Mn, Co, and Cr is less than 0.30 mass%, and the Al content is less than 0.15 mass%. The Cu content is [Cu] mass%, the Si content is [Si] mass%, and the Pb content is [P When the P content is [P] mass%, the Bi content is [Bi] mass%, and the Sn content is [Sn] mass%, the relationship of 58.0≦f1=[Cu]−4.6×[Si]+0.5×([Pb]+[Bi])−[P]−[Sn]≦60.2 is satisfied, and the relationship of f0=[Sn] / [Si]<0.6 is further satisfied, and when Bi is contained, the relationship of 0.004 ≦f2=[Pb]+[Bi]<0.10, and in the constituent phases of the metal structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, the following relationships hold: 30≦f3=(α)≦70, 30≦f4=(β1)≦70, 0≦f5=(γ)<1, 35<f6=(β1)×([Si]). 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 × 20 + ([P]) 1/2 ×15, and the β1 phase is characterized in that the grain boundaries are observable when etched with a mixed solution of hydrogen peroxide and aqueous ammonia.
[0025] The free-cutting copper alloy of Aspect 5 of the present invention is the free-cutting copper alloy of any one of Aspects 1 to 4 of the present invention, characterized in that it is used for appliances and parts relating to drinking water and sanitation facilities, valves, cocks, industrial piping parts, water meters, musical instruments, automobile parts, electric and electronic equipment parts, machine parts, stationery, toys, sliding parts, instrument parts, precision machine parts, and medical parts.
[0026] A method for producing a free-cutting copper alloy according to Aspect 6 of the present invention is a method for producing the free-cutting copper alloy according to any one of Aspects 1 to 4 of the present invention, comprising one or more hot working steps, wherein the hot working temperature in the final hot working step is greater than 540°C and less than 750°C, and the cooling process after the hot working starts with the hot-worked material at a temperature lower than 670°C and higher than 500°C, and the average cooling rate in the cooling process from the cooling start temperature to 500°C exceeds 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C exceeds 300°C / min.
[0027] A method for producing a free-cutting copper alloy according to Aspect 7 of the present invention is a method for producing the free-cutting copper alloy according to any one of Aspects 1 to 4 of the present invention, comprising one or more hot working steps and heat treatment steps, characterized in that in the final heat treatment step, the alloy is annealed at a temperature above 520°C and lower than 630°C for a holding time of 1 minute to 5 hours, and after annealing, a cooling treatment is initiated at a temperature above 500°C, and the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C exceeds 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C exceeds 300°C / min.
[0028] According to one aspect of the present invention, it is possible to provide a free-cutting copper alloy that has excellent hot workability, good machinability, dezincification corrosion resistance, and stress corrosion cracking resistance, high strength, an excellent balance between strength and ductility, and a significantly reduced Pb content, and a method for producing the free-cutting copper alloy.
[0029] 1A is a microstructure observation photograph of a copper alloy according to an embodiment. The copper alloy was obtained by subjecting Alloy No. S01 to Process No. A2. Specifically, Alloy No. S01 has a composition of Zn-63.3 mass% Cu-0.95 mass% Si-0.069 mass% P-0.063 mass% Pb-0.017 mass% Bi. In Process No. A2, hot extrusion was performed at 630°C, and cooling treatment was initiated at 580°C. The average cooling rates in the temperature range from 580°C to 300°C and in the temperature range from 500°C to 300°C were both 1020°C / min. The alloy of FIG. 1A was subjected to a dezincification corrosion test in accordance with the ISO 6509 test method. The cross-sectional metallographic photograph includes a portion exhibiting maximum corrosion depth. This is a photograph of the structure of a copper alloy according to an embodiment. The copper alloy was obtained by subjecting Alloy No. S11 to Process No. E2. Specifically, Alloy No. S11 has a composition of Zn-62.5 mass% Cu-0.96 mass% Si-0.064 mass% P-0.072 mass% Pb. In Process No. E2, hot extrusion was performed at 550°C, and an average cooling rate of 20°C / min was set in the temperature range from 500°C to 300°C to obtain a rod having a diameter of 50 mm and a length of 200 mm. The rod was heated, placed horizontally, and hot forged at 680°C to a thickness of 20 mm. Cooling treatment was initiated at 565°C, and the average cooling rates in the temperature range from 565°C to 300°C and in the temperature range from 500°C to 300°C were both 900°C / min. 2A shows the results of a dezincification corrosion test performed on the alloy in accordance with the ISO 6509 test method, and is a cross-sectional metallographic photograph including the portion exhibiting the maximum corrosion depth. This is a microstructure observation photograph of a copper alloy according to an embodiment, in which the copper alloy was obtained by subjecting Alloy No. S11 to Process No. E13H. Specifically, Alloy No. S11 has a composition of Zn-62.5 mass% Cu-0.96 mass% Si-0.064 mass% P-0.072 mass% Pb. In Process No. E13H, the alloy was hot extruded at 550°C, and an average cooling rate of 20°C / min was set in the temperature range from 500°C to 300°C to obtain a rod having a diameter of 50 mm and a length of 200 mm. The rod was heated, placed horizontally, and hot forged at 630°C to a thickness of 20 mm, followed by cooling at an average cooling rate of 35°C / min.Next, cooling treatment was initiated at 455°C, and the average cooling rate in the temperature range from 455°C to 300°C was 800°C / min. The alloy of FIG. 3A and the alloy of FIG. 2A differ in the cooling treatment start temperature. This is a cross-sectional metallographic photograph including the portion exhibiting the maximum corrosion depth, showing the results of a dezincification corrosion test performed on the alloy of FIG. 3A in accordance with the ISO 6509 test method. This is a photograph of the microstructure of a copper alloy according to an embodiment, obtained by performing Process No. E6 on Alloy No. S43. Specifically, Alloy No. S43 has a composition of Zn-63.3 mass% Cu-0.98 mass% Si-0.084 mass% P-0.060 mass% Pb-0.28 mass% Sn. Process No. For E6, a casting cast into a 55 mm diameter mold was cut to a diameter of 50 mm and a length of 200 mm. The casting was heated, placed horizontally, and hot forged at 630°C to a thickness of 20 mm. Cooling treatment was initiated at 565°C, with the average cooling rates in the temperature range from 565°C to 300°C and in the temperature range from 500°C to 300°C both being 900°C / min. This shows the results of a dezincification corrosion test performed on the alloy of FIG. 4A in accordance with the ISO 6509 test method, and is a cross-sectional metallographic photograph including the portion exhibiting the maximum corrosion depth. This is a microstructure observation photograph of a copper alloy according to an embodiment, where the copper alloy was obtained by performing Process No. A34H and Process No. G1 on Alloy No. S02. Specifically, Alloy No. S02 has a composition of Zn-62.9 mass% Cu-0.98 mass% Si-0.071 mass% P-0.071 mass% Pb. In Process No. A34H, an alloy was obtained by hot extrusion at 615°C, with an average cooling rate of 18°C / min from 500°C to 300°C. In Process No. G1, this alloy was further heated at 580°C for 30 minutes, and cooling treatment was started from 560°C, with the average cooling rates in the temperature range from 560°C to 300°C and in the temperature range from 500°C to 300°C both being 1800°C / min. This is a cross-sectional metallographic photograph showing the results of a dezincification corrosion test performed on the alloy of FIG. 5A in accordance with the ISO 6509 test method, including a portion exhibiting maximum corrosion depth. This is a microstructure observation photograph of a copper alloy in an embodiment, where the copper alloy is Alloy No. S02 was subjected to step No. E14H.Specifically, Alloy No. S02 has a composition of Zn-62.9 mass% Cu-0.98 mass% Si-0.071 mass% P-0.071 mass% Pb. In Process No. E14H, hot extrusion was performed at 550°C, and an average cooling rate of 20°C / min from 500°C to 300°C was used to obtain a rod having a diameter of 50 mm and a length of 200 mm. The rod was heated, placed horizontally, and hot forged at 630°C to a thickness of 20 mm, followed by natural cooling. The average cooling rate in the temperature range from 500°C to 300°C was 25°C / min. The alloy in Figure 6A was subjected to a dezincification corrosion test in accordance with the ISO 6509 test method. This is a cross-sectional metallographic photograph including the area exhibiting the maximum corrosion depth.
[0030] The free-cutting copper alloy and the method for producing the free-cutting copper alloy according to the embodiment of the present invention will be described below. Examples of applications include drinking water and sanitary equipment, instruments, tableware, electrical, home appliance, and electronic equipment parts, automobile parts, machine parts, stationery, precision machine parts, medical parts, and equipment and parts related to industrial water, wastewater, hydrogen, and other liquids and gases. Specific examples of parts include water taps, mixer taps, stop valves, valves, cocks, joints, water meters, gears, sensors, nuts, screws, etc.
[0031] In this specification, an element symbol in parentheses, such as [Zn], indicates the content (mass%) of that element. In this embodiment, this content representation method is used to define the compositional formulas f1, f2, and f0 as follows: The compositional formula f1 = [Cu] - 4.6 x [Si] + 0.5 x ([Pb] + [Bi]) - [P]. When Sn is contained in an amount exceeding 0.05 mass%, the compositional formula f1 = [Cu] - 4.6 x [Si] + 0.5 x ([Pb] + [Bi]) - [P] - [Sn]. When Bi is contained, the compositional formula f2 = [Pb] + [Bi]. When Sn is contained, the compositional formula f0 = [Sn] / [Si].
[0032] Furthermore, in this embodiment, in the constituent phases of the metal structure excluding non-metallic inclusions, the area ratio of the α phase is represented by (α)%, the area ratio of the γ phase by (γ)%, the area ratio of the unmodified β phase by (β)%, and the area ratio of the modified β1 phase by (β1)%. The area ratio of each phase is also referred to as the amount of each phase, the proportion of each phase, or the proportion occupied by each phase. In this embodiment, multiple structure relational equations are defined as follows: Structure relational equation f3 = (α) Structure relational equation f4 = (β1) Structure relational equation f4A = (β) Structure relational equation f5 = (γ) Structure-composition relational equation f6 = (β1) × ([Si]) 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 × 20 + ([P]) 1/2 x15
[0033] A free-cutting copper alloy according to a first embodiment of the present invention contains more than 60.5 mass% and less than 65.0 mass% Cu, more than 0.50 mass% and less than 1.20 mass% Si, 0.002 mass% or more and less than 0.20 mass% Pb, and more than 0.01 mass% and less than 0.18 mass% P, and contains, as an optional element, 0.0001 mass% or more and less than 0.20 mass% Bi, with the balance consisting of Zn and inevitable impurities, wherein the total content of Fe, Mn, Co, and Cr among the inevitable impurities is less than 0.40 mass%, and the content of Al is less than 0.30 mass%, the content of Cu is [Cu] mass%, the content of Si is [Si] mass%, When the Cu content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, the relationship of 57.5≦f1=[Cu]−4.6×[Si]+0.5×([Pb]+[Bi])−[P]≦60.5 is satisfied, and when Bi is contained, the relationship of 0.003≦f2=[Pb]+[Bi]<0.20 is satisfied. In addition, in the constituent phases of the metal structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, the following relationships are satisfied: 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, 27<f6=(β1)×([Si]). 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 × 20 + ([P])1/2 ×15, and the β1 phase is characterized in that the grain boundaries are observable when etched with a mixture of hydrogen peroxide and aqueous ammonia.
[0034] A free-cutting copper alloy according to a second embodiment of the present invention contains 61.2 mass% or more and 64.8 mass% or less of Cu, 0.65 mass% or more and 1.10 mass% or less of Si, 0.003 mass% or more and less than 0.10 mass% of Pb, and 0.03 mass% or more and 0.15 mass% or less of P, and optionally contains 0.001 mass% or more and less than 0.10 mass% of Bi, with the balance being Zn and inevitable impurities, wherein the total content of Fe, Mn, Co, and Cr among the inevitable impurities is less than 0.30 mass%, and the content of Al is less than 0.15 mass%, the content of Cu is [Cu] mass%, the content of Si is [Si] mass%, When the Cu content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, the relationship of 58.0≦f1=[Cu]−4.6×[Si]+0.5×([Pb]+[Bi])−[P]≦60.2 is satisfied, and when Bi is contained, the relationship of 0.004≦f2=[Pb]+[Bi]<0.10 is satisfied. In addition, in the constituent phases of the metal structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, the following relationships are satisfied: 30≦f3=(α)≦70, 30≦f4=(β1)≦70, 0≦f5=(γ)<1, 35<f6=(β1)×([Si]). 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 × 20 + ([P]) 1/2 ×15, and the β1 phase is characterized in that the grain boundaries are observable when etched with a mixture of hydrogen peroxide and aqueous ammonia.
[0035] A free-cutting copper alloy according to a third embodiment of the present invention contains more than 60.5 mass% and less than 65.0 mass% Cu, more than 0.50 mass% and less than 1.20 mass% Si, 0.002 mass% or more and less than 0.20 mass% Pb, more than 0.01 mass% and less than 0.18 mass% P, and more than 0.05 mass% and less than 0.90 mass% Sn, and any optional elements. The alloy contains 0.0001 mass% or more and less than 0.20 mass% Bi, with the balance consisting of Zn and inevitable impurities, and among the inevitable impurities, the total content of Fe, Mn, Co, and Cr is less than 0.40 mass%, and the Al content is less than 0.30 mass%, the Cu content is [Cu] mass%, the Si content is [Si] mass%, and the Pb content is [ When the P content is [Pb] mass%, the P content is [P] mass%, the Bi content is [Bi] mass%, and the Sn content is [Sn] mass%, the relationship of 57.5≦f1=[Cu]−4.6×[Si]+0.5×([Pb]+[Bi])−[P]−[Sn]≦60.5 is satisfied, and the relationship of f0=[Sn] / [Si]<1 is also satisfied, and when Bi is contained, the relationship of 0.0 03≦f2=[Pb]+[Bi]<0.20, and in the constituent phases of the metal structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, the following relationships hold: 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, 27<f6=(β1)×([Si]). 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 × 20 + ([P]) 1/2 ×15, and the β1 phase is characterized in that the grain boundaries are observable when etched with a mixture of hydrogen peroxide and aqueous ammonia.
[0036] A free-cutting copper alloy according to a fourth embodiment of the present invention contains 61.2 mass% or more and 64.8 mass% or less of Cu, 0.65 mass% or more and 1.10 mass% or less of Si, 0.003 mass% or more and less than 0.10 mass% of Pb, 0.03 mass% or more and 0.15 mass% or less of P, and 0.10 mass% or more and less than 0.50 mass% of Sn, and any optional elements. The alloy contains 0.001 mass% or more and less than 0.10 mass% Bi, with the balance consisting of Zn and inevitable impurities, and among the inevitable impurities, the total content of Fe, Mn, Co, and Cr is less than 0.30 mass%, and the content of Al is less than 0.15 mass%, the content of Cu is [Cu] mass%, the content of Si is [Si] mass%, and the content of Pb is is [Pb] mass%, the P content is [P] mass%, the Bi content is [Bi] mass%, and the Sn content is [Sn] mass%, the relationship of 58.0≦f1=[Cu]−4.6×[Si]+0.5×([Pb]+[Bi])−[P]−[Sn]≦60.2 is satisfied, and the relationship of f0=[Sn] / [Si]<0.6 is also satisfied, and when Bi is contained, the relationship of 0.0 The relationship of 04≦f2=[Pb]+[Bi]<0.10 is satisfied, and in the constituent phases of the metal structure excluding non-metallic inclusions, when the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, then 30≦f3=(α)≦70, 30≦f4=(β1)≦70, 0≦f5=(γ)<1, 35<f6=(β1)×([Si]). 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 × 20 + ([P]) 1/2 ×15, and the β1 phase is characterized in that the grain boundaries are observable when etched with a mixture of hydrogen peroxide and aqueous ammonia.
[0037] The reasons for defining the chemical composition, compositional relational formulas f0, f1, and f2, structure relational formulas f3, f4, and f5, structure-composition relational formula f6, metal structure, and the like as described above will be explained below.
[0038] <Component Composition> (Cu) Cu is the main element of the free-cutting copper alloy of this embodiment. To overcome the problems of the present invention, it is necessary to contain at least 60.5 mass% Cu. If the Cu content is 60.5 mass% or less, depending on the contents of Si, Zn, P, Pb, Bi, and Sn and the manufacturing process, the proportion of the β1 phase exceeds 80%, resulting in low ductility. Furthermore, the β phase is not sufficiently modified, resulting in poor dezincification corrosion resistance, stress corrosion cracking resistance, and machinability. Therefore, the lower limit of the Cu content is more than 60.5 mass%, preferably 61.2 mass% or more, more preferably 61.5 mass% or more, and even more preferably 62.0 mass% or more. On the other hand, if the Cu content is 65.0 mass% or more, the proportion of the β1 phase decreases, although this depends on the contents of Si, Zn, P, Pb, Bi, and Sn and the manufacturing process. As a result, excellent machinability cannot be obtained and strength also decreases. Therefore, the Cu content is less than 65.0 mass%, preferably 64.8 mass% or less, and more preferably 64.5 mass% or less.
[0039] (Si) Si is a major element in the free-cutting copper alloy of this embodiment, and Si contributes to the formation of metal phases such as the kappa, gamma, mu, beta, beta1, and zeta phases. By containing Cu, Zn, Si, and P in the above-mentioned ranges and adding a process, the beta phase is modified, and the beta1 phase is generated after a predetermined cooling treatment, as described below. The beta1 phase (modified beta phase) improves machinability while significantly improving the dezincification corrosion resistance and stress corrosion cracking resistance that were drawbacks of conventional beta phases. The typical composition of the modified beta1 phase is approximately 61 mass% Cu, approximately 1.2 mass% Si, approximately 37.5 mass% Zn, and approximately 0.1 mass% P.
[0040] On the other hand, a typical composition of the α phase is approximately 66 mass% Cu, approximately 0.7 mass% Si, and approximately 33 mass% Zn. Within the composition range of this embodiment, the inclusion of Si slightly improves the machinability of the α phase, while the inclusion of Si improves the dezincification corrosion resistance and stress corrosion cracking resistance of the α phase. The modified β1 phase and the improved α phase particularly improve the dezincification corrosion resistance and stress corrosion cracking resistance of the alloy. Note that a certain amount of α phase is required to modify the β phase; for example, if there is no α phase at all, the β phase will not be modified. To improve the dezincification corrosion resistance, stress corrosion cracking resistance, ductility, and machinability of the alloy, the α phase must have an area fraction of 20% or more, preferably 30% or more.
[0041] Si is an essential element for modifying the β phase to the β1 phase. The higher the Si content, the more the β phase is modified, resulting in a β1 phase with better properties. To modify the β phase and obtain a more modified β1 phase, the Si content must exceed 0.50 mass%. The Si content is preferably 0.60 mass% or more, more preferably 0.65 mass% or more, and even more preferably 0.75 mass% or more. On the other hand, once the Si content reaches a predetermined amount, the modification of the β1 phase saturates. Furthermore, if the Si content is too high, the conductivity decreases. In some cases, a γ phase appears, resulting in poor dezincification corrosion resistance, stress corrosion cracking resistance, and machinability. Patent Documents 2 to 8 state that the γ phase improves machinability. However, in the present invention, which is mainly composed of β1 phase and α phase, the presence of γ phase actually worsens machinability, reduces the ductility of the alloy, and deteriorates dezincification corrosion resistance and stress corrosion cracking resistance. Therefore, it is preferable to limit the amount of Si and the amount of γ phase. For these reasons, the amount of Si is less than 1.20 mass%, preferably 1.10 mass% or less. If conductivity is important, the amount of Si is 1.0 mass% or less.
[0042] (Zn) Zn, together with Cu and Si, is a major constituent element of the free-cutting copper alloy of this embodiment, and is an element necessary for improving machinability, strength, high-temperature properties, and castability. Although Zn is the balance, if forced to state, the Zn content is less than about 38.5 mass%, preferably less than 38.0 mass%, and more than about 32.0 mass%, preferably more than 33.0 mass%.
[0043] (P) Like Si, P is an essential element for reforming the β phase to the β1 phase. During hot working, P dissolves in the β phase. During cooling after hot working, the cooling process begins at a temperature above 500°C and below 670°C. By cooling at a cooling rate of more than 300°C / min in the temperature range from the start of the cooling process to 500°C and the temperature range from 500°C to 300°C, the β phase is reformed to the β1 phase, and the β1 phase is obtained. The reformation of the β phase to the β1 phase significantly improves the dezincification corrosion resistance and stress corrosion cracking resistance, which were issues with the conventional β phase. At the same time, the presence of the β1 phase reduces cutting resistance and improves chip separability during cutting. However, P-containing compounds reduce cutting resistance and improve chip breakability. However, when cooling is initiated at a rate of more than 300°C / min from a temperature above about 550°C or 530°C, P-containing compounds are absent or present in small amounts. From the viewpoint of improving machinability, the effect of modifying the β-phase to the β1-phase is greater than the effect of the presence of P-containing compounds in the β-phase. Particularly in the case of high-speed cutting exceeding about 100 m / min, the modification of the β-phase to the β1-phase provides better machinability than the presence of P-containing compounds in the β-phase. Furthermore, the inclusion of P improves the dezincification corrosion resistance and stress corrosion cracking resistance of the α-phase, leading to a significant improvement in the dezincification corrosion resistance and stress corrosion cracking resistance of alloys consisting of the β1-phase and the α-phase.
[0044] To reform the β phase into the β1 phase, the lower limit of the P content must be at least 0.01 mass%. Considering the amount of unavoidable impurities, the cooling treatment start temperature, and the cooling rate after the start of the cooling treatment (described later), the P content is preferably 0.03 mass% or more, more preferably 0.04 mass% or more. P easily forms compounds with Zn, Si, Mn, Fe, Cr, Co, Al, and the like. If P forms compounds and the amount of P dissolved in the β phase of the alloy after hot working decreases, the reforming of the β phase into the β1 phase is hindered. The formation of compounds between Zn and Si, the main elements of the present alloy, and P begins at approximately 550°C, and the amount of P compounds increases as the cooling rate slows. The formation of compounds between the inevitable impurities Mn, Fe, Cr, and Co and P begins at temperatures above about 550°C, and as their amounts increase, the formation of P compounds is further promoted. In other words, the presence of Mn, Fe, Cr, and Co hinders the transformation to the β1 phase, resulting in increased cutting resistance, poor chip separability, and poor dezincification corrosion resistance and stress corrosion cracking resistance. Therefore, the total content of at least Fe, Mn, Co, and Cr must be less than 0.40 mass%, preferably less than 0.30 mass%.
[0045] The formation of P-Zn and Si compounds has a positive effect on machinability, but the transformation of the β phase to the β1 phase and the presence of P-Zn and Si compounds are contradictory. As mentioned above, to form the β1 phase, after hot working, the cooling treatment must be initiated at a temperature above 500°C and below 670°C, and the cooling rate must be fast in the temperature range from the start of the cooling treatment to 300°C. On the other hand, to fully form P-Zn and Si compounds, slow cooling in the temperature range from about 530°C to about 450°C is required. Therefore, when a large amount of P compounds is formed, the formation of the β1 phase is slightly insufficient, i.e., the transformation of the β phase is slightly insufficient. Or, the β1 phase may not exist.
[0046] On the other hand, even if P is contained in an amount of 0.18 mass% or more, the effect of forming the β1 phase is already saturated, and the P dissolved in the β1 phase reduces ductility and electrical conductivity. Therefore, the P content is less than 0.18 mass%, preferably 0.15 mass% or less, and more preferably 0.12 mass% or less.
[0047] (Pb) In this embodiment, the β1 phase containing Si and P provides good machinability for the alloy, but the inclusion of a small amount of Pb further improves machinability. In the composition of this embodiment, approximately 0.001 mass% of Pb is dissolved in the matrix, and any excess Pb exists as fine Pb particles with diameters of approximately 0.1 to 2 μm. It is generally believed that a Pb content of approximately 0.1 mass% does not contribute much to improving machinability. For example, ASM Specialty Handbook, Copper and Copper Alloys, first edition, August 2001, p. 267, Fig. 6, shows the relationship between Pb content and machinability, assuming that the machinability of a Cu-Zn-Pb alloy containing 62-65 mass% Cu, approximately 3.2 mass% Pb, and the remainder Zn is 100%. It shows that a Pb content of 0.1 mass% only improves machinability by approximately 5%, reducing the machinability index from approximately 25% to approximately 30%. In contrast, in the present application, even trace amounts of Pb have a significant effect on machinability, and a Pb content of 0.002 mass% or more is effective. The Pb content is preferably 0.003 mass% or more, and more preferably 0.01 mass% or more. Furthermore, when cutting conditions become severe, such as when the cutting speed increases, the feed rate increases, the depth of cut increases, or the drill hole diameter increases, the Pb content is preferably 0.03 mass% or more. The machinability of the alloy is significantly improved by the inclusion of a small amount of Pb and a β1 phase with significantly improved machinability. It is well known that Pb improves the machinability of copper alloys. To achieve this, approximately 3 mass% of Pb is required in a Cu-Zn binary alloy, as exemplified by free-cutting brass bar C3604. In this embodiment, an alloy with excellent machinability is completed by incorporating a β1 phase containing Si and P and a small amount of Pb particles, or Pb and Bi particles (described later) in the metal structure. On the other hand, because Pb is harmful to the human body, the upper limit of Pb is set to less than 0.20 mass%. Furthermore, the Pb content is preferably less than 0.10 mass %, and in consideration of the effects on the human body and the environment, it is optimally 0.08 mass % or less.
[0048] (Bi) Like Pb, Bi dissolves in the matrix at approximately 0.0001 mass%, and any excess Bi exists as particles with diameters of approximately 0.1 to 2 μm. When both Pb and Bi are added, the Pb and Bi mixture generally exists as particles with diameters of approximately 0.1 to 2 μm. In this embodiment, it was found that by incorporating Bi together with Pb in the presence of the β1 phase, machinability equivalent to or superior to that achieved when Pb and Bi were each contained alone can be achieved. While the machinability-improving function of Bi was previously considered inferior to that of Pb, this embodiment has been found to exhibit the same effect as, and in some cases even greater than, Pb. Incidentally, Bi deteriorates the stress corrosion cracking resistance of brass, but when it exists as a mixture of Pb and Bi particles, or when the Bi content is small, its effect on stress corrosion cracking is almost eliminated.
[0049] When Bi is contained, at least 0.0001 mass% or more of Bi is required to have good machinability as an alloy. The Bi content is preferably 0.001 mass% or more, more preferably 0.002 mass% or more. Although the effects of Bi on the human body are currently unknown, the amount of Bi is less than 0.20 mass%, preferably less than 0.10 mass%, and even more preferably 0.08 mass% or less. As described above, in this embodiment, taking into consideration that Bi can satisfactorily substitute for Pb, the effects of Bi on the human body are unknown, Bi is a rare metal that has an impact on the environment, and is also contained in raw materials as an unavoidable impurity, Bi is included as an optional element and may not be included. Furthermore, in consideration of the effects on the human body and the environment, and on stress corrosion cracking, the total content of Pb and Bi (compositional relation f2 described below) is set to less than 0.20 mass%, preferably less than 0.10 mass%. In this embodiment, the amount of Pb, which is harmful to the human body, is limited to less than 0.20 mass%, including Bi in some cases, while aiming for excellent machinability.
[0050] (Sn) Sn dissolves in the β1 phase, further improving the dezincification corrosion resistance of the β1 phase and improving the dezincification corrosion resistance of the alloy. When Sn is contained, to obtain this effect, the Sn content must be more than 0.05 mass%, preferably 0.10 mass% or more. Incidentally, Sn is originally distributed more in the β phase and β1 phase than in the α phase, and a small amount of Sn improves dezincification corrosion resistance, but as the Sn concentration increases, the γ phase is more likely to form and the ductility decreases. The formation of the γ phase not only reduces the ductility of the alloy, but also reduces machinability and degrades dezincification corrosion resistance. In relation to the amount of Si, the Sn content must be kept below 0.90 mass%, preferably below 0.70 mass%, and more preferably below 0.50 mass%.
[0051] As mentioned above, Sn is distributed in large amounts in the β phase and β1 phase, and it has been found that a high Sn content can cause problems in modifying the β phase containing Si and P. Specifically, it has been found that if the amount of Sn is greater than the amount of Si, the modification of the β phase becomes insufficient, and the effect of Sn content in improving dezincification corrosion resistance is canceled out. As will be described later, the amount of Si must exceed the amount of Sn.
[0052] (Inevitable Impurities, Particularly Fe, Mn, Co, and Cr / Al) Examples of unavoidable impurities in this embodiment include Mn, Fe, Al, Ni, Mg, Se, Te, Sn, Bi, Co, Ca, Zr, Cr, Ti, In, W, Mo, B, Ag, and rare earth elements. Conventionally, free-cutting copper alloys, particularly free-cutting brass containing approximately 30 mass% or more of Zn, are primarily made from recycled copper alloys rather than high-quality raw materials such as electrolytic copper and electrolytic zinc. In downstream processes (downstream processing, machining processes) in this field, most components and parts are cut, resulting in a large amount of discarded copper alloy, at a ratio of 40 to 80 parts by mass per 100 parts by mass of raw material. Examples of such discarded copper alloys include chips, scraps, burrs, runners, and products with manufacturing defects. These discarded copper alloys are the primary raw material. Inadequate separation of cutting swarf and scraps can result in the contamination of raw materials such as Pb, Fe, Mn, Si, Se, Te, Sn, P, Sb, As, Bi, Ca, Al, Zr, Ni, and rare earth elements from Pb-added free-cutting brass, Pb-free free-cutting copper alloys containing Bi, special brass alloys containing Si, Mn, Fe, and Al, and other copper alloys. Cutting swarf also contains Fe, W, Co, Mo, and other elements from tools. Recycled waste products, including plated products, can contain Ni, Cr, and Sn. Furthermore, pure copper scrap used in place of electrolytic copper can contain Mg, Sn, Fe, Cr, Ti, Co, In, Ni, Se, and Te. Brass-based scrap used in place of electrolytic copper or electrolytic zinc is often plated with Sn, resulting in Sn contamination.
[0053] From the viewpoint of resource reuse and cost considerations, scrap containing these elements is used as a raw material, at least to the extent that it does not adversely affect the properties. In the JIS standard (JIS H 3250), Pb-added free-cutting brass bar C3604 contains the essential element Pb in an amount of approximately 3 mass%, and furthermore, as impurities, Fe is allowed to be 0.5 mass% or less, and Fe + Sn (the total amount of Fe and Sn) is allowed to be up to 1.0 mass%. In fact, high concentrations of Fe and Sn are sometimes contained in free-cutting brass bars.
[0054] Fe, Mn, Co, and Cr dissolve in the α and β phases of Cu-Zn alloys to a certain concentration. However, if Si or P is present, they tend to combine with the Si and P, potentially consuming the Si and P necessary for modifying the β phase. The Fe, Mn, Co, and Cr that combine with Si form Fe-Si compounds, Mn-Si compounds, Co-Si compounds, Cr-Si compounds, and other compounds in the metal structure. Similarly, the Fe, Mn, Co, and Cr that combine with P form Fe-P compounds, Mn-P compounds, Co-P compounds, Cr-P compounds, and other compounds in the metal structure. These intermetallic compounds are very hard, so they not only increase cutting resistance but also shorten tool life. Therefore, the amounts of Fe, Mn, Co, and Cr must be limited, and each content is preferably less than 0.30 mass%, more preferably less than 0.20 mass%, and even more preferably 0.15 mass% or less. In particular, the total content of Fe, Mn, Co, and Cr must be less than 0.40 mass%, preferably less than 0.30 mass%, more preferably less than 0.25 mass%, and even more preferably 0.20 mass% or less.
[0055] On the other hand, Al, which is mixed in from special brass rods, brass castings, etc., must be limited because a high content affects the modification of the β phase and Al forms compounds with P or Si. In the alloy of this embodiment, the Al content must be less than 0.30 mass%, preferably less than 0.15 mass%, and more preferably 0.10 mass% or less.
[0056] As for other major unavoidable impurity elements, experience has shown that Ni is often mixed in from scrap, etc. Although Ni has a relatively small effect on mechanical properties such as machinability, it is necessary to limit its content in consideration of its effects on the human body. The Ni content is preferably less than 0.20 mass%, more preferably less than 0.10 mass%. As for Ag, Ag is generally considered to be Cu and has almost no effect on various properties, so there is no need to particularly limit its content, but the Ag content is preferably less than 0.05 mass%. Te and Se themselves have free machinability, and although rare, there is a risk of their being mixed in large amounts. In consideration of their effects on ductility and impact properties, the respective contents of Te and Se are preferably less than 0.10 mass%, more preferably less than 0.05 mass%, and even more preferably 0.02 mass% or less. In addition, corrosion-resistant brass contains As and Sb to improve the corrosion resistance of brass, but in consideration of ductility and effects on the human body, the content of each of As and Sb is preferably less than 0.05 mass%, more preferably 0.02 mass% or less. The content of other elements such as Mg, Ca, Zr, Ti, In, W, Mo, B, and rare earth elements is preferably less than 0.05 mass%, more preferably less than 0.03 mass%, and even more preferably 0.02 mass% or less. The content of rare earth elements is the total amount of one or more of Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Tb, and Lu. As described above, the total amount of inevitable impurities other than Fe, Mn, Co, Cr, and Al is also preferably less than 0.70 mass%, more preferably less than 0.50 mass%.
[0057] (Compositional formula f1) Compositional formula f1 = [Cu] - 4.6 x [Si] + 0.5 x ([Pb] + [Bi]) - [P] - [Sn]. When the Sn content is 0.05 mass% or less, [Sn] in f1 is 0. When Bi is not contained, [Bi] in f1 is 0. When Sn is 0.05 mass% or less, the effect on compositional formula f1 is small, so it is not specified in compositional formula f1. f1 is a formula that represents the relationship between composition and metal structure. Even if the amount of each element is within the range specified above, the various properties targeted by this embodiment cannot be achieved unless this compositional formula f1 is satisfied. When compositional formula f1 is less than 57.5, the proportions of the β phase and β1 phase increase, the modification of the β phase becomes insufficient, and the ductility, dezincification corrosion resistance, and stress corrosion cracking resistance deteriorate. Therefore, the lower limit of the compositional relational formula f1 is 57.5 or more, preferably 58.0 or more, and more preferably 58.2 or more. As the compositional relational formula f1 falls within a more preferable range, the proportion of the α phase increases, the β phase is sufficiently modified, and excellent machinability is maintained, while good dezincification corrosion resistance and stress corrosion cracking resistance can be provided, and good ductility and cold workability can be obtained. On the other hand, the upper limit of the compositional relational formula f1 affects the proportions of the β phase and β1 phase. If the compositional relational formula f1 is greater than 60.5, the proportion of the β1 phase decreases, resulting in poor machinability and low strength. Therefore, f1 is 60.5 or less, preferably 60.2 or less, and more preferably 60.0 or less.
[0058] (Compositional Relational Formula f2) Bi is an optional element that substitutes for the function of Pb. However, when Bi is included, the following relational formula must be satisfied: 0.003≦f2=[Pb]+[Bi]<0.20. That is, considering that the effects of Bi on the human body are currently unknown and that Bi is a rare metal and has an environmental impact, it is necessary to limit the total amount of Pb and Bi. When Bi is included, the total amount of Pb and Bi must be less than 0.20 mass%, which is the upper limit for the amount of Pb, and preferably less than 0.10 mass%. On the other hand, in order to obtain good machinability, when Bi is included, the total amount of Pb and Bi must be 0.003 mass% or more, preferably 0.004 mass% or more, and more preferably 0.005 mass% or more.
[0059] (Compositional formula f0) Sn is contained to further improve dezincification corrosion resistance. Sn is contained in large amounts in the β phase, and the greater the amount of Sn, the more the dezincification corrosion of the β1 phase is delayed. On the other hand, if the amount of Sn is too large compared to the amount of Si, it may hinder the modification of the β phase and impair the dezincification corrosion resistance of the β1 phase. In other words, when f0 = [Sn] / [Si], in order to exert an effect commensurate with the inclusion of Sn taking other properties into consideration, f0 must be less than 1. f0 is preferably less than 0.8, more preferably less than 0.6, and even more preferably less than 0.5.
[0060] The free-cutting copper alloy of this embodiment contains a large amount of conventional β phase (or β1 phase in this application), yet has good dezincification corrosion resistance, stress corrosion cracking resistance, and mechanical properties. It also possesses the completely contradictory properties of machinability, which requires a type of brittleness that reduces cutting resistance and breaks chips into small pieces, and ductility. To achieve these excellent corrosion resistance, machinability, and mechanical properties, detailed consideration of not only the composition of each component but also the compositional relations f0, f1, and f2, as well as the structural relations f3 to f5 and the structural-compositional relation f6 described below, can provide an alloy that is more suited to the intended purpose and application. Note that Fe, Mn, Co, Cr, Al, and other unavoidable impurities, as well as those separately defined as unavoidable impurities, have little effect on the structural relation f1, so are not specified in the structural relation f1.
[0061] (Comparison with Patent Documents) Tables 1 to 4 show the results of comparing the compositions of the Cu—Zn—Si alloys described in the above-mentioned Patent Documents 1 to 15 with the alloy of this embodiment.
[0062]
[0063]
[0064]
[0065]
[0066] The present embodiment and Patent Document 8 differ in the contents of the major elements Si and Cu, the present embodiment and Patent Document 9 differ in the content of the major element Si, and the present embodiment and Patent Document 15 differ in the content of the major element Cu. Patent Documents 1, 13, and 15 state that Pb is not contained, and the Pb content differs. Patent Documents 8, 10, 11, and 12 significantly limit the β phase in the metal structure from the viewpoints of machinability, dezincification corrosion resistance, corrosion resistance, and the like. Although the β1 phase of the present application differs from the β phase in Patent Documents 8, 10, 11, and 12, the β phase is limited to 5% or less, 25% or less, 15% or less, and 0.9% or less, respectively.
[0067] Patent Document 10 relates to a near-net-shape tubular hot-forged product, and uses a tubular material. Patent Documents 1 and 9 state that heat treatment is performed at a temperature of 350 to 550°C or 400 to 600°C to reduce the β phase and to break up the β phase. Patent Document 9 states that the steel contains 0.2 mass% or more of Sn, and contains Sn and Si to improve the dezincification corrosion resistance of the β phase. It is hot extruded at a temperature of 700°C or higher to improve machinability, and heat treated at 400 to 600°C to improve corrosion resistance. The proportion of the β phase is approximately 5 to 20%, and the Si content is 0.01 to 0.50 mass%, and may be controlled to 0.2 mass% or less.
[0068] In Patent Documents 12, 13, and 14, Al is essential for improving discoloration resistance, castability, and dezincification corrosion resistance. Patent Document 14 requires the inclusion of at least 0.1 mass% or more of Sn and Al to improve dezincification corrosion resistance, and large amounts of Pb and Bi to obtain excellent machinability. Patent Document 15 requires the inclusion of a γ phase without Pb, and includes 65 mass% or more of Cu and Si, as well as trace amounts of Al, Sb, Sn, Mn, Ni, B, etc., to provide a corrosion-resistant copper alloy casting with good mechanical properties and castability.
[0069] All of Patent Documents 2 to 7 require that the cooling process after hot working be performed at an average cooling rate of about 0.1°C / min to about 70°C / min in the temperature range from about 530°C to about 450°C, resulting in the formation of P compounds present in the metal structure. Furthermore, they state that the γ phase is effective for machinability, and make no mention of modifying the β phase. They are silent on dezincification corrosion resistance and stress corrosion cracking resistance, and no data is disclosed. Furthermore, with the exception of Patent Document 7, no data is disclosed regarding cutting resistance under high-speed cutting conditions. In this application, the cooling process after hot working is initiated at temperatures below 670°C and above 500°C, and the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C and the average cooling rate in the temperature range from 500°C to 300°C exceed 300°C / min, which is fundamentally contrary to Patent Documents 2 to 7.
[0070] The most significant and clear difference between the present application and Patent Documents 2 to 7 is that none of Patent Documents 2 to 7 mentions the modification of the β phase or the modified β phase, i.e., the β1 phase. The β1 phase is formed under the following conditions: During hot working, a β phase containing a certain amount of Si and P is formed as a solid solution. Then, cooling treatment is initiated at a temperature higher than 500°C, and the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C exceeds 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C exceeds 300°C / min. The β1 phase is formed as described above. When etched with a mixture of hydrogen peroxide and aqueous ammonia, grain boundaries can be observed in the β1 phase if the β1 phase contains a certain amount of Si and P, but if the β phase remains unmodified, no grain boundaries can be observed in the β phase. Patent Documents 2 to 7 disclose metal structures etched with a mixture of hydrogen peroxide and aqueous ammonia, but in none of them are grain boundaries observed within the β phase. Patent Documents 2 to 7 do not define the cooling treatment start temperature after hot working, but even if the cooling treatment start temperature is below 530°C, the average cooling rate from the cooling treatment start temperature to 500°C is about 0.1°C / min or more and about 70°C / min or less, so the β1 phase (modified β phase) is not observed.
[0071] The β1 phase differs from conventional β phases in that it significantly improves dezincification corrosion resistance and stress corrosion cracking resistance, and further improves machinability, surpassing that achieved when P compounds are present. However, to achieve this, the β1 phase must be present in an area ratio of more than 25% in the metal structure. While this application states that the presence of the γ phase impairs machinability, Patent Documents 2 to 7 state that the γ phase is effective in improving machinability.
[0072] <Metal structure> Cu-Zn-Si alloys contain more than 10 types of phases, and complex phase changes occur, so the desired properties cannot necessarily be obtained by simply determining the composition range and elemental relationships. Ultimately, the desired properties can be obtained by identifying and determining the types of phases present in the metal structure and the range of their area ratios. Therefore, the structure relationships are specified as follows: 20≦f3=(α)<75, 25<f4=(β1)≦80, where β1 phase is a modified β phase. 0≦f5=(γ)<4
[0073] (β1 Phase) The metal structure of the present application, excluding nonmetallic inclusions, is composed of an α phase, a β1 phase, and in some cases, a small amount or no γ phase. The difference between the β phase and the β1 phase is that when the β1 phase is etched with a mixture of hydrogen peroxide and aqueous ammonia, a grain boundary pattern, i.e., a crystal grain boundary, is observed within the β phase, whereas no crystal grain boundary is observed within the β phase. The β1 phase in this embodiment is obtained by dissolving a certain amount of Si and P in the β phase at a high temperature during hot working, maintaining the temperature at 500 to 670°C, and then cooling from that temperature range (cooling at an average cooling rate of more than 300°C / min from the cooling treatment start temperature to 500°C and from 500°C to 300°C, and then continuing to cool to near room temperature) to maintain the metal structure state at 500 to 670°C. Specifically, the cooling rate is increased in the temperature range from the high-temperature cooling start temperature to 300°C, followed by rapid cooling to room temperature below 100°C. This allows the metal structure state at high temperatures to be maintained at room temperature. As a result, the β1 phase is obtained. The β1 phase cannot be obtained by performing the above-mentioned cooling treatment on the β phase of a Cu-Zn alloy that does not contain a predetermined amount of both Si and P. Similarly, the β1 phase cannot be obtained by performing a cooling treatment on an alloy containing Si and P at a temperature below 500°C, for example, from 450°C at a cooling rate exceeding 300°C / min. Note that a predetermined amount or more of the α phase is required to modify the β phase; if the α phase is absent or is small, the β1 phase cannot be obtained. Furthermore, the degree of modification of the β phase is also affected by the amounts of Si and P, the amount of unavoidable impurities, the cooling treatment start temperature, the average cooling rate in the temperature range from the start of the cooling treatment to 500°C, and the average cooling rate in the temperature range from 500°C to 300°C. When the degree of modification of the β phase is improved, i.e., when the β1 phase is further modified, a material with better machinability and excellent dezincification corrosion resistance and stress corrosion cracking resistance can be obtained. Although it depends on the amount of inevitable impurities such as Fe, the degree of modification of the β phase roughly begins to saturate at about 1 mass% Si and about 0.1 mass% P, and if these amounts are too high, there is a risk of causing adverse effects such as a decrease in conductivity and ductility and the appearance of a γ phase.The β1 phase (modified β phase) overcomes the drawbacks of the β phase in Cu—Zn-based alloys, namely, the alloy's dezincification corrosion resistance and stress corrosion cracking resistance, which have been major issues. Specifically, as an example, the corrosion progression of dezincification corrosion can be reduced by approximately 60% or more, and similarly, the progression of stress corrosion cracking can be delayed by approximately 50% or more. As described in patent documents, dezincification corrosion of Cu—Zn-based alloys containing a β phase is a major problem. Since dezincification corrosion occurs along the β phase, the amount of β phase is limited to 25% or less or 20% or less. Furthermore, to reduce the amount of β phase and disrupt the β phase, heat treatment at 350 to 550°C is performed. While strength largely depends on the area ratio of the constituent phases, the modified β phase, i.e., the β1 phase, has higher strength and better ductility than the β phase, resulting in an alloy with a good strength-ductility balance.
[0074] (β1 phase, structural formula f4) In the Cu—Zn—Si—P—Pb alloy, which is the free-cutting copper alloy of this embodiment, in order to achieve good machinability while minimizing the Pb content, the area fraction of the β1 phase must be at least 25%. Furthermore, in order to improve machinability and strength, the area fraction of the β1 phase is preferably 30% or more, more preferably 33% or more. On the other hand, if the β1 phase is too high, for example, 95%, the β phase is not modified. Because the β phase is modified in the presence of the α phase, a certain amount of the α phase is necessary. Furthermore, with regard to dezincification corrosion and stress corrosion cracking, although the β1 phase significantly slows the progression of dezincification corrosion and stress corrosion cracking compared to the β phase, it is still inferior to the α phase in dezincification corrosion resistance and stress corrosion cracking resistance. Specifically, with regard to dezincification corrosion, when a metal structure is composed of an α phase and a β phase (an unmodified β phase), the β phase is selectively dezincified and the dezincification corrosion depth reaches about 500 μm. When a metal structure is composed of an α phase and a β1 phase (a modified β phase), the β1 phase is selectively dezincified, but the dezincification corrosion depth is about 20 to about 200 μm, depending on the degree of modification to the β1 phase and the area ratio of the β1 phase, and the progress of dezincification corrosion is significantly suppressed. In this way, by modifying the β phase to the β1 phase, dezincification corrosion resistance is significantly improved, but even if improved, the dezincification corrosion resistance and ductility are inferior to those of the α phase, so if the area ratio of the β1 phase is high, the dezincification corrosion resistance and ductility of the alloy are reduced. Based on the above, and as a result of extensive research, it has been found that the area ratio of the β1 phase needs to be set to 80% or less, preferably 70% or less, and more preferably 65% or less.
[0075] (α phase, structural formula f3) The present invention is basically composed of α phase and β1 phase. Treatment is performed to transform the β phase into β1 phase, but the α phase is hardly affected by this treatment. Furthermore, a certain amount of α phase is required to transform the β phase. Too much β1 phase can cause problems with the alloy's ductility, so an appropriate amount of ductile α phase is necessary. Conversely, too much α phase reduces strength. Furthermore, α phases containing Si only slightly improve machinability compared to α phases without Si, and the amount of α phase is limited from the perspective of machinability. However, even if an alloy is composed of a β1 phase with excellent machinability and an α phase with slightly poor machinability, the α phase acts as a cushioning material during cutting, or acts as a stress concentration source at the boundary with the hard β1 phase during cutting. Therefore, even if the alloy contains up to approximately 75% α phase, the cutting resistance of the alloy remains low and chips are easily broken. Since the α phase acts as a cushioning material during cutting and as a stress concentration source at the boundary with the hard β1 phase, it is preferable that the α phase have a fine granular shape. As a result of extensive research into the modification of the β phase and the dezincification corrosion resistance, stress corrosion cracking resistance, machinability, and mechanical properties of the alloy, the amount of α phase must be 20% or more, preferably 30% or more, and more preferably 35% or more. On the other hand, the upper limit of the α phase is less than 75%, preferably 70% or less, and more preferably 67% or less.
[0076] (γ Phase, Structure Relationship Formula f5) As described in Patent Documents 8 and 10, the γ phase contributes to machinability in Cu—Zn—Si alloys having a Cu concentration of about 69 to about 80 mass% and a Si concentration of about 2 to about 4 mass%. Patent Document 15 states that the γ phase is essential in Pb-free Cu—Zn—Si alloys. Furthermore, Patent Documents 2 to 6 also state that the β phase containing Si has good machinability, while the γ phase containing Si also has good machinability. In this embodiment, the γ phase is considered to hinder the machinability of the alloy, and is assigned a negative coefficient greater than the coefficient for the amount of β1 phase in the structure-composition relationship formula f6 described below. Furthermore, the γ phase impairs ductility and deteriorates dezincification corrosion resistance. This is because the γ phase is not modified in this embodiment. In Cu—Zn—Si alloys, the appearance of the γ phase may be unavoidable, but must at least be limited. That is, the proportion (area ratio) of the γ phase is less than 4%, preferably less than 2%, more preferably less than 1%, and optimally, no γ phase is present, i.e., f5=0.
[0077] (Structure-composition relationship formula f6) f6 = (β1) × ([Si]) 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 × 20 + ([P]) 1/2×15 The structure-composition relationship f6 is a simple conditional expression for obtaining good machinability in an alloy. f6 expresses the amount of β1 phase, the amount of Si, the amount of Pb, the amount of Bi, and the amount of P contained in the alloy within the composition range of the present application as positive effects, and the amount of γ phase as negative effects. That is, for a β1 phase containing Si and P, it is calculated by multiplying the amount of β1 phase by the ½ power of the amount of Si, multiplying the sum of the amounts of Pb and Bi by a coefficient of 20, multiplying the amount of P by the ½ power of the amount of P by a coefficient of 15, and then subtracting the sum of these by multiplying the amount of γ phase by a coefficient of 2. The performance of the β1 phase (modified β phase) is directly affected by the Si concentration and also by the P concentration. The inclusion of even small amounts of Pb or Bi improves machinability. On the other hand, in the present application, the γ phase inhibits machinability. It has been discovered that the degree of improvement in machinability due to Pb or Bi is closely related to the 1 / 2 power of the amount of Pb and Bi. A very small amount of both Pb and Bi exerts a significant effect, and as the content increases, the effect of improving machinability increases, but the effect gradually becomes more gradual. With alloys composed of the β1 phase (modified β phase), trace amounts of Pb or Bi exert a significant effect on machinability, an effect that cannot be achieved by the relationship between the Pb content and machinability of conventional Cu-Zn-Pb alloys. As a result of extensive research, in order to obtain good machinability, f6 should be greater than 27, preferably 33 or greater, more preferably greater than 35, and even more preferably 38 or greater, approaching the machinability of free-cutting brass rods containing 3 mass% Pb.
[0078] 1A to 6B show metallographic photographs of various alloys and photographs of the results of ISO 6509 dezincification corrosion tests. FIG. 1A is a microstructure observation photograph of a copper alloy according to an embodiment. The copper alloy was obtained by subjecting Alloy No. S01 to Process No. A2. Specifically, Alloy No. S01 had a composition of Zn-63.3 mass% Cu-0.95 mass% Si-0.069 mass% P-0.063 mass% Pb-0.017 mass% Bi. In Process No. A2, hot extrusion was performed at 630°C, and cooling treatment was initiated at 580°C. The average cooling rates in the temperature range from 580°C to 300°C and in the temperature range from 500°C to 300°C were both 1020°C / min. The average cooling rate in the temperature range from 580°C (the cooling treatment start temperature) to 500°C can be easily calculated from the average cooling rate in the temperature range from 580°C to 300°C and the average cooling rate in the temperature range from 500°C to 300°C. Figure 1B shows the results of a dezincification corrosion test performed on the alloy of Figure 1A in accordance with the ISO 6509 test method, and is a cross-sectional metallographic photograph including the portion exhibiting the maximum corrosion depth. Figure 2A shows a microstructure observation photograph of a copper alloy according to an embodiment, obtained by performing Process No. E2 on Alloy No. S11. Specifically, Alloy No. S11 has a composition of Zn-62.5 mass% Cu-0.96 mass% Si-0.064 mass% P-0.072 mass% Pb. Process No. For E2, a rod having a diameter of 50 mm and a length of 200 mm was obtained by hot extrusion at 550°C, and an average cooling rate of 20°C / min was used in the temperature range from 500°C to 300°C. The rod was heated, placed horizontally, and hot forged at 680°C to a thickness of 20 mm. Cooling treatment was initiated at 565°C, and the average cooling rates in the temperature range from 565°C to 300°C and in the temperature range from 500°C to 300°C were both 900°C / min. Figure 2B shows the results of a dezincification corrosion test performed on the alloy of Figure 2A according to the ISO 6509 test method, and is a cross-sectional metallographic photograph including the portion exhibiting the maximum corrosion depth. Figure 3A shows a microstructure observation photograph of a copper alloy according to an embodiment, obtained by subjecting Alloy No. S11 to Process No. E13H.Specifically, Alloy No. S11 has a composition of Zn-62.5 mass% Cu-0.96 mass% Si-0.064 mass% P-0.072 mass% Pb. In Process No. E13H, a rod having a diameter of 50 mm and a length of 200 mm was obtained by hot extrusion at 550°C and an average cooling rate of 20°C / min in the temperature range from 500°C to 300°C. The rod was heated, hot forged at 630°C in a horizontal position to a thickness of 20 mm, and cooled at an average cooling rate of 35°C / min. The cooling treatment was then initiated at 455°C, and the average cooling rate in the temperature range from 455°C to 300°C was 800°C / min. The alloy of FIG. 3A and the alloy of FIG. 2A differ in the cooling treatment start temperature. Figure 3B shows the results of a dezincification corrosion test performed on the alloy shown in Figure 3A according to the ISO 6509 test method, and is a cross-sectional metallographic photograph including the area exhibiting the maximum corrosion depth. Figure 4A shows a microstructure observation photograph of a copper alloy according to an embodiment, obtained by performing Step No. E6 on Alloy No. S43. Specifically, Alloy No. S43 has a composition of Zn-63.3 mass% Cu-0.98 mass% Si-0.084 mass% P-0.060 mass% Pb-0.28 mass% Sn. In Step No. E6, the casting cast into a 55 mm diameter mold was cut to a diameter of 50 mm and a length of 200 mm. The casting was heated, placed horizontally, and hot forged at 630°C to a thickness of 20 mm. Cooling treatment was initiated at 565°C, with the average cooling rates in the temperature range from 565°C to 300°C and in the temperature range from 500°C to 300°C being both 900°C / min. Figure 4B shows the results of a dezincification corrosion test performed on the alloy of Figure 4A in accordance with the ISO 6509 test method, and is a cross-sectional metallographic photograph including the portion exhibiting the maximum corrosion depth. Figure 5A is a photograph of the microstructure of a copper alloy according to an embodiment, obtained by subjecting Alloy No. S02 to Process No. A34H and Process No. G1. Specifically, Alloy No. S02 has a composition of Zn-62.9 mass% Cu-0.98 mass% Si-0.071 mass% P-0.071 mass% Pb. In Process No. A34H, the alloy was obtained by hot extrusion at 615°C and cooling from 500°C to 300°C at an average rate of 18°C / min.In Process No. G1, this alloy was further heated at 580°C for 30 minutes, and cooling treatment was initiated at 560°C. The average cooling rates in the temperature range from 560°C to 300°C and in the temperature range from 500°C to 300°C were both 1800°C / min. Figure 5B shows the results of a dezincification corrosion test performed on the alloy of Figure 5A in accordance with the ISO 6509 test method, and is a cross-sectional metallographic photograph including the area exhibiting the maximum corrosion depth. Figure 6A is a photograph of the microstructure of a copper alloy according to an embodiment, obtained by performing Process No. E14H on Alloy No. S02. Specifically, Alloy No. S02 has a composition of Zn-62.9 mass% Cu-0.98 mass% Si-0.071 mass% P-0.071 mass% Pb. Process No. For E14H, a 50 mm diameter, 200 mm long bar was obtained by hot extrusion at 550°C and cooling from 500°C to 300°C at an average cooling rate of 20°C / min. The bar was heated, hot forged at 630°C horizontally to a thickness of 20 mm, and then naturally cooled. The average cooling rate in the temperature range from 500°C to 300°C was 25°C / min. Figure 6B shows the results of a dezincification corrosion test performed on the alloy of Figure 6A according to the ISO 6509 test method, and is a cross-sectional metallographic photograph including the area exhibiting the maximum corrosion depth.
[0079] As shown in Figures 1A, 2A, 4A, and 5A, in hot extruded materials, hot forged materials, hot forged materials made from cast materials, and extruded materials that have undergone additional heat treatment after hot extrusion, grain boundary patterns, i.e., grain boundaries, are observed in metallurgical microscope photographs in addition to α-phase grain boundaries within the β1 phase. Here, grain boundaries refer to the linear patterns that penetrate the β1-phase grains observed within the β1 phase, as shown in Figure 1A. As shown here, grain boundaries are recognized within the modified β phase, i.e., the β1 phase. On the other hand, in Figure 3A, slight black streaks are observed within the β phase, but no grain boundaries penetrating the β-phase grains are observed. In Figure 6A, even a trace of grain boundaries is not observed within the β phase. Instead, in Figures 3A and 6A, black granular precipitates of approximately 0.5 to 3 μm in size are present primarily within the β phase and at the phase boundary between the β and α phases. The granular precipitates are primarily P compounds, but also include Pb particles, mixed particles of Pb and Bi, compounds of Fe, oxides, and sulfides. While distinguishable by microscopic observation, they are somewhat difficult to distinguish from printed photographs. Precipitates outside the above-mentioned size range and present within the α phase are not P compounds. In Figures 3A and 6A, approximately 1,000 P compounds are present within the field of view of the printed photographs. In Figures 1A, 2A, 4A, and 5A, fine granular P compounds are absent or present only in small amounts, at least 1 / 10 or 1 / 50 of the number of precipitates in Figures 3A and 6A. From these results, the presence of grain boundaries in the β1 phase or β phase depends on whether the cooling treatment start temperature is higher or lower than approximately 500°C, and the presence of large amounts of P compounds depends on whether the cooling treatment start temperature is higher or lower than approximately 500°C. The results of the ISO 6509 dezincification corrosion tests of these alloys are shown in Figures 1B, 2B, 3B, 4B, 5B, and 6B. The maximum corrosion depths of the samples in which grain boundaries were observed within the β1 phase (Figures 1A, 2A, 4A, and 5A) were 120 μm or less, whereas the maximum corrosion depths of the samples in which grain boundaries were not observed within the β phase were 350 μm (Figure 3A) and 460 μm (Figure 6A), a difference of 3 to 5 times. The corrosion depth of the sample containing 0.28 mass% Sn was particularly favorable at 40 μm (Figure 4A).The dezincification corrosion occurs in both cases as a selective corrosion of the β1 and β phases. Although the β1 and β phases are preferentially dezincified, the β1 phase can slow the progress of dezincification corrosion to about one-third or less of that of the β phase.
[0080] <Characteristics> (Room temperature strength and high temperature properties) There is a strong demand for thinner and lighter materials and parts for which the present embodiment is used, such as plumbing equipment, piping parts, automobiles, and electrical parts. As for the necessary strength, tensile strength is considered important, and the balance between strength and ductility is also considered important. To this end, the hot extruded material, hot rolled material, and hot forged material must have a tensile strength of 460 N / mm in the hot-worked state without cold working. 2 The tensile strength is preferably 490 N / mm or more. 2 More preferably, 520 N / mm 2 Many parts used in valves, fittings, pressure vessels, air conditioners and refrigerators are made by hot extrusion and hot forging, and the tensile strength of the currently used Pb-added copper alloy, C3604, is about 390 to 420 N / mm 2 , and elongation is about 30-35%, so weight reduction can be achieved through high strength. On the other hand, cold working such as light crimping or bending may be performed on cutting materials, so it is necessary for them not to crack. Machinability requires a certain brittleness in the material so that chips can be broken, but this is an opposing property to cold workability. Similarly, tensile strength and ductility are opposing properties, but it is desirable to achieve a high level of balance between tensile strength and ductility (elongation). In other words, a tensile strength of at least 450 N / mm 2 The elongation is 10% or more, and the product of the tensile strength (S) and the 1 / 2 power of {(elongation (E%) + 100) / 100}, f7=S×{(E+100) / 100} 1/2 A value of 540 or more is one measure of a high strength, high ductility material. f7 is more preferably 570 or more, and even more preferably 600 or more. When cold working with a cold working rate of 3 to 15% is included, an elongation of 10% or more and a tensile strength of 520 N / mm 2In the case of the Pb-added copper alloy, f7 is about 470.
[0081] (Conductivity) Applications of this embodiment include electrical and electronic equipment components, automotive components for which the shift to electric vehicles is progressing, and other highly conductive members and components. Currently, phosphor bronze (JIS standard, C5191, C5210) containing 6 mass% or 8 mass% Sn is widely used for these applications, and their electrical conductivities are approximately 14% IACS and 12% IACS, respectively. Therefore, as long as the conductivity of the copper alloy of this embodiment is 15% IACS or higher, no problems arise with electrical conductivity. Note that the upper limit of the electrical conductivity is not particularly specified, since improved conductivity poses almost no practical problems.
[0082] (Hot workability) The free-cutting copper alloy of this embodiment is characterized by excellent deformability at 540 to 750°C, and can be hot extruded into a bar with a small cross-sectional area and hot forged into a complex shape. Due to energy considerations and the fact that the α phase has a good granular shape, the hot working temperature is preferably less than 750°C, more preferably less than 720°C, and from the viewpoint of hot deformation resistance, it is preferably greater than 540°C, more preferably greater than 560°C.
[0083] <Manufacturing Process> Next, a method for manufacturing a free-cutting copper alloy according to an embodiment of the present invention will be described. The metal structure of the alloy of this embodiment varies not only with the composition but also with the manufacturing process. It is affected not only by the hot working temperature and heat treatment conditions of hot extrusion and hot forging, but also by the average cooling rate during the cooling process in hot working and heat treatment. As a result of extensive research, it has been found that the metal structure is significantly affected by the cooling treatment start temperature, the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C, and the average cooling rate in the temperature range from 500°C to 300°C during the cooling process in hot working and heat treatment.
[0084] (Melting and Casting) Melting is performed at a temperature of about 950 to about 1200°C, which is about 100 to about 300°C higher than the melting point (liquidus temperature) of the alloy of this embodiment. Molten metal at a temperature of about 900 to about 1100°C, which is about 50 to about 200°C higher than the melting point, is cast into a predetermined mold and cooled by several cooling methods such as air cooling, slow cooling, and water cooling. After solidification, the constituent phases change in various ways.
[0085] (Hot Working) Examples of hot working include hot extrusion, hot forging, and hot rolling. When two or more hot working steps are performed, the final hot working step is performed under the following conditions. First, regarding hot extrusion, in a preferred embodiment, the material temperature (extrusion temperature) immediately after hot working is higher than 540°C and lower than 750°C, depending on the extrusion ratio (hot working rate) and equipment capacity. The extruded rod is wound into a coil, or if the cross-sectional area of the extruded rod is large, it is extruded as a straight rod onto a table. The lower limit of the hot extrusion temperature is related to hot deformation resistance. A lower extrusion temperature results in finer, more granular α-phase crystal grains, improving dezincification corrosion resistance, stress corrosion cracking resistance, and machinability. However, when the extrusion ratio is large, the extrusion temperature is preferably 560°C or higher due to the relationship between equipment capacity and the cooling treatment start temperature described below. The upper limit is related to the shape of the α-phase, and a stable metal structure can be obtained by controlling the temperature within a narrower range. When hot extrusion is performed at a temperature of 750°C or higher, the metal structure becomes a single β phase, or the proportion of β phase becomes 90% or more, and the shape of the α phase crystal grains tends to become acicular, or coarse α phase crystal grains tend to appear. When acicular and coarse α phase crystal grains appear, the strength is slightly reduced, the balance between strength and ductility is slightly impaired, and the coarse α phase crystal grains with large long sides hinder cutting, resulting in poor machinability. Furthermore, dezincification corrosion resistance and stress corrosion cracking resistance also deteriorate. The extrusion temperature is preferably 720°C or lower. The shape of the α phase crystal grains is related to the compositional relationship f1. When the compositional relationship f1 is 59.0 or less, the extrusion temperature is preferably lower than 720°C. By extruding at a lower temperature than copper alloys containing Pb, good machinability and strength can be achieved.
[0086] By adjusting the cooling conditions after hot extrusion, the β phase can be modified, resulting in a material with better machinability and excellent dezincification corrosion resistance and stress corrosion cracking resistance. Specifically, during the cooling process after hot extrusion, the cooling treatment is first initiated at a temperature lower than 670°C and higher than 500°C. The average cooling rates in the temperature range from the cooling treatment start temperature to 500°C and in the temperature range from 500°C to 300°C are set to at least 300°C / min, preferably higher than 600°C / min, and more preferably 900°C / min or higher. Here, in a typical embodiment, when a typical cooling method is used, the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C and the average cooling rate in the temperature range from 500°C to 300°C are roughly the same, or in some cases, the former is slightly faster. Furthermore, cooling at a more preferable cooling rate further modifies the β1 phase. Further modification of the β1 phase results in a material with better machinability and excellent dezincification corrosion resistance and stress corrosion cracking resistance. The upper limit of the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C and in the temperature range from 500°C to 300°C is sufficient if it is possible to perform the cooling at a normal production facility, and although not specifically specified, a cooling rate of approximately 9000°C / min or less is preferred. By cooling at an average cooling rate exceeding 300°C / min, the β phase is modified, and when the metal structure is etched with a mixture of hydrogen peroxide and aqueous ammonia and observed under a metallurgical microscope at 500x magnification, grain boundaries can be observed within the modified β phase. Note that when the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C and in the temperature range from 500°C to 300°C is 300°C / min or less, grain boundaries cannot be observed within the β phase. The degree of reforming to the reformed β phase, i.e., the β1 phase, increases as the cooling rate increases. When cooling from a temperature below 300°C to room temperature, the cooling rate slows slightly as the temperature approaches room temperature, but it is desirable to continue cooling in the temperature range from 500°C to 300°C. On the other hand, the starting temperature of the cooling treatment also affects the reforming of the β phase. It is preferable to start the cooling treatment at a temperature higher than 530°C, and more preferably at a temperature higher than 550°C.When cooling is initiated at a temperature below 550°C, if the cooling rate from 550°C to the cooling treatment start temperature is slow, compounds of P and Zn, or P and Zn, Si, begin to form, and the formation of P compounds is further promoted at 530°C or below. At a cooling rate exceeding 300°C / min, P compounds are hardly formed, but if the cooling treatment start temperature is lower than 550°C, P compounds are observed in the metal structure. However, if the cooling treatment start temperature is 670°C or higher, the proportion of the β1 phase becomes too high, degrading the ductility, dezincification corrosion resistance, and stress corrosion cracking resistance of the alloy. Therefore, the cooling treatment start temperature must be lower than 670°C, and preferably lower than 650°C.
[0087] In consideration of the measurement position where actual measurement is possible, the hot working temperature is defined as the temperature of the hot-worked material that can be measured approximately 2 or 3 seconds after the end of hot extrusion, hot forging, or hot rolling. The metal structure is affected by the temperature immediately after processing, which has caused large plastic deformation.
[0088] Next, hot forging will be described. Hot forging primarily uses hot extruded material as the raw material, but continuous cast rods are also used. Since the forging material is not the final hot processing step, no cooling techniques are required. Compared to hot extrusion, hot forging allows for faster processing speeds, resulting in complex shapes, and in some cases, wall thicknesses as low as approximately 3 mm. Furthermore, each forged product weighs several tens of grams to several kilograms. Smaller products are rapidly cooled during forging, and the subsequent cooling rate is also fast. Therefore, the heating temperature of the material during forging is higher than the heating temperature of the ingot during hot extrusion. In a preferred embodiment, the temperature of the hot forged product, i.e., the material temperature approximately 2 or 3 seconds after forging, is preferably above 540°C and lower than 750°C. Hot forging is also related to the compositional relationship f1. When the compositional relationship f1 is 59.0 or less, the hot forging temperature is preferably lower than 720°C. Although it depends on the processing rate of hot forging, the lower the temperature, the smaller the crystal grain size of the α phase, the change in the shape of the α phase crystal grains from needle-like to granular, the higher the strength, the better the balance between strength and ductility, and the better the machinability, dezincification corrosion resistance, and stress corrosion cracking resistance.
[0089] As with hot extrusion, by adjusting the cooling rate after hot forging, a material with good dezincification corrosion resistance, stress corrosion cracking resistance, and machinability can be obtained. That is, in the cooling process after hot forging, cooling is first initiated at a temperature lower than 670°C and higher than 500°C, and the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C and the average cooling rate in the temperature range from 500°C to 300°C are set to at least 300°C / min, preferably higher than 600°C / min, and more preferably 900°C / min or higher. Here, in a typical embodiment, when a general cooling method is used, the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C and the average cooling rate in the temperature range from 500°C to 300°C are roughly the same, or the former is slightly faster. By increasing the average cooling rate to more than 300°C / min, the β phase is modified. When the metal structure is etched with a mixture of hydrogen peroxide and aqueous ammonia and observed under a metallurgical microscope at 500x magnification, grain boundaries can be observed within the modified β phase. Note that, if the average cooling rate in the temperature range from 500°C to 300°C is 300°C / min or less, grain boundaries cannot be observed within the β phase. The degree of modification to the modified β phase, i.e., the β1 phase, increases with the cooling rate. As with hot extrusion, the cooling rate from temperatures below 300°C to room temperature slows slightly as the temperature approaches room temperature, but it is desirable to continue cooling in the temperature range from 500°C to 300°C. There are no specific upper limits for the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C and in the temperature range from 500°C to 300°C. However, if mentioned, a cooling rate of approximately 9000°C / min or less is preferred. On the other hand, the starting temperature of the cooling treatment also affects the modification of the β phase. It is preferable to start the cooling treatment at a temperature higher than 530°C, and more preferably at a temperature higher than 550°C. When the cooling treatment is started at a temperature lower than 550°C, if the cooling rate from 550°C to the starting temperature of the cooling treatment is slow, compounds of P and Zn, or P and Zn and Si, begin to form, and the formation of P compounds is further promoted at 530°C or lower. At a cooling rate exceeding 300°C / min, almost no P compounds are formed, but if the starting temperature of the cooling treatment is lower than 550°C, P compounds are observed in the metal structure.On the other hand, if the cooling treatment start temperature is 670°C or higher, the proportion of the β1 phase becomes too high, degrading the alloy's ductility, dezincification corrosion resistance, and stress corrosion cracking resistance. Therefore, the cooling treatment start temperature must be lower than 670°C, and preferably lower than 650°C. After hot forging, placing the alloy in a simple furnace with an ambient temperature set to approximately 550 to approximately 600°C for several tens of seconds to several minutes, and then starting the cooling treatment, can produce a more uniform and stable forged product. Furthermore, to improve stress corrosion cracking resistance, shot blasting is an effective means after the hot forging and cooling treatment. While the stress corrosion cracking resistance of other copper alloys can also be improved by applying compressive stress to the surface, such as by shot blasting, the effect of shot blasting is even greater in the case of the present alloy, which contains a β1 phase.
[0090] In hot rolling, the ingot is heated and repeatedly rolled 5 to 15 times. The material temperature at the end of the final hot rolling (the material temperature 2 to 3 seconds after the end) is preferably above 540°C and below 750°C, and more preferably below 670°C. After hot rolling, the rolled material is cooled. Similar to hot extrusion, the cooling process begins at a temperature above 500°C and below 670°C. The average cooling rate in the temperature range from the cooling process start temperature to 500°C and the average cooling rate in the temperature range from 500°C to 300°C are set to at least 300°C / min, preferably above 600°C / min, and more preferably 900°C / min or higher. When cooling from a temperature below 300°C to room temperature, the cooling rate slows slightly as the temperature approaches room temperature, but it is desirable to continue cooling in the temperature range from 500°C to 300°C. Although there are no particular upper limits to the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C and in the temperature range from 500°C to 300°C, it is preferable that the cooling rate be approximately 9000°C / min or less.
[0091] (Heat Treatment) In the present application, if the cooling treatment cannot be started at a temperature higher than 500°C after the final hot working, or if the cooling cannot be performed at an average cooling rate of more than 300°C / min in the temperature range from 500°C to 300°C, the β phase cannot be reformed. Furthermore, when producing small-diameter rods, wires, etc., the β phase is generally not reformed even when cold working and heat annealing are included. In these cases, the β phase is reformed and the β1 phase is formed by annealing at a temperature higher than 520°C and lower than 630°C for 1 minute to 5 hours, and the cooling after annealing is started at a temperature higher than 500°C, with an average cooling rate of more than 300°C / min in the temperature range from the cooling treatment start temperature to 500°C and an average cooling rate of more than 300°C / min in the temperature range from 500°C to 300°C. Regarding the annealing conditions, if there are multiple annealing steps, only the final annealing is required. From the viewpoint of the temperature at which P compounds are generated, the annealing temperature is preferably 530°C or higher, more preferably 550°C or higher. Furthermore, the average cooling rate in the temperature range from 500°C to 300°C is preferably set to more than 600°C / min, more preferably 900°C / min or higher, considering the degree of β1 phase modification. As mentioned above, this heat treatment is applied to hot-worked materials that cannot be cooled under specified conditions after hot working, and materials that have been cold-worked after hot working and then annealed one or more times. There are no particular restrictions on the upper limits of the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C and in the temperature range from 500°C to 300°C. However, if mentioned, the cooling rate is preferably about 9000°C / min or lower.
[0092] (Cold Working Process) In the case of hot extruded rods, cold working may be applied to the hot extruded material to obtain high strength, improve dimensional accuracy, or to make the extruded rod or coil material into a straight shape with minimal bending. For example, the hot extruded material is cold drawn at a working ratio of about 2 to about 30%, or in some cases, drawn, and then straightened. Thin rods, wires, or rolled materials are repeatedly subjected to cold working and annealing, and after the final heat treatment, are subjected to cold working and straightening at a final working ratio of 0 to about 30%. The closer the final working ratio is to 0%, the less likely the material is to crack when subjected to cold working such as light crimping or bending.
[0093] (Low-Temperature Annealing) In the case of bars, wires, forgings, and rolled materials, low-temperature annealing may be performed as a final process at a temperature below the recrystallization temperature, primarily for the purposes of removing residual stress, straightening the bar (bar straightness), and adjusting and improving the metal structure. However, the β1 phase modified by hot working and heat treatment is lost when heat is applied to the alloy. For example, heating at 300°C for 2 hours destroys the β1 phase modification, causing the modified β1 phase to revert to the original β phase, resulting in improved machinability, dezincification corrosion resistance, and stress corrosion cracking resistance, all of which are properties of the original β phase alloy. Therefore, low-temperature annealing is not recommended, but temperatures below approximately 150°C are permissible.
[0094] In the free-machining alloy according to the embodiment of the present invention having the above-described configuration, the alloy composition, compositional formula, metal structure, structure-structure formula, and structure-composition formula are defined as described above, and therefore, even with a low Pb content, excellent machinability can be obtained, and the alloy has good dezincification corrosion resistance and stress corrosion cracking resistance, excellent hot workability, high strength, and an excellent balance of strength and ductility.
[0095] Although the embodiment of the present invention has been described above, the present invention is not limited to this and can be modified as appropriate within the scope of the technical requirements of the invention.
[0096] The following shows the results of confirmation experiments conducted to confirm the effects of this embodiment. Note that the following examples are intended to explain the effects of this embodiment, and the components, processes, and conditions described in the examples do not limit the technical scope of this embodiment.
[0097] Trial tests of copper alloys were conducted using a low-frequency melting furnace and semi-continuous casting machine used in actual operation. Trial tests of copper alloys were also conducted using laboratory equipment. The alloy compositions are shown in Tables 5 to 7. The manufacturing processes are shown in Tables 8 to 17. In the compositions, "Mm" stands for misch metal, which indicates the total amount of rare earth elements. Each manufacturing process is described below. In Tables 8 to 12 and 14 to 16, the cooling rate of hot working, such as hot extrusion, hot forging, or hot compression, is the average cooling rate from the end of hot working to the start of cooling treatment.
[0098]
[0099]
[0100]
[0101]
[0102]
[0103]
[0104]
[0105]
[0106]
[0107]
[0108]
[0109]
[0110]
[0111] Actual Machine Production: Processes AA, AB, and AD (Process Nos. A1-A5, A11H-A14H, A21-A25, A31H-A34H, A41-A44, A46H, and A47H). 240 mm diameter billets were produced using a commercially available low-frequency melting furnace and semi-continuous casting machine. Raw materials were similar to those used in the commercial production process. The billets were cut into 800 mm lengths and heated. Round bars with a diameter of 20.9 mm were extruded using an indirect extruder with a nominal capacity of 2,750 tons. The extruded material (round bars) was then coiled in a tank located a short distance from the extruder. This tank was equipped with a water-cooling system with adjustable water flow. When the extruded material reached a predetermined temperature in the tank, the cooling process (water cooling) was initiated while adjusting the water flow. In some cases, the cooling process began immediately after the extruded material was placed in the tank. Temperature measurements were performed using a radiation thermometer, and the temperature of the extruded material was measured when it was extruded from the extruder, when the cooling process began, and until it reached 500° C. and 300° C. For subsequent temperature measurements during hot extrusion and hot forging, a radiation thermometer (Model IGA8Pro / MB20) manufactured by LumaSense Technologies Inc. was used in combination with a contact thermometer.
[0112] In process AA, i.e., process Nos. A1 to A5, A11H to A14H, the extrusion temperature was 630°C. In process AB, i.e., process Nos. A21 to A25, A31H to A34H, the extrusion temperature was 615°C. In process AD, i.e., process Nos. A41 to A44, A46H, and A47H, the extrusion temperature was 720°C. Then, after the coiled 20.9 mm diameter extruded material reached a predetermined temperature in the bath, a cooling process was initiated, and the time until the extruded material reached 500°C and 300°C was measured. Although the radiation thermometer cannot accurately measure temperatures below 300°C, cooling continued under the same cooling conditions until the material was cooled to a temperature of approximately 100°C or less. Detailed conditions are shown in Tables 8, 9, and 10 for process Nos. For Processes A1 to A5, A11H to A14H, Process Nos. A21 to A25, A31H to A34H, and Process Nos. A41 to A44, A46H, and A47H, the average cooling rate from after extrusion to the start of cooling treatment, the cooling treatment start temperature, the average cooling rate in the temperature range from the cooling treatment start temperature to 300°C, and the average cooling rate in the temperature range from 500°C to 300°C may differ. When the cooling treatment start temperature is lower than 500°C, the average cooling rate in the temperature range from the cooling treatment start temperature to 300°C is recorded as the cooling rate in the temperature range from 500°C to 300°C. The average cooling rate in the temperature range from the cooling treatment start temperature to 500°C can be easily calculated from the average cooling rate in the temperature range from the cooling treatment start temperature to 300°C and the average cooling rate in the temperature range from 500°C to 300°C, and it was therefore confirmed that the cooling rate in the temperature range from the cooling treatment start temperature to 500°C was the same as the cooling rate in the temperature range from 500°C to 300°C, or was slightly faster under some conditions. After completion of cooling after hot extrusion, the extruded material was put into a combined machine at a processing rate of 8.4% and drawn and straightened into a straight bar with a diameter of 20 mm.
[0113] In Process No. A25 and Process No. A31H, the bars obtained in Process No. A21 were used and further subjected to low-temperature annealing in the laboratory at 130°C for 5 hours and 300°C for 2 hours. These Process AA, Process AB, and Process AD materials were subjected to microscopic observation, cutting tests, dezincification corrosion tests, and tensile tests.
[0114] Process AC, φ50 mm Bar (Process No. A50) A φ50 mm bar was prepared as a prototype for forging material by Process AC shown in Table 11 (Process No. A50). A 240 mm diameter billet was produced using a commercially available low-frequency melting furnace and semi-continuous casting machine, and the billet was cut into 800 mm lengths. The billet was extruded at 550°C into a 50 mm diameter round bar using a direct extruder with a nominal capacity of 3,000 tons. The extruded straight bar was placed on a steel table and naturally cooled to room temperature. It was then straightened and used as a material for flat forging, as described below. Since the final hot working was intended to be hot forging, no special cooling treatment was performed; the average cooling rate from 500°C to 300°C was 20°C / min.
[0115] Laboratory Extrusion Material, Process B (Process Nos. B1, B2, B3H) In Process B, raw materials were melted in a laboratory at the specified component ratios shown in Table 12. The molten metal was poured into a mold with a diameter of 100 mm and a length of 200 mm to produce billets. Some billets also contained intentionally added impurities such as Fe. The concentrations of the intentionally added impurities, such as Fe, were approximately the same as or lower than those of commercially available brass containing Pb. These billets were heated, and in Process No. B1, the extrusion temperature was set to 670°C, and the extrusion was performed to produce round bars with a diameter of 20 mm. After extrusion, the cooling process began at 540°C, and the material was cooled from 500°C to 300°C at an average cooling rate of 960°C / min. It was confirmed that the average cooling rate from 540°C to 500°C was approximately the same as that from 500°C to 300°C. Thereafter, cooling continued under the same cooling conditions until the material was cooled to a temperature of approximately 100°C or less. In Process No. B3H, the extrusion temperature was 670°C, and after extrusion into a round bar with a diameter of 20 mm, no cooling treatment was performed, and the bar was cooled from 500°C to 300°C at an average cooling rate of 40°C / min. These Process Nos. B1 and B3H were subjected to microscopic observation, cutting test, dezincification corrosion test, and tensile test, and a portion of Process No. B3H was used as a hot forging material for Process D. In Process No. B2, the extrusion temperature was 590°C, and the bar was extruded into a diameter of 50 mm, and no cooling treatment was performed, and the bar was cooled from 500°C to 300°C at an average cooling rate of 25°C / min.
[0116] Process C, Forging and Hot Pressing Materials: Castings (Process Nos. C1 and C2) Castings used as forging materials were prepared in a laboratory by melting raw materials at a predetermined composition ratio. The molten metal at approximately 1000°C was poured into an iron mold with an inner diameter of 35 mm and a depth of 200 mm (Process No. C1) and another iron mold with an inner diameter of 55 mm and a depth of 200 mm (Process No. C2). When the temperature of the casting reached approximately 700°C, it was removed from the mold and allowed to cool naturally without any cooling treatment. As shown in Table 13, the average cooling rate from 500°C to 300°C was 35°C / min for Process No. C1 and 23°C / min for Process No. C2. The casting for Process No. C1 was machined to an outer diameter of 20 mm using a lathe, and then cast into an iron mold with an inner diameter of 20 mm and a depth of 200 mm (Process No. C2). The casting C2 was machined to an outer diameter of 50 mm and finished as a material for forging in process D and process E, and a material for hot compression in process F, which will be described later.
[0117] Forged Flare Nuts (Process D) In Process D, the flare nut forgings were made from the actual extruded rods (Process Nos. A1, A13H, A21, A34H, and A47H), the laboratory extruded rod (Process No. B3H), and the laboratory cast (Process C1). These rods were then cut to weigh 120±1 g (119 g to 121 g) and formed into flare nut forgings with a hexagonal cross section of 27 mm and a length of 26 mm using a 500-ton hot forging press. As shown in Table 14, the hot forging temperatures were 670°C for Process Nos. D1, D3-D7, and D12H-D14H, 710°C for Process No. D2, 740°C for Process No. D8, and 770°C for Process No. D15H. The average cooling rate from after forging to the start of the cooling treatment was 100°C / min except for Process Nos. D15H and D13H, and 120°C / min for Process No. D15H. Process No. D13H was naturally cooled without cooling treatment. As shown in Table 14, the cooling treatment start temperature was 475 to 695°C. The average cooling rate in the temperature range from the cooling treatment start temperature to 300°C and the average cooling rate in the temperature range from 500°C to 300°C were varied from 240°C / min to 1980°C / min except for Process No. D13H. In Process Nos. D1 to D7 and D14H, the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C was the same as the average cooling rate in the temperature range from 500°C to 300°C, but the former was slightly faster in Process Nos. D8 and D15H. In Process No. D12H, the average cooling rate from the cooling treatment start temperature of 475°C to 300°C was recorded as the average cooling rate in the temperature range from 500°C to 300°C. In Process No. D7, hot forging and cooling treatment were performed under the same conditions as Process No. D5, followed by a shot blasting process. The shot blasting was performed for 10 minutes using a 0.6 mm diameter steel ball. These hot forged products were machined into Class 1 flare nuts with an inner diameter of 5 / 8 inch (= 15.9 mm) conforming to JIS B 8607. The Process D materials were subjected to microscopic observation, dezincification corrosion tests, and stress corrosion cracking tests.
[0118] Plain forging (Process E) Process E was a process for laboratory forging. The raw materials used were the actual extruded bar from Process No. A50, the laboratory extruded bar from Process No. B2, and the laboratory cast from Process No. C2. Each was cut to a length of 180 mm. These round bars were placed horizontally and forged to a thickness of 20 mm using a hot forging press with a capacity of 150 tons.
[0119] (Steps E1 to E7, E11H to E15H) In steps E1, E4 to E6, and E12H to E15H, the forging temperature was 630°C, in step E2 the forging temperature was 680°C, in step E3 the forging temperature was 700°C, in step E7 the forging temperature was 720°C, and in step E11H the forging temperature was 740°C. After hot forging, except for step E14H, the average cooling rate until the start of the cooling treatment was 35°C / min. As shown in Table 15, the cooling treatment was started at a temperature of 690°C to 455°C, and the average cooling rate from the cooling treatment start temperature to 300°C was changed from 900°C / min to 200°C / min, and the material was cooled to room temperature using the same cooling method. Step No. It was confirmed that for E1 to E6 and E15H, the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C was roughly the same as the average cooling rate in the temperature range from 500°C to 300°C. For Process Nos. E12H and E13H, the average cooling rate in the temperature range from the cooling treatment start temperature to 300°C was recorded as the average cooling rate in the temperature range from 500°C to 300°C. For Process No. E14H, no cooling treatment was performed, and natural cooling was performed, with the average cooling rate from 500°C to 300°C being 25°C / min. These flat forged materials were sectioned and subjected to tests for cutting, mechanical properties, dezincification corrosion, and microscopic observation.
[0120] Hot Compression Test (Process F) The hot-extruded rods from the actual machine (Process Nos. A13H, A34H, and A47H), the hot-extruded rods from the laboratory (Process No. B3H), and the castings from Process C1 were used as materials and finished to a diameter of 15 mm and a height of 27 mm on a lathe. Then, as shown in Table 16, a 10-ton Amsler-type testing machine equipped with a heating furnace was used to hot-compress the samples to a height of 8 mm at 650°C under a strain rate of 0.02 / sec. In Processes F1 to F3, the hot-compressed samples were removed from the heating furnace and cooled at a cooling rate of 50°C / min. Next, cooling treatment was initiated at 560°C, and the average cooling rate in the temperature range from 500°C to 300°C was 2100°C / min. The treatment continued below 300°C, and the samples were cooled to room temperature. Process No. In Process No. F4H, cooling treatment began at 560°C, and cooling was carried out at an average cooling rate of 200°C / min from the cooling treatment start temperature to 300°C. In Process No. F5H, no special cooling treatment was carried out, and cooling was carried out at an average cooling rate of 40°C / min from 500°C to 300°C. The average cooling rate in the temperature range from the cooling treatment start temperature (560°C) to 500°C was roughly the same as the average cooling rate in the temperature range from 500°C to 300°C. These hot-compressed materials were subjected to microscopic observation and dezincification corrosion tests.
[0121] Heat Treatment (Process G) In Process G, as shown in Table 17, the bar stock and forged products obtained in Process Nos. A1, A21, A41, A13H, A34H, A47H, D1, and D13H were heat-treated in the laboratory to examine changes in properties. All annealing was performed at 580°C for 30 or 60 minutes. For Process Nos. G1, G2, and G3, after annealing, cooling treatment was initiated at 560°C, and the average cooling rate in the temperature range from the cooling treatment start temperature to 300°C was 1800°C / min. The average cooling rate in the temperature range from the cooling treatment start temperature (560°C) to 500°C was roughly the same as the average cooling rate from 500°C to 300°C. Process Nos. For Process Nos. G11H and G12H, after annealing at 580°C, the cooling treatment start temperature was 470°C, and cooling was performed from 470°C to 300°C at an average cooling rate of 1500°C / min. For Process Nos. G13H and G14H, after annealing at 580°C, no special cooling treatment was performed, and cooling was performed from 500°C to 300°C at an average cooling rate of 25°C / min. These heat-treated materials were observed with a metallurgical microscope, and the bars were subjected to cutting tests, dezincification corrosion tests, and tensile tests, and the forged products were subjected to dezincification corrosion tests and stress corrosion cracking tests.
[0122] (Comparative Materials) As comparative materials, φ20 mm rods made of free-cutting brass C3604 containing 3 mass% Pb were prepared. Also, φ50 mm and φ20 mm rods made of forging brass C3771 containing 2 mass% Pb were prepared. These materials, designated Alloys X, Y, and Z, were commercially available. Alloy Y was hot forged and cooled under the same conditions as in Process Nos. E14H and E1. Alloy Z was hot forged and cooled under the same conditions as in Process Nos. D13H and D1. Alloy X was subjected to metallurgical microscopy, cutting tests, dezincification corrosion tests, and tensile tests. Alloy Y was subjected to metallurgical microscopy, cutting tests, dezincification corrosion tests, and tensile tests. Alloy Z was subjected to metallurgical microscopy, dezincification corrosion tests, and stress corrosion cracking tests.
[0123] The above-mentioned test materials were evaluated for the following items. The evaluation results are shown in Tables 18 to 56. The area fraction of the β phase, i.e., the unmodified β phase, is listed in each table as f4A, distinguished from the area fraction of the β1 phase (f4). When f4 = (area fraction of β1) = 0, the value calculated using the value of f4A = (area fraction of β) instead of (β1) is listed in the (β1) term of the calculation formula for f6, marked with an asterisk (*), as a reference value for f6.
[0124] (Observation of Metal Structure) The metal structure was observed using the following method, and the area ratio (%) of each phase, including the α, β, and γ phases, was measured by image analysis. Note that β phases in which grain boundaries were observed were classified as β1 phases and distinguished from the β phase. The α', β', and γ' phases were included in the α, β, and γ phases, respectively. The α phase exhibits a granular, elliptical shape and is often accompanied by twin crystals. The β and β1 phases are present around the granular, elliptical α phase. This distinguishes the α, β, and β1 phases. Bars and forged products of each test material were cut parallel to the longitudinal direction or parallel to the flow direction of the metal structure. The surfaces were then mirror-polished and etched with a mixture of hydrogen peroxide and ammonia water. For etching, an aqueous solution containing 3 mL of 3 vol% hydrogen peroxide and 22 mL of 14 vol% ammonia water was used. The polished metal surface was immersed in this aqueous solution for about 2 to about 10 seconds at room temperature of about 15 to about 25° C. Note that when the β1 phase is present, corrosion resistance is improved compared to when the β phase is present, so the immersion time for etching had to be longer, about 5 to 10 seconds.
[0125] The metallographic structure was observed at 500x magnification using a metallurgical microscope to determine the proportion of each phase. Depending on the state of the metallographic structure, observation was performed at 1000x magnification to confirm the phases and compounds. In the five-field micrographs, each phase (α phase, β phase, β1 phase, γ phase) was manually filled in using the image processing software "Photoshop CC." To distinguish between β phase and β1 phase, if one or more β grain boundaries were observed within a field of view, all β phase within that field of view was filled in as β1 phase. The images were then binarized using the image analysis software "WinROOF2013" to determine the area ratio of each phase. Specifically, the average area ratio of each phase was calculated for the five fields of view, and this average value was used as the area ratio of each phase. Compounds containing P and Si, precipitates, oxides, Pb or Bi particles, sulfides, and precipitated particles were excluded, and the total area ratio of all constituent phases was set to 100%.
[0126] When the β phase is modified, grain boundary patterns, i.e., crystal grain boundaries, are observed within the β phase when observed with a metallurgical microscope using the etching solution. In this application, when crystal grain boundaries are observed within the β phase, the β phase is designated as the β1 phase and distinguished from ordinary β phase. Here, the crystal grain boundary refers to the linear pattern that penetrates the β1 phase grains observed within the β1 phase, as shown in Figure 1A. In addition to the β1 phase, compounds and precipitates of P and Si may also be present in the metallurgical structure. Compounds of P and Zn or Si are present as dark gray particles of approximately 0.5 to approximately 2 μm in size under a 500x metallurgical microscope, primarily within the β phase, the β1 phase, and at the phase boundary between the β phase and the α phase. Compounds of Fe, Mn, Cr, and P or Si can be seen as light blue particles of approximately 1 to approximately 5 μm in size. Pb or Bi particles and particles formed by combining Pb and Bi exist as fine black particles of 2 μm or less. These compounds can be roughly distinguished using a metallurgical microscope. In the characteristic evaluation table, when grain boundaries were observed within the β1 phase (β phase) in the metallographic structure, they were marked as "B" (present), and when they were not, they were marked as "D" (absent). Regarding P compounds, when the P content was 0.06 mass% and the average cooling rate from 500°C to 300°C was 15 to 50°C / min, approximately 500 to 1,000 P compounds were observed in a 500x magnification field (80 mm x 120 mm when printed). However, in the printed metallographic structure, it was difficult to distinguish between P compounds, Fe, Mn, Cr, P or Si compounds, Pb particles, etc. Therefore, when determining the presence or absence of P compounds from a printed metallographic photograph, if there were fewer than 50 P compounds and potential P compounds within the field of view of the photograph, the P compounds were deemed absent and rated as "D" (absent). If there were 50 or more but less than 300 particles, the P compounds were considered to be present but in small quantities and rated as "C" (fair). If there were 300 or more particles, the P compounds were considered to be present and rated as "B" (present). The presence or absence, and the amount, of P compounds is one indicator of whether the treatment was appropriate.
[0127] When it was difficult to identify the phases, compounds, and precipitates, the phases and precipitates were identified by the FE-SEM-EBSP (Electron Backscattering Diffracton Pattern) method using a field emission scanning electron microscope (FE-SEM) (JSM-7000F manufactured by JEOL Ltd.) and an attached EDS under conditions of an acceleration voltage of 15 kV and a current value (set value 15) at a magnification of 500x or 2000x.
[0128] (Conductivity) Conductivity was measured using a conductivity measuring device (SIGMATEST D2.068) manufactured by Nippon Foerster Co., Ltd. In this specification, the terms "electrical conduction" and "conductivity" are used interchangeably. In addition, since thermal conductivity and electrical conductivity are strongly correlated, the higher the conductivity, the better the thermal conductivity.
[0129] (Tensile strength / elongation) Each test material was processed into a No. 10 test piece of JIS Z 2241, and the tensile strength and elongation were measured. The tensile strength of the hot extruded material or hot forged material that was not subjected to the cold working process is preferably 460 N / mm 2 More preferably, 490 N / mm 2 More preferably, 520 N / mm 2 If the alloy has a tensile strength of S (N / mm), it is at the highest level among free-cutting copper alloys, and can be used in various fields to reduce the thickness and weight of components, or to increase the allowable stress. 2 ), and elongation is E (%), the characteristic relational equation that shows the balance between strength and ductility is f7=S×{(E+100) / 100} 1/2 A value of 540 or more is one measure of high strength and high ductility material. f7 is more preferably 570 or more, and even more preferably 600 or more. This can be said to be a very high standard among free-cutting copper alloys. Many parts used in faucets, valves, joints, pressure vessels, air conditioners and refrigerators are made from hot forged or hot extruded rods, and the tensile strength of the currently used Pb-added copper alloy, C3604, is about 390 to 420 N / mm 2In contrast to the conventional steel, which has an elongation of 30 to 35% and an f7 of approximately 470, the present embodiment achieves a lighter weight due to its high strength, good dezincification corrosion resistance, and good stress corrosion cracking resistance.
[0130] <Machinability Test Using a Lathe> Machinability was evaluated by a cutting test using a lathe as follows. Hot extruded bar material (processes AA, AB, and B) and hot forged material (process E) were cut to produce test materials with a diameter of 18 mm. A K10 carbide tool (chip) without a chip breaker was attached to the lathe. Using this lathe, the circumference of a test material with a diameter of 18 mm was cut under dry conditions with a rake angle of 0°, a nose radius of 0.4 mm, a clearance angle of 6°, a cutting speed of 40 m / min or 110 m / min, a cutting depth of 1.0 mm, and a feed rate of 0.11 mm / rev. In the present embodiment, the effect of cutting speed was also investigated.
[0131] The signals emitted from a three-part dynamometer (AST-type tool dynamometer AST-TL1003, manufactured by Miho Electric Manufacturing Co., Ltd.) attached to the tool were converted into electrical voltage signals and recorded on a recorder. These signals were then converted into cutting resistance (principal force, feed force, thrust force, N). In order to reduce the influence of tip wear, the cutting test was carried out twice, going back and forth from A → B → C → ... C → B → A, and measurements were taken four times for each sample. The cutting resistance can be calculated using the following formula: Cutting resistance (resultant of principal force, feed force, thrust force) = ((principal force) 2 + (feed force) 2 + (back force) 2 ) 1/2Here, the principal component of cutting resistance is the largest, and since the magnitude of the principal component determines the cutting resistance, the principal component was used as the cutting resistance, and the average of four measured values was calculated and used as the cutting resistance. The cutting resistance (principal component of cutting resistance) of a commercially available free-cutting brass bar C3604 (Alloy X, φ20 mm) made of a Zn-59 mass% Cu-3 mass% Pb-0.2 mass% Fe-0.3 mass% Sn alloy was set to 100, and the relative value of the cutting resistance (machinability index) of the sample was calculated and relative evaluation was performed. In other words, the higher the machinability index, the lower the cutting resistance and the better the machinability. The machinability index was calculated as follows: Index of cutting test results of sample (machinability index) = (Cutting resistance (principal component of cutting resistance) of C3604 / Cutting resistance (principal component of cutting resistance) of sample) × 100
[0132] Cutting resistance (principal force) depends on the shear strength and tensile strength of the material, and the stronger the material, the higher the cutting resistance tends to be. For example, in the case of a copper alloy that has the same good chip breakability as C3604 but is approximately 1.2 times stronger than C3604, cutting resistance is proportional to the material strength, so the cutting resistance is approximately 20% higher than C3604. Therefore, for copper alloys with high strength, a cutting resistance that is approximately 40% higher than C3604 is considered good for practical use. In this embodiment, the tensile strength and shear strength of the extruded material are approximately 1.2 times higher than C3604. Therefore, the machinability evaluation criteria in this embodiment were evaluated using a machinability index of approximately 72 as the boundary (boundary value). Specifically, a machinability index of 80 or higher was evaluated as having excellent machinability (rating: A, excellent) and equivalent machinability to C3604. If the machinability index was 72 or more and less than 80, the machinability was evaluated as good (evaluation: B, good). If the machinability index was 66 or more and less than 72, the machinability was evaluated as fair (evaluation: C, fair). If the machinability index was less than 66, the machinability was evaluated as unacceptable (evaluation: D, poor). In this application, the aim was to achieve good machinability, so a machinability index of 72 or more was considered acceptable.
[0133] (Dezincification corrosion test: ISO 6509 dezincification corrosion test) The dezincification corrosion test method was evaluated using the ISO 6509 dezincification corrosion test. This test method has been adopted in many countries and is also specified in the JIS standard, JIS H 3250. The dezincification corrosion test procedure involves first embedding the test material in a phenolic resin material, specifically embedding the exposed sample surface in the phenolic resin material so that it is perpendicular to the extrusion direction of the extruded material. The sample surface was polished with emery paper up to 1200 grit, then ultrasonically cleaned in pure water and dried. Each sample was then polished with 1.0% cupric chloride dihydrate (CuCl 2 ・2H 2 The specimens were immersed in an aqueous solution (12.7 g / L) of HCl (O) and held at 75°C for 24 hours. The specimens were then removed from the aqueous solution. The specimens were re-embedded in phenolic resin so that the exposed surface was perpendicular to the extrusion direction, longitudinal direction, or forging flow direction. The specimens were then cut so that the longest cross-section of the corroded area was obtained. The specimens were then polished. Using a metallurgical microscope, corrosion depth was observed at 100-500x magnifications in 10 fields of view. The deepest corrosion point was recorded as the maximum dezincification corrosion depth. In ISO 6509 testing, a maximum corrosion depth of 200 μm or less is considered acceptable for practical corrosion resistance. When excellent corrosion resistance is required, the maximum corrosion depth is preferably 100 μm or less. In this test, a maximum corrosion depth exceeding 200 μm was rated as unacceptable (rating: D, poor). When the maximum corrosion depth was more than 100 μm and 200 μm or less, it was evaluated as good (evaluation: B, good).When the maximum corrosion depth was 100 μm or less, it was evaluated as excellent (evaluation: A, excellent).
[0134] (Stress Corrosion Cracking Test) To determine whether the specimens could withstand a stress corrosion cracking environment, a stress corrosion cracking test was conducted using the following procedure. First, a φ20 mm rod was cut to a weight of 120±1 g (119-121 g) as the test material. This was then formed into a hexagonal flare nut forged material with a 27 mm opposite side and a 26 mm length using a 500-ton hot forging press under the conditions of Table 14, Process D. Furthermore, as shown in Table 14, some samples were subjected to shot blasting in the same manner as Process No. D7. Furthermore, as shown in Table 17, the forged materials were subjected to heat treatment under several conditions (Process Nos. G2, G3, G12H, and G14H). These forged materials were threaded and the end faces were finished by cutting, resulting in flare nuts shaped in accordance with JIS B 8607, with an inner diameter of 5 / 8 inch (= 15.9 mm). In order to apply a load stress to the flare nut, a C6932 base was prepared, which was machined to the male thread shape of a flare nut joint with a nominal diameter of 5 / 8 inch (= 15.9 mm) conforming to JIS B 8607. The base was tightened using a torque gauge until the specified torque was reached. Ammonia water of a specified concentration was placed in a desiccator, and the flare nut with the load stress applied was placed 60 mm from the liquid surface. After holding for a specified time, the flare nut was removed. The test was carried out in a room controlled at 25 ± 1 ° C (24-26 ° C) by air conditioning. The stress corrosion cracking test was carried out using the following two methods.
[0135] (Stress Corrosion Cracking Test-1) Ammonia water with an ammonia concentration of 14 vol% was used. 1000 ml of ammonia water was placed in a desiccator, and a torque of 70 N m was applied to the sample. The sample was exposed in the desiccator for 48 hours and 96 hours. The sample was washed with 10 vol% sulfuric acid, then visually observed, and evaluated for the presence or absence of cracks. This test was conducted in accordance with JIS H 3250 except for the exposure time. While JIS H 3250 requires an exposure time of 2 hours, this method was a more severe stress corrosion cracking test, requiring an exposure time of 20 times longer. Since the present application aims for good stress corrosion cracking resistance, samples in which cracks were observed after 48 hours of exposure were rated "D" (poor). Samples in which no cracks were observed after 48 hours of exposure but cracks were observed after 96 hours of exposure were rated "C" (fair). Samples in which no cracks were observed after 96 hours of exposure were rated "B" (good). A rating of "C" was deemed acceptable.
[0136] (Stress Corrosion Cracking Test-2) In another stress corrosion cracking test, 200 ml of ammonia water with an ammonia concentration of 28 vol% was placed in a desiccator, and a sample was exposed to a torque of 150 N·m and held in the desiccator for 75 hours. The sample was removed from the desiccator, washed with 10 vol% sulfuric acid, and then visually inspected for cracks. Compared to Stress Corrosion Cracking Test-1, the ammonia concentration was higher and the load torque was greater, so the following evaluation criteria were used. A sample with the largest visible crack measuring more than half the length of the 26 mm of the sample, i.e., a crack of 13 mm or more, was rated "D" (poor). A sample with a clearly visible crack measuring more than approximately 1 / 5 of the length of the 26 mm of the sample, i.e., a crack of 5 mm to 13 mm, was rated "C" (fair). The specimens with cracks smaller than about 1 / 5 of the 26 mm length, i.e., those with no cracks or cracks smaller than 5 mm observed by visual inspection, were rated as "B" (good). A rating of "C" was deemed acceptable.
[0137]
[0138]
[0139]
[0140]
[0141]
[0142]
[0143]
[0144]
[0145]
[0146]
[0147]
[0148]
[0149]
[0150]
[0151]
[0152]
[0153]
[0154]
[0155]
[0156]
[0157]
[0158]
[0159]
[0160]
[0161]
[0162]
[0163]
[0164]
[0165]
[0166]
[0167]
[0168]
[0169]
[0170]
[0171]
[0172]
[0173]
[0174]
[0175]
[0176] 1) It has been confirmed that by satisfying the composition of this embodiment, the compositional relations f0 to f2, the requirements of the metal structure, the structure relations f3 to f5, and the structure-composition relation f6, even with a small amount of Pb, it is possible to obtain hot extruded and hot forged materials that have good machinability, good dezincification corrosion resistance and stress corrosion cracking resistance, high electrical conductivity of 15% IACS or higher, high strength, good ductility, and a high balance of strength and ductility (characteristic relation f7). Furthermore, while the presence of P compounds has the effect of significantly improving machinability, the β1 phase, which is a modified β phase, further improves machinability. At the same time, it has been confirmed as follows (Alloy Nos. S01, S02, S03, S11, S12, S13, S21 to S46), that the dezincification corrosion resistance and stress corrosion cracking resistance, which were major problems with the conventional β phase, can be significantly improved by modifying the β phase.
[0177] 2) By adding more than 0.50 mass% Si, the β phase was modified, and grain boundaries were observed within the β1 phase. As a result, dezincification corrosion resistance and stress corrosion cracking resistance were improved, and cutting resistance was reduced (machinability index was increased). With an Si content of 0.65 mass% or more, dezincification corrosion resistance, stress corrosion cracking resistance, and machinability were further improved. In other words, it is believed that the β phase was further modified. On the other hand, when the Si content exceeded 1.20 mass%, electrical conductivity decreased (Alloy Nos. S01, S37, S48, S49, S74, S78, S80, etc.). 3) By adding more than 0.01 mass% P, the β phase was modified, and grain boundaries were observed within the β1 phase. As a result, dezincification corrosion resistance and stress corrosion cracking resistance were improved, and cutting resistance was reduced. When the P content was 0.03 mass% or more, the dezincification corrosion resistance, stress corrosion cracking resistance, and machinability were further improved. In other words, it is believed that the β phase was further modified. When the P content exceeded 0.18 mass%, the elongation value decreased (Alloy Nos. S01, S31, S71, S75, etc.). 4) When the Cu content exceeded 60.5 mass%, the β phase was modified, and grain boundaries were observed within the β1 phase. As a result, the dezincification corrosion resistance and stress corrosion cracking resistance improved, ductility improved, and cutting resistance decreased. When the Cu content was high, the β phase was reduced, and in some cases, the γ phase began to appear, resulting in a poor balance between strength and ductility and poor machinability (Alloy Nos. S01, S35, S38, S47, S48, S72, S80, Figures 1A to 6A).
[0178] 5) When the Pb content was less than 0.002 mass%, the machinability was poor (Alloy No. S73). When the Pb content was 0.003 mass% or more, or even 0.01 mass% or more, the machinability was improved (Alloy Nos. S33 and S23). It was confirmed that the inclusion of Bi reduced the cutting resistance equivalent to that of Pb (Alloy Nos. S01, S32, etc.). 6) When the Sn content exceeded 0.05 mass%, the dezincification corrosion resistance improved. When the Sn content exceeded 0.10 mass%, the dezincification corrosion resistance was further improved. In addition, the stress corrosion cracking resistance was also improved. On the other hand, when the Sn content was 0.90 mass% or more, the γ phase appeared, which actually worsened the dezincification corrosion resistance, reduced ductility, and increased the cutting resistance (lowered the machinability index). Furthermore, when the Sn / Si ratio was 1 or more, the β phase was not modified, and the dezincification corrosion resistance was poor (Alloy Nos. S01, S39 to S46, S82, and S83).
[0179] 7) It was confirmed that the inclusion of unavoidable impurities at levels common in actual production did not significantly affect various properties (Alloy Nos. S01, S02, S03, S11-S13, S27-S30). 8) When the total content of the unavoidable impurities Fe, Mn, Co, and Cr was 0.40 mass% or more, the β phase was modified, but cutting resistance was high, the strength-ductility balance was poor, and dezincification corrosion resistance was slightly poor. When the total content of Fe, Mn, Co, and Cr was less than 0.40 mass%, cutting resistance was reduced, the strength-ductility balance was improved, and dezincification corrosion resistance and stress corrosion cracking resistance were good. Furthermore, when the total content of Fe, Mn, Co, and Cr was less than 0.30 mass%, cutting resistance was further reduced, the strength-ductility balance was improved, and dezincification corrosion resistance and stress corrosion cracking resistance were good. The decrease in cutting resistance, strength / ductility balance, and dezincification corrosion resistance is believed to be due to the following reasons: Fe, Mn, etc., combined with some of the Si and P, forming intermetallic compounds of Fe, Mn, etc., with Si and P. As a result, the presence of compounds of Fe, etc., with Si and P and the reduction in the concentrations of Si and P, which effectively modify the β phase, are believed to have resulted in poor machinability and corrosion resistance (Alloy Nos. S01, S02, S84, S25-S30). 9) When the amount of Al, an unavoidable impurity, was 0.30 mass% or more, the β phase was not modified and dezincification corrosion resistance was poor. When the amount of Al was less than 0.30 mass%, the β phase was modified and the dezincification corrosion resistance was improved, and when the amount of Al was less than 0.15 mass%, the machinability, strength-ductility balance, dezincification corrosion resistance, and stress corrosion cracking resistance were improved (Alloy Nos. S01, S85, S26, and S28 to S30).
[0180] 10) When the value of the compositional relational expression f1 was small, the β phase was not modified, resulting in poor dezincification corrosion resistance. When the value of the compositional relational expression f1 was large, the area fraction of the β1 phase decreased (Alloy Nos. S76 and S79). When the value of the compositional relational expression f1 was 57.5 or more, the β phase was modified, resulting in good dezincification corrosion resistance, and when the value of the compositional relational expression f1 was 58.0 or more, the area fraction of the β1 phase increased. When the value of the compositional relational expression f1 was 60.5 or less, the area fraction of the β1 phase increased, and when the value of the compositional relational expression f1 was 60.2 or less, the area fraction increased, resulting in a high machinability index (e.g., Alloy Nos. S01, S03, S35, and S36).
[0181] 11) When the area ratio of the β1 phase was 25% or less, good machinability was not obtained. When the area ratio of the β1 phase exceeded 25%, and even 30% or more, the cutting resistance decreased. When the area ratio of the β1 phase exceeded 80%, the β phase was often not modified, i.e., grain boundaries were no longer observed within the β phase. As a result, the cutting resistance, particularly at 110 m / min, was high and the dezincification corrosion resistance and stress corrosion cracking resistance were poor. When the area ratio of the β1 phase was 80% or less, and even 70% or less, the β phase was modified, and the dezincification corrosion resistance and stress corrosion cracking resistance improved. Regarding dezincification corrosion, although the β phase was modified and the progression of dezincification corrosion was significantly delayed, the β1 phase was dezincified more than the α phase. Therefore, a high area fraction of the β1 phase slightly accelerated the progression of dezincification corrosion (Alloy Nos. S03, S11, S72, S81, S76, Processes D1, D11H, E1, E11H, Figure 1B, etc.). 12) When the area fraction of the γ phase was 4% or more, the elongation value was low. Also, the cutting resistance was high (Alloy Nos. S78, S82). 13) When the structure-composition relationship f6 was low, the machinability was poor (Alloy No. S81). When f6 was greater than 35, the machinability was improved (e.g., Alloy No. S12, Processes E3, E4, Alloy No. S02, Process D11H).
[0182] 14) After hot extrusion, when the starting temperature of the cooling treatment exceeded 500°C and the average cooling rate in the temperature range from the starting temperature of the cooling treatment to 300°C and the average cooling rate in the temperature range from 500°C to 300°C exceeded 300°C / min, the β phase was modified and grain boundaries were observed within the β1 phase. When the β phase was modified, cutting resistance was reduced, dezincification corrosion resistance and stress corrosion cracking resistance were significantly improved, strength was high, and the strength-ductility balance was improved. Regarding machinability, when the β phase was modified, there was only a slight decrease in machinability even when the cutting speed increased (Process Nos. A1 to A5, D1 to D5, E1 to E5, F1 to F3, G1 to G3, Figures 1A to 6A, etc.). 15) When the cooling treatment start temperature exceeded 500°C and was lower than approximately 530°C, and when the average cooling rate in the temperature range from 500°C to 300°C was approximately 400 to approximately 500°C / min, grain boundaries were observed within the β1 phase, and small amounts of P compounds were sometimes present. When small amounts of P compounds were present, the cutting resistance was slightly higher and the dezincification corrosion resistance was slightly worse than when no P compounds were present (Steps Nos. A1 to A5, D1 to D5, E1 to E5, F1 to F3, G1 to G3, Figures 1A to 6A, Figures 1B to 6B, etc.).
[0183] 16) When the average cooling rate in the temperature range from 500°C to 300°C was approximately 200-250°C / min, no grain boundaries were observed within the β1 phase, and small amounts of P compounds were often present. As a result of the absence of grain boundaries in the β1 phase, machinability, particularly at 110 m / min, deteriorated, and dezincification corrosion resistance deteriorated (Process Nos. A14H, D14H, etc.). 17) When the cooling treatment starting temperature was 550°C or higher, and the average cooling rate in the temperature range from the cooling treatment starting temperature to 300°C and the average cooling rate in the temperature range from 500°C to 300°C were preferable, the machinability index was high, and the dezincification corrosion resistance and stress corrosion cracking resistance were good. In other words, it is believed that when the cooling treatment was started at an appropriate temperature and the cooling rate was fast, the β phase was further modified. (Step Nos. A1 to A5, A11H to A14H, D1 to D5, D11H to D14H, E1 to E5, E11H to E15H, F1 to F3, F4H, F5H, G1 to G3, G11H to G14H, Figures 1B to 6B, etc.). 18) When the starting temperature of the cooling treatment was higher than 670°C, the proportion of the β1 phase increased, the cutting resistance was slightly high, especially at 110 m / min, and the dezincification corrosion resistance was slightly poor. When the proportion of the β1 phase became too high, the β phase was sometimes not modified. Note that the dezincification corrosion occurred in a selective manner, and a high proportion of the β1 phase seemed to slightly accelerate the rate of dezincification corrosion (Step Nos. A1 to A5, D1 to D5, E1 to E5, F1 to F3, G1 to G3, etc.).
[0184] 19) When the β phase was modified and the β1 phase was observed, the stress corrosion cracking resistance improved, and all samples were rated "B" in Stress Corrosion Cracking Test-1 (Process Nos. D1 to D5). 20) By performing shot blasting after hot working (hot forging), the stress corrosion cracking resistance was further improved, and all samples were rated "B" in Stress Corrosion Cracking Test-1 and Stress Corrosion Cracking Test-2. On the other hand, for samples in which the β1 phase was not observed or samples with a low Si content, shot blasting did not improve the stress corrosion cracking resistance (Process Nos. D3, D7, Alloy Nos. S71 and 80).
[0185] 21) When two hot working processes are performed, for example, when hot-extruded bar material is hot-forged, regardless of the cooling method after the first hot working process, it was confirmed that the β phase is reformed if the final hot working process, i.e., the cooling treatment of the hot forging, is appropriate (Process Nos. D1-D5, D7). 22) Even when the hot-forged material is a cast, it was confirmed that the β1 phase is observed and the same properties are obtained as in hot-extruded material if the cooling treatment after hot forging is appropriate (Process Nos. D6, E6, F1). 23) When the alloy with reformed β phase was held at 300°C for 2 hours, the β1 phase grain boundaries disappeared. As a result, machinability and dezincification corrosion resistance were also deteriorated. At 130°C for 5 hours, the β1 phase grain boundaries were observed, and no deterioration in machinability or dezincification corrosion resistance was observed (Process Nos. A21, A25, A31H).
[0186] 24) Even when the specified cooling treatment is not performed in the final hot working, the hot-worked material is annealed at a temperature above 520°C and lower than 630°C for 1 minute to 5 hours, and after annealing, the cooling treatment is started at a temperature higher than 500°C, and the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C and in the temperature range from 500°C to 300°C exceeds 300°C / min. This has been confirmed to reform the β phase, and in particular to significantly improve the dezincification corrosion resistance and stress corrosion cracking resistance (Steps Nos. G1 to G3, Figures 5A and 5B).
[0187] From the above, the alloy of this embodiment, in which the contents of each additive element, the compositional relationship, and the structural relationship are within appropriate ranges, has excellent hot workability, machinability, mechanical properties, dezincification corrosion resistance, and stress corrosion cracking resistance. Furthermore, in order to obtain excellent properties from the alloy of this embodiment, it is possible to achieve this by setting the manufacturing conditions for hot extrusion and hot forging and the conditions for heat treatment within appropriate ranges.
[0188] The free-cutting copper alloy of this embodiment has a low Pb content, excellent hot workability and machinability, high strength, and an excellent balance of strength and elongation. Therefore, the free-cutting copper alloy of this embodiment is suitable for drinking water and sanitary equipment and parts, food utensils, electrical and electronic equipment parts, automobile parts, machine parts, stationery, toys, musical instruments, sliding parts, instrument parts, precision machine parts, medical parts, drinking water equipment and parts, water meters, and parts related to liquids and gases such as industrial water, wastewater, and hydrogen. Specifically, the free-cutting copper alloy is suitable for use in the above-mentioned fields as a component material for water taps, stop valves, mixer taps, shower heads, valves, joints, cocks, gears, shafts, bearings, trumpets, shafts, sleeves, spindles, sensors, bolts, nuts, flare nuts, pen nibs, insert nuts, cap nuts, nipples, spacers, screws, and other products.
Claims
1. Cu is more than 60.5 mass% and less than 65.0 mass%, Si is more than 0.50 mass% and less than 1.20 mass%, Pb is 0.002 mass% or more and less than 0.20 mass%, P is more than 0.01 mass% and less than 0.18 mass%, Bi is 0.0001 mass% or more and less than 0.20 mass% as an optional element, and the balance is Zn and inevitable impurities, wherein the total content of Fe, Mn, Co and Cr among the inevitable impurities is less than 0.40 mass%, and the content of Al is less than 0.30 mass%, When the Cu content is [Cu] mass%, the Si content is [Si] mass%, the Pb content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, the relationship of 57.5≦f1=[Cu]-4.6×[Si]+0.5×([Pb]+[Bi])-[P]≦60.5 is satisfied, and when Bi is contained, the relationship of 0.003≦f2=[Pb]+[Bi]<0.20 is satisfied. In addition, when the area ratio of the α phase, the area ratio of the γ phase, and the area ratio of the β1 phase, which is a modified β phase, are (α)%, (γ)%, and (β1)%, respectively, in the constituent phases of the metal structure excluding non-metallic inclusions, the area ratio of the α phase, the area ratio of the γ phase, and the area ratio of the β1 phase, which is a modified β phase, are (β1), the following relationships are satisfied: 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, 27<f6=(β1)×([Si]) 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 ×20+([P]) 1/2 ×15, and the β1 phase has grain boundaries that can be observed when etched with a mixed solution of hydrogen peroxide and aqueous ammonia.
2. Contains 61.2 mass% or more and 64.8 mass% or less of Cu, 0.65 mass% or more and 1.10 mass% or less of Si, 0.003 mass% or more and less than 0.10 mass% of Pb, and 0.03 mass% or more and 0.15 mass% or less of P, and contains 0.001 mass% or more and less than 0.10 mass% of Bi as an optional element, with the balance being Zn and inevitable impurities, wherein the total content of Fe, Mn, Co and Cr among the inevitable impurities is less than 0.30 mass%, and the content of Al is less than 0.15 mass%, When the Cu content is [Cu] mass%, the Si content is [Si] mass%, the Pb content is [Pb] mass%, the P content is [P] mass%, and the Bi content is [Bi] mass%, the relationship of 58.0≦f1=[Cu]-4.6×[Si]+0.5×([Pb]+[Bi])-[P]≦60.2 is satisfied, and when Bi is contained, the relationship of 0.004≦f2=[Pb]+[Bi]<0.10 is satisfied. In addition, when the area ratio of the α phase, the area ratio of the γ phase, and the area ratio of the β1 phase, which is a modified β phase, are (α)%, (γ)%, and (β1)%, respectively, in the constituent phases of the metal structure excluding non-metallic inclusions, the area ratio of the α phase, the area ratio of the γ phase, and the area ratio of the β1 phase, which is a modified β phase, are (β1), the following relationships are satisfied: 30≦f3=(α)≦70, 30≦f4=(β1)≦70, 0≦f5=(γ)<1, 35<f6=(β1)×([Si]) 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 ×20+([P]) 1/2 ×15, and the β1 phase has grain boundaries that can be observed when etched with a mixed solution of hydrogen peroxide and aqueous ammonia.
3. Cu is more than 60.5 mass% and less than 65.0 mass%, Si is more than 0.50 mass% and less than 1.20 mass%, Pb is 0.002 mass% or more and less than 0.20 mass%, P is more than 0.01 mass% and less than 0.18 mass%, Sn is more than 0.05 mass% and less than 0.90 mass%, Bi is contained as an optional element in an amount of 0.0001 mass% or more and less than 0.20 mass%, and the balance is Zn and inevitable impurities, wherein the total content of Fe, Mn, Co and Cr among the inevitable impurities is less than 0.40 mass%, and the content of Al is less than 0.30 mass%, When the Cu content is [Cu] mass%, the Si content is [Si] mass%, the Pb content is [Pb] mass%, the P content is [P] mass%, the Bi content is [Bi] mass%, and the Sn content is [Sn] mass%, there is a relationship of 57.5≦f1=[Cu]-4.6×[Si]+0.5×([Pb]+[Bi])-[P]-[Sn]≦60.5, and there is also a relationship of f0=[Sn] / [Si]<1, and when Bi is contained, there is a relationship of 0.003≦f2=[Pb]+[Bi]<0.20, and In the constituent phases of the metal structure excluding nonmetallic inclusions, if the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, then 20≦f3=(α)<75, 25<f4=(β1)≦80, 0≦f5=(γ)<4, 27<f6=(β1)×([Si]) 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 ×20+([P]) 1/2 ×15, and the β1 phase has grain boundaries that can be observed when etched with a mixed solution of hydrogen peroxide and aqueous ammonia.
4. The alloy contains 61.2 mass% or more and 64.8 mass% or less of Cu, 0.65 mass% or more and 1.10 mass% or less of Si, 0.003 mass% or more and less than 0.10 mass% of Pb, 0.03 mass% or more and 0.15 mass% or less of P, and 0.10 mass% or more and less than 0.50 mass% of Sn, and contains 0.001 mass% or more and less than 0.10 mass% of Bi as an optional element, with the balance being Zn and inevitable impurities, and among the inevitable impurities, the total content of Fe, Mn, Co and Cr is less than 0.30 mass%, and the content of Al is less than 0.15 mass%, When the Cu content is [Cu] mass%, the Si content is [Si] mass%, the Pb content is [Pb] mass%, the P content is [P] mass%, the Bi content is [Bi] mass%, and the Sn content is [Sn] mass%, there is a relationship of 58.0≦f1=[Cu]-4.6×[Si]+0.5×([Pb]+[Bi])-[P]-[Sn]≦60.2, and there is further a relationship of f0=[Sn] / [Si]<0.6, and when Bi is contained, there is a relationship of 0.004≦f2=[Pb]+[Bi]<0.10, and In the constituent phases of the metal structure excluding nonmetallic inclusions, if the area ratio of the α phase is (α)%, the area ratio of the γ phase is (γ)%, and the area ratio of the β1 phase, which is a modified β phase, is (β1)%, then 30≦f3=(α)≦70, 30≦f4=(β1)≦70, 0≦f5=(γ)<1, 35<f6=(β1)×([Si]) 1/2 -(γ)×2+([Pb]+[Bi]) 1/2 ×20+([P]) 1/2 ×15, and the β1 phase has grain boundaries that can be observed when etched with a mixed solution of hydrogen peroxide and aqueous ammonia.
5. The free-cutting copper alloy according to any one of claims 1 to 4, characterized in that it is used for appliances and parts relating to drinking water and sanitation facilities, valves, cocks, industrial piping parts, water meters, musical instruments, automobile parts, electric and electronic equipment parts, machine parts, stationery, toys, sliding parts, instrument parts, precision machine parts, and medical parts.
6. A method for producing a free-cutting copper alloy according to any one of claims 1 to 4, comprising one or more hot working steps, wherein the hot working temperature in the final hot working step is greater than 540°C and less than 750°C, and during the cooling process after the hot working, the cooling treatment of the hot-worked material is started at a temperature lower than 670°C and higher than 500°C, and during the cooling treatment, the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C exceeds 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C exceeds 300°C / min.
7. A method for producing a free-cutting copper alloy according to any one of claims 1 to 4, comprising one or more hot working steps and heat treatment steps, wherein in the final heat treatment step, the alloy is annealed at a temperature above 520°C and below 630°C for 1 minute to 5 hours, and after annealing, a cooling treatment is started at a temperature above 500°C, the average cooling rate in the temperature range from the cooling treatment start temperature to 500°C exceeds 300°C / min, and the average cooling rate in the temperature range from 500°C to 300°C exceeds 300°C / min.
Citation Information
Patent Citations
Lead-free free cutting brass excellent in dezincification corrosion resistance and its production method
JP2002003967A
Lead-free free-cutting silicon brass alloy
JP2010133006A
Brass excellent in corrosion resistance
JP2018048398A
Lead-free, free-cutting brass alloy with excellent castability, its manufacturing method, and its uses
JP2019508584A
Free-cutting copper alloy and method for producing free-cutting copper alloy
JP2021042459A