LTCC substrate having low coefficient of thermal expansion, and space transformer using same

The LTCC substrate with a low thermal expansion coefficient and high strength is achieved by using a specific ceramic composition and firing process, addressing the reliability and mechanical strength issues in semiconductor device testing, allowing for efficient and reliable testing across various temperatures.

WO2024228525A1PCT designated stage expired Publication Date: 2024-11-07SEMCNS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005751
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-25
Filing Date
2024-04-29
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Low-temperature co-fired ceramic (LTCC) substrates used in space transformers for semiconductor device testing have high thermal expansion coefficients, leading to reliability issues and reduced mechanical strength during temperature changes, hindering high-speed and reliable testing across various temperature ranges.

Method used

A ceramic substrate composition incorporating cordierite, alumina, and other fillers with varying densities and thermal expansion properties, combined with a glass matrix, is used to create an LTCC substrate with a low thermal expansion coefficient and high strength, achieved through specific filler ratios and firing processes.

Benefits of technology

The resulting LTCC substrate exhibits a low thermal expansion coefficient of 4.0 ppm/°C and high bending strength of 200 MPa, enabling high-reliability and high-speed testing of semiconductor devices across different temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005751_07112024_PF_FP_ABST
    Figure KR2024005751_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an LTCC ceramic substrate, a substrate for a space transformer (STF) including same, and a probe card. The LTCC ceramic substrate contains cordierite (Mg2Al4Si5O18) and alumina (Al2O3), and in an X-ray diffraction analysis irradiating Cu Kα, the ratio I2 / I1 of peak I2 derived from the cordierite to peak I1 derived from the alumina may be at least about 0.14 or at least about 0.15.
Need to check novelty before this filing date? Find Prior Art

Description

LTCC substrate with low thermal expansion coefficient and space converter using the same

[0001] The present invention relates to a ceramic structure, and more particularly, to a low-temperature co-fired ceramic substrate having a low coefficient of thermal expansion (Low CTE) and a space converter using the same.

[0002] Typically, probe cards are used to inspect electrical defects in wafers formed with multiple semiconductor devices, such as memory. These probe cards have a composite ceramic substrate called a space transformer (STF), which acts as an interposer between a plurality of probes and a printed circuit board connected to a test device.

[0003] In the electrical defect inspection using the above space transformer (STF), the probe card is electrically connected to the tester, and at the same time, a plurality of probes are brought into contact with the connection terminals of the semiconductor element (hereinafter referred to as Device Under Test (DUT)). Then, by inputting and outputting power and various signals necessary for testing between the tester and the semiconductor element, it is possible to determine defects or errors such as open or short circuits in the semiconductor element.

[0004] Recently, to increase the throughput of electrical inspection of semiconductor devices, there has been a growing demand for simultaneous inspection of multiple semiconductor devices at the wafer level. Such inspections may involve burn-in testing at high temperatures and cold testing at low temperatures, as well as room temperature, during which the space transducer also experiences corresponding contraction and expansion.

[0005] Recently, with the trend toward larger wafer diameters and higher integration of semiconductor devices, the diameter of space transformers is increasing, and the spacing between probes is also decreasing. Typically, low-temperature co-fired ceramic (LTCC) substrates are used as substrates for space transformers (STFs), as they allow for low-resistance metal wiring such as copper and silver to accommodate the miniaturization of semiconductor devices. However, typical LTCC substrates have relatively low strength compared to high-temperature co-fired ceramic (HTCC) substrates and a relatively high coefficient of thermal expansion compared to silicon wafers. Therefore, various problems may arise when LTCC substrates are applied to STFs. For example, as the spacing between the electrode pads of semiconductor devices decreases, the large coefficient of thermal expansion of LTCC substrates compared to silicon wafers may deteriorate the contact reliability between the probe pins and the electrode pads of semiconductor devices during defect inspections such as burn-in tests or cold tests of semiconductor devices. Furthermore, if the space transducer has a higher coefficient of thermal expansion than the silicon wafer during burn-in or cold testing, it takes time for the temperature of the space transducer to stabilize for accurate testing, hindering increased test throughput. Furthermore, thermal deformation of the LTCC substrate due to repeated temperature changes can degrade its mechanical strength and lifespan.

[0006] Therefore, to enable high-speed testing with high reliability across a wide range of temperatures and repeated thermal deformation cycles, technologies that can enhance the physical properties of LTCC substrates by improving their coefficient of thermal expansion are required. In particular, reducing the coefficient of thermal expansion of LTCC substrates typically results in reduced strength, making it crucial to simultaneously ensure a low coefficient of thermal expansion while maintaining strength.

[0007] The technical problem to be achieved by the present invention is to provide a low thermal expansion coefficient ceramic substrate having low thermal expansion characteristics and high strength, and a space converter including the same.

[0008] The problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the description below.

[0009] According to one embodiment of the present invention, cordierite (Mg2Al4Si5O 18 ) and alumina (Al2O3), and in X-ray diffraction analysis by Cu Kα irradiation, a ratio I2 / I1 of the peak I2 derived from the cordierite to the peak I1 derived from the alumina is about 0.14 or more or about 0.15 or more.

[0010] The above ceramic substrate may further include anorthite and gahnite.

[0011] The ceramic substrate may include a matrix including a glass component, a plurality of first fillers in the shape of particles dispersed within the matrix, and a plurality of second fillers in the shape of particles, wherein the first fillers may have a higher strength than the second fillers, and the second fillers may have a lower coefficient of thermal expansion than the first fillers.

[0012] The first filler may include at least one of alumina, mullite, and diopside.

[0013] The second filler may include at least one of cordierite, fused silica, willemite, eucryptite, zirconia, and celsian.

[0014] According to another embodiment of the present invention, an LTCC (low temperature co-fired ceramic) substrate for a space transformer (STF) is provided, comprising a fired ceramic sheet, the fired ceramic sheet comprising: a matrix layer comprising a crystalline material and a glass material; a first particulate filler dispersed within the matrix layer; and a second particulate filler dispersed within the matrix layer, wherein the first filler has a higher strength than the second filler, and the second filler has a lower coefficient of thermal expansion than the first filler.

[0015] The above ceramic sheet is made of cordierite (Mg2Al4Si5O 18 ) and alumina (Al2O3), and in X-ray diffraction analysis by Cu Kα irradiation, the ratio I2 / I1 of the peak I2 derived from the cordierite to the peak I1 derived from the alumina may be about 0.14 or more or about 0.15 or more.

[0016] The first filler may include at least one of alumina, mullite, and diopside.

[0017] The second filler may include at least one of cordierite, fused silica, willemite, eucryptite, zirconia, and celsian.

[0018] The above crystalline material may further include anorthite and gahnite.

[0019] According to another embodiment of the present invention, a probe card including an STF (space transformer) using the above-described LTCC substrate is provided.

[0020] According to embodiments of the present invention, an LTCC substrate having a low expansion coefficient and high strength is provided.

[0021] In addition, when the LTCC substrate according to the embodiment of the present invention is used as a space transformer (STF), a probe card having high strength and high reliability can be manufactured.

[0022] FIG. 1 is a drawing for explaining the composition of slurry for manufacturing LTCC (low temperature co-fired ceramic) ceramic for STF (space transformer) according to one embodiment of the present invention.

[0023] Figure 2 is a schematic diagram illustrating a firing process of a ceramic sheet according to one embodiment of the present invention.

[0024] FIG. 3 is a schematic diagram for explaining the firing process of a green sheet in a method for manufacturing LTCC ceramics according to one embodiment of the present invention.

[0025] Figure 4 is a SEM (scanning electron microscope) photographic image showing the microstructure of the LTCC ceramic corresponding to Example 3 of Table 2.

[0026] Figure 5 is an SEM photograph image showing the microstructure of the LTCC ceramic corresponding to Example 7 of Table 2.

[0027] Figure 6 is an SEM photograph image showing the microstructure of the LTCC ceramic corresponding to Example 5 of Table 2.

[0028] Figure 7 is an SEM photograph image showing the microstructure of the LTCC ceramic corresponding to Example 10 of Table 2.

[0029] FIG. 8 is a graph showing the ratio of peak I2 derived from a cordierite crystal phase to peak I1 derived from an alumina crystal phase of LTCC ceramics according to embodiments of the present invention (i.e., I2 / I1) and the flexural strength and coefficient of thermal expansion (CTE).

[0030] Figure 9 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention.

[0031] Figure 10 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention.

[0032] Fig. 11 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention.

[0033] Fig. 12 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention.

[0034] Fig. 13 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention.

[0035] Fig. 14 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention.

[0036] FIG. 15 is a cross-sectional view exemplarily showing a laminated substrate structure for manufacturing an LTCC substrate according to one embodiment of the present invention.

[0037] FIG. 16 is a cross-sectional view exemplarily showing a laminated substrate structure for manufacturing an LTCC substrate according to another embodiment of the present invention.

[0038] FIG. 17 is a cross-sectional view exemplarily showing an STF (space transformer) manufactured according to one embodiment of the present invention.

[0039] FIG. 18 is a cross-sectional view exemplarily showing a probe card including an STF manufactured according to one embodiment of the present invention.

[0040] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings.

[0041] The embodiments of the present invention described below are provided to more clearly explain the present invention to a person having ordinary skill in the art, and the scope of the present invention is not limited by the following embodiments, and the following embodiments can be modified in various other forms.

[0042] The terminology used herein is used to describe particular embodiments and is not intended to limit the present invention. The singular forms used herein may include the plural forms unless the context clearly dictates otherwise. In addition, the terms "comprise" and / or "comprising" used herein specify the presence of a stated feature, step, number, operation, element, element, and / or group thereof, but do not exclude the presence or addition of one or more other features, steps, numbers, operations, elements, elements, and / or groups thereof. In addition, the term "connected" used herein not only means that certain elements are directly connected, but also includes a concept that indirectly connects elements by interposing another element between them.

[0043] In addition, when it is said in this specification that a certain element is located "on" another element, this includes not only cases where a certain element is in contact with another element, but also cases where another element exists between the two elements. The term "and / or" as used in this specification includes any one of the listed items and any and all combinations of one or more of them. In addition, terms of degree such as "about", "substantially", etc. as used in this specification are used to mean a range of or close to the numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly using the disclosure that mentions exact or absolute numbers provided to help the understanding of this specification.

[0044] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. The sizes and thicknesses of areas or parts illustrated in the attached drawings may be somewhat exaggerated for clarity and convenience of explanation. Like reference numbers designate like components throughout the detailed description.

[0045] FIG. 1 is a drawing for explaining the composition of slurry for manufacturing an LTCC (low temperature co-fired ceramic) substrate for an STF (space transformer) according to one embodiment of the present invention.

[0046] Referring to FIG. 1, a slurry composition according to the present embodiment may be used to manufacture a green sheet (i.e., a micronized ceramic sheet) applied to manufacture an LTCC substrate for STF. The slurry composition may include a glass frit (10), a first filler (20) composed of a plurality of first particles having a particle shape, a second filler (30) composed of a plurality of second particles having a particle shape, a binder (40), and a solvent (50). The first filler (20) is a material for increasing the strength of a ceramic structure (or LTCC ceramic) obtained by firing the green sheet. The second filler (30) is a filler that serves to reduce the thermal expansion coefficient of the ceramic structure.

[0047] The glass frit (10) may have a material composition that can react with a part or all of the first filler (20) and a part of the second filler (30) during the sintering process of the green sheet to form (precipitate) a predetermined crystal phase. During this process, the glass frit (10) may be partially or completely consumed, and the remaining glass frit components together with the generated crystal phase constitute a matrix of the sintered LTCC ceramic structure. In one embodiment, the glass frit (10) may include a part or all of SiO2, Al2O3, MgO, CaO, SrO, BaO, B2O3, ZnO, Na2O, and K2O. These glass flits (10) can form a cordierite series crystal phase, anorthite series crystal phase, or gahnite series crystal phase through a firing process.

[0048] The above cordierite (Mg2Al2Si5O) 18) series crystal phase, the glass frit (10) may include SiO2, Al2O3, MgO, and other components. In order to form the anorthite series crystal phase, the glass frit (10) may include CaO, Al2O3, and SiO2 components. In order to form the gahnite series crystal phase, the glass frit (10) may include ZnO and Al2O3. In order to form each crystal phase of the cordierite, anorthite, and gahnite series, the glass frit may be consumed in the reaction of the sintering process, and the remainder may remain as a glass component constituting the matrix of the fired LTCC ceramic. For example, SrO, BaO, B2O3, Na2O, and K2O constituting the glass frit (10) may remain as a glass component in the fired LTCC ceramic structure. These crystal phases and glass components can play a role in improving the sintering properties (i.e., low-temperature sintering properties) and enhancing the strength of the green sheet manufactured therefrom.

[0049] As described above, the first filler (20) may react with part or all of the glass flit (10) during the firing process to increase the strength of the LTCC ceramic. In this regard, the first filler (20) may have higher strength (physical strength) than the second filler (30). The first filler (20) may be composed of a plurality of first particles. The first particles may have a diameter of, for example, about 0.2 μm to 5 μm. The first particles may include, for example, at least one of alumina (Al2O3), mullite (3Al2O3 ·2SiO2), and diopside (Ca(Mg,Fe)Si2O6). However, the specific material of the first filler (20) disclosed herein is exemplary, and other materials may also be applied.

[0050] The second filler (30) may partially react with the glass flit (10) and / or the first filler (20) during the firing process and may remain in the LTCC ceramic to lower the coefficient of thermal expansion (CTE) of the LTCC ceramic. In this regard, the second filler (30) may have a lower coefficient of thermal expansion (CTE) than the first filler (20). The second filler (30) may include, for example, at least one of cordierite, fused silica, willemite (ZnSiO4), eucryptite (LiAlSiO4), zirconia (ZrO2), and celsian (BaAl2Si2O8). In another embodiment, the second filler (30) may include zirconium tungstate; ZrW2O8), or wollastonite (CaSiO3) may be further included. The second filler (30) may have an average larger diameter than the first filler (20), for example, may have a diameter of about 0.5 μm to 10 μm. Since the second filler (30) has a larger diameter than the first filler (20), it can be consumed during firing within the LTCC ceramic but still remain in sufficient quantity to accommodate thermal deformation according to temperature change of the matrix, thereby effectively reducing the thermal expansion coefficient of the LTCC ceramic.

[0051] Referring back to FIG. 1, in the slurry composition, the ratio of the combined weight of the first filler (20) and the second filler (30) to the glass frit (10), i.e., the ratio of the combined weight of the fillers to the weight of the glass frit (10), may be in the range of 30 wt% to 70 wt%, and preferably in the range of 40 wt% to 60 wt%. In one embodiment, in the slurry composition, the weight ratio of the second filler (30) to the weight of the first filler (20) may be in the range of 20 wt% to 80 wt%, and preferably in the range of 30 wt% to 65 wt%. The content of the second filler (30) may be controlled so that only a portion reacts with the glass frit (10) and the first filler (20) during the firing process and a significant portion remains. In the case of the first filler (20), since it can play a role in generating a crystal phase by reacting with the glass frit (10) during the firing process, the amount of the first filler (20) added can be intentionally increased when manufacturing the slurry, taking into account the amount consumed for generating the crystal phase. A portion of the first filler (20) is consumed for generating the crystal phase, and the remaining portion of the first filler (20) can play a role in increasing the strength of the LTCC substrate.

[0052] The binder (40) may include, for example, at least one of acryl, epoxy, polyvinyl butyral (PVB), and ethyl cellulose (EC). The solvent (50) may include, for example, at least one of methanol, ethanol, isopropanol, methyl ethyl ketone, toluene, acetone, and diethyl ether. The content of the binder (40) in the entire slurry composition may be, for example, about 6 wt% to 15 wt%, and the content of the solvent (50) may be, for example, about 20 wt% to 40 wt%. In addition, the slurry composition may further include a dispersant or other additives.

[0053] Using the slurry composition according to the embodiment described above, a green sheet, i.e., an unsintered sheet, can be formed from the slurry composition. In one embodiment, the slurry composition can be cast by a method such as tape casting, to form the green sheet. A wiring pattern can be formed on the surface of the green sheet, a via hole can be formed in the thickness direction of the green sheet, and a conductive material can be filled in the via hole to form a via conductor electrically connected to the wiring pattern. The wiring pattern and the via conductor can be a low-resistance metal such as, but not limited to, copper, silver, or an alloy containing the same, and any metal for forming a known LTCC substrate can be used.

[0054] Next, a plurality of green sheets may be laminated to form a laminated structure, and the laminated structure may be fired to form an LTCC ceramic or an LTCC substrate therefrom. The laminated structure may include a wiring pattern formed on its surface and inside. The wiring pattern may be a low-resistance metal, metal alloy, or compound having a low melting point as described above, and thus the firing may be a low-temperature firing performed at a temperature of about 1,000°C or lower. For example, the firing temperature may be about 600°C to 1,000°C. The LTCC substrate manufactured in this manner may be applied to the manufacture of an STF (space transformer) device through an additional subsequent process.

[0055] In the step of forming the LTCC substrate by firing the above-described laminated structure, a portion of the glass frit (10) and the first filler (20) and the second filler (30) react to form a predetermined crystalline material to constitute the matrix, and the remaining first filler (20) and the newly formed crystalline material serve to increase the strength of the LTCC substrate, and the remaining second filler (30) serves to reduce the thermal expansion coefficient of the LTCC substrate. In one embodiment, the crystalline material may be a cordierite crystal phase, anorthite crystal phase, or gahnite crystal phase. In some embodiments, the crystalline material may further include a eucryptite crystal phase.

[0056] Fig. 2 is a schematic diagram illustrating a firing process of a ceramic sheet according to an embodiment of the present invention. Fig. 2 shows the composition of an LTCC ceramic obtained after a heat treatment of a non-sintered ceramic sheet (green sheet) obtained from a slurry composition according to an embodiment of the present invention described with reference to Fig. 1.

[0057] Referring to FIG. 2, a green sheet according to an embodiment of the present invention may have a structure in which a first filler (F10) composed of a plurality of first particles and a second filler (F20) composed of a plurality of second particles are dispersed within a matrix layer (M10). Here, the matrix layer (M10) may include glass frit as a main component and may further include some other materials such as a binder. The glass frit may correspond to the glass frit (10) described with reference to FIG. 1. The first filler (F10) and the second filler (F20) may correspond to the first filler (20) and the second filler (30) described with reference to FIG. 1, respectively.

[0058] When the microporous ceramic sheet (green sheet) is fired, a part of the glass frit (M10) and a part or all of the first filler (F10), and a part of the glass frit (M10) and a part of the second filler (F10) may react to precipitate a crystalline material (F30) within the matrix. In the glass frit (M10), the remainder that did not participate in the reaction during the firing may remain as a glass material. In addition, the remainder of the first filler (F10) that did not participate in the reaction during the firing may also remain. Meanwhile, the second filler (F20) may react with the glass frit and the first filler (F10) during the firing process, or a part of it may remain, or may not react with the glass frit and the first filler (F10) and not be consumed. In this case, the second filler (F20) may remain almost or substantially in its state before the firing.

[0059] Therefore, referring to the drawing after firing on the right side in FIG. 2, the LTCC ceramic after firing may have a structure in which a first filler (F10) composed of a plurality of first particles and a second filler (F20) composed of a plurality of second particles are dispersed within the matrix layer (M10'). Here, the matrix layer (M10') may react with the first filler (F10) or the second filler (F20) to be completely consumed, or a portion thereof may react and remain. In addition, the glass phase forming the glass frit (M10) before sintering and the matrix layer (M10') after sintering may be the same or different. The crystalline material (F30) generated after sintering is a main constituent material, for example, cordierite (Mg2Al4Si5O 18), Anorthite, Gahnite, willemite (ZnSiO4), Eucryptite (LiAlSiO4), Celsian (BaAl2Si2O8), Wollastonite (CaSiO3), and zinc aluminate (ZnAl2O4) crystal phases.

[0060] The total amount of the first filler (F10) may be less than the total amount of the first filler (F10) of the green sheet before firing. This may be because a portion of the first filler (F10) is consumed to form the above-mentioned crystalline material. In this regard, the number of particles constituting the first filler (F10) may decrease or the volume (diameter) of the particles may decrease. Meanwhile, the second filler (F20) may also be consumed to some extent, but conversely, the state before firing may be maintained almost the same or substantially the same.

[0061] After the firing, the content of the first filler (F10) relative to the total amount of the crystalline material (F30), the glass material, the first filler (F10), and the second filler (F20) in the LTCC ceramic may be about 10 wt% to 40 wt%. Meanwhile, the content of the second filler (F20) relative to the total amount of the crystalline material, the glass material, the first filler (F10), and the second filler (F20) in the LTCC ceramic may be about 5 wt% to 30 wt%. The material composition of the first filler (F10) and the second filler (F20) is the same as that described with reference to FIG. 1, and a repeated description thereof will be omitted.

[0062] Through firing, a portion of the first filler (20) is consumed in the formation of the above-described crystal phase, and the remaining portion of the first filler (20) can serve to increase the strength of the LTCC ceramic. In addition, the second filler (30) dispersed within the matrix (M10') is a low-expansion material that can accommodate thermal deformation according to temperature changes of the LTCC ceramic after firing, thereby securing a low coefficient of thermal expansion. Accordingly, the LTCC ceramic according to the embodiment of the present invention can obtain a high strength of about 200 MPa while having a low coefficient of thermal expansion, for example, a coefficient of thermal expansion of 4.0 ppm / ℃. Such LTCC ceramics have high strength when applied to LTCC substrates and, further, space transformers, and have a low coefficient of thermal expansion, thereby enabling high-reliability, high-speed, and high-efficiency testing in the evaluation of semiconductor devices performed in various temperature ranges.

[0063] Fig. 3a shows the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention, and Fig. 3b shows the results of X-ray diffraction analysis of LTCC ceramics according to a comparative example. The X-ray analysis was performed on a cross-section of the LTCC ceramic using Cu Kα rays as a light source. The range of the diffraction angle 2θ was 5° to 90°, and the scan speed was 0.0065° / step. The X-axis values ​​in Figs. 3a and 3b represent 2θ (degree).

[0064] Referring to FIG. 3a, in the analysis of the LTCC ceramic after firing, a sample having a strength of 200 MPa or more and a coefficient of thermal expansion of 4.0 ppm / ℃ or less may have a ratio of a peak I2 derived from a cordierite crystal phase to a peak I1 derived from an alumina crystal phase, i.e., I2 / I1, of about 0.14 or more or about 0.15 or more. In addition, the I2 / I1 may be, for example, less than about 1. Preferably, the I2 / I1 may be about 0.6 or less or about 0.5 or less. The alumina crystal phase is derived from the first filler (F10 in FIG. 2), and the cordierite crystal phase is derived from the matrix (M10) and the second filler (F20). Furthermore, a low coefficient of thermal expansion can be obtained when the ratio of peak I3 derived from the anosite crystal phase to peak I1 derived from the alumina crystal phase, i.e., I3 / I1, is about 1.9 or more or 2.0 or more. Meanwhile, the ratio of peak I4 derived from the zinc aluminate crystal phase to peak I1 derived from the alumina crystal phase, i.e., I4 / I1, can be about 1.5 or less, about 1.2 or less, or about 1 or less. A low coefficient of thermal expansion can be obtained when the I4 / I1 is about 1.5 or less, about 1.2 or less, or about 1 or less.

[0065] In contrast, referring to Fig. 3b, when the ratio I2 / I1 is less than 0.1, the thermal expansion coefficient is as high as 4.3 or more. This means that a portion of the glass frit (M10) and a portion or most of the second filler (F20) reacted and were almost consumed, and in this case, it was found that there was no effect of reducing the thermal expansion coefficient along with the strength.

[0066] Table 1 shows the analysis values ​​of strength, coefficient of thermal expansion, and peak ratio of examples and comparative examples of the present invention.

[0067] Sample StrengthCoefficient of Thermal ExpansionI2 / I1I3 / I1I4 / I1Example 12004.00.181.980.27Comparative Example 12304.501.350.25Comparative Example 22104.30.061.620.21Comparative Example 32504.70.11.20.25

[0068] Referring to Table 1, securing high strength and low thermal expansion coefficient of LTCC ceramic materials after firing can be achieved by analyzing the above ratio I2 / I1 without complex analysis, and optionally I3 / I1 and By additionally checking I4 / I1, LTCC ceramics with high strength while having a low coefficient of thermal expansion can be detected, and manufacturing processes can be designed targeting products with the above XRD intensity ratio. Table 2 below summarizes the results of X-ray diffraction analysis and property evaluation of LTCC ceramics according to embodiments of the present invention.

[0069]

[0070] Referring to Table 2 above, in the analysis of the LTCC ceramic after firing, the ratio of the peak I2 derived from the cordierite crystal phase to the peak I1 derived from the alumina crystal phase, i.e., I2 / I1, may be about 0.14 or more or about 0.15 or more. In addition, the I2 / I1 may be, for example, less than about 1. Preferably, the I2 / I1 may be about 0.6 or less or about 0.5 or less. The alumina crystal phase may be derived from the first filler (F10 in FIG. 2), and the cordierite crystal phase may be derived from the matrix (M10) and the second filler (F20). The ratio of the peak I3 derived from the anorthite crystal phase to the peak I1 derived from the alumina crystal phase, i.e., I3 / I1, may be about 1.9 or more or 2.0 or more. The above I3 / I1 may be, for non-limiting examples, about 5 or less or about 4 or less. When the I3 / I1 is about 1.9 or more or 2.0 or more, it may be advantageous to obtain a low coefficient of thermal expansion. Meanwhile, the ratio of the peak I4 derived from the zinc aluminate crystal phase to the peak I1 derived from the alumina crystal phase, i.e., I4 / I1, may be about 1.5 or less or about 1.2 or less or about 1 or less. When the I4 / I1 is about 1.5 or less or about 1.2 or less or about 1 or less, it may be advantageous to obtain a low coefficient of thermal expansion.

[0071] In the above Table 2, Al2O3① corresponds to one of the two Main 2θs of Al2O3 (corresponding to 35.1 degree), and Al2O3② corresponds to the other of the two Main 2θs of Al2O3 (corresponding to 43.3 degree). The peak intensity of the alumina crystal phase used in the above I2 / I1, I3 / I1, and I4 / I1 may be the peak intensity of Al2O3②. Meanwhile, ZnAl2O4 may be gahnite.

[0072] In addition, as shown in Table 2, the LTCC ceramic (LTCC ceramic substrate) according to the embodiment of the present invention can have a high flexural strength (bending strength) of about 180 MPa or more or about 200 MPa or more while having a low coefficient of thermal expansion of about 4.0 ppm / ℃ or less. Here, the measurement of the flexural strength (bending strength) was performed under three-point bending strength conditions using a UTM (Universal Testing Machine) device.

[0073] Figure 4 is a SEM (scanning electron microscope) photographic image showing the microstructure of the LTCC ceramic corresponding to Example 3 of Table 2.

[0074] Figure 5 is an SEM photograph image showing the microstructure of the LTCC ceramic corresponding to Example 7 of Table 2.

[0075] Figure 6 is an SEM photograph image showing the microstructure of the LTCC ceramic corresponding to Example 5 of Table 2.

[0076] Figure 7 is an SEM photograph image showing the microstructure of the LTCC ceramic corresponding to Example 10 of Table 2.

[0077] FIG. 8 is a graph showing the ratio of peak I2 derived from a cordierite crystal phase to peak I1 derived from an alumina crystal phase of LTCC ceramics according to embodiments of the present invention (i.e., I2 / I1) and the flexural strength and coefficient of thermal expansion (CTE).

[0078] Referring to Fig. 8, the samples of Examples 3 and 10 are shrinkage type LTCCs, and the samples of Examples 7 and 5 are non-shrinkage type LTCCs. As I2 / I1 increases within a given range, the coefficient of thermal expansion (CTE) tends to decrease. All samples can have a low coefficient of thermal expansion of about 4.0 ppm / ℃ or less. In addition, all samples can have a high flexural strength of about 180 MPa or more.

[0079] Fig. 9 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention. Fig. 9 shows the results for Example 2 of Table 2.

[0080] Table 3 below is obtained from Fig. 9 and summarizes the 2θ and peak intensities of the crystal phases.

[0081]

[0082] Table 4 below summarizes the coefficient of thermal expansion (CTE), Er, and strength of anorthite, alumina (Al2O3), cordierite, and gahnite, respectively. Here, the unit of the coefficient of thermal expansion (CTE) is ppm / ℃, and the unit of strength is MPa. Meanwhile, Er represents the permittivity, and its unit is F / m.

[0083]

[0084] Fig. 10 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention. Fig. 10 shows the results for a sample corresponding to Example 5 of Table 2. At this time, EL was 80 μm. Here, the EL represents a ceramic sheet mixed with glass and cordierite.

[0085] Fig. 11 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention. Fig. 11 shows the results for a sample corresponding to Example 5 of Table 2. At this time, EL was 70 μm.

[0086] Fig. 12 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention. Fig. 12 shows the results for a sample corresponding to Example 7 of Table 2.

[0087] Fig. 13 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention. Fig. 13 shows the results for a sample corresponding to Example 3 of Table 2.

[0088] Fig. 14 is a graph showing the results of X-ray diffraction analysis of LTCC ceramics according to an embodiment of the present invention. Fig. 14 shows the results for a sample corresponding to Example 10 of Table 2.

[0089] FIG. 15 is a cross-sectional view exemplarily showing a laminated substrate structure for manufacturing an LTCC substrate according to one embodiment of the present invention.

[0090] Referring to FIG. 15, a laminated substrate structure for manufacturing an LTCC substrate according to the present embodiment may include a plurality of green sheets (micro-fired ceramic sheets) (101). The thickness of each green sheet (101) may be, for example, about 20 ㎛ to 200 ㎛. A plurality of via holes (VH) may be formed in the plurality of green sheets (101), and conductive plugs (103) may be formed in the via holes (VH). In addition, a conductive pattern layer (104) for electrically connecting the conductive plugs (103) may be formed between the plurality of green sheets (101). The arrangement of the via holes (VH) and the arrangement, shape, etc. of the conductive plugs (103) and the conductive pattern layer (104) are exemplary and may be varied in various ways.

[0091] After forming a via hole (VH) in the micronized green sheet as described in FIG. 2, a conductive plug (103) and a conductive pattern layer (104) can be formed, and a plurality of such micronized green sheets can be laminated to manufacture a laminated substrate structure as shown in FIG. 15. Accordingly, the material composition of the plurality of green sheets (101) in FIG. 15 can correspond to the material composition of the green sheet before firing in FIG. 2. By performing a firing process (low-temperature firing process) on the laminated substrate structure, an LTCC substrate can be manufactured.

[0092] According to another embodiment of the present invention, some of the plurality of ceramic sheets (101) may have a different material composition than the pre-sintering green sheet of FIG. 2.

[0093] FIG. 16 is a cross-sectional view exemplarily showing a laminated substrate structure for manufacturing an LTCC substrate according to another embodiment of the present invention.

[0094] Referring to FIG. 16, a laminated substrate structure for manufacturing an LTCC substrate according to the present embodiment may include a structure in which at least one green sheet (101) and at least one constraint sheet (102) are laminated. For example, at least one green sheet (101) and at least one constraint sheet (102) may be alternately and repeatedly laminated. A via hole (VH) may be formed in the ceramic sheet (101) and the constraint sheet (102), and a conductive plug (103) may be formed in the via hole (VH). In addition, a conductive pattern layer (104) for electrically connecting the conductive plugs (103) may be formed between the green sheet (101) and the constraint sheet (102). The arrangement of the via hole (VH) and the arrangement, shape, etc. of the conductive plug (103) and the conductive pattern layer (104) are exemplary and may be variously changed. In addition, the stacking order and arrangement method of the green sheet (101) and the restraint sheet (102) can be varied.

[0095] The material composition of the green sheet (101) may correspond to the material composition of the green sheet before firing described with reference to FIG. 2. The thickness of the green sheet (101) may be, for example, about 20 to 200 μm. Meanwhile, the restraint sheet (102) may play a role in suppressing / preventing or minimizing the firing shrinkage of the entire laminated substrate structure during the firing process. The restraint sheet (102) may have a higher firing temperature than the green sheet (101). In addition, the restraint sheet (102) may have a lower shrinkage rate than the green sheet (101) during the firing process. The restraint sheet (102) may be an unfired ceramic sheet having a different material composition from the green sheet (101). The restraint sheet (102) may have a very low glass content so as not to be fired (sintered) at the firing (sintering) temperature of the ceramic sheet (101). The restraint sheet (102) may include, for example, alumina (Al2O3) as a main component. Accordingly, the restraint sheet (102) may be an alumina-based ceramic sheet. In addition, the restraint sheet (102) may further include a ceramic filler and an organic binder. The restraint sheet (102) may have a thickness thinner than the ceramic sheet (101), but in some cases, may have a thickness similar to that of the ceramic sheet (101).

[0096] An LTCC substrate can be manufactured by performing a firing process (low-temperature firing process) on the laminated substrate structure illustrated in Fig. 16. During this firing process, the glass component of the green sheet (101) can penetrate (diffuse) into the interior of the restraining sheet (102), and interlayer bonding and sintering effects can be achieved through this penetration (diffusion) of the glass component. The restraining sheet (102) can play a role in achieving a shrinkage-free process of the laminated substrate structure during the firing process.

[0097] FIG. 17 is a cross-sectional view exemplarily showing an STF (space transformer) manufactured according to one embodiment of the present invention.

[0098] Referring to FIG. 17, an STF manufactured according to an embodiment of the present invention may include an LTCC substrate (LS10) and a wiring layer member (WL10) formed on an upper surface of the LTCC substrate (LS10). The LTCC substrate (LS10) may be manufactured according to the embodiment described with reference to FIGS. 1 to 16, etc. The wiring layer member (WL10) may be formed as a multilayer wiring layer by alternately and repeatedly stacking a metal wiring pattern layer and an organic insulating layer (interlayer insulating film) on an upper surface of the LTCC substrate (LS10). A conductive via structure may be formed in the organic insulating layer. The organic insulating layer may include, for example, polyimide (PI), but the material is not limited thereto.

[0099] A plurality of first electrode pads (PD10) may be formed on the wiring layer member (WL10). A plurality of micro probes are arranged on the plurality of first electrode pads (PD20). On the lower surface of the LTCC substrate (LS10), wiring is formed to achieve electrical connection with a printed circuit board for power and signal transmission to a tester, or connection with a pogo pin is made.

[0100] FIG. 18 is a cross-sectional view exemplarily showing a probe card including an STF manufactured according to one embodiment of the present invention.

[0101] Referring to FIG. 18, a probe card according to an embodiment of the present invention may include a printed circuit board (1) to which an electrical signal is applied from the outside, an STF (space transformer) (3) having a plurality of micro probes (2) that come into contact with connection pads of a test object (not shown) such as a semiconductor chip, and an interface member (4) that electrically connects the printed circuit board (1) and the STF (3) to each other. Here, the STF (3) may be an electronic circuit board that electrically connects a plurality of micro probes (2) each having a size of several tens of micrometers while performing pitch conversion in order to test the printed circuit board (1) and an ultra-highly integrated semiconductor device. Although not shown, the printed circuit board (1) may be connected to a predetermined tester device. The probe card may serve to connect numerous measurement points (wafer pads) existing on a wafer, which is a test object (not shown), to the tester device.

[0102] A method for manufacturing a probe card according to an embodiment of the present invention may include a step of manufacturing an LTCC substrate using the method described above, a step of manufacturing an STF including the LTCC substrate, and a step of manufacturing a probe card using the STF.

[0103] As described above, according to embodiments of the present invention, an LTCC substrate having high strength and low expansion (i.e., low thermal expansion) characteristics can be realized. Furthermore, by using an STF applying an LTCC substrate according to embodiments of the present invention, a probe card having high strength and high reliability can be manufactured.

[0104] In this specification, preferred embodiments of the present invention have been disclosed, and although specific terms have been used, they have been used in a general sense only to easily explain the technical contents of the present invention and to help the understanding of the invention, and are not intended to limit the scope of the present invention. It will be apparent to those skilled in the art that other modifications based on the technical idea of ​​the present invention can be implemented in addition to the embodiments disclosed herein. For example, those skilled in the art will recognize that the slurry composition for manufacturing an LTCC substrate, the method for manufacturing an LTCC substrate, the LTCC substrate, the probe card, and the method for manufacturing the probe card according to the embodiments described with reference to FIGS. 1 to 18 can be variously modified. Therefore, the scope of the invention should not be defined by the described embodiments, but should be defined by the technical idea described in the claims.

[0105] Embodiments of the present invention can be applied to ceramic structures and devices / devices including the same. Embodiments of the present invention can be applied to co-fired ceramic substrates and spatial converters and probe cards including the same.

Claims

1. Cordierite (Mg2Al4Si5O) 18 ) and alumina (Al2O3), A ceramic substrate in which, in X-ray diffraction analysis by Cu Kα irradiation, the ratio I2 / I1 of the peak I2 derived from the cordierite to the peak I1 derived from the alumina is 0.15 or more.

2. In paragraph 1, The above ceramic substrate is a ceramic substrate further comprising anorthite and gahnite.

3. In paragraph 1, The ceramic substrate comprises a matrix comprising a glass component, a plurality of first fillers in particle shape dispersed within the matrix, and a plurality of second fillers in particle shape, A ceramic substrate wherein the first filler has higher strength than the second filler, and the second filler has a lower coefficient of thermal expansion than the first filler.

4. In paragraph 3, The first filler is a ceramic substrate comprising at least one of alumina, mullite and diopside.

5. In paragraph 3, A ceramic substrate wherein the second filler comprises at least one of cordierite, fused silica, willemite, eucryptite, zirconia, and celsian.

6. As a LTCC (low temperature co-fired ceramic) substrate for STF (space transformer), Contains a fired ceramic sheet, The above fired ceramic sheet, A matrix layer comprising a crystalline material and a glass material; A first filler in the form of particles dispersed within the matrix layer; and comprising a second filler in the form of particles dispersed within the matrix layer; An LTCC substrate for STF, wherein the first filler has a higher strength than the second filler, and the second filler has a lower coefficient of thermal expansion than the first filler.

7. In paragraph 6, The above ceramic sheet is made of cordierite (Mg2Al4Si5O 18 ) and alumina (Al2O3), An LTCC substrate for STF, wherein the ratio I2 / I1 of the peak I2 derived from the cordierite to the peak I1 derived from the alumina in X-ray diffraction analysis by Cu Kα irradiation is 0.15 or more.

8. In paragraph 6, An LTCC substrate for STF, wherein the first filler comprises at least one of alumina, mullite, and diopside.

9. In paragraph 6, An LTCC substrate for STF, wherein the second filler comprises at least one of cordierite, fused silica, willemite, eucryptite, zirconia, and celsian.

10. In paragraph 6, The above crystalline material is an LTCC substrate for STF further comprising anorthite and gahnite.

11. A probe card including an STF (space transformer) using the LTCC substrate described in any one of claims 6 to 10.

Citation Information

Patent Citations

  • Cordierite porous sintered compact, and ceramic filter obtained by using the same

    JP2004203724A

  • Ceramic honeycomb structure and process for producing same

    KR1020120022845A

  • Sintering aid glasses for machinable phyllosilicate based structures

    KR1020180102195A

  • The available multi-purpose mats

    KR1020240067552A

  • Process for making cordierite glass-ceramic having nucleating agent and increased percent cordierite crystallinity

    US3940255A