Self-supporting separator for electrochemical device, and electrochemical device comprising same
The self-supporting separator with controlled inorganic particle content and surface roughness addresses thermal shrinkage issues in electrochemical devices, enhancing compression and heat resistance to improve energy density and lifespan.
Patent Information
- Application Number
- PCT/KR2024/005914
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-30
- Filing Date
- 2024-05-02
- Publication Date
- 2024-11-07
AI Technical Summary
Conventional electrochemical device separators, particularly those with polyolefin substrates, suffer from reduced energy density and lifespan due to thermal shrinkage causing electrical short circuits and heat generation, necessitating improved compression resistance and heat resistance.
A self-supporting separator with a high content of inorganic particles (70 parts by weight or more) and a polymer binder, featuring a surface roughness of 600 nm to 1100 nm and an average particle diameter of 40 nm to 300 nm, which enhances compression resistance and heat resistance without a porous polymer substrate, allowing for improved energy density and lifespan.
The solution significantly improves compression resistance and heat resistance, preventing electrical short circuits and maintaining performance over multiple cycles, thereby enhancing the energy density and lifespan of electrochemical devices.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Self-supporting separator for electrochemical devices and electrochemical devices including the same
[0001] This invention claims the benefit of Korean Patent Application No. 10-2023-0058001, filed on May 3, 2023, and Korean Patent Application No. 10-2024-0057294, filed on April 30, 2024, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a self-supporting separator for an electrochemical device and an electrochemical device including the same, and more particularly, to a self-supporting separator for an electrochemical device having an anode including a silicon-based active material, wherein the surface roughness (Sa) of the separator is controlled by controlling the content and average particle diameter of inorganic particles, thereby improving compression resistance, increasing energy density, and exhibiting high electrochemical device life characteristics, and to an electrochemical device including the same.
[0003] Among the components of electrochemical devices, the separator comprises a porous polymer substrate located between the anode and cathode. It isolates the anode and cathode, prevents electrical short-circuiting between the two electrodes, and allows the passage of electrolytes and ions. While the separator itself does not participate in electrochemical reactions, its physical properties, such as wettability with electrolyte, degree of porosity, and thermal shrinkage, influence the performance and safety of the electrochemical device.
[0004] Accordingly, various methods have been attempted to enhance the physical properties of membranes by adding a coating layer to a porous polymer substrate and by adding various substances to the coating layer to change the properties of the coating layer. For example, inorganic substances may be added to the coating layer to enhance the mechanical strength of the membrane, or inorganic substances or hydrates may be added to the coating layer to enhance the flame retardancy and heat resistance of the polymer substrate.
[0005] The separator can be bonded to the electrode through a lamination process, and a polymer binder can be added to the coating layer composition of the separator to secure adhesion between the electrode and the separator.
[0006] Meanwhile, polyolefin resins, which are widely used as porous polymer substrates for electrochemical devices, have a problem in that they shrink when exposed to high temperatures, causing the positive and negative electrodes to come into contact, resulting in an electrical short circuit between the two electrodes, and causing heat generation, which in turn causes thermal runaway due to a decomposition reaction of the electrolyte and active material.
[0007] Therefore, research on self-supporting membranes that can improve the energy density and lifespan characteristics of electrochemical devices was needed.
[0008] The technical problem to be achieved by the present invention is to provide a self-supporting separator for an electrochemical device having a cathode including a silicon-based active material, wherein the surface roughness (Sa) of the separator is controlled by controlling the content of inorganic particles, thereby improving the compression resistance and improving the energy density and lifespan characteristics of the electrochemical device, and an electrochemical device including the same.
[0009] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.
[0010] One embodiment of the present invention provides a self-supporting separator for an electrochemical device having a negative electrode including a silicon-based active material, the self-supporting separator including inorganic particles and a polymer binder provided on part or all of the surface of the inorganic particles, and including pores, the content of the inorganic particles being 70 parts by weight or more with respect to 100 parts by weight of the separator, and the surface roughness (Sa) of the separator being 600 nm or more and 1100 nm or less.
[0011] According to one embodiment of the present invention, the inorganic particles may have an average particle diameter (D50) of 40 nm or more and 300 nm or less.
[0012] According to one embodiment of the present invention, the content of the silicon-based active material in the negative electrode may be 50 wt% or more.
[0013] According to one embodiment of the present invention, the hardness of the cathode may be 50 MPa or more and 350 MPa or less.
[0014] According to one embodiment of the present invention, the content of the polymer binder may be 30 parts by weight or less with respect to 100 parts by weight of the separator.
[0015] According to one embodiment of the present invention, the polymer binder may be an acrylic binder, a polyvinylidene binder, or a combination thereof.
[0016] According to one embodiment of the present invention, the thickness of the separation membrane may be 10 ㎛ or more and 30 ㎛ or less.
[0017] According to one embodiment of the present invention, the change rate of air permeability of the separation membrane according to the following mathematical formula 1 may be 10% or less.
[0018] [Mathematical Formula 1]
[0019] Change in air permeability (%) = {(air permeability of the membrane after pressure application - air permeability of the membrane before pressure application) / air permeability of the membrane before pressure application} X 100
[0020] One embodiment of the present invention provides an electrochemical device comprising: a positive electrode; a negative electrode including a silicon-based active material; and a separator interposed between the positive electrode and the negative electrode including the silicon-based active material.
[0021] According to one embodiment of the present invention, the operating voltage range of the electrochemical device may be 2.5 V to 4.2 V.
[0022] A self-supporting separator for an electrochemical device according to one embodiment of the present invention can have improved compression resistance.
[0023] An electrochemical device including a self-supporting separator for an electrochemical device according to one embodiment of the present invention can improve energy density and life characteristics by utilizing a lower limit voltage.
[0024] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0025] In this specification, “A and / or B” means “A and B, or A or B.”
[0026] In this specification, when it is said that a component is “provided on”, this does not exclude other components being placed in between, unless otherwise specifically stated, and it means that other components may be further placed.
[0027] In this specification, the characteristic of “having pores” means that the object includes a plurality of pores and that the pores are interconnected with each other, thereby allowing gaseous and / or liquid fluids to pass from one side of the object to the other side.
[0028] In this specification, the separator has a porous characteristic including a large number of pores, and acts as a porous ion-conducting barrier that allows ions to pass while blocking electrical contact between the cathode and the anode in an electrochemical device.
[0029] In this specification, “self-supporting separator for electrochemical devices” means a separator for electrochemical devices that includes inorganic particles and a polymer binder but does not have a porous polymer substrate.
[0030] Hereinafter, the present invention will be described in more detail.
[0031]
[0032] One embodiment of the present invention provides a self-supporting separator for an electrochemical device including a negative electrode including a silicon-based active material, the self-supporting separator including inorganic particles and a polymer binder provided on part or all of the surface of the inorganic particles, the self-supporting separator including pores, the content of the inorganic particles being 70 parts by weight or more based on 100 parts by weight of the separator, and the surface roughness (Sa) of the separator being 600 nm or more and 1100 nm or less.
[0033] A self-supporting separator for an electrochemical device according to one embodiment of the present invention can have improved compression resistance. In addition, when the separator for an electrochemical device according to one embodiment of the present invention is applied to an electrochemical device including an anode comprising a silicon-based active material, the energy density and life characteristics of the electrochemical device can be improved. That is, among the anode active materials used in the anode of the electrochemical device, the silicon-based active material has a capacity that is about 10 times higher than that of a carbon-based active material, and thus has the advantage of being able to realize a high energy density even with a thin electrode due to the high capacity.
[0034] According to one embodiment of the present invention, the self-supporting separator for an electrochemical device does not include a porous polymer substrate. Since the self-supporting separator for an electrochemical device does not include the porous polymer substrate, the heat resistance of the separator is improved, and the shrinkage of the separator at high temperatures can be prevented, resulting in an electrical short circuit of the electrode.
[0035] According to one embodiment of the present invention, the separator comprises inorganic particles and a polymer binder. As described above, by including the inorganic particles and the polymer binder, the heat resistance of the separator is improved, and the shrinkage of the separator at high temperatures, which causes an electrical short circuit of the electrode, can be prevented. Furthermore, pores can be formed within the separator.
[0036] According to one embodiment of the present invention, the separation membrane includes inorganic particles. Non-limiting examples of the inorganic particles include BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, Al(OH)3, TiO2, aluminum peroxide, zinc tin hydroxide (ZnSn(OH)6), tin-zinc oxide (Zn2SnO4, ZnSnO3), antimony trioxide (Sb2O3), antimony tetroxide (Sb2O4), antimony pentoxide (Sb2O5), zeolite A, zeolite X, zeolite Y, γ-AlO(OH), etc., and may include one or more of these. As described above, by including the inorganic particles in the separation membrane, the heat resistance of the separation membrane can be improved.
[0037] According to one embodiment of the present invention, the separator includes a polymer binder provided on part or all of the surface of the inorganic particles. As described above, by including the polymer binder provided on part or all of the surface of the inorganic particles, the inorganic particles can be densely stacked, thereby improving the compression resistance of the separator.
[0038] According to one embodiment of the present invention, the separator comprises pores. Specifically, it may comprise multiple pores. More specifically, the separator may be a porous separator comprising multiple pores within its interior. As described above, by including pores in the separator, it can physically block the negative and positive electrodes while allowing lithium ions to pass through and conduct current.
[0039] According to one embodiment of the present invention, the separator may be formed by inorganic particles being bound by a polymer binder and integrated within a layer. The pores within the separator may be derived from interstitial volumes, which are empty spaces between the inorganic particles. Specifically, as described below, the structure and size of the pores may vary depending on the content and average particle diameter of the inorganic particles. Furthermore, depending on the difference in the structure and size of the pores, the transition metal eluted from the anode can be prevented from moving toward the cathode surface.
[0040] According to one embodiment of the present invention, the content of the inorganic particles is 70 parts by weight or more with respect to 100 parts by weight of the separator. Specifically, it may be 70 parts by weight or more and less than 100 parts by weight, 75 parts by weight or more and 95 parts by weight or less, or 80 parts by weight or more and 90 parts by weight or less with respect to 100 parts by weight of the separator. By controlling the content of the inorganic particles within the above-described range, the heat resistance and compression resistance of the separator can be improved, and the separator can be manufactured as a self-supporting separator.
[0041] According to one embodiment of the present invention, the surface roughness (Sa) of the separator is 600 nm or more and 1100 nm or less. Specifically, the surface roughness (Sa) of the separator may be 650 nm or more and 1050 nm or less, 700 nm or more and 1000 nm or less, 750 nm or more and 950 nm or less, or 750 nm or more and 900 nm or less. In the present specification, the surface roughness (Sa) may be defined as the arithmetic mean of the differences in the direction perpendicular to the center line of each randomly extracted portion from the surface facing the electrode of the separator with the long axis of the separator as the center line. By controlling the surface roughness of the separator within the above-described range, the compression resistance of the separator can be improved without agglomeration of the inorganic particles and the polymer binder.
[0042] According to one embodiment of the present invention, the surface roughness (Sa) of the separation membrane can be measured using an Optical Profiler NV 2700 from Nanosystem. The upper surface of the separation membrane is set as the measurement surface on a sample stage, and an average value in four different measurement areas can be calculated. The setting conditions of the measurement device are as follows.
[0043] Cutoff: 0.8 mm, Scan speed: 0.1 mm / s, Magnification: 500x
[0044] According to one embodiment of the present invention, the inorganic particles may have an average particle diameter (D50) of 40 nm to 300 nm. Specifically, the average particle diameter (D50) of the inorganic particles may be 50 nm to 290 nm, 60 nm to 280 nm, 70 nm to 270 nm, 80 nm to 260 nm, 90 nm to 250 nm, 100 nm to 240 nm, 110 nm to 230 nm, 120 nm to 220 nm, 130 nm to 210 nm, 140 nm to 200 nm, 150 nm to 190 nm, or 160 nm to 180 nm. By controlling the average particle diameter (D50) of the inorganic particles within the above-described range, the phase separation speed and phase separation efficiency between the polymer binder and the inorganic particles in a membrane slurry, which is an emulsion containing the polymer binder dispersed in water, can be improved. Furthermore, when the average particle diameter is less than 40 nm, the dispersibility of the inorganic particles in the slurry prepared for membrane manufacturing may be reduced, and when it exceeds 300 nm, the compressibility of the formed membrane may be reduced.
[0045] In this specification, "D50 particle size" means the particle size at the 50% point of the cumulative distribution of particle numbers according to particle size. The particle size can be measured using a laser diffraction method. Specifically, after the powder to be measured is dispersed in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and when the particles pass through the laser beam, the difference in the diffraction pattern according to the particle size is measured to calculate the particle size distribution. By calculating the particle diameter at the point where the cumulative distribution of particle numbers according to particle size in the measuring device becomes 50%, the D50 particle size can be measured.
[0046] According to one embodiment of the present invention, the inorganic particles usable in the separator may be electrochemically stable. That is, the inorganic particles usable in one embodiment of the present invention may be stable within the operating voltage range of the applied electrochemical device (e.g., Li / Li). + It may be that no oxidation and / or reduction reaction occurs at a voltage of 0 V to 5 V as a reference.
[0047] According to one embodiment of the present invention, the negative electrode includes a silicon-based active material. Specifically, the negative electrode may include a silicon-based compound as the silicon-based active material. Non-limiting examples of the silicon-based compound include Si, SiO. x (0 <x<2), Si-Y(Y는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 전이금속, 희토류 원소 또는 이들의 조합이며, Si은 아닌 것) 합금 및 Si-C 복합체 등을 들 수 있으며 이 중 하나 또는 둘 이상을 포함할 수 있다. 구체적으로 음극에 상기 실리콘계 음극 활물질을 포함할 경우, 에너지 밀도 및 급속 충전 성능이 향상될 수 있다.
[0048] According to one embodiment of the present invention, the content of the silicon-based active material in the negative electrode may be 50 wt% or more. Specifically, the content of the silicon-based active material in the negative electrode may be 50 wt% or more and less than 100 wt%, 55 wt% or more and 95 wt% or less, 60 wt% or more and 90 wt% or less, 65 wt% or more and 85 wt% or less, or 70 wt% or more and 80 wt% or less. By controlling the content of the silicon-based active material within the above-described range, the hardness of the negative electrode can be maintained within a certain range, thereby preventing pore deformation of the separator.
[0049] According to one embodiment of the present invention, the hardness of the negative electrode may be 50 MPa or more and 350 MPa or less. Specifically, the hardness of the negative electrode may be 75 MPa or more and 325 MPa or less, 100 MPa or more and 300 MPa or less, 125 MPa or more and 275 MPa or less, 150 MPa or more and 250 MPa or less, or 175 MPa or more and 225 MPa or less. By controlling the hardness of the negative electrode within the above-described range, it is possible to prevent the pores of the separator from being deformed during the assembly process of the electrochemical device.
[0050] According to one embodiment of the present invention, the hardness of the cathode can be measured using a micro-indenter measuring device. The micro-indenter measuring device can be an indentation device manufactured by Anton Paar. The electrode was indented to a depth of 5 μm, and the hardness was measured by loading / unloading at a rate of 2 N per minute at 5 points per indentation depth.
[0051] According to one embodiment of the present invention, the content of the polymer binder may be 30 parts by weight or less with respect to 100 parts by weight of the separator. Specifically, the content of the polymer binder may be more than 0 parts by weight and less than or equal to 30 parts by weight, 5 parts by weight or more and 25 parts by weight or less, or 10 parts by weight or more and 20 parts by weight or less with respect to 100 parts by weight of the separator. By controlling the content of the polymer binder within the above-described range, the porosity of the separator can be maintained, and even if the coating layer is wetted by the electrolyte after activation of the battery, the adhesive strength can be maintained.
[0052] According to one embodiment of the present invention, the polymer binder may be in the form of particles or non-particulates. Specifically, as described below, the polymer binder may be one that does not dissolve in a dispersion medium or solvent and maintains a particle shape, or the polymer binder may be one that dissolves in a dispersion medium or solvent and does not maintain a particle shape. As described above, by selecting the polymer binder as being in the form of particles or non-particulates, the mechanical properties and porosity of the separation membrane can be controlled.
[0053] According to one embodiment of the present invention, the average particle diameter (D50) of the particulate polymer binder is 1.0 ㎛ or less. Specifically, the average particle diameter (D50) of the first polymer binder particles may be 0.10 ㎛ or more and 0.90 ㎛ or less, 0.15 ㎛ or more and 0.85 ㎛ or less, 0.20 ㎛ or more and 0.70 ㎛ or less, 0.25 ㎛ or more and 0.65 ㎛ or less, or 0.30 ㎛ or more and 0.50 ㎛ or less. By controlling the average particle diameter (D50) of the particulate polymer binder within the above-described range, the phase separation speed and phase separation efficiency between the particulate polymer binder and the inorganic particles in the slurry for a coating layer, which is an emulsion in which the particulate polymer binder is dispersed in water, can be improved.
[0054] According to one embodiment of the present invention, the polymer binder may be an acrylic binder, a polyvinylidene binder, or a combination thereof.
[0055] According to one embodiment of the present invention, the polymer binder may include two or more types of polymer binders. As described above, by including two or more types of polymer binders, the adhesive strength between inorganic materials of the coating layer can be improved, the porosity of the coating layer can be improved, and the dry adhesive strength before injecting the electrolyte and the wet adhesive strength after injecting the electrolyte can be improved at the same time.
[0056] According to one embodiment of the present invention, the polymer binder may include an acrylic binder. This can maintain the porosity of the separator, improve the adhesion between the electrode and the separator during the battery lamination process, thereby enhancing the ease of battery manufacturing, and stably implementing the stacking process.
[0057] According to one embodiment of the present invention, the acrylic binder is a polymer containing a carboxylic acid ester as a repeating unit, and may preferably be a (meth)acrylic acid ester or an acrylic-styrene copolymer.
[0058] According to one embodiment of the present invention, specific examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, n-amyl (meth)acrylate, i-amyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, ethylene glycol (meth)acrylate, di(meth)acrylate, propylene glycol (meth)acrylate, Examples thereof include trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, allyl (meth)acrylate, and ethylene di(meth)acrylate, and the like may be at least one selected from these. Among these, at least one selected from methyl (meth)acrylate, ethyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate is preferable, and methyl (meth)acrylate is particularly preferable.
[0059] According to one embodiment of the present invention, the acrylic-styrene copolymer may include an acrylic binder, and the acrylic binder may be a polyacrylate. For example, the binder may be at least one selected from the group consisting of styrenebutadiene rubber, nitrile-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, and acrylate polymers, and more specifically, may be a copolymer including acrylate.
[0060] According to one embodiment of the present invention, the polymer binder may include a polyvinylidene-based binder. Specifically, according to one embodiment of the present invention, the polyvinylidene-based binder may be a copolymer of polyvinylidene fluoride and hexafluoropropylene. As described above, by selecting the polymer binder as a polyvinylidene-based binder, the porosity of the separator can be maintained, and even if the coating layer is wetted by the electrolyte after activation of the battery, the adhesive strength can be maintained. Furthermore, the stiffness of the battery can be improved, and bending of the separator can be prevented.
[0061] According to one embodiment of the present invention, the polyvinylidene-based binder may be an aqueous binder. Specifically, by selecting the polyvinylidene-based binder as an aqueous binder, pollutants emitted during the manufacturing process of the separator can be minimized, thereby reducing the manufacturing cost of the battery.
[0062] According to one embodiment of the present invention, the thickness of the separator may be 10 ㎛ or more and 30 ㎛ or less, but is not particularly limited thereto. Specifically, the thickness of the separator may be 12 ㎛ or more and 28 ㎛ or less, 14 ㎛ or more and 26 ㎛ or less, 16 ㎛ or more and 24 ㎛ or less, or 18 ㎛ or more and 22 ㎛ or less. The thickness can be adjusted to an appropriate range by a person skilled in the art in terms of heat resistance or electrical resistance. As described above, since the inorganic particles constituting the separator form a dense laminated structure and the average particle diameter (D50) of the inorganic particles is 300 nm or less, the thickness of the separator can be adjusted to an appropriate range within the above-described range.
[0063] According to one embodiment of the present invention, the thickness of the separator can be measured using a contact thickness measuring device. The contact thickness measuring device can be, for example, the VL-50S-B from Mitutoyo.
[0064] According to one embodiment of the present invention, the separator may have improved compression resistance. Specifically, the compression resistance of the separator can be improved by controlling the content and average particle diameter (D50) of the inorganic particles included in the separator. Furthermore, a separator having improved compression resistance can improve the performance of an electrochemical device by suppressing deformation of the pores of the separator when a silicon-based negative electrode active material having a high volume expansion rate during charge and discharge is used as the negative electrode.
[0065] According to one embodiment of the present invention, the change in air permeability of the separator may be 10% or less. Specifically, the change in air permeability of the separator may be more than 0% and less than 10%, 1% or more and less than 9%, 2% or more and less than 8%, 3% or more and less than 7%, or 4% or more and less than 6%. As described above, by controlling the content and average particle diameter (D50) of the inorganic particles included in the separator to improve compression resistance, the change in pores is not large even after the lamination process, so that the change in air permeability of the separator may be low.
[0066] In this specification, “change rate of air permeability” may mean the change rate measured by measuring the air permeability of the membrane before and after the lamination process.
[0067] According to one embodiment of the present invention, the porosity of the separator may be 30% by volume or more. Specifically, the porosity of the separator may be 30% by volume or more and 70% by volume or less, 32% by volume or more and 68% by volume or less, 34% by volume or more and 66% by volume or less, 36% by volume or more and 64% by volume or less, 38% by volume or more and 62% by volume or less, 40% by volume or more and 60% by volume or less, 42% by volume or more and 58% by volume or less, 44% by volume or more and 56% by volume or less, 46% by volume or more and 54% by volume or 48% by volume or more and 52% by volume. By controlling the porosity of the separator within the above-described range, it is possible to maintain the movement of ions in the separator and prevent an increase in resistance of the separator. Specifically, if the porosity is 70% by volume or less, mechanical properties that can withstand the pressing process for bonding with the electrode can be secured, and the surface opening ratio is not too high, making it suitable for securing adhesive strength. On the other hand, if the porosity is 30% by volume or more, it is advantageous from the perspective of ion permeability.
[0068] In this specification, “porosity” means the ratio of the volume occupied by pores to the total volume, and uses volume % as its unit, and can be used interchangeably with terms such as porosity and porosity.
[0069] In this specification, porosity corresponds to a value obtained by subtracting the volume converted to the weight and density of each component of the membrane from the volume calculated by the thickness, width, and length of the membrane.
[0070] In one embodiment of the present invention, the porosity and pore size of the membrane can be measured by the BET 6-point method using a scanning electron microscope (SEM) image, a mercury porosimeter, a capillary flow porometer, or a porosimetry analyzer (Bell Japan Inc, Belsorp-II mini) through a nitrogen gas adsorption flow method. In this case, it may be advantageous to use a capillary flow porometer.
[0071] According to one embodiment of the present invention, the method for forming the separation membrane is as follows, for example. First, a polymer solution or polymer emulsion is prepared by dissolving a polymer binder in an appropriate solvent or dispersing it in a dispersion medium. Non-limiting examples of usable solvents or dispersion mediums include N-methyl-2-pyrrolidone (NMP), acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, cyclohexane, water, or mixtures thereof.
[0072] Next, the inorganic particles are dispersed in an appropriate solvent to prepare an inorganic slurry. Usable solvents include propylene carbonate (PC), ethylene carbonate (EC), N-methyl-2-pyrrolidone (NMP), or mixtures thereof. According to one embodiment of the present invention, the content ratio of the inorganic particles and the polymer binder is as described above, and is appropriately adjusted in consideration of the thickness, pore size, and porosity of the final separation membrane of the present invention.
[0073] Next, the inorganic slurry prepared above is applied to at least one side of the prepared PET release film and dried. The method for applying the inorganic slurry to the surface of the PET release film is not particularly limited to any one method, and any conventional method known in the art can be used. For example, various methods such as dip coating, die coating, roll coating, comma coating, or a combination thereof can be used.
[0074] The above drying process is performed under appropriate temperature and time conditions to minimize the occurrence of surface defects in the membrane. The drying may be performed using a drying oven or a drying auxiliary device, such as hot air, within an appropriate range.
[0075] After the above drying process, the PET release film can be removed to manufacture the separator.
[0076] According to one embodiment of the present invention, the separator is interposed between the negative electrode and the positive electrode and is manufactured into an electrochemical device through a lamination process that applies heat and / or pressure to bond them. In one embodiment of the present invention, the lamination process can be performed by a roll press device including a pair of pressure rollers. That is, the negative electrode, the separator, and the positive electrode can be sequentially laminated and placed between the pressure rollers to achieve interlayer bonding. At this time, the lamination process can be performed by a hot press method.
[0077] One embodiment of the present invention provides an electrochemical device comprising: a positive electrode; a negative electrode including a silicon-based active material; and a separator interposed between the positive electrode and the negative electrode including the silicon-based active material.
[0078] An electrochemical device according to one embodiment of the present invention comprises an inorganic particle and a polymer binder provided on a part or all of the surface of the inorganic particle, includes pores, has a surface roughness (Sa) of 600 nm or more and 1100 nm or less, and includes a separator without a porous polymer substrate, thereby improving heat resistance and compression resistance and improving energy density and life characteristics of a battery.
[0079] According to one embodiment of the present invention, the operating voltage range of the electrochemical device may be 2.5 V to 4.2 V. Specifically, by including the separator with improved compression resistance, the lower voltage limit of a battery including a negative electrode including the silicon-based active material can be utilized.
[0080] In the present invention, the electrochemical device is a device that converts chemical energy into electrical energy through an electrochemical reaction, and is a concept encompassing a primary battery and a secondary battery. In the present specification, the secondary battery is capable of charging and discharging, and refers to a lithium secondary battery, a nickel-cadmium battery, a nickel-hydrogen battery, etc. The lithium secondary battery uses lithium ions as an ion conductor, and examples thereof include, but are not limited to, a non-aqueous electrolyte secondary battery including a liquid electrolyte, an all-solid-state battery including a solid electrolyte, a lithium polymer battery including a gel polymer electrolyte, and a lithium metal battery using lithium metal as an anode.
[0081] According to one embodiment of the present invention, the positive electrode has a positive electrode current collector and a positive electrode active material layer including a positive electrode active material, a conductive material, and a binder resin on at least one surface of the positive electrode current collector. The positive electrode active material is a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M x Ni-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn 1-xA lithium manganese composite oxide represented by MxO2 (wherein, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein, M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a portion of Li in the chemical formula is replaced by an alkaline earth metal ion; a disulfide compound; or a mixture of two or more of Fe2(MoO4)3.
[0082] According to one embodiment of the present invention, the negative electrode has a negative electrode current collector and a negative electrode active material layer including a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode active material is Si, SiO x (0 <x<2), Si-Y 합금 및 Si-C 복합체로 이루어진 군으로부터 선택되는 1종 이상의 실리콘계 음극 활물질을 포함할 수 있다. 나아가, 상기 음극은 음극 활물질로 리튬 금속산화물, 난흑연화 탄소, 흑연계 탄소 등의 탄소; LixFe2O3(0≤x≤1), Li x WO2(0≤x≤1), Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬 금속; 리튬 합금; 규소계 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, 및 Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물 중 선택된 1종 또는 2종 이상의 혼합물을 더 포함할 수 있다.
[0083] According to one embodiment of the present invention, the conductive material may be, for example, one selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, activated carbon, and polyphenylene derivatives, or a mixture of two or more conductive materials among these. More specifically, the conductive material may be one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more conductive materials among these.
[0084] According to one embodiment of the present invention, the current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, stainless steel, copper, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used.
[0085] According to one embodiment of the present invention, the binder resin may be a polymer commonly used in electrodes in the art. Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-cotrichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples thereof include, but are not limited to, cellulose acetatepropionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxyl methyl cellulose.
[0086] According to one embodiment of the present invention, the positive electrode slurry for manufacturing the positive electrode active material layer may include a dispersant, and the dispersant may be a pyrrolidone-based compound. Specifically, it may be N-methylpyrrolidone (ADC-01, LG Chemical).
[0087] According to one embodiment of the present invention, the content of the dispersant included in the positive electrode slurry may be more than 0 part by weight and less than or equal to 0.5 part by weight with respect to 100 parts by weight of the positive electrode slurry. Specifically, the content of the dispersant included in the positive electrode slurry may be more than 0.05 part by weight and less than or equal to 0.4 part by weight with respect to 100 parts by weight of the positive electrode slurry.
[0088] According to one embodiment of the present invention, the negative electrode slurry for manufacturing the negative electrode active material layer may include a dispersant, and the dispersant may be a CMC dispersant (SWCNT, Ocsial, Tuball dispersion).
[0089] According to one embodiment of the present invention, the content of the dispersant included in the negative electrode slurry may be more than 0 part by weight and less than or equal to 1.0 part by weight with respect to 100 parts by weight of the negative electrode slurry. Specifically, the content of the dispersant included in the negative electrode slurry may be more than 0.1 part by weight and less than or equal to 0.9 part by weight, more than 0.2 part by weight and less than or equal to 0.8 part by weight, more than 0.3 part by weight and less than or equal to 0.7 part by weight, or more than 0.4 part by weight and less than or equal to 0.6 part by weight with respect to 100 parts by weight of the negative electrode slurry.
[0090] According to one embodiment of the present invention, an electrochemical device prepared as described above can be placed in an appropriate case and an electrolyte can be injected to manufacture a battery.
[0091] According to one embodiment of the present invention, the electrolyte is A + B - As a salt with the same structure, A + is Li +, Na + , K + B containing an ion composed of an alkali metal cation or a combination thereof; - is PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2) 2- , C(CF2SO2) 3- Salts containing anions such as or combinations thereof are dissolved or dissociated in organic solvents such as propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone (γ-butyrolactone) or mixtures thereof, but are not limited thereto.
[0092] One embodiment of the present invention provides a battery module including a battery including the electrochemical element as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source. Specific examples of the device include, but are not limited to, a power tool that is powered by an electric motor; an electric vehicle including an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), etc.; an electric two-wheeled vehicle including an electric bicycle (E-bike) and an electric scooter (E-scooter); an electric golf cart; and a power storage system.
[0093] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.
[0094]
[0095] <Example 1>
[0096] <Manufacturing of membranes>
[0097] Boehmite (Sasol, Disperal60) with an average particle diameter (D50) of 60 nm and boehmite (Sasol, Disperal80) with an average particle diameter (D50) of 80 nm were added to propylene carbonate (PC), a solvent, at a weight ratio of 3:2 and dispersed to prepare an oil-based slurry.
[0098] A polymer binder solution was prepared by dispersing PVDF (Solvay, Solef5140-02) as a polymer binder in an NMP solvent, adding the polymer binder solution to an oil-based slurry in an appropriate weight ratio, and stirring at 3000 rpm for 45 minutes to prepare an inorganic slurry.
[0099] Afterwards, the above-mentioned inorganic slurry was applied to one side of a PET release film using a doctor blade by bar coating and dried with air at 50°C using a heat gun. The weight ratio of the above-mentioned inorganic particles and the above-mentioned polymer binder was 73:27.
[0100] Afterwards, the PET release film was removed to manufacture a separation membrane having a total thickness of 14.7 ㎛ and a surface roughness (Sa) of 750 nm.
[0101] An electrochemical device including the above-mentioned manufactured separator was manufactured and an experiment was conducted with the operating voltage range being 2.5 V to 4.2 V.
[0102]
[0103] <Manufacturing of electrochemical devices>
[0104] 1) Manufacturing of the anode
[0105] Cathode active material (LiNi) 0.8 Mn 0.1 Co 0.1 O2), a conductive agent (carbon black), a dispersant (N-methylpyrrolidone, ADC-01, LG Chemical), and a binder resin (a mixture of PVDF-HFP and PVDF) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for a positive electrode active material layer with a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of an aluminum thin film (thickness 10 μm) and dried to manufacture a positive electrode having a positive electrode active material layer (thickness 120 μm).
[0106]
[0107] 2) Manufacturing of cathode
[0108] Silicon particles (Elkem, M702), PAM binder (Arakawa, BUH0452), conductive agent (Imerys, SFG-6L), conductive agent (SWCNT, Ocsial, Tuball dispersion), and CMC dispersant (SWCNT, Ocsial, Tuball dispersion) were mixed with water in a weight ratio of 80:9.4:9.6:0.4:0.6 to prepare a slurry for the negative electrode active material layer with a concentration of 25 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of a copper thin film (8 ㎛ thick) and dried to obtain a negative electrode loading of 8 mAh / cm. 2 A cathode having a was manufactured.
[0109]
[0110] 3) Lamination process
[0111] The separators of the examples and comparative examples were interposed between the manufactured cathodes and anodes, and a lamination process was performed to obtain an electrode assembly. The lamination process was performed using a hot press at 70°C and 5.2 MPa for 10 seconds.
[0112]
[0113] <Example 2>
[0114] A separation membrane was manufactured in the same manner as in Example 1, except that the weight ratio of the inorganic particles and the polymer binder was 75:25, the surface roughness (Sa) was 600 nm, and the thickness was 14.8 ㎛.
[0115] An electrochemical device including the above-mentioned manufactured separator was manufactured and an experiment was conducted with the operating voltage range being 2.5 V to 4.2 V.
[0116]
[0117] <Example 3>
[0118] A separation membrane was manufactured in the same manner as in Example 1, except that boehmite (Sasol, Disperal60) with an average particle diameter (D50) of 60 nm and boehmite (Sasol, Disperal80) with an average particle diameter (D50) of 80 nm were used in a weight ratio of 9:1, the weight ratio of the inorganic particles and the polymer binder was 70:30, and the surface roughness (Sa) was 1100 nm and the thickness was 14.9 μm.
[0119] An electrochemical device including the above-mentioned manufactured separator was manufactured and an experiment was conducted with the operating voltage range being 2.5 V to 4.2 V.
[0120]
[0121] <Comparative Example 1>
[0122] A separation membrane was manufactured in the same manner as in Example 1, except that boehmite (Sasol, Disperal80) having an average particle diameter (D50) of 500 nm was added instead of 80 nm in Example 1, and that the surface roughness (Sa) was 300 nm and the thickness was 14.6 μm.
[0123] An electrochemical device including the above-mentioned manufactured separator was manufactured and an experiment was conducted with the operating voltage range being 2.5 V to 4.2 V.
[0124]
[0125] Comparative Example 2
[0126] A separation membrane was manufactured in the same manner as in Example 1, except that a polyolefin substrate having a thickness of 7 μm was used in the above Example 1, the inorganic slurry of Example 1 was coated on both sides of the polyolefin substrate, the weight ratio of the inorganic particles and the polymer binder was 50:50, and the surface roughness (Sa) was 450 nm and the thickness was 14.8 μm.
[0127] An electrochemical device including the above-mentioned manufactured separator was manufactured and an experiment was conducted with the operating voltage range being 2.5 V to 4.2 V.
[0128]
[0129] <Comparative Example 3>
[0130] In the above Example 1, a polyolefin substrate having a thickness of 7 μm was used, and on both sides of the polyolefin substrate, boehmite (Sasol, Disperal80) having an average particle diameter (D50) of 500 nm was added instead of 80 nm in the above Example 1, and the weight ratio of the inorganic particles and the polymer binder was 50:50, and a separation membrane was manufactured in the same manner as in the above Example 1, except that the surface roughness (Sa) was 300 nm and the thickness was 15.0 μm.
[0131] An electrochemical device including the above-mentioned manufactured separator was manufactured and an experiment was conducted with the operating voltage range being 2.5 V to 4.2 V.
[0132]
[0133] <Comparative Example 4>
[0134] A separation membrane was manufactured in the same manner as in Example 1, except that a polyolefin substrate having a thickness of 7 μm was used in Example 1, the inorganic slurry of Example 1 was coated on both sides of the polyolefin substrate, the weight ratio of the inorganic particles and the polymer binder was 50:50, and the surface roughness (Sa) was 450 nm and the thickness was 14.7 μm.
[0135] An electrochemical device including the above-mentioned manufactured separator was manufactured and an experiment was conducted with the operating voltage range being 3.0 V to 4.2 V.
[0136]
[0137] Comparative Example 5
[0138] In the above Example 1, a polyolefin substrate having a thickness of 7 μm was used, and the inorganic slurry of Comparative Example 1, to which inorganic particles having an average particle diameter (D50) of 500 nm were applied, was coated on both sides of the polyolefin substrate, and the weight ratio of the inorganic particles and the polymer binder was 50:50, and a separation membrane was manufactured in the same manner as in the above Example 1, except that the surface roughness (Sa) was 300 nm and the thickness was 14.9 μm.
[0139] An electrochemical device including the above-mentioned manufactured separator was manufactured and an experiment was conducted with the operating voltage range being 3.0 V to 4.2 V.
[0140]
[0141] Comparative Example 6
[0142] A separation membrane was manufactured in the same manner as in Example 1, except that inorganic particles having an average particle diameter (D50) of 60 nm were added, the weight ratio of the inorganic particles and the polymer binder was 65:35, and the surface roughness (Sa) was 1200 nm and the thickness was 15.0 μm.
[0143] An electrochemical device including the above-mentioned manufactured separator was manufactured and an experiment was conducted with the operating voltage range being 2.5 V to 4.2 V.
[0144]
[0145] <Experimental Example 1: Change in membrane permeability>
[0146] The air permeability (air permeability time, Gurley) of the membranes of the examples and comparative examples was measured according to the ASTM D-2873 method. The Gurley value was measured using a Gurley type densometer (No. 158) from Toyoseiki according to the Gurley (JIS) measurement method of the Japanese Industrial Standard. The air permeability refers to the time it takes for 100 cc of air to permeate the membrane or other object of air permeability measurement, and the unit thereof can be used as second / 100 cc. The air permeability change rate was expressed by measuring the air permeability before and after the membranes of the examples and comparative examples went through the lamination process.
[0147]
[0148] <Experimental Example 2: Performance Maintenance Rate of Electrochemical Devices>
[0149] In order to evaluate the life of electrochemical devices manufactured including the separators of the examples and comparative examples, each electrochemical device was charged to 4.2 V at 1.0 C and discharged to 2.5 V or 3.0 V at 0.5 C for 100 cycles, and the initial capacity and residual capacity were measured to indicate the rate of change.
[0150]
[0151] Membrane thickness (㎛)Membrane permeability change rate (%)Electrochemical device operating voltage range (V)Electrochemical device performance maintenance rate (%)Example 1 14.75 2.5-4.29 7.3Example 2 14.88 2.5-4.29 7.0Example 3 14.9 10 2.5-4.29 6.8Comparative example 1 14.6 1 12.5-4.29 5.2Comparative example 2 14.8 3 5 2.5-4.28 9.8Comparative example 3 15.0 4 5 2.5-4.28 7.4Comparative example 4 14.7 3 5 3.0-4.29 1.3Comparative example 5 14.9 4 5 3.0-4.29 0.4Comparative example 6 15.0 1 2.5-4.29 5.0
[0152]
[0153] Referring to Table 1 above, it was confirmed that the separator of Example 1 according to one embodiment of the present invention had the lowest change in air permeability after internal compression, and the performance maintenance rate of the electrochemical device was the best even when the operating voltage range of the electrochemical device was used from 2.5 V to 4.2 V.
[0154] In addition, it was confirmed that the change rate of air permeability after compression was maintained low in the surface roughness (Sa) range of 600 nm to 1100 nm through the above examples 1 to 3, and that the performance of the electrochemical device was excellent even when the operating voltage range of the electrochemical device was used from 2.5 V to 4.2 V.
[0155] In this regard, it was confirmed that Comparative Example 1 had a lower change rate in air permeability than Example 1, and that the performance retention rate also decreased when the same electrochemical device driving voltage range as Examples 1 to 3 was applied. This is believed to be because the compression resistance characteristics were deteriorated because the pore size of the separator increased and the pore distribution widened as the size of the inorganic material applied to the separator increased.
[0156] Comparative Examples 2 and 3 are separators manufactured by coating the inorganic slurries of Example 1 and Comparative Example 1 on both sides of a 7 μm thick polyolefin substrate, respectively. When a polyolefin substrate, which is softer and less hard than the inorganic substrate, was applied to the separator, the rate of change in air permeability after compression tended to increase rapidly. As a result, when the voltage driving range of the manufactured electrochemical device was evaluated in the same manner as in Example 1, it was confirmed that the performance retention rate of the electrochemical device was drastically reduced.
[0157] Comparative Examples 4 and 5 are experiments conducted using the same membrane as Comparative Examples 2 and 3, but changing the voltage operating range of the electrochemical device to 3.0 V to 4.2 V. Therefore, it was confirmed that the change rate of the air permeability after the internal compression of the membrane was the same as Comparative Examples 2 and 3. It was confirmed that when the voltage operating range of the electrochemical device was changed to a narrower range (3.0 V to 4.2 V) than Comparative Examples 2 and 3 (2.5 V to 4.2 V), the performance maintenance rate of the electrochemical device was slightly improved, but it was confirmed that the level did not reach that of Example 1.
[0158] Comparative Example 6 showed a lower change rate in air permeability than Example 1, and when the same electrochemical device operating voltage range was applied, the performance retention rate also decreased. This is believed to be due to the decrease in the size of the inorganic material applied to the separator, which increased the roughness of the separator surface, resulting in a deterioration in compression resistance.
[0159] A self-supporting separator for an electrochemical device according to one embodiment of the present invention can be expected to improve compression resistance, enhance energy density, and have excellent performance retention of the electrochemical device by controlling the surface roughness (Sa) of the separator by controlling the content and average particle diameter of inorganic particles, thereby improving the life characteristics.
Claims
1. In a self-supporting separator for an electrochemical device having a cathode containing a silicon-based active material, Comprising an inorganic particle and a polymer binder provided on part or all of the surface of the inorganic particle, Includes pores, The content of the above inorganic particles is 70 parts by weight or more with respect to 100 parts by weight of the above separation membrane, A self-supporting separator for an electrochemical device, wherein the surface roughness (Sa) of the above separator is 600 nm or more and 1100 nm or less.
2. In claim 1, The above inorganic particles are, A self-supporting separator for an electrochemical device, having an average particle diameter (D50) of 40 nm or more and 300 nm or less.
3. In claim 1, A self-supporting separator for an electrochemical device, wherein the content of the silicon-based active material in the cathode is 50 wt% or more.
4. In claim 1, A self-supporting separator for an electrochemical device, wherein the hardness of the cathode is 50 MPa or more and 350 MPa or less.
5. In claim 1, A self-supporting separator for an electrochemical device, wherein the content of the polymer binder is 30 parts by weight or less with respect to 100 parts by weight of the separator.
6. In claim 1, A self-supporting separator for an electrochemical device, wherein the polymer binder is an acrylic binder, a polyvinylidene binder, or a combination thereof.
7. In claim 1, A self-supporting separator for an electrochemical device, wherein the thickness of the separator is 10 ㎛ or more and 30 ㎛ or less.
8. In claim 1, A self-supporting separator for an electrochemical device, wherein the change in permeability of the separator according to the following mathematical formula 1 is 10% or less. [Mathematical Formula 1] Change in air permeability (%) = {(air permeability of the membrane after pressure application - air permeability of the membrane before pressure application) / air permeability of the membrane before pressure application} X 100 9. An electrochemical device comprising: a positive electrode; a negative electrode including a silicon-based active material; and a separator interposed between the positive electrode and the negative electrode including the silicon-based active material, the separator of claim 1.
10. In claim 9, An electrochemical device, wherein the operating voltage range of the electrochemical device is 2.5 V to 4.2 V.
Citation Information
Patent Citations
A selfsupporting separator for an electrochemical device and an electrochemical device comprising the same
KR1020240161030A
Separator and nonaqueous electrolyte battery
JP2013137984A
Apparatus and method for diagnosing disease of target part based on medicial image
KR102555996B1
Dismantling apparatus of scaffold structure for liquefied gas storage tank and dismantling method of scaffold structure usiing the same
KR102610363B1
Electroluminescent Display
KR102870627B1