Positive electrode active material, positive electrode slurry comprising same, manufacturing method thereof, and positive electrode and lithium secondary battery comprising same
The development of a lithium nickel-based oxide positive electrode active material with a cobalt-containing coating layer and specific compositional adjustments addresses the challenges of crack formation and viscosity issues in lithium nickel-based oxide batteries, achieving improved electrochemical performance and stability.
Patent Information
- Application Number
- PCT/KR2024/005937
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-02
- Filing Date
- 2024-05-02
- Publication Date
- 2024-11-07
AI Technical Summary
Lithium nickel-based oxide positive electrode active materials in secondary batteries face issues with crack formation during charging and discharging due to their secondary particle form, leading to high resistance and low output, and the transition to single particles increases viscosity and stability problems in the slurry during manufacturing.
A positive electrode active material with a lithium nickel-based oxide composition, including a cobalt-containing coating layer, is developed, with specific adjustments to particle size, residual LiOH content, and Co/Ni ratio to enhance phase stability and reduce resistance, featuring a molar ratio of Ni to all transition metals of 80 mol% or more, a cobalt-containing coating layer of 2.0 mol% or more, and a particle size of 3.7 to 6.0 μm, which improves the electrochemical properties.
The solution results in a positive electrode with low charge transfer resistance, high initial efficiency, and excellent high-temperature lifespan characteristics, while maintaining stable electrode production and yield by optimizing the slurry viscosity and binder adsorption.
Smart Images

Figure KR2024005937_07112024_PF_FP_ABST
Abstract
Description
Positive electrode active material, positive electrode slurry containing the same, method for producing the same, positive electrode containing the same, and lithium secondary battery
[0001] Cross-citation with related applications
[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2023-0057356, filed May 2, 2023, the entire contents of which are incorporated herein by reference.
[0003] Technology field
[0004] The present invention relates to a positive electrode active material, a positive electrode slurry containing the same, a method for producing the same, a positive electrode containing the same, and a lithium secondary battery.
[0005]
[0006] As technological development and demand for mobile devices increase, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which boast high energy density and voltage, long cycle life, and low self-discharge rates, are commercialized and widely used.
[0007] Lithium-transition metal composite oxides are used as cathode active materials in lithium secondary batteries. Among these, lithium-nickel oxides, which facilitate the implementation of large-capacity batteries, are being actively researched and developed. However, the secondary particle form has the problem of exacerbating cracking within the cathode active material during charge and discharge.
[0008] To solve the above problems, a technology was proposed to manufacture a cathode active material in the form of a single particle rather than a secondary particle by increasing the sintering temperature during the manufacture of lithium nickel oxide.
[0009] However, single-particle cathode active materials have problems such as low interparticle interfaces, which serve as passageways for lithium ions, and long lithium diffusion paths within the particles, resulting in high resistance and low output. Therefore, conventionally, the average particle size has been formed to be approximately 4.0 μm, thereby minimizing increased resistance and reduced output of single-particle cathode active materials.
[0010] However, in order to ensure that the average particle size of the positive electrode active material in the form of a single particle is approximately 4.0 ㎛, a process of crushing with strong crushing strength must be performed. In this process, a large amount of fine particles are generated, which causes the viscosity of the slurry to increase, resulting in a problem of rapid deterioration in phase stability.
[0011] Therefore, there is a need for a technology to improve the phase stability of slurry to secure stable electrode production and yield.
[0012]
[0013] The present invention is intended to solve the above problems, and provides a cathode active material having improved phase stability of a slurry by controlling the particle size distribution of the cathode active material, the residual LiOH content, and the cobalt-containing coating layer content within specific ranges, a cathode slurry containing the same, and a method for producing the same.
[0014] The present invention relates to a D of a positive electrode active material 50 The purpose is to provide a positive electrode and lithium secondary battery with excellent electrochemical properties by controlling the range within a specific range.
[0015]
[0016] In one aspect, the present invention is a cathode active material comprising a lithium nickel-based oxide containing nickel (Ni) and cobalt (Co), wherein the molar ratio of Ni among the total transition metals is 80 mol% or more; and a cobalt-containing coating layer formed on the surface of the lithium nickel-based oxide, wherein the lithium nickel-based oxide is in the form of a single particle consisting of one single nodule or a quasi-single particle which is a composite of 30 or fewer nodules, and the cobalt-containing coating layer is included in an amount of 2.0 mol% or more with respect to 100 mol of the lithium nickel-based oxide, and the cathode active material is D 50 A cathode active material is provided, which has a diameter of 3.7 μm to 6.0 μm, a residual LiOH content of 0.20 wt% or less, and a Co / Ni ratio of 0.15 to 0.40 at a depth of 45 nm from the surface.
[0017] The above lithium nickel-based oxide may have a molar ratio of Ni of 93 mol% or more among the total transition metals.
[0018] The above positive electrode active material may have a residual lithium content of 0.60 wt% or less.
[0019] The above positive electrode active material may have a residual Li2CO3 content of 0.40 wt% or less.
[0020] The above positive electrode active material is D min This can be 1.0㎛ or more.
[0021] The above lithium nickel-based oxide may be represented by the following chemical formula 1.
[0022] [Chemical Formula 1]
[0023] Li a Ni b Co c M 1 d M 2 e O2
[0024] In the above chemical formula 1, M 1 is at least one selected from the group consisting of Mn and Al, and M 2is at least one selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb, and Mo, and 1.0≤a≤1.5, 0.8≤b≤1.0, 0≤c≤0.2, 0≤d≤0.2, 0≤e≤0.1.
[0025]
[0026] In another aspect, the present invention provides a cathode slurry comprising the above-described cathode active material and binder.
[0027] The adsorption amount of the binder to the positive electrode active material is 25.0 mg / m 2 It could be as follows:
[0028] The viscosity change rate calculated by Equation 1 below at 25℃ may be 1,000% or less.
[0029] [Formula 1]
[0030]
[0031]
[0032] In another aspect, the present invention is a method for producing a positive electrode active material, comprising the steps of: mixing a lithium nickel-based transition metal hydroxide precursor containing nickel (Ni) and cobalt (Co) and a lithium raw material and first firing the mixture to form a lithium nickel-based oxide; and second firing the mixture of the lithium nickel-based oxide with a cobalt-containing raw material to form a positive electrode active material including a cobalt-containing coating layer; wherein the positive electrode active material comprises a lithium nickel-based oxide having a molar ratio of Ni of 80 mol% or more among the total transition metals, and a cobalt-containing coating layer formed on the surface of the lithium nickel-based oxide, wherein the lithium nickel-based oxide is in the form of a single particle consisting of one single nodule or a quasi-single particle which is a composite of 30 or fewer nodules, and the positive electrode active material is D 50The present invention provides a method for producing a positive electrode active material, wherein the positive electrode active material has a particle size of 3.7 μm to 6.0 μm, a residual LiOH content of 0.20 wt% or less, the cobalt-containing coating layer is included in an amount of 2.0 mol% or more with respect to 100 mol of the lithium nickel-based oxide, and the secondary firing is performed at 600°C to 700°C.
[0033] The above cobalt-containing raw materials are Co(OH)2, CoOOH, Co(OCOCH3) 2· 4H2O, Co(NO3) 2· 6H2O, CoSO4, and Co(SO4) 2· It may include at least one selected from the group consisting of 7H2O.
[0034] The above primary firing can be performed at 750°C to 880°C.
[0035]
[0036] In another aspect, the present invention provides a positive electrode comprising the positive electrode active material described above.
[0037]
[0038] In another aspect, the present invention provides a lithium secondary battery including the above-described positive electrode.
[0039]
[0040] The cathode active material according to the present invention includes a cobalt-containing coating layer on the surface of a lithium nickel-based oxide, and by controlling the particle size, residual LiOH content, and content of the cobalt-containing coating layer within a specific range, an increase in the viscosity of the slurry is suppressed and the amount of adsorption with a binder is reduced, thereby improving the phase stability of the slurry and realizing excellent processability.
[0041] The positive electrode active material according to the present invention is D 50 By controlling the resistance to a specific range to have low charge transfer resistance and diffusion resistance, high initial efficiency, low initial resistance, and excellent high-temperature life characteristics can be realized.
[0042]
[0043] Figure 1 is a SEM (Scanning Electron Microscope) image of a positive electrode active material powder manufactured according to Example 1 of the present invention.
[0044] Figure 2 is a SEM (Scanning Electron Microscope) image of the positive electrode active material powder manufactured by Example 2 of the present invention.
[0045] Figure 3 is a SEM (Scanning Electron Microscope) image of the positive electrode active material powder manufactured by Example 3 of the present invention.
[0046] Figure 4 is a SEM (Scanning Electron Microscope) image of the positive electrode active material powder manufactured by Comparative Example 1 of the present invention.
[0047] Figure 5 is a SEM (Scanning Electron Microscope) image of the positive electrode active material powder manufactured by Comparative Example 2 of the present invention.
[0048] Figure 6 is a SEM (Scanning Electron Microscope) image of the positive electrode active material powder manufactured by Comparative Example 3 of the present invention.
[0049] Figure 7 is a SEM (Scanning Electron Microscope) image of the positive electrode active material powder manufactured by Comparative Example 4 of the present invention.
[0050] Figure 8 is a graph showing the XPS depth profile of the cobalt-containing coating layer included in the positive electrode active materials manufactured in Examples 1 to 3 and Comparative Examples 1 to 4.
[0051]
[0052] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the embodiments described in detail below together with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below and may be implemented in various different forms. These embodiments are provided only to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined only by the scope of the claims. Like reference numerals designate like elements throughout the specification.
[0053] Unless otherwise defined, all terms (including technical and scientific terms) used herein may be used in their common sense to those of ordinary skill in the art to which the present invention pertains. Furthermore, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively unless explicitly and specifically defined otherwise.
[0054] The terminology used herein is for the purpose of describing embodiments and is not intended to limit the present invention. In this specification, singular forms also include plural forms, unless specifically stated otherwise. As used herein, the terms "comprises" and / or "comprising" do not exclude the presence or addition of one or more other components in addition to the components mentioned.
[0055] In this specification, when it is said that a part includes a certain component, this does not mean that other components are excluded, but rather that other components may be included, unless specifically stated otherwise.
[0056] In this specification, the description of “A and / or B” means A, or B, or A and B.
[0057] In this specification, “%” means weight percent unless explicitly indicated otherwise.
[0058] In this specification, “particle” may include any one or all of a single particle, a quasi-single particle, a primary particle, a nodule, and a secondary particle.
[0059] In this specification, a "single particle" is a particle composed of one single nodule. In the present invention, a "quasi-single particle" means a composite particle formed of 30 or fewer nodules.
[0060] In this specification, "nodule" means a particle unit body constituting a single particle and a pseudo-single particle, and the nodule may be a single crystal lacking a crystalline grain boundary, or a polycrystal having no apparent grain boundary when observed under a field of view of 5,000 to 20,000 times using a scanning electron microscope (SEM). The average particle diameter of the nodule may be measured as the arithmetic mean of the particle diameters of each nodule measured using a scanning electron microscope (SEM).
[0061] In this specification, "secondary particle" means a particle formed by the agglomeration of tens to hundreds of primary particles. More specifically, a secondary particle is an agglomerate of 40 or more primary particles.
[0062] In this specification, "D 50 " is the average particle diameter, which means the particle diameter at the point where the particle volume according to the particle diameter is 50% in the particle size distribution of the positive electrode active material. The average particle diameter (D 50) can be measured using a commercially available laser PSD (Particle Size Distribution) particle size measuring device. For example, after dispersing the positive active material powder in a dispersion medium, it is introduced into a commercially available laser PSD (Particle Size Distribution) particle size measuring device (e.g., Microtrac S3500), and when the particles pass through a laser beam, the difference in diffraction pattern according to particle size is measured to calculate the particle size distribution.
[0063] In this specification, the concentration gradient composition and concentration of the transition metal in the positive electrode active material particles can be confirmed using a method such as X-ray photoelectron spectroscopy (XPS), an electron probe micro analyzer (EPMA), an inductively coupled plasma - atomic emission spectrometer (ICP-AES), or a time of flight secondary ion mass spectrometry (ToF-SIMS). Specifically, the positive electrode active material particles can be etched with Ar gas for 3000 seconds using X-ray photoelectron spectroscopy (XPS), and the element ratio (atomic ratio) of each metal can be measured while etching from the surface to the center of the positive electrode active material.
[0064]
[0065] Hereinafter, the present invention will be described in more detail.
[0066]
[0067] positive electrode active material
[0068] The cathode active material according to the present invention is a cathode active material comprising a lithium nickel-based oxide containing nickel (Ni) and cobalt (Co), and having a molar ratio of Ni of the total transition metal of 80 mol% or more; and a cobalt-containing coating layer formed on the surface of the lithium nickel-based oxide, wherein the lithium nickel-based oxide is in the form of a single particle consisting of one single nodule or a quasi-single particle which is a composite of 30 or fewer nodules, and the cobalt-containing coating layer is included in an amount of 2.0 mol% or more with respect to 100 mol of the lithium nickel-based oxide, and the cathode active material is D 50 It is characterized by having a diameter of 3.7 μm to 6.0 μm, a residual LiOH content of 0.20 wt% or less, and a Co / Ni ratio of 0.15 to 0.40 at a depth of 45 nm from the surface.
[0069]
[0070] Research and development on lithium nickel-based oxides is becoming increasingly active. However, secondary particle-based oxides have the disadvantage of exacerbating cracking within the cathode active material during charge and discharge. To address this issue, a technology has been proposed to increase the sintering temperature during lithium nickel-based oxide production to produce single-particle cathode active materials rather than secondary particles.
[0071] However, single-particle cathode active materials have problems such as low interparticle interfaces, which serve as passageways for lithium ions, and long lithium diffusion paths within the particles, resulting in high resistance and low output. Therefore, conventionally, the average particle size has been formed to be approximately 4.0 μm, thereby minimizing increased resistance and reduced output of single-particle cathode active materials.
[0072] However, in order to ensure that the average particle size of the positive electrode active material in the form of a single particle is approximately 4.0 ㎛, a process of crushing with strong crushing strength must be performed. In this process, a large amount of fine particles are generated, which causes the viscosity of the slurry to increase, resulting in a problem of rapid deterioration in phase stability.
[0073]
[0074] The cathode active material according to the present invention comprises a lithium nickel-based oxide containing nickel (Ni) and cobalt (Co), wherein the molar ratio of Ni among the total transition metals is 80 mol% or more, preferably 90 mol% or more, and more preferably 93 mol% or more. When the molar ratio of Ni satisfies the above range, excellent capacity characteristics can be realized.
[0075] However, Ni-based cathode active materials containing high concentrations of Ni have a high content of nickel among the transition metals constituting the cathode active material compared to other transition metals, so they have high capacity but have unstable Ni present on the surface of the cathode active material. 3+ , Ni 4+ There is a limitation of structural instability due to ions. To address this structural instability, various technologies are being studied to modify the surface of the positive electrode active material.
[0076] In this regard, the inventor of the present invention introduced a cobalt-containing coating layer on the surface of a Ni-based positive electrode active material containing a high concentration of Ni to improve surface stability, and the cobalt-containing coating layer is included in an amount of 2.0 mol% or more with respect to 100 mol of lithium nickel-based oxide, and D 50 When a positive electrode active material having a diameter of 3.7 μm to 6.0 μm, a residual LiOH content of 0.20 wt% or less, and a Co / Ni ratio of 0.15 to 0.40 at a depth of 45 nm from the surface is applied, it was found that the viscosity change rate of the slurry decreases and the amount of adsorption with the binder decreases, thereby improving the phase stability of the slurry.
[0077]
[0078] The lithium nickel-based oxide is in the form of a single particle consisting of one single nodule or a composite of 30 or fewer, preferably 2 to 20, and more preferably 2 to 10 nodules, in the form of a pseudo-single particle. Such lithium nickel-based oxide in the form of a single particle and / or pseudo-single particle has higher particle strength than conventional lithium nickel-based oxide in the form of a secondary particle consisting of tens to hundreds of primary particles aggregated together, and thus is less prone to particle breakage during rolling.
[0079] In addition, in the case of the lithium nickel-based oxide in the form of single particles or pseudo-single particles according to the present invention, since the number of sub-components (i.e., nodules) constituting the particles is small, the change due to volume expansion and contraction of the primary particles during charge and discharge is small, and accordingly, the occurrence of cracks inside the particles is also significantly reduced.
[0080]
[0081] The above positive electrode active material is D 50 This may be 3.7㎛ to 6.0㎛, preferably 3.7㎛ to 5.7㎛, more preferably 3.7㎛ to 5.0㎛. The above D 50 If it is less than 3.7㎛, the fine powder content may be high during slurry production, which may cause the viscosity of the slurry to become excessively high, and D 50 If it exceeds 6.0㎛, lithium mobility in the positive electrode active material may decrease, which may increase the initial resistance of the lithium secondary battery containing it.
[0082]
[0083] The residual lithium of the positive electrode active material according to the present invention may be at least one selected from the group consisting of LiOH and Li2CO3.
[0084] The residual LiOH content may be 0.20 wt% or less, preferably 0.01 wt% to 0.20 wt%, and more preferably 0.05 wt% to 0.15 wt%. In general, Ni-based positive electrode active materials containing a high concentration of Ni have a problem in that it is difficult to suppress an increase in resistance or a decrease in capacity because the proportion of LiOH remaining on the surface of the positive electrode active material increases as LiOH is used as a lithium raw material in the precursor to obtain a high capacity. Therefore, it is necessary to control the residual LiOH content. If the residual LiOH content exceeds the above numerical range, when it is dissolved in a solvent (NMP) during the electrode manufacturing process, the solvent becomes alkaline, and the alkaline solvent is mixed with a binder (PVdF) to gel the slurry, making it difficult to manufacture the electrode.
[0085] The above-mentioned positive electrode active material may have a residual lithium content of 0.60 wt% or less, preferably 0.01 wt% to 0.60 wt%, and more preferably 0.05 wt% to 0.50 wt%. The residual Li2CO3 content may be 0.40 wt% or less, preferably 0.10 wt% to 0.35 wt%, and more preferably 0.20 wt% to 0.30 wt%. If the residual lithium or residual Li2CO3 content exceeds the above numerical range, it may react with the electrolyte after application to the battery, causing adverse effects such as swelling and gas generation, which may cause expansion and ignition of the battery. In addition, since the residual lithium acts as a coating layer forming raw material in the coating layer forming process described later, if the residual lithium exists in excess on the surface of the lithium nickel-based oxide, the coating layer is formed thickly, which causes a problem in that the resistance characteristics increase.
[0086]
[0087] The cobalt-containing coating layer may be included in an amount of 2.0 mol% or more based on 100 mol of the lithium nickel-based oxide. Preferably, the cobalt-containing coating layer may be included in an amount of 2.0 mol% to 5.5 mol%, more preferably 2.0 mol% to 3.5 mol% based on 100 mol of the lithium nickel-based oxide. If the cobalt-containing coating layer according to the present invention exceeds the above content range, the coating layer may be formed too thickly, which may result in increasing the initial resistance. On the other hand, if the cobalt-containing coating layer is less than the above content range, unstable Ni present on the surface of the positive electrode active material may be present. 3+ , Ni 4+ There is a problem that the structural instability caused by ions is not resolved.
[0088]
[0089] In addition, the cobalt-containing coating layer may have a Co / Ni ratio of 0.15 to 0.40, preferably 0.16 to 0.30, and more preferably 0.17 to 0.25 at a depth of 45 nm from the surface. In the present invention, the D of the positive electrode active material 50 And when the Co / Ni ratio at the 45 nm depth satisfies the above range along with the residual LiOH content, the increase in viscosity of the slurry can be suppressed and the amount of adsorption with the binder can be reduced, thereby improving the phase stability of the slurry and realizing excellent processability.
[0090]
[0091] The positive electrode active material according to the present invention is D min The minimum particle size of the positive electrode active material may be 1.0 μm or more, preferably 1.0 μm to 6.0 μm, and more preferably 1.0 μm to 5.0 μm. D min If this above range is satisfied, the viscosity may increase excessively during slurry production, which may harm the processability.
[0092]
[0093] Meanwhile, the positive electrode active material according to the present invention may include a lithium nickel-based oxide, and specifically, may include a lithium nickel-based oxide having a composition as represented by the following chemical formula 1.
[0094] [Chemical Formula 1]
[0095] Li a Ni b Co c M 1 d M 2 e O2
[0096] In the above chemical formula 1, M 1 is at least one selected from the group consisting of Mn and Al, preferably Mn or a combination of Mn and Al, and M 2 is at least one selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb and Mo. M 2 Although elements are not essential, when included in appropriate amounts, they can promote grain growth during firing or play a role in improving crystal structure stability.
[0097] The above a represents the molar ratio of lithium in the lithium nickel-based oxide, and may be 1.0≤a≤1.5, 1.0≤a<1.5, or 1.0≤a≤1.2. When the molar ratio of lithium satisfies the above range, a stable layered crystal structure can be formed.
[0098] The above b represents the molar ratio of nickel among all metals excluding lithium in the lithium nickel-based oxide, and may be 0.8≤b≤1.0, 0.85≤b≤1.0, or 0.90≤b≤1.0. When the molar ratio of nickel satisfies the above range, excellent capacity characteristics are exhibited, and in particular, when the molar ratio of nickel is 0.90 or more, even better capacity characteristics can be realized.
[0099] The above c represents the molar ratio of cobalt among all metals excluding lithium in the lithium nickel oxide, and 0≤c≤0.2, 0 <c<0.2, 0<c≤0.18, 또는 0<c<0.18일 수 있다.
[0100] The above d is M of all metals except lithium in lithium nickel oxide. 1 It represents the molar ratio of , 0≤d≤0.2, 0 <d<0.2, 0<d≤0.18, 또는 0<d<0.18일 수 있다.
[0101] The above e is M of all metals except lithium in lithium nickel oxide. 2 It represents the molar ratio of elements, 0≤e≤0.1, 0 <e<0.1, 또는 0<e≤0.08일 수 있다.
[0102]
[0103] Method for manufacturing positive electrode active material
[0104] Next, a method for manufacturing the positive electrode active material of the present invention will be described.
[0105]
[0106] When manufacturing a cathode active material in which the molar ratio of nickel among the total transition metals is 80 mol% or more, the high sintering temperature can result in a low surface structural integrity of the cathode active material and a high concentration of residual lithium. Furthermore, large particle sizes of the cathode active material can lead to a problem of high initial resistance. Therefore, a technology is needed that can improve the surface structural integrity, reduce the concentration of residual lithium, and lower the initial resistance through optimization of coating conditions by forming a coating layer on the surface of lithium nickel-based oxide particles.
[0107]
[0108] A method for manufacturing a cathode active material according to the present invention includes a step of mixing a lithium nickel-based transition metal hydroxide precursor containing nickel (Ni) and cobalt (Co) and a lithium raw material and firing the mixture for the first time to form a lithium nickel-based oxide, and a step of mixing the lithium nickel-based oxide with a cobalt-containing raw material and firing the mixture for the second time to form a cathode active material including a cobalt-containing coating layer.
[0109] The lithium nickel-based transition metal oxide is a single particle having a molar ratio of Ni of 80 mol% or more among the total transition metals, or a pseudo-single particle consisting of one single nodule or a composite of 30 or fewer nodules. In addition, the cathode active material is D 50 This is 3.7㎛ to 6.0㎛, the residual LiOH content is 0.20 wt% or less, the cobalt-containing coating layer is included in an amount of 2.0 mol% or more with respect to 100 mol of the lithium nickel-based oxide, and the secondary firing is performed at 600℃ to 700℃. Since the above-described content applies equally, redundant explanation is omitted.
[0110]
[0111] Hereinafter, each step of the method for manufacturing a positive electrode active material is described in detail.
[0112]
[0113] (1) Step of forming lithium nickel oxide
[0114] First, a lithium nickel-based transition metal hydroxide precursor containing nickel (Ni) and cobalt (Co) and a lithium raw material are mixed and calcined for the first time to form a lithium nickel-based oxide.
[0115]
[0116] At this time, the lithium nickel-based transition metal hydroxide precursor, i.e., the cathode active material precursor, may be purchased and used as a commercially available precursor such as nickel-cobalt-manganese-based hydroxide, or may be manufactured according to a precursor manufacturing method known in the art, such as a co-precipitation method.
[0117] For example, nickel (Ni), cobalt (Co) and M 1 After preparing a transition metal-containing solution containing an ammonium cation, a complex forming agent containing an ammonium cation and a basic aqueous solution are added to the transition metal-containing solution to cause a co-precipitation reaction, thereby preparing a positive electrode active material precursor.
[0118] The above transition metal-containing solution comprises nickel-containing raw material, cobalt-containing raw material, M 1 May contain raw materials, and the M 1 The containing raw material may be a manganese-containing raw material and / or an aluminum-containing raw material.
[0119] The nickel-containing raw material may be, for example, a nickel-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide or oxyhydroxide, and specifically, may be, but is not limited to, Ni(OH)2, NiO, NiOOH, NiCO3ㆍ2Ni(OH)2ㆍ4H2O, NiC2O2ㆍ2H2O, Ni(NO3)2ㆍ6H2O, NiSO4, NiSO4ㆍ6H2O, fatty acid nickel salts, nickel halides or combinations thereof.
[0120] The cobalt-containing raw material may be a cobalt-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide or oxyhydroxide, and specifically, may be, but is not limited to, Co(OH)2, CoOOH, Co(OCOCH3)2ㆍ4H2O, Co(NO3)2ㆍ6H2O, CoSO4, Co(SO4)2ㆍ7H2O or a combination thereof.
[0121] The manganese-containing raw material may be, for example, a manganese-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, oxyhydroxide or a combination thereof, and specifically, may be, but is not limited to, manganese oxides such as Mn2O3, MnO2, Mn3O4; manganese salts such as MnCO3, Mn(NO3)2, MnSO4, manganese acetate, manganese dicarboxylic acid salts, manganese citrate, manganese fatty acid salts; manganese oxyhydroxide, manganese chloride or a combination thereof.
[0122] The aluminum-containing raw material may be, for example, Al2O3, Al(OH)3, Al(NO3)3, Al2(SO4)3, (HO)2AlCH3CO2, HOAl(CH3CO2)2, Al(CH3CO2)3 aluminum halides or combinations thereof.
[0123] The transition metal-containing solution contains nickel-containing raw materials, cobalt-containing raw materials, and M 1 It is manufactured by adding the containing raw material to a solvent, specifically, water, or a mixed solvent of an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water, or an aqueous solution of a nickel-containing raw material, an aqueous solution of a cobalt-containing raw material, and M 1 It may be manufactured by mixing the raw materials contained therein.
[0124] The ammonium cation-containing complex forming agent may be, but is not limited to, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, NH4CO3, or a combination thereof. Meanwhile, the ammonium cation-containing complex forming agent may be used in the form of an aqueous solution, and in this case, the solvent may be water, or a mixture of water and an organic solvent (specifically, alcohol, etc.) that can be uniformly mixed with water.
[0125] The basic compound may be a hydroxide of an alkali metal or alkaline earth metal, such as NaOH, KOH, or Ca(OH)2, a hydrate thereof, or a combination thereof. The basic compound may also be used in the form of an aqueous solution, in which case the solvent may be water, or a mixture of water and an organic solvent that is uniformly miscible with water (specifically, alcohol, etc.).
[0126] The basic compound is added to adjust the pH of the reaction solution, and can be added in an amount such that the pH of the metal solution becomes 8 to 12.
[0127] The co-precipitation reaction can be carried out in an inert atmosphere such as nitrogen or argon, at a temperature range of 35°C to 80°C.
[0128] Nickel-cobalt-M by the above process 1 The positive electrode active material precursor particles of hydroxide are generated and precipitated in the reaction solution. Nickel-containing raw material, cobalt-containing raw material and M 1 By controlling the concentration of the contained raw material, a positive electrode active material precursor having a nickel (Ni) content of 80 mol% or more among the total metal content can be manufactured. The precipitated positive electrode active material precursor particles can be separated and dried according to a conventional method to manufacture a positive electrode active material precursor.
[0129]
[0130] Afterwards, the lithium nickel-based transition metal hydroxide precursor and the lithium raw material can be mixed.
[0131] The lithium raw material may include lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and is not particularly limited as long as it can be dissolved in water. Specifically, the lithium raw material may be Li2CO3, LiNO3, LiNO2, LiOH, LiOHㆍH2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, or Li3C6H5O7, and any one of these or a mixture of two or more thereof may be used.
[0132] The positive electrode active material precursor and the lithium source material may be mixed in a molar ratio of, for example, but not limited to, about 1:1, about 1:1.05, about 1:1.10, about 1:1.15, or about 1:1.20.
[0133]
[0134] Thereafter, the mixture may be subjected to a primary firing. The primary firing may be performed in an air or oxygen atmosphere. The primary firing may be performed at a temperature of 750°C to 880°C, 780°C to 880°C, 800°C to 870°C, or 820°C to 870°C. The primary firing may be performed for 5 to 20 hours, 6 to 12 hours, or 8 to 10 hours.
[0135]
[0136] (2) Step of mixing lithium nickel oxide with cobalt-containing raw material
[0137] Next, the lithium nickel-based oxide is mixed with a cobalt-containing raw material and subjected to secondary firing to form a cathode active material including a cobalt-containing coating layer.
[0138]
[0139] For example, the surface of the lithium nickel-based oxide is coated with a cobalt-containing raw material. The cobalt-containing raw material is Co(OH)2, CoOOH, Co(OCOCH3). 2· 4H2O, Co(NO3) 2· 6H2O, CoSO4, and Co(SO4) 2· 7H2O may be any one or more of them. Specifically, Co(OH)2 may be added to the lithium nickel-based oxide to form a cathode active material including a cobalt-containing coating layer.
[0140]
[0141] By forming a cobalt-containing coating layer on the surface of the lithium nickel-based oxide in this way, a larger amount of unstable Ni ions present on the surface of the positive electrode active material can be stabilized, thereby improving the stability of the positive electrode active material.
[0142]
[0143] The secondary firing can be performed at a temperature of 600°C to 700°C, preferably 630°C to 690°C, and more preferably 640°C to 690°C.
[0144] If the secondary firing temperature exceeds 700°C, cobalt may diffuse into the cathode active material, causing changes in the crystal structure of the cathode active material and altering the residual lithium content, which may adversely affect the lifespan and resistance characteristics of the cathode active material. In other words, it may be difficult to achieve the desired residual lithium content and cobalt-containing coating layer content.
[0145] When the secondary firing temperature is lower than 600°C, the cobalt-containing coating layer may detach from the positive electrode active material due to weak bonding with the positive electrode active material surface, and a coating layer with a lower cobalt content may be formed compared to when the secondary firing is performed within the above temperature range, so the effect of improving the high-temperature life characteristics may be minimal.
[0146]
[0147] The secondary firing can be performed for 2 to 8 hours, preferably 3 to 7 hours, and more preferably 4 to 6 hours.
[0148]
[0149] As a result of secondary firing by mixing lithium nickel-based oxide with cobalt-containing raw material within the above-mentioned firing temperature and firing time range, a cobalt-containing coating layer having a desired content is formed on the surface of the lithium nickel-based oxide, thereby enabling the implementation of a secondary battery having low initial resistance.
[0150]
[0151] A separate washing process may not be included between the first and second firings. Conventionally, a process was performed to wash away residual lithium present on the surface of the positive electrode active material. This is because, when residual lithium exists, side reactions with the electrolyte occur when applied to a battery, and there are problems such as increased gas generation during high-temperature storage. On the other hand, in the manufacturing method according to an embodiment of the present invention, since a separate washing process is not performed, residual lithium exists on the particle surface, and this residual lithium can react with cobalt to form a coating form of LiCoO2 on the particle surface, thereby realizing excellent high-temperature life characteristics.
[0152]
[0153] anode slurry
[0154] Next, the cathode slurry according to the present invention will be described.
[0155] The positive electrode slurry according to the present invention is characterized by comprising the positive electrode active material and binder according to the present invention.
[0156] Specifically, the positive electrode slurry according to the present invention may optionally include a conductive agent as needed. Specifically, the positive electrode slurry may be prepared by mixing a positive electrode active material, a binder, and / or a conductive agent in a solvent.
[0157]
[0158] The adsorption amount of the binder for the positive electrode active material according to the present invention is 25.0 mg / m 2 Below, preferably 10.0 mg / m 2 25.0 mg / m 2 , more preferably 15.0 mg / m 2 23.0 mg / m 2 It can be. When the adsorption amount of the binder for the positive electrode active material satisfies the above range, the viscosity of the slurry can be reduced and the phase stability of the slurry can be improved.
[0159]
[0160] According to the present invention, the viscosity change rate of the positive electrode slurry at 25°C, calculated using the following equation 1, may be 1,000% or less, preferably 800% or less, and more preferably 10% to 600%. When the viscosity change rate satisfies the above range, the phase stability of the slurry can be improved, and when applied to a battery, stable electrode production and improved yield can be achieved.
[0161] [Formula 1]
[0162]
[0163]
[0164] The above binder serves to improve the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylalcohol, polyacrylonitrile, polymethyl methacrylate, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, polyacrylic acid, and polymers in which hydrogens of these are substituted with Li, Na, or Ca, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The above binder may be included in an amount of 1 wt% to 30 wt%, preferably 1 wt% to 20 wt%, and more preferably 1 wt% to 10 wt%, based on the total solid content of the positive electrode slurry.
[0165]
[0166] The conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any particular limitation. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive tubes such as carbon nanotubes; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One type alone or a mixture of two or more types of the conductive material may be used. The conductive material may be included in an amount of 0.01 wt% to 10 wt%, 0.1 wt% to 9 wt%, or 0.1 wt% to 5 wt% based on the total solid content of the positive electrode slurry.
[0167]
[0168] The solvent may be a solvent generally used in the relevant technical field, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), dimethyl formamide (DMF), acetone, or water, and one of these may be used alone or as a mixture of two or more. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, binder, and conductive agent in consideration of the coating thickness and manufacturing yield of the positive electrode slurry, and to have a viscosity that can exhibit excellent thickness uniformity during subsequent coating for manufacturing the positive electrode.
[0169]
[0170] anode
[0171] The positive electrode according to the present invention comprises the positive electrode active material of the present invention described above. Specifically, the positive electrode comprises a positive electrode current collector, a positive electrode active material layer formed on the positive electrode current collector, and the positive electrode active material layer comprises a positive electrode slurry comprising the positive electrode active material of the present invention. Since the positive electrode active material and the positive electrode slurry have been described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.
[0172]
[0173] The positive electrode current collector may include a highly conductive metal, and is not particularly limited as long as it is a metal to which the positive electrode active material layer can be easily adhered, but is not reactive in the voltage range of the battery. The positive electrode current collector may be made of, for example, stainless steel, aluminum, nickel, titanium, heat-treated carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode current collector may typically have a thickness of 3 μm to 500 μm, and fine unevenness may be formed on the surface of the current collector to increase the adhesion of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0174]
[0175] The above positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the positive electrode active material described above is used. Specifically, the positive electrode slurry described above can be manufactured by applying it to a positive electrode current collector, followed by drying and rolling.
[0176] Alternatively, the positive electrode may be manufactured by casting the positive electrode slurry onto a separate support, then peeling the film from the support and laminating the resulting film onto a positive electrode current collector.
[0177]
[0178] lithium secondary battery
[0179] Next, a lithium secondary battery according to the present invention will be described.
[0180]
[0181] The lithium secondary battery specifically includes a positive electrode, a negative electrode positioned opposite the positive electrode, and a separator and electrolyte interposed between the positive electrode and the negative electrode. Since the positive electrode is the same as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.
[0182] In addition, the lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0183]
[0184] In the above lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.
[0185] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, heat-treated carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 ㎛ to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0186]
[0187] The above negative electrode active material layer optionally includes a binder and a conductive material together with the negative electrode active material.
[0188] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples thereof include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, and Al alloy; metallic oxides capable of doping and dedoping lithium, such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fibers, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature heat-treated carbon such as petroleum or coal tar pitch derived cokes.
[0189] The above negative electrode active material may be included in an amount of 80 wt% to 99 wt%, 82 wt% to 99 wt%, or 84 wt% to 99 wt% based on the total weight of the negative electrode active material layer.
[0190]
[0191] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and is typically added in an amount of 0.1 wt% to 10 wt% based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0192]
[0193] The conductive agent is a component for further improving the conductivity of the negative electrode active material, and may be included in an amount of 1 wt% to 30 wt%, 1 wt% to 20 wt%, or 1 wt% to 10 wt% based on the total weight of the negative electrode active material layer. The conductive agent is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; fluorinated carbon; metal powder such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0194]
[0195] The above negative electrode active material layer can be manufactured by applying and drying a negative electrode slurry composition prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, on a negative electrode current collector, or by casting the negative electrode slurry composition on a separate support, and then laminating the obtained film by peeling it off from the support on a negative electrode current collector.
[0196]
[0197] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in lithium secondary batteries can be used without special restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.
[0198]
[0199] In addition, examples of the electrolyte used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0200] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0201] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R represents a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.
[0202]
[0203] The above lithium salt can be used without any special limitation as long as it is a compound that can provide lithium ions used in a lithium secondary battery. Specifically, the anion of the above lithium salt is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - At least one selected from the group consisting of, and the lithium salt is LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2) 2. LiCl, LiI, or LiB(C2O4)2 can be used. The concentration of the lithium salt is preferably within the range of 0.1M to 4.0M, preferably 0.5M to 3.0M, and more preferably 1.0M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.
[0204]
[0205] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 10.0 wt% based on the total weight of the electrolyte.
[0206]
[0207] As described above, a lithium secondary battery including a cathode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0208] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.
[0209] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as power tools; electric vehicles including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); or power storage systems.
[0210]
[0211] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.
[0212]
[0213] Examples and Comparative Examples
[0214] Example 1 - Preparation of positive electrode active material
[0215] Ni, a precursor of positive electrode active material 0.93 Co 0.05 Mn 0.02 (OH)2 and lithium raw material LiOH were put into a 700 L Henschel mixer so that the molar ratio of Li: transition metal (Ni+Co+Mn) was 1.05:1 and mixed at 400 rpm in the center for 20 minutes. The mixed powder was put into an alumina crucible measuring 330 mm × 330 mm and calcined at 850°C for 12 hours in an oxygen atmosphere to obtain LiNi 0.93 Co 0.05 Mn 0.02 O2 was manufactured.
[0216] Afterwards, the primary calcined material was mixed with 12,000 ppm of Co(OH)2 so that the molar ratio of the primary calcined material to Co was 100:2, and then secondary calcination was performed at 680°C for 5 hours to manufacture a positive electrode active material powder having a cobalt-containing coating layer formed thereon.
[0217]
[0218] Example 2 - Preparation of positive electrode active material
[0219] A positive electrode active material powder was manufactured in the same manner as in Example 1, except that the primary calcined material was mixed with 18,000 ppm of Co(OH)2 so that the molar ratio of the primary calcined material to Co was 100:3, and then secondary calcined at 680°C for 5 hours.
[0220]
[0221] Example 3 - Preparation of positive electrode active material
[0222] A positive electrode active material powder was manufactured in the same manner as in Example 1, except that the secondary firing was performed at 660°C for 5 hours.
[0223]
[0224] Example 4 - Preparation of positive electrode active material
[0225] The positive electrode active material powder was prepared in the same manner as in Example 1.
[0226]
[0227] Example 5 - Preparation of positive electrode active material
[0228] The positive electrode active material powder was prepared in the same manner as in Example 1.
[0229]
[0230] Comparative Example 1 - Preparation of positive electrode active material
[0231] A positive electrode active material powder was manufactured in the same manner as in Example 1, except that the secondary firing was performed at 720°C for 5 hours.
[0232]
[0233] Comparative Example 2 - Preparation of positive electrode active material
[0234] A positive electrode active material powder was manufactured in the same manner as in Example 1, except that the secondary firing was performed at 800°C for 5 hours.
[0235]
[0236] Comparative Example 3 - Preparation of positive electrode active material
[0237] A positive electrode active material powder was manufactured in the same manner as in Example 1, except that the primary calcined material was mixed with 6,000 ppm of Co(OH)2 so that the molar ratio of the primary calcined material to Co was 100:1, and then secondary calcination was performed at 680°C for 5 hours.
[0238]
[0239] Comparative Example 4 - Preparation of positive electrode active material
[0240] A positive electrode active material was manufactured in the same manner as in Example 1, except that the first firing was performed at 850°C for 10 hours.
[0241]
[0242] Comparative Example 5 - Preparation of positive electrode active material
[0243] A positive electrode active material powder was manufactured in the same manner as in Example 1, except that the positive electrode active material precursor and the lithium raw material LiOH were placed in a Henschel mixer, mixed at 400 rpm in the center for 30 minutes, and then calcined for the first time at 950°C for 12 hours in an oxygen atmosphere.
[0244]
[0245] Experimental Example 1 - Particle size distribution of positive electrode active material
[0246] After dispersing 0.05 g of each of the positive electrode active materials manufactured in Examples 1 to 5 and Comparative Examples 1 to 5 in a dispersion medium H2O, the particles were introduced into a commercially available laser PSD (Particle Size Distribution) particle size measuring device (e.g., Microtrac S3500) and the difference in diffraction pattern according to particle size was measured when the particles passed through a laser beam to calculate the particle size distribution.
[0247] D 50 In the particle size distribution of the above-mentioned positive electrode active material, the particle size refers to the particle size at the point where the particle volume according to the particle size is 50%. The results are shown in Tables 1 and 2 below.
[0248]
[0249] Experimental Example 2 - Surface observation of positive electrode active material
[0250] Using a scanning electron microscope, SEM images of each of the positive electrode active material particles manufactured in Examples 1 to 3 and Comparative Examples 1 to 4 were obtained. These SEM images are shown in FIGS. 1 to 7.
[0251] Through FIGS. 1 to 3, it can be confirmed that the positive electrode active materials manufactured in Examples 1 to 3 have a cobalt-containing coating layer formed in a layered or island shape on the surface of the lithium nickel-based oxide.
[0252] On the other hand, through FIGS. 4 to 7, it can be confirmed that the positive electrode active materials manufactured in Comparative Examples 1 and 2 have a smooth surface because cobalt diffuses into the particles due to the high secondary firing temperature, and thus hardly any cobalt-containing coating layer is formed on the surface of the lithium nickel-based oxide. It can be confirmed that the positive electrode active material manufactured in Comparative Example 3 has a low content of cobalt-containing raw material, so hardly any cobalt-containing coating layer is formed. The positive electrode active material manufactured in Comparative Example 4 differs only in that the primary firing time is reduced compared to Examples 1 to 3, and it can be confirmed that a cobalt-containing coating layer is formed on the surface of the lithium nickel-based oxide.
[0253]
[0254] Experimental Example 3 - XPS Analysis of Positive Electrode Active Material
[0255] The Co / Ni ratio according to etching time was measured while etching from the surface to the center of the cobalt-containing coating layer included in the positive electrode active materials manufactured in Examples 1 to 3 and Comparative Examples 1 to 4 using a depth profile using X-ray photoelectron spectroscopy (XPS) (Thermo Fisher Scientific, Nexsa2 ESCA system). The measurement results are shown in Fig. 8.
[0256] Specifically, the positive electrode active material particles manufactured in Examples 1 to 3 and Comparative Examples 1 to 4 were introduced into a vacuum chamber and then measured under the following conditions.
[0257] - X-ray source: Monochromated Al Kα (1486.6eV)
[0258] - X-ray spot size: 400㎛
[0259] - Sputtering: monatomic Ar (energy: 1000eV, raster width: 2mm)
[0260] - Etching rate: 0.09 nm / s based on Ta2O5
[0261] - Operation mode: CAE (Constant Analyzer Energy) mode
[0262] - Survey scan: pass energy 200eV, energy step 1eV
[0263] - Narrow scan: scanned mode, pass energy 50eV, energy step 0.1eV
[0264] - Charge compensation: flood gun 2V, 250㎂
[0265]
[0266] Experimental Example 4 - Measurement of Residual Lithium Content in Positive Electrode Active Material
[0267] The residual lithium content of each positive electrode active material manufactured in Examples 1 to 3 and Comparative Examples 1 to 4 was measured. The measurement results are shown in Table 1 below.
[0268] The residual lithium content present on the surface of the positive electrode active material was measured through pH titration, using a T5 pH meter from Mettler Toledo. Specifically, 10 g of each of the positive electrode active material powders manufactured in Examples 1 to 3 and Comparative Examples 1 to 4 was stirred in 100 mL of distilled water for 5 minutes, and then a 0.1 N HCl solution was added to the solution, thereby performing pH titration.
[0269]
[0270] Experimental Example 5 - Measurement of adsorption amount with binder
[0271] <Preparation of slurry for measuring adsorption amount>
[0272] The positive electrode active materials and PVdF binder (KF9700) manufactured in Examples 1 to 3 and Comparative Examples 1 to 4, respectively, were mixed in a weight ratio of 98.11:1.89 to prepare a slurry for measuring adsorption amount having a solid content of 76.2 wt%. Specifically, the slurry for measuring adsorption amount was manufactured by mixing under dry room conditions at 45°C and a speed of 2500 rpm for 6 hours.
[0273] The slurry for measuring the above adsorption amount was centrifuged, and the solids content of the supernatant liquid was measured. The adsorption amount with the binder was calculated using a TA instruments Rheometer based on the viscosity master curve for each solids content of the binder / slurry. The calculation results are shown in Table 1 below.
[0274]
[0275] As shown in Table 1, the adsorption amount of the binder of the positive electrode active materials manufactured in Examples 1 to 3 is at a level equivalent to that of the positive electrode active material manufactured in Comparative Example 3, but it can be confirmed to be lower than that of the positive electrode active materials manufactured in Comparative Examples 1 to 2 and 4.
[0276]
[0277] Experimental Example 6 - Viscosity Measurement of Positive Slurry
[0278] <Manufacturing of positive electrode slurry>
[0279] The positive electrode active materials manufactured in Examples 1 to 3 and Comparative Examples 1 to 3, respectively, polyvinylidene fluoride (PVdF) (KF9700, Solef5130) as a binder, nitrile butadiene rubber (H-NBR) (HPD01) as a dispersant, carbon black (B.CNT, SFG6L) as a conductive material, and single-walled carbon nanotubes were mixed in a weight ratio of 97.02:1.87:0.002:0.18:0.60:0.30:0.01 to manufacture a positive electrode slurry having a solid content of 67 wt%.
[0280] Specifically, the slurry for viscosity measurement was prepared by mixing at 45°C and 2500 rpm for 75 minutes under dry room conditions.
[0281]
[0282] The viscosity of each cathode slurry was measured using a viscosity measuring device (TA Instruments Rheometers). The measurement results are shown in Table 1 below.
[0283]
[0284] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4D 50 (㎛)4.123.743.784.215.424.274.05LiOH content (wt%)0.100.070.100.100.280.100.35Adsorption amount (mg / m 2 )23.019.322.325.029.222.933.4Slurry viscosity (cP)Initial viscosity (cP)4,6964,7406,1156,2153,5133,7843,9562Viscosity after standing for 2 days (cP)7,12331,0528,384109,000(gelled)211,440(gelled)195,000(gelled)204,560(gelled)Viscosity change rate (%)53555371,6545,9185,0535,078
[0285] As shown in Table 1, it was confirmed that the viscosity change rate of the positive electrode active materials manufactured in Examples 1 to 3 was very low compared to the positive electrode active materials manufactured in Comparative Examples 1 to 4.
[0286] Experimental Example 6 - Analysis of Electrochemical Characteristics of Lithium Secondary Batteries
[0287] The initial efficiency, initial resistance, and high-temperature life characteristics of lithium secondary battery half cells manufactured as described above using each of the positive electrode active materials manufactured in Examples 4 to 5 and Comparative Example 5 were analyzed. The analysis results are shown in Table 2 below.
[0288]
[0289] <Manufacturing of Lithium Secondary Batteries>
[0290] The positive electrode active material, conductive agent (Carbon Black, Denka), and PVDF binder manufactured in Examples 4 to 5 and Comparative Example 5, respectively, were mixed in N-methylpyrrolidone at a weight ratio of 95:2:3 to manufacture a positive electrode slurry. The positive electrode slurry was applied to one surface of an aluminum current collector, dried at 500°C, and then rolled to manufacture a positive electrode.
[0291] Lithium metal was used as the cathode.
[0292] An electrode assembly was manufactured by interposing a separator between the positive and negative electrodes manufactured by the above-described method, and then positioning it inside a battery case, and then injecting an electrolyte into the case to manufacture a battery cell. The electrolyte was manufactured by dissolving 0.6 M LiPF6 in a mixed organic solvent of ethylene carbonate (EC): dimethyl carbonate (DMC): ethyl methyl carbonate (EMC) = 1:2:1 by volume, and adding 2 wt% of vinylene carbonate (VC).
[0293]
[0294] <Analysis of initial efficiency, initial resistance, and high-temperature life characteristics>
[0295] Charging and discharging were performed on the lithium secondary battery manufactured as described above.
[0296]
[0297] Specifically, the initial efficiency was determined by performing a single charge-discharge cycle at 25°C in CC-CV mode, charging at 0.2C to 4.25 V and discharging at 0.2C to 2.5 V. The initial efficiency was derived by the following calculation.
[0298] Initial efficiency (%) = (discharge capacity per charge / discharge / charge capacity per charge / discharge) x 100
[0299]
[0300] Specifically, the initial resistance was calculated based on the discharge capacity measured at 0.2C for one charge / discharge cycle, and the voltage change rate when a current of 1.0C is applied for 10 seconds after setting SOC.95% at 0.2C for two charge / discharge cycles. In addition, the voltage change rate was calculated after setting SOC.50% for two charge / discharge cycles and the voltage change rate after setting SOC.10% for two charge / discharge cycles.
[0301]
[0302] Specifically, the high-temperature life characteristics were evaluated by measuring the capacity retention rate after performing 50 charge-discharge cycles, each of which was charged to 4.25 V at 0.5 C and discharged to 2.5 V at 1.0 C in CC-CV mode at 45°C. The capacity retention rate was derived by the following calculation.
[0303] Capacity retention rate (%) = (discharge capacity after n charge / discharge cycles / discharge capacity after 1 charge / discharge cycle) x 100
[0304]
[0305] Example 4 Example 5 Comparative Example 5D 50 (㎛)3.965.647.41Initial Efficiency (%)90.588.387.7Initial Resistance (Ω)SoC.951.431.591.64SoC.501.411.471.53SoC.101.691.852.01Capacity Retention (%)88.887.783.6
[0306] As shown in Table 2, D 50 A lithium secondary battery including the positive electrode active material of Comparative Example 5 exceeding 6.0㎛ is D 50 It can be confirmed that the lithium secondary battery including the positive electrode active material of Examples 4 to 5 having a diameter of 3.7 μm to 6.0 μm has lower initial efficiency, higher initial resistance, and lower capacity retention rate. D 50It is believed that the cathode active material exceeding 6.0㎛ exhibits decreased lithium mobility due to the increased intraparticle diffusion distance of lithium ions, thereby increasing the initial resistance of lithium secondary batteries containing it. Furthermore, it is believed that the increased charge transfer resistance and diffusion resistance result in poor initial efficiency and capacity retention.
Claims
1. A cathode active material comprising a lithium nickel-based oxide containing nickel (Ni) and cobalt (Co), wherein the molar ratio of Ni among the total transition metals is 80 mol% or more; and a cobalt-containing coating layer formed on the surface of the lithium nickel-based oxide. The above lithium nickel oxide is in the form of a single particle consisting of one single nodule or a quasi-single particle complex consisting of 30 or fewer nodules, The cobalt-containing coating layer is included in an amount of 2.0 mol% or more with respect to 100 mol of the lithium nickel-based oxide, The above positive electrode active material is D 50 A cathode active material having a diameter of 3.7 μm to 6.0 μm, a residual LiOH content of 0.20 wt% or less, and a Co / Ni ratio of 0.15 to 0.40 at a depth of 45 nm from the surface.
2. In claim 1, The above lithium nickel oxide is a positive electrode active material in which the molar ratio of Ni among the total transition metals is 93 mol% or more.
3. In claim 1, The above positive electrode active material is a positive electrode active material having a residual lithium content of 0.60 wt% or less.
4. In claim 1, The above positive electrode active material is a positive electrode active material having a residual Li2CO3 content of 0.40 wt% or less.
5. In claim 1, The above positive electrode active material is D min This positive electrode active material is 1.0㎛ or larger.
6. In claim 1, The above lithium nickel-based oxide is a positive electrode active material represented by the following chemical formula 1. [Chemical Formula 1] Li a Ni b Co c M 1 d M 2 e O2 In the above chemical formula 1, M 1 is at least one selected from the group consisting of Mn and Al, and M 2 is at least one selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb, and Mo, and 1.0≤a≤1.5, 0.8≤b≤1.0, 0≤c≤0.2, 0≤d≤0.2, 0≤e≤0.
1.
7. A cathode slurry comprising the cathode active material and binder of any one of claims 1 to 6 above.
8. In claim 7, The adsorption amount of the binder to the positive electrode active material is 25.0 mg / m 2 Below is the positive electrode slurry.
9. In claim 7, A cathode slurry having a viscosity change rate of 1,000% or less calculated by the following equation 1 at 25°C. [Formula 1] 10. A step of forming a lithium nickel-based oxide by mixing a lithium nickel-based transition metal hydroxide precursor containing nickel (Ni) and cobalt (Co) and a lithium raw material and performing a first calcination; and A method for manufacturing a positive electrode active material, comprising the step of mixing the lithium nickel-based oxide with a cobalt-containing raw material and performing a second firing to form a positive electrode active material including a cobalt-containing coating layer; The above positive electrode active material includes a lithium nickel-based oxide having a molar ratio of Ni of 80 mol% or more among the total transition metals, and a cobalt-containing coating layer formed on the surface of the lithium nickel-based oxide. The above lithium nickel oxide is in the form of a single particle consisting of one single nodule or a quasi-single particle complex of 30 or fewer nodules, and the positive electrode active material is D 50 This is 3.7㎛ to 6.0㎛, the residual LiOH content is 0.20 wt% or less, and the cobalt-containing coating layer is included in an amount of 2.0 mol% or more with respect to 100 mol of the lithium nickel-based oxide, A method for manufacturing a positive electrode active material, wherein the above secondary firing is performed at 600°C to 700°C.
11. In claim 10, The above cobalt-containing raw materials are Co(OH)2, CoOOH, Co(OCOCH3) 2· 4H2O, Co(NO3) 2· 6H2O, CoSO4, and Co(SO4) 2· A method for producing a positive electrode active material comprising at least one selected from the group consisting of 7H2O.
12. In claim 10, A method for manufacturing a positive electrode active material, wherein the above primary firing is performed at 750°C to 880°C.
13. A positive electrode comprising the positive electrode active material of any one of claims 1 to 6.
14. A lithium secondary battery comprising the positive electrode of claim 13.
Citation Information
Patent Citations
Manufacuring method of cathode active material for lithium rechargeable battery, and cathode active material made by the same
KR101567039B1
Positive active material for rechargeable lithium battery, method for manufacturing the same, and rechargeable lithium battery including the same
KR1020180057864A
Mask assembly with moisture absorbing and aroma function
KR1020220025975A
Hemostatic agent with film and method for preparing thereof
KR1020230164270A
Single-crystal high-nickel positive electrode material and preparation method therefor and application thereof