Water-soluble dispersant, preparation method therefor, and use thereof
The water-soluble dispersant prepared by compounding polyether modified polymers and polyamide polymers has solved the problems of traditional dispersed dye stability and environmental pollution, achieved efficient and environmentally friendly dye dispersion effect, and reduced production costs.
Patent Information
- Application Number
- PCT/CN2023/105169
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2023-06-30
- Publication Date
- 2024-11-14
AI Technical Summary
Traditional dispersing dyes require a large amount of dispersing additives when dispersing, resulting in short stability cycle, serious environmental pollution, high production costs, and difficult to preserve for a long time.
The water-soluble dispersant is prepared by combining polyether modified polymer A and polyamide polymer B. By controlling the proportion of polymer monomers and functional group structure, the wetting, anti-sinking and anti-flocculation of the dispersant is improved. , reduce the amount of dispersant used, save energy consumption, and improve the stability of dye dispersion.
It significantly improves the stability and use performance of dye dispersion, reduces the use of dispersant, reduces environmental pollution, extends the storage cycle of the dispersion system, and improves dyeing rate and production efficiency.
Smart Images

Figure PCTCN2023105169-FTAPPB-I100001 
Figure PCTCN2023105169-FTAPPB-I100002 
Figure PCTCN2023105169-FTAPPB-I100003
Abstract
Description
A water-soluble dispersant and its preparation method and application Technical Field
[0001] The embodiments of the present application belong to the technical field of color paste additives, such as a water-soluble dispersant and its preparation method and application. Background Art
[0002] Dispersant is a surfactant that has two opposite properties, lipophilicity and hydrophilicity, in its molecule. It can evenly disperse the solid and liquid particles of inorganic and organic pigments that are difficult to dissolve in liquids. It can also prevent the sedimentation and aggregation of particles, forming the amphiphilic reagent required for a stable suspension.
[0003] Disperse dyes have a small molecular structure, do not contain water-soluble groups, and only contain polar groups. Their water solubility is extremely low. When used, they must be assisted by a dispersant to form a uniform dispersion.
[0004] Traditional disperse dyes are added with large amounts of lignin salts, naphthalenesulfonates and other dispersing aids during dispersion. The amount of these dispersing aids added during dispersion is relatively large, ranging from 70% to 150% of the dye. In addition, the liquid disperse dye slurry is difficult to store for a long time due to its short stability period. The high amount of dispersant added leads to the presence of a large amount of organic pollutants in the printing and dyeing wastewater, causing difficulties in treatment and serious environmental damage.
[0005] CN114644762A discloses a kind of multiple modified lignin dye dispersant and preparation method thereof, with industrial alkali lignin as raw material, under alkaline conditions, with sulfonating agent 1, sulfonating agent 2 as sulfonating agent system, introduce sulfonic acid group simultaneously at different sites, can greatly improve the content of hydrophilic group sulfonic acid group.Then selectively add blocking agent, reduce residual hydroxyl content, while improving molecular weight.This multiple modified lignin sulfonate can be applied to dye dispersant, the disperse dye system with good dispersibility and excellent high temperature stability that can be obtained without grinding, and it has extremely low staining property, has lower reduction rate to azo dyes, can significantly improve dye uptake rate simultaneously, can greatly reduce the production cost of printing and dyeing industry.But the dispersant of this application is added in a higher ratio when used for disperse dye.
[0006] Therefore, it is desirable in the art to develop a water-soluble dispersant for dye dispersion.
[0007] Summary of the Invention
[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0009] The present application embodiment provides a kind of water-soluble dispersant and its preparation method and application. Compared with the traditional small molecule dye dispersant with a single anchoring group and a wetting group, the water-soluble dispersant provided by the present application contains aromatic, carboxylic acid ester, carboxylic acid pigment-friendly groups, has good wettability, excellent anti-settling property, anti-flocculation and the ability of floating color and flowery color, its structural modification is strong, the raw material source is rich, and it is applicable to many pigment dispersion fields. The water-soluble dispersant provided by the present application can control the microscopic electrostatic repulsion, multi-point adsorption capacity, solvation chain effect and steric hindrance of the dispersant by controlling the ratio of polymer unit monomers, controlling the degree of polymerization of the polymer, regulating and controlling the structural type, quantity, distribution density, etc. of the functional group, so as to ensure the wettability, anti-settling property, anti-flocculation and other properties of the dispersant.
[0010] Compared with traditional dye dispersants, the water-soluble dispersant provided in this application can not only reduce the amount of dispersant added, save processing equipment and processing energy consumption, and reduce environmental pollution; but also the slurry is evenly dispersed and has good stability, thereby significantly improving the final use performance of the dispersion system.
[0011] In a first aspect, an embodiment of the present application provides a water-soluble dispersant, wherein the water-soluble dispersant comprises a polyether-modified polymer A and a polyamide-based polymer B;
[0012] The raw materials for preparing the polyether-modified polymer A include vinylbenzene monomers, allyl succinic anhydride, active macromonomer polyether and alkyl monoalcohol;
[0013] The polyamide-based high molecular polymer B includes a homopolymer of vinyl pyrrolidone and / or a copolymer of vinyl pyrrolidone.
[0014] The present application provides a water-soluble dispersant obtained by compounding a polyether-modified polymer A and a polyamide-based high molecular polymer B, wherein the polyether-modified polymer A, under the initiation of a peroxide initiator, uses bulk free radical polymerization to initiate polymerization of vinylbenzene monomers, allyl succinic anhydride, and active macromonomer polyether to obtain a prepolymer product, and an alkyl monool, under the action of an acid catalyst, esterifies and ring-opens the anhydride groups in the prepolymer product to form carboxylate and carboxylic acid groups, thereby obtaining the polyether-modified polymer A; the polyether-modified polymer A is a comb-shaped structure polymer containing multiple characteristic functional groups, the active macromonomer polyether provides hydrophilic chain segments on the polymer side chains, the conjugated effect of the benzene ring groups contained in the vinylbenzene monomers provides an affinity anchoring effect on the dye groups, and the anhydride groups, which are ring-esterified by the alkyl monool, simultaneously provide carboxylate functional groups with pigment affinity, as well as ionized carboxylic acid groups that have wetting effects on dye particles and electrostatic repulsion effects. The composite system of polyether-modified polymer A and polar polyamide polymer B diversifies the types of functional groups in the water-soluble dispersant system, improves the wetting and protective effects of the dispersant on disperse dye particles, and improves the grinding efficiency of disperse dyes, the proportion of dye particles in the slurry, and the stability of the slurry.
[0015] Preferably, the active macromonomer polyether is prepared by the following preparation method:
[0016] Adding polyetheramine and allyl succinic anhydride into the reactor, raising the temperature and keeping the temperature until no water is distilled out during the reaction, thereby obtaining the active macromonomer polyether.
[0017] Preferably, the polyetheramine is a monoprimary amino polyether in which the terminal hydroxyl group is converted into an amine by using a monoalcohol as an initiator to initiate the self-polymerization of ethylene oxide or the copolymerization of ethylene oxide and propylene oxide.
[0018] Preferably, the weight average molecular weight of the polyetheramine is 500 to 2500 g / mol, for example, 500 g / mol, 800 g / mol, 1000 g / mol, 1300 g / mol, 1500 g / mol, 1800 g / mol, 2000 g / mol, 2300 g / mol or 2500 g / mol.
[0019] Preferably, the polyetheramine includes any one of JEFFAMINE M-2070, JEFFAMINE M-1000 or JEFFAMINE M-600, or a combination of at least two thereof.
[0020] Preferably, the molar ratio of the polyetheramine to allylsuccinic anhydride is (0.5-1.5):1, for example, 0.5:1, 1:1 or 1.5:1, and preferably 1:1. It should be noted that the allylsuccinic anhydride herein only includes the allylsuccinic anhydride used in the preparation of the active macromonomer polyether, and does not include the allylsuccinic anhydride directly used in the preparation of the polyether-modified polymer A.
[0021] Preferably, the temperature is raised to 120-160°C, such as 120°C, 130°C, 140°C, 150°C or 160°C.
[0022] Preferably, the insulation time is 2 to 6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.
[0023] Preferably, the preparation process of the reactive macromonomer polyether is carried out under the protection of an inert gas.
[0024] Preferably, the reactive macromonomer polyether has a structure as shown in the following formula I:
[0025] wherein R1 is hydrogen or methyl, R2 is methyl, ethyl, propyl or butyl, m is an integer from 10 to 60, such as 10, 15, 20, 25, 30, 35, 40, 45, 50, 55 or 60, and n is an integer from 0 to 15, such as 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15.
[0026] Preferably, the vinylbenzene monomer includes any one of styrene, β-methylstyrene, allylbenzene, 3-methylstyrene, 2-methylstyrene or 2-isopropenyltoluene, or a combination of at least two thereof.
[0027] Preferably, the alkyl monoalcohol includes any one of methanol, ethanol, propanol, n-butanol, isopropanol, isobutanol or tert-butanol, or a combination of at least two thereof.
[0028] Preferably, the mass ratio of the vinylbenzene monomer, allyl succinic anhydride, and reactive macromonomer polyether is (2-10):(5-20):(30-80), for example, 2:5:30, 10:20:80, or 5:10:50. It should be noted that the allyl succinic anhydride herein only includes the allyl succinic anhydride directly used in the preparation of the polyether-modified polymer A, and does not include the allyl succinic anhydride used in the preparation of the reactive macromonomer polyether.
[0029] Preferably, the molar ratio of the alkyl monoalcohol to the allyl succinic anhydride is (0.1-1):1, for example, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1 or 1:1, and preferably 1:1. It should be noted that the allyl succinic anhydride herein also only includes the allyl succinic anhydride directly used in the preparation of the polyether-modified polymer A, and does not include the allyl succinic anhydride used in the preparation of the reactive macromonomer polyether.
[0030] Preferably, the raw materials for preparing the polyether-modified polymer A also include an initiator and a catalyst.
[0031] Preferably, the initiator comprises any one or a combination of at least two of benzoyl peroxide, tert-butyl benzoyl peroxide, methyl ethyl ketone peroxide, dicumyl peroxide, di-tert-butyl peroxide or 2,2-bis(tert-butyl peroxide)butane.
[0032] Preferably, the catalyst comprises any one of p-toluenesulfonic acid, sulfuric acid, propionic acid, aminosulfonic acid or hydrochloric acid, or a combination of at least two thereof.
[0033] Preferably, the raw materials for preparing the polyether-modified polymer A include the following components in parts by weight:
[0034] Preferably, the raw materials for preparing the polyether-modified polymer A are calculated by weight, and the amount of the vinylbenzene monomer used can be 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts or 20 parts, etc.
[0035] Preferably, the amount of allylsuccinic anhydride used in the preparation of the polyether-modified polymer A can be 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts or 40 parts by weight.
[0036] Preferably, the raw materials for preparing the polyether-modified polymer A are calculated in parts by weight, and the amount of the active macromonomer polyether used can be 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, 95 parts, 100 parts, 105 parts, 110 parts, 115 parts, 120 parts, 125 parts, 130 parts, 135 parts, 140 parts, 145 parts, 150 parts, 155 parts or 160 parts, etc.
[0037] Preferably, the raw materials for preparing the polyether-modified polymer A have a molar ratio of alkyl monoalcohol to allyl succinic anhydride of 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1 or 1:1, etc., calculated by weight.
[0038] Preferably, the amount of the initiator used in the preparation of the polyether-modified polymer A can be 0.5 parts, 1 part, 1.5 parts or 2 parts by weight.
[0039] Preferably, the amount of the catalyst used in the preparation of the polyether-modified polymer A can be 1 part, 2 parts or 3 parts by weight.
[0040] Preferably, the weight average molecular weight of the polyether modified polymer A is 5000-100000 g / mol, for example, 5000 g / mol, 8000 g / mol, 10000 g / mol, 20000 g / mol, 30000 g / mol, 40000 g / mol, 50000 g / mol, 60000 g / mol, 70000 g / mol, 80000 g / mol, 90000 g / mol or 100000 g / mol, etc., preferably 20000-60000 g / mol.
[0041] Preferably, the weight average molecular weight of the polyamide polymer B is 2000-100000 g / mol, for example, 2000 g / mol, 5000 g / mol, 8000 g / mol, 10000 g / mol, 20000 g / mol, 30000 g / mol, 40000 g / mol, 50000 g / mol, 80000 g / mol or 100000 g / mol, etc., preferably 10000-50000 g / mol.
[0042] Preferably, the polyamide polymer B includes any one of PVPK25, PVPK30, PVPK35 or copovidone VA64, or a combination of at least two thereof.
[0043] Preferably, the mass ratio of the polyether modified polymer A to the polyamide polymer B is (7-22):(4-7), for example, 7:4, 7:6, 7:7, 15:4, 15:6, 15:7, 22:4, 22:6 or 22:7.
[0044] Preferably, the water-soluble dispersant further includes deionized water and a pH regulator.
[0045] Preferably, the pH adjuster includes any one or a combination of at least two of sodium hydroxide, potassium hydroxide, monoethanolamine, diethanolamine, triethanolamine, 2-amino-2-methyl-1-propanol or N,N-dimethylethanolamine, preferably sodium hydroxide and / or potassium hydroxide.
[0046] Preferably, the raw materials for preparing the water-soluble dispersant include the following components in parts by weight:
[0047] Preferably, the raw materials for preparing the water-soluble dispersant are calculated in parts by weight, and the amount of polyether-modified polymer A used can be 70 parts, 80 parts, 90 parts, 100 parts, 110 parts, 120 parts, 130 parts, 140 parts, 150 parts, 160 parts, 170 parts, 180 parts, 190 parts, 200 parts, 210 parts or 220 parts, etc.
[0048] Preferably, the amount of the polyamide polymer B used in the preparation of the water-soluble dispersant can be 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts or 70 parts by weight.
[0049] Preferably, the raw materials for preparing the water-soluble dispersant are calculated by weight, and the amount of deionized water used can be 80 parts, 90 parts, 100 parts, 110 parts, 120 parts, 130 parts, 140 parts, 150 parts, 160 parts, 170 parts, 180 parts, 190 parts or 200 parts, etc.
[0050] In a second aspect, the present invention provides a method for preparing the water-soluble dispersant according to the first aspect, the method comprising the following steps:
[0051] (1) adding a formulated amount of active macromonomer polyether into a reactor, raising the temperature, then adding vinylbenzene monomer, allyl succinic anhydride, and an optional initiator, and keeping the temperature for reaction, then sequentially adding an alkyl monoalcohol and an optional catalyst, and keeping the temperature for reaction again, sampling and testing every 30 minutes until the difference in the acid value of the system between two adjacent times is ≤2 mgKOH / g, terminating the reaction, and obtaining the polyether-modified polymer A;
[0052] (2) Cooling the polyether-modified polymer A obtained in step (1), then adding optional deionized water and polyamide polymer B, and then adding an optional pH regulator, stirring to obtain the water-soluble dispersant.
[0053] Preferably, the heating in step (1) is to 100-150°C, for example, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C.
[0054] Preferably, when adding the vinylbenzene monomer, allylsuccinic anhydride and optional initiator in step (1), these three raw materials are first prepared into a mixed solution and then added dropwise, and the addition time is controlled to be 2 to 8 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours.
[0055] Preferably, the temperature of the insulation reaction in step (1) is 100-150°C, for example, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, and the insulation reaction time is 1-3 hours, for example, 1 hour, 2 hours or 3 hours.
[0056] Preferably, the temperature of the second insulation reaction in step (1) is 100-150°C, for example, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, and the time of the second insulation reaction is 2-10 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours, etc.
[0057] Preferably, the acid value in step (1) is measured by titration using neutral ethanol as solvent and standard sodium hydroxide or potassium hydroxide solution as neutralizing titrant.
[0058] It should be noted that the difference between the two adjacent system acid values in step (1) refers to the difference between the larger value and the smaller value measured twice in succession, which is ≤2 mgKOH / g.
[0059] Preferably, both step (1) and step (2) are carried out under the protection of an inert gas.
[0060] Preferably, the cooling in step (2) is cooling to 50-60°C, such as 50°C, 55°C or 60°C.
[0061] In a third aspect, an embodiment of the present application provides a use of the water-soluble dispersant as described in the first aspect in dye dispersion.
[0062] Compared with the related art, the embodiments of the present application have at least the following beneficial effects:
[0063] In the embodiments of the present application, vinylbenzene monomers, allyl succinic anhydride, and active macromonomer polyethers are subjected to bulk free radical polymerization and then esterified with alkyl monoalcohols to obtain polyether-modified polymer A. The polyether-modified polymer A and polyamide-based high molecular polymer B are compounded to obtain a water-soluble dispersant. The types of functional groups in the system of the water-soluble dispersant are more diversified, which improves the wetting and protective effects of the dispersant on the disperse dye particles, thereby improving the grinding efficiency of the disperse dye, the proportion of dye particles in the slurry, and the stability of the slurry.
[0064] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION
[0065] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0066] Preparation Example 1
[0067] In this preparation example, a reactive macromonomer polyether is provided, and the preparation method comprises the following steps:
[0068] 200 g of polyetheramine JEFFAMINE M-2070 and 14 g of allyl succinic anhydride (molar ratio of 1:1) were added to a reaction flask protected by N2, and the temperature was raised to 120°C and kept warm for 6 hours until anhydrous water was distilled off during the reaction to obtain the active macromonomer polyether, which was recorded as a1.
[0069] Preparation Example 2
[0070] In this preparation example, a reactive macromonomer polyether is provided, and the preparation method comprises the following steps:
[0071] 200 g of polyetheramine JEFFAMINE M-1000 and 28 g of allyl succinic anhydride (molar ratio of 1:1) were added to a reaction flask protected by N2, and the temperature was raised to 160°C and kept warm for 2 hours until anhydrous water was distilled off during the reaction to obtain the active macromonomer polyether, recorded as a2.
[0072] Comparative Preparation Example 1
[0073] The only difference between this comparative preparation example and preparation example 1 is that allyl succinic anhydride is replaced by an equimolar amount of maleic anhydride, and the obtained polyether is recorded as D-a1.
[0074] Example 1
[0075] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:
[0076] (1) Add 60 parts by weight of active macromonomer polyether a1 into a reaction flask protected by N2, stir and heat to 100°C; uniformly dropwise add a mixture of 20 parts of styrene, 15 parts of allyl succinic anhydride, and 0.5 parts of benzoyl peroxide, and complete the addition within 3 hours. After the addition is complete, heat and react at 100°C for 1 hour, maintain the temperature in the flask at 100°C, add 7.9 parts of n-butanol and 1 part of p-toluenesulfonic acid in order by weight, heat and react for 6 hours, sample and test every 30 minutes, and terminate the reaction until the difference in the acid value of the system between two adjacent times is ≤2 mgKOH / g to obtain a polyether-modified polymer A;
[0077] (2) 90 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, cooled to 60°C, and then 120 parts of deionized water and 40 parts of PVPK30 were added. Potassium hydroxide was then added to adjust the pH value of the system to 8.5, and the mixture was stirred evenly to obtain the water-soluble dispersant.
[0078] Example 2
[0079] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:
[0080] (1) Add 120 parts by weight of active macromonomer polyether a2 into a reaction flask protected by N2, stir and heat to 110°C; uniformly add a mixture of 4 parts of allylbenzene, 20 parts of allylsuccinic anhydride and 0.8 parts of benzoyl peroxide, and complete the addition within 2 hours. After the addition is completed, keep the mixture at 110°C for 1 hour, maintain the temperature in the flask at 110°C, add 3.3 parts of ethanol and 1.2 parts of sulfuric acid in order by weight, keep the mixture for 1 hour, take samples every 30 minutes for testing, and terminate the reaction until the difference in the acid value of the system is ≤2 mgKOH / g for two consecutive times to obtain a polyether-modified polymer A;
[0081] (2) 130 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, cooled to 60°C, and then 100 parts of deionized water and 45 parts of PVPK35 were added. Then, sodium hydroxide was added to adjust the pH value of the system to 7.5, and stirred evenly to obtain the water-soluble dispersant.
[0082] Example 3
[0083] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:
[0084] (1) 80 parts of active macromonomer polyether a1 weighed in parts by weight were added to a reaction flask protected by N2, and the temperature was raised to 125°C with stirring; a mixture of 10 parts of 2-methylstyrene, 30 parts of allylsuccinic anhydride, and 1.8 parts of tert-butyl benzoyl peroxide was evenly added dropwise, and the addition was completed within 8 hours. After the addition was completed, the mixture was kept warm at 125°C for 2 hours, and the temperature in the flask was maintained at 125°C. 6.9 parts of methanol and 1.6 parts of aminosulfonic acid were added in sequence by weight, and the mixture was kept warm for 2 hours. Samples were taken every 30 minutes for testing, and the difference in the acid value of the system between two adjacent samples was ≤2 mgKOH / g. The reaction was terminated to obtain a polyether-modified polymer A;
[0085] (2) 110 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, and the mixture was cooled to 60°C. 160 parts of deionized water and 60 parts of povidone VA64 were then added, followed by potassium hydroxide to adjust the pH value of the system to 10, and the mixture was stirred evenly to obtain the water-soluble dispersant.
[0086] Example 4
[0087] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:
[0088] (1) 140 parts of active macromonomer polyether a2 weighed by weight were added to a reaction flask protected by N2, and the temperature was raised to 145°C with stirring; a mixed solution containing 15 parts of styrene, 25 parts of allyl succinic anhydride, and 1.5 parts of di-tert-butyl peroxide was evenly added dropwise, and the addition was completed within 7 hours. After the addition was completed, the mixture was kept at 145°C for 2 hours, and the temperature in the flask was maintained at 145°C. 10.7 parts of isopropyl alcohol and 2.6 parts of p-toluenesulfonic acid were added in sequence by weight, and the mixture was kept at this temperature for 8 hours. Samples were taken every 30 minutes for detection, and the difference in the acid value of the system between two adjacent samples was ≤2 mgKOH / g. The reaction was terminated to obtain a polyether-modified polymer A;
[0089] (2) 160 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, cooled to 60°C, and then 155 parts of deionized water and 70 parts of PVPK30 were added. Then, sodium hydroxide was added to adjust the pH value of the system to 8.5, and the mixture was stirred evenly to obtain the water-soluble dispersant.
[0090] Example 5
[0091] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:
[0092] (1) 160 parts of active macromonomer polyether a1 weighed by weight were added to a reaction flask protected by N2, and the temperature was raised to 115°C with stirring; a mixed solution containing 17 parts of styrene, 35 parts of allyl succinic anhydride, and 2 parts of benzoyl peroxide was evenly added dropwise and the addition was completed within 5 hours. After the addition was completed, the mixture was kept at 115°C for 2.5 hours, and the temperature in the flask was maintained at 115°C. 18.5 parts of tert-butyl alcohol and 2.8 parts of hydrochloric acid were added in sequence by weight, and the mixture was kept at this temperature for 6 hours. Samples were taken every 30 minutes for testing, and the difference in the acid value of the system between two adjacent samples was ≤2 mgKOH / g. The reaction was terminated to obtain a polyether-modified polymer A;
[0093] (2) Add 210 parts by weight of the polyether-modified polymer A obtained in step (1) into a reaction flask protected by N2, cool to 60°C, then add 175 parts of deionized water and 50 parts of PVPK35, and then add potassium hydroxide to adjust the pH value of the system to 9.5, stir evenly, and obtain the water-soluble dispersant.
[0094] Example 6
[0095] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:
[0096] (1) Add 50 parts by weight of active macromonomer polyether a1 and 50 parts by weight of active macromonomer polyether a2 into a reaction flask protected by N2, stir and heat to 130°C; uniformly dropwise add a mixed solution containing 9 parts of 3-methylstyrene, 40 parts of allylsuccinic anhydride and 1.2 parts of dicumyl peroxide, and complete the dropwise addition within 6 hours. After the dropwise addition is completed, heat and react at 130°C for 3 hours, maintain the temperature in the flask at 130°C, add 9.1 parts of methanol and 3 parts of propionic acid in sequence by weight, heat and react for 4 hours, sample and test every 30 minutes, and terminate the reaction until the difference in the acid value of the system is ≤2 mgKOH / g for two consecutive times to obtain a polyether-modified polymer A;
[0097] (2) 140 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, and the mixture was cooled to 60°C. 200 parts of deionized water and 70 parts of PVPK30 were then added, and then sodium hydroxide was added to adjust the pH value of the system to 7.5. The mixture was stirred evenly to obtain the water-soluble dispersant.
[0098] Example 7
[0099] The only difference between this embodiment and embodiment 1 is that the weight portion of the reactive macromonomer polyether a1 in step (1) is 50 parts.
[0100] Example 8
[0101] The only difference between this embodiment and embodiment 5 is that the weight portion of the reactive macromonomer polyether a1 in step (1) is 170 parts.
[0102] Comparative Example 1
[0103] The only difference between this comparative example and Example 1 is that the active macromonomer polyether a1 in step (1) is replaced by allyl polyether APEG2400 in equal parts by weight.
[0104] Comparative Example 2
[0105] The only difference between this comparative example and Example 1 is that the vinylbenzene monomer (styrene) in step (1) is replaced by an equal weight portion of sodium p-styrenesulfonate.
[0106] Comparative Example 3
[0107] The only difference between this comparative example and Example 1 is that the allylsuccinic anhydride in step (1) is replaced by maleic anhydride in equal parts by weight.
[0108] Comparative Example 4
[0109] The only difference between this comparative example and Example 1 is that the alkyl monoalcohol (n-butanol) in step (1) is replaced by an equimolar amount of lauryl alcohol.
[0110] Comparative Example 5
[0111] The only difference between this comparative example and Example 1 is that the polyamide polymer B (PVPK30) in step (2) is replaced by PVPK12 in equal parts by weight.
[0112] Comparative Example 6
[0113] The only difference between this comparative example and Example 1 is that the active macromonomer polyether a1 in step (1) is replaced by the polyether D-a1 prepared in Comparative Preparation Example 1 in equal parts by weight.
[0114] Comparative Example 7
[0115] A commercially available dispersant is NNO.
[0116] Test Case
[0117] By laboratory sand milling, according to the total amount of slurry formula of 200g, dispersant, water, and disperse dye (Disperse Red 167) were added in proportion; after stirring evenly, 400g of zirconium beads with a particle size of 0.8-1mm were added and sealed in a glass jar, shaken for 15 hours, and filtered to obtain the color paste.
[0118] The specific formula of the color paste prepared in this application is shown in Table 1:
[0119] Table 1
[0120] Performance Testing
[0121] (1) Viscosity: measured using NDJ-1B rotational viscometer, Shanghai Changji Geological Instrument Co., Ltd.; “-” indicates that the viscosity is too high to be measured;
[0122] (2) Particle size: Measured using BT-90 laser particle size analyzer, Dandong Better Instrument Co., Ltd.; “\” represents precipitation or lack of fluidity and cannot be measured;
[0123] (3) Storage stability: Store at 55°C for 7 days, observe the color paste state, and re-measure the particle size and viscosity of the color paste;
[0124] (4) Centrifugal sedimentation rate (%): After centrifuging the dye paste at 4000 rpm for 20 minutes, wash with anhydrous ethanol, dry at 90°C to constant weight, and accurately weigh the sedimentation weight; Sedimentation rate = sedimentation weight ÷ (dye content in the paste × sample volume) × 100%; where "+" indicates no fluidity and cannot be tested.
[0125] The specific test results are shown in Table 2:
[0126] Table 2
[0127] As can be seen from Table 2, the water-soluble dispersant obtained by compounding the polyether-modified polymer A and the polyamide polymer B in the present application has a good dispersing effect on the dye paste (particle size D50 (initial): 290-331 nm) under the premise of a small amount of use. The viscosity of the paste can also meet the requirements (viscosity (initial): 237-264 mPa·s), the centrifugal sedimentation rate is low (3.3%-4.9%), and the paste has good stability (stored at 55°C for 7 days, the viscosity and particle size of the paste do not change significantly), and the storage period is long, which is superior to commercially available dispersants.
[0128] From the comparison between Test Example 7 and Test Example 1, it can be seen that if the amount of active macromonomer polyether added is too little, the viscosity, particle size and centrifugal sedimentation rate of the dye paste will be significantly increased, and the stability of the system will deteriorate; from the comparison between Test Example 8 and Test Example 5, it can be seen that if the amount of active macromonomer polyether added is too much, the particle size and viscosity of the dye paste will be significantly increased, the corresponding storage index increase will be too large, and the centrifugal sedimentation rate will be significantly increased.
[0129] From the comparison between Test Example 1 and Comparative Test Examples 1-6, it can be seen that replacing any one of the raw materials for the preparation of polyether-modified polymer A (vinylbenzene monomer, allyl succinic anhydride, active macromonomer polyether, alkyl monool) with other components, or replacing the polyamide polymer B with other components, will significantly increase the viscosity, particle size and centrifugal sedimentation rate of the dye paste.
[0130] The applicant declares that this application uses the above-mentioned embodiments to illustrate the water-soluble dispersant of this application, its preparation method, and application, but this application is not limited to the above-mentioned embodiments, that is, it does not mean that this application must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvements to this application, equivalent replacement of various raw materials of the product of this application, addition of auxiliary ingredients, selection of specific methods, etc., all fall within the scope of protection and disclosure of this application.
Claims
1. A water-soluble dispersant comprising a polyether-modified polymer A and a polyamide-based high molecular polymer B; The raw materials for preparing the polyether-modified polymer A include vinylbenzene monomers, allyl succinic anhydride, active macromonomer polyether and alkyl monoalcohol; The polyamide-based high molecular polymer B includes a homopolymer of vinyl pyrrolidone and / or a copolymer of vinyl pyrrolidone.
2. The water-soluble dispersant according to claim 1, wherein The active macromonomer polyether is prepared by the following preparation method: Add polyetheramine and allyl succinic anhydride into the reactor, raise the temperature, and keep the temperature until anhydrous water is distilled out during the reaction to obtain the active macromonomer polyether.
3. The water-soluble dispersant according to claim 2, wherein The polyetheramine is a monoprimary amino polyether in which the terminal hydroxyl group is converted into an amine by using a monoalcohol as an initiator to initiate the self-polymerization of ethylene oxide or the copolymerization of ethylene oxide and propylene oxide.
4. The water-soluble dispersant according to claim 2 or 3, wherein The weight average molecular weight of the polyetheramine is 500 to 2500 g / mol.
5. The water-soluble dispersant according to any one of claims 2 to 4, wherein The polyetheramine includes any one of JEFFAMINE M-2070, JEFFAMINE M-1000 or JEFFAMINE M-600 or a combination of at least two thereof; Preferably, the molar ratio of the polyetheramine to allyl succinic anhydride is (0.5-1.5):1, preferably 1:1; Preferably, the heating is to 120-160°C; Preferably, the insulation time is 2 to 6 hours; Preferably, the preparation process of the reactive macromonomer polyether is carried out under the protection of an inert gas.
6. The water-soluble dispersant according to any one of claims 1 to 5, wherein The active macromonomer polyether has a structure as shown in the following formula I: Among them, R1 is hydrogen or methyl, R2 is methyl, ethyl, propyl or butyl, m is an integer of 10 to 60, and n is an integer of 0 to 15.
7. The water-soluble dispersant according to any one of claims 1 to 6, wherein The vinylbenzene monomer includes any one or a combination of at least two of styrene, β-methylstyrene, allylbenzene, 3-methylstyrene, 2-methylstyrene or 2-isopropenyltoluene; Preferably, the alkyl monoalcohol includes any one or a combination of at least two of methanol, ethanol, propanol, n-butanol, isopropanol, isobutanol or tert-butanol; Preferably, the mass ratio of the vinylbenzene monomer, allyl succinic anhydride, and active macromonomer polyether is (2-10):(5-20):(30-80); Preferably, the molar ratio of the alkyl monoalcohol to the allyl succinic anhydride is (0.1-1):1, preferably 1:
1.
8. The water-soluble dispersant according to any one of claims 1 to 7, wherein The raw materials for preparing the polyether-modified polymer A also include an initiator and a catalyst; Preferably, the initiator comprises any one or a combination of at least two of benzoyl peroxide, tert-butyl benzoyl peroxide, methyl ethyl ketone peroxide, diisopropylbenzene peroxide, di-tert-butyl peroxide or 2,2-bis(tert-butyl peroxide)butane; Preferably, the catalyst comprises any one or a combination of at least two of p-toluenesulfonic acid, sulfuric acid, propionic acid, aminosulfonic acid or hydrochloric acid; Preferably, the raw materials for preparing the polyether-modified polymer A include the following components in parts by weight:
9. The water-soluble dispersant according to any one of claims 1 to 8, wherein The weight average molecular weight of the polyether modified polymer A is 5000 to 100000 g / mol, preferably 20000 to 60000 g / mol; Preferably, the weight average molecular weight of the polyamide polymer B is 2000 to 100000 g / mol, preferably 10000 to 50000 g / mol; Preferably, the polyamide polymer B includes any one of PVPK25, PVPK30, PVPK35 or copolyvidone VA64, or a combination of at least two thereof; Preferably, the mass ratio of the polyether modified polymer A to the polyamide polymer B is (7-22):(4-7).
10. The water-soluble dispersant according to any one of claims 1 to 9, wherein The water-soluble dispersant also includes deionized water and a pH regulator; Preferably, the raw materials for preparing the water-soluble dispersant include the following components in parts by weight:
11. A method for preparing a water-soluble dispersant as claimed in any one of claims 1 to 10, comprising the following steps: (1) adding a formulated amount of active macromonomer polyether into a reactor, raising the temperature, then adding vinylbenzene monomer, allyl succinic anhydride, and an optional initiator, and keeping the temperature for reaction, then sequentially adding an alkyl alcohol and an optional catalyst, and keeping the temperature for reaction again, sampling and testing every 30 minutes, until the difference in the acid value of the system between two adjacent times is ≤2 mgKOH / g, terminating the reaction, and obtaining the polyether-modified polymer A; (2) Cooling the polyether-modified polymer A obtained in step (1), then adding optional deionized water and polyamide polymer B, and then adding an optional pH adjuster, stirring, to obtain the water-soluble dispersant.
12. The preparation method according to claim 11, wherein The heating in step (1) is to heat the mixture to 100-150°C.
13. The preparation method according to claim 11 or 12, wherein: The temperature of the insulation reaction in step (1) is 100 to 150° C., and the insulation reaction time is 1 to 3 hours; Preferably, the temperature of the second heat preservation reaction in step (1) is 100 to 150° C., and the time of the second heat preservation reaction is 2 to 10 hours.
14. The preparation method according to any one of claims 11 to 13, wherein: Step (1) and step (2) are both carried out under the protection of an inert gas; Preferably, the cooling in step (2) is cooling to 50-60°C.
15. Use of the water-soluble dispersant according to any one of claims 1 to 10 in dye dispersion.
Citation Information
Patent Citations
Preparation method of high-performance dispersing agent, polymer polyol and polyurethane foam
CN109721703A
Water-based thickening dispersant and water-based binder for lithium ion battery and preparation method of water-based thickening dispersant
CN113527572A
Water-soluble polymer polyol and preparation method thereof
CN114213600A
Use of cationic polymers in cosmetic formulations, especially shampoos and other hair-care preparations, involves using polymers obtained by polymerisation of quaternary nitrogen monomers in presence of polyether compounds
DE10212705A1
Acid anhydride group-containing organosiloxane and method for producing the same
JP2013129809A