Multilayer material, and abrasive material used by same and use thereof
Patent Information
- Application Number
- PCT/CN2024/090914
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-05
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-14
Smart Images

Figure CN2024090914_14112024_PF_FP_ABST
Abstract
Description
Multilayer materials and abrasive materials and applications thereof
[0001] This application claims priority to the Chinese patent application filed with the State Intellectual Property Office of China on May 5, 2023, with application number 202310498644.7 and application name “Multi-layer materials, abrasive materials used therefor and applications thereof”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application relates to the technical field of multilayer materials, and in particular to a multilayer material and a grinding layer used therein and applications thereof. Background Art
[0003] Multilayer materials are a crucial auxiliary material used in substrate surface planarization. They typically consist of a stacked base layer, an adhesive layer, and a porous abrasive layer. The abrasive layer, which comes into contact with the substrate being treated, is the core functional layer that influences the planarization results. Polyurethane elastomers are commonly used for abrasive layers, but their elastic modulus decreases rapidly with increasing temperature, resulting in an unstable planarization rate. Furthermore, within the operating temperature range of multilayer materials, the abrasive layer has a high loss factor, making the surface susceptible to plastic deformation, which can affect the planarization rate and even lead to pore blockage and premature end of life.
[0004] Summary of the Invention
[0005] In view of this, an embodiment of the present application provides a polishing layer material that can be used for multi-layer materials to solve the problems of unstable planarization rate and short service life of existing multi-layer materials for substrates.
[0006] In a first aspect of an embodiment of the present application, a grinding material is provided for surface treatment of a substrate. The grinding material is a porous polyurethane elastomer. The ratio of the tensile elastic modulus of the grinding material at 25°C and 85°C is in the range of 1-2, and the loss factor of the grinding material in the temperature range of 25-85°C is less than 0.1.
[0007] The tensile elastic modulus of the abrasive material decreases less with increasing temperature, and its loss factor is low within the temperature range of the substrate flattening process. This ensures that the flattening rate of the multilayer material using the abrasive material is stable, scratches are not easily generated on the substrate surface, and the multilayer material has a long service life.
[0008] In some embodiments of the present application, the loss factor of the abrasive material is less than or equal to 0.059 within a temperature range of 25-85°C. In this case, the abrasive layer is less likely to plasticize and deform after being subjected to stress during operation of the multilayer material, thereby reducing the probability of its pore structure becoming clogged and unable to perform its abrasive function.
[0009] In some embodiments of the present application, the ratio of the tensile elastic modulus of the abrasive material at 25° C. to that at 85° C. is in the range of 1-1.5. In this case, the decrease in the tensile elastic modulus of the abrasive material is smaller as the temperature increases, which is more conducive to ensuring a stable grinding rate for the multilayer material.
[0010] In the embodiment of the present application, the ratio of the tensile elastic modulus of the abrasive material at 25°C to that at 60°C is within a range of 1-2. Thus, the rate of change of the tensile elastic modulus of the abrasive material at 60°C, an intermediate temperature during the substrate planarization process, compared to the rate of change at the initial operating temperature of 25°C is not large. This substantially ensures that the tensile elastic modulus of the abrasive material does not vary significantly across the entire operating temperature range, further facilitating a stable polishing rate for multilayer materials.
[0011] In an embodiment of the present application, the porous polyurethane elastomer is obtained by curing raw materials including an isocyanate-terminated prepolymer, a curing agent, and a porogen. The prepolymer is obtained by reacting a diisocyanate with a macromolecular polyol, wherein the diisocyanate comprises a diisocyanate with all atoms in the same plane; and the curing agent comprises a small molecule diol. The diisocyanate with all atoms in the same plane has a very regular planar structure. When the diisocyanate structure in the NCO-terminated prepolymer formed by the reaction reacts with the curing agent to form a polyurethane hard segment, the hard segments have a high degree of regularity in arrangement. The small molecule diol curing agent also provides the hard segments with more time to arrange, thereby ensuring that the resulting porous polyurethane elastomer has a low E'25 / E'85 value and a low Tanδ value at different temperatures.
[0012] A second aspect of an embodiment of the present application provides a multilayer material, which includes a base layer, an adhesive layer and a grinding layer stacked in sequence, wherein the grinding layer includes the grinding material described in the first aspect of the embodiment of the present application.
[0013] The multilayer material used for the flat substrate introduces the above-mentioned grinding layer material with a smaller decrease in tensile elastic modulus with increasing temperature and a lower loss factor. This ensures that the grinding rate of the substrate by the multilayer material is stable and it is not easy to scratch the surface of the substrate. The flattening effect of the substrate after processing in different batches is similar, and the service life of the multilayer material is long.
[0014] A third aspect of the present invention provides the use of the abrasive material described in the first aspect of the present invention, or the multilayer material described in the second aspect of the present invention, in substrate surface treatment. The substrate may include, but is not limited to, a wafer, glass, metal, ceramic, etc.; and the substrate surface treatment may specifically be a substrate surface planarization treatment.
[0015] A fourth aspect of the embodiments of the present application provides a substrate surface treatment device, which includes the multilayer material described in the second aspect of the embodiments of the present application.
[0016] In some embodiments of the present application, the substrate surface treatment device includes a work platform and a grinding head suspended above the work platform, the surface of the work platform is provided with the multi-layer material, or the multi-layer material is installed on the grinding head.
[0017] By using a substrate surface treatment device with the multilayer material, the flattening rate of the substrate surface is stable and the flattening effect is good, scratches are not easily generated on the substrate surface, and the service life of the device is long. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] FIG1A and FIG1B are two structural schematic diagrams of a multilayer material 100 provided in an embodiment of the present application.
[0019] FIG2 is a schematic structural diagram of a substrate surface treatment device 200 provided in an embodiment of the present application. DETAILED DESCRIPTION
[0020] The technical solution of this application will be described below in conjunction with the drawings in the embodiments of this application.
[0021] Multilayer materials are important auxiliary materials used in surface planarization processes such as chemical mechanical polishing (CMP) to determine the surface treatment quality of substrates (such as semiconductor substrates, glass, metals, ceramics, and optical devices). Referring to Figures 1A and 1B , a multilayer material 100 for substrate surface treatment provided in an embodiment of the present application includes a base layer 11, an adhesive layer 12, and a porous polishing layer 13 stacked in sequence.
[0022] The surface of the base layer 11 facing away from the polishing layer 13 serves as the adsorption surface of the multilayer material 100, ensuring that the multilayer material 100 adheres to the substrate surface treatment device. In some cases, the side of the base layer 11 facing away from the polishing layer 13 may also be provided with an adhesive layer 14 (see FIG. 1B ) to ensure more stable adhesion of the multilayer material 100 to the substrate surface treatment device. The surface of the polishing layer 13 facing away from the base layer 11 serves as the working surface of the multilayer material 100, intended to contact the substrate surface to be processed, thereby achieving a flat surface for the substrate through the mechanical action of the multilayer material 100 and the chemical action of the polishing fluid.
[0023] In the present application, the grinding layer 13 is made of the following grinding material provided in the embodiment of the present application, which is a porous polyurethane elastomer. The ratio of the tensile elastic modulus of the grinding material at 25°C and 85°C (expressed as E'25 / E'85) is in the range of 1-2, and the loss factor of the grinding material in the temperature range of 25-85°C (denoted as Tanδ(25~85°C)) is less than 0.1.
[0024] Among them, 25℃ is a common starting working temperature for multilayer materials, and 85℃ is a common maximum working temperature for multilayer materials. The present application controls the ratio of the tensile elastic modulus of the constituent materials of the grinding layer 13 at 25℃ and 85℃ to be 1-2, which can ensure that the tensile elastic modulus of the grinding layer decreases less with increasing temperature within its working temperature range, thereby ensuring that its grinding rate is stable during operation. In addition, the smaller elastic modulus change can also reflect that the hardness of the grinding layer decreases less with increasing temperature, so that a grinding layer material with a lower hardness at 25℃ can be selected for contact treatment with the substrate, thereby helping to reduce the possibility of scratches on the surface of the substrate. At the same time, the loss factor of the grinding layer material in the temperature range of 25-85℃ is less than 0.1, indicating that it can basically recover to its initial deformation after being deformed under the action of external force. This can ensure the good resilience of the grinding layer 13 and reduce the probability of plastic deformation on the surface of the grinding layer 13 causing its pore structure to be blocked, thereby also ensuring a stable grinding rate. Therefore, using such a polishing layer 13 can ensure that the multilayer material 100 flattens the substrate at a stable rate, is less likely to cause scratches on the substrate surface, and has a longer service life.
[0025] Specifically, the E'25 / E'85 ratio of the abrasive material can be 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2.0. In some embodiments of the present application, the E'25 / E'85 ratio of the abrasive material is within the range of 1-1.5. In this case, the tensile modulus of the abrasive material decreases less with increasing temperature, which is more conducive to ensuring a stable polishing rate for the multilayer material 100.
[0026] In some embodiments of the present application, the loss factor of the above-mentioned grinding material in the temperature range of 25-85°C can be less than 0.059, for example, specifically 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.055, 0.057, 0.058, 0.059, etc. In this case, the grinding layer is more likely to return to its initial deformation after being subjected to force during the operation of the multilayer material (that is, it is less likely to plasticize and deform), reducing the probability of its pore structure being clogged and unable to perform the grinding function. In some embodiments, the loss factor of the grinding material in the temperature range of 25-85°C can be less than 0.05.
[0027] In the embodiment of the present application, the ratio of the tensile elastic modulus of the abrasive material at 25°C to that at 60°C is within a range of 1-2. The tensile elastic modulus of the abrasive material at an intermediate temperature (60°C) during the flattening process is also maintained at a higher rate than at the initial operating temperature of 25°C, without a sudden increase in the tensile elastic modulus. This essentially ensures that the tensile elastic modulus of the abrasive material does not vary significantly across the entire operating temperature range, further facilitating a stable polishing rate for multilayer materials.
[0028] The loss factor (Tanδ) and tensile modulus (E') of the abrasive material at different temperatures can be obtained through dynamic mechanical analysis (DMA). Tanδ and E' can be measured according to ISO 6721-4, using a 1 Hz test frequency and a heating rate of 3°C / min.
[0029] In an embodiment of the present application, the tensile elastic modulus E'25 of the abrasive material at 25° C. may be 20-500 MPa. In some embodiments, the E'25 of the abrasive material may be 50-350 MPa, or further may be 85-250 MPa.
[0030] In the embodiment of the present application, the Shore hardness of the above-mentioned abrasive material is in the range of 70A-70D. Since the tensile elastic modulus of the abrasive material decreases less with increasing temperature, an abrasive material with lower hardness can be selected for use in the multilayer material 100, thereby reducing the possibility of scratches on the surface of the substrate. In some embodiments, the Shore hardness of the above-mentioned abrasive material is in the range of 70A-55D, for example, specifically 75A, 30D, 35D, 38D, 40D, 42D, 46D, 50D, 52D, 55D, etc. Among them, when the hardness is below 30D, it is more accurate to measure it with Shore hardness A. In some embodiments, the Shore hardness of the grinding layer 13 is 30D-55D, and can further be 35D-54D.
[0031] In the embodiment of the present application, the abrasive material has a porous structure with an average pore size of 10 μm to 60 μm. The appropriate average pore size facilitates the rapid delivery of the abrasive working fluid, ensuring that the multilayer material 100 processes the substrate at a faster speed while reducing surface defects on the substrate after treatment.
[0032] In the embodiment of the present application, the density of the grinding material is 0.4-1.0 g / cm 3 The density in this range can reflect to a certain extent that the grinding layer 13 has a suitable porosity for conveying the grinding working fluid, while at the same time not being too light to affect its mechanical properties.
[0033] In an embodiment of the present application, the above-mentioned grinding material - porous polyurethane elastomer can be obtained by curing raw materials including an isocyanate group (NCO)-terminated prepolymer, a curing agent and a porogen, wherein the prepolymer is obtained by reacting a diisocyanate substance with a macromolecular polyol, and the diisocyanate substance includes a diisocyanate in which all atoms are in the same plane; the curing agent includes a small molecule diol.
[0034] Among them, the diisocyanate with all atoms in the same plane has a very regular planar structure. When the diisocyanate structure in the NCO-terminated prepolymer formed by it reacts with the curing agent to form the polyurethane hard segment, the hard segments of adjacent molecules / or the same molecule are more easily arranged regularly, forming a structurally stable hard segment component. At the same time, due to the regular stacking of the hard segments, better phase separation can be achieved between the soft segment and the hard segment. The hard segment arrangement of the porous polyurethane elastomer is highly regular, making it difficult to be destroyed under the action of external forces. The external force mainly causes elastic deformation and low heat loss, that is, its loss modulus E" is low, so its Tanδ value (Tanδ=E" / E') is low, which is conducive to the material returning to its initial deformation and the probability of plastic deformation is low, which is conducive to ensuring its stable grinding rate of the substrate and improving its own service life. The elastic modulus of a porous polyurethane elastomer is primarily determined by its hardness. Because the hard segments of the porous polyurethane elastomer of this application have a high degree of regularity in arrangement and are less likely to be damaged as the temperature rises, the elastic modulus can be maintained at a relatively stable level. Therefore, the E'25 / E'85 value is relatively low, close to 1, thereby ensuring a stable polishing rate for the polishing layer 13 on the substrate. Furthermore, the application utilizes a small molecule diol as a curing agent rather than a diamine curing agent, ensuring a suitable curing rate for the NCO-terminated prepolymer, thereby preventing the resulting porous polyurethane elastomer from exhibiting poor mechanical property consistency due to an excessively fast curing rate. Furthermore, a suitable curing rate also provides the polyurethane elastomer with more time for the hard segments to arrange during the synthesis process, thereby reducing the E'25 / E'85 value and Tanδ value of the polishing material at different temperatures.
[0035] In the embodiment of the present application, the diisocyanate with all atoms in the same plane is specifically an aromatic diisocyanate with all atoms in the same plane, which can include one or more of p-phenylene diisocyanate (PPDI) and 1,5-naphthalene diisocyanate (NDI), but is not limited thereto. PPDI and NDI have a very regular planar structure with all atoms in the same plane. When the NCO-terminated prepolymer end groups of PPDI and / or NDI formed react with a curing agent to form a polyurethane hard segment, the hard segments of adjacent molecules and / or the same molecule are more easily arranged regularly, forming a structurally stable hard segment component.
[0036] In the present application, the molecular weight of the small molecule diol is less than 500, and further may be less than or equal to 300, or less than or equal to 200. In the embodiment of the present application, the small molecule diol may include one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, etc., but is not limited thereto. These small molecule diols are green and non-toxic, and the reaction conditions are mild. They can ensure that the curing rate of the prepolymer obtained by reacting the diisocyanate with the macromolecular polyol in which all the atoms mentioned above are in the same plane is within a more suitable range, thereby ensuring that the physical properties of the obtained porous polyurethane elastomer are good, while also reducing the risk of preparing the porous polyurethane elastomer and having good controllability.
[0037] In the embodiment of the present application, the molar ratio of the diisocyanate with all atoms in the same plane in the diisocyanate substance can be 10-100%. Wherein, when the molar ratio is 100%, it represents that the diisocyanate substance is only PPDI and / or NDI; when the molar ratio is less than 100%, it represents that the diisocyanate substance can also include other diisocyanates in addition to the diisocyanate with all atoms in the same plane (such as PPDI and / or NDI). In this case, the molar ratio of PPDI and / or NDI with high structural regularity is controlled to be more than 10%, and further to 50% or 70% to ensure that the hard segment arrangement regularity of the porous polyurethane elastomer is high and its Tanδ value is low. Wherein, other diisocyanates can be other aromatic diisocyanates (that is, all atoms are not in the same plane) or aliphatic diisocyanates. In some embodiments of the present application, the molar ratio of the diisocyanate with all atoms in the same plane in the diisocyanate substance is 100%. This is more conducive to ensuring that the Tanδ value of the porous polyurethane elastomer is low at different temperatures.
[0038] In an embodiment of the present application, the molecular weight of the macromolecular polyol is 500-5000. Further, the functionality of the macromolecular polyol is 2-4, and the hydroxyl value is 30-200 mgKOH / g. Exemplarily, the macromolecular polyol may include one or more of polyvinyl lactone diol (PCL), polytetramethylene glycol (PTMEG), polyoxypropylene polyol (PPG), polyoxyethylene polyol (PEG), etc.
[0039] In an embodiment of the present application, the concentration of unreacted NCO in the prepolymer is 4-8.5 wt %. This further ensures better controllability of the curing reaction between the NCO-terminated prepolymer and the small molecule diol curing agent, resulting in more consistent mechanical properties across regions of the resulting abrasive material. This effectively ensures a more stable polishing rate for substrate surfaces using the multilayer material with the abrasive layer, and a higher degree of surface flatness.
[0040] In the embodiment of the present application, the molar number of hydroxyl groups in the small molecule diol accounts for 10-100% of the total molar number of groups that can react with isocyanate groups in the curing agent. Among them, the groups that can react with isocyanate groups can be only hydroxyl groups, or hydroxyl groups and amino groups, etc. When the molar ratio is 100%, it means that the curing agent is only the aforementioned small molecule diol. When the molar ratio is less than 100%, it means that in addition to the aforementioned small molecule diol, the curing agent can also include other curing agents, such as diamine substances. In this case, the molar ratio of hydroxyl groups in the small molecule diol can be controlled to be more than 10%, which is more conducive to ensuring that the curing rate of the NCO-terminated prepolymer is appropriate. Further, the molar ratio is more than 30%, more than 50%, more than 60%, more than 70%, more than 80%, more than 90%, or even 100%. In some embodiments of the present application, the curing agent includes the above-mentioned small molecule diol and diamine substances (such as aromatic diamines). The molar number of the hydroxyl group in the small molecule diol can account for 10-100% of the total molar number of the amino group in the diamine substance and the hydroxyl group in the small molecule diol.
[0041] In the present application, the ratio of the total molar number of groups reactive with isocyanate groups in the curing agent to the molar number of NCO in the NCO-terminated prepolymer is in the range of 0.9-1.2.
[0042] In the embodiments of the present application, the porogen includes one or more of a chemical foaming agent, a physical foaming agent, and foaming microspheres. The foaming microspheres may specifically be hollow polymer microspheres or fluid-filled hollow polymer microspheres. The size of the porogen can be determined based on the pore size of the desired porous structure in the grinding layer 13.
[0043] In the present application, the above-mentioned grinding layer material can be prepared by production methods well known in the art, including but not limited to casting molding, melt extrusion molding, coating curing method, etc. In the following, the present application takes the casting molding method as an example to illustrate a method for preparing the grinding layer material. The preparation method may include the following steps:
[0044] (1) Preparing an NCO-terminated prepolymer: performing a prepolymerization reaction on a diisocyanate and a macromolecular polyol to obtain the prepolymer; wherein the diisocyanate comprises one or more of p-phenylene diisocyanate (PPDI) and 1,5-naphthalene diisocyanate (NDI); and the NCO concentration in the prepolymer may be 4-8.5 wt%;
[0045] (2) mixing the raw materials comprising the prepolymer, the porogen and the curing agent, introducing the mixture into a mold, performing a heat treatment, and curing to obtain a porous polyurethane elastomer; wherein the curing agent comprises a small molecule diol.
[0046] In step (1), the diisocyanate may include only PPDI and / or NDI, or may include PPDI and / or NDI and other diisocyanate substances. Optionally, in step (1), the weight parts of the diisocyanate may be 20-60 parts based on 100 parts by weight of the macromolecular polyol.
[0047] In step (2), the molar number of hydroxyl groups in the small molecule diol accounts for 10-100% of the total molar number of groups that can react with NCO in the curing agent. The ratio of the total molar number of groups that can react with NCO in the curing agent to the molar number of NCO in the NCO-terminated prepolymer is in the range of 0.9-1.2. In some embodiments, based on 100 parts by weight of the prepolymer, the weight parts of the curing agent can be 3-20 parts, for example, 4-15 parts, 5-12 parts, etc. In the embodiment of the present application, based on 100 parts by weight of the prepolymer, the weight parts of the porogen can be 0.5-5 parts, for example, 0.6, 0.7, 0.8, 1.0, 1.25, 1.5, 1.75, 1.8, 2, 2.5, 3 or 4 parts, etc. Wherein, the porogen can include one or more of foaming microspheres and water-soluble particles. Wherein, the foaming microspheres can specifically be hollow polymer microspheres and fluid-filled hollow polymer microspheres. The size of the porogen can affect the pore size of the resulting porous polyurethane elastomer. In the embodiment of the present application, the average pore size of the porous polyurethane elastomer can be in the range of 10 μm to 60 μm, and further in the range of 20 μm to 50 μm.
[0048] In step (2), before mixing the prepolymer with the porogen, the prepolymer may be heated and vacuum degassed to remove gases and small molecules from the prepolymer, thereby reducing the purity of the porous polyurethane elastomer obtained in the subsequent reaction and improving the dimensional uniformity of the porous structure. The heating may be performed at 50-80° C. The vacuum degassing may be performed at a vacuum degree not exceeding 0.1 MPa, for example, 0.01-0.095 MPa; and the degassing time may be 0.5-3 hours.
[0049] The "mixing" mentioned herein may specifically include: first mixing the prepolymer with the porogen, degassing under vacuum, and then adding the curing agent. This reduces the risk of the prepolymer partially curing due to the curing agent being added first, resulting in insufficient mixing of the other raw materials, thereby ensuring that the resulting porous polyurethane elastomer has superior grinding properties. The specific means of mixing may include, but are not limited to, one or more of stirring and shearing. Furthermore, when the raw materials also include additives such as catalysts and antioxidants, these additives may be mixed with the prepolymer along with the porogen.
[0050] In some embodiments of the present application, the "heat treatment" in step (2) may include: pre-baking the mold containing the mixed raw materials at a first temperature, and then heating it to a second temperature for curing. Pre-baking mainly allows the mixed raw materials to be initially formed into semi-cured sheets, which are then convenient for the curing reaction to occur at high temperature. Among them, the first temperature can be in the range of 50-80°C, and the second temperature can be in the range of 100-150°C. In some other embodiments of the present application, if the mixed raw materials are introduced into a preheated mold, the raw materials may undergo a certain degree of gelation in the preheated mold, and the heat treatment at this time may only include: curing at the second temperature. Afterwards, the obtained porous polyurethane elastomer is taken out of the mold and processed into the required shape as needed.
[0051] The method for preparing the abrasive material of the present application is simple to operate and suitable for industrial mass production. The ratio of the tensile elastic modulus E'25 / E'85 of the prepared abrasive material at 25°C and 85°C can be within the range of 1-2, and the loss factor Tanδ (25-85°C) within the temperature range of 25-85°C is less than 0.1. As a result, the multilayer material using the abrasive layer can achieve a stable polishing rate for substrates and a long service life, thus having broad market application prospects.
[0052] In other embodiments of the present application, the polishing layer material can also be prepared by the following coating and curing method: a raw material comprising the above-mentioned prepolymer, a porogen, and a curing agent is mixed in a solvent, the resulting composition is coated into a film (for example, on a carrier), and then baked and cured. The coating method can include any one or more of spin coating, blade coating, roller coating, spray coating, etc. The carrier can be a hard material, or a base layer for forming the multilayer material 100.
[0053] The embodiment of the present application further provides a multi-layer material, which includes the above-mentioned grinding layer 13. The material of the grinding layer 13 can include the above-mentioned porous polyurethane elastomer.
[0054] In an embodiment of the present application, as shown in FIG1A , the multilayer material 100 may include a base layer 11, an adhesive layer 12, and the polishing layer 13 stacked in sequence. In some embodiments, the multilayer material 100 further includes an adhesive layer 14 located on a side of the base layer 11 facing away from the polishing layer 13.
[0055] The base layer 11 primarily supports and cushions the grinding layer 13, ensuring pressure balance across the grinding layer 13 during operation of the multilayer material 100. The surface of the base layer 11 facing away from the grinding layer 13 serves as the adsorption surface of the multilayer material 100, ensuring that the multilayer material 100 adheres to a substrate surface treatment device, such as a work platform. The presence of an adhesive layer 14 on the side of the base layer 11 facing away from the grinding layer 13 further helps ensure more stable adhesion of the multilayer material 100 to the substrate surface treatment device. The adhesive layer 12 primarily serves to ensure a good connection between the base layer 11 and the grinding layer 13, reducing the probability of interlayer separation during operation of the multilayer material 100. The adhesive layer 12 can specifically be a solvent-free adhesive. The surface of the grinding layer 13 facing away from the base layer 11 serves as the working surface of the multilayer material 100, contacting the surface of the substrate to be processed, thereby achieving a flat surface under the mechanical action of the multilayer material 100 and the chemical action of the grinding fluid.
[0056] In the embodiment of the present application, the thickness of the grinding layer 13 used in the multilayer material can be in the range of 0.3 mm to 3 mm, which is convenient for ensuring that the grinding layer 13 has appropriate hardness and compressibility, and fully plays the role of flattening the substrate.
[0057] The present application also provides an embodiment of the present application, wherein the above-mentioned grinding material or the above-mentioned multilayer material is used in substrate surface treatment. The substrate surface treatment is specifically a substrate surface flattening process. The application can specifically be used in a chemical mechanical polishing process.
[0058] The present invention also provides a substrate surface treatment device comprising the multilayer material described above. The substrate surface treatment device can be used to planarize the surface of a substrate. The surface treatment device can be referred to as a "planarization device" and can be used in a CMP process. The substrate can include, but is not limited to, a wafer, a semiconductor substrate, glass, metal, ceramic, optical devices, and the like.
[0059] Generally, the substrate surface treatment device may include a work platform and a grinding head suspended above the work platform, wherein the multi-layer material is laid on the surface of the work platform or the multi-layer material is mounted on the grinding head. The work platform may be referred to as a "work plate" in some cases.
[0060] Referring to FIG. 2 , some embodiments of the present application provide a surface treatment device 200 comprising a work platform 1, a multilayer material 100 laid on the surface of the work platform 1, a polishing head 2 suspended above the work platform 1, and a working fluid supply unit 4. A substrate 3 to be treated is mounted on the polishing head 2, and its surface to be processed can contact the multilayer material 100, specifically the polishing layer 13 of the multilayer material 100, during polishing. The work platform 1 or the polishing head 2 can rotate clockwise or counterclockwise under the action of electrodes to initiate the treatment / processing process.
[0061] As previously described in this application, the multilayer material 100 can be adhered to the work platform 1, and its grinding layer 13 is away from the work platform 1. The multilayer material 100 can be adhered specifically by a backing layer 14 provided on the side of the base layer 11 away from the grinding layer 13 to prevent the multilayer material 100 from moving arbitrarily during processing. The grinding head 2 is used to carry or clamp the substrate 3 to be processed, and press the substrate 3 to be processed against the multilayer material 100 with a certain pressure, so that the substrate 3 is located between the grinding head 2 and the multilayer material 100. The working liquid supply unit 4 is used to provide a working liquid, which is generally a chemical solution containing abrasive particles. During the processing of the substrate, the working liquid supply unit 4 can spray the working liquid onto the multilayer material 100. The substrate 3 to be processed reacts chemically with the working liquid, and the surface is flattened under mechanical friction with the multilayer material 100.
[0062] In some embodiments of the present application, the surface treatment device 200 further includes a trimming unit 5. The trimming unit 5 is used to trim the multilayer material 100. During the processing of the substrate, the trimming unit 5 can be pressed against the multilayer material 100 and remove debris and reactants on the surface of the multilayer material 100 when the trimming unit 5 and the multilayer material 100 rub against each other.
[0063] By using the surface treatment device 200 with the multilayer material 100 according to the embodiment of the present application, the surface planarization treatment effect of the substrate 3 to be treated is good, and the device can work for a long time.
[0064] The technical solutions of the embodiments of the present application are further described below with reference to a number of embodiments.
[0065] Example 1
[0066] Preparation of a grinding layer material for a multi-layer material, comprising the following steps:
[0067] (1) 57 parts by weight of PPDI (p-phenylene diisocyanate, NCO content of 52-52.5 wt %, purity of 99.5%) and 100 parts by weight of PTMEG-650 (polytetramethylene glycol with a molecular weight of 650, a functionality of 2, and a hydroxyl value of 166.2-179.5 mgKOH / g) were reacted at 80° C. for 4 h to obtain an NCO-terminated prepolymer, wherein the mass percentage of unreacted NCO groups in the prepolymer was 9.7 wt %.
[0068] (2) The NCO-terminated prepolymer was heated to 80°C and vacuum degassed for 2 hours at a vacuum degree of 0.095 MPa to remove the gas and small molecular compounds in the prepolymer; then 1.75 parts by weight of a porogen (specifically, hollow polymer microspheres with a particle size D50 of 20 μm) was uniformly dispersed in 100 parts by weight of the above vacuum-degassed prepolymer by stirring, and vacuum degassed again at a vacuum degree of 0.095 MPa for 30 minutes to obtain a first mixture. 10.7 parts by weight of a curing agent, 1,4-butanediol, was heated to 35°C and kept constant for 5 minutes, then added to the above first mixture, and shear mixed at high speed, and the obtained second mixture was poured into a cylindrical mold. The mold containing the material is pre-baked in an 80°C oven for 30 minutes. The oven temperature is then raised to 104°C over the next 30 minutes and cured for 16 hours. After curing, the oven cools down to room temperature, and the sample removed from the mold is a porous polyurethane elastomer ready for use as a polishing layer. This sample can then be tested for related properties such as hardness, density, and elastic modulus.
[0069] Example 2
[0070] A grinding layer material for a multilayer material is prepared, which differs from Example 1 only in that: based on 100 parts by weight of the prepolymer, the added amount of the hollow polymer microspheres is 1.25 parts by weight, and the curing agent used is 7.55 parts by weight of ethylene glycol.
[0071] Example 3
[0072] A preparation method for a grinding layer material for a multilayer material is described. The difference between the second embodiment and the second embodiment is the molding method. Specifically, the second mixture is poured into a rotating mold with a preheating device at the bottom. The mold is preheated and maintained constant at 100°C. After curing in the mold for 2 hours, the mold is transferred to a 104°C oven for curing for 16 hours.
[0073] Example 4
[0074] A preparation method for a grinding layer material for a multilayer material, which differs from Example 1 in that: 1) the NCO-terminated prepolymer used is obtained by reacting 34 parts by weight of PPDI with 100 parts by weight of PTMEG-1000 (polytetramethylene glycol with a molecular weight of 1000, a functionality of 2, and a hydroxyl value of 109-115 mgKOH / g); the mass percentage of unreacted NCO groups in the prepolymer is 5.7% by weight, and after heating the prepolymer to 80°C and vacuum degassing, the free monomer content is less than 0.5% by weight; 2) based on 100 parts by weight of the prepolymer, the amount of hollow polymer microspheres added is 1 part by weight, and the curing agent used is 6.44 parts by weight of 1,4-butanediol.
[0075] Example 5
[0076] A preparation method for a grinding layer material for a multilayer material, which differs from Example 1 in that: 1) the NCO-terminated prepolymer used is obtained by reacting 38 parts by weight of PPDI with 100 parts by weight of PTMEG-1000, the mass percentage of unreacted NCO groups in the prepolymer is 7.6% by weight, and after heating the prepolymer to 80°C and vacuum degassing, the content of free monomers is less than 0.5% by weight; 2) based on 100 parts by weight of the prepolymer, the amount of hollow polymer microspheres added is 1.5 parts by weight, and the curing agent used is 8.5 parts by weight of 1,4-butanediol.
[0077] Example 6
[0078] A preparation method for a grinding layer material for a multilayer material, which differs from Example 1 in that: 1) the NCO-terminated prepolymer used is obtained by reacting 26 parts by weight of NDI (1,5-naphthalene diisocyanate, NCO content of 52-52.5wt%, purity of 99.5%) with 100 parts by weight of PTMEG-650, and the mass percentage of unreacted NCO groups in the prepolymer is 7.9wt%; 2) based on 100 parts by weight of the prepolymer, the amount of hollow polymer microspheres added is 1.25 parts by weight, and the curing agent used is 9.02 parts by weight of 1,4-butanediol.
[0079] Example 7
[0080] A preparation method for a grinding layer material for a multilayer material, which differs from Example 1 in that: 1) the NCO-terminated prepolymer used is obtained by reacting 20 parts by weight of NDI with 100 parts by weight of PTMEG-1000, and the mass percentage of unreacted NCO groups in the prepolymer is 6 wt%; 2) based on 100 parts by weight of the prepolymer, the amount of hollow polymer microspheres added is 1.25 parts by weight, and the curing agent used is 6.75 parts by weight of 1,4-butanediol.
[0081] Example 8
[0082] A preparation method for a grinding layer material for a multilayer material, which differs from Example 1 in that: 1) the NCO-terminated prepolymer used is obtained by reacting 26 parts by weight of NDI with 100 parts by weight of PTMEG-650, and the mass percentage of unreacted NCO groups in the prepolymer is 8.1 wt%; 2) based on 100 parts by weight of the prepolymer, the amount of hollow polymer microspheres added is 1.5 parts by weight, and the curing agent used is 9.14 parts by weight of 1,4-butanediol.
[0083] Example 9
[0084] A preparation method for a grinding layer material for a multilayer material is described. The difference between the method and Example 8 is that the amount of the hollow polymer microspheres added is 1.75 parts by weight based on 100 parts by weight of the prepolymer used in Example 8.
[0085] Example 10
[0086] A preparation method for a grinding layer material for a multilayer material is described. The difference between the method and Example 8 is that the amount of the hollow polymer microspheres added is 0.7 parts by weight based on 100 parts by weight of the prepolymer used in Example 8.
[0087] Example 11
[0088] A preparation method for a grinding layer material for a multilayer material, which differs from Example 1 in that: 1) the NCO-terminated prepolymer used is obtained by reacting 14 parts by weight of NDI with 100 parts by weight of PCL-1000 (a polyvinyl lactone diol with a molecular weight of 1000, a functionality of 2, and a hydroxyl value of 108-116 mgKOH / g); the mass percentage of unreacted NCO groups in the prepolymer is 4 wt%; 2) based on 100 parts by weight of the prepolymer, the amount of hollow polymer microspheres added is 1.5 parts by weight, and the curing agent used is 4.51 parts by weight of 1,4-butanediol.
[0089] Example 12
[0090] A preparation method for a grinding layer material for a multilayer material, which differs from Example 5 in that: based on 100 parts by weight of the prepolymer of Example 5, the amount of hollow polymer microspheres added is 1.5 parts by weight, and the curing agent used is a mixture of 8.53 parts by weight of 1,4-butanediol and 0.95 parts by weight of MOCA (3,3'-dichloro-4,4'-diphenylmethanediamine).
[0091] Example 13
[0092] A preparation method for a grinding layer material for a multilayer material is described, which differs from Example 5 in that: based on 100 parts by weight of the prepolymer of Example 4, the amount of hollow polymer microspheres added is 1.5 parts by weight, and the curing agents used are 6.16 parts by weight of 1,4-butanediol and 1.54 parts by weight of MOCA.
[0093] Example 14
[0094] A preparation method for a grinding layer material for a multilayer material is described, which differs from Example 7 in that: based on 100 parts by weight of the prepolymer of Example 7, the amount of hollow polymer microspheres added is 1.25 parts by weight, and the curing agents used are 8.78 parts by weight of 1,6-hexanediol and 0.98 parts by weight of MOCA.
[0095] Example 15
[0096] A grinding layer material for a multilayer material is prepared based on the method described in Example 1, using 10 parts by weight of the PPDI prepolymer used in Example 5, 90 parts by weight of the TDI prepolymer used in Comparative Example 1, 1.85 parts by weight of hollow polymer microspheres, 17.69 parts by weight of a curing agent MOCA, and 1.97 parts by weight of a curing agent ethylene glycol.
[0097] Example 16
[0098] A grinding layer material for a multilayer material is prepared based on the method described in Example 1, using 10 parts by weight of the NDI prepolymer used in Example 7, 90 parts by weight of the TDI prepolymer used in Comparative Example 1, 1.6 parts by weight of hollow polymer microspheres, 14.43 parts by weight of a curing agent MOCA, and 1.61 parts by weight of a curing agent ethylene glycol.
[0099] In order to highlight the beneficial effects of the technical solution of the present application, the following comparative examples 1-2 are provided.
[0100] Comparative Example 1
[0101] A preparation method for a grinding layer material for a multilayer material, which differs from Example 1 in that: 1) the NCO-terminated prepolymer used is obtained by reacting 60 parts by weight of TDI (toluene diisocyanate, wherein the 2,4-toluene diisocyanate content is 80wt%, the 2,6-toluene diisocyanate content is 20wt%, and the NCO content in TDI is ≥48.0wt%) with 100 parts by weight of PTMEG-650, and the mass percentage of unreacted NCO groups in the prepolymer is 9.81wt%; 2) a diamine curing agent is used, specifically 32.73 parts by weight of MOCA (3,3'-dichloro-4,4'-diphenylmethanediamine), with an amine value of 7.4-7.6mmol / g.
[0102] Comparative Example 2
[0103] A preparation method for a grinding layer material for a multilayer material, which differs from Example 1 in that: 1) the NCO-terminated prepolymer used is obtained by reacting 58 parts by weight of TDI (same as in Comparative Example 1) with 100 parts by weight of PTMEG-650, and the mass percentage of unreacted NCO groups in the prepolymer is 8.8 wt%; 2) the curing agent is a diamine substance, specifically 29.43 parts by weight of MOCA, and the amount of hollow polymer microspheres added is 1.65 parts by weight.
[0104] The porous polyurethane elastomer samples prepared in the above Examples and Comparative Examples were subjected to hardness and density tests, as well as DMA testing, to obtain their loss factor (Tanδ) and tensile modulus (E') at various temperatures. The relevant results are summarized in Table 1 below. Hardness was measured according to ISO 48-4:2018. Tanδ and tensile modulus (E') were measured according to ISO 6721-4.
[0105] Table 1
[0106] As shown in Table 1, the porous polyurethane elastomers prepared in Comparative Examples 1-2 using an NCO-terminated prepolymer obtained by reacting a structurally less symmetrical TDI with a macromolecular polyol and a diamine curing agent exhibit a rapid decrease in tensile modulus with increasing temperature. The ratio of the tensile moduli at 25°C to 85°C, E'25 / E'85, is large and falls outside the range of 1-2. Furthermore, the loss factor, Tanδ(25-85°C), within the temperature range of 25-80°C is high, exceeding 0.1. This makes it difficult to maintain a stable polishing rate or increase the service life of the porous polyurethane elastomers prepared in Comparative Examples 1-2 when used to prepare multilayer materials for planarizing substrates.
[0107] To further support the beneficial effects of the present application, the porous polyurethane elastomer samples prepared in the above embodiments and comparative examples were used as grinding layers to manufacture multilayer materials for planarizing substrates, and the performance of the multilayer materials was tested. Table 2 below summarizes the relevant test results of the multilayer materials prepared using the porous polyurethane elastomer samples of Examples 1, 5, 9, 10 and Comparative Examples 1-2. Among them, the multilayer materials prepared using the porous polyurethane elastomer samples of Examples 1, 5, 9, and 10 are respectively recorded as M1, M2, M3, and M4, and the multilayer materials prepared using the porous polyurethane elastomer samples of Examples 1-2 are respectively recorded as D1 and D2.
[0108] As shown in Figure 1B , the multilayer material includes a base layer 11, an adhesive layer 12, and a 2 mm thick abrasive layer 13, which are stacked in this order. Base layer 11 is specifically a 1 mm thick foam cushioning layer with a compression ratio of 25%. A 0.1 mm thick adhesive layer 14 is also provided on the side of base layer 11 facing away from abrasive layer 13. This adhesive layer 14 allows the resulting multilayer material to be adhered to an abrasive testing device (as shown in Figure 2 ).
[0109] The polishing test equipment used was a Huahai Qingke Universal-300D. The polishing fluid used was a T851 model purchased from Anjie Technology Co., Ltd. The cleaning fluid used was ultrapure deionized water. The substrate being polished was a metal tungsten wafer. An LPX-W diamond conditioning disc (Cesor Diamond Industries, Ltd.) was used to condition the polishing layer of the multilayer material. Unless otherwise stated, the experimental conditions used in all polishing tests remained consistent: a platen speed of 67 rpm (i.e., the rotational speed of the polished substrate); a carrier speed of 67 rpm (i.e., the rotational speed of the polishing platform); a polishing fluid flow rate of 250 mL / min; and a specified downforce of 2 Psi.
[0110] The number of defects on the surface of the tungsten wafer obtained after the initial grinding can be measured using wafer defect detection equipment (CANNA 600, China Science Feice Testing). The relative defect value of the tungsten wafer obtained after the initial grinding of the multilayer material of each embodiment is equal to the ratio of the number of defects on the tungsten wafer to the number of defects on the tungsten wafer after the initial grinding of the multilayer material using D1.
[0111] Before and after each grinding experiment, the removal rate of the wafer was measured using a four-point probe tester (Napson RT-3000 / RG-3000). The thickness of 37 test points at the same position on the same wafer was measured, and the removal rate was calculated by the thickness difference. Removal rate = (substrate thickness before grinding - substrate thickness after grinding) / grinding time. In order to consider the grinding stability of the multilayer material, the removal rate of each multilayer material after grinding the 360th and 720th wafers, as well as the thickness wear value of the multilayer material itself and the wear rate of the grinding layer after grinding were also tested. Among them, the wear rate of the grinding layer is equal to the thickness wear value of the grinding layer divided by the number of wafers ground. From this, the average wear rate of the grinding layer can be calculated.
[0112] Table 2
[0113] Note: Taking the M1 sample as an example in Table 2, the average wear rate of the grinding layer is equal to [35 / 360+62 / 720] / 2=0.092μm / piece.
[0114] As can be seen from Table 2, after the first grinding of a tungsten wafer using the multilayer material of the present embodiment, the surface defects of the polished tungsten wafer were far lower than those of the multilayer materials D1 and D2 of the comparative examples. Furthermore, as the number of wafers ground using the multilayer material increases, the multilayer materials M1 to M4 of the present embodiment continue to provide a very stable tungsten removal rate, and the thickness wear values of the multilayer materials are far lower than those of the multilayer materials D1 and D2 of the comparative examples. Furthermore, the average wear rate of the polishing layer is also far lower than that of the comparative examples.
Claims
1. A grinding material for substrate surface treatment, characterized in that: The grinding material is a porous polyurethane elastomer, the ratio of the tensile elastic modulus of the grinding material at 25°C to that at 85°C is in the range of 1-2, and the loss factor of the grinding material in the temperature range of 25-85°C is less than 0.
1.
2. The abrasive material according to claim 1, characterized in that The loss factor of the grinding material in the temperature range of 25-85° C. is less than or equal to 0.
059.
3. The abrasive material according to claim 1 or 2, characterized in that: The ratio of the tensile elastic modulus of the abrasive material at 25°C to that at 60°C is in the range of 1-2.
4. The grinding material according to any one of claims 1 to 3, characterized in that The tensile elastic modulus of the abrasive material at 25° C. is 20-500 MPa.
5. The grinding material according to any one of claims 1 to 4, characterized in that: The Shore hardness of the abrasive material is in the range of 70A-70D.
6. The abrasive material according to any one of claims 1 to 5, characterized in that: The density of the grinding material is 0.4-1.0 g / cm 3 .
7. The abrasive material according to any one of claims 1 to 6, characterized in that: The porous polyurethane elastomer is obtained by curing raw materials including an isocyanate-terminated prepolymer, a curing agent and a porogen, wherein the prepolymer is obtained by reacting a diisocyanate substance with a macromolecular polyol, the diisocyanate substance includes a diisocyanate in which all atoms are in the same plane; and the curing agent includes a small molecule diol.
8. The abrasive material according to claim 7, characterized in that The small molecule diol includes one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,6-hexanediol.
9. The abrasive material according to claim 7 or 8, characterized in that: The concentration of isocyanate groups in the prepolymer is 4-8.5 wt %.
10. The grinding material according to any one of claims 7 to 9, characterized in that: The diisocyanate with all atoms in the same plane includes one or more of p-phenylene diisocyanate and 1,5-naphthalene diisocyanate.
11. The abrasive material according to any one of claims 7 to 10, characterized in that: The molar proportion of the diisocyanate with all atoms in the same plane in the diisocyanate substance is more than 10%.
12. The abrasive material according to any one of claims 7 to 11, characterized in that: The curing agent also includes diamine substances.
13. The grinding material according to any one of claims 7 to 12, characterized in that: The molar number of the hydroxyl groups in the small molecule diol accounts for 10-100% of the total molar number of the groups in the curing agent that can react with isocyanate groups.
14. The abrasive material according to any one of claims 1 to 13, characterized in that: The grinding material has a porous structure with an average pore diameter of 10-60 μm.
15. A multilayer material, characterized in that It comprises a base layer, an adhesive layer and a grinding layer which are stacked in sequence, and the grinding layer comprises the grinding material according to any one of claims 1 to 14.
16. The multilayer material according to claim 15, characterized in that A back adhesive layer is also provided on the side of the base layer away from the grinding layer.
17. The abrasive material according to claim 15 or 16, characterized in that: The thickness of the grinding layer is 0.3 mm-3 mm.
18. Use of the abrasive material according to any one of claims 1 to 14, or the multilayer material according to any one of claims 15 to 17 in surface treatment of a substrate.
19. A substrate surface treatment device, characterized in that: The substrate surface treatment device carries the multilayer material according to any one of claims 15-17.
Citation Information
Patent Citations
Polymer material, foam obtained from same, and polishing pad using those
CN101268111A
Polishing pad and method for manufacturing polished product
WO2022071205A1
Polishing pad and method for manufacturing polished workpiece
WO2022201254A1