A coated cutting tool

A coated cutting tool with a cBN material tip and a braze joint of specific metallic elements, coated with a single-phase a-ALOs layer, addresses the adhesion and wear resistance challenges of traditional CVD coatings, achieving enhanced performance in machining hardened steel.

WO2024231451A1PCT designated stage expired Publication Date: 2024-11-14WALTER AG
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/062724
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2024-05-08
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Traditional CVD coatings face challenges in achieving good adhesion to brazed cBN materials and are limited to solid full-cBN inserts, making it difficult to achieve high wear resistance in cutting tools for machining hardened steel.

Method used

A coated cutting tool with a cBN material tip attached to a cemented carbide supporting body via a braze joint comprising 25-35 wt% Cu, 1-6 wt% Ti, and 45-74 wt% Ag, coated with a single-phase a-ALOs layer, optionally including an intermediate TiOx layer, to enhance bonding and wear resistance.

Benefits of technology

The solution provides improved adhesion and wear resistance, extending tool life and reducing flank wear during machining of hardened steel, while maintaining chemical stability and manufacturability of the cBN material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024062724_14112024_PF_FP_ABST
    Figure EP2024062724_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a coated cutting tool comprising a supporting body and a cutting edge tip of a cBN material, wherein the cutting edge tip is attached to the supporting body via a braze joint, the supporting body is of cemented carbide, wherein the braze alloy comprises 25-35 wt% Cu, 1-6 wt% Ti, 0-14 wt% In and 45-74 wt% Ag, and wherein the cBN cutting edge tip is coated with a coating comprising a layer of α-Al2O3.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] A COATED CUTTING TOOL

[0002] TECHNICAL FIELD

[0003] The present invention relates to a coated cutting tool comprising a supporting body and a cutting edge tip of a cBN material, wherein the cutting edge tip is attached to the supporting body via a braze joint and wherein the cutting edge tip is coated with a coating comprising a layer of a-ALOs.

[0004] BACKGROUND

[0005] Cubic boron nitride (cBN) is the second hardest material and has a higher temperature stability in contact with ferrous metals as compared to diamond. Cutting tools with edges of a cBN material are therefore used to machine hardened steel with a hardness higher than 55HRC. The cBN material is a sintered composite having cBN grains in a ceramic or metallic matrix. Also full-cBN can be used as cutting tool material. The cutting tool can be made up completely from the cBN material or it could be provided at just the cutting edges, for example in the form of brazed tips on cemented carbide carriers.

[0006] It is well known in the art that a coating such as a CVD coating, can reduce the tool wear of a cutting tool by reducing the interaction between the cBN material and the workpiece. The problem with traditional CVD coatings is the high deposition process temperatures, and to achieve good enough coating adhesion. It is difficult to achieve a good coating bonding to a brazed cBN material and the presently commercially available CVD coatings are on solid full-cBN inserts.

[0007] It is an object of the present invention to provide a coated cutting tool comprising a tip of a cBN material brazed in a cemented carbide support body with a high wear resistance in turning in hardened steel.

[0008] DESCRIPTION OF THE INVENTION

[0009] At least one of the above-mentioned objects is achieved by a cutting tool according to claim 1. Preferred embodiments are disclosed in the dependent claims.

[0010] The present invention relates to a coated cutting tool comprising a supporting body and a cutting edge tip of a cBN material, wherein the cBN material consists of 45 - 90 vol% cBN in a ceramic binder, wherein the cutting edge tip is attached to the supporting body via a braze joint, the supporting body is of cemented carbide, wherein the braze joint comprises the metallic elements 25-35 wt% Cu, 1-6 wt% Ti, 0-14 wt% In and 45-74 wt% Ag, the cutting tool is coated with a coating comprising a layer of a-AfeOs, preferably the a-ALOs layer is a single phase a-ALOs free of other phases such as kappa and gamma phase.

[0011] The specific composition of the braze joint is advantageous since it can provide a strong bond between the cBN material and cemented carbide. Cu in the range 25-35 wt% contributes with a suitable melting temperature range. Ti in the range 1-6 wt% contributes with chemical reactivity to bond the cBN material tip and the cemented carbide to the braze. Some percentage of In can be added to the braze to increase the surface wettability and also to reduce porosity. This braze is used in a so called active brazing where not only the braze melts, this brazing also involves a chemical reaction with elements from one of both the materials that are to be joined. There is a thin reaction layer between the braze joint and the cemented carbide. There is substantially no material from the WC grains or from the cBN diffusing into the braze joint. If metallic elements are diffused from the cemented carbide or from the cBN material and into the braze joint, these metallic elements are to be excluded in calculating the Cu, Ti, In and Ag content as defined in the claims.

[0012] By “cutting tool” is herein meant a cutting tool for metal cutting such as an insert, an end mill or a drill. The application areas can be turning, milling or drilling.

[0013] The supporting body is of cemented carbide. In one embodiment the cemented carbide consists of WC in a metallic binder, for example 88-92 wt% WC in a metallic binder of Co or Ni and Co.

[0014] In one embodiment of the present invention the braze joint comprises the metallic elements 25-30 wt% Cu, 2-4 wt% Ti, and 66-73 wt% Ag.

[0015] In one embodiment of the present invention the braze joint comprises the metallic elements 25-35 wt% Cu, 1-6 wt% Ti, 0-14 wt% In and balance Ag.

[0016] In one embodiment of the present invention the braze joint comprises the metallic elements 25-30 wt% Cu, 2-4 wt% Ti, and balance Ag.

[0017] In one embodiment of the present invention the coating further comprises an intermediate layer between the cutting edge tip and the a-AhOs layer, the thickness of said intermediate layer is preferably 30-300 nm. In one embodiment said intermediate layer is in direct contact with the cBN material of the cutting edge tip and in direct contact with the a-AhOs layer. Said intermediate layer can be advantageous in providing improved adhesion between the cutting edge tip and the a-AhC layer.

[0018] In one embodiment of the present invention the coating further comprises an intermediate layer of TiOx, wherein 1<x<2.5, preferably 1.5<x<2.3, between the cutting edge tip and the a-ALOs layer, preferably the TiOxlayer is in direct contact with the cBN material of the cutting edge tip and with the a-ALOs layer, preferably the thickness of the TiOxlayer is SO- SOO nm.

[0019] In one embodiment of the present invention the cBN material contains 45 - 75 vol% cBN in a ceramic binder, preferably 60-70 vol% cBN in a ceramic binder. If the content of cBN in the cutting edge tip is less the cBN material is too brittle, while if the cBN content is too high in the cBN material, the chemical stability in cutting is too low. Another drawback with a high cBN content is that this material is difficult to manufacture.

[0020] In one embodiment of the present invention the ceramic binder in the cBN material is TiN, TiC or TiCN, preferably TiCN.

[0021] In one embodiment of the present invention the thickness of the braze joint is 5-150 pm, preferably 5-100 pm, more preferably 10-80 pm and most preferably 10-30 pm. A braze joint that is too thick weakens the mechanical strength of the joint, and a braze joint that is too thin reduces the quality of chemical bonding of the tip. Thickness outside the claimed range also increases the risk for porosity in the joint.

[0022] In one embodiment of the present invention the thickness of said coating is about 1.5-10 pm. A thinner coating gives less wear resistance, while a thicker coating increases the risk for flaking, spallation, and brittleness giving cracks in the substrate and edge chipping.

[0023] In one embodiment of the present invention the liquidus temperature of the metal alloy of the braze joint is 750 - 850°C, preferably 800 - 830 °C, more preferably 810 - 820 °C.

[0024] In one embodiment of the present invention the coating includes at least one layer of a- AI2O3 applied by chemical vapor deposition at a deposition temperature that is lower than the liquidus temperature of the metal alloy of the braze joint. An advantage with this is that the tip does not move and there is less risk of braze alloy to flow out of the joint and ruining the CVD coating adhesion and the coating growth.

[0025] In one embodiment of the present invention the liquidus temperature of the metal alloy of the braze joint is 810°C - 820°C, and the coating is a CVD coating. In one embodiment of the present invention the a-AfeOs layer exhibits a texture coefficient TC(h k I), as measured by X-ray diffraction using CuKa radiation and 0-20 scan, defined according to Harris formula where l(h k I) is the measured intensity (integrated area) of the (h k I) reflection, lo(h k I) is the standard intensity according to ICDD's PDF-card No. 00-010-0173, n is the number of reflections used in the calculation, and where the (h k I) reflections used are (1 0 4), (1 1 0), (0 2 4), (1 1 6), (2 1 4) and (3 0 0) wherein TC(3 0 0) > 2, more preferably > 2.5, most preferably > 3.

[0026] BRIEF DESCRIPTION OF DRAWINGS

[0027] Embodiments of the invention and also references will be described with reference to the accompanying drawings, wherein:

[0028] Figure 1 is a schematic drawing of a cutting tool 1 comprising a supporting body 2 and cutting edge tips 3,

[0029] Figure 2 is a cross-sectional SEM micrograph showing the AhOs-layer on the cBN material of Invention 1 ,

[0030] Figure 3 is a cross-sectional light optical image of the braze joint between the cBN material tip (dark grey) and the cemented carbide supporting body (light grey) of Invention 1 ,

[0031] Figure 4 is a top view SEM micrograph showing the outer surface of Invention 1 , where the coated braze joint is visible,

[0032] Figure 5 is a cross-sectional SEM micrograph showing the AhOs-layer on the cBN material of Invention 2,

[0033] Figure 6 is a cross-sectional light optical image of the braze joint between the cBN material tip (dark grey) and the cemented carbide supporting body (light grey) of invention 2, and

[0034] Figure 7 is a top view SEM micrograph showing the outer surface of Invention 2, where the coated braze joint is visible. METHODS

[0035] The composition of the ceramic binder in the cBN material can be analyzed by means or, for instance, energy dispersive X-ray analysis. The volume fraction cBN can be analysed by studying a cross section of the cutting edge tip of cBN material and calculating the area fraction cBN grains and assume that the area fraction corresponds to the volume fraction.

[0036] The brazing of the cBN material tip to the supporting body was in the present invention made by vacuum brazing. Cemented carbide supporting bodies were provided with ground pockets to accommodate tips of cBN material. An active Ag-Cu-Ti braze alloy in the form of a paste with an organic binder was applied to the pockets and the cBN material tips were then placed in the pockets. A gentle pressure was applied to remove air inclusions and to set the thickness of the filler paste. After the tip application the organic binder in the braze paste was removed by drying at atmospheric pressure. The cBN material tipped supporting bodies were the placed in a vacuum furnace which was evacuated to a pressure of 10-5mBar. The supporting bodies were then heated to about 840 °C, i.e. at least 15°C above the liquidus temperature of the used braze alloy (815°C).

[0037] The composition of the braze alloy can be analyzed by means or, for instance, energy dispersive X-ray analysis. The liquidus temperature of the braze alloy is specified in the manufacturers data sheet but can also be measured on the final braze joint using, for instance, differential scanning calorimetry.

[0038] For CVD coatings an industrial sized radial flow CVD coating chamber with an inner reactor height of 1580 mm, an inner reactor diameter of 500 mm and an inner volume of approximately 300 litres was used. The reaction gas was fed into the reactor through a central gas inlet pipe and introduced into the reaction zone through openings distributed along the inlet pipe to provide an essentially radial gas flow over the substrate bodies. Water was evaporated from the liquid state by spraying liquid water into a H2 carrier gas stream at 100 °C under reduced pressure. The evaporated amount was controlled by a liquid mass flow controller calibrated to units of g / h from which the gas volume flow in litres per hour is calculated using the molar mass of H2O and ideal gas volume at normal conditions 0°C and 1.013 bar(abs.). AICI3 was generated in situ and evaporated using the technically and industrially common technique of chlorinating Al pellets with HCI gas at elevated temperatures. As usual in publications of thermal CVD of aluminum oxide, it is reasonably assumed that the chlorination reaction Al + 3 HCI AICI3 + 1.5 H2proceeds almost instantaneously and quantitatively, yielding only the monomer molecule of aluminum trichloride. Process gas compositions and volume ratios given herein take AICI3 and H2 flows into account accordingly. The process gas mixture is introduced into the reactor by two separate gas inlets. Metal chlorides (AICI3), optionally additional HCI and / or sulfur containing gases, H2 and optionally carrier gases like Ar or N2 are fed in through one, the precursors (e.g. H2O ) acting as sources for oxygen in the coating materials, the remainders of H2 and optional carrier gases through another inlet. The ratio of total gas flows being supplied to the two different inlets was kept in the range of 0.5 to 2. It is within the purview of the person skilled in the art to adapt this parameter to obtain the desired coating properties. The present invention is not limited to specific setups of reactor design and gas feeding systems.

[0039] Volume ratios of the process gas composition as introduced into the reactor refer to the aforementioned gas flows in litres per hour, referenced to 0°C and 1.013 bar(abs.).

[0040] If not otherwise indicated, in the examples herein, the reactor was filled up to about its full capacity, whereby sample inserts to be investigated were distributed at various different positions within the reactor, and the remaining sample positions within the reactor were filled with “scrap” inserts to simulate, as close as possible, full scale deposition conditions and volume usage within the respective reactor.

[0041] In order to investigate the texture of the layer(s), X-ray diffraction was conducted on the rake face of cutting tool inserts using a Xpert-Pro diffractometer system equipped with a X’Celerator RTMS detector type. The coated cutting tool inserts were mounted in sample holders to ensure that the surface of the cutting tool inserts was parallel to the reference surface of the sample holder and also that the cutting tool surface was at appropriate height. Cu-Ka radiation was used for the measurements, with a voltage of 45 kV and a current of 40 mA. A 0.02 radian soller slit and a 0.25 degree divergence slit were used for the incident beam path. For the diffracted beam a 0.25 degree anti-scatter slit and 0.02 radian soller slit were used. The Beta-filter Nickel had a thickness of 0.020 mm. The diffracted intensity from the coated cutting tool was measured in the range 15° to 140° 20, i.e. over an incident angle 0 range from 7.5 to 70°.

[0042] The data analysis, including background subtraction, Cu-Ka2 stripping and profile fitting of the data, was done using PANalytical’s X’Pert HighScore Plus software. A general description of the fitting is made in the following. The output (integrated peak areas for the profile fitted curve) from this program was then used to calculate the texture coefficients of the layer by comparing the ratio of the measured intensity data to the standard intensity data according to a PDF-card of a-A^Os, using the Harris formula (1) as disclosed above. Since the layer is finitely thick the relative intensities of a pair of peaks at different 20 angles are different than they are for bulk samples, due to the differences in path length through the layer. Therefore, thin film correction was applied to the extracted integrated peak area intensities for the profile fitted curve, taken into account also the linear absorption coefficient of the layer, when calculating the TC values. Since possible further layers above the a-ALOs layer will affect the X-ray intensities entering the a-ALOs layer and exiting the whole coating, corrections need to be made for these as well, taken into account the linear absorption coefficient for the respective compound in a layer. Alternatively, a further layer, such as TiN, above an alumina layer can be removed by a method that does not substantially influence the XRD measurement results, e.g. chemical etching.

[0043] In order to investigate the texture of the a-AI2O3 layer X-ray diffraction was conducted using CuKaradiation and texture coefficients TC (h k I) for different growth directions of the columnar grains of the a-AfeOs layer were calculated according to Harris formula (1), where l(h k I) = measured (integrated area) intensity of the (h k I) reflection, lo(h k l)=standard intensity according to ICDD’s PDF-card no 00-010-0173, n=number of reflections to be used in the calculation. In this case the (h k I) reflections used are: (1 0 4), (1 1 0), (0 2 4), (1 1 6), (2 1 4) and (3 0 0).

[0044] It is to be noted that peak overlap is a phenomenon that can occur in X-ray diffraction analysis of coatings comprising for example several crystalline layers and / or that are deposited on a substrate comprising crystalline phases, and this has to be considered and compensated for. An overlap of peaks from the a-ALOs layer with peaks from another layer such as a TiCN layer might influence measurement and needs to be considered. It is also to be noted that for example cBN in the cBN tip can have diffraction peaks close to the relevant peaks of the present invention.

[0045] From the XRD measurement it can also be concluded if other phases such as gamma or kappa phases are present in the a-A^Ch layer. If no peaks relating to other AI2O3 phases are detected, but only a-A^Ch peaks are present, then the layer is an a-AhOs layer.

[0046] The thickness of the braze joint was measured in a polished cross section perpendicular to the cBN material tip / supporting body interface and coating and the layer thicknesses were measured in a cross section perpendicular to the coati ng / cutti ng edge tip interface. EXAMPLES

[0047] Exemplifying embodiments of the present invention will now be disclosed in more detail and compared to reference embodiments. Coated cutting tools (inserts) were manufactured, analyzed and tested in a metal cutting operation. To simplify, the cutting edge tip of cBN material is in this section called the cBN tip, even though the cBN content in the tips differs from 100%.

[0048] Supporting bodies were provided, made of cemented carbide consisting of WC in a metallic binder of 7 wt% Co. The cutting edge tips Tip 1- 4 was composed of cBN grains in a binder phase, the cBN fractions and cBN binder phase compositions are presented in Table 1. Also the insert geometry is listed in Table 1.

[0049] Table 1. cBN material compositions

[0050] Brazing

[0051] Active vacuum brazing was performed to attach the cBN tip to the cemented carbide supporting body. Cemented carbide supporting bodies were provided with ground pockets to accommodate tips of cBN. An active Ag-Cu-Ti braze alloy in the form of a paste with an organic binder was first applied to the pockets and the cBN tips were then placed in the pockets. A gentle pressure was applied to remove air inclusions and to minimize the thickness of the paste. In order to minimize the risk for braze joint porosity excess of paste was coming out along the entire boundary line between supporting body and cBN tip. After the tip application the organic binder in the braze paste was removed by drying at atmospheric pressure.

[0052] The cBN tipped supporting bodies were placed in a vacuum furnace which was evacuated to a pressure of KT5mBar. The supporting bodies were then heated to about 840 °C, i.e. at least 15°C above the liquidus temperature of the used braze alloy (815°C). A braze joint was thereby formed between the supporting body and the cBN tip. After cooling in vacuum, the furnace was ventilated to atmospheric pressure and the supporting bodies with brazed cBN tips were retrieved. The resulting braze joint thickness was about 20 pm, measured in a polished cross section perpendicular to the cBN tip / supporting body interface. The composition of the braze joint after brazing was, as analyzed by EDS, 70 wt% Ag, 27 wt% Cu and 3 wt% Ti.

[0053] CVD

[0054] Cutting tools with a supporting body of cemented carbide and a brazed cBN material tip were coated in CVD processes to provide the samples Invention 1-7 and Comparative 1-3, see table 3. All the cutting tools were coated with an a-AI2Os layer. Some of the coatings comprise a TiOxlayer between the cBN tip and the a-AI2Os layer. Table 2 gives an overview of the experimental conditions for deposition of different embodiments of the TiOx, and AI2O3 layers. All layers were deposited at a temperature of 800°C and a pressure of 1 kPA. Table 3 is an overview of the coated samples.

[0055] Table 2. Process parameters and reaction gases during CVD deposition Table 3. An overview of the coated samples

[0056] Coating analysis

[0057] The coatings were analysed with EDS and XRD. The TiOxlayer composition of sample Invention 5 was determined by EDS using 10kEV electron energy and the Ti and O Ka- peak intensities from an area in the middle of the TiOxlayer in a polished cross section prepared perpendicular to the substrate and coating interface. The composition of this layer was Ti32O68, i.e. x= 2.1 in TiOx.

[0058] The texture coefficients (TC) of the AI2O3 layers were calculated in accordance with the method disclosed above in the method section, including corrections for thin film and absorption, and using the Harris formula (1). The TC values are shown in Table 4. Table 4. Texture coefficients and phases

[0059] From the XRD analysis it was concluded that the Comparative 1 and Comparative 2 did not only have a-AhOs in the AI2O3 but also other phases were detected.

[0060] Calotte Grinding Evaluation

[0061] Calotte grinding was used to assess adhesion between individual sublayers of the coating. The insert was placed on an inclined magnetic holder of the ball cratering set-up. A spherical calotte was ground in the coating and substrate material by a rotating 30 mm steel ball wetted with a drop of 3 pm water-based diamond suspension (Struers, DP-Lubricant Green) and driven by a driving shaft at > 500 rpm. The grinding process was stopped when the calotte diameter in the substrate material reached approx. 1000 pm. The adhesion between individual sublayers of the coating was studied using light optical microscopy (LOM).

[0062] The adhesion of the inventive layers, Invention 1-5 was good, while Invention 3 slightly less good adhesion compared to the samples Invention 1 ,2,4 and 5. A conclusion was that the TiOxstart layer provided an increased adhesion of the a-ALOs layer. The adhesion of the layers of Comparative 1 and Comparative 2 was good which shows that a TiOxstart layer of 6 nm thickness is enough to achieve a good adhesion. The adhesion of the coating on the Comparative 3 was bad, probably due to that the binder phase in the cBN material of Tip 4 is metallic.

[0063] Turning tests

[0064] The coated cutting tool Invention 1 was evaluated in a cutting test and compared with two commercial reference cutting tools. The Reference 1 and 2 cutting tools both have cBN tips brazed to cemented carbide base bodies and are coated with state of the art PVD TiAIN layers.

[0065] The performance test was a noninterrupted finishing longitudinal turning operation with a cutting speed of 120 m / min, a cutting depth of 0.20mm and a feed rate of 0.15 mm, using inserts of type CNGA1204012. The test was done in a WFL M35G turning center. Workpieces were D61xL200mm round bars of high alloy tool steel X153CrVMo12-1 (1.2379), through-hardened to 62HRC. For wet conditions external emulsion was used at 20 Bar. The tool life criteria were maximum flank wear 0.20mm, fracture or max. 18-20 minutes time in cut. The flank wear was measured after 10 minutes and the results are presented in Table 5 below.

[0066] Table 5. Performance testing results

[0067] As can be seen in Table 5, the Invention 1 showed less flank wear after 10 minutes cutting time as compared to the Reference 1 and 2 samples.

[0068] While the invention has been described in connection with various exemplary embodiments, it is to be understood that the invention is not to be limited to the disclosed exemplary embodiments; on the contrary, it is intended to cover various modifications and equivalent arrangements within the appended claims.

Claims

CLAIMS1. A coated cutting tool (1) comprising a supporting body (2) and a cutting edge tip (3) of a cBN material, wherein the cBN material consists of 45 - 90 vol% cBN in a ceramic binder, wherein the cutting edge tip (3) is attached to the supporting body (2) via a braze joint, the supporting body (2) is of cemented carbide, wherein the braze joint comprises the metallic elements 25-35 wt% Cu, 1-6 wt% Ti, 0-14 wt% In and 45-74 wt% Ag, the cutting tool is coated with a coating comprising a layer of a-ALOs.

2. The coated cutting tool of claim 1, wherein the braze joint comprises the metallic elements 25-30 wt% Cu, 2-4 wt% Ti and 66-73 wt% Ag.

3. The coated cutting tool in accordance with any of claim 1 or claim 2, wherein the coating further comprises an intermediate layer between the cutting edge tip and the a-AI2O3 layer, the thickness of said intermediate layer is 30-300 nm.

4. The coated cutting tool in accordance with claim 3 wherein said intermediate layer is in direct contact with the cBN material of the cutting edge tip and in direct contact with the a-AhOs layer.

5. The coated cutting tool in accordance with claim 3 or claim 4, wherein the intermediate layer is of TiOx, wherein 1<x<2.5.

6. The coated cutting tool in accordance with any of the preceding claims, wherein the cBN material contains 45 - 75 vol% cBN in a ceramic binder.

7. The coated cutting tool in accordance with any of the preceding claims, wherein the cBN material comprises 60-70 vol% cBN in a ceramic binder.

8. The coated cutting tool in accordance with any of the preceding claims, wherein the ceramic binder in the cBN material is TiN, TiC or TiCN, preferably TiCN.

9. The coated cutting tool in accordance with any of the preceding claims, wherein the thickness of the braze joint (4) is 5-150 pm, preferably 5-100 pm, more preferably 10- 80 pm, and most preferably 10-30 pm.

10. The coated cutting tool in accordance with any of the preceding claims, wherein the thickness of said coating is about 1.5-10 pm.

11. The coated cutting tool in accordance with any of the preceding claims, wherein the liquidus temperature of the metal alloy of the braze joint is 750 - 850 °C.

12. The coated cutting tool in accordance with any of the preceding claims, wherein the coating includes at least one layer of a-ALOs applied by chemical vapor deposition at a deposition temperature that is lower than the liquidus temperature of the metal alloy of the braze joint.

13. The coated cutting tool in accordance with any of the preceding claims, wherein the liquidus temperature of the metal alloy of the braze joint is 810°C - 820°C, and wherein the coating is a CVD coating.

14. The coated cutting tool in accordance with any of the preceding claims, wherein the a- AI2O3 layer exhibits a texture coefficient TC(h k I), as measured by X-ray diffraction using CuKa radiation and 0-20 scan, defined according to Harris formulawhere l(h k I) is the measured intensity (integrated area) of the (h k I) reflection, lo(h k I) is the standard intensity according to ICDD's PDF-card No. 00-010-0173, n is the number of reflections used in the calculation, and where the (h k I) reflections used are (1 04), (1 1 0), (02 4), (1 1 6), (2 1 4) and (3 0 0), wherein TC(3 00) > 2, preferably > 3.

Citation Information

Patent Citations

  • Composite coating PCBN cutting tool and preparation method thereof

    CN111910172A

  • Cutting tool whose cutting edge piece has excellent brazing joining strength