Nitride semiconductor device and method for manufacturing nitride semiconductor device
The nitride semiconductor device on an amorphous glass substrate with a concavo-convex structure and compensation layer addresses the thermal strain issue, achieving enhanced crystallinity and reducing impurities, resulting in improved nitride semiconductor performance.
Patent Information
- Application Number
- PCT/JP2024/015251
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-14
AI Technical Summary
The challenge is to form gallium nitride-based semiconductor films on amorphous glass substrates while maintaining crystallinity and reducing thermal strain, as glass substrates absorb moisture and have isotropic thermal expansion, differing from the anisotropic expansion of gallium nitride films, leading to impurities and distortion.
A nitride semiconductor device is created with an amorphous glass substrate having a concavo-convex structure, where a buffer layer and nitride semiconductor stack are formed on the uneven surface, and a compensation layer is added to reduce thermal expansion mismatch and promote crystallinity, using techniques like MOCVD and HVPE for film growth.
This approach enhances the crystallinity of gallium nitride films, reduces thermal stress, and improves the growth of homogeneous crystals, leading to higher-quality nitride semiconductor devices with improved light emission characteristics.
Smart Images

Figure JP2024015251_14112024_PF_FP_ABST
Abstract
Description
NITRIDE SEMICONDUCTOR DEVICE AND METHOD FOR MANUFACTURING NITRIDE SEMICONDUCTOR DEVICE
[0001] One embodiment of the present invention relates to a nitride semiconductor device having a nitride semiconductor layer formed on an amorphous glass substrate and a method for fabricating the same.
[0002] Gallium nitride semiconductor films that form light-emitting diodes are formed on sapphire substrates at temperatures of 800°C to 1100°C by metal organic chemical vapor deposition (MOCVD) or hydride vapor phase epitaxy (HVPE). Because sapphire substrates are expensive, development is underway to form gallium nitride semiconductor films on glass substrates such as those used in display manufacturing. For example, a silicon oxide film is formed on a glass substrate, and then an amorphous silicon film and Al are deposited on the silicon oxide film. x Ga 1-x A technique has been disclosed in which an N buffer layer is formed, and a crystalline nitride-based compound semiconductor is deposited thereon at a temperature of about 700° C. to 850° C. (see Patent Document 1).
[0003] Japanese Patent Application Laid-Open No. 2000-124140
[0004] Generally, glass substrates have a low glass transition temperature, so when depositing gallium nitride semiconductor films, it is necessary to lower the deposition temperature while maintaining crystallinity. Amorphous glass substrates are more hygroscopic than sapphire substrates. Therefore, when heated during deposition, the absorbed moisture is released and incorporated as impurities into the gallium nitride semiconductor film, resulting in a decrease in crystallinity. Furthermore, while glass substrates have an amorphous structure and exhibit isotropic thermal expansion, gallium nitride semiconductor films, such as gallium nitride, exhibit anisotropic thermal expansion, resulting in unintended thermal distortion of the gallium nitride semiconductor film on the amorphous glass substrate.
[0005] A nitride semiconductor device according to one embodiment of the present invention includes an amorphous glass substrate having a first surface and a second surface opposite to the first surface, a buffer layer provided on the first surface of the amorphous glass substrate, and a nitride semiconductor stack including at least one gallium nitride layer on the buffer layer, wherein the first surface of the amorphous glass substrate has a concave-convex structure consisting of a flat convex surface and a flat concave surface, and the buffer layer and the nitride semiconductor stack are formed on the concave-convex structure.
[0006] A method for fabricating a nitride semiconductor device according to one embodiment of the present invention includes forming a concave-convex structure consisting of a flat convex surface and a flat concave surface on the first surface of an amorphous glass substrate having a first surface and a second surface opposite to the first surface, forming a buffer layer on the concave-convex structure, and forming a nitride semiconductor stack including at least one gallium nitride layer on the buffer layer, and forming the concave-convex structure by etching the amorphous glass substrate.
[0007] 2B is a diagram showing a cross-sectional structure of a nitride semiconductor device 100 according to one embodiment of the present invention. FIG. 2C is a plan view showing the configuration of an amorphous glass substrate used in the nitride semiconductor device 100 according to one embodiment of the present invention. FIG. 2D is a cross-sectional view of the amorphous glass substrate corresponding to the section A1-A2 shown in FIG. 2A. FIG. 2E is a plan view showing the configuration of an amorphous glass substrate used in the nitride semiconductor device 100 according to one embodiment of the present invention. FIG. 2F is a plan view showing the configuration of an amorphous glass substrate used in the nitride semiconductor device 100 according to one embodiment of the present invention. FIG. 2G is a plan view showing the configuration of an amorphous glass substrate used in the nitride semiconductor device 100 according to one embodiment of the present invention. FIG. 2H is a plan view showing the configuration of an amorphous glass substrate used in the nitride semiconductor device 100 according to one embodiment of the present invention. FIG. 2H is a flow chart illustrating a method for fabricating a nitride semiconductor device according to one embodiment of the present invention. FIG. 2I is a flow chart illustrating a method for fabricating a nitride semiconductor device according to one embodiment of the present invention. FIG. 2J is a cross-sectional view illustrating a method for fabricating a nitride semiconductor device according to one embodiment of the present invention. The present invention relates to a nitride semiconductor device, a nitride semiconductor device including a nitride semiconductor layer, a nitride semiconductor layer ...
[0008] Hereinafter, embodiments of the present invention will be described with reference to the drawings. However, the present invention can be implemented in many different forms, and should not be construed as being limited to the description of the following exemplary embodiments. For clarity of explanation, the drawings may show schematic representations of the width, thickness, shape, etc. of each part compared to the actual form. However, these are merely examples and are not intended to limit the interpretation of the present invention. Furthermore, in this specification and each drawing, elements similar to those previously described with reference to the preceding drawings are designated by the same reference numerals (or reference numerals with A, B, a, b, etc. suffixed thereto), and detailed descriptions may be omitted as appropriate. Furthermore, the letters "first" and "second" attached to each element are convenient labels used to distinguish each element and have no further meaning unless otherwise specified.
[0009] 1 shows a cross-sectional view of a nitride semiconductor device 100A according to one embodiment of the present invention. The nitride semiconductor device 100A includes a buffer layer 104 provided on an amorphous glass substrate 102, a nitride semiconductor stack 106 provided on the buffer layer 104, a passivation layer 108, an n-electrode 110, and a p-electrode 112. As is clear from this structure, the nitride semiconductor device 100A shown in this embodiment is a device that functions as a light-emitting diode (LED).
[0010] The amorphous glass substrate 102 has a first surface F1 and a second surface F2, and a buffer layer 104, a nitride semiconductor stack 106, a passivation layer 108, an n-electrode 110, and a p-electrode 112 are provided on the first surface F1. A compensation layer 114 is provided on the second surface F2 of the amorphous glass substrate 102. The compensation layer 114 is provided in a region overlapping with the buffer layer 104 and the nitride semiconductor stack 106.
[0011] 1 shows a nitride semiconductor stack 106 having a stacked structure of an undoped nitride semiconductor layer 1062, an n-type nitride semiconductor layer 1064, a light-emitting layer 1066, and a p-type nitride semiconductor layer 1068. At least one of the undoped nitride semiconductor layer 1062, the n-type nitride semiconductor layer 1064, and the p-type nitride semiconductor layer 1068 is made of gallium nitride, and the gallium nitride layer has crystallinity. The light-emitting layer 1066 has a structure in which multiple types of gallium nitride-based semiconductor layers with different band gaps are stacked so as to form a quantum well.
[0012] The structure of the nitride semiconductor stack 106 shown in FIG. 1 is an example, and other stack structures may be used as long as they can function as an LED.
[0013] The passivation layer 108 is provided so as to cover the nitride semiconductor stack 106, and has openings in a region in contact with the n-type nitride semiconductor layer 1064 and a region in contact with the p-type nitride semiconductor layer 1068. Through these openings, the n-electrode 110 forms contact with the n-type nitride semiconductor layer 1064, and the p-electrode 112 forms contact with the p-type nitride semiconductor layer 1068.
[0014] The amorphous glass substrate 102 has a concave-convex structure on its first surface F1. That is, the first surface F1 of the amorphous glass substrate 102 has recesses 1022 and protrusions 1024. The recesses 1022 are regions recessed from the protrusions 1024, and the protrusions 1024 are regions protruding from the recesses 1022. The first surface F1 of the amorphous glass substrate 102 is a growth surface for a crystalline nitride semiconductor layer, and the nitride semiconductor stack 106 is formed on this concave-convex surface. Each part of the nitride semiconductor device 100A will be described in detail below.
[0015] (1) Amorphous Glass Substrate Fig. 2A shows a plan view of the amorphous glass substrate 102, and Fig. 2B shows a cross-sectional view corresponding to the line A1-A2 shown in the plan view. As described above, the amorphous glass substrate 102 has a first surface F1 and a second surface F2 opposite to the first surface F1, and the first surface F1 has an uneven structure.
[0016] As shown in the cross-sectional view of FIG. 2B , the recess 1022 has a flat bottom surface, and the protrusion 1024 has a flat top surface. A step is formed at the boundary between the recess 1022 and the protrusion 1024. This step may be vertical or may be an inclined surface as shown. The buffer layer 104 and the nitride semiconductor stack 106 are formed on the first face F1. Considering the coverage of the deposited film, it is preferable that the surface of the step at the boundary between the recess 1022 and the protrusion 1024 has a certain degree of inclination, forming an inclined surface. Furthermore, in order to grow a crystalline gallium nitride-based semiconductor on the first face F1, it is preferable that the recess 1022 has a flat bottom surface, and the protrusion 1024 has a flat top surface.
[0017] The maximum length D1 of the flat surface of the recess 1022 is 5 μm to 80 μm. Similarly, the maximum length D2 of the flat surface of the protrusion 1024 (the distance between the recess 1022 and an adjacent recess) is 5 μm to 80 μm. Furthermore, when the upper plane of the protrusion 1024 is used as a reference, the depth of the recess 1022 is 0.3 μm to 3.0 μm. The amorphous glass substrate 102 has a thickness of 0.5 mm to 1.1 mm. The recess 1022 can also be considered as a region where the surface of the amorphous glass substrate 102 is removed by 1 / 100 or less of its thickness.
[0018] The recesses 1022 and protrusions 1024 having such sizes may be randomly arranged on the first surface F1 of the amorphous glass substrate 102, but are preferably arranged periodically as shown in the figure. The size of the nitride semiconductor device 100A in a planar view can be set as appropriate. The nitride semiconductor device 100A may be, for example, a micro LED having a diagonal length of several tens of micrometers or a mini LED having a diagonal length of approximately one hundred micrometers, or may be a regular LED having a diagonal length of approximately several millimeters. It can be said that the size of the uneven structure formed by the recesses 1022 and protrusions 1024 is sufficiently small compared to such a chip size. In order to grow a homogeneous gallium nitride crystal on the amorphous glass substrate 102 and reduce variation between fabricated devices, the recesses 1022 and protrusions 1024 are preferably arranged periodically.
[0019] The amorphous glass substrate 102 preferably has a low alkali metal content to prevent metal contamination of the nitride semiconductor stack 106. For example, the alkali metal content of the amorphous glass substrate 102 is preferably 0.1 mass % or less. Specifically, the amorphous glass substrate 102 is preferably amorphous glass made of, for example, aluminoborosilicate glass or aluminosilicate glass. The amorphous glass substrate 102 is used in liquid crystal displays and organic electroluminescence (organic electroluminescence) displays, and large-area glass substrates known as mother glass that are available on the market can be used.
[0020] Although there are no limitations on the thickness of the amorphous glass substrate 102, from the viewpoint of reducing warpage, it is preferable that the thickness be sufficiently thicker than the thickness of the nitride semiconductor stack 106. For example, it is preferable that the amorphous glass substrate 102 has a thickness that is 50 times or more the thickness of the nitride semiconductor stack 106. As described above, it is preferable that the amorphous glass substrate 102 has a thickness of 0.5 mm to 1.0 mm.
[0021] The amorphous glass substrate 102 is generally amorphous and does not have a crystalline structure, but may have a crystalline structure in a small amount. The amorphous glass substrate 102 is preferably transparent to visible light.
[0022] The amorphous glass substrate 102 preferably has heat resistance capable of withstanding the process temperature (maximum processing temperature) of the nitride semiconductor device 100A. For example, when the process temperature (maximum processing temperature) of the nitride semiconductor device 100A is less than 650°C, the amorphous glass substrate 102 preferably has a heat resistance of at least 650°C. Specifically, the lower limit of the glass transition point of the amorphous glass substrate 102 is 650°C or higher, and preferably 720°C or higher. The upper limit of the glass transition point of the amorphous glass substrate 102 is 900°C or lower, and preferably 810°C or lower. For the same reason, the lower limit of the softening point of the amorphous glass substrate 102 is 900°C or higher, and preferably 950°C or higher. The upper limit of the softening point of the amorphous glass substrate 102 is 1150°C or lower, and preferably 1050°C or lower.
[0023] The upper limit of the thermal expansion coefficient of the amorphous glass substrate 102 is 4.2×10 -6 / K (4.2 ppm / K), or even less than 4.0 × 10 -6 The lower limit of the thermal expansion coefficient of the amorphous glass substrate 102 is preferably less than 3.0×10 -6 / K (3.0 ppm / K) and even 3.5 × 10 -6 / K (3.5 ppm / K). That is, the thermal expansion coefficient of the amorphous glass substrate 102 is approximately 3.5×10 -6 ~3.9 x 10 -6 / K (3.5 to 3.9 ppm / K).
[0024] In contrast to these thermal expansion coefficients, the thermal expansion coefficients of aluminum oxide and aluminum nitride as the buffer layer 104 and compensation layer 114 formed on the amorphous glass substrate 102, and gallium nitride constituting the nitride semiconductor stack 106, are different. Table 1 shows the main physical properties of each component, specifically the thermal expansion coefficients, densities, lattice constants, and refractive indices of glass, aluminum oxide, aluminum nitride, and gallium nitride. Focusing on the thermal expansion coefficient, glass (amorphous glass substrate) is amorphous and therefore has no anisotropy in its thermal expansion coefficient, whereas aluminum oxide, aluminum nitride, and gallium nitride are crystalline and have different thermal expansion coefficients in the a-axis direction (direction parallel to the substrate surface) and the c-axis direction (direction perpendicular to the substrate surface).
[0025] While the amorphous glass substrate 102 thermally expands isotropically, gallium nitride thermal expansion is not isotropic, and there is a large difference between the thermal expansion coefficients of the two in the a-axis direction. Therefore, it is expected that thermal stress will act in an unintended direction on the gallium nitride on the amorphous glass substrate 102, causing distortion in the crystal.
[0026] As described above, the amorphous glass substrate 102 according to this embodiment has a concave-convex structure on the first surface F1, which includes thick regions (regions with large volume) and thin regions (regions with small volume). By locally varying the thickness (volume) of the amorphous glass substrate 102 in this manner, the isotropy of thermal expansion can be alleviated, thereby reducing the effect of thermal stress on the gallium nitride layer deposited thereon. Furthermore, by providing a concave-convex structure on the amorphous glass substrate 102, the nitride semiconductor formed in the recesses is subjected to greater compressive stress due to substrate heating during film formation than the portions adjacent to the protrusions, which has an advantageous effect on three-dimensional crystal growth.
[0027] Although not shown, a base layer may be provided on the first surface F1 of the amorphous glass substrate 102 to prevent diffusion of impurities (e.g., moisture or sodium (Na)). The base layer is preferably formed of an inorganic insulating material such as silicon oxide or silicon nitride.
[0028] (2) Compensation Layer The compensation layer 114 is provided on the second surface F2 of the amorphous glass substrate 102. The compensation layer 114 has a thermal expansion coefficient within a predetermined range, thereby reducing warping of the amorphous glass substrate 102 due to differences in the thermal expansion coefficient between the amorphous glass substrate 102 and each layer forming the nitride semiconductor stack 106. The thermal expansion coefficient of the compensation layer 114 preferably exceeds that of the amorphous glass substrate 102 and is less than that of each layer of the nitride semiconductor stack 106 (the undoped nitride semiconductor layer 1062, the n-type nitride semiconductor layer 1064, the light-emitting layer 1066, and the p-type nitride semiconductor layer 1068).
[0029] The lower limit of the thermal expansion coefficient of the compensation layer 114 is, for example, 4.0×10 -6 / K (4.0 ppm / K), preferably 4.1 × 10 -6 / K (4.1 ppm / K). The upper limit of the thermal expansion coefficient of the compensation layer 114 is, for example, 5.0×10 -6 / K (5.0 ppm / K), preferably 4.6 × 10 -6 / K (4.6 ppm / K) or less. As shown in Table 1, the thermal expansion coefficient of aluminum oxide is 4.5 (a-axis) to 5.3 (c-axis), and the thermal expansion coefficient of aluminum nitride is 4.2 (a-axis) to 5.3 (c-axis), and they can be suitably used as the compensation layer 114. However, the upper and lower limits of the thermal expansion coefficient of the compensation layer 114 are not limited to these.
[0030] The thermal conductivity of the compensation layer 114 is, for example, preferably greater than 10 W / m·K, and even greater than 40 W / m·K. By setting the thermal conductivity of the compensation layer 114 within a predetermined range, heat can be conducted evenly throughout the amorphous glass substrate 102 in the process of forming the nitride semiconductor stack 106, thereby achieving uniform in-plane characteristics. The thermal conductivity of the compensation layer 114 can be adjusted by the film density. The lower limit of the film density of the compensation layer 114 is, for example, 2.50 g / cm. 3 or more, and further 2.60 g / cm 3 The upper limit of the film density of the compensation layer 114 is 4.10 g / cm 3 or less, and further 4.00 g / cm 3 It is preferable that:
[0031] As shown in Table 1, when aluminum oxide is used as the compensation layer 114, 3 When aluminum nitride is used, a film density of 3.30 g / cm can be obtained. 3 In contrast, the density of glass is 2.50 to 2.59 g / cm 3 Therefore, by using aluminum oxide or aluminum nitride, it is possible to form a dense compensation layer 114. Furthermore, by densifying the compensation layer 114, it is possible to reduce outgassing from the amorphous glass substrate 102, and it is possible to reduce the amount of impurities introduced into the nitride semiconductor layer to be deposited.
[0032] The material forming the compensation layer 114 is not particularly limited as long as it satisfies the above-described physical properties. For example, the compensation layer 114 can be formed of a single layer of aluminum nitride or aluminum oxide. The compensation layer 114 may have a structure in which multiple layers are stacked. For example, the compensation layer 114 may have a structure in which an aluminum oxide layer and an aluminum nitride layer are stacked in this order from the second surface F2 side of the amorphous glass substrate 102.
[0033] As shown in Table 1, the refractive index of aluminum oxide is 1.77, and the refractive index of aluminum nitride is 2.05. In contrast, the refractive index of glass is 1.51. Therefore, when aluminum oxide or aluminum nitride is used as the compensation layer 114, the difference in refractive index allows light to be reflected at the interface with the amorphous glass substrate 102. That is, as shown in FIG. 1 , of the light emitted from the light-emitting layer 1066, the light that has transmitted through the amorphous glass substrate 102 can be reflected at the interface between the amorphous glass substrate 102 and the compensation layer 114, thereby increasing the amount of light emitted from the first surface F1.
[0034] There are no limitations on the film thickness of the compensation layer 114, and the film thickness can be set appropriately from the viewpoint of preventing warpage of the amorphous glass substrate 102. It is preferable that the compensation layer 114 is not made excessively thinner than the thickness of the nitride semiconductor stack 106. For example, the compensation layer 114 may have a thickness that is 80% or more of the thickness of the nitride semiconductor stack 106.
[0035] (3) Buffer Layer The buffer layer 104 is provided on the first face F1 of the amorphous glass substrate 102. The buffer layer 104 is provided to improve the crystal orientation of the nitride semiconductor film formed on the amorphous glass substrate 102. In other words, the buffer layer 104 is provided to promote crystal growth of the nitride semiconductor film in the c-axis direction.
[0036] Nitride semiconductors such as gallium nitride have a hexagonal close-packed structure and grow in the c-axis direction to minimize surface energy. As shown in Table 1, the amorphous glass substrate 102 is amorphous, so its lattice constant cannot be specified, whereas the lattice constant of gallium nitride is 0.3189 nm (3.189 Å), resulting in a lattice mismatch between the two. Therefore, even if a gallium nitride film is deposited directly on the amorphous glass substrate 102, crystal growth will not occur due to the lattice mismatch, and the c-axis orientation will not be achieved. Therefore, to promote crystallization of the nitride semiconductor film, a buffer layer 104 is provided on the amorphous glass substrate 102. It is preferable that the buffer layer 104 be c-axis oriented.
[0037] The buffer layer 104 is formed of a thin film having a hexagonal close-packed structure, a face-centered cubic structure, or a structure equivalent thereto. Here, a hexagonal close-packed structure or a structure equivalent thereto refers to a crystal structure in which the c-axis does not form a 90° angle with respect to the a-axis and the b-axis. When the buffer layer 104 has such a structure, crystal growth in the c-axis direction of the nitride semiconductor film is promoted, thereby improving the crystallinity.
[0038] The buffer layer 104 is made of, for example, aluminum nitride (AlN) or aluminum oxide (Al x O y ), zinc oxide (ZnO), lithium niobate (LiNbO), BiLaTiO, SrFeO, BiFeO, BaFeO, ZnFeO, PMnN-PZT, or biological apatite (BAp) can be used. The buffer layer 104 can be formed by sputtering, vapor phase growth, or the like.
[0039] The buffer layer 104 may be a single layer made of an insulating material as described above, or may have a structure in which multiple layers are stacked. For example, the buffer layer 104 may have a structure in which an aluminum oxide layer and an aluminum nitride layer are stacked in this order from the first surface F1 side of the amorphous glass substrate 102.
[0040] Referring to Table 1, it can be seen that the difference in thermal expansion coefficient between aluminum oxide / aluminum nitride and gallium nitride is smaller than the difference in thermal expansion coefficient between glass and gallium nitride. That is, by using aluminum oxide or aluminum nitride as the buffer layer 104, the difference in thermal expansion coefficient between the buffer layer 104 and the gallium nitride layer as a nitride semiconductor layer can be made smaller than the difference in thermal expansion coefficient between the amorphous glass substrate 102 and the gallium nitride layer as a nitride semiconductor layer. In this way, by providing a concave-convex structure on the first surface F1 of the amorphous glass substrate 102 and providing the buffer layer 104 between the amorphous glass substrate 102 and the nitride semiconductor stack 106, the difference in thermal expansion coefficient can be alleviated.
[0041] Furthermore, as shown in Table 1, the refractive index of aluminum oxide is 1.77, and the refractive index of aluminum nitride is 2.05. These refractive indices are intermediate between the refractive index of glass, 1.51, and the refractive index of gallium nitride, 2.4. Therefore, by using aluminum oxide or aluminum nitride as the buffer layer 104, it is possible to prevent light emitted from the light-emitting layer 1066 of the nitride semiconductor stack 106 from being reflected at the interface with the amorphous glass substrate 102.
[0042] Furthermore, by forming the buffer layer 104 and the compensation layer 114 from the same material, aluminum oxide and aluminum nitride, the amorphous glass substrate 102 is sandwiched between layers made of the same material, thereby reducing warping.
[0043] The crystallinity of a nitride semiconductor film is affected not only by the crystallinity of the base but also by minute irregularities on the surface of the base. Therefore, it is preferable that the buffer layer 104 has a smooth surface with minimal irregularities. For example, the arithmetic mean roughness (Ra) of the surface of the buffer layer 104 is preferably smaller than 2.3 nm. Furthermore, the root-mean-square roughness (Rq) of the surface of the buffer layer 104 is preferably smaller than 2.9 nm. If the surface roughness of the buffer layer 104 is within this range, the crystallinity of the nitride semiconductor film can be improved. From the viewpoint of improving the surface flatness, it is preferable that the film thickness of the buffer layer 104 be 20 nm or more.
[0044] (4) Nitride Semiconductor Stack The nitride semiconductor stack 106 includes an undoped nitride semiconductor layer 1062, an n-type nitride semiconductor layer 1064, a light emitting layer 1066, and a p-type nitride semiconductor layer 1068. Details of each layer are provided below.
[0045] (4-1) Undoped Nitride Semiconductor Layer In order to reduce crystal dislocations in the n-type nitride semiconductor layer 1064, an undoped nitride semiconductor layer 1062 is provided on the buffer layer 104. The undoped nitride semiconductor layer 1062 is formed using the same semiconductor material as the n-type nitride semiconductor layer 1064. For example, the undoped nitride semiconductor layer 1062 is formed of gallium nitride. Note that "undoped" means that the layer does not intentionally contain impurity elements intended for valence electron control, and the undoped nitride semiconductor layer 1062 may contain unavoidable impurity elements such as oxygen, carbon, and hydrogen. There are no particular limitations on the film thickness of the undoped nitride semiconductor layer 1062.
[0046] (4-2) n-Type Nitride Semiconductor Layer The n-type nitride semiconductor layer 1064 is doped with impurities such as silicon (Si) or germanium (Ge) to impart n-type conductivity to the nitride semiconductor film. That is, an n-type nitride semiconductor layer 1064 in which silicon (Si) or germanium (Ge) is doped to a nitride semiconductor film is used as the n-type nitride semiconductor layer 1064. There are no particular limitations on the thickness of the n-type nitride semiconductor layer 1064, but it is preferable that the n-type nitride semiconductor layer 1064 have a thickness of, for example, 50 nm or more and less than 3000 nm. By forming the n-type nitride semiconductor layer 1064 with such a thickness in addition to the undoped nitride semiconductor layer 1062, the uneven structure formed on the first surface F1 of the amorphous glass substrate 102 can be embedded, thereby obtaining a flat surface.
[0047] (4-3) Light-Emitting Layer The light-emitting layer 1066 is a region that emits light by recombining electrons transported from the n-type nitride semiconductor layer 1064 and holes transported from the p-type nitride semiconductor layer 1068. The light-emitting layer 1066 has a multiple quantum well (MQW) structure. The light-emitting layer 1066 preferably has a quantum well structure in which, for example, gallium nitride (GaN) layers and indium gallium nitride (InGaN) layers are alternately stacked.
[0048] (4-4) p-Type Nitride Semiconductor Layer The p-type nitride semiconductor layer 1068 is doped with an impurity such as magnesium (Mg) to impart p-type conductivity to the nitride semiconductor film. That is, a p-type nitride semiconductor film in which magnesium is doped is used as the p-type nitride semiconductor layer 1068. Zinc (Zn) can also be used as the impurity of the p-type nitride semiconductor layer 1068. There are no particular limitations on the thickness of the p-type nitride semiconductor layer 1068, but it is preferable that the thickness be, for example, 50 nm or more and less than 500 nm.
[0049] (5) Passivation Layer The passivation layer 108 is formed of a silicon oxide film, a silicon nitride film, or an aluminum oxide film. The passivation layer 108 may have a structure in which a silicon oxide film and a silicon nitride film are stacked. The passivation layer 108 is provided so as to cover the nitride semiconductor stack 106.
[0050] (6) n-Electrode and p-Electrode The n-electrode 110 and p-electrode 112 are provided on the passivation layer 108. The n-electrode 110 makes contact with the n-type nitride semiconductor layer 1064 through an opening formed in the passivation layer 108 that exposes the n-type nitride semiconductor layer 1064, and the p-electrode 112 makes contact with the p-type nitride semiconductor layer 1068 through an opening formed in the passivation layer 108 that exposes the p-type nitride semiconductor layer 1068.
[0051] The n-electrode 110 is formed of a metal material. When the work function of the n-type nitride semiconductor layer 1064 is 3 eV to 4 eV, the n-electrode 110 is formed of a conductive material with a work function of 4.5 eV or higher, such as nickel (Ni), gold (Au), platinum (Pt), silver (Ag), or p-type silicon. The n-electrode 110 may have a metal layer such as aluminum (Al) stacked on top of such a metal layer. The n-electrode 110 may also be formed, for example, including copper (Cu) and a barrier metal layer that prevents the diffusion of copper (Cu). The barrier metal layer may be formed of titanium (Ti), titanium nitride (TiN), tantalum (Ta), tantalum nitride (TaN), or the like. The n-electrode 110 may have a structure in which titanium (Ti), titanium nitride (TiN), and copper (Cu) are stacked in this order.
[0052] The p-electrode 112 is formed of a metal material such as gold (Au), titanium (Ti)-gold (Au) alloy, or nickel (Ni), or a transparent conductive film such as indium tin oxide (ITO). As a material for forming the p-electrode 112, for example, a metal material having a work function of less than 4.5 eV, such as aluminum (Al) or titanium (Ti), is selected. Although not shown, the p-electrode 112 is formed by depositing an indium tin oxide (In 2 O 3 The conductive layer 12 may be formed of a conductive metal oxide material such as zinc oxide (ZnO) or indium tin oxide (ITO).
[0053] As described above, the nitride semiconductor device 100A according to this embodiment can reduce the isotropy of thermal expansion by forming an uneven structure on the surface of the amorphous glass substrate 102, and can also reduce the mismatch between the thermal expansion coefficient of the amorphous glass substrate 102 and the thermal expansion coefficient of the gallium nitride based semiconductor layer that forms the nitride semiconductor stack 106. As a result, distortion due to thermal stress can be prevented from being applied to the nitride semiconductor stack 106 formed on the amorphous glass substrate 102, and the crystallinity of the gallium nitride based semiconductor layer can be improved.
[0054] [Second embodiment] In Fig. 2A, the shape of the recess 1022 is quadrangular in plan view, but the uneven structure formed on the first surface F1 of the amorphous glass substrate 102 is not limited to this shape. For example, as shown in Fig. 2C, the shape of the recess 1022 may be circular in plan view. Furthermore, as shown in Fig. 2D, the shape of the recess 1022 may be hexagonal in plan view. Furthermore, although not shown, the shape of the recess 1022 may be any polygonal shape.
[0055] 2A, 2C, and 2D show examples in which the recesses 1022 are of the same shape and size and are periodically arranged, but the uneven structure formed on the first surface F1 of the amorphous glass substrate 102 is not limited to such shapes. For example, as shown in FIGS. 2E and 2F, the recesses may have different sizes in a planar view, and the uneven structure may be formed by a large pattern of recesses 1022A and a small pattern of recesses 1022B. FIG. 2E shows an example in which the recesses 1022A and 1022B are circular, and FIG. 2F shows an example in which the recesses 1022A and 1022B are hexagonal, but the recesses 1022A and 1022B may be rectangular or polygonal with a greater number of corners.
[0056] Although not shown, the uneven structure formed on the first surface F1 of the amorphous glass substrate 102 shown in Figures 2A, 2C, 2D, 2E, and 2F may have a structure in which the height relationship between the recesses 1022 and the protrusions 1024 is reversed.
[0057] The configuration of the amorphous glass substrate 102 shown in this embodiment can be applied to the nitride semiconductor device 100A shown in the first embodiment, and can achieve the same effects.
[0058] Third Embodiment This embodiment shows an example of a method for fabricating the nitride semiconductor device 100A shown in the first embodiment. Fig. 3A is a flowchart illustrating the order of the method for fabricating the nitride semiconductor device 100A, and Figs. 4A to 4F are cross-sectional views illustrating each step. The following description will be made with reference to these drawings as appropriate.
[0059] First, the amorphous glass substrate 102 is prepared ( FIG. 3A : S200), and the compensation layer 114 is formed on the second surface F2 ( FIG. 3A : S202). Then, the first surface F1 side of the amorphous glass substrate 102 is processed ( FIG. 3A : S204). Processing the first surface F1 side of the amorphous glass substrate 102 includes the steps of forming a resist mask ( FIG. 3A : S2042), etching the first surface F1 of the amorphous glass substrate 102 ( FIG. 3A : S2044), and then peeling off the resist mask.
[0060] 4A shows a step in which a compensation layer 114 is formed on the second face F2 of the amorphous glass substrate 102 and a resist mask 150 is formed on the first face F1. The compensation layer 114 is formed, for example, by sputtering. As shown in the first embodiment, the compensation layer 114 is formed of a material such as aluminum oxide or aluminum nitride. Then, a resist mask 150 is formed on the first face F1 of the amorphous glass substrate 102. The resist mask 150 is formed, for example, by applying a photoresist and exposing it to light. The resist mask 150 has a pattern that covers the regions of the first face F1 of the amorphous glass substrate 102 that will become the convex portions 1024 and exposes the regions that will become the concave portions 1022.
[0061] Then, as shown in FIG. 4B , the amorphous glass substrate 102 is etched. Wet etching is used to etch the amorphous glass substrate 102. For example, an etching solution containing hydrofluoric acid, ammonium fluoride, and hydrochloric acid as its main components can be used. This etching process forms a recess 1022 on the first surface F1 of the amorphous glass substrate 102. Because the recess 1022 is formed by wet etching, the sidewall surface is not necessarily vertical but is formed in a slightly inclined shape. Although not shown in FIG. 4B , a protective film may be attached to the second surface F2 of the amorphous glass substrate 102 to prevent it from being eroded by the etching solution. After etching is completed, the resist mask 150 is removed.
[0062] Next, the buffer layer 104 is formed on the first face F1 of the amorphous glass substrate 102 ( FIG. 3A : S206), and then the nitride semiconductor stack 106 is formed ( FIG. 3AA : S208). The nitride semiconductor stack 106 is formed in the following order: the undoped nitride semiconductor layer 1062 ( FIG. 3A : S2082), the n-type nitride semiconductor layer 1064 ( FIG. 3A : S2084), the light-emitting layer 1066 ( FIG. 3A : S2086), and the p-type nitride semiconductor layer 1068 ( FIG. 3A : S2088).
[0063] 4C shows a stage in which a buffer layer 104 is formed and a nitride semiconductor stack 106 is formed on the buffer layer 104. As shown in the first embodiment, the buffer layer 104 is formed of a material such as aluminum oxide or aluminum nitride. For example, an aluminum nitride film is formed as the buffer layer 104 by a sputtering method. As described in the first embodiment, the aluminum nitride film formed as the buffer layer 104 is a crystalline film with a c-axis orientation.
[0064] The undoped nitride semiconductor layer 1062, n-type nitride semiconductor layer 1064, light-emitting layer 1066, and p-type nitride semiconductor layer 1068 are formed in this order on the buffer layer 104 by sputtering. For example, the undoped nitride semiconductor layer 1062, n-type nitride semiconductor layer 1064, and p-type nitride semiconductor layer 1068 are formed of intrinsic or respective conductivity type gallium nitride films. As described in the first embodiment, the light-emitting layer 1066 is formed to have a quantum well structure by alternately stacking gallium nitride films and indium gallium nitride films.
[0065] The deposition of a gallium nitride film by sputtering uses a gallium nitride sintered body as the sputtering target. An inert gas such as argon (Ar) or krypton (Kr) is used as the sputtering gas, and the substrate heating temperature during deposition is controlled to 400°C to 600°C. By using a multi-chamber sputtering apparatus and installing sputtering targets suitable for depositing the undoped nitride semiconductor layer 1062, n-type nitride semiconductor layer 1064, light-emitting layer 1066, and p-type nitride semiconductor layer 1068 in each chamber, these layers can be deposited consecutively in a vacuum. The nitride semiconductor stack 106 is formed on the buffer layer 104, which has c-axis-oriented crystallinity, and therefore has controlled crystal orientation and high crystallinity.
[0066] After each layer of the nitride semiconductor layer is formed, a heat treatment for activation is performed ( FIG. 3A : S210). The heat treatment is preferably performed in a nitrogen atmosphere at a temperature of 600° C. to less than 800° C. This heat treatment activates impurities for valence electron control in the n-type nitride semiconductor layer 1064 and the p-type nitride semiconductor layer 1068, improving the conductivity.
[0067] Through the above steps, the buffer layer 104 and the nitride semiconductor stack 106 are formed over substantially the entire first surface F1 of the amorphous glass substrate 102. Then, the nitride semiconductor stack 106 is processed by photolithography and etching so that the nitride semiconductor stack 106 remains in an island shape in the region where the nitride semiconductor device will be formed and so that a contact can be formed with the n-type nitride semiconductor layer 1064 ( FIG. 3A : S212).
[0068] 4D shows the state in which the nitride semiconductor stack 106 and the buffer layer 104 have been etched. In the etching process, a predetermined resist pattern is formed on the nitride semiconductor stack 106 by photolithography, and then etching is performed using a dry etching apparatus. The etching gas used is Cl 2 A chlorine-based etching gas such as the following is used. Since the buffer layer 104 is thin, it is etched simultaneously with the nitride semiconductor stack 106 during this etching process.
[0069] 4E shows a step of forming a contact region for the n-electrode 110 to make contact with the n-type nitride semiconductor layer 1064. In order for the n-electrode 110 to make contact with the n-type nitride semiconductor layer 1064, the p-type nitride semiconductor layer 1068 and the light emitting layer 1066 are selectively etched to expose the n-type nitride semiconductor layer 1064. In this manner, the nitride semiconductor stack 106 on the first face F1 side of the amorphous glass substrate 102 is etched, but the compensation layer 114 on the second face F2 of the amorphous glass substrate 102 remains to prevent warping of the substrate during the process.
[0070] Next, the passivation layer 108 is formed ( FIG. 3A : S214). FIG. 4F shows the stage where the passivation layer 108 is formed so as to cover the nitride semiconductor stack 106. Note that the passivation layer 108 is not limited to being formed by sputtering, and may be formed by, for example, CVD.
[0071] Thereafter, contact holes are formed in the passivation layer 108 ( FIG. 3A : S216), followed by the formation of the n-electrode 110 ( FIG. 3A : S218), and the formation of the p-electrode 112 ( FIG. 3A : S220). Furthermore, annealing is performed so that the n-electrode 110 and the p-electrode 112 make ohmic contact with their respective nitride semiconductor layers ( FIG. 3A : S222). The contact holes are formed in the passivation layer 108 to expose the top surfaces of the n-type nitride semiconductor layer 1064 and the p-type nitride semiconductor layer 1068. The n-electrode 110 and the p-electrode 112 are then formed. As described in the first embodiment, the conductive material suitable for forming the n-electrode 110 and the conductive material suitable for forming the p-electrode 112 are different, and therefore, these two types of electrodes are fabricated in separate processes. The order in which the n-electrode 110 and the p-electrode 112 are fabricated is not limited, and the p-electrode 112 may be fabricated first. Thereafter, annealing is performed to reduce the contact resistance of the n-electrode 110 and the p-electrode 112. Even at this stage, the compensation layer 114 is provided over the entire second surface F2 of the amorphous glass substrate 102, thereby preventing the substrate from warping due to the heat treatment.
[0072] The nitride semiconductor device 100A shown in FIG. 1 is fabricated through the above steps. According to the method for fabricating the nitride semiconductor device 100A shown in this embodiment, providing a concave-convex structure on the first surface F1 of the amorphous glass substrate 102 reduces isotropic thermal expansion, thereby reducing stress acting on the nitride semiconductor stack 106 due to differences in thermal expansion coefficients. Furthermore, the nitride semiconductor stack 106 is subjected to compressive stress in the recessed portions, which promotes three-dimensional crystal growth. These effects prevent the layers forming the nitride semiconductor stack 106 from peeling off from the amorphous glass substrate 102 during the manufacturing process, enabling the formation of high-quality crystals.
[0073] Fourth Embodiment This embodiment illustrates a nitride semiconductor device 100B that differs from the first embodiment in the configuration of the compensation layer 114 and is capable of emitting light from the side of the amorphous glass substrate 102. In the following description, only the parts that are different from the first embodiment will be described, and descriptions of the parts that are in common with the first embodiment will be omitted as appropriate.
[0074] 5 shows the configuration of a nitride semiconductor device 100B according to this embodiment. The nitride semiconductor device 100B is similar to the nitride semiconductor device 100A shown in the first embodiment in that a buffer layer 104, a nitride semiconductor stack 106, a passivation layer 108, an n-electrode 110, and a p-electrode 112 are provided on the first face F1 side of the amorphous glass substrate 102, and a compensation layer 114 is provided on the second face F2 side. However, the nitride semiconductor device 100B differs from the nitride semiconductor device 100A shown in the first embodiment in that the compensation layer 114 does not cover the entire surface of the amorphous glass substrate 102, but has openings 1142 that expose portions of the second face F2. The size and shape (pattern) of the openings 1142 in a plan view are arbitrary, and may have a dotted pattern, a striped pattern, or a grid pattern.
[0075] When an aluminum oxide or aluminum nitride layer is provided as compensation layer 114, the light emitted from light-emitting layer 1066 is reflected due to the difference in refractive index with amorphous glass substrate 102, as shown in Table 1. In contrast, an interface with air is formed in the region where opening 1142 is provided, making it possible to efficiently extract light from the second surface side.
[0076] 3B shows a flowchart illustrating the process of forming the opening 1142 in the compensation layer 114. The formation of the opening 1142 in the compensation layer 114 is performed after the contact annealing (FIG. 3B: S222) is completed. Because no high-temperature heat treatment is performed in the subsequent steps, removing a portion of the compensation layer 114 does not cause a problem such as warping of the amorphous glass substrate 102.
[0077] First, a protective film is attached to the first surface of the amorphous glass substrate 102 to protect the nitride semiconductor stack 106, the n-electrode 110, and the p-electrode 112. Then, the compensation layer 114 is processed ( FIG. 3C : S226). In processing the compensation layer 114, a resist mask is formed in a predetermined pattern ( FIG. 3C : S2262), followed by etching ( FIG. 3B : S2264). The compensation layer 114 is etched, for example, by dry etching. When an aluminum nitride film is formed as the compensation layer 114, etching can be performed using a chlorine-based gas. The resist mask is then peeled off, and the protective film is removed ( FIG. 3B : S228), yielding the nitride semiconductor device 100B having the structure shown in FIG. 5.
[0078] According to this embodiment, it is possible to provide a nitride semiconductor device 100B that can emit light from the amorphous glass substrate 102 side by removing a portion of the compensation layer 114. The nitride semiconductor device 100 is similar to the nitride semiconductor device 100A shown in the first embodiment except for the structure of the compensation layer 114, and can achieve the same effects.
[0079] Fifth Embodiment This embodiment illustrates an example of a nitride semiconductor device 100C having a structure in which the nitride semiconductor stack 106 is separated from the amorphous glass substrate 102. In the following description, differences from the first embodiment will be described, and descriptions of common parts will be omitted as appropriate.
[0080] Fig. 6 shows the configuration of a nitride semiconductor device 100C according to this embodiment. As shown in Fig. 6, the nitride semiconductor device 100C has a structure in which the layers above the nitride semiconductor stack 106 are peeled off and thinned at the interface between the buffer layer 104 and the undoped nitride semiconductor layer 1062. Separation into the amorphous glass substrate 102 side and the nitride semiconductor stack 106 side can be performed by irradiating with laser light.
[0081] 3C shows a flowchart illustrating the process of separating layers above the nitride semiconductor stack 106 from the amorphous glass substrate 102. When the nitride semiconductor device shown in the third embodiment is manufactured using a large-area amorphous glass substrate called mother glass, a scribing process is performed to divide the large-area amorphous glass substrate into multiple pieces before the peeling process by laser light irradiation (FIG. 3C: S230). The scribing process is performed by a laser scribing method or a mechanical scribing method. The laser scribing method is a method of processing the amorphous glass substrate by irradiating it with concentrated laser light to locally heat and melt it, while the mechanical scribing method is a method of breaking the amorphous glass substrate by scoring the glass with a scribing blade (e.g., a scribing wheel).
[0082] Thereafter, laser light is irradiated from the amorphous glass substrate 102 side to perform a peeling process on the nitride semiconductor stack 106 ( FIG. 3C : S232). The laser light used is laser light that is transmitted through the amorphous glass substrate 102 and has a wavelength that is absorbed by the nitride semiconductor. For example, since the band gap of gallium nitride is 3.4 eV, by using the third harmonic (355 nm, 3.49 eV) of a YAG laser, the laser light is not absorbed by the aluminum oxide and aluminum nitride that form the amorphous glass substrate 102, buffer layer 104, and compensation layer 114, and can be peeled off by locally heating the undoped nitride semiconductor layer 1062 at the interface between the nitride semiconductor stack 106 and the buffer layer 104.
[0083] During the peeling process, a protective film may be attached to the first surface F1 of the amorphous glass substrate 102 to protect the nitride semiconductor device 100C after peeling. The peeled nitride semiconductor device 100C has a thickness of about 10 μm, and is therefore mounted on a predetermined die for chip formation ( FIG. 3C : S234). The peeled nitride semiconductor device 100C can also be mounted on an array substrate (also called a "backplane") on which pixel circuits are formed using thin-film transistors.
[0084] According to this embodiment, the nitride semiconductor device 100C can be made thinner by peeling off the layers above the nitride semiconductor stack 106 from the amorphous glass substrate 102. The nitride semiconductor device 100C has a structure in which the layers are peeled off at the interface between the buffer layer 104 and the nitride semiconductor stack 106, and the peeled surface has an uneven surface that imitates the uneven structure of the amorphous glass substrate 102. Therefore, by using this surface as a light emission surface, the light extraction efficiency can be improved.
[0085] As described above, the configurations of the nitride semiconductor devices shown in the first to fifth embodiments can be combined as appropriate as long as they are not mutually contradictory. Furthermore, even if a person skilled in the art appropriately adds or deletes components or modifies the design based on each embodiment, or adds or omits processes or modifies conditions, these will also be included in the scope of the present invention as long as they comply with the gist of the present invention.
[0086] Even if there are other effects and advantages different from those brought about by the above-mentioned embodiments, if they are clear from the description in this specification or can be easily predicted by a person skilled in the art, they are naturally understood to be brought about by the present invention.
[0087] 100: nitride semiconductor device, 102: amorphous glass substrate, 1022: recess, 1024: protrusion, 104: buffer layer, 106: nitride semiconductor stack, 1062: undoped nitride semiconductor layer, 1064: n-type nitride semiconductor layer, 1066: light-emitting layer, 1068: p-type nitride semiconductor layer, 108: passivation layer, 110: n-electrode, 112: p-electrode, 114: compensation layer, 1142: opening, 150: resist mask, F1: first surface, F2: second surface
Claims
1. A nitride semiconductor device comprising: an amorphous glass substrate having a first surface and a second surface opposite to the first surface; a buffer layer provided on the first surface of the amorphous glass substrate; and a nitride semiconductor stack including at least one gallium nitride layer on the buffer layer, wherein the first surface of the amorphous glass substrate has a concave-convex structure consisting of a flat convex surface and a flat concave surface, and the buffer layer and the nitride semiconductor stack are formed on the concave-convex structure.
2. The nitride semiconductor device according to claim 1, wherein the uneven structure has a length of the flat convex surface and the flat concave surface of 5 μm to 80 μm, and a height difference between the flat convex surface and the flat concave surface of 0.3 μm to 3 μm.
3. The nitride semiconductor device according to claim 1, wherein a thermal expansion coefficient of the buffer layer has a value between a thermal expansion coefficient of the amorphous glass substrate and a thermal expansion coefficient of the at least one gallium nitride layer, and a difference between the thermal expansion coefficient of the buffer layer and the thermal expansion coefficient of the at least one gallium nitride layer is smaller than a difference between the thermal expansion coefficients of the amorphous glass substrate and the at least one gallium nitride layer.
4. The nitride semiconductor device according to claim 3, wherein the refractive index of said buffer layer has a value between the refractive index of said amorphous glass substrate and the refractive index of said at least one gallium nitride layer.
5. The nitride semiconductor device according to claim 1, further comprising a compensation layer on said second surface of said amorphous glass substrate, said compensation layer having a refractive index between the refractive index of said amorphous glass substrate and the refractive index of said at least one gallium nitride layer.
6. The nitride semiconductor device according to claim 1, wherein the buffer layer includes at least one layer selected from an aluminum nitride layer and an aluminum oxide layer.
7. The nitride semiconductor device according to claim 5, wherein the compensation layer includes at least one layer selected from an aluminum nitride layer and an aluminum oxide layer.
8. The nitride semiconductor device according to claim 1, wherein the buffer layer is formed by laminating an aluminum oxide layer and an aluminum nitride layer in this order from the first surface side.
9. The nitride semiconductor device according to claim 5, wherein the compensation layer is formed by laminating an aluminum oxide layer and an aluminum nitride layer in this order from the second surface side.
10. The nitride semiconductor device according to claim 1, wherein the nitride semiconductor stack has a structure in which an n-type nitride semiconductor layer, a light emitting layer, and a p-type nitride semiconductor layer are stacked from the buffer layer side, and the at least one gallium nitride layer is composed of the n-type nitride semiconductor layer and the p-type nitride semiconductor layer.
11. The nitride semiconductor device according to claim 10, wherein the nitride semiconductor laminate is peeled off from an interface with the buffer layer, and the peeled surface serves as a light emitting surface.
12. A method for manufacturing a nitride semiconductor device, comprising: forming a concave-convex structure consisting of flat convex surfaces and flat concave surfaces on an amorphous glass substrate having a first surface and a second surface opposite to the first surface; forming a buffer layer on the concave-convex structure; and forming a nitride semiconductor stack including at least one gallium nitride layer on the buffer layer; wherein the concave-convex structure is formed by etching the amorphous glass substrate.
13. The method of claim 12, further comprising forming a compensation layer on the second surface of the amorphous glass substrate.
14. The method for manufacturing a nitride semiconductor device according to claim 12, wherein the uneven structure is formed so that the lengths of the flat convex surface and the flat concave surface are 5 μm to 80 μm, and the height difference between the flat convex surface and the flat concave surface is 0.3 μm to 3 μm.
15. The method for producing a nitride semiconductor device according to claim 12, wherein the buffer layer is formed of at least one layer selected from an aluminum nitride layer and an aluminum oxide layer.
16. The method for producing a nitride semiconductor device according to claim 12, wherein the compensation layer is formed of at least one layer selected from an aluminum nitride layer and an aluminum oxide layer.
17. The method for producing a nitride semiconductor device according to claim 12, wherein the buffer layer is formed by laminating an aluminum oxide layer and an aluminum nitride layer in this order from the first surface side.
18. The method for producing a nitride semiconductor device according to claim 13, wherein the compensation layer is formed by laminating an aluminum oxide layer and an aluminum nitride layer in this order from the second surface side.
19. The method for producing a nitride semiconductor device according to claim 12, further comprising irradiating a laser beam from the amorphous glass substrate side to peel off the nitride semiconductor laminate from the interface with the buffer layer.
Citation Information
Patent Citations
Nitride semiconductor light emitting element and manufacturing method of the same
JP2016219593A
UV light-emitting device and method for manufacturing the same
JP2017050439A
Semiconductor structure and semiconductor element
JP2018110174A
Method of manufacturing semiconductor light-emitting device
JP2019029546A
Display device
WO2022210402A1
Cited By
Semiconductor structure, preparation method thereof and electronic equipment
CN119384210A