Method for directional cyclic resource utilization of refined phosphoric acid desulfurization slag

By using methyl isobutyl ketone and fatty alcohol as leaching agents, combined with treatment steps involving calcium carbonate, barium carbonate, ammonia, and carbon dioxide, high-purity barium sulfate, ammonium sulfate, and phosphoric acid are extracted from phosphoric acid desulfurization residue. This solves the problem of low utilization rate of phosphogypsum and achieves efficient and environmentally friendly material recycling.

WO2024234214A1PCT designated stage expired Publication Date: 2024-11-21GUANGDONG BRUNP RECYCLING TECH CO LTD +1

Patent Information

Application Number
PCT/CN2023/094120
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

In existing technologies, the resource utilization rate of phosphogypsum and phosphoric acid desulfurization residue is low, leading to environmental pollution and land occupation problems. Moreover, existing utilization methods have high energy consumption, low product purity and yield, and cannot achieve large-scale continuous production.

Method used

Using methyl isobutyl ketone and fatty alcohol as leaching agents, high-purity barium sulfate, ammonium sulfate and phosphoric acid are extracted from refined phosphoric acid desulfurization residue through leaching, filtration, desulfurization and back-extraction. Desulfurization is carried out using calcium carbonate and barium carbonate, and the materials are recycled by using ammonia and carbon dioxide.

Benefits of technology

It has achieved the preparation of phosphoric acid, barium sulfate and ammonium sulfate with high recovery rate and high purity, reduced environmental pollution, reduced energy consumption, has industrialization potential, and the products have high added value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023094120_21112024_PF_FP_ABST
    Figure CN2023094120_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a method for directional cyclic resource utilization of refined phosphoric acid desulfurization slag. The method comprises the following steps: carrying out first mixing on desulfurization slag and a leaching agent, and obtaining a first suspension, the leaching agent comprising an organic solvent, and the organic solvent comprising methyl isobutyl ketone and fatty alcohol; performing first filtration on the first suspension, and obtaining a first filtrate; sequentially carrying out desulfurization treatment and second filtration on the first filtrate, and obtaining a second filtrate; and carrying out reverse extraction on the second filtrate, and obtaining phosphoric acid. According to the method provided by the present application, cyclic utilization of materials can be achieved, the process is simple, industrialization is easy to achieve, and high economic benefits and environmental benefits are attained.
Need to check novelty before this filing date? Find Prior Art

Description

A method for directional recycling of refined phosphoric acid desulfurization slag Technical Field

[0001] The embodiments of the present application relate to the field of resource utilization of desulfurization slag, for example, a method for directional recycling resource utilization of refined phosphoric acid desulfurization slag. Background Art

[0002] With the increasing demand for electronic-grade and food-grade phosphoric acid and the rapid development of the lithium iron phosphate battery industry, phosphoric acid purification and refining has become an important industry in the current phosphorus chemical industry. Refined phosphoric acid desulfurization slag is a by-product of phosphoric acid refining, purification and desulfurization.

[0003] The primary component of refined phosphoric acid desulfurization slag is calcium sulfate, which is also the primary component of phosphogypsum. Currently, the global annual production capacity of wet-process phosphoric acid approaches 300 million tons (measured in P2O5), and this industry chain alone emits nearly 1.5 billion tons of phosphogypsum annually. However, the actual utilization rate of phosphogypsum is less than 5%. Large quantities of phosphogypsum are stored in open-air storage, which not only occupies significant land but also pollutes the environment through its leachate. Furthermore, the global annual production capacity of industrial phosphoric acid is approximately 60 million tons (measured in P2O5), while desulfurization slag output is approximately 20 million tons, significantly increasing the pressure on phosphogypsum disposal.

[0004] At present, the comprehensive utilization of phosphogypsum is mainly in the fields of cement retarder, roadbed materials and building gypsum powder. This utilization method not only has high energy consumption, but also cannot be produced continuously on a large scale, and will cause secondary pollution to the environment. In addition, the shortcomings of phosphogypsum such as high impurities and low whiteness have led to relatively low enthusiasm for the utilization of phosphogypsum in industry.

[0005] CN106744769A discloses a method for producing calcium feed and ammonium sulfate using phosphogypsum, which is a by-product solid waste of phosphate fertilizer plants, as raw material, undergoes defluorination and activation, adds reaction aids to react with ammonium dihydrogen phosphate, and then undergoes filtering, concentration, crystallization, drying and other process steps to prepare feed-grade calcium hydrogen phosphate products and co-produce industrial ammonium sulfate. CN115180598A discloses a comprehensive utilization process for phosphogypsum, comprising the following steps: (1) phosphogypsum is purified to obtain calcium sulfate, the calcium sulfate is pulped and then mixed with an organic acid and a diluent for extraction, phase separation, and the resulting aqueous phase is dilute sulfuric acid; (2) the oil phase obtained by phase separation is back-extracted with phosphoric acid, phase separation, and the resulting aqueous phase is sent to the calcium hydrogen phosphate production system, and the oil phase is returned to step (1) for mixed extraction. Although the above method can produce some products using phosphogypsum, the degree of resource utilization of phosphogypsum is not high, and the product cannot achieve high yield and high purity.

[0006] Directed recycling is the process of recycling a discarded product by rationally decomposing and reassembling it to create a similar product with the same or similar performance. Therefore, providing a method for recycling refined phosphoric acid desulfurization slag based on the principle of directed recycling is of great significance.

[0007] Summary of the Invention

[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0009] The embodiment of the present application provides a method for the directional recycling and resource utilization of refined phosphoric acid desulfurization slag. Compared with related technologies, the method provided by the present application can prepare high-purity barium sulfate, ammonium sulfate and phosphoric acid, can realize the recycling of materials, has a simple process, is easy to industrialize, and has high environmental benefits.

[0010] The present invention provides a method for directional recycling of refined phosphoric acid desulfurization slag for resource utilization, the method comprising the following steps:

[0011] performing a first mixing of the desulfurized slag and the leaching agent to obtain a first suspension, wherein the leaching agent comprises an organic solvent, and the organic solvent comprises methyl isobutyl ketone and a fatty alcohol;

[0012] performing a first filtration on the first suspension to obtain a first filtrate;

[0013] performing a desulfurization treatment and a second filtration on the first filtrate in sequence to obtain a second filtrate;

[0014] The second filtrate is stripped to obtain phosphoric acid.

[0015] The method provided in the present application uses refined phosphoric acid desulfurization slag as raw material, the main component of which is calcium sulfate, and also contains a small amount of barium sulfate, trace amounts of barium carbonate, calcium carbonate and phosphates (such as calcium phosphate, barium phosphate or iron aluminum magnesium phosphate), etc. The present application obtains high-purity and high-recovery phosphoric acid through operations such as leaching, first filtration, desulfurization treatment, second filtration and back extraction. The present application uses methyl isobutyl ketone and fatty alcohol as leaching agents, wherein methyl isobutyl ketone is an organic solvent with a low boiling point (116°C) and low viscosity (0.5mPa·s), which is easy to evaporate and regenerate, and has good binding force to phosphoric acid; fatty alcohol can form a hydrogen bond structure with phosphoric acid, further enhancing the leaching ability of phosphoric acid, and at the same time fatty alcohol can be used as a defoaming agent to quickly eliminate bubbles generated during the leaching process, enhance the effect of mixed washing, and thus greatly improve the leaching rate of phosphoric acid.

[0016] In one embodiment, the desulfurization slag is crushed before the first mixing.

[0017] In one embodiment, the average particle size of the crushed desulfurization slag is ≤0.1 mm, for example, it can be 0.1 mm, 0.09 mm, 0.08 mm or 0.07 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the volume ratio of methyl isobutyl ketone to fatty alcohol is (20-50):1, for example, 20:1, 25:1, 30:1, 35:1, 40:1, 45:1 or 50:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] In one embodiment, the fatty alcohol includes any one of n-butanol, isobutanol, and isopentanol, or a combination of at least two thereof.

[0020] In one embodiment, the mass percentage of solids in the first suspension is 35-45%, for example, it can be 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44% or 45%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0021] In one embodiment, pH adjustment is further performed before the first filtration.

[0022] In one embodiment, the pH adjustment includes: mixing the first suspension and a pH adjuster and stirring.

[0023] In one embodiment, the pH adjuster includes sulfuric acid.

[0024] In one embodiment, the mass percentage concentration of the sulfuric acid is ≥98%, for example, it can be 98.1%, 98.2%, 98.3%, 98.4% or 98.5%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] In one embodiment, the stirring time during the pH adjustment is 1-2 hours, for example, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] In one embodiment, the end point of the pH adjustment is pH < 4, for example, 3.9, 3.8, 3.7 or 3.6, but not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0027] In one embodiment, the first filtrate is subjected to cyclic washing and concentration in sequence before the desulfurization treatment.

[0028] In one embodiment, the cyclic washing includes: returning the first filtrate to the first suspension, and then performing a first filtration until the first filtrate reaches a target specific gravity.

[0029] In one embodiment, the target specific gravity of the first filtrate after the cyclic washing is greater than 0.85, for example, it can be 0.86, 0.87, 0.88, 0.89 or 0.9, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] In one embodiment, the mass percentage of phosphorus pentoxide in the first filtrate after the circulating washing is 8-10%, for example, 8%, 8.5%, 9%, 9.5% or 10%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] In one embodiment, the specific gravity of the concentrated liquid obtained by the concentration is 0.95-1, for example, it can be 0.95, 0.96, 0.97, 0.98, 0.98 or 1, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0032] In one embodiment, the mass percentage of phosphorus pentoxide in the concentrated solution is 15-20%, for example, 15%, 16%, 17%, 18%, 19% or 20%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] In one embodiment, the organic vapor obtained by the concentration is used to prepare an organic solvent, and then reused in the first mixing.

[0034] In one embodiment, the desulfurization agent used in the desulfurization treatment includes calcium carbonate and barium carbonate.

[0035] In one embodiment, the mass ratio of calcium carbonate to barium carbonate in the desulfurizer is (8-12):1, for example, it can be 8:1, 9:1, 10:1, 11:1 or 12:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] In one embodiment, the molar amount of the desulfurizer is SO4 in the concentrate. 2- 110-150% of the molar amount can be, for example, 110%, 120%, 130%, 140% or 150%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] In one embodiment, the desulfurization treatment includes: adding a desulfurizing agent to the concentrated liquid while stirring.

[0038] In the present application, it is preferred to stir simultaneously to increase the contact area between the desulfurizer and the concentrated liquid and prevent the desulfurizer from agglomerating.

[0039] In one embodiment, the time for adding the desulfurizer is 30-60 minutes, for example, it can be 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes or 60 minutes, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0040] In one embodiment, the stirring is continued for 20-40 minutes after the desulfurizer is added, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] In one embodiment, the desulfurizing agent is added by first adding calcium carbonate and then adding barium carbonate.

[0042] In one embodiment, the stripping agent used in the stripping comprises water.

[0043] In the present application, the number of stripping stages is not particularly limited and can be selected as needed.

[0044] In one embodiment, the stripping temperature is 50-60°C, for example, 50°C, 52°C, 54°C, 56°C, 58°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] In one embodiment, the ratio of the second filtrate to the stripping agent in the stripping is (3-6):1, for example, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1 or 6:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] In one embodiment, the organic phase obtained by the stripping is regenerated to obtain an organic solvent, which is then reused in the first mixing.

[0047] In the present application, the regeneration agent used for the regeneration is not particularly limited and can be any regeneration agent commonly used in the art, for example, sodium hydroxide or sodium carbonate solution.

[0048] In one embodiment, the first filtration further produces a first filter residue.

[0049] In one embodiment, the first filter residue and the ammonium sulfate solution are mixed for a second time to obtain a second suspension.

[0050] In one embodiment, excess ammonia and excess carbon dioxide are sequentially introduced into the second suspension, and then a third filtration is performed to obtain barium sulfate and a third filtrate.

[0051] In one embodiment, the third filtrate is heated and filtered for the fourth time in sequence to obtain calcium carbonate and ammonium sulfate solution.

[0052] In the present application, the first filter residue contains calcium sulfate and barium sulfate, excess ammonia is used to make the second suspension alkaline, carbon dioxide is used to first convert calcium sulfate into calcium carbonate, and then further convert calcium bicarbonate into calcium carbonate and dissolve it, and then the third filtration is performed to obtain barium sulfate and a third filtrate containing calcium bicarbonate, the third filtrate is heated and decomposed to obtain carbon dioxide and calcium carbonate, and the fourth filtration is performed to obtain calcium carbonate and ammonium sulfate solution.

[0053] In one embodiment, the first filter residue is dried before the second mixing.

[0054] In one embodiment, the drying temperature is 80-100° C., for example, 80° C., 85° C., 90° C., 95° C. or 100° C., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0055] In one embodiment, the drying time is 30-60 minutes, for example, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes or 60 minutes, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0056] In one embodiment, the organic vapor obtained by drying is used to prepare an organic solvent, and then reused in the first mixing.

[0057] In one embodiment, water is further added into the second mixing.

[0058] In one embodiment, the volume ratio of ammonium sulfate solution to water in the second mixture is (4-6):1, for example, 4:1, 4.2:1, 4.5:1, 4.8:1, 5:1, 5.2:1, 5.5:1, 5.8:1 or 6:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0059] In one embodiment, the mass percentage concentration of the ammonium sulfate solution used in the second mixing is 38-40%, for example, it can be 38%, 38.2%, 38.5%, 38.8%, 39%, 39.2%, 39.5%, 39.8% or 40%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0060] In one embodiment, the temperature of the second mixing is 50-60°C, for example, 50°C, 52°C, 54°C, 56°C, 58°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] In one embodiment, the mass percentage of solids in the second suspension is 30-40%, for example, 30%, 32%, 34%, 36%, 38% or 40%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0062] In one embodiment, the pH value of the second suspension after the excess ammonia gas is introduced is ≥12, for example, it can be 12, 12.5 or 13, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0063] In one embodiment, the time for introducing the excess carbon dioxide is 1-2 hours, for example, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0064] In one embodiment, the heating temperature is 70-80°C, for example, it can be 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 78°C, 79°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0065] In one embodiment, the carbon dioxide generated by the heating is recycled and introduced into the second suspension.

[0066] In one embodiment, the calcium carbonate is recycled to prepare desulfurization slag.

[0067] In the present application, the calcium carbonate can be returned to the desulfurization section for desulfurization to obtain desulfurization slag.

[0068] In one embodiment, the ammonium sulfate solution obtained by the fourth filtration is sequentially subjected to evaporation concentration, cooling crystallization, and a fifth filtration to obtain ammonium sulfate crystals and ammonium sulfate mother liquor.

[0069] In one embodiment, the temperature of the evaporation concentration is 105-107° C., for example, 105° C., 105.5° C., 106° C., 106.5° C. or 107° C., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0070] In one embodiment, the cooling rate of the cooling crystallization is 3-4°C / min, for example, it can be 3°C / min, 3.2°C / min, 3.4°C / min, 3.6°C / min, 3.8°C / min or 4°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0071] In one embodiment, the ammonia gas obtained by the evaporation and concentration is recycled and fed into the second suspension.

[0072] In one embodiment, the ammonium sulfate mother liquor obtained by the fifth filtration is used to prepare an ammonium sulfate solution and then reused in the second mixing.

[0073] As a preferred technical solution of this application, the method includes the following steps:

[0074] After crushing the desulfurization slag to an average particle size of ≤0.1 mm, the desulfurization slag and a leaching agent are first mixed to obtain a first suspension, wherein the leaching agent is prepared from methyl isobutyl ketone and a fatty alcohol in a volume ratio of (20-50):1, and the weight percentage of solids in the first suspension is 35-45%; mixing the first suspension with sulfuric acid having a weight percentage concentration of ≥98% and stirring for 1-2 hours to adjust the pH value to a pH value of <4, and then performing a first filtration to obtain a first filtrate and a first filter residue;

[0075] The first filtrate is subjected to a circulating washing, and the circulating washing comprises: returning the first filtrate to the first suspension, and then performing a first filtration until the specific gravity of the first filtrate is greater than 0.85, and the mass percentage of phosphorus pentoxide in the first filtrate after the circulating washing is 8-10%; then, the first filtrate after the circulating washing is concentrated to obtain a concentrated solution, the specific gravity of the concentrated solution is 0.95-1, and the mass percentage of phosphorus pentoxide in the concentrated solution is 15-20%, the organic vapor obtained by the concentration is used to prepare an organic solvent, and then returned to the first mixing; a desulfurizer is added to the concentrated solution, the time for adding the desulfurizer is 30-60 minutes, and then stirring is continued for 20-40 minutes for desulfurization treatment, the desulfurizer is calcium carbonate and barium carbonate with a mass ratio of (8-12):1, and the molar amount of the desulfurizer is SO4 in the concentrated solution. 2- The method comprises the following steps: performing a second filtration to obtain a second filtrate; stripping the second filtrate with water at a temperature of 50-60° C., wherein the ratio of the second filtrate to water in the stripping is (3-6):1, to obtain phosphoric acid; and regenerating the organic phase obtained by the stripping to obtain an organic solvent, which is reused in the first mixing;

[0076] The first filter residue is dried at a temperature of 80-100° C. for 30-60 minutes, and the organic vapor obtained by the drying is used to prepare an organic solvent and reused in the first mixing; then, the first filter residue, ammonium sulfate solution and water are mixed for a second time at 50-60° C. to obtain a second suspension, wherein the weight percentage of solids in the second suspension is 30-40%, the volume ratio of ammonium sulfate solution to water in the second mixing is (4-6):1, and the weight percentage concentration of the ammonium sulfate solution is 38-40%; then, excess ammonia gas is introduced into the second suspension until the pH value of the second suspension is ≥12, and then excess carbon dioxide is introduced for 1-2 hours, and then a third Filter to obtain barium sulfate and a third filtrate; heat the third filtrate at a temperature of 70-80°C, and the carbon dioxide generated by the heating is recycled and introduced into the second suspension, and then perform a fourth filtration to obtain calcium carbonate and ammonium sulfate solution; the calcium carbonate is recycled to prepare desulfurization slag; the ammonium sulfate solution obtained by the fourth filtration is evaporated and concentrated at 105-107°C, and then cooled and crystallized at a cooling rate of 3-4°C / min, and then perform a fifth filtration to obtain ammonium sulfate crystals and ammonium sulfate mother liquor, the ammonia obtained by the evaporation and concentration is recycled and introduced into the second suspension, and the ammonium sulfate mother liquor obtained by the fifth filtration is used to prepare ammonium sulfate solution and recycled into the second mixing.

[0077] Compared with the related art, the embodiments of the present application have the following beneficial effects:

[0078] (1) The method provided in the embodiment of the present application uses refined phosphoric acid desulfurization slag as raw material. Except for a small amount of reagents such as sulfuric acid that need to be added additionally, the organic solvent, carbon dioxide, calcium carbonate, ammonia and ammonium sulfate in the reaction process can all be recycled in the reaction process, no waste is generated, and it has high environmental benefits.

[0079] (2) The method provided in the examples of the present application uses a combination of methyl isobutyl ketone and fatty alcohol as a leaching agent, which can improve the binding force to phosphoric acid and at the same time defoam and increase the mixing effect, thereby improving the recovery rate and purity of phosphoric acid.

[0080] (3) The method provided in the embodiments of the present application can realize the directional recycling resource utilization of refined phosphoric acid desulfurization slag, and obtain phosphoric acid with high recovery rate and high purity barium sulfate, ammonium sulfate and phosphoric acid, which can be used to produce downstream products with higher added value and have broad market prospects.

[0081] (4) The method provided in the embodiments of the present application has simple raw material pretreatment, low cost, mild reaction conditions, simple and easy production process, low energy consumption, no environmental pollutants, and is easy to industrialize.

[0082] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0083] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.

[0084] FIG1 is a flow chart of the method described in Example 1 of the present application. DETAILED DESCRIPTION

[0085] Example 1

[0086] This embodiment provides a method for directional recycling and resource utilization of refined phosphoric acid desulfurization slag. The desulfurization slag used in this embodiment comprises, by mass percentage, 95% calcium sulfate, 4.5% barium sulfate, 0.2% calcium carbonate, 0.25% phosphate, and 0.05% barium carbonate. As shown in FIG1 , the method comprises the following steps:

[0087] After crushing the desulfurization slag to an average particle size of 0.1 mm, the desulfurization slag and a leaching agent are first mixed to obtain a first suspension, wherein the leaching agent is prepared from methyl isobutyl ketone and n-butanol in a volume ratio of 20:1, and the mass percentage of solids in the first suspension is 35%; the first suspension is mixed with 98.5% sulfuric acid and stirred for 1.5 hours to adjust the pH value to 3.8, and then a first filtration is performed to obtain a first filtrate and a first filter residue;

[0088] The first filtrate is subjected to a circulating washing, and the circulating washing includes: returning the first filtrate to the first suspension, and then performing a first filtration until the specific gravity of the first filtrate is 0.85, and the mass percentage of phosphorus pentoxide in the first filtrate after the circulating washing is 8%; then, the first filtrate after the circulating washing is concentrated to obtain a concentrated solution, the specific gravity of the concentrated solution is 0.95, and the mass percentage of phosphorus pentoxide in the concentrated solution is 15%, the organic vapor obtained by the concentration is used to prepare an organic solvent, and then returned to the first mixing; a desulfurizer is added to the concentrated solution, the time for adding the desulfurizer is 30 minutes, and then stirring is continued for 30 minutes for desulfurization treatment, the desulfurizer is calcium carbonate and barium carbonate with a mass ratio of 8:1, and the molar amount of the desulfurizer is SO4 in the concentrated solution. 2- The molar weight of the reaction mixture was 110%, and a second filtration was performed to obtain a second filtrate; the second filtrate was stripped with water at a temperature of 50° C., wherein the ratio of the second filtrate to water in the stripping was 3:1 to obtain phosphoric acid; the organic phase obtained by the stripping was regenerated with 5% sodium hydroxide to obtain an organic solvent, which was reused in the first mixing;

[0089] The first filter residue is dried at a temperature of 90° C. for 50 min, and the organic vapor obtained by the drying is used to prepare an organic solvent and reused in the first mixing; then, the first filter residue, ammonium sulfate solution and water are mixed for a second time at 50° C. to obtain a second suspension, wherein the weight percentage of solids in the second suspension is 30%, the volume ratio of ammonium sulfate solution to water in the second mixing is 4:1, and the weight percentage concentration of the ammonium sulfate solution is 38%; then, excess ammonia is introduced into the second suspension until the pH value of the second suspension reaches 12, and then excess carbon dioxide is introduced for 1 hour, and then a third filtration is performed to obtain sulfur dioxide. barium sulfate and a third filtrate; heating the third filtrate at a temperature of 70°C, and the carbon dioxide generated by the heating is recycled to be passed into the second suspension, and then a fourth filtration is performed to obtain calcium carbonate and ammonium sulfate solution; the calcium carbonate is recycled to prepare desulfurization slag; the ammonium sulfate solution obtained by the fourth filtration is evaporated and concentrated at 105°C, and then cooled and crystallized at a cooling rate of 3°C / min, and then a fifth filtration is performed to obtain ammonium sulfate crystals and ammonium sulfate mother liquor, the ammonia obtained by the evaporation and concentration is recycled to be passed into the second suspension, and the ammonium sulfate mother liquor obtained by the fifth filtration is used to prepare ammonium sulfate solution and recycled to the second mixing.

[0090] Example 2

[0091] This embodiment provides a method for directional recycling of refined phosphoric acid desulfurization slag. The desulfurization slag used in this embodiment is the same as that in Example 1. The method comprises the following steps:

[0092] After crushing the desulfurization slag to an average particle size of 0.08 mm, the desulfurization slag and a leaching agent are first mixed to obtain a first suspension, wherein the leaching agent is prepared from methyl isobutyl ketone and isobutyl alcohol in a volume ratio of 35:1, and the mass percentage of solids in the first suspension is 40%; the first suspension is mixed with 98.5% sulfuric acid and stirred for 1 hour to adjust the pH value to 3.9, and then a first filtration is performed to obtain a first filtrate and a first filter residue;

[0093] The first filtrate is subjected to a circulating washing, and the circulating washing includes: returning the first filtrate to the first suspension, and then performing a first filtration until the specific gravity of the first filtrate is 0.87, and the mass percentage of phosphorus pentoxide in the first filtrate after the circulating washing is 9%; then, the first filtrate after the circulating washing is concentrated to obtain a concentrated solution, the specific gravity of the concentrated solution is 0.97, and the mass percentage of phosphorus pentoxide in the concentrated solution is 17%, the organic vapor obtained by the concentration is used to prepare an organic solvent, and then returned to the first mixing; a desulfurizer is added to the concentrated solution, the time for adding the desulfurizer is 45 minutes, and then stirring is continued for 20 minutes for desulfurization treatment, the desulfurizer is calcium carbonate and barium carbonate with a mass ratio of 10:1, and the molar amount of the desulfurizer is SO4 in the concentrated solution. 2- The reaction mixture was subjected to a second filtration to obtain a second filtrate; the second filtrate was stripped with water at a temperature of 55° C., wherein the ratio of the second filtrate to water in the stripping was 4:1 to obtain phosphoric acid; the organic phase obtained by the stripping was regenerated with a 15% sodium carbonate solution to obtain an organic solvent, which was reused in the first mixing;

[0094] The first filter residue was dried at 80° C. for 60 min, and the organic vapor obtained by the drying was used to prepare an organic solvent and reused in the first mixing; then, the first filter residue, ammonium sulfate solution and water were mixed for a second time at 55° C. to obtain a second suspension, wherein the weight percentage of solids in the second suspension was 35%, the volume ratio of ammonium sulfate solution to water in the second mixing was 5:1, and the weight percentage concentration of the ammonium sulfate solution was 39%; then, excess ammonia gas was introduced into the second suspension until the pH value of the second suspension reached 12.2, and then excess carbon dioxide was introduced for 1.5 h, and then a third filtration was performed to obtain barium sulfate and the third filtrate; heating the third filtrate at a temperature of 75°C, and the carbon dioxide generated by the heating is recycled to be passed into the second suspension, and then a fourth filtration is performed to obtain calcium carbonate and ammonium sulfate solution; the calcium carbonate is recycled to prepare desulfurization slag; the ammonium sulfate solution obtained by the fourth filtration is evaporated and concentrated at 106°C, and then cooled and crystallized at a cooling rate of 3.5°C / min, and then a fifth filtration is performed to obtain ammonium sulfate crystals and ammonium sulfate mother liquor, the ammonia obtained by the evaporation and concentration is recycled to be passed into the second suspension, and the ammonium sulfate mother liquor obtained by the fifth filtration is used to prepare ammonium sulfate solution and recycled to the second mixing.

[0095] Example 3

[0096] This embodiment provides a method for directional recycling of refined phosphoric acid desulfurization slag. The desulfurization slag used in this embodiment is the same as that in Example 1. The method comprises the following steps:

[0097] After crushing the desulfurization slag to an average particle size of 0.07 mm, the desulfurization slag and a leaching agent are first mixed to obtain a first suspension, wherein the leaching agent is prepared from methyl isobutyl ketone and ethanol in a volume ratio of 50:1, and the weight percentage of solids in the first suspension is 45%; the first suspension is mixed with 98.5% sulfuric acid and stirred for 2 hours to adjust the pH to 3.7, and then filtered to obtain a first filtrate and a first filter residue;

[0098] The first filtrate is subjected to a circulating washing, and the circulating washing includes: returning the first filtrate to the first suspension, and then performing a first filtration until the specific gravity of the first filtrate is 0.9, and the mass percentage of phosphorus pentoxide in the first filtrate after the circulating washing is 10%; then, the first filtrate after the circulating washing is concentrated to obtain a concentrated solution, the specific gravity of the concentrated solution is 1.0, and the mass percentage of phosphorus pentoxide in the concentrated solution is 20%, the organic vapor obtained by the concentration is used to prepare an organic solvent, and then returned to the first mixing; a desulfurizer is added to the concentrated solution, the time for adding the desulfurizer is 60 minutes, and then stirring is continued for 40 minutes for desulfurization treatment, the desulfurizer is calcium carbonate and barium carbonate with a mass ratio of 12:1, and the molar amount of the desulfurizer is SO4 in the concentrated solution. 2- The molar weight of the reaction mixture was 150%, and a second filtration was performed to obtain a second filtrate; the second filtrate was stripped with water at a temperature of 60° C., wherein the ratio of the second filtrate to water in the stripping was 6:1 to obtain phosphoric acid; the organic phase obtained by the stripping was regenerated with a 15% sodium carbonate solution to obtain an organic solvent, which was reused in the first mixing;

[0099] The first filter residue was dried at a temperature of 100° C. for 30 minutes, and the organic vapor obtained by the drying was used to prepare an organic solvent and reused in the first mixing; then, the first filter residue, ammonium sulfate solution and water were mixed for a second time at 60° C. to obtain a second suspension, wherein the weight percentage of solids in the second suspension was 40%, the volume ratio of ammonium sulfate solution to water in the second mixing was 6:1, and the weight percentage concentration of the ammonium sulfate solution was 40%; thereafter, excess ammonia gas was introduced into the second suspension until the pH value of the second suspension reached 12.3, and then excess carbon dioxide was introduced for 2 hours, and then a third filtration was performed to obtain barium sulfate and a third filtrate; heating the third filtrate at a temperature of 80°C, and the carbon dioxide generated by the heating is recycled and introduced into the second suspension, and then a fourth filtration is performed to obtain calcium carbonate and ammonium sulfate solution; the calcium carbonate is recycled and used to prepare desulfurization slag; the ammonium sulfate solution obtained by the fourth filtration is evaporated and concentrated at 107°C, and then cooled and crystallized at a cooling rate of 4°C / min, and then a fifth filtration is performed to obtain ammonium sulfate crystals and ammonium sulfate mother liquor, the ammonia obtained by the evaporation and concentration is recycled and introduced into the second suspension, and the ammonium sulfate mother liquor obtained by the fifth filtration is used to prepare an ammonium sulfate solution and recycled into the second mixing.

[0100] Example 4

[0101] This embodiment provides a method for directional recycling and resource utilization of refined phosphoric acid desulfurization slag. The only difference compared with Example 1 is that the volume ratio of methyl isobutyl ketone and n-butanol is 10:1.

[0102] Example 5

[0103] This embodiment provides a method for directional recycling and resource utilization of refined phosphoric acid desulfurization slag. The only difference compared with Example 1 is that the volume ratio of methyl isobutyl ketone and n-butanol is 60:1.

[0104] Example 6

[0105] This embodiment provides a method for directional recycling and resource utilization of refined phosphoric acid desulfurization slag, which differs from the method in Example 1 only in that the mass ratio of calcium carbonate to barium carbonate is 5:1.

[0106] Example 7

[0107] This embodiment provides a method for directional recycling and resource utilization of refined phosphoric acid desulfurization slag, which is different from the method in Example 1 only in that the mass ratio of calcium carbonate to barium carbonate is 15:1.

[0108] Comparative Example 1

[0109] This comparative example provides a method for resource utilization of refined phosphoric acid desulfurization slag, which differs from Example 1 only in that the leaching agent is replaced by an equal volume of water.

[0110] Comparative Example 2

[0111] This comparative example provides a method for resource utilization of refined phosphoric acid desulfurization slag, which differs from Example 1 only in that methyl isobutyl ketone is replaced by an equal volume of n-butanol.

[0112] Comparative Example 3

[0113] This comparative example provides a method for resource utilization of refined phosphoric acid desulfurization slag, which differs from Example 1 only in that n-butanol is replaced by an equal volume of methyl isobutyl ketone.

[0114] The recovery rates of phosphoric acid in Examples 1-7 and Comparative Examples 1-3 were measured using the method specified in JC / T 2073-2011. The results are shown in Table 1.

[0115] The impurity content of phosphoric acid in Examples 1-7 and Comparative Examples 1-3 was measured using the method specified in HG / T 4069-2008, as shown in Table 1.

[0116] The purity of phosphoric acid, barium sulfate, and ammonium sulfate in Examples 1-7 and Comparative Examples 1-3 was determined according to HG / T 4069-2008, GB / T 2899-2008, and GB / T 29206-2012, respectively. The results are shown in Table 1.

[0117] Table 1

[0118] The following points can be seen from the data in Table 1:

[0119] (1) From the data of Examples 1-7, it can be seen that the method provided by the present application can make the recovery rate of phosphoric acid reach more than 98.30%, the impurity content of phosphoric acid reach less than 0.0009wt%, the purity of barium sulfate reach more than 99.08wt%, and the purity of ammonium sulfate reach more than 99.32wt%. Under better conditions, the recovery rate of phosphoric acid can reach more than 95.32%, the impurity content of phosphoric acid reaches less than 0.0008wt%, the purity of barium sulfate reaches more than 99.32wt%, and the purity of ammonium sulfate reaches more than 99.68wt%.

[0120] (2) A comprehensive comparison of the data of Example 1 and Examples 4-5 shows that the volume ratio of methyl isobutyl ketone to n-butanol in Example 1 is 20:1. Compared with 10:1 and 60:1 in Examples 4-5, respectively, the recovery rate of phosphoric acid in Example 1 is significantly higher than that in Examples 4-5. Therefore, it can be seen that the present application preferably controls the volume ratio of methyl isobutyl ketone to n-butanol, which can further improve the recovery rate of phosphoric acid.

[0121] (3) A comprehensive comparison of the data of Example 1 and Examples 6-7 shows that the mass ratio of calcium carbonate to barium carbonate in Example 1 is 8:1, compared with 5:1 and 15:1 in Examples 6-7, respectively. The purity of barium sulfate and ammonium sulfate in Example 1 is significantly higher than that in Examples 6-7. It can be seen that the present application preferably controls the mass ratio of calcium carbonate to barium carbonate, which can further improve the purity of barium sulfate and ammonium sulfate.

[0122] (4) A comprehensive comparison of the data of Example 1 and Comparative Examples 1-3 shows that in Example 1, methyl isobutyl ketone and n-butanol are used as leaching agents. Compared with Comparative Examples 1-3, which respectively use only water, n-butanol, and methyl isobutyl ketone as leaching agents, the recovery rate of phosphoric acid in Example 1 is significantly higher than that in Comparative Examples 1-3, and the impurity content in Example 1 is significantly lower than that in Comparative Example 1. Therefore, the use of a leaching agent composed of methyl isobutyl ketone and n-butanol in the present application can further improve the recovery rate of phosphoric acid and reduce the impurity content.

[0123] In summary, the method provided in this application can prepare high-purity barium sulfate, ammonium sulfate and phosphoric acid, can realize the recycling of materials, has a simple process, is easy to industrialize, and has high economic and environmental benefits.

Claims

1. A method for directional recycling of refined phosphoric acid desulfurization slag, comprising the following steps: The desulfurized slag and the leaching agent are first mixed to obtain a first suspension, wherein the leaching agent comprises an organic solvent, and the organic solvent comprises methyl isobutyl ketone and a fatty alcohol; Performing a first filtration on the first suspension to obtain a first filtrate; The first filtrate is sequentially subjected to desulfurization treatment and second filtration to obtain a second filtrate; The second filtrate is stripped to obtain phosphoric acid.

2. The method according to claim 1, wherein: The desulfurization slag is crushed before the first mixing.

3. The method according to claim 1 or 2, wherein: The average particle size of the crushed desulfurized slag is ≤0.1 mm.

4. The method according to any one of claims 1 to 3, wherein: The volume ratio of the methyl isobutyl ketone to the fatty alcohol is (20-50):

1.

5. The method according to any one of claims 1 to 4, wherein: The fatty alcohol includes any one of n-butanol, isobutanol or isopentanol, or a combination of at least two of them.

6. The method according to any one of claims 1 to 5, wherein: The mass percentage of solid in the first suspension is 35-45%.

7. The method according to claims 1-6, wherein: The pH value is also adjusted before the first filtration; Preferably, the pH value adjustment comprises: mixing the first suspension and the pH adjuster and stirring; Preferably, the pH adjuster comprises sulfuric acid; Preferably, the mass percentage concentration of the sulfuric acid is ≥98%; Preferably, the stirring time during the pH adjustment is 1-2h; Preferably, the end point of the pH adjustment is pH <4.

8. The method according to any one of claims 1 to 7, wherein: Before the desulfurization treatment, the first filtrate is sequentially subjected to cyclic washing and concentration; Preferably, the cyclic washing comprises: returning the first filtrate to the first suspension, and then performing a first filtration until the first filtrate reaches a target specific gravity; Preferably, the target specific gravity of the first filtrate after the cyclic washing is > 0.85; Preferably, the mass percentage of phosphorus pentoxide in the first filtrate after the cyclic washing is 8-10%; Preferably, the specific gravity of the concentrated solution obtained by the concentration is 0.95-1; Preferably, the mass percentage of phosphorus pentoxide in the concentrated solution is 15-20%; Preferably, the organic vapor obtained by the concentration is used to prepare an organic solvent and then reused in the first mixing.

9. The method according to any one of claims 1 to 8, wherein: The desulfurization agent used in the desulfurization treatment includes calcium carbonate and barium carbonate; Preferably, the mass ratio of calcium carbonate to barium carbonate in the desulfurizer is (8-12):1; Preferably, the molar amount of the desulfurizing agent is SO4 in the concentrate. 2- 110-150% of the molar amount; Preferably, the desulfurization treatment comprises: adding a desulfurizing agent to the concentrated liquid while stirring; Preferably, the time for adding the desulfurizing agent is 30-60 minutes; Preferably, the stirring is continued for 20-40 minutes after the desulfurizing agent is added; Preferably, the desulfurizing agent is added by first adding calcium carbonate and then adding barium carbonate.

10. The method according to any one of claims 1 to 9, wherein: The stripping agent used in the stripping includes water; Preferably, the stripping temperature is 50-60°C; Preferably, the ratio of the second filtrate to the stripping agent in the stripping is (3-6):1; Preferably, the organic phase obtained by the stripping is regenerated to obtain an organic solvent, which is then reused in the first mixing.

11. The method according to any one of claims 1 to 10, wherein: The first filtration also obtains a first filter residue; Preferably, the first filter residue and the ammonium sulfate solution are mixed for a second time to obtain a second suspension; Preferably, excess ammonia and excess carbon dioxide are sequentially introduced into the second suspension, followed by a third filtration to obtain barium sulfate and a third filtrate; Preferably, the third filtrate is sequentially heated and filtered for a fourth time to obtain calcium carbonate and ammonium sulfate solution.

12. The method according to claim 11, wherein: Drying the first filter residue before the second mixing; Preferably, the drying temperature is 80-100°C; Preferably, the drying time is 30-60 minutes; Preferably, the organic vapor obtained by drying is used to prepare an organic solvent and then reused in the first mixing.

13. The method according to claim 11, wherein: Water is also added to the second mixing; Preferably, the volume ratio of the ammonium sulfate solution to water in the second mixture is (4-6):1; Preferably, the mass percentage concentration of the ammonium sulfate solution used in the second mixing is 38-40%; Preferably, the temperature of the second mixing is 50-60°C; Preferably, the mass percentage of solids in the second suspension is 30-40%; Preferably, the pH value of the second suspension after the excess ammonia gas is introduced is ≥12; Preferably, the excess carbon dioxide is introduced for 1-2 hours.

14. The method according to claim 11, wherein: The heating temperature is 70-80°C; Preferably, the carbon dioxide generated by the heating is recycled and introduced into the second suspension; Preferably, the calcium carbonate is recycled to prepare desulfurization slag; Preferably, the ammonium sulfate solution obtained by the fourth filtration is sequentially subjected to evaporation concentration, cooling crystallization and fifth filtration to obtain ammonium sulfate crystals and ammonium sulfate mother liquor; Preferably, the temperature of the evaporation concentration is 105-107°C; Preferably, the cooling rate of the cooling crystallization is 3-4°C / min; Preferably, the ammonia gas obtained by evaporation and concentration is recycled and introduced into the second suspension; Preferably, the ammonium sulfate mother liquor obtained by the fifth filtration is used to prepare an ammonium sulfate solution and then reused in the second mixing.

Citation Information

Patent Citations

  • Technology and device for co-producing ofproducing industrial monoammonium phosphate and co-producing high-quality monoammonium phosphate by utilizing middle-grade and low-grade collophanite

    CN107381525A

  • Method for recycling phosphorus from slag of tungsten concentrate disintegrated by phosphate

    CN108689391A

  • Multifunctional treatment method for tailings

    CN112831653A

  • Wet-process phosphoric acid purification method

    CN114044498A

  • Process for producing monopotassium phosphate and calcium sulfate whiskers from phosphorite

    CN115092900A

Cited By

  • Industrial grade monoammonium phosphate crystal, preparation method thereof and iron phosphate crystal