High-resolution quantum dot pixelated light-emitting thin film and preparation method therefor

High-resolution quantum dot pixelated luminescent films are prepared by spin-coating photoresist, drying, exposure treatment and electrostatic adsorption technology, which solves the damage problem of photolithographic deposition and development solutions to the quantum dot layer, and achieves high resolution and stability Quantum dot pixelated luminescent film improves the integrity of the displayed image.

WO2024234425A1PCT designated stage expired Publication Date: 2024-11-21SUZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/098825
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2023-06-07
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing methods for patterned quantum dot luminescent film preparation can damage the quantum dot layer when using photolithography deposition and development solutions, affecting the luminescent performance and the integrity of the displayed image.

Method used

Using spin-coated photoresist, drying, exposure treatment, development, depositing PFTS insulating layer, removing photoresist patterns, spin-coated PEI layer and dripping QD solution, the preparation of high-resolution quantum dot pixelated luminescent film is achieved by electrostatic action. , avoid direct use of photolithography deposition and development solutions.

Benefits of technology

The film formation quality of the quantum dot layer is improved, the damage to the QDs layer by the photolithography process is avoided, and a high-resolution and stable quantum dot pixelated luminescent film is achieved, which enhances the integrity of the displayed image.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023098825_21112024_PF_FP_ABST
    Figure CN2023098825_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a high-resolution quantum dot pixelated light-emitting thin film and a preparation method therefor, and belongs to the technical field of quantum dots. The method comprises: spin-coating a substrate with a photoresist; drying the substrate; exposing the substrate by using a photoetching device; coating a preset position on the substrate with a developing agent to obtain a photoresist pattern layer; depositing an insulating layer on the photoresist pattern layer by using silane; removing the photoresist pattern in the insulating layer; spin-coating the insulating layer with a PEI solution to obtain a PEI layer; and dropping a QD solution on the PEI layer to deposit a QD layer. In the present invention, by means of the hydrophobicity of silane, a dewetting effect is achieved so as to achieve pixelation of the quantum dots; by means of the hydrophobicity of the insulating layer, the PEI solution is spontaneously deposited to the position of the photoresist pattern; and the QD solution is adsorbed into the PEI solution on the basis of the electrostatic interaction between the QD solution and the PEI solution, such that a high-resolution quantum dot pixelated light-emitting thin film is obtained, the film forming quality is improved, and surface defects of a QD layer are passivated.
Need to check novelty before this filing date? Find Prior Art

Description

A high-resolution quantum dot pixelated luminescent film and its preparation method Technical Field

[0001] The present invention relates to the field of quantum dot technology, and in particular to a high-resolution quantum dot pixelated luminescent film and a preparation method thereof, as well as a transparent quantum dot light-emitting diode and a preparation method thereof. Background Art

[0002] Resolution is a crucial parameter for displays, enabling them to vividly present images. With the advent of head-mounted devices for virtual reality (VR), augmented reality (AR), and mixed reality (MR), the demand for bright, high-resolution electroluminescent (EL) devices has become urgent. One such technology is AR, which cleverly merges virtual information with the real world, effectively reflecting real-world content while also enabling the display of subtle, overlapping virtual information. In visual AR, users need to be able to overlay the real world with computer graphics on top of the head-mounted display, allowing them to fully see the surrounding real world. Therefore, near-eye displays with high-resolution pixels and the ability to render transparent are crucial for the realization of AR and artificial intelligence. Liquid crystal displays (LCDs) and organic light-emitting diodes (OLEDs) face significant obstacles in achieving high resolution for near-eye displays due to cost and inherent material limitations. Quantum dots (QDs), with their narrow half-width (FWHM) and wide color gamut, are considered promising candidates for future luminescent materials. Pixelation is an important step in incorporating it into display, anti-counterfeiting and optical chip applications. In addition, red (R), green (G), and blue (B) micron / submicron pixels made using QDs have the advantage of providing bright and vivid immersive content images at close viewing distances without visual discomfort, making it an important frontier in the display field.

[0003] Currently, methods for patterning quantum dot (QD) light-emitting films primarily include nanoimprinting, inkjet printing, and photolithography. However, technical barriers remain for pattern transfer and alignment using nanoimprinting, and the scalability and maturity required for large-scale production remain limited to laboratory-scale demonstrations. Inkjet printing is a widely studied and promising method for producing patterned QD films with regular luminescent structures. However, due to unstable drying kinetics, issues with resolution and thickness uniformity persist. In recent years, with the advancement of semiconductor technology and the development and application of national photolithography equipment, photolithography has become a research hotspot in the field of high-resolution displays due to its advantages in large-scale and rapid fabrication of QD patterns, attracting significant attention from research institutions both domestically and internationally. With the development of quantum dot patterning techniques using photolithography, research has demonstrated significant advantages in achieving ultra-high-resolution QDs, including the ability to form micron- to submicron-scale patterns over large areas of the desired substrate, the ability to simultaneously define patterns across large areas of the panel, and the ability to fabricate patterns using UV light solely through optical diffraction from the edge of the pattern mask, thus providing extremely high pattern quality. It is noteworthy that QDs are composed of a limited number of atoms, have large surface energy, and are subject to chemical, optical, or thermal instabilities. Therefore, the structural degradation and unstable optical properties of QDs pose a major challenge to their integration into arrays of high-resolution display and imaging sensor systems. QDs require solution processing, while the organic light-emitting diodes used in OLEDs can be patterned via thermal evaporation. Conventional photolithography uses a photoresist, a photolithographic polymer layer, as a mask layer applied to the quantum dot film and then depatterned by development. However, the solution processing used for photolithographic deposition and development can damage the underlying QD layer. Furthermore, to obtain full-color RGB images, at least three photolithography steps are required, which inevitably damages the already patterned QD layer. The damaged pattern can affect the device's luminescence performance and even prevent the complete display image. Therefore, patterning with conventional photoresists can cause devastating damage to QDs.

[0004] In summary, the existing method for preparing patterned quantum dot luminescent films requires the use of solutions for photolithographic deposition and development on the QDs layer, which will damage the QDs layer, affect the luminescence performance of the device, and result in the display pattern cannot be fully presented.

[0005] Summary of the Invention

[0006] To this end, the technical problem to be solved by the present invention is to overcome the problem that the method for preparing patterned quantum dot luminescent films in the prior art requires the use of solutions for photolithographic deposition and development on the QDs layer, which will cause damage to the QDs layer.

[0007] To solve the above technical problems, the present invention provides a method for preparing a high-resolution quantum dot pixelated luminescent film, comprising:

[0008] Spin coating the photoresist on the substrate surface;

[0009] Drying the substrate on which the photoresist is spin-coated;

[0010] Expose the dried substrate using a photolithography device;

[0011] Applying a developer to a preset position on the surface of the substrate for development to obtain a photoresist pattern layer;

[0012] Depositing a PFTS insulating layer on the surface of the photoresist pattern layer using a silane self-assembly technique;

[0013] removing the photoresist pattern in the PFTS insulating layer to obtain a PFTS insulating layer having a mesh pattern;

[0014] Spin-coating a PEI solution on the surface of the PFTS insulating layer having a mesh pattern to obtain a PEI layer;

[0015] The QD solution is dropped onto the surface of the PEI layer to deposit a QD layer, thereby obtaining a high-resolution quantum dot pixelated luminescent film.

[0016] In one embodiment of the present invention, the step of spin coating the photoresist on the substrate surface further comprises:

[0017] Clean the substrate with acetone and then isopropyl ketone;

[0018] The cleaned substrate was placed on a heating table to dry.

[0019] In one embodiment of the present invention, the step of dropping the QD solution onto the surface of the PEI layer to deposit the QD layer and obtaining a high-resolution quantum dot pixelated luminescent film further comprises using an energy dispersion spectrometer in a scanning electron microscope to detect the element distribution on the surface of the high-resolution quantum dot pixelated luminescent film.

[0020] In one embodiment of the present invention, the substrate is a transparent conductive film glass or a silicon wafer.

[0021] In one embodiment of the present invention, the shape of the photoresist pattern includes but is not limited to circle, square, and hexagon.

[0022] In one embodiment of the present invention, the PEI solution is a PEI aqueous solution.

[0023] The present invention also provides a high-resolution quantum dot pixelated luminescent film, which is prepared by the above-mentioned high-resolution quantum dot pixelated luminescent film preparation method.

[0024] The present invention also provides a method for preparing a transparent quantum dot light-emitting diode, comprising:

[0025] Providing a PFTS insulating layer having a mesh pattern prepared using the above-mentioned method for preparing a high-resolution quantum dot pixelated light-emitting film;

[0026] Spin-coating a colloid-doped oxide semiconductor solution onto the surface of the PFTS insulating layer having a mesh pattern to obtain an electron transport layer;

[0027] Spin coating the PEI solution on the surface of the electron transport layer to obtain a PEI layer;

[0028] Dropping the QD solution on the surface of the PEI layer to deposit the QD layer;

[0029] Spin-coating a chlorobenzene solution on the surface of the QD layer to obtain a hole transport layer;

[0030] Placing a kaoton tape with a preset pattern as a mask on a first preset position on the surface of the hole transport layer, and coating silver nanowires on the surface of the mask to obtain a cathode electrode;

[0031] A kaoton tape with a preset pattern is placed as a mask on a second preset position on the surface of the hole transport layer, and indium tin oxide is coated on the surface of the mask to obtain an anode electrode.

[0032] In one embodiment of the present invention, the PEI solution is a PEI ethanol solution.

[0033] The present invention also provides a transparent quantum dot light emitting diode, which is prepared by the above-mentioned transparent quantum dot light emitting diode preparation method.

[0034] The method for preparing a high-resolution quantum dot pixelated luminescent film provided by the present invention includes: spin-coating a photoresist on a substrate surface and drying and exposing the substrate; applying a developer to a predetermined position on the substrate surface to obtain a photoresist pattern layer; depositing a PFTS insulating layer on the surface of the photoresist pattern layer using silane self-assembly technology; removing the photoresist pattern in the PFTS insulating layer; spin-coating a PEI solution on the surface of the PFTS insulating layer to obtain a PEI layer; and finally, dropping a QD solution on the surface of the PEI layer to deposit the QD layer. The present invention utilizes the hydrophobicity of silane to achieve a dewetting effect to achieve quantum dot pixelation, and utilizes the hydrophobicity of PFTS to allow the PEI solution to spontaneously deposit at the location of the photoresist pattern. Finally, based on the electrostatic interaction between the QD solution and the PEI solution, the QD solution is spontaneously adsorbed into the PEI solution to obtain a high-resolution quantum dot pixelated luminescent film. This avoids direct photolithography on the QDs layer, prevents damage to the QDs layer during this process, improves the film quality of the QDs layer, and passivates surface defects of the QDs layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below based on specific embodiments of the present invention in conjunction with the accompanying drawings, wherein

[0036] FIG1 is a flow chart of a method for preparing a high-resolution quantum dot pixelated light-emitting film provided by the present invention;

[0037] FIG2 is a schematic diagram of the process for preparing a high-resolution quantum dot pixelated luminescent film provided by the present invention;

[0038] FIG3 (a) is a schematic diagram of a verification result provided by the present invention;

[0039] FIG3( b ) is a schematic diagram of the second verification result provided by the present invention;

[0040] (c) in FIG3 is a schematic diagram of the third verification result provided by the present invention;

[0041] (d) in FIG3 is a schematic diagram of the fourth verification result provided by the present invention;

[0042] FIG4 is a fluorescence microscope image of a high-resolution quantum dot pixelated luminescent film provided by the present invention;

[0043] FIG5 (a) is a fluorescence microscope image of the second high-resolution quantum dot pixelated luminescent film provided by the present invention;

[0044] FIG5( b ) is a fluorescence microscope image of the third high-resolution quantum dot pixelated luminescent film provided by the present invention;

[0045] FIG6 is a flow chart of a method for preparing a transparent quantum dot light-emitting diode provided by the present invention. DETAILED DESCRIPTION

[0046] The present invention will be further described below with reference to the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it. However, the embodiments are not intended to limit the present invention.

[0047] Example 1:

[0048] 1 is a flow chart of a method for preparing a high-resolution quantum dot pixelated luminescent film according to the present invention, comprising:

[0049] S10: Spin-coating photoresist on the surface of the substrate.

[0050] Optionally, the substrate may be a transparent conductive thin film glass or a silicon wafer.

[0051] In some embodiments, before step S10 , the substrate is cleaned in sequence using acetone and isopropyl tone; and the cleaned substrate is placed on a heating platform for drying.

[0052] For example, the substrate can be cleaned with acetone or isopropyl alcohol, then placed on a hot plate and dried at 110°C for 10 minutes to prevent moisture from affecting the subsequently spun-on photoresist. After the substrate has dried and cooled, AZ5214 photoresist is applied to the entire substrate, spin-coated at 3500 rpm for 40 seconds.

[0053] In other embodiments, other temperatures and times may be set when drying the substrate to prevent moisture on the substrate surface from affecting the photoresist; optionally, other photoresists may be coated on the substrate surface, which is not limited in this application.

[0054] S20: Drying the substrate on which the photoresist is spin-coated.

[0055] In some embodiments, step S20 is specifically implemented by drying the substrate at 105° C. for 5 minutes to increase the interaction between the photoresist and the substrate to prevent the photoresist from falling off during the subsequent development process.

[0056] In other embodiments, other temperatures and times may be set when drying the substrate, which is not limited in this application.

[0057] S30: performing exposure processing on the dried substrate using a photolithography device.

[0058] In this embodiment, the lithography equipment used is ARM / 6 / 350 / NUV / DCCD / BSV / M, USA. In other embodiments, other types of lithography equipment can also be used, and this application does not limit this.

[0059] S40: applying a developer to a predetermined position on the surface of the substrate for development to obtain a photoresist pattern layer, as shown in FIG. 2 ( a ).

[0060] Optionally, the shape of the pattern on the photoresist pattern layer can be circular, square, hexagonal, etc.

[0061] In this embodiment, the developer used is AZ400K. In other embodiments, other developers may also be used, and this application does not limit this.

[0062] S50: depositing a perfluorooctyltrichlorosilane (PFTS) insulating layer on the surface of the photoresist pattern layer using a silane self-assembly technique, as shown in FIG. 2( b ).

[0063] Alternatively, the silane can be fluorosilane or other hydrophobic functional silane. This is because the hydrophobicity of silane can achieve a dewetting effect to achieve QD pixelation, and it can also be used as an insulating layer in the subsequent alternating process of PEI solution and photoresist patterning.

[0064] S60: removing the photoresist pattern in the PFTS insulating layer to obtain a PFTS insulating layer with a mesh pattern, as shown in (c) in FIG. 2 .

[0065] S70: Spin-coating a polyethyleneimine (PEI) solution on the surface of the PFTS insulating layer having a mesh pattern to obtain a PEI layer.

[0066] After the PEI solution is spin-coated on the surface of the PFTS insulating layer, due to the hydrophobicity of PFTS, the PEI solution will spontaneously deposit on the hydrophilic area, that is, the original photoresist pattern area, as shown in (d) in Figure 2.

[0067] Specifically, the PEI solution in this embodiment adopts a PEI aqueous solution.

[0068] S80: Dropping the quantum dot QD solution on the surface of the PEI layer to deposit the QD layer to obtain a high-resolution quantum dot pixelated luminescent film.

[0069] Due to the electrostatic interaction between the QD solution and the PEI solution, the QD solution will spontaneously adsorb into the PEI solution, that is, the original photoresist pattern area, as shown in (e) in Figure 2, and finally a high-resolution quantum dot pixelated luminescent film is obtained, as shown in (f) in Figure 2.

[0070] The method for preparing a high-resolution quantum dot pixelated luminescent film provided in this embodiment uses hydrophobic silane to deposit an insulating layer to form a dewetting layer, and utilizes the electrostatic interaction between the PEI solution and the QD solution to form an electrosorption layer. Due to the difference in their surface free energy, the QDs undergo dewetting and are selectively deposited to construct a pattern. This method does not require photolithography on the QD layer, avoiding damage to the QD layer caused by the deposition and development solutions used in the process, improving the film quality of the QD layer, and passivating surface defects of the QD layer.

[0071] To verify the above solution, after obtaining the high-resolution quantum dot pixelated luminescent film, this embodiment also used the energy dispersive spectrometer (EDS) provided by the scanning electron microscope (SEM) to detect the element distribution on the surface of the high-resolution quantum dot pixelated luminescent film. The detection results are as follows:

[0072] As shown in (a) and (b) in Figure 3, the N element signal is mainly concentrated in the initial photoresist pattern area, and there is almost no N element signal in other areas. It can be seen that the PEI solution, based on the hydrophobicity of the PFTS insulating layer, mainly forms an electro-adsorption layer in the initial photoresist pattern area.

[0073] As shown in (c) and (d) of Figure 3, the signal of the Si element is in the peripheral area of ​​the initial photoresist pattern, and the distribution of the F element signal shows that the PFTS insulating layer is mainly distributed in the peripheral area of ​​the photoresist pattern to form a dewetting layer.

[0074] The staggered mesh arrangement of the dewetting layer and the electro-adsorption layer can enable the QD solution to be adsorbed in the required area to obtain a high-resolution quantum dot pixelated luminescent film, thereby achieving the purpose of pixelation.

[0075] For example, based on the above embodiments and test results, the embodiments of the present application also provide three high-resolution quantum dot pixelated luminescent films prepared using this method. As shown in Figure 4, the high-resolution quantum dot pixelated luminescent film with a line pattern with a line width of 5 μm provided in this embodiment is shown in Figure 5 (a). The high-resolution quantum dot pixelated luminescent film with a rectangular pattern with a resolution of 1104PPI provided in this embodiment is shown in Figure 5 (b). The high-resolution quantum dot pixelated luminescent film with a square pattern with a resolution of 2522PPI provided in this embodiment is shown.

[0076] In addition, in other embodiments, a zinc blende (CdSe) QD pattern with a minimum size of 5 μm×5 μm was manufactured based on the above preparation method, and its resolution exceeded 2522 PPI.

[0077] Based on the above embodiment 1, the present application also provides a high-resolution quantum dot pixelated luminescent film, which is obtained by using the above-mentioned high-resolution quantum dot pixelated luminescent film preparation method.

[0078] Example 2:

[0079] Based on the above embodiment 1, the present embodiment further provides a method for preparing a transparent quantum dot light-emitting diode. FIG7 is a flow chart of the method for preparing a transparent quantum dot light-emitting diode, comprising:

[0080] S200: providing a PFTS insulating layer having a mesh pattern prepared by the preparation method of the above-mentioned embodiment 1.

[0081] S210: spin-coating a colloid-doped oxide semiconductor solution onto a surface of the PFTS insulating layer having a mesh pattern to obtain an electron transport layer.

[0082] In this embodiment, the specific implementation of step S210 is: spin coating the colloid-doped oxide semiconductor solution on the surface of the PFTS insulating layer with a mesh pattern at a speed of 2000 rpm for 40 seconds to obtain an electron transport layer, and placing the substrate on a hot plate at 100°C for annealing for 20 minutes.

[0083] For example, the colloid-doped oxide semiconductor solution in this embodiment is a colloidal Mg-doped ZnO nanocrystal solution. Optionally, in other embodiments, other solutions may also be used, and this application does not limit this.

[0084] S220: Spin-coating the PEI solution on the surface of the electron transport layer to obtain a PEI layer.

[0085] Specifically, the PEI solution in this embodiment is a PEI ethanol solution.

[0086] Optionally, in other embodiments, the concentration of the PEI solution may be adjusted as needed to obtain PEI layers of different thicknesses.

[0087] S230: Dropping the QD solution on the surface of the PEI layer to deposit a QD layer.

[0088] In this embodiment, the specific implementation of step S230 is: dropping the QD solution on the surface of the PEI layer to deposit the QD layer, and drying the substrate at 60° C. for several minutes to dry the QD layer.

[0089] S240: Spin-coating the chlorobenzene solution on the surface of the QD layer to obtain a hole transport layer.

[0090] In this embodiment, the specific implementation method of step S260 is: spin coating a chlorobenzene solution with a concentration of 8 mg / ml on the surface of the QD layer at a speed of 2000 rpm for 40 seconds to obtain a hole transport layer, and annealing the substrate at 120°C for 15 minutes to obtain a light-emitting layer of a transparent quantum dot light-emitting diode.

[0091] S250: placing a kaoton tape with a preset pattern as a mask on a first preset position on the surface of the hole transport layer, and coating silver nanowires (AgNWs) on the surface of the mask to obtain a cathode electrode.

[0092] Specifically, the silver nanowires in this embodiment are prepared in an isopropyl alcohol solution with a concentration of 8 mg / ml.

[0093] Optionally, the preset pattern on the kapton tape can be engraved by laser as needed.

[0094] S260: placing a kaoton tape with a preset pattern as a mask on a second preset position on the surface of the hole transport layer, and coating indium tin oxide (ITO) on the surface of the mask to obtain an anode electrode.

[0095] The transparent electrode made of ITO and AgNWs in the embodiment of the present application has both high conductivity and high visible light transmittance, which can improve the transmittance of the transparent quantum dot light-emitting diode.

[0096] Based on the above embodiments, the present application further provides a transparent quantum dot light emitting diode, which is obtained by the above transparent quantum dot light emitting diode preparation method.

[0097] In this embodiment, the intersection of the anode electrode and the cathode electrode is used to define the effective area of ​​a single transparent quantum dot light-emitting diode as 1 mm*1 mm, so as to facilitate detection and measurement.

[0098] The transparent quantum dot light-emitting diode provided in this embodiment utilizes a PEI layer to precisely adjust a high-precision QD pattern, while the PFTS insulating layer acts as a barrier layer, suppressing the significant leakage current between the charge carrier transport layers and improving the performance of the transparent quantum dot light-emitting diode. Furthermore, the transparent quantum dot light-emitting diode produced using this method has a resolution ranging from 1104 PPI to 3031 PPI, an efficiency of up to 15.6%, and can be significantly reduced in size to produce a higher-density LED pixel array. Furthermore, the transparent quantum dot light-emitting diode has a transmittance of up to 90.7%, exhibiting high efficiency and transmittance, and is expected to be used in augmented reality display technology and automotive head-up display devices in the future.

[0099] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will appreciate that other variations or modifications can be made based on the above description. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications arising therefrom remain within the scope of protection of the present invention.

Claims

1. A method for preparing a high-resolution quantum dot pixelated luminescent film, characterized in that: include: Spin coating the photoresist on the substrate surface; Drying the substrate on which the photoresist is spin-coated; Using a photolithography device to perform exposure processing on the dried substrate; Applying a developer to a preset position on the surface of the substrate for development to obtain a photoresist pattern layer; Depositing a PFTS insulating layer on the surface of the photoresist pattern layer using a silane self-assembly technique; Removing the photoresist pattern in the PFTS insulating layer to obtain a PFTS insulating layer with a mesh pattern; Spin coating the PEI solution on the surface of the PFTS insulating layer having the mesh pattern to obtain a PEI layer; The QD solution is dropped onto the surface of the PEI layer to deposit the QD layer, thereby obtaining a high-resolution quantum dot pixelated luminescent film.

2. The method for preparing a high-resolution quantum dot pixelated luminescent film according to claim 1, characterized in that: The method further comprises: before spin coating the photoresist on the substrate surface: Clean the substrate using acetone and then isopropyl ketone; The cleaned substrate was placed on a heating table to dry.

3. The method for preparing a high-resolution quantum dot pixelated luminescent film according to claim 1, characterized in that: The method further comprises dripping the QD solution on the surface of the PEI layer to deposit the QD layer, and after obtaining a high-resolution quantum dot pixelated luminescent film, using an energy dispersion spectrometer in a scanning electron microscope to detect the element distribution on the surface of the high-resolution quantum dot pixelated luminescent film.

4. The method for preparing a high-resolution quantum dot pixelated luminescent film according to claim 1, characterized in that: The substrate is transparent conductive film glass or silicon wafer.

5. The method for preparing a high-resolution quantum dot pixelated luminescent film according to claim 1, characterized in that: The shape of the photoresist pattern includes but is not limited to circle, square, and hexagon.

6. The method for preparing a high-resolution quantum dot pixelated luminescent film according to claim 1, characterized in that: The PEI solution is a PEI aqueous solution.

7. A high-resolution quantum dot pixelated luminescent film, characterized in that: The high-resolution quantum dot pixelated luminescent film is prepared by the high-resolution quantum dot pixelated luminescent film preparation method according to any one of claims 1 to 6.

8. A method for preparing a transparent quantum dot light-emitting diode, characterized in that: include: Providing a PFTS insulating layer having a mesh pattern prepared by the method for preparing a high-resolution quantum dot pixelated light-emitting film according to any one of claims 1 to 6; Spin coating a colloid-doped oxide semiconductor solution onto the surface of the PFTS insulating layer having a mesh pattern to obtain an electron transport layer; Spin coating the PEI solution on the surface of the electron transport layer to obtain a PEI layer; Dropping a QD solution on the surface of the PEI layer to deposit a QD layer; Spin coating the chlorobenzene solution on the surface of the QD layer to obtain a hole transport layer; Placing a kaoton tape with a preset pattern as a mask on a first preset position on the surface of the hole transport layer, and coating silver nanowires on the surface of the mask to obtain a cathode electrode; A kaoton tape with a preset pattern is placed as a mask on a second preset position on the surface of the hole transport layer, and indium tin oxide is coated on the surface of the mask to obtain an anode electrode.

9. The method for preparing a transparent quantum dot light-emitting diode according to claim 8, characterized in that: The PEI solution is a PEI ethanol solution.

10. A transparent quantum dot light emitting diode, characterized in that: The transparent quantum dot light-emitting diode is prepared by the transparent quantum dot light-emitting diode preparation method according to claim 8.

Citation Information

Patent Citations

  • Preparation method and application of high-precision patterned quantum dot light emitting layer

    CN107611021A

  • Light extraction structure, method of fabricating the same, and light emitting device including the same

    KR1020140140207A