Positive electrode material and preparation method therefor, positive electrode sheet, battery, and electric device

By introducing one-dimensional conductive materials and reducing chalcogens on the surface of the positive electrode active substance of lithium-ion batteries, a conductive network and interface film is formed, the negative impact of residual lithium compounds on battery performance is solved, and the conductivity and cycle stability of the battery is improved. .

WO2024234591A1PCT designated stage expired Publication Date: 2024-11-21CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/131304
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2023-11-13
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The surface of the positive electrode active substance in lithium-ion batteries is prone to form residual lithium compounds with poor conductivity, increasing the interface impedance, deteriorating discharge capacity and cycling stability performance.

Method used

One-dimensional conductive material and reducing chalcogens are introduced as additives on the surface of the positive electrode active material, and intermediate products and final products are generated through redox reactions to form a positive electrode-electrolyte interface film, remove residual lithium compounds, and enhance the material through the conductive network Conductivity.

Benefits of technology

The conductivity and electrochemical properties of the positive electrode active material are improved, the cycle stability and capacity retention of the battery are enhanced, and polarization and internal resistance are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023131304_21112024_PF_FP_ABST
    Figure CN2023131304_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A positive electrode material and a preparation method therefor, a positive electrode sheet, a battery, and an electric device. The positive electrode material comprises a positive electrode active material, and a one-dimensional conductive material and an additive distributed on the surface of the positive electrode active material, wherein at least part of the one-dimensional conductive material is wrapped by the additive, and the additive comprises a chalcogen with reducibility. By introducing the additive containing a chalcogen with reducibility to the surface of the positive electrode active material, a residual lithium compound on the surface of the positive electrode active material can be effectively removed by means of the additive; moreover, the one-dimensional conductive material is further introduced to the surface of the positive electrode active material, at least part of the one-dimensional conductive material is wrapped by the additive, and the one-dimensional conductive material is used as a carrier to anchor the additive, and can also construct a three-dimensional conductive system to improve the conductivity of the positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode material and preparation method thereof, positive electrode sheet, battery and electrical device

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 15, 2023, with application number 2023105432655 and invention name “Positive electrode material and preparation method thereof, positive electrode sheet, battery and electrical device”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of battery technology, and in particular to a positive electrode material and a preparation method thereof, a positive electrode sheet, a battery and an electrical device. Background Art

[0003] Lithium-ion batteries, as secondary batteries, reversibly convert chemical energy into electrical energy, making them an ideal carrier for human energy utilization and storage. Since their advent, they have been widely used due to their long lifespan, high energy density, and low maintenance costs. Currently, lithium-ion batteries are used in a variety of fields, including portable electronic devices, new energy vehicles, and energy storage systems.

[0004] The positive electrode active material is a key factor influencing the performance of lithium-ion batteries, often determining their cycle life, energy density, and power density. Due to the preparation process or the characteristics of the positive electrode active material itself, residual lithium compounds (RLCs), such as lithium hydroxide, lithium carbonate, and lithium oxide, are easily formed on the surface of the positive electrode active material. These residual lithium compounds typically have poor conductivity, increasing the cathode / electrolyte interface impedance, exacerbating battery polarization, and deteriorating discharge capacity and cycle stability, negatively impacting battery performance.

[0005] Application Contents

[0006] The purpose of the embodiments of the present application is to provide a positive electrode material and a preparation method thereof, a positive electrode plate, a battery and an electrical device, in order to alleviate the negative impact of residual lithium compounds in the positive electrode active material on battery performance.

[0007] The technical solution adopted in the embodiment of this application is:

[0008] In a first aspect, a positive electrode material is provided, comprising: a positive electrode active material and a one-dimensional conductive material and an additive distributed on the surface of the positive electrode active material, at least a portion of the one-dimensional conductive material is wrapped by the additive, and the additive contains a reducing chalcogen element.

[0009] In a second aspect, a method for preparing a positive electrode material is provided, comprising:

[0010] A one-dimensional conductive material and an additive are mixed to obtain a mixture, wherein the additive comprises a chalcogen element having reducing properties;

[0011] sintering the mixed material to melt the additive and at least a portion of the one-dimensional conductive material is wrapped by the additive, thereby obtaining a sintered material;

[0012] The sintered material is stirred with the positive electrode active material to obtain the positive electrode material.

[0013] In a third aspect, a positive electrode plate is provided, comprising a positive electrode current collector and a positive electrode material layer bonded to the positive electrode current collector, wherein the positive electrode material layer comprises the positive electrode material provided in the first aspect of the embodiment of the present application or the positive electrode material prepared by the preparation method of the positive electrode material provided in the second aspect of the embodiment of the present application.

[0014] In a fourth aspect, a battery is provided, comprising the positive electrode plate provided in the third aspect of the embodiment of the present application.

[0015] In a fifth aspect, an electrical device is provided, comprising the battery provided in the fourth aspect of the embodiment of the present application.

[0016] The positive electrode material provided by the embodiment of the present application has the following beneficial effects: by introducing an additive on the surface of the positive electrode active material, the additive contains a chalcogen with reducing properties (usually a chalcogen in a low-valent state), the chalcogen with reducing properties in the additive is easily oxidized and reacts with the residual lithium compound (such as LiOH, Li2O, Li2CO3, etc.) on the surface of the positive electrode active material to generate an intermediate product (such as Li2S2O3, Li2Se2O3, Li2Te2O3, etc.) containing a chalcogen in an intermediate valence state on the surface of the positive electrode active material, and in the subsequent chemical reaction, the chalcogen in the additive is easily oxidized and reacts with the residual lithium compound (such as LiOH, Li2O, Li2CO3, etc.) on the surface of the positive electrode active material to generate an intermediate product (such as Li2S2O3, Li2Se2O3, Li2Te2O3, etc.) containing a chalcogen in an intermediate valence state on the surface of the positive electrode active material. During the process, the intermediate products continue to react, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and eventually generate final products containing high-valent sulfide elements (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the formation process, the final products further form a positive electrode-electrolyte interface (CEI) film on the surface of the positive electrode active material, thereby removing the residual lithium compounds on the surface of the positive electrode active material and improving the conductivity and electrochemical properties of the positive electrode active material. Furthermore, a one-dimensional conductive material is introduced onto the surface of the positive electrode active material. Since the one-dimensional conductive material is located on the surface of the positive electrode active material and can overlap with each other to construct a conductive system, the overall conductivity of the material is improved. At the same time, at least part of the one-dimensional conductive material is wrapped by the additive, which can increase the area of ​​physical bonding between the additive and the one-dimensional conductive material. Since the one-dimensional conductive material itself has a high specific surface area, the bonding area between the additive and the one-dimensional carbon material is further increased, and the bonding force between the additive and the one-dimensional conductive material is increased, thereby improving the stability of the bonding between the two and achieving anchoring of the additive. Since the additive is wrapped on the surface of the one-dimensional conductive material, when the one-dimensional conductive material overlaps, the additive will also wrap the nodes of the one-dimensional conductive material overlap, so as not to affect the conductive system constructed by the one-dimensional conductive material. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments or exemplary technical descriptions. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0018] FIG1 is a schematic structural diagram of a vehicle according to some embodiments of the present application;

[0019] FIG2 is a schematic diagram of an exploded structure of a battery according to some embodiments of the present application;

[0020] FIG3 is a schematic diagram of an exploded structure of a battery cell according to some embodiments of the present application;

[0021] FIG4 is a schematic structural diagram of an electrode assembly according to some embodiments of the present application;

[0022] FIG5 is a schematic diagram of the structure of the positive electrode material provided in some embodiments of the present application.

[0023] The accompanying drawings in the specific implementation manner are as follows:

[0024] 10. Pole piece;

[0025] 20. Electrode assembly; 101. Negative electrode sheet; 102. Positive electrode sheet; 201. Negative electrode tab; 202. Positive electrode tab; 203. Separator;

[0026] 30. Battery cell; 301. Housing; 302. End cap; 303. Negative electrode adapter; 304. Positive electrode adapter; 305. Insulator;

[0027] 40. Battery; 401. Box body; 4011. Box body; 4012. Box cover;

[0028] 50. Electrical device; 501. Controller; 502. Motor;

[0029] 6. Positive electrode active material particles;

[0030] 71. First sub-cladding layer; 72. Second sub-cladding layer; 73. Third sub-cladding layer. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of this application more clearly understood, the present application is further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit this application.

[0032] It should be noted that "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c" or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or plural.

[0033] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0034] The weights of the relevant components mentioned in the examples of this application may not only refer to the specific content of each component, but also represent the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the examples of this application, it is within the scope disclosed in the examples of this application. Specifically, the mass in the examples of this application may be μg, mg, g, kg, etc., which are mass units known in the chemical industry.

[0035] In order to illustrate the technical solution provided by this application, a detailed description is given below with reference to specific drawings and embodiments.

[0036] The present invention introduces an additive on the surface of the positive electrode active material, wherein the additive contains a chalcogen with reducing properties (usually a chalcogen in a low-valent state). The chalcogen with reducing properties in the additive is easily oxidized and reacts with the residual lithium compound (such as LiOH, Li2O, Li2CO3, etc.) on the surface of the positive electrode active material to generate an intermediate product (such as Li2S2O3, Li2Se2O3, Li2Te2O3, etc.) containing a chalcogen in an intermediate valence state in situ on the surface of the positive electrode active material. In the subsequent chemical formation process, the intermediate product is further oxidized. The reaction continues, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and eventually generate final products containing high-valent sulfide elements (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the formation process, the final products further form a positive electrode-electrolyte interface (CEI) film on the surface of the positive electrode active material, thereby removing the residual lithium compounds on the surface of the positive electrode active material and improving the conductivity and electrochemical properties of the positive electrode active material. Furthermore, a one-dimensional conductive material is introduced onto the surface of the positive electrode active material. Since the one-dimensional conductive material is located on the surface of the positive electrode active material and can overlap with each other to construct a conductive system, the overall conductivity of the material is improved. At the same time, at least part of the one-dimensional conductive material is wrapped by the additive, which can increase the area of ​​physical bonding between the additive and the one-dimensional conductive material. At the same time, since the one-dimensional conductive material itself has a high specific surface area, the bonding area between the additive and the one-dimensional conductive material is further increased, and the bonding force between the additive and the one-dimensional conductive material is increased, thereby improving the stability of the bonding between the two and achieving anchoring of the additive. Since the additive is wrapped on the surface of the one-dimensional conductive material, when the one-dimensional conductive material overlaps, the additive will also wrap the nodes of the one-dimensional conductive material overlap, so as not to affect the conductive system constructed by the one-dimensional conductive material.

[0037] The batteries disclosed in some embodiments of the present application may be used, but are not limited to, in electrical devices such as vehicles, ships, or aircraft. A power supply system comprising the batteries disclosed in the present application may be used to form the electrical device.

[0038] Some embodiments of the present application provide an electrical device using a battery as a power source, which may be, but is not limited to, a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy, an electric tool, etc. Vehicles may be, but are not limited to, fuel-powered vehicles, gas-powered vehicles, or new energy vehicles; new energy vehicles may be, but are not limited to, pure electric vehicles, hybrid vehicles, or extended-range vehicles; spacecraft include, but are not limited to, airplanes, rockets, space shuttles, and spacecraft; electric toys include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys; and electric tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers.

[0039] For the convenience of description, the following embodiments are described by taking a vehicle as an example of an electrical device according to an embodiment of the present application.

[0040] Please refer to Figure 1, which is a schematic diagram of the structure of a vehicle provided in some embodiments of the present application. A battery 40 is provided inside the vehicle, and the battery 40 can be located at the bottom, front, or rear of the vehicle. The battery 40 can be used to power the vehicle, for example, the battery 40 can serve as the operating power source of the vehicle. The vehicle may also include a controller 501 and a motor 502. The controller 501 is used to control the battery 40 to power the motor 502, for example, to meet the power requirements of the vehicle during startup, navigation, and driving.

[0041] In some embodiments of the present application, the battery 40 can serve not only as the operating power source of the vehicle, but also as the driving power source of the vehicle, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle.

[0042] In some embodiments of the present application, the battery 40 is a secondary battery, which has various forms, including but not limited to battery cells, battery modules, and battery packs. A secondary battery here refers to a battery that can be recharged to activate the active material after discharge and continue to be used.

[0043] Please refer to Figure 2, which is an exploded view of a battery 40 provided in some embodiments of the present application. Battery 40 includes a housing 401 and battery cells 30, with battery cells 30 housed within housing 401. Housing 401 is a component used to provide accommodation for battery cells 30 and can adopt a variety of structures.

[0044] In some embodiments, the box body 401 may include a box body 4011 and a box cover 4012, which cover each other and together define a storage space for accommodating the battery cells 30. Alternatively, the box body 4011 may be a hollow structure with one end open, and the box cover 4012 may be a plate-like structure that covers the open side of the box body 4011.

[0045] In the battery 40, there can be multiple battery cells 30, and the multiple battery cells 30 can be connected in series, in parallel, or in a mixed connection. Mixed connection means that the multiple battery cells 30 are both connected in series and in parallel. The multiple battery cells 30 can be directly connected in series, in parallel, or in a mixed connection, and then the whole formed by the multiple battery cells 30 is accommodated in the box 401; of course, the battery 40 can also be a battery module formed by first connecting multiple battery cells 30 in series, in parallel, or in a mixed connection, and then the multiple battery modules are connected in series, in parallel, or in a mixed connection to form a whole, and accommodated in the box 401. The battery 40 may also include other structures, such as a confluence component (not shown), which is used to achieve electrical connection between the multiple battery cells 30. Among them, the battery cells 30 may be cylindrical, flat, rectangular, or other shapes.

[0046] Please refer to Figure 3, which shows an exploded view of a battery cell 30 in some embodiments of the present application. A battery cell 30 is the basic unit that enables the conversion of chemical energy into electrical energy and is the smallest unit in a battery. As shown in Figure 3, a battery cell 30 includes a housing 301, an end cap 302, an electrode assembly 20, and other functional components.

[0047] The shell 301 is a hollow structure with one end open. The shell 301 is used to cooperate with the end cap 302 to form an internal environment for accommodating the electrode assembly 20, the electrolyte and other functional components. The shell 301 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shape of the shell 301 can be determined according to the specific shape and size of the electrode assembly 20. The material of the shell 301 can be, but is not limited to, copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and is not limited here.

[0048] The end cap 302 refers to a component that covers the opening of the shell 301 to isolate the internal environment of the battery cell 30 from the external environment. Optionally, the shape of the end cap 302 can be adapted to the shape of the shell 301 to match the shell 301. Optionally, the end cap 302 can be made of a material with a certain hardness and strength (such as aluminum alloy). In this way, the end cap 302 is not easily deformed when squeezed or collided, so that the battery cell 30 can have a higher structural strength and improved safety performance. The material of the end cap 302 can be, but is not limited to, copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and is not limited here.

[0049] In some embodiments, the battery cell 30 further includes functional components such as a negative electrode adapter 303 and a positive electrode adapter 304. The negative electrode adapter 303 is used to electrically connect to the negative electrode tab on the electrode assembly 20, and the positive electrode adapter 304 is used to electrically connect to the positive electrode tab on the electrode assembly 20 to output or input electrical energy to the battery cell 30. It is understood that the negative electrode adapter 303 is made of a conductive material, and the material of the negative electrode adapter 303 can be, but is not limited to, copper, iron, aluminum, etc. The positive electrode adapter 304 is made of a conductive material, and the material of the positive electrode adapter 304 can be, but is not limited to, copper, iron, aluminum, etc.

[0050] In some embodiments, the battery cell 30 further includes an insulating member 305 located inside the housing 301 to isolate the housing 301 from the electrode assembly 20 and reduce the risk of short circuits. For example, the insulating member 305 may be made of plastic, rubber, or the like.

[0051] One or more electrode assemblies 20 may be contained within the housing 301 .

[0052] Please refer to Figure 4, which is a schematic diagram of the structure of the electrode assembly 20 in some embodiments of the present application. The electrode assembly 20 is the component in the battery cell 30 where the electrochemical reaction occurs. The electrode assembly 20 is primarily formed by winding or stacking a negative electrode sheet 101 and a positive electrode sheet 102 into an integrated structure, and a separator 203 is typically provided between adjacent negative electrode sheets 101 and positive electrode sheets 102.

[0053] The negative electrode sheet 101 includes a negative electrode current collector and a negative electrode material layer, which is coated on the surface of the negative electrode current collector. Taking a lithium-ion battery as an example, the negative electrode current collector may be made of copper, and the negative electrode material layer may include a negative electrode material, which may include a silicon-based material.

[0054] The positive electrode sheet 102 includes a positive electrode current collector and a positive electrode material layer, which is coated on the surface of the positive electrode current collector. Taking a lithium-ion battery as an example, the positive electrode current collector may be made of aluminum, and the positive electrode material layer may include a positive electrode material, such as lithium cobalt oxide, lithium iron phosphate, ternary lithium, or lithium manganese oxide.

[0055] The isolation membrane 203 is a porous plastic film that allows lithium ions in the electrolyte to pass freely, but isolates the negative electrode plate 101 and the positive electrode plate 102, so that electrons inside the battery cannot pass freely.

[0056] The negative electrode current collector and the positive electrode current collector also have portions that are not coated with the active material layer. These portions without the active material layer are provided with connecting tabs. Specifically, the negative electrode current collector is connected to the negative electrode tab 201, and the positive electrode current collector is connected to the positive electrode tab 202. During the charge and discharge process of the battery, the positive electrode material layer and the negative electrode material layer react with the electrolyte, the negative electrode tab 201 is connected to the negative electrode adapter 303, and the positive electrode tab 202 is connected to the positive electrode adapter 304 to form a current loop. Of course, in some embodiments, the portions of the negative electrode current collector and the positive electrode current collector that are not coated with the active material layer each constitute a tab.

[0057] Some embodiments of the present application provide a positive electrode material, a positive electrode active material, and a one-dimensional conductive material and an additive distributed on the surface of the positive electrode active material, at least part of the one-dimensional conductive material is wrapped by the additive, and the additive contains a reducing chalcogen element.

[0058] The positive electrode material includes a positive electrode active material, which refers to a compound with a three-dimensional lithium ion channel, which is used on the positive electrode for reversible insertion and removal of lithium ions. Optionally, the positive electrode active material includes but is not limited to at least one of lithium nickel cobalt oxide, lithium nickel manganese oxide and lithium nickel cobalt manganese oxide. Lithium nickel cobalt oxide (LiNi 1-x Co x O2, referred to as NC binary material) is a layered structure with good electrochemical performance and thermal stability. x Mn 2-x O4, referred to as NM binary material) is a material with a spinel structure prepared by improving the original spinel lithium manganese oxide. Compared with lithium manganese oxide, it has higher cycle stability and voltage platform. Lithium nickel cobalt manganese oxide (referred to as NCM ternary material) contains three transition metal elements: Ni, Co and Mn. It effectively overcomes the shortcomings of the three materials LiNiO2, LiCoO2 and LiMnO2, and in the electrochemical performance and thermal stability tests, these three transition metals can show their respective characteristics in this material, and it has high development potential. Optionally, the positive electrode active material can also be doped and modified. Optionally, the doping elements include but are not limited to at least one of Zr, Zn, Cu, V, Ti, Sr, Sb, Y, W, Nb, B, Ba, Ce, Si, Ga, Sn, Mo, P, Al, Fe, Mg, Cr, F, N, S, and Cl.

[0059] One-dimensional conductive materials refer to fibrous or tubular materials in which electrons can move freely in only one non-nanoscale direction. One-dimensional conductive materials include, but are not limited to, metal nanowires and one-dimensional conductive carbon materials. Metal nanowires include, but are not limited to, silver nanowires and copper nanowires. One-dimensional conductive carbon materials can be one-dimensional nanocarbon materials or one-dimensional micron carbon materials. Alternatively, the one-dimensional conductive carbon material includes at least one of carbon fibers, nanocarbon fibers, and carbon nanotubes.

[0060] The additive includes a chalcogen with reducing properties, where chalcogen refers to sulfur and elements with similar chemical properties to sulfur. Optionally, the chalcogen includes elements from the chalcogen family other than oxygen. Optionally, the chalcogen includes at least one of sulfur (S), selenium (Se), and tellurium (Te). The additive includes a chalcogen, where the additive can be a compound with the chalcogen as one of the constituent elements of the compound, or a single substance, such as a single substance of the chalcogen itself. Chalcogen has reducing properties, meaning that the chalcogen can increase in valence through redox reactions. Optionally, the chalcogen has a valence less than or equal to zero, i.e., a low-valent chalcogen, which is easily oxidized to a high-valent chalcogen. As an example, the chalcogen includes sulfur, where the valence of low-valent sulfur is -2 or zero, and the valence of high-valent sulfur is +6 or +4.

[0061] The one-dimensional conductive material and additives are distributed on the surface of the positive electrode active material. The one-dimensional conductive material and additives can be loosely distributed on the surface of the positive electrode active material, or the one-dimensional conductive material and additives can form a coating layer wrapped around the surface of the positive electrode active material.

[0062] At least a portion of the one-dimensional conductive material is coated with an additive. The additive may be attached to the surface of the one-dimensional conductive material in the form of a film, forming a skin-core structure with the one-dimensional conductive material as the core and the additive as the skin. Alternatively, the additive may be formed into a substrate layer, with the one-dimensional conductive material at least partially embedded within the substrate layer to form a conductive network structure. For example, the additive may be melted and then solidified on the surface of the one-dimensional conductive material, thereby coating the surface of the one-dimensional conductive material with the additive. For example, the additive may be sublimated into a gaseous state and then solidified on the surface of the one-dimensional conductive material, thereby coating the surface of the one-dimensional conductive material with the additive. Here, the additive coating the surface of the one-dimensional conductive material. For a single one-dimensional conductive material, the entire surface of the one-dimensional conductive material may be coated with the additive, or only a portion of the surface may be coated with the additive. For example, when the additive content is low, the majority of the surface of the one-dimensional conductive material may be coated with the additive, leaving a small portion of the surface exposed. Alternatively, when the additive content is high but processing is affected, a small portion of the surface of the one-dimensional conductive material may not be coated with the additive and may be exposed. At least part of the one-dimensional conductive material is wrapped by the additive. This refers to all the one-dimensional conductive materials. Part of the one-dimensional conductive material can be wrapped by the additive, or all of the one-dimensional conductive material (ie, every one-dimensional conductive material) can be wrapped by the additive.

[0063] The positive electrode material provided in the embodiment of the present application includes a positive electrode active material, a one-dimensional conductive material and an additive, at least part of the one-dimensional conductive material is wrapped by the additive, the one-dimensional conductive material and the additive are distributed on the surface of the positive electrode active material, and the additive includes a sulfide element with reducing properties. By introducing an additive on the surface of the positive electrode active material, the additive includes a sulfide element with reducing properties (usually a sulfide element in a low-valent state), the sulfide element with reducing properties in the additive is easily oxidized and reacts with the residual lithium compound (such as LiOH, Li2O, Li2CO3, etc.) on the surface of the positive electrode active material to generate an intermediate product (such as Li2S2O3, Li2Se2O3, Li2Te2O3, etc.) containing an intermediate valence sulfide element in situ on the surface of the positive electrode active material, and in the subsequent formation process, the intermediate product continues to The reaction occurs, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and eventually generate final products containing high-valent sulfide elements (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the formation process, the final products further form a positive electrode-electrolyte interface (CEI) film on the surface of the positive electrode active material, thereby removing the residual lithium compounds on the surface of the positive electrode active material and improving the conductivity and electrochemical properties of the positive electrode active material. Furthermore, a one-dimensional conductive material is introduced onto the surface of the positive electrode active material. Since the one-dimensional conductive material is located on the surface of the positive electrode active material and can overlap with each other to construct a conductive system, the overall conductivity of the material is improved. At the same time, at least part of the one-dimensional conductive material is wrapped by the additive, which can increase the area of ​​physical bonding between the additive and the one-dimensional conductive material. At the same time, since the one-dimensional conductive material itself has a high specific surface area, the bonding area between the additive and the one-dimensional conductive material is further increased, and the bonding force between the additive and the one-dimensional conductive material is increased, thereby improving the stability of the bonding between the two and achieving anchoring of the additive. Since the additive is wrapped on the surface of the one-dimensional conductive material, when the one-dimensional conductive material overlaps, the additive will also wrap the nodes of the one-dimensional conductive material overlap, so as not to affect the conductive system constructed by the one-dimensional conductive material.

[0064] To sum up, in the embodiments of the present application, the one-dimensional conductive material not only serves as a carrier to anchor the additive, but the one-dimensional conductive material is also distributed on the surface of the positive electrode active material. With the help of the conductive network constructed by the one-dimensional conductive material, the overall conductivity of the positive electrode material is better; in addition, the one-dimensional conductive material has a large specific surface area, which not only promotes its anchoring of the additive but also increases the contact area between the one-dimensional conductive material and the positive electrode active material, thereby accelerating the electron / ion transfer rate on the positive electrode material and the kinetic reaction rate of the chalcogen element.

[0065] In some embodiments, the chalcogen element includes at least one of sulfur, selenium, and tellurium.

[0066] Optionally, the chalcogen element includes sulfur, that is, the additive includes a reducing sulfur element. As an example, the additive is sulfur element, and the positive electrode material is obtained by introducing sulfur element S and a one-dimensional conductive material into the surface of a positive electrode active material (e.g., a nickel-rich active material). Part of the sulfur element S in the positive electrode material undergoes an oxidation-reduction reaction with the metal cations in the positive electrode active material. At the same time, residual lithium compounds (e.g., LiOH, Li2O, Li2CO3, etc.) on the surface of the positive electrode active material also participate in the reaction. In this process, the sulfur element S is oxidized and combines with the residual lithium compound to form Li2S2O3. The positive electrode material is further prepared into a positive electrode sheet and applied to a battery. During the formation process of the battery, Li2S2O3 is further oxidized and converted into Li2SO3 and / or Li2SO4. At the same time, the sulfur element S in the positive electrode material continues to react with the residual lithium compound to generate Li2SO3 and / or Li2SO4. During the formation process, the battery is charged and discharged, and a CEI film is formed on the positive electrode of the battery. Li2SO3 and / or Li2SO4 can participate in the growth of the CEI film, thereby converting residual lithium compounds that have a negative impact on battery performance into a CEI film, thereby improving the electrochemical performance of the battery. In addition, when elemental sulfur S reacts with residual lithium compounds and generates Li2SO3 and / or Li2SO4, additional lithium ions are usually released. The lithium ions can be used to compensate for the lithium ion loss caused by the formation of the SEI film in the battery, thereby ensuring the capacity of the battery.

[0067] Optionally, the chalcogen element includes tellurium, that is, the additive contains a reducing tellurium element. As an example, the additive is tellurium element, and the positive electrode material is obtained by introducing tellurium element Te and a one-dimensional conductive material onto the surface of a positive electrode active material (e.g., a nickel-rich active material). Similar to sulfur element S, part of the tellurium element Te in the positive electrode material first combines with residual lithium compounds to form Li2Te2O3, and in the subsequent battery formation process, Li2Te2O3 and tellurium element Te are further converted into Li2TeO3 and / or Li2TeO4 and participate in the growth of CEI film, thereby improving the electrochemical performance of the battery; in this process, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of SEI film, thereby ensuring the capacity of the battery.

[0068] Optionally, the sulfide element includes selenium, that is, the additive contains selenium with reducing properties. As an example, the additive is selenium element, and the positive electrode material is obtained by introducing selenium element Se and a one-dimensional conductive material into the surface of the positive electrode active material (such as nickel-rich active material). Similar to sulfur element S, part of the selenium element Se in the positive electrode material first combines with the residual lithium compound to form Li2Se2O3, and in the subsequent battery formation process, Li2Se2O3 and selenium element Se are further converted into Li2SeO3 and / or Li2SeO4 and participate in the growth of CEI film, thereby improving the electrochemical performance of the battery; in this process, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of SEI film, thereby ensuring the capacity of the battery.

[0069] Optionally, the chalcogen element includes selenium and sulfur. Optionally, the chalcogen element includes sulfur and tellurium. Optionally, the chalcogen element includes selenium and tellurium. Optionally, the chalcogen element includes sulfur, selenium, and tellurium.

[0070] By setting the additive to include a reducing chalcogen element, the chalcogen element includes at least one of sulfur, selenium and tellurium, and utilizing the above-mentioned chalcogen element to react with residual lithium compounds, consuming the residual lithium compounds while promoting the growth of the CEI film on the positive electrode, thereby improving the electrochemical performance of the battery; in this process, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of the SEI film in the battery, thereby ensuring the capacity of the battery.

[0071] In some embodiments, the chalcogen element includes elemental sulfur, and the additive includes at least one of elemental sulfur, metal sulfide, polysulfide, sulfur-containing organic polymer or copolymer, and polymeric sulfur.

[0072] Chalcogens include sulfur elements, that is, the additive contains sulfur elements, and the additive can be a sulfur element or a sulfur-containing compound. Optionally, the sulfur-containing compound includes metal sulfides. Optionally, the metal sulfides include transition metal sulfides, and the basic chemical formula of transition metal sulfides (TMDs) is MS2, where M represents a transition metal element, including Ti, V, Ta, Mo, W, Re, etc. Optionally, the sulfur-containing compound includes polysulfides, which are compounds containing polysulfide ions. Optionally, the polysulfide is a polysulfide of an alkali metal or an alkaline earth metal. Optionally, the polysulfide includes lithium polysulfide (Li2S n , wherein n=2 to 8). Optionally, the sulfur-containing compound comprises a sulfur-containing organic polymer or copolymer. Optionally, the sulfur-containing compound comprises polymerized sulfur, which is a product obtained by polymerization reaction of sulfur element and organic matter at high temperature.

[0073] The above-mentioned additives all contain sulfur element, and the valence of sulfur element is relatively low. Sulfur element has reducing properties, which is beneficial to eliminate residual lithium compounds on the surface of the positive electrode active material.

[0074] In some embodiments, the additive includes a chalcogen.

[0075] The additive includes a chalcogen element. Optionally, the chalcogen element includes at least one of sulfur, selenium and tellurium. The additive includes at least one of sulfur, selenium and tellurium.

[0076] The valence of the sulfide element is zero, and the sulfide element itself has strong reducing properties, which makes it easy for the sulfide element to eliminate residual lithium compounds. At the same time, the composition of the sulfide element is single. Introducing the sulfide element into the surface of the positive electrode active material can reduce the introduction of other elements, thereby reducing the risk of side reactions.

[0077] In some embodiments, the one-dimensional conductive material includes a one-dimensional conductive carbon material.

[0078] One-dimensional conductive carbon materials refer to fibrous or tubular carbon materials in which electrons can move freely in only one non-nanoscale direction.

[0079] In addition to having a large specific surface area, the one-dimensional conductive carbon material also has a strong adsorption capacity, which enables the one-dimensional conductive carbon material to effectively adsorb additives attached to the surface of the one-dimensional conductive carbon material, enhance the binding ability between the one-dimensional conductive carbon material and the additive, and improve the anchoring effect of the one-dimensional conductive carbon material on the additive.

[0080] In some embodiments, the one-dimensional conductive carbon material includes at least one of short carbon fiber filaments, nanocarbon fibers, and carbon nanotubes.

[0081] Short carbon fiber filaments refer to carbon fiber filaments with shorter length and smaller diameter. Optionally, the length of the short carbon fiber filaments is less than 10 microns. Optionally, the diameter of the short carbon fiber filaments is less than 1 micron.

[0082] Nanocarbon fibers, also known as carbon nanofibers (CNFs), generally have a diameter of 50 nm to 500 nm and a length of 50 μm to 100 μm. They are one-dimensional conductive carbon materials between carbon nanotubes and ordinary carbon fibers.

[0083] Carbon nanotubes (CNTs) are tubular nanoscale graphite crystals. They are seamless nanotubes made of single or multiple layers of graphite sheets coiled around a central axis at a specific helical angle. Their diameter is typically less than 50 nm.

[0084] The above-mentioned one-dimensional conductive carbon material has good conductivity, which is conducive to building a more developed conductive network. It also has a large specific surface area, which is conducive to increasing the contact area between the one-dimensional conductive carbon material and the additive and enhancing the anchoring effect on the additive.

[0085] In some embodiments, the short carbon fiber filaments include at least one of PAN-based carbon fiber, phenolic-based carbon fiber, viscose-based carbon fiber, pitch-based carbon fiber, biomass-based carbon fiber, and activated carbon fiber.

[0086] PAN-based carbon fibers are made by high-temperature thermosolid-liquid polymerization of polyurethane (PA) and nylon (N).

[0087] Phenolic-based carbon fiber is an amorphous carbon fiber made from phenolic precursor.

[0088] Viscose-based carbon fiber refers to carbon fiber prepared by pre-oxidation and carbonization of viscose fiber.

[0089] Pitch-based carbon fiber refers to a type of carbon fiber prepared from asphalt and other materials rich in polycyclic aromatic hydrocarbons through polymerization, spinning, infusibility, and carbonization.

[0090] Bio-based carbon fibers are made from cellulose and lignin, which come from trees.

[0091] Activated carbon fiber is a kind of activated carbon fiber. Specifically, a certain carbon fiber (such as phenolic fiber, PAN fiber, viscose fiber, asphalt fiber, etc.) is activated at high temperature (different activation methods have different activation temperatures) to produce nano-scale pores on its surface, increasing the specific surface area.

[0092] The above-mentioned short carbon fiber filaments not only have good conductivity and large specific surface area, but also the raw materials are easily available and have high cost performance.

[0093] In some embodiments, the short carbon fiber filaments have a diameter of 100 nm to 500 nm.

[0094] Generally, the diameter of short carbon fiber filaments will affect the specific surface area of ​​the short carbon fiber filaments. The smaller the diameter of the short carbon fiber filaments, the larger the specific surface area of ​​the short carbon fiber filaments. However, if the diameter of the short carbon fiber filaments is too small, it will cause the short carbon fiber filaments to aggregate, which is not conducive to the dispersion of the short carbon fiber filaments. Instead, it will affect the construction of the conductive system and thus affect the conductivity of the positive electrode material.

[0095] Optionally, the diameter of the short carbon fiber filaments is any value among 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm and 500 nm, or a range between any two values.

[0096] By setting the diameter of the short carbon fiber filaments to 100nm-500nm, it is beneficial to ensure that the short carbon fiber filaments have a larger specific surface area, thereby improving the anchoring effect on additives. At the same time, the short carbon fiber filaments have good dispersibility, which is beneficial to improving the conductivity of the positive electrode material.

[0097] In some embodiments, the length of the short carbon fiber filaments is 1 μm to 5 μm.

[0098] The longer the short carbon fiber filaments are, the easier it is for them to entangle and overlap together, thereby building a three-dimensional conductive network. However, the positive electrode active material is usually granular, and the short carbon fiber filaments are distributed on the surface of the positive electrode active material. If the length of the short carbon fiber filaments is too long, it will be detrimental to the contact between the short carbon fiber filaments and the positive electrode active material, affecting the transmission of current between different materials; if the length of the short carbon fiber filaments is too short, it will affect the overlapping effect between the short carbon fiber filaments, especially after the short carbon fiber filaments are wrapped with additives, the short carbon fiber filaments are easily completely wrapped by the additives to produce conductive dead corners, thereby reducing the conductive effect of the positive electrode material.

[0099] Optionally, the length of the short carbon fiber filaments is any value among 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm and 5 μm, or a range between any two values.

[0100] By setting the length of the short carbon fiber filaments to 1μm-5μm, it is beneficial to ensure the contact effect between the short carbon fiber filaments and the surface of the positive electrode active material. At the same time, the short carbon fiber filaments can be well overlapped together to build a conductive network, thereby improving the conductivity of the positive electrode material.

[0101] In some embodiments, the mass percentage of the chalcogen element is 0.02 wt % to 5 wt % based on the total mass of the positive electrode material.

[0102] The content of sulfide in the positive electrode material will affect the removal effect of residual lithium compounds. When the content of sulfide in the positive electrode material is too low, especially when the mass percentage of sulfide in the positive electrode material is less than 0.02wt%, the residual lithium compounds on the surface of the positive electrode active material are difficult to be eliminated. The presence of residual lithium compounds will affect the conductivity of the positive electrode material and will also cause side reactions, thereby causing the battery's cycle stability to deteriorate. Generally, the greater the amount of sulfide loaded in the positive electrode material, the more conducive it is for the sulfide to be dispersed on the surface of the positive electrode active material and react with the residual lithium compounds to eliminate the residual lithium compounds. However, when the mass percentage of sulfide in the positive electrode material is greater than 5wt%, it is easy to cause additive residues, reduce the conductivity of the positive electrode material, increase battery polarization, increase the battery internal resistance (DRC), and continuously consume the active lithium inside the battery during battery storage, causing the battery performance to deteriorate.

[0103] Optionally, based on the total mass of the positive electrode material, the mass percentage of the sulfide element is any point value among 0.02wt%, 0.05wt%, 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% and 5wt%, or a range value between any two points.

[0104] By setting the mass percentage of chalcogen in the positive electrode material to 0.02 wt% to 5 wt%, residual lithium compounds on the surface of the positive electrode active material can be effectively removed, while preventing excessive chalcogen from causing increased battery polarization.

[0105] In some embodiments, the mass percentage of the one-dimensional conductive material is greater than 0 and less than or equal to 1 wt % based on the total mass of the positive electrode material.

[0106] One-dimensional conductive materials are mainly used to improve the conductivity of positive electrode materials. The higher the content of one-dimensional conductive materials in the positive electrode materials, the better the conductivity of the positive electrode materials. However, one-dimensional conductive materials themselves are prone to agglomeration. If the content of one-dimensional conductive materials in the positive electrode materials is too high, especially when the content of one-dimensional conductive materials in the positive electrode materials is greater than 1wt%, it will easily lead to an increase in the surface energy of the positive electrode material particles, prone to physical gelation, and poor processing performance of the positive electrode materials.

[0107] Optionally, based on the total mass of the positive electrode material, the mass percentage of the one-dimensional conductive material is any point value among 0.001wt%, 0.05wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% and 1wt%, or a range value between any two points.

[0108] By setting the mass percentage of the one-dimensional conductive material in the positive electrode material to be greater than 0 and less than or equal to 1 wt %, the positive electrode material has both better conductivity and processing performance.

[0109] Referring to FIG. 5 , in some embodiments, the surface of the positive electrode active material is coated with a coating layer, which includes a first sub-coating layer 71 . The first sub-coating layer 71 includes a one-dimensional conductive material and an additive wrapped around the one-dimensional conductive material.

[0110] Specifically, the positive electrode active material includes positive electrode active material particles 6, and the one-dimensional conductive material and additives are distributed on the surface of the positive electrode active material. The one-dimensional conductive material and additives are wrapped around the surface of the positive electrode active material particles 6 and form a coating layer. For ease of distinction, the coating layer comprising the one-dimensional conductive material and the additive wrapped around the one-dimensional conductive material is defined as the first sub-coating layer 71. The coating layer includes the first sub-coating layer 71. In some embodiments, the coating layer may include only the first sub-coating layer 71. In other embodiments, the coating layer may also include other sub-coating layers.

[0111] By wrapping the one-dimensional conductive material wrapped with the additive on the surface of the positive electrode active material to form the first sub-coating layer 71, the additive is facilitated to eliminate the residual lithium compounds on the surface of the positive electrode active material, thereby improving the performance of the positive electrode active material.

[0112] Please refer to Figure 5. In some embodiments, the coating layer further includes a second sub-coating layer 72, which is arranged on the side of the first sub-coating layer 71 away from the positive electrode active material. The second sub-coating layer 72 contains a conductive agent, a binder and an additive. The content of chalcogen in the second sub-coating layer 72 is greater than or equal to 0 and less than the content of chalcogen in the first sub-coating layer 71.

[0113] Specifically, the coating layer includes at least two sub-coating layers, namely a first sub-coating layer 71 and a second sub-coating layer 72, wherein the first sub-coating layer 71 is directly coated on the surface of the positive electrode active material particles 6, and the second sub-coating layer 72 is arranged on the outside of the first sub-coating layer 71, that is, the first sub-coating layer 71 is arranged between the positive electrode active material particles 6 and the second sub-coating layer 72. Here, the first sub-coating layer 71 and the second sub-coating layer 72 can be in direct contact or arranged at intervals. Furthermore, the second sub-coating layer 72 contains a conductive agent, a binder and an additive. The conductive agent in the second sub-coating layer 72 includes but is not limited to at least one of conductive carbon black, carbon nanotubes, conductive graphite, graphene, acetylene black and nano-carbon fibers. In other words, the conductive agent in the second sub-coating layer 72 can be selected from the above-mentioned one-dimensional conductive materials, or other conductive materials can be used, which increases the material selection range of the second sub-coating layer 72 and helps control the cost of the positive electrode material. The binder in the second sub-coating layer 72 is used to bond the conductive agent and additives together and further bond the conductive agent to the first sub-coating layer 71. The binder includes, but is not limited to, at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and a fluorinated olefin, polyvinyl pyrrolidone, polyacrylonitrile, polymethyl acrylate, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyurethane, fluorinated rubber, and polyvinyl alcohol. The chalcogen content in the second sub-coating layer 72 is greater than or equal to zero and less than the chalcogen content in the first sub-coating layer 71. It is understood that the second sub-coating layer 72 may contain additives (i.e., the chalcogen content is greater than zero) or may not contain additives (i.e., the chalcogen content is equal to zero). When the second sub-coating layer 72 contains additives, the chalcogen content in the second sub-coating layer 72 is less than the chalcogen content in the first sub-coating layer 71.

[0114] The first sub-coating layer 71 and the second sub-coating layer 72 are sequentially coated on the surface of the positive electrode active material, and the content of the chalcogen element in the first sub-coating layer 71 is greater than the content of the chalcogen element in the second sub-coating layer 71. The first sub-coating layer 71 is used as the inner layer. A one-dimensional conductive material with a high specific surface area is used as the conductive material in the first sub-coating layer 71, which is conducive to fixing the additive and inhibiting the diffusion of the chalcogen element outward. The second sub-coating layer 72 is used as the outer layer. It can use a one-dimensional conductive material as a conductive agent or other carbon materials as a conductive agent, thereby expanding the positive electrode active material. The material selection range is expanded, which is conducive to cost control, and the content of sulfide elements in the second sub-coating layer 72 is less than the content of sulfide elements in the first sub-coating layer 71. On the one hand, the sulfide element content in the second sub-coating layer 72 is reduced, which can reduce the outward diffusion of sulfide elements. At the same time, the outer second sub-coating layer 72 can form a barrier to the inner first sub-coating layer 71, alleviating the outward diffusion of sulfide elements in the first sub-coating layer 71. Because the sulfide elements are easy to flow to the negative electrode after diffusing outward, the sulfide elements at the negative electrode react with the active lithium to cause lithium consumption, thereby reducing the battery capacity.

[0115] Please refer to Figure 5. In some embodiments, the content of chalcogen in the second sub-coating layer 72 is greater than 0. The coating layer also includes a third sub-coating layer 73. The third sub-coating layer 73 is coated on the surface of the second sub-coating layer 72. The third sub-coating layer 73 contains a conductive agent and a binder.

[0116] Specifically, the coating layer includes at least three sub-coating layers, namely a first sub-coating layer 71, a second sub-coating layer and a third sub-coating layer 73. The second sub-coating layer 72 contains additives, while the third sub-coating layer 73 does not contain additives. The third sub-coating layer 73 contains a conductive agent and a binder.

[0117] The surface of the positive electrode active material is coated with a first sub-coating layer 71, a second sub-coating layer and a third sub-coating layer 73 in sequence, and the content of chalcogen elements in each sub-coating layer decreases from the inside to the outside. At the same time, the outermost third sub-coating layer 73 does not contain chalcogen elements, which can provide a diffusion space for chalcogen elements, enhance the barrier effect on chalcogen elements, and confine chalcogen elements as much as possible inside the positive electrode material.

[0118] In some embodiments, the coating layer has a thickness of 100 nm to 1000 nm.

[0119] The thickness of the coating layer refers to the total thickness of the coating layer. When the coating layer includes multiple sub-cladding layers, the thickness of the coating layer is the sum of the thicknesses of each of the sub-cladding layers. For example, when the coating layer includes only the first sub-cladding layer 71, the thickness of the coating layer is the thickness of the first sub-cladding layer 71. For example, when the coating layer includes the first sub-cladding layer 71, the second sub-cladding layer, and the third sub-cladding layer 73, the thickness of the coating layer is the sum of the thicknesses of the three sub-cladding layers.

[0120] The coating layer primarily contains conductive materials and additives and contributes little to the battery capacity. Excessive coating thickness can reduce the theoretical specific capacity of the positive electrode material, while excessively thin coating can result in uneven coating, which can affect the removal of residual lithium compounds. Optionally, the coating layer has a thickness of 100 nm to 1000 nm. Specifically, the coating layer can have a thickness of any of 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, and 1000 nm, or a range between any two of these values.

[0121] By setting the thickness of the coating layer to 100 nm to 1000 nm, the theoretical specific capacity of the positive electrode material is guaranteed while the residual lithium compounds are effectively removed.

[0122] In some embodiments, the mass percentage of the coating layer is 0.01 wt % to 6 wt % based on the total mass of the positive electrode material.

[0123] As described above, the coating layer makes little contribution to the battery capacity. Excessive mass percentage of the coating layer in the positive electrode material reduces the theoretical specific capacity of the positive electrode material, while too small a mass percentage affects the removal of residual lithium compounds. Optionally, the mass percentage of the coating layer in the positive electrode material is 0.01 wt% to 6 wt%. Specifically, the mass percentage of the coating layer is any of 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 5.5 wt%, and 6 wt%, or a range between any two of these values.

[0124] Optionally, the mass percentage of the coating layer is 0.1 wt % to 1 wt %.Within this range, the removal effect of the residual lithium compound in the positive electrode material and the theoretical specific capacity of the positive electrode material are optimally balanced.

[0125] By setting the mass percentage of the coating layer in the positive electrode material to 0.01 wt% to 6 wt%, the theoretical specific capacity of the positive electrode material can be guaranteed while effectively removing residual lithium compounds.

[0126] In some embodiments, the positive electrode active material includes a chemical formula of Li a Ni m Co n M 1-m-n A nickel-rich active material containing O2, wherein M comprises at least one of Mn and Al, wherein m≥0.6, n≤0.2, and 0.9≤a≤1.2.

[0127] The chemical formula of nickel-rich active material is Li a Ni m Co n M 1-m-n O2, wherein M includes at least one of Mn and Al. As an example, M includes Mn, and the chemical formula of the nickel-rich active material is Li a Ni m Co n M 1-m-n O2. As an example, M includes Al, and the chemical formula of the nickel-rich active material is Li a Ni m Co n Al 1-m-nO2. Specifically, m≥0.6, and the content of nickel in the nickel-rich active material is increased by increasing the value of m, thereby increasing the reversible lithium insertion capacity of the positive electrode material. Optionally, m is any one of 0.6, 0.7, 0.8, 0.9, 0.95 and 0.99, or a range value between any two of them. Optionally, m≥0.9, and the reversible lithium insertion capacity of the positive electrode material is large within this range. Specifically, n≤0.2, the nickel-rich active material is usually a layered structure, and Co can stabilize the layered structure, but the high price of Co will lead to an increase in the cost of the nickel-rich active material. The cost of the nickel-rich active material can be controlled by controlling n≤0.2. Optionally, n is any one of 0.05, 0.1, 0.15 and 0.2, or a range value between any two of them. 0.9≤a≤1.2, that is, the lithium content in the nickel-rich active material can be greater than 1, equal to 1, or less than 1. When a is greater than 1, the nickel-rich active material is a lithium-rich positive electrode material. As an example, for a nickel-rich active material obtained by pre-lithiation, the Li content can be greater than 1. Optionally, a is any one of 0.9, 0.95, 1, 1.05, 1.1, 1.15 and 1.2, or a value in a range between any two of them.

[0128] However, the nickel element in nickel-rich active materials is alkaline. As the nickel content increases, the nickel-rich active materials are easily exposed to air and absorb moisture and carbon dioxide, and form residual lithium compounds (RLCs) on their surface, such as lithium hydroxide (LiOH) and lithium carbonate (Li2CO3), further increasing the pH of the nickel-rich active materials and seriously affecting the electrochemical properties and storage performance of the nickel-rich active materials.

[0129] Based on this, the present invention introduces additives on the surface of nickel-rich active material, the additives contain reducing chalcogens, and the Ni, Co, Mn in the nickel-rich active material are Ni 3+ / Ni 2+ 、Co 3+ and Mn 4+The nickel-rich active material exists in the form of ions, and the reducing sulfide elements in the additive are easily oxidized by the nickel-rich active material and react with the residual lithium compounds on the surface of the nickel-rich active material, thereby in situ generating an intermediate product containing an intermediate-valent sulfide element on the surface of the nickel-rich active material. In the subsequent chemical formation process, the intermediate product continues to react, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and finally generate a final product containing a high-valent sulfide element (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the chemical formation process, the final product further forms a positive electrode-electrolyte interface (CEI) film on the surface of the nickel-rich active material, thereby removing the residual lithium compounds on the surface of the nickel-rich active material and improving the conductivity and electrochemical properties of the nickel-rich active material. In this process, additional lithium ions will be released synchronously to compensate for the lithium ion loss caused by the formation of the SEI film in the battery, thereby ensuring the capacity of the battery.

[0130] In some embodiments, the DV50 particle size of the positive electrode active material is 5 μm to 15 μm.

[0131] The average particle size is generally expressed as DV50, which means that the powder particles larger and smaller than this particle size each account for 50%. Positive electrode active materials are usually granular, and the particle size of the positive electrode active material affects the processing and electrochemical properties of the positive electrode material. Generally, the larger the particle size of the positive electrode active material, the longer the migration path of lithium ions in the positive electrode active material, which affects the rate performance of the battery. However, the smaller the particle size of the positive electrode active material, the more unstable the viscosity of the positive electrode material will be during the slurrying process, affecting the subsequent slurry coating effect.

[0132] Optionally, the DV50 particle size of the positive electrode active material is any one of 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm and 15 μm, or a range value between any two of them.

[0133] By setting the DV50 particle size of the positive electrode active material to 5 μm to 15 μm, it can be ensured that the positive electrode material has better processing performance and electrochemical performance.

[0134] Some embodiments of the present application also provide a method for preparing a positive electrode material, comprising:

[0135] The one-dimensional conductive material and an additive are mixed to obtain a mixture, wherein the additive includes a chalcogen element having reducing properties;

[0136] sintering the mixed material so that the additive is melted and at least a portion of the one-dimensional conductive material is wrapped by the additive, thereby obtaining a sintered material;

[0137] The sintered material is stirred with the positive electrode active material to obtain the positive electrode material.

[0138] As described above, a one-dimensional conductive material refers to a fibrous or tubular material in which electrons can move freely in only one non-nanoscale direction. One-dimensional conductive materials include, but are not limited to, metal nanowires and one-dimensional conductive carbon materials. Metal nanowires include, but are not limited to, silver nanowires, copper nanowires, etc. The one-dimensional conductive carbon material can be a one-dimensional nanocarbon material or a one-dimensional micron carbon material. Alternatively, the one-dimensional conductive carbon material includes at least one of carbon fibers, nanocarbon fibers, and carbon nanotubes.

[0139] The additive includes a chalcogen with reducing properties, where chalcogen refers to sulfur and elements with similar chemical properties to sulfur. Optionally, the chalcogen includes elements from the chalcogen family other than oxygen. Optionally, the chalcogen includes at least one of sulfur (S), selenium (Se), and tellurium (Te). The additive includes a chalcogen, where the additive can be a compound with the chalcogen as one of the constituent elements of the compound, or a single substance, such as a single substance of the chalcogen itself. Chalcogen has reducing properties, meaning that the chalcogen can increase in valence through redox reactions. Optionally, the chalcogen has a valence less than or equal to zero, i.e., a low-valent chalcogen, which is easily oxidized to a high-valent chalcogen. As an example, the chalcogen includes sulfur, where the valence of low-valent sulfur is -2 or zero, and the valence of high-valent sulfur is +6 or +4.

[0140] The mixing process of the one-dimensional conductive material and the additive refers to mixing the additive and the one-dimensional conductive material together so that the additive is pre-attached to the one-dimensional conductive material.

[0141] Sintering refers to heat treating the mixture at a suitable temperature so that the additive melts, but the additive only changes in physical form and does not react chemically. The additive melts into a more fluid liquid during the sintering process. The liquid additive spreads and disperses on the surface of the one-dimensional conductive material. After the temperature is lowered, the liquid additive solidifies into a solid additive and maintains the spread state, and the additive wraps the one-dimensional conductive material in the form of a film and / or a block. At this time, the one-dimensional conductive material and the additive are physically combined, but because the contact area is relatively large, the binding stability of the additive is enhanced. Optionally, the mixture is sintered under a protective atmosphere, and the protective atmosphere is used to isolate oxygen and prevent the mixture from high-temperature oxidation. The protective atmosphere here can be an inert gas or nitrogen. It is understandable that there are many types of chalcogens, so there will be more types of additives. Different additives have different melting temperatures, so the temperature of the sintering process will also be different, as long as the sintering temperature is controlled to melt the additive.

[0142] The preparation method of the positive electrode material provided in the embodiment of the present application is to mix a one-dimensional conductive material and an additive and then sinter the mixture so that the additive is melted, and at least a portion of the one-dimensional conductive material is wrapped by the additive, thereby increasing the physical contact area between the additive and the one-dimensional conductive material. Combined with the large specific surface area of ​​the one-dimensional conductive material itself, the binding ability of the additive and the one-dimensional conductive material is enhanced, thereby effectively fixing the additive containing the sulfide element. The sintered material obtained after the sintering treatment is further stirred and mixed with the positive electrode active material, so that the one-dimensional conductive material with the additive wrapped on the surface is distributed on the surface of the positive electrode active material, thereby forming a positive electrode material. Since the one-dimensional conductive material itself has good conductivity, a conductive network is formed by bridging the one-dimensional conductive material. Even after being wrapped with the additive, the conductive network can be well connected, thereby ensuring the overall conductive effect of the positive electrode material. In addition, the additives wrapped on the surface of the one-dimensional conductive material will come into contact with the positive electrode active material. During this process, the reducing sulfide elements in the additives will undergo redox reactions with the metal cations in the positive electrode active material and consume the residual lithium compounds on the surface of the positive electrode active material to in situ generate intermediate products containing sulfide elements with intermediate valence (such as Li2S2O3, Li2Se2O3, Li2Te2O3, etc.) on the surface of the positive electrode active material. In the subsequent chemical formation process, the intermediate products continue to react, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and finally generate final products containing high-valence sulfide elements (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the chemical formation process, the final products further form a positive electrode-electrolyte interface (CEI) film on the surface of the positive electrode active material, thereby removing the residual lithium compounds on the surface of the positive electrode active material and improving the conductivity and electrochemical properties of the positive electrode active material. During the conversion of the reducing chalcogen into the CEI film, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of the SEI film, thereby ensuring the battery's capacity. Furthermore, the preparation method of the positive electrode material provided in the embodiments of the present application is simple and easy to operate, facilitating industrialization.

[0143] In some embodiments, the chalcogen element includes at least one of sulfur, selenium, and tellurium.

[0144] As mentioned above, by setting the additive to include a reducing chalcogen element, the chalcogen element includes at least one of sulfur, selenium and tellurium, and the above-mentioned chalcogen element can react with the residual lithium compound, consume the residual lithium compound while promoting the growth of the CEI film on the positive electrode, thereby improving the electrochemical performance of the battery; in this process, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of the SEI film in the battery, thereby ensuring the capacity of the battery.

[0145] In some embodiments, the additive includes a chalcogen.

[0146] The additive includes a chalcogen element. Optionally, the chalcogen element includes at least one of sulfur, selenium and tellurium. The additive includes at least one of sulfur, selenium and tellurium.

[0147] The valence of the sulfide element is zero, and the sulfide element itself has strong reducing properties, which makes it easy for the sulfide element to eliminate residual lithium compounds. At the same time, the composition of the sulfide element is single. Introducing the sulfide element into the surface of the positive electrode active material can reduce the introduction of other elements, thereby reducing the risk of side reactions.

[0148] In some embodiments, the one-dimensional conductive material includes a one-dimensional conductive carbon material.

[0149] One-dimensional conductive carbon materials refer to fibrous or tubular carbon materials in which electrons can move freely in only one non-nanoscale direction.

[0150] In addition to having a large specific surface area, the one-dimensional conductive carbon material also has a strong adsorption capacity, which enables the one-dimensional conductive carbon material to effectively adsorb additives attached to the surface of the one-dimensional conductive carbon material, enhance the binding ability between the one-dimensional conductive carbon material and the additive, and improve the anchoring effect of the one-dimensional conductive carbon material on the additive.

[0151] In some embodiments, the additive includes elemental sulfur, the sintering temperature is 180° C. to 220° C., and / or the sintering time is 5 hours to 7 hours.

[0152] Usually, the temperature of sintering treatment will affect the melting effect of sulfur. If the temperature is too low, sulfur cannot melt, and if the temperature is too high, sulfur will undergo chemical reactions.

[0153] Optionally, the temperature of the sintering process is any one of 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C and 220°C, or a range between any two of them.

[0154] The sintering time will affect the amount of sulfur coated on the surface of the one-dimensional conductive material. If the sintering time is too short, the sulfur content in the positive electrode material will be too low, and the effect of removing residual lithium compounds will be poor. If the sintering time is too long, the sulfur content in the positive electrode material will be too high, resulting in sulfur residue, which will eventually affect the internal resistance of the battery and increase the battery polarization.

[0155] Optionally, the sintering time is any one of 5 h, 5.5 h, 6 h, 6.5 h and 7 h, or a range value between any two of them.

[0156] By using sulfur as an additive, compared to other additives, the chemical properties of sulfur are more active, and the effect of removing residual lithium compounds is better. In addition, the raw materials of sulfur are easy to obtain and the cost is low. Using sulfur as an additive is cost-effective. Furthermore, by setting the sintering temperature to 180°C to 220°C, sulfur can exist stably in the form of a molten liquid within this temperature range and then be coated on the surface of the one-dimensional conductive material. In addition, by setting the sintering time to 5h to 7h, the content of sulfur in the positive electrode material can be effectively controlled, so that sulfur can effectively remove residual lithium compounds without increasing battery polarization.

[0157] In some embodiments, the additive has a DV50 particle size greater than 0 and less than or equal to 1 μm.

[0158] Usually, in the preparation of positive electrode materials, it is necessary to first mix the additives and the one-dimensional conductive material so that the additives are pre-loaded on the one-dimensional conductive material. In this process, the binding force between the additives and the one-dimensional conductive material is very weak. If the particle size of the additives is too large, it is not conducive to the pre-loading of the additives. However, if the particle size of the additives is too small, the additives may agglomerate and cannot be well dispersed on the one-dimensional conductive material, which will also affect the pre-loading effect.

[0159] Optionally, the DV50 particle size of the additive is any one of 10 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm and 1 μm, or a range value between any two of them.

[0160] Optionally, the DV50 particle size of the additive is 100 nm to 500 nm. Within this particle size range, the dispersibility of the additive and its bonding with the one-dimensional conductive material achieve an optimal balance.

[0161] By setting the DV50 particle size of the additive to be greater than 0 and less than or equal to 1 μm, within this range, the additive has a good dispersion effect, and the additive and the one-dimensional conductive material have good binding properties when pre-loaded.

[0162] In some embodiments, the mixing process includes ball milling.

[0163] In order to prevent the additives from agglomerating, the additives usually selected have a larger particle size. However, the larger particle size of the additives will result in poor binding between the additives and the one-dimensional conductive material during pre-load. Based on this, a ball milling process is designed during the mixing process to make the additive particles larger and better dispersed during the initial mixing of the additives and the one-dimensional conductive material. Then, the ball milling process is used to reduce the particle size of the additives, thereby improving the binding stability between the additives and the one-dimensional conductive material.

[0164] By designing a ball milling process in the mixing process, on the one hand, the restriction on the particle size of the additive before the mixing process can be reduced, and the ball milling process can also reduce the particle size of the additive, thereby improving the bonding stability between the additive and the one-dimensional conductive material.

[0165] In some embodiments, the stirring process has a rotation speed of 400 rpm to 1000 rpm.

[0166] Optionally, the rotation speed of the stirring process is any one of 400 r / s, 500 r / s, 600 r / s, 700 r / s, 800 r / s, 900 r / s and 1000 r / s, or a range value between any two of them.

[0167] By setting the rotation speed of the stirring process to 400 r / s to 1000 r / s, the sintering material and the positive electrode active material can be effectively mixed together.

[0168] In some embodiments, the positive electrode active material includes a chemical formula of Li a Ni m Co n M 1-m-n A nickel-rich active material containing O2, wherein M comprises at least one of Mn and Al, wherein m≥0.6, n≤0.2, and 0.9≤a≤1.2.

[0169] The chemical formula of nickel-rich active material is Li a Ni m Co n M 1-m-n O2, wherein M includes at least one of Mn and Al. As an example, M includes Mn, and the chemical formula of the nickel-rich active material is Li a Ni m Co n Mn 1-m-n O2. As an example, M includes Al, and the chemical formula of the nickel-rich active material is Li a Ni m Co n Al 1-m-nO2. Specifically, m≥0.6, and the content of nickel in the nickel-rich active material is increased by increasing the value of m, thereby increasing the reversible lithium insertion capacity of the positive electrode material. Optionally, m is any one of 0.6, 0.7, 0.8, 0.9, 0.95 and 0.99, or a range value between any two of them. Optionally, m≥0.9, and the reversible lithium insertion capacity of the positive electrode material is large within this range. Specifically, n≤0.2, the nickel-rich active material is usually a layered structure, and Co can stabilize the layered structure, but the high price of Co will lead to an increase in the cost of the nickel-rich active material. The cost of the nickel-rich active material can be controlled by controlling n≤0.2. Optionally, n is any one of 0.05, 0.1, 0.15 and 0.2, or a range value between any two of them. 0.9≤a≤1.2, that is, the lithium content in the nickel-rich active material can be greater than 1, equal to 1, or less than 1. When a is greater than 1, the nickel-rich active material is a lithium-rich positive electrode material. As an example, for a nickel-rich active material obtained by pre-lithiation, the Li content can be greater than 1. Optionally, a is any one of 0.9, 0.95, 1, 1.05, 1.1, 1.15 and 1.2, or a value in a range between any two of them.

[0170] However, the nickel element in nickel-rich active materials is alkaline. As the nickel content increases, the nickel-rich active materials are easily exposed to air and absorb moisture and carbon dioxide, and form residual lithium compounds (RLCs) on their surface, such as lithium hydroxide (LiOH) and lithium carbonate (Li2CO3), further increasing the pH of the nickel-rich active materials and seriously affecting the electrochemical properties and storage performance of the nickel-rich active materials.

[0171] Based on this, the present invention introduces additives on the surface of nickel-rich active material, the additives contain reducing chalcogens, and the Ni, Co, Mn in the nickel-rich active material are Ni 3+ / Ni 2+ 、Co 3+ and Mn 4+The nickel-rich active material exists in the form of ions, and the reducing sulfide elements in the additive are easily oxidized by the nickel-rich active material and react with the residual lithium compounds on the surface of the nickel-rich active material, thereby in situ generating an intermediate product containing an intermediate-valent sulfide element on the surface of the nickel-rich active material. In the subsequent chemical formation process, the intermediate product continues to react, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and finally generate a final product containing a high-valent sulfide element (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the chemical formation process, the final product further forms a positive electrode-electrolyte interface (CEI) film on the surface of the nickel-rich active material, thereby removing the residual lithium compounds on the surface of the nickel-rich active material and improving the conductivity and electrochemical properties of the nickel-rich active material. In this process, additional lithium ions will be released synchronously to compensate for the lithium ion loss caused by the formation of the SEI film in the battery, thereby ensuring the capacity of the battery.

[0172] Please refer to Figure 4. Some embodiments of the present application also provide a positive electrode plate 102, including a positive electrode current collector and a positive electrode material layer combined with the positive electrode current collector, and the positive electrode material layer includes the above-mentioned positive electrode material or the positive electrode material prepared according to the above-mentioned positive electrode material preparation method.

[0173] A current collector is a structure or component in a battery that collects current. It's typically made of metal foil. The positive electrode current collector is the structure or component in a battery's positive electrode that collects current. Positive electrode current collectors include, but are not limited to, aluminum foil.

[0174] The positive electrode material layer refers to a film layer disposed on the positive electrode current collector and containing the positive electrode active material. The positive electrode material layer can be disposed on one surface of the positive electrode current collector or on both surfaces. Optionally, the positive electrode material layer includes a conductive agent and a binder.

[0175] The positive electrode plate 102 provided in the embodiment of the present application includes a positive electrode current collector and a positive electrode material layer. The positive electrode material layer includes the above-mentioned positive electrode material, so that the content of residual lithium compounds in the positive electrode plate 102 is low, the overall conductivity of the positive electrode plate 102 is improved, and the cycle performance is improved.

[0176] Please refer to FIG. 2 . Some embodiments of the present application further provide a battery 40 . The battery 40 includes the above-mentioned positive electrode plate 102 .

[0177] Optionally, the battery 40 is a secondary battery, which has many different forms, including but not limited to battery cells, battery modules, and battery packs.

[0178] The battery 40 provided in the embodiment of the present application includes the above-mentioned positive electrode plate 102, and the battery 40 has stable cycle performance and good rate performance.

[0179] Please refer to FIG. 1 . Some embodiments of the present application further provide an electrical device 50 . The electrical device 50 includes the battery 40 described above.

[0180] As described above, the electric device 50 may be, but is not limited to, a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy, an electric tool, and the like.

[0181] The following describes the details in conjunction with specific embodiments.

[0182] Example 1

[0183] S1. Preparation of positive electrode material: sulfur element and polypropylene-based carbon fiber were mixed evenly by ball milling, and then sintered in an inert atmosphere at a temperature of 200°C for 6 hours. Finally, the obtained sintered material was mixed with the positive electrode active material NCM (LiNi 0.9 Co 0.05 Mn 0.05 ) were mixed and stirred at a rotation speed of 600 r / s to obtain a modified positive electrode material, wherein the mass ratio of sulfur elemental: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material was 0.02:0.5:99.48.

[0184] S2. Preparation of positive electrode sheets: The positive electrode material prepared in the above S1, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are dissolved in the solvent N-methylpyrrolidone (NMP) in a weight ratio of 96.5:1.5:2, and the mixture is thoroughly stirred and mixed to obtain a positive electrode slurry; the positive electrode slurry is then evenly coated on the positive electrode collector with a primer, and then dried, cold pressed, and cut to obtain a positive electrode sheet.

[0185] S3. Preparation of negative electrode sheets: The negative electrode active materials graphite, silicon, conductive agent acetylene black, styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) are dissolved in solvent deionized water at a weight ratio of 90:5:2:2:1 and evenly mixed to prepare a negative electrode slurry. The slurry is coated on copper foil, dried, and then cold-pressed and cut to obtain negative electrode sheets.

[0186] S4. Preparation of secondary batteries: stack the positive electrode sheet, separator, and negative electrode sheet in order, so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wind to obtain a bare cell, weld the tabs to the bare cell, and put the bare cell into an aluminum shell, and bake it at 80°C to remove water, then inject electrolyte and seal it to obtain an uncharged battery. The uncharged battery then undergoes static, hot and cold pressing, formation, shaping, capacity testing and other processes in sequence to obtain a secondary battery product. The above-mentioned separator is a PE separator, and its surface is coated with PVDF and alumina coating to improve adhesion and heat resistance. The preparation process of the above-mentioned electrolyte is to mix ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 1:1:1, and then evenly dissolve LiPF6:LiFSI (2:8) in the above-mentioned solution to obtain an electrolyte, in which the concentration of lithium salt is 1 mol / L.

[0187] Example 2

[0188] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the obtained sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a speed of 600 r / s to obtain a modified positive electrode material. According to the mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 1:0.5:98.5.

[0189] Example 3

[0190] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the obtained sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a speed of 600 r / s to obtain a modified positive electrode material. According to the mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 3:0.5:96.5.

[0191] Example 4

[0192] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the obtained sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a speed of 600 r / s to obtain a modified positive electrode material. According to the mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 5:0.5:94.5.

[0193] Example 5

[0194] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the obtained sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a speed of 600 r / s to obtain a modified positive electrode material. According to the mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 6:0.5:93.5.

[0195] Example 6

[0196] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the obtained sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a speed of 600 r / s to obtain a modified positive electrode material. According to the mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 6:1.5:92.5.

[0197] Example 7

[0198] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the obtained sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a speed of 600 r / s to obtain a modified positive electrode material. According to the mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 3:0.02:96.98.

[0199] Example 8

[0200] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the obtained sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a speed of 600 r / s to obtain a modified positive electrode material. According to the mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 3:1:96.

[0201] Example 9

[0202] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the obtained sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a speed of 600 r / s to obtain a modified positive electrode material. According to the mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 3:1.5:95.5.

[0203] Example 10

[0204] The same as Example 3, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the obtained sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a speed of 600r / s to obtain a positive electrode material having a first coating layer on the surface. The mass ratio of sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 2.5:0.5:96.5; the obtained positive electrode material is then mixed with sulfur element, conductive carbon black, and PVDF in a mass ratio of 100:2:2:1 to obtain a positive electrode material having a double-layer coating on the surface; and then mixed with conductive carbon black and PVDF in a mass ratio of 95:3:2 to obtain a three-layer coated positive electrode material.

[0205] Comparative Example 1

[0206] Same as Example 1, except that S1: no sulfur and polypropylene-based carbon fiber are added.

[0207] Comparative Example 2

[0208] The same as Example 1, except that S1: sulfur element and positive electrode active material NCM are mixed, and stirred and mixed at a speed of 600 r / s to obtain a modified positive electrode material, and the mass ratio of sulfur element in the positive electrode material to positive electrode active material NCM is 0.02:99.98.

[0209] Comparative Example 3

[0210] The same as Example 1, except that S1: polypropylene-based carbon fiber filaments are mixed with the positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material. The mass ratio of polypropylene-based carbon fiber filaments to positive electrode active material NCM in the positive electrode material is 0.5:99.5.

[0211] In order to verify the progress of the embodiments of the present application, the secondary batteries prepared in Examples 1 to 10 and Comparative Examples 1 to 3 were subjected to the following tests:

[0212] 1. Secondary battery discharge DCR test:

[0213] Each secondary battery was left at rest for 30 minutes at 25°C, then charged to 4.25V at a rate of 1 / 3C and held at constant voltage until 0.05C was reached. After 10 minutes of rest, the battery was discharged at a rate of 1 / 3C until the battery reached 50% of its full charge capacity, referred to as 50% SOC. After 60 minutes of rest, the battery was discharged at a rate of 4C for 10 seconds, and the DCR value of the battery was recorded.

[0214] 2. Storage test:

[0215] Each secondary battery was stored at 60°C and 97% SOC. Before and during storage, the initial reversible capacity (C0) and actual reversible capacity (Cn) of the cell were measured. The battery was then removed and tested every 15 days. The test procedure was as follows: Each secondary battery was allowed to rest at 25°C for 30 minutes, then charged at a rate of 1 / 3C to 4.25V, then charged to 0.05C at constant voltage. After resting for 30 minutes, the battery was discharged at a rate of 1 / 3C to 2.8V, and the initial reversible capacity (C0) was recorded. Testing was repeated every 15 days, and Cn (n = 1, 2, 3, 4, 5, etc.) was recorded. When Cn / C0 ≤ 80%, n was recorded. The number of days of end-of-life storage (EOL) was 15*n.

[0216] 3. Cycle test:

[0217] Adjust the temperature to 45°C and hold for 2 hours. Let the battery rest for 5 minutes, then charge at 1 / 3C to 4.25V. Continue charging at 4.25V at a constant voltage of 0.05C. Let the battery rest for 5 minutes, then discharge at 0.5C to 2.8V. Let the battery rest for 5 minutes, and repeat the above process until the capacity decays to 80%.

[0218] The test results are shown in Table 1.

[0219] Table 1

[0220] From the comparison of Example 1 and Comparative Example 1 in Table 1, it can be seen that compared with not adding sulfur and carbon fiber, sulfur and carbon fiber are added simultaneously to the positive electrode active material NCM, and the capacity retention rate of the battery is improved both after storage and after cycling. This is because sulfur and carbon fiber filaments are simultaneously introduced onto the surface of the positive electrode active material NCM, and the carbon fiber filaments can construct a conductive network on the surface of the positive electrode active material NCM to improve the conductivity of the positive electrode material and reduce the polarization loss of the battery. At the same time, the carbon fiber filaments anchor the sulfur element, thereby introducing sulfur onto the surface of the positive electrode active material NCM, promoting the full action of sulfur and residual lithium compounds on the surface of the positive electrode active material NCM and generating an artificial CEI film on the surface of the positive electrode active material NCM, effectively reducing the amount of residual lithium compounds, thereby reducing the occurrence of side reactions in the battery, improving the stability of the positive electrode material structure and the interface stability on the positive electrode, and maintaining the capacity of the battery. In the process of the action of sulfur and residual lithium compounds, additional lithium ions are also released synchronously to compensate for the lithium ion loss caused by the formation of SEI film in the battery, thereby ensuring the stock of active lithium and further ensuring the capacity of the battery.

[0221] From the comparison of Example 1 and Comparative Example 2 in Table 1, it can be seen that compared with the addition of only sulfur, when sulfur and carbon fiber are added to the positive electrode active material NCM at the same time, the capacity retention rate of the battery is improved both after storage and after cycling. This is because the conductivity of sulfur itself is poor. Adding only sulfur will make the conductivity of the positive electrode material poor, increase the battery polarization, and at the same time, the sulfur is insufficiently anchored in the positive electrode active material NCM and is easily separated from the positive electrode active material NCM, resulting in insufficient reaction between the sulfur and the residual lithium compound, and the battery capacity cannot be effectively maintained.

[0222] From the comparison of Example 1 and Comparative Example 3 in Table 1, it can be seen that compared with adding only carbon fiber, when sulfur and carbon fiber are added simultaneously to the positive electrode active material NCM, the capacity retention rate of the battery is improved both after storage and after cycling. This is because the conductivity of the positive electrode material is improved by adding only carbon fiber, but the residual lithium compounds on the surface of the positive electrode active material NCM cannot be eliminated. The presence of residual lithium compounds will affect the conductivity of the positive electrode active material NCM on the one hand, and will also promote the occurrence of side reactions, thereby affecting the capacity of the battery.

[0223] It can be seen from Examples 1 to 5 in Table 1 that the carbon fiber content is fixed. As the sulfur content increases, the capacity retention rate after storage and the capacity retention rate after cycle both increase. However, when the sulfur content is greater than 5wt%, the capacity retention rate after storage and the capacity retention rate after cycle decrease instead. This is because the excessive sulfur content leads to sulfur residue, which reduces the conductivity of the positive electrode material and increases the battery polarization. In addition, the active lithium inside the battery will continue to be consumed during battery storage, and the battery performance will deteriorate.

[0224] It can be seen from Example 7, Example 3, Example 8 and Example 9 in Table 1 that when the sulfur content is fixed and the carbon fiber content is increased, the battery DCR decreases, and the battery capacity retention rate after storage and the capacity retention rate after cycle are relatively high.

[0225] It can be seen from Examples 6 and 9 in Table 1 that although increasing the carbon fiber content can reduce the battery DCR, when the carbon fiber content is greater than 1 wt%, for example, 1.4 wt% or 1.5 wt%, physical gelation of the positive electrode material is likely to occur during slurrying, and the processing performance of the positive electrode material deteriorates.

[0226] In addition, from the comparison of Example 3 and Example 10 in Table 1, it can be seen that a multi-layer coating is provided on the surface of the positive electrode active material NCM, and from the inside to the outside, the content of elemental sulfur in each coating layer decreases successively, and the capacity retention rate of the battery after storage is significantly improved. This is because the outer coating layer with a low sulfur content can block the inner coating layer with a high sulfur content, thereby limiting as much sulfur as possible inside the positive electrode material, inhibiting the sulfur from flowing to the negative electrode to react with the active lithium and causing lithium consumption, thereby improving the battery capacity retention rate.

[0227] The above are merely optional embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included within the scope of the claims of the present application.

Claims

1. A positive electrode material, characterized in that: include: A positive electrode active material and a one-dimensional conductive material and an additive distributed on the surface of the positive electrode active material, at least part of the one-dimensional conductive material is wrapped by the additive, and the additive contains a reducing chalcogen element.

2. The positive electrode material according to claim 1, characterized in that The chalcogen element includes at least one of sulfur, selenium and tellurium.

3. The positive electrode material according to claim 1 or 2, characterized in that The chalcogen element includes sulfur element, and the additive includes at least one of sulfur element, metal sulfide, polysulfide, sulfur-containing organic polymer or copolymer, and polymerized sulfur.

4. The positive electrode material according to any one of claims 1 to 3, characterized in that The additive includes a simple substance of chalcogen.

5. The positive electrode material according to any one of claims 1 to 4, characterized in that: The one-dimensional conductive material includes a one-dimensional conductive carbon material.

6. The positive electrode material according to claim 5, characterized in that The one-dimensional conductive carbon material includes at least one of short carbon fiber filaments, nano carbon fibers and carbon nanotubes; optionally, the short carbon fiber filaments include at least one of PAN-based carbon fibers, phenolic-based carbon fibers, viscose-based carbon fibers, asphalt-based carbon fibers, biomass-based carbon fibers and activated carbon fibers.

7. The positive electrode material according to claim 6, characterized in that The diameter of the short carbon fiber filaments is 100 nm-500 nm; and / or the length of the short carbon fiber filaments is 1 μm-5 μm.

8. The positive electrode material according to any one of claims 1 to 7, characterized in that: Based on the total mass of the positive electrode material, the mass percentage of the chalcogen element is 0.02 wt % to 5 wt %.

9. The positive electrode material according to any one of claims 1 to 8, characterized in that Based on the total mass of the positive electrode material, the mass percentage of the one-dimensional conductive material is greater than 0 and less than or equal to 1 wt %.

10. The positive electrode material according to any one of claims 1 to 9, characterized in that: The surface of the positive electrode active material is coated with a coating layer, wherein the coating layer includes a first sub-coating layer, and the first sub-coating layer includes the one-dimensional conductive material and the additive wrapped on the one-dimensional conductive material.

11. The positive electrode material according to claim 10, characterized in that The coating layer also includes a second sub-coating layer, which is arranged on a side of the first sub-coating layer away from the positive electrode active material, the second sub-coating layer contains a conductive agent and a binder, and the content of the chalcogen element in the second sub-coating layer is greater than or equal to 0 and less than the content of the chalcogen element in the first sub-coating layer.

12. The positive electrode material according to claim 11, characterized in that The content of the chalcogen element in the second sub-coating layer is greater than 0, and the coating layer further includes a third sub-coating layer, which is coated on the surface of the second sub-coating layer, and the third sub-coating layer contains the conductive agent and the binder.

13. The positive electrode material according to any one of claims 10 to 12, characterized in that: The coating layer has a thickness of 100 nm to 1000 nm.

14. The positive electrode material according to any one of claims 10 to 13, characterized in that: Based on the total mass of the positive electrode material, the mass percentage of the coating layer is 0.01wt% to 6wt%; optionally, the mass percentage of the coating layer is 0.1wt% to 1wt%.

15. The positive electrode material according to any one of claims 1 to 14, characterized in that: The positive electrode active material includes a chemical formula of Li a Ni m Co n M 1-m-n O2-rich nickel active material, wherein M includes at least one of Mn and Al, wherein m≥0.6, n≤0.2, 0.9≤a≤1.2; optionally, m≥0.

9.

16. The positive electrode material according to any one of claims 1 to 15, characterized in that: The DV50 particle size of the positive electrode active material is 5 μm to 15 μm.

17. A method for preparing a positive electrode material, characterized in that: include: The one-dimensional conductive material and an additive are mixed to obtain a mixture, wherein the additive comprises a chalcogen element having reducing properties; Sintering the mixed material so that the additive is melted and at least a portion of the one-dimensional conductive material is wrapped by the additive, thereby obtaining a sintered material; The sintered material is stirred with the positive electrode active material to obtain the positive electrode material.

18. The method for preparing the positive electrode material according to claim 17, characterized in that: The chalcogen element includes at least one of sulfur, selenium and tellurium.

19. The method for preparing a positive electrode material according to any one of claims 17 or 18, characterized in that: The additive includes a chalcogen element; and / or the one-dimensional conductive material includes a one-dimensional conductive carbon material.

20. The method for preparing the positive electrode material according to claim 19, characterized in that: The additive includes elemental sulfur, the sintering temperature is 180° C. to 220° C., and / or the sintering time is 5 h to 7 h.

21. The method for preparing a positive electrode material according to any one of claims 17 to 20, characterized in that: The DV50 particle size of the additive is greater than 0 and less than or equal to 1 μm; optionally, the DV50 particle size of the additive is 100 nm to 500 nm.

22. The method for preparing a positive electrode material according to any one of claims 17 to 21, characterized in that: The mixing process includes ball milling; and / or the stirring process has a rotation speed of 400 r / s to 1000 r / s.

23. The method for preparing a positive electrode material according to any one of claims 17 to 22, characterized in that: The positive electrode active material includes a chemical formula of Li a Ni m Co n M 1-m-n O2-rich nickel active material, wherein M includes at least one of Mn and Al, wherein m≥0.6, n≤0.2, 0.9≤a≤1.2; optionally, m≥0.

9.

24. A positive electrode plate, characterized in that: It comprises a positive electrode current collector and a positive electrode material layer bonded to the positive electrode current collector, wherein the positive electrode material layer comprises the positive electrode material according to any one of claims 1 to 16 or the positive electrode material prepared by the method for preparing the positive electrode material according to any one of claims 17 to 23.

25. A battery, characterized in that: Comprising the positive electrode sheet according to claim 24.

26. An electrical device, characterized in that: Comprising a battery according to claim 25.

Citation Information

Patent Citations

  • Sulfur-containing composite anode, preparation method thereof and lithium-sulfur battery using sulfur-containing composite anode as anode

    CN104716296A

  • Preparation method of positive electrode composite material for lithium sulfur battery

    CN107978741A

  • Low-temperature vapor deposition coated high-nickel ternary layered positive electrode material and preparation method thereof

    CN112768662A

  • Slurry, positive pole piece, secondary battery, battery module, battery pack and electric device

    CN115832299A

  • Lithium-sulfur secondary battery

    US20220173382A1

Cited By

  • Lithium-rich lithium ferrite lithium supplement agent as well as synthesis method and application thereof

    CN119905695A

  • Positive electrode material and preparation method and application thereof

    CN120432512A

  • A positive electrode material, a preparation method and application thereof

    CN120432512B

  • Lithium-ion battery positive electrode material and preparation method therefor, and lithium-ion battery

    WO2026223420A1