Silicon-carbon negative electrode material, and preparation method therefor and application thereof
By using porous carbon skeleton and silicon-based components in lithium-ion batteries, combined with carbon cladding protection, the volume expansion problem of silicon-based negative electrode materials is solved, the circulation performance and energy density are improved, and lithium ion is realized High-efficiency energy density and long life of the battery.
Patent Information
- Application Number
- PCT/CN2023/133665
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2023-11-23
- Publication Date
- 2024-11-21
AI Technical Summary
The existing silicon-based anode materials are insufficient in cycling and electrochemical properties due to volume expansion in lithium-ion batteries, making it difficult to effectively improve energy density.
Using a porous carbon skeleton as the core, the silicon-based components are deposited to form a silicon-carbon negative electrode material. By regulating the porous structure of the porous carbon skeleton and the particle size of the silicon-based components, the volume expansion of the silicon-based components is limited and the electron and ionic conductivity is improved. The rate, combined with carbon cladding protection, improves the circulation and rate performance of the material.
It significantly reduces the volume expansion of silicon-based components during charging and discharging, improves the cycling and rate performance of silicon-carbon negative electrode materials, increases the energy density, and the specific capacity can reach 500mAh/g to 800mAh/g, which significantly improves the The energy density and cycle life of lithium-ion batteries.
Smart Images

Figure CN2023133665_21112024_PF_FP_ABST
Abstract
Description
A silicon-carbon negative electrode material and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of secondary battery materials and preparation methods thereof, and in particular to a silicon-carbon negative electrode material and a preparation method and application thereof. Background Art
[0002] In the current power battery and consumer battery markets, lithium-ion batteries have become the dominant energy storage system due to their significant advantages in voltage, lifespan, self-discharge, and energy density. Furthermore, due to the endless demand for improved battery life in various usage scenarios, increasing the energy density (ED) (volume energy density (VED) and mass energy density (GED)) of lithium-ion batteries is the ultimate goal, provided that other basic performance characteristics are met.
[0003] Both positive and negative electrode materials affect the energy density of lithium-ion batteries. Positive electrode materials have reached their capacity limits or have only seen modest improvements (lithium iron phosphate 150 / 175mAh / g, nickel-cobalt-manganese ternary cathode 190 / 205mAh / g, lithium manganese oxide 142 / 148mAh / g). Graphite, due to its high stability and suitable voltage, is a commonly used commercial anode material. However, graphite anodes have reached a compromise between capacity and initial efficiency (355 / 372mAh / g). To overcome this energy density bottleneck, silicon-based anodes are increasingly being used in consumer batteries and are beginning to develop in power batteries. Their primary value lies in their high gram capacity, more than ten times that of graphite (4200mAh / g vs. 372mAh / g). However, because they can accommodate a large number of lithium ions for alloying reactions, they experience volume expansion exceeding 300% during the lithium insertion and extraction process during battery cycling. This volume expansion significantly impacts the cycling performance of silicon-based anode materials.
[0004] The routes of silicon-based negative electrodes mainly include silicon-oxygen route, pre-lithiation silicon-oxygen material and silicon-carbon material. Among them, in the silicon-oxygen route, the first efficiency of the negative electrode material is too low (~76%), which will cause a large loss of active lithium ions in the positive electrode; pre-lithiation silicon-oxygen material can make up for the problem of too low first efficiency of silicon-oxygen material to a certain extent, but in the pre-lithiation process, the lithium source used is expensive, and the first efficiency improvement is close to the limit (82%); the preparation method of traditional silicon-carbon material is mostly to mix silicon source and carbon source and grind them to reduce the particle size of silicon source. The lower limit of silicon particle size in grinding method is very close (20nm thick, 100nm long flake), but the obtained silicon-carbon material still cannot solve the structural impact of its lithium insertion expansion on the battery cell.
[0005] In summary, current industrial introduction verification has proved that the commonly used solutions for silicon-based negative electrodes have reached the design capacity limits: 390mAh / g, 420mAh / g, and 400mAh / g; and the volume expansion problem of the resulting silicon-based negative electrode materials still cannot be well solved, that is, the cycle performance and other electrochemical properties of batteries including the above-mentioned silicon-based negative electrode materials need to be further improved.
[0006] Summary of the Invention
[0007] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a silicon-carbon anode material that can effectively improve the rate performance and cycle performance of silicon-carbon-based anode materials.
[0008] The present invention also provides a method for preparing the silicon-carbon negative electrode material.
[0009] The present invention also provides a lithium ion battery comprising the silicon-carbon negative electrode material.
[0010] The present invention also provides applications of the lithium ion battery.
[0011] According to an embodiment of the first aspect of the present invention, a silicon-carbon negative electrode material is provided, wherein the silicon-carbon negative electrode material comprises a core and a shell wrapped around the surface of the core; the true density of the silicon-carbon negative electrode material is p RD ;
[0012] The core comprises a porous carbon skeleton and a silicon-based component dispersed in the porous carbon skeleton; the pore volume of the porous carbon skeleton is PV, and the true density is ρ C ; The true density of the silicon-based component is ρ Si ;
[0013] And satisfy formula (I):
[0014] Where: 1.5g / cc≤ρ RD ≤2.4g / cc; 0.45cc / g≤PV≤1.55cc / g; 1g / cc≤ρ Si ≤2.35g / cc; 1.2g / cc≤ρ C ≤2.28g / cc.
[0015] The silicon-carbon negative electrode material according to the embodiment of the present invention has at least the following beneficial effects:
[0016] (1) In traditional technology, silicon-based materials are mostly crushed by mechanical methods in order to obtain small-particle silicon-based materials that can alleviate volume expansion, but the effect obtained by this technical means is not obvious.
[0017] The preparation method provided by the present invention limits the dispersion of the silicon-based component in the porous carbon skeleton, thereby allowing the particle size of the silicon-based component to be limited by the size of the pores of the porous carbon skeleton. Therefore, the particle size of the silicon-based component can be adjusted more conveniently and within a wider range, thereby minimizing the degradation of electrochemical performance caused by the volume expansion of the silicon-based component during the charge and discharge process.
[0018] Specifically, the volume expansion of the silicon-carbon negative electrode material provided by the present invention in a fully embedded state is reduced by about 50% compared to the volume expansion of the silicon-carbon negative electrode material prepared by a traditional grinding method in a fully embedded state.
[0019] (2) Compared with the traditional silicon carbon (produced by degradation of Si grinding particles, 20nm thin, 100nm long, and flaky) produced by Samsung and other companies, in the silicon-carbon negative electrode material provided by the present invention, the silicon-based component is evenly dispersed in the porous carbon skeleton, which maximizes the dispersion of the silicon-based component, thereby maximizing the stress distribution of the silicon-carbon negative electrode material caused by the expansion of the silicon-based component during lithium extraction and insertion, and minimizing the impact of the expansion of the silicon-based component on the battery core structure in the lithium-ion battery. In addition, this dispersed distribution method can significantly enhance the synergistic effect between the silicon-based component and the porous carbon skeleton, and enhance the electronic conductivity and ionic conductivity of the silicon-carbon negative electrode material. Ultimately, the cycle performance and rate performance of the obtained silicon-carbon negative electrode material are improved.
[0020] (3) The silicon-carbon negative electrode material provided by the present invention has a shell, which can protect it from being stirred in the aqueous binder during the battery cell preparation process, corroded and oxidized during the slurrying process, and producing other gases such as hydrogen that are not conducive to the battery cell production process.
[0021] (4) The silicon-carbon negative electrode material itself is known for its high gram capacity density. Even if the gram capacity density is high, if the true density is too low, the volume density of the silicon-carbon negative electrode material will be low. Therefore, the true density is a key indicator of whether the silicon-carbon negative electrode material can bring a real energy density improvement effect to the battery cell. The present invention defines the relationship between the true density of the silicon-carbon negative electrode material, the pore volume of the porous carbon skeleton, the true density and the true density of the silicon-based component, so as to maximize the suppression of the volume change caused by the deintercalation and deintercalation of lithium by the silicon-based component in the silicon-carbon negative electrode material on the volume impact of the silicon-carbon negative electrode material particles themselves: ultimately achieving the large-scale application and introduction of silicon-based components in the negative electrode of the battery cell.
[0022] (5) The present invention selects a porous carbon skeleton with appropriate parameters based on the particle size and crystalline structure achievable by the silicon-based component production process, and regulates both the space provided by the porous carbon skeleton for the silicon-based component and the mechanical strength of the porous carbon skeleton itself, thereby synthesizing a low-expansion, highly compatible silicon-carbon negative electrode material for lithium-ion batteries. In other words, the porous carbon skeleton's pore structure (pore volume), mechanical strength (pressure bearing capacity), degree of graphitization (true density), particle size of the silicon-based component (limited by pore size), distribution dispersion (affected by pore distribution), and crystalline structure (true density of the silicon-based component) interact synergistically, significantly improving its overall performance.
[0023] Specifically, currently, under the premise of ensuring cell expansion, the composite capacity of a "silicon + graphite" composite anode system can only reach about 400 mAh / g. However, using the "silicon-carbon anode material + graphite" provided by the present invention, the volume expansion of the soft-pack battery cell can be minimized in different cell structure designs, increasing the composite capacity of the anode from 355 mAh / g of graphite to 500 mAh / g, and even reaching an upper limit of 800 mAh / g.
[0024] According to some embodiments of the present invention, in formula (I), p RD The concentration is 1.75 to 2.25 g / cc. Specifically, it can be about 1.9 g / cc, 2.1 g / cc, or 2.2 g / cc.
[0025] According to some embodiments of the present invention, in formula (I), PV is 0.55 to 0.95 cc / g, for example, about 0.65 cc / g, 0.7 cc / g, 0.75 cc / g, or 0.9 cc / g.
[0026] According to some embodiments of the present invention, in formula (I), p Si It is 1.25~1.75g / cc.
[0027] According to some embodiments of the present invention, in formula (I), p C The concentration is 1.5 to 2.2 g / cc. Specifically, it can be about 1.8 g / cc or 2.1 g / cc.
[0028] According to some embodiments of the present invention, the mass percentage of the silicon-based component in the silicon-carbon negative electrode material is W Si , the lithium insertion capacity of the silicon-carbon negative electrode material is CAP; and satisfies formula (II); 180≤CAP-3769×W Si ≤680 Formula (II);
[0029] Among them, 30% ≤ W Si ≤60%.
[0030] According to some embodiments of the present invention, in formula (II), W Si The value range is 30~57%.
[0031] According to some embodiments of the present invention, in formula (II), W Si The value range is 35% to 55%.
[0032] According to some embodiments of the present invention, in formula (II), W Si The value range of is 43-47%, for example, it can be about 45%.
[0033] According to some embodiments of the present invention, the particle size D of the silicon-based component is Si Range: 2nm≤D Si ≤10nm. The upper limit of the particle size of the silicon-based component is limited by the pore size in the polycarbon skeleton. However, when it is less than or equal to the above pore size, D Si It can be adjusted according to the actual preparation process.
[0034] According to some embodiments of the present invention, the tap density of the silicon-carbon negative electrode material is TD The range is: 0.8g / cc≤ρ TD ≤1.2g / cc.
[0035] According to some embodiments of the present invention, the tap density of the silicon-carbon negative electrode material is TD The range is 0.82~1.13g / cc.
[0036] According to some embodiments of the present invention, the tap density of the silicon-carbon negative electrode material is TD The range is 0.84~1.1g / cc.
[0037] According to some embodiments of the present invention, the tap density of the silicon-carbon negative electrode material is TD The range is 0.92 to 0.97 g / cc. For example, it can be about 0.95 g / cc.
[0038] According to some embodiments of the present invention, the particle size of the silicon-carbon negative electrode material satisfies: 0.45 μm ≤ D n10 ≤1μm.
[0039] According to some embodiments of the present invention, the particle size of the silicon-carbon negative electrode material satisfies: 1.2 μm ≤ D V10 ≤5.2μm、6μm≤D V50 ≤9μm、11μm≤D V90 ≤18μm、19μm≤D V99 ≤26μm、27μm≤D VMAX ≤35μm.
[0040] According to some embodiments of the present invention, in the silicon-carbon negative electrode material, the sum of the mass percentages of silicon and carbon elements is greater than 98%.
[0041] According to some embodiments of the present invention, the material of the shell includes at least one of carbon, metal oxide and organic polymer.
[0042] According to some embodiments of the present invention, the metal oxide includes at least one of aluminum oxide, iron oxide, magnesium oxide, cobalt oxide, nickel oxide, copper oxide, and zinc oxide.
[0043] According to some embodiments of the present invention, the organic polymer includes at least one of a conductive polymer and a non-conductive polymer.
[0044] The conductive polymer includes at least one of polyacetylene, polypyrrole, polythiophene, polyphenylene vinylene and polyaniline.
[0045] The non-conductive polymer includes at least one of polyethylene, polypropylene, polystyrene, epoxy resin and phenolic resin.
[0046] According to some embodiments of the present invention, the mass percentage of the shell to the silicon-carbon negative electrode material is 0.7-5.3%.
[0047] According to some embodiments of the present invention, the shell accounts for 1.5-2.5% by mass of the silicon-carbon negative electrode material, for example, about 1.9%, 2.1% or 2.2%.
[0048] According to some embodiments of the present invention, the FCE of the silicon-carbon negative electrode material 2.0V 84% ≤ FCE 2.0V ≤94.5%.
[0049] According to some embodiments of the present invention, the FCE of the silicon-carbon negative electrode material 2.0V The range is 86-94%.
[0050] According to some embodiments of the present invention, the FCE of the silicon-carbon negative electrode material 2.0V The range is 87~91.5%.
[0051] According to some embodiments of the present invention, the FCE of the silicon-carbon negative electrode material 2.0V The range is 88-91%, for example, about 89% or 90%.
[0052] According to some embodiments of the present invention, the FCE of the silicon-carbon negative electrode material 0.8V 75% ≤ FCE 0.8V ≤84.5%.
[0053] According to some embodiments of the present invention, the FCE of the silicon-carbon negative electrode material 0.8V The range is 78-83%.
[0054] According to some embodiments of the present invention, the FCE of the silicon-carbon negative electrode material 0.8V The range is 78-82.5%, for example, about 80% or 81%.
[0055] The FEC here is: the first effect of the silicon-carbon negative electrode material when the button cell is assembled with the silicon-carbon negative electrode material as the test electrode and the lithium sheet as the counter electrode; more specifically, FCE 2.0V To test the first effect of the silicon-carbon negative electrode material when the upper voltage limit is 2.0V, FCE 0.8V The first effect of the silicon-carbon negative electrode material is measured when the upper limit of the test voltage is 0.8V.
[0056] According to some embodiments of the present invention, the gram-specific capacity of the silicon-carbon anode material is 1600 to 2600 mAh / g, for example, about 1650 mAh / g, 2000 mAh / g, 2100 mAh / g, 2150 mAh / g, 2180 mAh / g, 2200 mAh / g, or 2500 mAh / g.
[0057] According to some embodiments of the present invention, a negative electrode sheet using the silicon-carbon negative electrode material as the negative electrode active material exhibits a thickness increase of ≤140% when fully intercalated with lithium. Consequently, when blended with a graphite negative electrode as the negative electrode active material, the gram-specific capacity of the negative electrode can be significantly increased without significant volume expansion. This thickness increase can be as low as 83%, and can specifically be approximately 85%, 90%, 95%, 100%, or 110%.
[0058] According to an embodiment of the second aspect of the present invention, a method for preparing the silicon-carbon negative electrode material is provided, the method comprising the following steps:
[0059] S1. cracking the carbon raw material to obtain the porous carbon skeleton;
[0060] S2. Depositing the silicon-based component in the porous carbon skeleton to obtain the core;
[0061] S3. Wrapping the substance obtained in step S2 to form the shell.
[0062] Since the preparation method adopts all the technical solutions of the silicon-carbon negative electrode material of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.
[0063] Furthermore, conventional technologies also use graphite as a substrate. The preparation method provided by the present invention uses cracked carbon as a porous carbon skeleton, which has the following advantages:
[0064] (1) It overcomes the problems of obvious graphite layer cleavage, interlayer slip, and poor isotropic expansion suppression in traditional technologies, that is, obvious anisotropy of internal stress, and has the advantage of good isotropy.
[0065] (2) It overcomes the problem that the cracked carbon in traditional technology has good controllability and can be synthesized from different organic raw materials, while the graphite matrix is single and the performance controllability is poor, and has the advantage of controllable performance.
[0066] (3) It overcomes the problem that the pores of graphite in traditional technologies are difficult to expand and modify, so the connectivity between pores in micron-level particles may be poor, that is, the pores in porous graphite are difficult to be evenly distributed. Therefore, even if silicon-based components are deposited therein, the problem of uniform dispersion of silicon-based components cannot be achieved. It has the advantages of easy modification of pore structure and better uniformity and dispersion of silicon-based components.
[0067] That is, the present invention uses cracked carbon as a porous carbon skeleton, which has the advantages of good isotropy, controllable performance, easy modification of pore structure, and better distribution uniformity and dispersibility of silicon-based components.
[0068] The present invention uses a deposition method to produce silicon-based components, a bottom-up approach to micro-nanoparticle construction. Compared to traditional top-down construction methods such as grinding, the silicon-based component's particle size is smaller and limited by the pore size of the porous carbon framework. Furthermore, the silicon-based component can be dispersed as much as possible within the porous carbon framework. This further mitigates the stress impact on the battery caused by the volume change of the silicon-based component during charge and discharge.
[0069] According to some embodiments of the present invention, the carbon raw material includes at least one of a bio-based carbon raw material and other organic matter.
[0070] According to some embodiments of the present invention, the bio-based carbon raw materials include at least one of corn straw, wheat straw, rice straw, peanut straw, soybean straw, sorghum straw, cotton straw, reed straw, Changpu, Alpinia officinalis, sesame straw, wood powder, peanut shells, husks, rice husks, walnut shells, oak shells, sugarcane bagasse, red atractylodes residue, soybean residue, pine needles, pine cones, apple branches, pear branches, peach branches, eucalyptus branches, pig manure, cow manure, sheep manure, chicken manure, kitchen waste, apples and bananas.
[0071] According to some embodiments of the present invention, the other organic matter includes at least one of a benzene ring, C=C, a nitrogen atom, a sulfur atom, a heterocycle, and a bridged ring.
[0072] According to some embodiments of the present invention, the cracking temperature is 350-1200°C.
[0073] According to some embodiments of the present invention, the cracking temperature is 500-700°C, for example, about 650°C.
[0074] According to some embodiments of the present invention, the lysis time is 0.5 to 24 hours.
[0075] According to some embodiments of the present invention, the lysis time is 1 to 3 hours, for example, about 2 hours.
[0076] Under the above temperature and time conditions, the obtained pyrolysis products can be directly used as porous carbon skeletons, or can be convenient for subsequent pore modification.
[0077] When calculating the mass percentages of carbon and silicon in the silicon-carbon negative electrode material, it is assumed that the porous carbon skeleton produced by cracking is entirely carbon.
[0078] According to some embodiments of the present invention, step S1 further comprises performing pore modification on the pyrolysis product after the pyrolysis, thereby further facilitating the deposition of the silicon-based component in step S2 and obtaining the silicon-based component with the target particle size and content.
[0079] According to some embodiments of the present invention, the pore modification includes at least one of pore enlargement, pore blocking and chemical modification.
[0080] According to some embodiments of the present invention, the pore modification method comprises at least one of a physical method and a chemical method.
[0081] According to some embodiments of the present invention, in the pore modification, the chemical method includes using an alkali or salt to expand the pores of the cleavage product, thereby generating a large number of mesopores and micropores in the cleavage product.
[0082] The base includes at least one of potassium hydroxide and sodium hydroxide;
[0083] When alkali is used for the pore modification, the method includes soaking the cleavage product in an alkali solution until the pore structure of the product meets the requirements. The concentration of the alkali solution is 1 to 4 mol / L, for example, specifically about 2 mol / L or 3 mol / L. The mass ratio of the alkali in the alkali solution to the cleavage product is 1:8 to 12. Specifically, it can be about 1:10. At this time, the temperature of the pore modification is 50 to 200°C. For example, it can be about 100°C or 175°C.
[0084] The salt includes at least one of potassium carbonate and zinc chloride.
[0085] According to some embodiments of the present invention, in the pore modification, the physical method includes heat-treating the pyrolysis product with carbon dioxide or water vapor, thereby expanding the pores of the obtained pyrolysis product.
[0086] According to some embodiments of the present invention, during the pore modification, carbon-containing organic gas may be used to perform CVD deposition in the pores, i.e., pore filling, pore blocking, etc., to further refine the pore volume distribution.
[0087] According to some embodiments of the present invention, in step S2, the deposition method includes chemical vapor deposition.
[0088] Specifically, the chemical vapor deposition method includes diffusing a gaseous silicon source into the pores of the porous carbon skeleton and then pyrolyzing it, or includes diffusing the pyrolysis products of the gaseous silicon source into the pores of the porous carbon skeleton; or both mechanisms occur simultaneously.
[0089] According to some embodiments of the present invention, the silicon source is in a gas phase at 500°C.
[0090] According to some embodiments of the present invention, the silicon source includes at least one of silane and substituted silane.
[0091] According to some embodiments of the present invention, the silane includes SiH4, Si2H6, Si2H4, Si3H8, Si3H6, Si3H4, Si4H 10 、Si4H8、Si4H6、Si5H 12 、Si5H 10 、Si5H8、Si5H6、Si6H 14 、Si6H 12 、Si6H 10 、Si6H8、Si6H6、Si7H 16 、Si7H 14 、Si7H 12 、Si7H 10 、Si7H8、Si7H6、Si8H 18 、Si8H 16 、Si8H 14 、Si8H 12 、Si8H 10 、Si8H8、Si9H 20 、Si9H 18 、Si9H 16 、Si9H 14 、Si9H 12 、Si9H 10 、Si9H8、Si 10 H 22 、Si 10 H 20 、Si 10 H 18 、Si 10 H 16 、Si 10 H14 and Si 10 H 10 At least one of .
[0092] According to some embodiments of the present invention, the substituted silane is obtained by replacing H of the silane with at least one of B, N, F, P, S and Cl.
[0093] Compared to traditional silicon-oxygen materials, pre-lithiated silicon-oxygen materials, and silicon-carbon materials produced by grinding, the silicon-carbon anode material proposed in this invention utilizes silicon raw materials from a relatively upstream segment of the silicon supply chain, offering significant cost advantages when calculated per unit capacity. Specifically, referring to the recent selling price of Shin-Etsu silicon-carbon (>160w / ton), the silicon-carbon anode material proposed in this invention can achieve a 50% cost reduction while maintaining production profitability.
[0094] According to some embodiments of the present invention, the chemical vapor deposition temperature of the silicon-based component is 250°C to 1100°C.
[0095] According to some embodiments of the present invention, the chemical vapor deposition temperature of the silicon-based component is 450-800° C., for example, about 600° C.
[0096] The chemical vapor deposition ends when the designed amount of the silicon-based component is deposited, typically between 3 and 12 hours, for example, approximately 4 hours.
[0097] Under the above-mentioned vapor deposition conditions, uniform and dispersed deposition of the silicon-based component can be obtained, and parameters such as the true density of the obtained silicon-based component can also fall within the design value range.
[0098] When calculating the mass percentages of carbon and silicon in the silicon-carbon negative electrode material, it is assumed that the material of the silicon-based component obtained by the above-mentioned silane deposition is pure silicon.
[0099] According to some embodiments of the present invention, in step S3, when the material of the shell includes carbon, the encapsulation is obtained by chemical vapor deposition using a gaseous precursor; wherein the gaseous precursor includes acetylene. At this time, the temperature of the chemical vapor deposition is 350 to 750°C. For example, it can be about 500°C, 550°C or 600°C. The deposition time is determined according to the feed amount of the gaseous precursor until the gaseous precursor reacts completely. For example, it can be 0.5 to 6 hours. More specifically, it can be about 2 hours or 3 hours. The flow rate of the gaseous precursor is 1.5 to 7.5 L / min, for example, it can be about 4 L / min.
[0100] Under the above deposition conditions, the formed carbon coating layer is more uniform, and the quality of the obtained carbon coating layer is basically consistent with the design value.
[0101] According to some embodiments of the present invention, in step S3, when the material of the shell includes carbon, the encapsulation is obtained by mixing a liquid precursor and the core and then pyrolyzing the mixture; wherein the liquid precursor includes asphalt.
[0102] According to some embodiments of the present invention, in step S3, when the shell material includes the metal oxide, the encapsulation is obtained by at least one of spray drying, ALD, wet coating, and ball milling. The wet coating includes in-situ deposition, i.e., placing the core in a dispersion comprising the shell precursor, so that the shell is deposited on the surface of the core.
[0103] According to some embodiments of the present invention, in step S3, when the material of the shell includes the organic polymer, the encapsulation is obtained by a method comprising sequentially performing liquid-phase in-situ polymerization and drying.
[0104] According to an embodiment of the third aspect of the present invention, a lithium-ion battery is provided, wherein the raw materials for preparing the lithium-ion battery include the silicon-carbon material.
[0105] Since the lithium-ion battery adopts all the technical solutions of the silicon-carbon negative electrode material of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment.
[0106] Furthermore, the lithium-ion battery also has the following beneficial effects:
[0107] (1) Because the silicon-carbon negative electrode material can significantly improve the gram-to-gram capacity without obvious volume expansion, when it is used to prepare lithium-ion batteries (taking the 4690 cylindrical battery cell, which is the mainstream of current power batteries, as an example), compared with the traditional pure graphite system, it can achieve a GED (gravimetric energy density) improvement of about 20%.
[0108] (2) Due to the structural design and parameter constraints of the silicon-carbon negative electrode material, its volume change during the charge and discharge process is significantly suppressed, and it has high structural compatibility with lithium-ion batteries. Therefore, it can be used on a large scale in lithium-ion batteries, for example, all using the silicon-carbon negative electrode material provided by the present invention as the negative electrode active material. Therefore, the lithium-ion battery provided by the present invention can achieve a significant increase in ED (energy density) due to the introduction of the silicon-carbon negative electrode material.
[0109] In general, the lithium-ion battery provided by the present invention can significantly improve energy density while maintaining cycle performance and rate performance.
[0110] According to some embodiments of the present invention, when the lithium-ion battery is a button-type battery, the number of cycles required to achieve 80% capacity decay is ≥ 665 cycles, and can reach 1105 cycles. Specifically, it can be 700 cycles, 800 cycles, 900 cycles, or 1000 cycles.
[0111] According to some embodiments of the present invention, when the lithium-ion battery is a full cell and the test temperature is approximately 25°C, the number of cycles required for the capacity to decay to 80% is ≥ 620 cycles, up to 1320 cycles. For example, the number of cycles may be approximately 800 cycles, 900 cycles, 1100 cycles, 1200 cycles, or 1300 cycles.
[0112] According to some embodiments of the present invention, when the lithium-ion battery is a full cell and the test temperature is approximately 45°C, the number of cycles required for the capacity to decay to 80% is ≥390 cycles, up to 1100 cycles, and specifically, approximately 650 cycles, 700 cycles, 800 cycles, 900 cycles, or 1000 cycles.
[0113] According to an embodiment of the fourth aspect of the present invention, there is provided an application of the lithium-ion battery in the fields of energy storage batteries, 3C batteries and power batteries.
[0114] Since the application adopts all the technical solutions of the lithium-ion battery of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment.
[0115] Unless otherwise specified, the term “about” in the present invention means that the error is allowed to be within the range of ±2%. For example, about 100 is actually 100±2%×100.
[0116] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values 2 and 3.
[0117] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0118] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the following description of the embodiments with reference to the accompanying drawings, in which:
[0119] FIG1 is a schematic diagram of the main process of the preparation method in Example 1 of the present invention. DETAILED DESCRIPTION
[0120] The following will clearly and completely describe the concept and technical effects of the present invention in conjunction with the embodiments to fully understand the purpose, features and effects of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0121] In the description of the present invention, reference to terms such as "one embodiment," "some embodiments," "illustrative embodiments," "examples," "specific examples," or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the exemplary expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.
[0122] Example 1
[0123] This embodiment prepares a silicon-carbon negative electrode material, and the specific steps are as follows:
[0124] S1. The carbon source wood powder was pyrolyzed in the precursor at 650°C in an air-tight atmosphere (nitrogen protection) for 120 min to obtain cracked carbon. After pore volume testing, it was found that the pore volume did not meet the requirements of Table 1.
[0125] S2. The cracked carbon obtained in step S1 is pore-modified with an alkali solution;
[0126] The solute in the alkali solution is sodium hydroxide with a concentration of 2 mol / L; the mass ratio of the alkali in the alkali solution to the cracked carbon obtained in step S1 is 1:10.
[0127] In this step, the temperature for pore modification is 100° C., and the pore volume test is performed every 10 minutes until the design in Table 1 is met (within 2% error), and then the pore modification is stopped.
[0128] S3. Place the porous carbon framework obtained in step S2 in a chemical vapor deposition chamber and deposit silicon at 600°C for 4 hours using SiH4 as a silicon source to obtain a core (the amount added is calculated based on the deposited amount). The amount of deposited silicon is shown in Table 1. The process of this step and the schematic diagram of the lithium removal and lithium insertion mechanism of the obtained core are shown in Figure 1.
[0129] S4. The core obtained in step S3 is further placed in a chemical vapor deposition chamber, and a gaseous hydrocarbon source (acetylene is used in this embodiment) is introduced for CVD coating (carbon deposition), wherein the hydrocarbon introduction gas flow rate is 4 L / min, the temperature is 550°C, and the deposition time is 2 h, to obtain the coated carbon mass in Table 1, that is, a silicon-carbon negative electrode material coated with a carbon shell.
[0130] In order to verify the influence of the design parameters of the silicon-carbon negative electrode material on its final physical and chemical properties and electrochemical properties, the present invention also designed Examples 2 to 9 and Comparative Examples 1 to 3.
[0131] In order to verify the influence of various parameters on the performance of the obtained silicon-carbon negative electrode material, the present invention designed Examples 2 to 9 and Comparative Examples 1 to 3. The specific differences from Example 1 are:
[0132] Example 2
[0133] In step S2, the duration of silicon deposition is increased by 2 hours in Example 2.
[0134] Example 3
[0135] In step S2, the duration of silicon deposition is increased by 3.5 hours compared with Example 1.
[0136] Example 4
[0137] In step S4, the acetylene gas flow rate is 50% of that in implementation 1-3.
[0138] Example 5
[0139] In step S4, the gas flow rate of acetylene is 2.5 times that in embodiment 1-3.
[0140] Example 6
[0141] In step S2, the temperature for pore modification is 50°C.
[0142] Example 7
[0143] In step S2, the temperature for pore modification is 175°C.
[0144] Example 8
[0145] In step S2, the concentration of the alkaline solution used for pore modification was 4 mol / L, and the overall modification time was the same.
[0146] Example 9
[0147] In step S2, the concentration of the alkaline solution used for pore modification was 1 mol / L, and the overall modification time was the same.
[0148] Comparative Example 1
[0149] Step S4 is not included.
[0150] Comparative Example 2
[0151] Step S2 is not included.
[0152] Comparative Example 3
[0153] In step S2, the duration of silicon deposition is reduced by 1 hour in Example 1.
[0154] Test Example 1
[0155] This example first tested the physical and chemical parameters of the silicon-carbon negative electrode materials obtained in Examples 1 to 9 and Comparative Examples 1 to 3. The specific method is as follows:
[0156] ρ C and ρ RD The test method for ρ is the helium specific gravity method; the test method for PV is the gas adsorption and desorption method, and the specific gases used are N2 and CO2. The adsorption and desorption curves are then integrated using the NLDFT method to obtain the test value; ρ Si The test method and ρ C The test method is similar to that of the conventional method, which uses the difference method to calculate the difference between the core loaded with silicon and the porous carbon matrix. Si The mass ratio of the carbon coating was calculated using the difference method. The mass of the deposited silicon-based component was obtained by the difference before and after step S3, and the mass of the deposited shell was obtained by the difference before and after step S4. The test results are shown in Table 1.
[0157] Table 1 Physicochemical parameters of silicon-carbon negative electrode materials in Examples 1 to 9 and Comparative Examples 1 to 3
[0158] This test example also tested the particle size of the silicon-based component in the silicon-carbon negative electrode materials obtained in Examples 1 to 9 and Comparative Examples 1 to 3. The specific test method is to use FIB-TEM for optical observation, but the particle size of the silicon-based component is generally less than 10nm. Optical observation at this scale can only obtain the difference in light and dark contrast, so it can only be obtained that the particle size of the silicon component is in the range of 2 to 10nm, and a definite numerical value cannot be obtained. However, within this scale range, the volume change of the silicon-based component during the lithium insertion and extraction process can be alleviated as much as possible. Improve the application performance of the silicon-carbon negative electrode material obtained by the present invention in lithium-ion batteries.
[0159] This example also tested the tap density of the silicon-carbon negative electrode materials obtained in Examples 1 to 9 and Comparative Examples 1 to 3. The electrochemical performance of the obtained silicon-carbon negative electrode materials in button batteries was also tested. The specific method is as follows:
[0160] The test electrode formula is: Si84% + CNTs slurry + 10% PAA-Li (lithiated PAA binder) + 5% sp; in the CNTs slurry, the solids are CNTs and CMC mixed in a mass ratio of 4:6, and the solid mass accounts for 1% of the total solid mass in the test electrode formula.
[0161] The counter electrode is a lithium metal sheet.
[0162] Battery case: 2032, and set a shrapnel, nickel foam or gasket between the test electrode or negative electrode and the battery case to avoid short circuit, which can accurately reflect the test results.
[0163] Electrolyte: 1M lithium hexafluorophosphate carbonate solution, containing FEC15% + VC1-2%.
[0164] Test electrode coating weight: ~4 mg / cm2;
[0165] Test voltage range: 2V-0.005V, or 0.8V~0.005V.
[0166] Testing process:
[0167] Let it stand for 8h-12h; let it stand for 5min at 0.05C lithium insertion to 5mV; let it stand for 5min at 50uA lithium insertion to 5mV; let it stand for 5min at 10uA lithium insertion to 5mV; let it stand for 5min at 0.05C lithium removal to 2V.
[0168] The test obtained the gram-specific capacity, first efficiency and percentage increase in thickness when fully embedded with lithium of the obtained silicon-carbon negative electrode material.
[0169] At the same time, at a charge and discharge rate of 0.33C (1C current is 1700mAh / g), the number of cycles when the gram-specific capacity decays to 90% was tested (compared with the first week at a rate of 0.33C).
[0170] The test results are shown in Table 2.
[0171] Table 2 Physical and chemical properties of silicon-carbon negative electrodes obtained in Examples 1 to 9 and Comparative Examples 1 to 3 and electrochemical properties of button batteries
[0172] Table 2 Test results description:
[0173] Examples 1-3 used the same carbon matrix (PV ~ 0.7g / cc) and deposited silicon at different contents. As the amount of silicon deposited increased, the material became denser, the fewer pores remained inside, the better the electronic and ionic conductivity, and the denser the material. As a result, its true density and tap density also increased, and in button cells, it showed a higher first efficiency. At the same time, due to the increase in the amount of silicon-based component deposited and the large lithium expansion of the silicon-based component itself, it inevitably led to a large increase in the percentage of full embedding thickness in the button cell pole piece, thereby accelerating the attenuation. The ρ of Example 1 TD The value exceeds its preferred range, which shows that the material's first efficiency is obviously low. This is because the pores inside the carbon matrix are not fully utilized, and the underutilized pores will cause the silicon-carbon negative electrode material that has been embedded with lithium to have some "dead lithium" when it is delithiated.
[0174] Taking Implementation 2 as a comparison, Examples 4, 5 and Comparative Example 1 show the difference in the effect of carbon coating on the silicon-carbon negative electrode material designed by the present invention and its performance in button batteries. The increase in the amount of carbon coating has a slight effect on the true density and tap density of the silicon-carbon negative electrode material itself, and the effect of reducing its capacity is more obvious, because the capacity of the silicon-based component is much greater than that of the deposited carbon. At the same time, the agglomeration of small particles and the reduction in the specific surface area of particles brought about by the increase in carbon coating also have a certain improvement effect on the initial effect of the silicon-carbon negative electrode material. Less carbon coating, especially the absence of carbon coating in Comparative Example 1, will have an important impact on the cycle performance of the silicon-carbon negative electrode material designed by the present invention in button batteries: in the absence of or less carbon coating, due to the sensitivity of the silicon-based component to the electrolyte, more SEI components will be formed, thereby increasing the impedance of the silicon-carbon negative electrode material during the cycle, causing the cycle to decay rapidly.
[0175] The silicon-based component in the silicon-carbon negative electrode material designed by the present invention should be mostly present in the pore volume of the porous carbon skeleton. Compared with Example 2, although the lithium insertion capacity of Examples 6, 7 and Comparative Example 2 is similar, that is, the total lithium insertion capacity provided by the silicon-based component and the porous carbon skeleton is similar, the carbon matrix PV used is 0.47g / cc, 0.92g / cc, and 0.11g / cc, respectively. Under the same silicon-based component deposition amount, Example 6 and Comparative Example 2 have insufficient pore volume (the carbon matrix PV used in Example 6 is less than the lower limit of the preferred range, and the comparative example is even reduced to 0.11g / cc, and exceeds the lower limit of the specified range), resulting in a certain amount of silicon being deposited on the outer layer of the particles, forming a pure silicon coating layer, especially in Comparative Example 2. The silicon deposition in Example 7 did not fully utilize the pores in the carbon matrix. In terms of true density and tap density, the order of Comparative Example 2>Example 6>Example 2>Example 7 is as follows. Due to the presence of the pure silicon coating layer, the initial efficiency of the silicon-carbon negative electrode material in the button battery in Comparative Example 1 will be improved. At the same time, because there is no porous carbon matrix to fully inhibit the expansion of the silicon-based components, the lithium insertion expansion of the obtained silicon-carbon negative electrode material will increase. Furthermore, due to excessive expansion, the ion and electron bridges in the electrode will be broken, and the battery cycle attenuation will be accelerated.
[0176] Compared with Example 2, Examples 8, 9, and Comparative Example 3 use carbon matrices with different strengths, and the order of strength is Example 9 > Example 2 > Example 8 > Comparative Example 3. Because the isotropic strength uniformity and graphitization degree of the porous carbon skeleton are in an opposing relationship, and a high degree of graphitization often corresponds to a porous carbon skeleton with a higher true density, and a porous carbon skeleton with a high degree of graphitization is beneficial to the first effect of the silicon-carbon negative electrode material designed by the present invention, the relationship between the true density and tap density of these four is: Comparative Example 3 > Example 9 > Example 2 > Example 8; the relationship of the first effect of the button battery is: Comparative Example 3 > Example 9 > Example 2 > Example 8. However, it should be pointed out that the high true density of the porous carbon skeleton in Comparative Example 3 is no different from that of graphite, because the true density, graphitization degree and strength of the porous carbon skeleton are mutually constrained. Because too high a true density will lead to a decrease in the isotropic strength uniformity of the porous carbon skeleton due to a higher degree of graphitization: especially Example 8 is lower than the preferred range, so it has a better expansion inhibition effect; Comparative Example 3 exceeds the upper limit of the limited range, but because of the increase in graphitization, the uniformity of the expansion inhibition effect in all directions inside the obtained silicon-carbon negative electrode material is reduced, so the relationship between expansion and circulation in the button battery is: Example 8> Example 2> Example 9> Comparative Example 3.
[0177] Test Example 2
[0178] In this test example, the silicon-carbon negative electrode material obtained in the embodiment and the comparative example and the commercial graphite material (purchased from Jiangxi Zichen Technology Co., Ltd., the raw material is artificial graphite of raw rubber) are used as the negative electrode active material (the proportion of the silicon-carbon negative electrode material in the negative electrode active material is shown in Table 3), and the 9-series ternary (purchased from Jiangmen Keheng Industrial Co., Ltd., the molar content of nickel in the transition metal is about 90%) is used as the positive electrode material, and a soft-pack battery with an NP ratio of 1.08 is designed. The obtained soft-pack battery is electrochemically tested in the voltage range of 2.5-4.2V, at a charge rate of 0.5C and a discharge rate of 1C. Specifically, the first effect of the soft-pack battery, the gram-to-gram capacity, the percentage increase in the thickness of the negative electrode sheet when fully embedded with lithium, and the number of cycles at which the capacity decays to 80% at 25°C and 45°C are tested. Some of the design parameters and results are shown in Table 3.
[0179] Table 3 Performance of silicon-carbon negative electrode materials obtained in Examples 1 to 9 and Comparative Examples 1 to 3 in soft-pack batteries
[0180] Table 3 Results Description:
[0181] For the tests numbered 1 to 3, the silicon-carbon negative electrode material obtained in Example 2 was used to prepare the negative electrode sheets according to the same negative electrode formula (96.6%). And when the negative electrode first efficiency calculated according to the NP ratio matches the positive electrode first efficiency, the silicon-carbon doping amount provided by the present invention is 10.3%, so when designing the 420mAh / g negative electrode capacity, the first efficiency of the full cell is based on the positive electrode material. When the amount of silicon-carbon negative electrode material used is further increased and the negative electrode design capacity reaches 500mAh / g and 630mAh / g, the first efficiency of the full cell is determined by the negative electrode first efficiency. At the same time, due to the increase in the amount of silicon-carbon negative electrode material used, the negative electrode lithium insertion expansion ratio increases; at the same time, it is more likely to cause the electron and ion bridges of the negative electrode sheet in the full cell to be broken during the cycle, so the cycle life decreases accordingly.
[0182] The soft-pack batteries Nos. 4-5 and 10 used the silicon-carbon negative electrode materials obtained in Examples 4, 5, and Comparative Example 1, respectively. The negative electrode active formulation was designed using the same negative electrode specific capacity as the soft-pack battery No. 2. The results showed a similar trend to the button-type battery results in Table 2. Without sufficient carbon coating, or even without the elastic coating in Comparative Example 1, the silicon-carbon negative electrode material in the full cell's negative electrode material lacked adequate protection, resulting in a large accumulation of SEI. This continuously consumed the limited active lithium ions in the positive electrode material during cycling, leading to cycle degradation.
[0183] In the soft-pack batteries of serial numbers 6 to 7 and 11, the silicon-carbon negative electrode materials used are from Examples 6, 7 and Comparative Example 2, respectively. The negative electrode specific capacity design and negative electrode active material formula of the soft-pack batteries are the same as those of the soft-pack batteries in serial number 2. The test results trend of the soft-pack full battery is similar to the test results of the button battery in Table 2: under the matching porous carbon skeleton pore volume, the volume expansion control of the silicon-carbon negative electrode material is relatively reasonable, and the volume inside the material can be fully utilized to alleviate the impact of its lithium insertion expansion on the battery cell structure and cycle performance; under the rich porous carbon skeleton pore volume, the cycle performance of the full battery cell is significantly improved, but its insufficient first effect will lead to an increase in the use of silicon-carbon negative electrode material; under insufficient, or even very small porous carbon skeleton pore volume as in Comparative Example 2, there is an obvious silicon layer in the silicon-carbon negative electrode material, and it cannot be fully protected by the carbon coating layer during the cycle, thereby causing a similar cycle accelerated attenuation phenomenon as the button battery.
[0184] In the soft-pack batteries of serial numbers 8 to 9 and 12, the silicon-carbon negative electrode materials used are respectively from Examples 8, 9 and Comparative Example 3. The negative electrode specific capacity design and negative electrode active material formula of the soft-pack batteries are the same as those of the soft-pack battery in serial number 2. The trend of the full-electric test results is similar to the trend of the button battery test results: the greater the strength of the porous carbon skeleton, the more it can restrain the lithium insertion expansion of the silicon-based components in the silicon-carbon negative electrode material. However, due to the contradiction between the strength of the porous carbon skeleton and the degree of graphitization, the increase in the strength of the porous carbon skeleton will cause the first efficiency of the silicon-carbon negative electrode material to tend to decrease. As shown in the silicon-carbon negative electrode material obtained in Comparative Example 3, although its porous carbon skeleton can significantly inhibit the lithium insertion expansion of the silicon-carbon negative electrode material and ensure the cycle performance, its low first efficiency leads to a significant increase in the use of silicon-carbon negative electrode materials under the same negative electrode specific capacity design, resulting in an increase in the BoM cost of battery cell production.
[0185] In summary, the silicon-carbon anode material provided by this invention, through structural design and parameter constraints, can improve comprehensive performance, including cycle performance, safety performance (volume change), and initial efficiency, while maintaining minimal volume expansion. It is expected to be widely used in the fields of energy storage batteries, 3C batteries, and power batteries.
[0186] While the embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to the embodiments described above. Various modifications may be made within the scope of knowledge possessed by a person skilled in the art without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof may be combined with one another unless there is a conflict.
Claims
1. A silicon-carbon negative electrode material, characterized in that: The silicon-carbon negative electrode material comprises a core and a shell wrapped around the surface of the core; the true density of the silicon-carbon negative electrode material is p RD ; The core includes a porous carbon skeleton and a silicon-based component dispersed in the porous carbon skeleton; the pore volume of the porous carbon skeleton is PV, and the true density is ρ C ; The true density of the silicon-based component is ρ Si ; And satisfy formula (I): Where: 1.5g / cc≤ρ RD ≤2.4g / cc; 0.45cc / g≤PV≤1.55cc / g; 1g / cc≤ρ Si ≤2.35g / cc; 1.2g / cc≤ρ C ≤2.28g / cc.
2. The silicon-carbon negative electrode material according to claim 1, characterized in that: In formula (I), ρ RD is 1.75 to 2.25 g / cc; preferably, in formula (I), PV is 0.55 to 0.95 cc / g; preferably, in formula (I), ρ Si is 1.25 to 1.75 g / cc; preferably, ρ C It is 1.5~2.2g / cc.
3. The silicon-carbon negative electrode material according to claim 1, characterized in that: The mass percentage of the silicon-based component in the silicon-carbon negative electrode material is W Si , the lithium insertion capacity of the silicon-carbon negative electrode material is CAP; and satisfies formula (II); 180≤CAP-3769×W Si ≤680 Formula (II); Among them, 30% ≤ W Si ≤60%.
4. The silicon-carbon negative electrode material according to any one of claims 1 to 3, characterized in that: The particle size D of the silicon-based component Si Range: 2nm≤D Si ≤10nm; Preferably, the tap density of the silicon-carbon negative electrode material is TD The range is: 0.8g / cc≤ρ TD ≤1.2g / cc.
5. The silicon-carbon negative electrode material according to any one of claims 1 to 3, characterized in that: In the silicon-carbon negative electrode material, the sum of the mass percentages of silicon and carbon is greater than 98%.
6. The silicon-carbon negative electrode material according to any one of claims 1 to 3, characterized in that: The material of the shell includes at least one of carbon, metal oxide and organic polymer.
7. A method for preparing a silicon-carbon negative electrode material, characterized in that: The preparation method comprises the following steps: S1. cracking carbon raw materials to obtain porous carbon skeleton; S2. Depositing the silicon-based component in the porous carbon skeleton to obtain a core; S3. Wrap the substance obtained in step S2 to form a shell.
8. The preparation method according to claim 7, characterized in that: In step S1, the process further comprises performing pore modification on the pyrolysis product after the pyrolysis; preferably, in step S2, the deposition method comprises chemical vapor deposition.
9. A lithium ion battery, characterized in that: The raw material for preparing the lithium-ion battery includes the silicon-carbon negative electrode material as described in any one of claims 1 to 6 or the silicon-carbon negative electrode material prepared by the preparation method as described in claim 7 or claim 8.
10. Application of the lithium-ion battery according to claim 9 in the fields of energy storage batteries, 3C batteries and power batteries.
Citation Information
Patent Citations
Silicon-carbon composite anode material and preparing method thereof
CN102509781A
Silicon-carbon negative electrode material and preparation method and application thereof
CN115863600A
Negative electrode material, negative electrode plate and battery
CN116053447A
Silicon-carbon negative electrode material and preparation method and application thereof
CN116598452A
Silicon-based carbon composite, preparation method therefor, and anode active material comprising same
WO2021246544A1
Cited By
Porous silicon carbon negative electrode material and preparation method and application thereof
CN119797367A