Separator, secondary battery, and electric device
By using nanocellulose and separator design that controls the through-hole structure, the problem of insufficient heat resistance of lithium-ion battery separators is solved, and high thermal stability and safety performance are improved.
Patent Information
- Application Number
- PCT/CN2023/141609
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2023-12-25
- Publication Date
- 2024-11-21
AI Technical Summary
The existing lithium-ion battery separators have poor heat resistance and are prone to shrink at high temperatures, resulting in safety hazards and unstable battery performance.
Nanocellulose is used as the base film material to control the porosity and through-pore structure to ensure that the membrane maintains stability at high temperatures, and the wetting and ionic conductivity of the electrolyte is improved through oxygen-containing functional groups.
The high thermal stability of the diaphragm is achieved, the risk of contact short circuit of positive and negative electrodes is reduced, and the safety performance and cycle life of the battery are improved.
Smart Images

Figure CN2023141609_21112024_PF_FP_ABST
Abstract
Description
A diaphragm, secondary battery and electrical equipment
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on May 18, 2023, with application number 202310565790.7 and invention name “A diaphragm, a secondary battery and an electrical device”. The entire contents of the Chinese patent application are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of battery technology, and more specifically, to a separator, a secondary battery including the separator, and an electrical device. Background Art
[0004] The diaphragm is one of the important components in the battery. It has the function of isolating the positive and negative electrodes and allowing ions to pass through. Therefore, the performance of the battery diaphragm determines the safety performance of the battery to a certain extent.
[0005] Currently, polyolefin dry- and wet-process membranes are the most widely used lithium-ion battery separators on the market, offering significant advantages in manufacturing process and cost. However, the growing demand for higher energy density and safety has limited the application of polyolefin-based separators in advanced lithium-ion batteries. This is because, on the one hand, the hydrophobic nature of polyolefins results in a low affinity for carbonate electrolytes. On the other hand, polyolefin membranes (such as PP and PE) shrink dramatically when heated due to their low melting points and glass transition temperatures, which can easily cause short circuits between the positive and negative electrodes and lead to safety accidents. Furthermore, the macroporous polyolefin skeleton cannot ensure uniform deposition of lithium ions on the anode surface, resulting in the uncontrolled growth of dendritic lithium.
[0006] Currently commercialized ceramic separators still suffer from poor heat resistance. They shrink significantly at relatively high temperatures, failing to effectively improve battery cell safety. Furthermore, baking the wound battery cells to remove moisture is a common process in battery cell manufacturing, and significant thermal shrinkage can also affect the consistency of cell production. Therefore, separators with high heat resistance are crucial to battery performance.
[0007] Therefore, it is necessary to provide a separator with higher thermal stability.
[0008] Summary of the Invention
[0009] In view of the defect of poor heat resistance of battery separators in the prior art, the purpose of this application is to provide a separator with higher thermal stability.
[0010] According to the first aspect of the present application, a diaphragm is provided, which includes a base membrane, and the base membrane includes nanocellulose. The diaphragm is heated from an initial temperature T0 to T1 at a heating rate of 5 to 10°C / min, and the porosity P of the diaphragm satisfies: (P0-P1) / P0≤5%; wherein, 30°C≤T1-T0≤60°C, 80°C≤T0≤100°C, P0 is the porosity of the diaphragm at T0, and P1 is the porosity of the diaphragm at T1.
[0011] Optionally, the diaphragm has a plurality of through-hole structures, and the through-hole structure distribution satisfies: the through-holes with a pore diameter of 40-60 nm account for 40-70%, the through-holes with a pore diameter less than 40 nm account for 10-30%, and the through-holes with a pore diameter greater than 60 nm account for 5-35%.
[0012] Optionally, the fiber diameter of the nanocellulose is 10 to 500 nm.
[0013] Optionally, the base film has a thickness of 9 to 30 μm.
[0014] Optionally, the surface of the nanocellulose includes oxygen-containing functional groups, and the oxygen-containing functional groups include at least one of aldehyde groups, ketone groups, and carboxylic acid groups.
[0015] Optionally, the separator has a longitudinal shrinkage MD of ≤0.4% and a transverse shrinkage TD of ≤0.1% at 120° C. for 2 hours.
[0016] Optionally, the elastic modulus of the diaphragm is 60 to 95 GPa.
[0017] Optionally, the longitudinal tensile strength of the diaphragm is ≥200 MPa, and the transverse tensile strength of the diaphragm is ≥250 MPa.
[0018] According to a second aspect of the present application, a secondary battery is provided, comprising the separator according to the first aspect of the present application.
[0019] According to a third aspect of the present application, an electric device is provided, wherein the electric device comprises the secondary battery according to the second aspect of the present application, and the secondary battery provides electric energy for the electric device.
[0020] The technical solution adopted in this application can achieve the following beneficial effects:
[0021] The diaphragm provided in the present application has high thermal stability and is not prone to shrinkage and deformation when heated, thereby improving the safety performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0023] FIG1 is a flow chart of the preparation of a diaphragm according to Example 12 of the present application. DETAILED DESCRIPTION
[0024] To make the purpose, technical solutions, and advantages of this application more clear, the technical solutions of this application will be clearly and completely described below in conjunction with the specific embodiments of this application and the corresponding drawings. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0025] According to one embodiment of the present application, a membrane is provided, which includes a base membrane, which includes nanocellulose, and when the membrane is heated from an initial temperature T0 to a temperature T1 at a heating rate of 5 to 10°C / min, the porosity P of the membrane satisfies the following conditions: (P0-P1) / P0≤5%; wherein, 30°C≤T1-T0≤60°C, 80°C≤T0≤100°C, P0 is the porosity of the membrane at T0, and P1 is the porosity of the membrane at T1. For example, the initial temperature T0 can be 90°C, 85°C, 90°C, 95°C, 100°C, or any temperature value between the above temperature values; the temperature difference between T1 and T0 can be 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, or any value between the above values. Higher temperatures will destroy the diaphragm structure to a certain extent and shrink the pores of the diaphragm. However, the diaphragm provided by the present application remains basically unchanged or changes very little after the initial temperature (80-100°C) is increased by 30-60°C at a specific heating rate. For example, when the diaphragm provided by the present application is heated from 90°C to 150°C, the porosity of the diaphragm changes by less than 5%, indicating that the diaphragm provided by the present application is resistant to high temperatures and will not shrink severely at high temperatures. It can maintain its mechanical integrity even at high temperatures and has high thermal stability. This higher thermal stability is due to the fine nanostructure of nanocellulose, which forms a relatively dense network structure with each other. At the same time, its good mechanical properties can keep the pore structure basically unchanged at high temperatures.
[0026] The fiber diameter of the nanocellulose can be in the range of 10 to 500 nm. The thickness of the base film can be 9 to 30 μm, for example, 9, 10, 12, 14, 16, 18, 20, 22, 24, 25, 26, 28, 30 μm or any value between the above values. Cellulose is directly extracted from plants and has the advantages of biodegradability, good heat resistance and sustainable development. Therefore, it can be used as a favorable candidate for lithium-ion battery separators. And thanks to the polymerized glucose units in cellulose, there is a high affinity between the cellulose skeleton and the electrolyte. More importantly, the diameter of cellulose can be adjusted from micrometer to nanometer scale by physical or chemical methods. The nanocellulose of the above-mentioned specific size selected in this application has a nanometer-scale diameter and high crystallinity, which can provide significant mechanical properties and thermal stability.
[0027] In this embodiment, the diaphragm has a through-pore structure, and the through-pore structure has a relatively uniform pore size distribution. For example, the distribution of the through-pore structure satisfies: through-pores with a pore size of 40 to 60 nm account for 40 to 70%, through-pores with a pore size less than 40 nm account for 10 to 30%, and through-pores with a pore size greater than 60 nm account for 5 to 35%. Preferably, through-pores with a pore size within 20 to 40 nm but not including 40 nm account for 10 to 30%, and through-pores with a pore size within 60 to 140 nm but not including 60 nm account for 5 to 35%. The through-pore structure can build a bridge for the rapid migration of ions (for example, lithium ions) in the electrolyte, allowing the ions to migrate in the through-pore structure, so that the formed battery diaphragm has a higher ionic conductivity. A suitable through-pore structure allows electrolyte ions (e.g., lithium ions) to pass freely and more smoothly, forming a charge-discharge circuit. This effectively prevents accelerating the battery's self-discharge process and reducing battery consistency. Furthermore, a suitable pore size distribution reduces electrolyte infiltration time and improves the membrane's wettability. Therefore, the membrane provided herein with the aforementioned through-pore size distribution can achieve excellent ionic conductivity and wettability.
[0028] In one embodiment of the present application, the liquid absorption rate of the diaphragm is 152% to 216%, for example, it can be 152%, 160%, 186%, 190%, 200%, 211%, 216% or the range of both of the above. In another embodiment of the present application, the liquid retention capacity of the diaphragm is 12g to 21.1g, for example, it can be 12g, 13g, 15g, 18g, 20g, 21.1g or the range of both of the above. Wherein the liquid retention capacity means the liquid per 25cm 2 The maximum mass of electrolyte that a diaphragm can absorb. The liquid absorption rate and liquid retention rate of a diaphragm can both reflect the diaphragm's wettability. The liquid absorption rate and liquid retention of the diaphragm of the present application are within the above ranges, indicating that the diaphragm of the present application has excellent wettability. Its application in batteries can improve the battery's dynamic performance.
[0029] In one embodiment of the present application, the ionic conductivity of the diaphragm is 1.0 to 1.4 mS / cm, for example, it can be 1.0 mS / cm, 1.05 mS / cm, 1.12 mS / cm, 1.2 mS / cm, 1.28 mS / cm, 1.3 mS / cm, 1.35 mS / cm, 1.4 mS / cm or a range of two of the above. When the ionic conductivity of the diaphragm is within the above range, the lithium ions in the electrolyte can shuttle smoothly in the diaphragm, and have better lithium ion transmission efficiency.
[0030] The provided diaphragm may have a porosity of 30% to 80% at room temperature (25±5°C). In other embodiments, the diaphragm may have a porosity in the range of 30%, 40%, 55%, 60%, 80%, or any two of these at room temperature. A porosity within the above range can impart a high liquid absorption rate to the diaphragm, forming a good interface structure between the diaphragm and the positive and negative electrodes, thereby improving the cycle life of the battery. It can also enhance the wettability of the diaphragm to the electrolyte, thereby improving the air permeability and ionic conductivity of the diaphragm.
[0031] The surface of the nanocellulose may include oxygen-containing functional groups, which may include at least one of aldehyde, ketone, and carboxylic acid. These oxygen-containing functional groups can form complexes with certain groups in the organic electrolyte, resulting in a carbonaceous oxide composite material through a one-step carbonization process, thereby improving the wettability of the separator with the electrolyte. The presence of these oxygen-containing functional groups can thus enhance the ionic conductivity and permeability of the separator.
[0032] The separator provided in the present application has a low thermal shrinkage rate. Specifically, the longitudinal shrinkage rate MD of the separator at 120° C. for 2 hours is ≤0.4%, and the transverse shrinkage rate TD is ≤0.1%.
[0033] The diaphragm provided in the present application has excellent mechanical strength, wherein the elastic modulus of the diaphragm (the stress under the unidirectional stress state divided by the strain in that direction, that is, the elastic modulus) can be in the range of 60 to 95 GPa; the longitudinal tensile strength of the diaphragm can be ≥200 MPa, and the transverse tensile strength of the diaphragm can be ≥250 MPa.
[0034] The diaphragm provided in the above implementation scheme has excellent resistance to heat shrinkage, good wettability to electrolyte and high liquid absorption rate, which can effectively prevent short-circuit accidents caused by contact between positive and negative electrodes due to heat shrinkage of the diaphragm; the high liquid absorption rate can form a good interface structure between the diaphragm and the positive and negative electrodes, thereby improving the cycle life of the battery.
[0035] According to another embodiment of the present application, there is provided a method for preparing the above-mentioned diaphragm, comprising:
[0036] a) homogenizing the cellulose slurry in sequence to obtain a nanocellulose suspension;
[0037] b) adding microspheres to the nanocellulose suspension to prepare a uniform mixed solution containing the microspheres, and transferring the mixed solution to a mold to prepare an intermediate film;
[0038] c) placing the intermediate film in an organic solvent to dissolve the microspheres, and drying to obtain the above-mentioned separator.
[0039] In the membrane preparation step, the specific parameters are as follows:
[0040] In step a), the solid content of the cellulose pulp can be 5-20%. Before the cellulose pulp is homogenized, the cellulose pulp can be ground, and the grinding can be performed using a PFI pulper at a speed of 1500-30000 rpm; preferably, after the cellulose pulp is ground, the ground cellulose pulp can also be oxidized. Specifically, the oxidation of the cellulose pulp includes: adding an oxidant to the cellulose pulp, wherein the oxidant can be selected from a combination of one or more of 2,2,6,6-tetramethylpiperidin-1-oxyl free radical oxidation system, sodium bromate, nitric acid, phosphoric acid and hypochlorous acid; the concentration (solid content) of the nanocellulose suspension finally obtained in this step is 1 -10%; wherein, in this step, the purpose of oxidation is that: cellulose is mainly composed of polysaccharide polymerization, and polysaccharides contain multiple hydroxyl groups, which will form hydrogen bonds between hydroxyl groups. The more hydrogen bonds formed, the greater the binding force between cellulose molecules. The above-mentioned oxidation treatment can oxidize the hydroxyl groups in cellulose glucose into carboxyl groups, aldehyde groups or ketone groups, which can weaken the intermolecular forces and facilitate subsequent treatments, such as the embedding and de-embedding of monodisperse colloids. At the same time, as mentioned above, oxygen-containing functional groups such as aldehyde groups, ketone groups, and carboxylic acids can be complexed with some groups in the organic electrolyte, which can obtain a carbonaceous oxide composite material through one-step carbonization, thereby improving the wettability of the electrolyte to the diaphragm.
[0041] In this step, the homogenization process is performed using a homogenizer.
[0042] The microspheres in step b) can be made of low-heat-resistant polymers so that the micropores can be selectively dissolved at a lower temperature in step c) to form a diaphragm with a through-pore structure. By using low-heat-resistant polymers as a means of pore formation, the controllable porosity of the diaphragm can be achieved.
[0043] Specifically, the microspheres in step b) can be monodisperse polystyrene (PS) colloids, and the particle size of the PS spheres is 40 to 200 nm. By adjusting the size and number of the polystyrene spheres, the pore size and porosity of the through-pore structure of the final diaphragm can be adjusted; the monodisperse colloid and the nanocellulose suspension can be mixed according to a mass ratio of the monodisperse polystyrene (PS) colloid to the nanocellulose solids in the nanocellulose suspension of 1:9 to 3:2.
[0044] Preferably, before transferring the uniform mixed liquid containing the microspheres into the mold, a step of sucking the uniform mixed liquid can be included, wherein the purpose of sucking the uniform mixed liquid is to remove bubbles in the mixed liquid. For example, vacuum suction can be performed for 30 minutes to remove bubbles in the mixed liquid, and the intermediate film can be formed by casting the uniform mixed liquid after degassing into a glass mold, solidifying, dehydrating, and drying.
[0045] Wherein, dehydration and drying can be implemented in the following manner:
[0046] The solidified sample is transferred to an ethanol bath for dehydration for 12 hours to obtain a mechanically stable gel. The gel is then baked in an oven for a certain period of time, for example, at 40-60°C for 4-8 hours to produce a dry film as an intermediate membrane. In this step, dehydration with an organic solvent and oven drying after dehydration can make the polystyrene balls more tightly bound to the cellulose molecules, which is conducive to the formation of a porosity-controlled diaphragm by dissolving the polystyrene balls in the subsequent step. Here, it is worth mentioning that the ethanol bath can also alleviate the capillary action between the cellulose fibers during the drying process, thereby forming a loose cellulose network and promoting the migration of electrolyte ions.
[0047] The organic solvent in step c) can be selected from at least one of toluene and xylene. Those skilled in the art will appreciate that any organic solvent can be selected as long as it selectively dissolves the microspheres without dissolving the separator. The low-heat-resistant polymer styrene microspheres, because they are soluble in organic solvents, can form a through-pore structure of a certain size in the separator.
[0048] Specifically, in step c), the intermediate film obtained in step b) can be immersed in a toluene bath at room temperature to dissolve the polystyrene balls embedded in the nanocellulose network. Finally, the membrane sample is dried at 40-60°C and then taken out. It is worth mentioning that the present application uses monodispersed polystyrene (PS) balls, mainly due to the following factors: (1) PS balls can be evenly dispersed in water and can be evenly embedded in the nanocellulose host after stirring. (2) PS balls can quickly dissolve in toluene or xylene, leaving a large number of micropores in the cellulose network, thereby obtaining a higher porosity, improving the liquid absorption and retention performance of the diaphragm, and effectively improving the perfection of the interface between the diaphragm and the positive and negative electrodes in the battery, thereby improving the cycle life of the battery.
[0049] Therefore, the present application provides a diaphragm with adjustable pore size and porosity prepared with nanocellulose as the main body through pore engineering. The diaphragm has great mechanical strength and can withstand the puncture of lithium dendrites and external impact, thereby improving the safety performance of the battery. The uniform pores obtained are mostly nanopores, which are conducive to the uniform evolution of the electrode-electrolyte interface, increase the speed and amount of electrolyte absorption by the diaphragm, thereby enhancing the wettability of the diaphragm to the electrolyte, and improving the air permeability and ionic conductivity of the diaphragm.
[0050] According to another embodiment of the present application, a secondary battery is provided, comprising the aforementioned separator. The separator provided herein has high mechanical strength, capable of withstanding penetration by lithium dendrites and external impacts, and high thermal stability, making it less susceptible to shrinkage and deformation when heated, thereby improving the safety performance of the separator and, in turn, the service life and safety performance of the secondary battery.
[0051] Specifically, the secondary battery may be a lithium-ion battery.
[0052] The following describes the method with reference to specific embodiments.
[0053] Example 1:
[0054] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0055] (a) Using softwood fiber as the raw material, 200.0 g of softwood cellulose pulp, with a cellulose solids content of 10%, was refined using a PFI refiner at 30,000 rpm until the cellulose pulp was visibly crushed. 500.0 g of deionized water was then added and magnetically stirred for 30 minutes to dilute the cellulose pulp to a 1% suspension. The suspension was passed through a homogenizer 12 times to obtain a viscous nanocellulose suspension with a solids content of 1%. Finally, the concentration of the nanocellulose suspension was increased from 1% to 2% by rotary evaporation.
[0056] (b) 30.0 g of monodisperse polystyrene (PS) colloids with diameters ranging from 40 to 200 nm were uniformly mixed with the prepared nanocellulose suspension at a mass ratio of 3:2 (PS monodisperse to nanocellulose solids in the nanocellulose suspension). The mixture was stirred for 1 hour to obtain a uniform dispersion. After vacuum extraction for 30 minutes to remove air bubbles, the dispersion was uniformly cast into a glass mold. The sample was then transferred to an ethanol bath for dehydration for 12 hours to obtain a mechanically stable gel. The gel was then baked in a 50°C oven for 5 hours to produce a dry film that served as the intermediate film.
[0057] (c) The resulting membrane sample was then immersed in a toluene bath for 5 h to dissolve the PS spheres embedded in the nanocellulose network. Finally, the membrane sample was dried in a 50°C oven for 12 h and then removed to obtain a separator.
[0058] Example 2:
[0059] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0060] The preparation method of the diaphragm is the same as that in Example 1, except that in step b), the mass ratio of the polystyrene (PS) monodisperse colloid to the nanocellulose solid in the nanocellulose suspension is 5:5.
[0061] Example 3:
[0062] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0063] The method for preparing the diaphragm is the same as that in Example 1, except that in step b), the mass ratio of the polystyrene (PS) monodisperse colloid to the nanocellulose solid in the nanocellulose suspension is 4.5:5.5.
[0064] Example 4:
[0065] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0066] The method for preparing the diaphragm is the same as that in Example 1, except that in step b), the mass ratio of the polystyrene (PS) monodisperse colloid to the nanocellulose solid in the nanocellulose suspension is 1:9.
[0067] Example 5:
[0068] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0069] The method for preparing the diaphragm is the same as that in Example 1, except that in step b), the mass ratio of the polystyrene (PS) monodisperse colloid to the nanocellulose solid in the nanocellulose suspension is 1:12.
[0070] Example 6:
[0071] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0072] The method for preparing the diaphragm is the same as that in Example 1, except that in step b), the mass ratio of the polystyrene (PS) monodisperse colloid to the nanocellulose solid in the nanocellulose suspension is 4:2.
[0073] Example 7:
[0074] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0075] The method for preparing the diaphragm is the same as that in Example 1, except that in step b), the PFI refiner is used for refining at a rotation speed of 25,000 rpm.
[0076] Example 8:
[0077] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0078] The method for preparing the diaphragm is the same as that in Example 1, except that in step b), the PFI refiner is used for refining at a rotation speed of 20,000 rpm.
[0079] Example 9:
[0080] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0081] The method for preparing the diaphragm is the same as that in Example 1, except that in step b), the PFI refiner is used for refining at a rotation speed of 15,000 rpm.
[0082] Example 10:
[0083] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0084] The method for preparing the diaphragm is the same as that in Example 1, except that in step b), the PFI refiner is used for refining at a rotation speed of 10,000 rpm.
[0085] Example 11:
[0086] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0087] The method for preparing the diaphragm is the same as that in Example 1, except that in step b), the PFI refiner is used for refining at a rotation speed of 5000 rpm.
[0088] Example 12:
[0089] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0090] The diaphragm preparation method is the same as that in Example 1, except that: in step a), after the cellulose pulp is refined with a PFI refiner, 10.0 g of TEMPO oxidant with a NaClO concentration of 10 mmol / g is used to pretreat the cellulose pulp to obtain TEMPO oxidized pulp, and then 500.0 g of deionized water is added and magnetically stirred for 30 minutes to dilute the oxidized pulp to a 1% suspension. The specific preparation method is shown in Figure 1.
[0091] Example 13:
[0092] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0093] The method for preparing the diaphragm is the same as that in Example 12, except that in step a), the concentration of NaClO in the TEMPO oxidant is 8 mmol / g.
[0094] Example 14:
[0095] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0096] The method for preparing the diaphragm is the same as that in Example 12, except that in step a), the concentration of NaClO in the TEMPO oxidant is 6 mmol / g.
[0097] Example 15:
[0098] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0099] The method for preparing the diaphragm is the same as that in Example 12, except that in step a), the concentration of NaClO in the TEMPO oxidant is 4 mmol / g.
[0100] Example 16:
[0101] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0102] The method for preparing the diaphragm is the same as that in Example 12, except that in step a), the concentration of NaClO in the TEMPO oxidant is 2 mmol / g.
[0103] Example 17:
[0104] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0105] The method for preparing the diaphragm is the same as that in Example 12, except that in step a), the concentration of NaClO in the TEMPO oxidant is 1 mmol / g.
[0106] Example 18:
[0107] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0108] The method for preparing the diaphragm is the same as that in Example 12, except that in step a), the oxidant is sodium bromate.
[0109] Example 19:
[0110] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0111] The method for preparing the diaphragm is the same as that in Example 12, except that in step a), the oxidant is nitric acid.
[0112] Example 20:
[0113] A diaphragm is provided, and the preparation process of the diaphragm is as follows:
[0114] The method for preparing the diaphragm is the same as that in Example 12, except that in step a), the oxidant is phosphoric acid.
[0115] Comparative Example 1
[0116] The nanocellulose suspension prepared using the process described in Example 1 was passed through a homogenizer 12 times to obtain a viscous nanocellulose suspension with a solids content of 1%. Finally, the concentration of the nanocellulose suspension was increased from 1% to 2% using rotary evaporation. After vacuuming for 30 minutes to remove air bubbles, the suspension was uniformly cast into a glass mold. The sample was then transferred to an ethanol bath for dehydration for 12 hours to obtain a mechanically stable gel. The gel was then stored in an oven at 50°C for 12 hours before removal to produce a separator.
[0117] Comparative Example 2
[0118] The polypropylene separator was purchased from Shenzhen ZTE New Materials Technology Co., Ltd. and had a thickness of 25 μm.
[0119] Comparative Example 3
[0120] The polyethylene separator was purchased from Shenzhen ZTE New Materials Technology Co., Ltd. and had a thickness of 25 μm.
[0121] Performance testing:
[0122] 1) Porosity determination
[0123] After recording the initial mass Wm of the diaphragms in each embodiment and comparative example, soak them in n-butanol for 1 hour, remove them, remove the surface liquid with filter paper, and weigh the mass Ws. The porosity ε is: ε=[(Ws-Wb) / ρb] / [(Ws-Wb) / ρb+Wm / ρm]
[0124] Wm and Ws are the weights of the dry film and the film after immersion in n-butanol for 1 hour, respectively; Wb is the original mass of n-butanol. ρb and ρm are the densities of n-butanol and the dry film, respectively. The room temperature measurement results are shown in Table 1.
[0125] 2) Thermal stability
[0126] In order to further test the thermal stability of the diaphragm, the porosity changes of the diaphragms of each embodiment and comparative example at high temperature were also measured. The specific measurement method is:
[0127] The diaphragm is heated to a set temperature, then cooled to room temperature, and the porosity at each temperature is measured using the same method as above. Wherein, the initial temperature T0 can be set to 90°C, and the porosity of the diaphragm at T0 is defined as P0. The diaphragm is then heated at a heating rate of 5 to 10°C / min. After heating to T1 (30°C ≤ T1-T0 ≤ 60°C), the porosity P1 of the diaphragm is measured. Wherein, T1 is taken as 120°C, 135°C and 150°C respectively. The porosity measurement results of the diaphragms of each embodiment and comparative example at high temperature are shown in Table 1.
[0128] 3) Pore size distribution
[0129] The following method was used to measure the through-hole size and through-hole distribution of each embodiment and comparative example:
[0130] ① Use liquid to completely wet and fill the through-hole of the diaphragm to be tested. Due to the capillary phenomenon, positive pressure is formed in the hole.
[0131] ② Place the diaphragm in a closed groove and use gas pressure to squeeze the liquid out of the capillary holes.
[0132] ③ Based on the relative relationship between the pressure applied when the liquid in a single through-hole is completely squeezed out of the capillary pore and the through-hole diameter, the diaphragm pore diameter can be calculated using the Laplace equation. The Laplace equation is as follows: d = -(4yCosθ / p) x 100%, where d is the through-hole diameter, P is the pressure, γ is the liquid surface tension, and θ is the contact angle between the diaphragm and the liquid. At different pressures, the liquid in the diaphragm is gradually squeezed out, generating a certain amount of gas flow through. The relationship between pressure and flow can be used to calculate the pore size and pore size distribution. The results are shown in Table 1.
[0133] 4) Cellulose diameter
[0134] The nanocellulose diameter of the separators in each example and comparative example was measured. The specific method was to spray-coat the separator sample with gold for 100 seconds, and then confirm its cross-sectional morphology using a scanning electron microscope. A negative staining method was used, and the nanocellulose suspension was diluted to obtain a high-resolution transmission electron micrograph of the nanofiber morphology. The results are shown in Table 2.
[0135] 5) Heat shrinkage
[0136] The thermal shrinkage performance of the diaphragms in the examples and comparative examples was tested using an electric constant temperature blast drying oven. The specific testing method is as follows:
[0137] Fold the membranes into three stacks, flatten them, and expel the air between the membranes. Remove the cutting board (140*70mm), cut out the membrane samples, and measure the membrane length A1 and width B1. Set the oven temperature to 100°C. Once the temperature stabilizes at 100°C, place the samples in the oven and keep them warm for 2 hours. Use a stopwatch or the oven's built-in timer to time the time. After 2 hours, remove the membranes, let them cool for 10 minutes, and then measure the sample length A2 and width B2.
[0138] Diaphragm longitudinal thermal shrinkage = (A1-A2) / A1*100%
[0139] Transverse thermal shrinkage of the diaphragm = (B1-B2) / B1*100%
[0140] The longitudinal and transverse thermal shrinkages of the diaphragm at 100°C for 2 hours were calculated according to the above formulas.
[0141] The above method was repeated, with the oven temperature set to 120°C and 190°C, respectively. The longitudinal and transverse thermal shrinkages were measured at 120°C and 190°C for 2 hours, respectively. The test results are shown in Table 2.
[0142] 6) Liquid absorption rate and liquid retention
[0143] Specific testing method: Cut the separators in each embodiment and comparative example into 5cm×5cm samples, weigh W1, then place the samples in electrolyte, leave them at room temperature for 10 minutes, remove them, and use filter paper to absorb the electrolyte on the separator surface. Weigh W2, and the liquid absorption rate = (W2-W1) / W1*100%. Repeat 5 times and take the average value. The electrolyte is a solution of LiPF6 with a concentration of 1 mol / L, and the solvent composition of the solution is dimethyl carbonate DMC:ethylene carbonate EC:ethyl methyl carbonate EMC = 1:1:1 by volume.
[0144] Liquid retention capacity test method: Cut the diaphragm into 5cm×5cm samples, weigh W1, then place the sample in the electrolyte and weigh it every 1 hour. When the weight remains unchanged, record it as Wt. Liquid retention capacity = Wt-W1.
[0145] The test results of the membrane liquid absorption rate and battery liquid filling and retention capacity in each embodiment and comparative example are shown in Table 3.
[0146] 7) Mechanical properties
[0147] The tensile strength and elastic modulus of the diaphragm are tested as follows:
[0148] Use a thickness gauge to measure the thickness of the separator, recording it as A (see Table 2 for thickness data for each separator). Fold the separator and place it between A4 sheets of paper. Place this on a cutting board and cut into 15mm wide strips along the separator's winding direction. Mark lines at 10cm intervals on the cut separator strips. Then clamp the separator to the universal tester and enter the parameters A, width (15mm), and gauge length (100mm) before starting the measurement. When the separator is broken, the longitudinal tensile strength, longitudinal elongation, and longitudinal elastic modulus are displayed. The test results are shown in Table 3.
[0149] Use a thickness gauge to measure the thickness of the separator, recording it as A. Fold the separator and place it between A4 sheets of paper. Place this on a cutting board and cut it into 15mm wide strips perpendicular to the separator's winding direction. Mark lines at 10cm intervals on the cut separator strips. Then clamp the separator to the universal tester and enter parameters such as A, width (15mm), and gauge length (100mm). The measurement begins. When the separator is broken, the transverse tensile strength, transverse elongation, and transverse elastic modulus are displayed. The test results are shown in Table 3.
[0150] 8) Ionic conductivity
[0151] Symmetrical batteries were fabricated and the electrochemical impedance spectroscopy (EIS) of the battery samples was tested using an electrochemical workstation with a frequency of 0.1 MHz to 0.1 Hz and an amplitude of 10 mV. The specific formula is:
[0152] σ=L / AR;
[0153] L (cm) is the thickness of the diaphragm, A (cm 2 ) is the area of the stainless steel electrode, and R is the resistance obtained from the curve. The test results are shown in Table 4.
[0154] 9) Test the short circuit performance and cycle performance of lithium-ion batteries.
[0155] According to the above battery preparation method, the separators prepared in Examples 1-20 and Comparative Examples 1-3 were further assembled into batteries. The short-circuit performance and cycling performance of the batteries were then tested using a battery testing system. The short-circuit performance test procedure was as follows: the battery was fully charged to 4.3V and placed in an environment at 20±5°C. When the battery surface temperature reached 20±5°C, it was allowed to stand for 30 minutes. A 3mΩ internal resistance wire was used to short-circuit the positive and negative electrodes of the battery for 10 minutes. After the test, the battery surface temperature was measured and observed at ambient temperature for 1 hour to see if any explosion or fire occurred. The cycling performance test procedure was as follows: at 25°C, the battery was allowed to stand for 5 minutes, then charged at a constant current rate of 1C to 4.1V, then charged at a constant voltage to a current of less than or equal to 0.05C, then allowed to stand for 5 minutes, and then discharged at a constant current rate of 1C to 2.8V. This constituted one charge-discharge cycle, and the discharge capacity of this cycle was recorded as the discharge capacity of the lithium-ion secondary battery in the first cycle. The lithium ion secondary battery was charged and discharged for 900 cycles according to the above method, and the discharge capacity at 900 cycles was recorded. The capacity retention rate (%) = discharge capacity at the 900th cycle / discharge capacity at the first cycle × 100%.
[0156] The test results are shown in Table 4. The assembly process of the lithium-ion battery is as follows:
[0157] a. Preparation of negative electrode sheets for lithium-ion batteries
[0158] The negative electrode active material graphite, the conductive agent superconducting carbon (SP), the dispersant sodium carboxymethyl cellulose (CMC), and the binder (SBR) were mixed in deionized water at a ratio of 96:1:1:2 to form a uniform slurry. The prepared negative electrode slurry was coated on both sides of the copper foil and dried at 85°C. The coated electrode was further cold-pressed, slit, and cut into pieces. After cutting, the electrode was dried at 90°C for 4 hours to obtain the negative electrode sheet for the lithium-ion battery.
[0159] b. Preparation of positive electrode sheets for lithium-ion batteries
[0160] The positive electrode active material, nickel-cobalt-manganese ternary material (NCM622), conductive agent (SP), and binder PVDF were mixed in N-methylpyrrolidone (NMP) at a mass ratio of 98:1:1 to form a positive electrode slurry with a certain viscosity. The prepared slurry was evenly coated on both sides of aluminum foil and dried at 110°C. The coated electrode was further cold-pressed, slit, and cut into pieces. After cutting, the pieces were dried at 100°C for 2 hours to obtain the positive electrode sheets.
[0161] c. Preparation of lithium-ion battery electrolyte
[0162] The electrolyte lithium hexafluorophosphate is dissolved in a mixed solvent of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in a volume ratio of 1:1.5:1 to obtain a lithium ion battery electrolyte.
[0163] d. Lithium-ion battery assembly
[0164] The prepared positive electrode sheet, the above-mentioned separator and the negative electrode sheet are wound into a bare battery cell; after the bare battery cell is hot-pressed and the tabs are trimmed, the positive electrode is welded with an aluminum tab and the negative electrode is welded with a nickel-plated copper tab; finally, the welded battery cell is placed in an aluminum-plastic packaging bag and encapsulated, and the above-prepared electrolyte is injected, and then the battery cell is made into a lithium-ion battery through processes such as packaging, formation, and capacity division.
[0165] The performance test results are shown in Tables 1-4 below, where Ex represents an example and CEx represents a comparative example:
[0166] Table 1
[0167] Table 2 Note: “ / ” in the thermal shrinkage test results means the thermal shrinkage is greater than 50%. The diaphragm is rolled up and the specific shrinkage rate cannot be measured.
[0168] Table 3
[0169] Table 4
[0170] 1) In the porosity test, as shown in Table 1, the room temperature porosity of the membranes provided in Examples 1-20 of the present application ranged from 30% to 80%. Specifically, the room temperature porosity of the membrane in Example 12 reached 80%, which was much higher than the room temperature porosity of the membranes in Comparative Examples 1-3.
[0171] 2) In the thermal stability test, when the initial temperature T0 is set to 90°C, the porosity of the diaphragm at T0 is defined as P0. The diaphragm is then heated at a heating rate of 5-10°C / min to T1 (30°C ≤ T1-T0 ≤ 60°C, with T1 taken as 120°C, 135°C, and 150°C, respectively). The porosity P1 of the diaphragm is measured. From Table 1 above, it can be calculated that the porosity change in Examples 1-20 is 2.86% ≤ (P0-P1) / P0 ≤ 5%; while the porosity change of Comparative Examples 1-3 is greater than 5% under high temperature heating. It can be seen from this that under high temperature heating, the porosity change of the diaphragm provided by the present application is ≤5% compared to Comparative Examples 1-3, indicating that the diaphragm provided by the present application has good heat resistance and high thermal stability.
[0172] 3) The pore size distribution measurement results of Examples 1-6 show that the pore size distribution of the through-pore structure in the diaphragm can be adjusted by adjusting the mass ratio of the polystyrene monodisperse colloid to the nanocellulose solids in the nanocellulose suspension. When the mass ratio of the polystyrene monodisperse colloid to the nanocellulose solids in the nanocellulose suspension is in the range of 1:9 to 3:2, the through-pore structure distribution satisfies: through-pores with a pore diameter of 40 to 60 nm account for 40 to 70%, through-pores with a pore diameter less than 40 nm (specifically, a pore diameter in the range of 20 to 40 nm and excluding 40 nm) account for 10 to 30%, and through-pores with a pore diameter greater than 60 nm (specifically, a pore diameter in the range of 60 to 140 nm and excluding 60 nm) account for 5 to 35%, and this through-pore structure distribution can make the diaphragm have good wettability and ionic conductivity. When the mass ratio of the polystyrene monodisperse colloid to the nanocellulose solids in the nanocellulose suspension is too large (for example, 4:2 in Example 6) or too small (for example, 1:12 in Example 5), the proportion of through-pores with a pore size of 40 to 60 nm is too large (80%) or too small (30%), which in turn reduces the wettability and ionic conductivity of the diaphragm.
[0173] 4) The cellulose diameter measurement results in Table 2 show that the nanocellulose diameters of the membranes in Examples 1-20 are all within the range of 10 to 500 nm. Furthermore, Examples 1 and 7-11 show that the higher the refiner speed, the smaller the nanocellulose diameter in the prepared membranes. Furthermore, the basement membrane thickness measurement results in Table 2 show that the basement membrane thicknesses of the membranes in Examples 1-20 are all within the range of 9 to 30 μm. Furthermore, Examples 12-17 show that as the oxidant concentration decreases, the membrane thickness gradually increases.
[0174] 5) It can be seen from the heat shrinkage test data in Table 2 that the heat shrinkage rates of the diaphragms provided in Examples 1-20 of the present application are much smaller than those of the diaphragms in Comparative Examples 2 and 3. In particular, the longitudinal shrinkage rate MD of the diaphragms in Examples 1-20 at 120°C for 2 hours is 0.25% to 0.4%, and the transverse shrinkage rate TD is 0.08% to 0.1%, while the longitudinal shrinkage rate MD of the diaphragms in Comparative Examples 2 to 3 at 120°C for 2 hours is 4% to 5%, and the transverse shrinkage rate TD is 1% to 2%, indicating that the diaphragms of the present application have good heat shrinkage properties and high thermal stability.
[0175] 6) The liquid absorption rate and liquid retention test results in Table 3 show that, compared with Comparative Examples 1-3, the liquid absorption rate and liquid retention of the diaphragm provided in Examples 1-20 are significantly improved. This indicates that the diaphragm with a nanoporous structure in the present application exhibits excellent affinity for the electrolyte and has excellent liquid absorption and retention properties. In particular, Examples 12-17 show that when an oxidant is added to the diaphragm preparation method, the wettability of the diaphragm is improved to a certain extent compared to other examples (e.g., Examples 1-11). The higher the degree of oxidation, the stronger the wettability of the diaphragm, and accordingly, the greater the ionic conductivity.
[0176] 7) As can be seen from the data in Table 3, the longitudinal tensile strength of the diaphragms provided by Examples 1 to 20 of the present application is in the range of 200 to 256.3 MPa, which is higher than the longitudinal tensile strength of Comparative Examples 2 to 3; and the transverse tensile strength of the diaphragms is in the range of 250 to 300.6 MPa, which is also higher than the transverse tensile strength of Comparative Examples 2 to 3, indicating that the diaphragms provided by the present application have high mechanical strength. At the same time, the elastic modulus of the diaphragms of Examples 1 to 20 of the present application is in the range of 60 to 95 GPa, which is higher than the elastic modulus of the diaphragms of Comparative Examples 1 to 3, indicating that the diaphragms provided by the preparation method of the present application have high mechanical properties.
[0177] 8) As can be seen from the ionic conductivity results in Table 4, the ionic conductivity of the membranes provided in Examples 12 to 17 of the present application is higher than the ionic conductivity of the membranes in Examples 1 to 11, and much higher than the ionic conductivity of Comparative Examples 2 to 3. This is because in Examples 12 to 17, the oxidant oxidizes the alcohol hydroxyl groups in the cellulose polysaccharide into aldehyde groups, ketone groups or carboxyl groups, thereby further increasing the ionic conductivity of the membrane.
[0178] 9) The short-circuit performance and cycle performance test results of the batteries in Table 4 show that, compared with batteries using the separators of Comparative Examples 1-3, batteries using the separators prepared in Examples 1-20 of the present application have a significant advantage in preventing battery short-circuit fires. Furthermore, batteries using the separators prepared in Examples 1-20 of the present application exhibit superior cycle performance compared to batteries using the separators prepared in Comparative Examples 1-3, demonstrating that the separators of the present application can improve battery safety.
[0179] In summary, the diaphragm provided by the present application has greater mechanical strength and can withstand the puncture of lithium dendrites and external impacts, thereby improving the safety performance of the battery; the diaphragm provided by the present application has a uniform through-pore structure, and the pore size of the through-pore structure is mostly concentrated in the range of 40 to 60 nm. The presence of the nano-through-pore structure is conducive to the uniform evolution of the electrode-electrolyte interface, improves the speed and amount of electrolyte absorption by the diaphragm, improves the electrolyte wettability, and then improves the permeability and ion conductivity of the diaphragm; and the diaphragm provided by the present application has a higher porosity, for example, the room temperature porosity can be as high as 80%. The higher porosity can improve the liquid absorption and retention performance of the diaphragm, and can effectively improve the perfection of the interface between the diaphragm and the positive and negative electrodes in the battery, thereby improving the cycle life of the battery. And the prepared diaphragm is used in the production of lithium-ion batteries, so that the battery's interface stability and cycle life at high current density are significantly improved.
[0180] The above embodiments of this application focus on the differences between the various embodiments. As long as the different optimization features between the various embodiments are not contradictory, they can be combined to form a better embodiment. Considering the simplicity of the text, they will not be repeated here.
[0181] The foregoing is merely an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application should all be included within the scope of the claims of the present application.
Claims
1. A diaphragm, comprising a base film, the base film comprising nanocellulose, the diaphragm being heated from an initial temperature T0 to T1 at a heating rate of 5 to 10°C / min, the porosity P of the diaphragm satisfying: (P0-P1) / P0≤5%; wherein, 30℃≤T1-T0≤60℃, 80℃≤T0≤100℃, P0 is the porosity of the diaphragm at T0, and P1 is the porosity of the diaphragm at T1.
2. The diaphragm according to claim 1, wherein The diaphragm has a through-hole structure, and the through-hole structure distribution satisfies that through-holes with a pore size of 40-60 nm account for 40-70%, through-holes with a pore size less than 40 nm account for 10-30%, and through-holes with a pore size greater than 60 nm account for 5-35%.
3. The diaphragm according to claim 1, wherein The fiber diameter of the nanocellulose is 10 to 500 nm.
4. The diaphragm according to claim 3, wherein: The base film has a thickness of 9 to 30 μm.
5. The diaphragm according to claim 4, wherein The surface of the nanocellulose includes oxygen-containing functional groups, and the oxygen-containing functional groups include at least one of an aldehyde group, a ketone group, and a carboxylic acid group.
6. The separator according to any one of claims 1 to 5, wherein The longitudinal shrinkage MD of the separator at 120° C. for 2 hours is ≤0.4%, and the transverse shrinkage TD is ≤0.1%.
7. The separator according to any one of claims 1 to 5, wherein The elastic modulus of the diaphragm is 60 to 95 GPa.
8. The separator according to any one of claims 1 to 5, wherein The longitudinal tensile strength of the diaphragm is ≥200Mpa, and the transverse tensile strength of the diaphragm is ≥250Mpa. 9 . A secondary battery comprising the separator according to claim 1 .
10. An electrical device, characterized in that: The electric device comprises the secondary battery according to claim 9, and the secondary battery provides electric energy for the electric device.
Citation Information
Patent Citations
Preparation method of fiber-based lithium ion battery separator
CN109244329A
Diaphragm for lithium ion battery as well as preparation method and application of diaphragm
CN114050372A
Lightweight cellulose-based lithium battery diaphragm and preparation method thereof
CN114899549A
Preparation method and application of zirconium ion modified nano cellulose paper-based battery diaphragm
CN115149209A
Diaphragm, secondary battery and electric equipment
CN116722314A