Ag-based organic coordination nanoparticle and preparation method therefor, and photoresist composition and use thereof

Through the preparation of Ag-based organic coordination nanoparticles and photoresist composition, the problems of high absorption rate and poor solubility change reaction mechanism in extreme ultraviolet photolithography are solved, and high resolution, high sensitivity and low The lithographic properties of line roughness are suitable for manufacturing semiconductor devices with characteristic sizes of less than 20 nanometers.

WO2024235234A1PCT designated stage expired Publication Date: 2024-11-21TSINGHUA UNIVERSITY +1

Patent Information

Application Number
PCT/CN2024/093186
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-14
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

In the process of extreme ultraviolet photolithography, existing photoresist has problems such as high absorption rate and poor solubility change reaction mechanism, which affects its comprehensive performance, especially when manufacturing semiconductor devices with characteristic sizes of less than 20 nanometers, it is difficult to meet higher fineness. degree requirements.

Method used

Ag-based organic coordination nanoparticles were prepared by stirring, filtering and crystallizing silver salt and organic ligand at a specific temperature and solvent to form 1nm-4nm Ag-based organic coordination nanoparticles, and they were combined with a photoinitiator. Combined with an organic dispersing solvent, a photoresist composition is formed, and a pattern is formed by electron beam or extreme ultraviolet exposure development.

Benefits of technology

The photoresist is achieved with high resolution, high sensitivity and low line roughness. After development, it can effectively remove non-exposure areas, obtain patterns of desired shapes, and improve lithography performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024093186_21112024_PF_FP_ABST
    Figure CN2024093186_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an Ag-based organic coordination nanoparticle and a preparation method therefor, and a photoresist composition and the use thereof. The general formula of the Ag-based organic coordination nanoparticle is [Agm(R)n(Q)x]y. The preparation method for the Ag-based organic coordination nanoparticle comprises: separately adding a silver salt and a first organic ligand to a sample bottle, adding an organic solvent thereto to dissolve same, stirring same for a certain period of time under certain temperature conditions, subjecting same to filtration, concentration, and cooling crystallization or evaporative crystallization, and finally, performing recrystallization in an organic solvent, so as to obtain the Ag-based organic coordination nanoparticle. The nanoparticle composition can be used as an electron beam, medium-ultraviolet, deep-ultraviolet or EUV photoresist.
Need to check novelty before this filing date? Find Prior Art

Description

Ag-based organic coordination nanoparticles and preparation method thereof, photoresist composition and application thereof Technical Field

[0001] The present invention relates to the technical field of photoresists, in particular to Ag-based organic coordination nanoparticles and a preparation method thereof, a photoresist composition and application thereof. Background Art

[0002] Photoresist refers to a corrosion-resistant thin film material whose solubility is altered by exposure to ultraviolet light, electron beams, ion beams, extreme ultraviolet (EUV), or soft X-rays. It is widely used for pattern transfer in the fabrication of high-end micro- and nanostructures, including semiconductor integrated circuits, liquid crystal display panels, and high-end optical devices. With the continuous advancement of semiconductor technology and the growth of Moore's Law, semiconductor process sizes have continued to shrink, placing higher demands on the reduction of feature sizes. To meet the needs of more advanced semiconductor processes and achieve smaller feature sizes, photolithography technology has continued to evolve, from I-line, G-line, and deep ultraviolet (DUV) (including 248nm KrF lithography and 193nm ArF lithography) to EUV lithography, electron beam lithography, and other precision fabrication methods. After the photoresist film is exposed and developed to form the lithographic pattern, it is then etched using either dry or wet methods. The portions of the substrate material not covered by the photoresist film are directly etched, while the covered substrate surface is protected by the photoresist film. Etching resistance is a very important evaluation index of photoresist. Excellent etching resistance can ensure that the photoresist can protect the substrate surface from damage during the etching process, effectively simplify the etching process, and greatly improve the yield of the etched product.

[0003] Extreme ultraviolet lithography has attracted attention as a fundamental technology for manufacturing next-generation semiconductor devices. EUV lithography is a pattern-forming technology that uses EUV radiation with a wavelength of approximately 13.5 nanometers as an exposure light source. According to EUV lithography, it is known that extremely fine patterns (e.g., less than or equal to approximately 20 nanometers) can be formed in the exposure process during the manufacture of semiconductor devices. For exposure in the EUV band, the absorptivity of the photoresist itself, the reaction mechanism that causes solubility changes after exposure, and the size distribution of the photoresist components have a significant impact on the overall performance of the photoresist. Because metal elements have a higher absorptivity to EUV radiation, metal-containing photoresist materials have attracted interest, and metal oxide nanoparticle photoresists are one of the hot research directions. The Ober group at Cornell University in the United States first introduced the concept of metal oxide nanoparticles as a next-generation EUV photoresist material. These nanoparticles are typically synthesized by controlled hydrolysis of Zr or Hf alkoxides in an excess of carboxylic acid, followed by precipitation, to produce nanoparticle photoresists containing organic ligands, ZrO₂ or HfO₂. The size of the corresponding nanoparticles is controlled to be between 2 and 5 nm, making them suitable for photolithography below 20 nm. To further develop more efficient metal-organic nanophotoresists, this paper focuses on Ag-based organic ligand nanoparticle photoresists and has produced photoresists with excellent lithographic performance. Technical issues

[0004] The problem solved by the embodiments of the present invention is to provide a novel Ag-based organic coordination nanoparticle and a preparation method thereof, a photoresist composition containing the same and application thereof. Technical Solutions

[0005] The present invention provides a Ag-based organic coordination nanoparticle, the general formula of which is: [Ag m (R) n (Q) x ] y ,

[0006] Among them, R can be selected from bis(diphenylphosphino)methane (dppm), bis(dicyclohexylphosphino)methane (abbreviated as dcpm), bis(diphenylamino)methane, N,N-bis(diphenylphosphino)amine (abbreviated as dppa), N,N,N',N'-tetramethyldiaminomethane, N,N,N',N'-tetraethyldiaminomethane, etc.

[0007] Q can be selected from CH3COO, C2H5COO, C3H7COO, i-C3H7COO, C4H9COO, C6H 13 COO, C9H 19 COO, C6H5COO, CF3COO, C2F5COO, C3F7COO, i-C3F7COO, C4F9COO, C6F13 COO, C9F 19 COO, C6H5COO, etc. wherein m, n, x, and y are all in the range of 1-4.

[0008] Furthermore, the Ag-based organic coordination nanoparticles may have the following structure:

[0009] Ag2(dppm)2(CH3COO)2;

[0010] Ag4(dppm)2(CH3COO)4;

[0011] Ag4(dppm)2(CF3COO)4;

[0012] Ag2(dppm)2(C2H5COO)2;

[0013] Ag4(dppm)2(C2F5COO)4;

[0014] Ag4(dppm)2(C4F9COO)4;

[0015] Ag2(dcpm)2(CH3COO)2;

[0016] Ag4(dppa)2(CH3COO)4

[0017] The size of the Ag-based organic coordination nanoparticle crystals is 1 nm-4 nm, preferably 1 nm-2 nm.

[0018] The above-mentioned Ag-based organic coordination nanoparticles are prepared by the following method:

[0019] The silver salt and the first organic ligand are added to a sample bottle respectively, and an organic solvent is added to dissolve them. The silver salt and the first organic ligand are stirred for a certain time under certain temperature conditions, filtered, concentrated, cooled and crystallized or evaporated and finally recrystallized in an organic solvent to obtain Ag-based organic coordination nanoparticles.

[0020] Furthermore, the ratio of the silver salt to the first organic ligand is 1:(0.5-1);

[0021] The organic solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-ethoxy-2-propanol, tetrahydrofuran, methanol, ethanol, propanol, dichloromethane, and chloroform. The stirring temperature is controlled at 0-120°C, preferably 15-80°C, and more preferably 20-40°C.

[0022] The present invention also provides a photoresist composition comprising the above nanoparticles.

[0023] Furthermore, the above-mentioned photoresist composition further includes a photoinitiator and an organic dispersing solvent. The photoinitiator preferably occupies 0.1 wt%-10 wt% of the composition, and the nanoparticles preferably occupy 1 wt%-20 wt% of the composition.

[0024] Furthermore, the photoinitiator is selected from any one or more of N-hydroxynaphthalimide trifluoromethanesulfonic acid, 1,4-aminonaphthalenesulfonic acid, 2-amino-5,7-naphthalenedisulfonic acid, tert-butylphenyliodonium salt perfluorooctanesulfonic acid, triphenylsulfonium perfluorobutanesulfonic acid, triphenylsulfonium perfluorobutyl and triphenylsulfonium trifluorosulfonic acid.

[0025] Furthermore, the organic dispersing solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-methoxy-2-propanol, propylene glycol mono-n-propyl ether, propylene glycol butyl ether, 1-ethoxy-2-propanol, methanol, ethanol, and propanol. The solvent is preferably 1-ethoxy-2-propanol.

[0026]

Method for patterning metal-organic coordination nanoparticles photoresist

[0027] The present invention also provides a method for forming a photolithographic pattern, which uses the above-mentioned photoresist composition, drops the photoresist composition onto a substrate, spin-coats it into a film, heats it on a hot table, exposes it with an electron beam or mid-ultraviolet, deep ultraviolet, or extreme ultraviolet, and develops it with a developer.

[0028] Furthermore, the spin coating speed is 1000-6000 rpm; the heating temperature of the hot stage is controlled at 50-110° C., and the heating time is controlled at 30-900 s.

[0029] Furthermore, the exposure dose is 50 to 8000 mJ / cm 2 .

[0030] Furthermore, the developer is selected from a mixture of any one or more of decahydronaphthalene, tetrahydronaphthalene, indene, indane, quinoline, 1-methylnaphthalene, toluene, o-xylene, m-xylene, p-xylene, ethyl acetate, butyl acetate, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, propylene glycol mono-n-propyl ether, propylene glycol butyl ether, n-hexane and cyclohexane, and the developing temperature is room temperature or 20°C to 50°C.

[0031] The thickness of the pre-film layer after removing the organic dispersing solvent may be 10 nm to 100 nm. Specifically, the thickness of the pre-film layer may be 10 nm to 20 nm, 20 nm to 30 nm, 30 nm to 40 nm, 40 nm to 50 nm, 50 nm to 60 nm, 60 nm to 70 nm, 70 nm to 80 nm, 80 nm to 90 nm, or 90 nm to 100 nm.

[0032] The substrate is selected from a silicon plate. Other substrates that are insoluble in developer can also be selected according to actual needs.

[0033] Furthermore, the aforementioned nanoparticles are used in the field of photoresists, particularly electron beam, mid-UV, deep UV, and EUV photoresists. Regarding the mask, deep UV and longer wavelength light sources are transmissive masks, while extreme UV is reflective. Electron beam exposure is performed according to the pattern set by the software. Beneficial effects

[0034] Compared with the prior art, the technical solution of the present invention has the following advantages:

[0035] The Ag-based organic coordination nanoparticles provided by the embodiments of the present invention have a special structure. The photoacid generator generates photoacid after being irradiated by ultraviolet light. The photoacid can interact with the Ag-based organic coordination nanoparticles, thereby changing the polarity of the Ag-based organic coordination nanoparticles, causing the nanoparticles to agglomerate. Therefore, the solubility of the Ag-based organic coordination nanoparticles before and after exposure changes. Due to these characteristics, the Ag-based organic coordination nanoparticles are used as photoresist components. The solubility of the photosensitive portion and the light-shielding portion of the photoresist in the developer can be different. The photosensitive portion agglomerates in the developer, and the solubility is reduced, while the light-shielding portion does not agglomerate and dissolves in the developer. Thus, after development, the non-exposed area can be removed to obtain a pattern of the desired shape. Using the Ag-based organic coordination nanoparticles of the present invention as photoresist components can achieve more excellent lithographic performance such as high resolution, high sensitivity, and low line roughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] FIG1 is the structural formula of the crystalline compound prepared in Example 1 of the present invention;

[0037] FIG2 is a hydrogen NMR spectrum of the crystalline compound prepared in Example 1 of the present invention;

[0038] FIG3 is a dynamic light scattering particle size test result of Example 1 of the present invention;

[0039] FIG4 is an exposure pattern of Example 1 of the present invention;

[0040] FIG5 is a structural formula of Example 2 of the present invention;

[0041] FIG6 is a hydrogen NMR spectrum of Example 2 of the present invention;

[0042] FIG7 is a dynamic light scattering particle size test result of Example 2 of the present invention;

[0043] FIG8 is an exposure pattern of Example 2 of the present invention;

[0044] FIG9 is a structure of Example 3 of the present invention;

[0045] FIG10 is a H-NMR spectrum of Example 3 of the present invention;

[0046] FIG11 is a dynamic light scattering particle size test result of Example 3 of the present invention;

[0047] FIG. 12 is an exposure pattern according to Example 3 of the present invention. Modes for Carrying Out the Invention

[0048] To facilitate understanding of the present invention, the present invention will be described more fully below with reference to the accompanying drawings. Preferred embodiments of the present invention are shown in the accompanying drawings. However, the present invention may be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and comprehensive understanding of the present disclosure.

[0049] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0050] The present invention provides a Ag-based organic coordination nanoparticle, the general formula of which is: [Ag m (R) n (Q) x ] y

[0051] Among them, R can be selected from bis(diphenylphosphino)methane (dppm), bis(dicyclohexylphosphino)methane (abbreviated as dcpm), bis(diphenylamino)methane, N,N-bis(diphenylphosphino)amine (abbreviated as dppa), N,N,N',N'-tetramethyldiaminomethane, N,N,N',N'-tetraethyldiaminomethane, etc.

[0052] Q can be selected from CH3COO, C2H5COO, C3H7COO, i-C3H7COO, C4H9COO, C6H 13 COO, C9H 19 COO, C6H5COO, CF3COO, C2F5COO, C3F7COO, i-C3F7COO, C4F9COO, C6F 13 COO, C9F 19 COO, C6H5COO, etc., where m, n, x, and y are all in the range of 1-4;

[0053] Furthermore, the Ag-based organic coordination nanoparticles may have the following structure:

[0054] Ag2(dppm)2(CH3COO)2;

[0055] Ag4(dppm)2(CH3COO)4;

[0056] Ag4(dppm)2(CF3COO)4;

[0057] Ag2(dppm)2(C2H5COO)2;

[0058] Ag4(dppm)2(C2F5COO)4;

[0059] Ag4(dppm)2(C4F9COO)4;

[0060] Ag2(dcpm)2(CH3COO)2;

[0061] Ag4(dppa)2(CH3COO)4.

[0062] The size of the Ag-based organic coordination nanoparticle crystals is 1 nm-4 nm, preferably 1 nm-2 nm.

[0063] The Ag-based organic coordination nanoparticles provided by the embodiments of the present invention have a special structure. The photoacid generator generates photoacid after being irradiated by ultraviolet light. The photoacid can interact with the Ag-based organic coordination nanoparticles, thereby changing the polarity of the Ag-based organic coordination nanoparticles, causing the nanoparticles to agglomerate. Therefore, the solubility of the Ag-based organic coordination nanoparticles before and after exposure changes. Due to these characteristics, the Ag-based organic coordination nanoparticles are used as photoresist components. The solubility of the photosensitive portion and the light-shielding portion of the photoresist in the developer can be different. The photosensitive portion agglomerates and the solubility is reduced in the developer, while the light-shielding portion does not agglomerate and dissolves in the developer. Thus, after development, the non-exposed area can be removed to obtain a pattern of the desired shape. Using the Ag-based organic coordination nanoparticles of the present invention as photoresist components can achieve more excellent lithographic performance such as high resolution, high sensitivity, and low line roughness.

[0064] The above-mentioned Ag-based organic coordination nanoparticles are prepared by the following method:

[0065] The silver salt and the first organic ligand are added to a sample bottle respectively, and an organic solvent is added to dissolve them. The silver salt and the first organic ligand are stirred for a certain time under certain temperature conditions, filtered, concentrated, cooled and crystallized or evaporated and crystallized. Finally, the silver salt and the first organic ligand are recrystallized in an organic solvent to obtain Ag-based organic coordination nanoparticles.

[0066] Furthermore, the ratio of the silver salt to the first organic ligand is 1:(0.5-1);

[0067] The organic solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-ethoxy-2-propanol, tetrahydrofuran, methanol, ethanol, propanol, dichloromethane, and chloroform. The stirring temperature is controlled at 0-120°C, preferably 15-80°C, and more preferably 20-40°C.

[0068] Some embodiments of the present invention provide Ag organic coordination nanoparticle photoresist compositions, including the above-mentioned nanoparticles, a photoinitiator and an organic dispersing solvent, wherein the photoinitiator preferably occupies 0.1wt%-10wt% of the composition, and the nanoparticles preferably occupy 1wt%-20% of the composition.

[0069] Furthermore, the photoinitiator is selected from any one or more of N-hydroxynaphthalimide trifluoromethanesulfonic acid, 1,4-aminonaphthalenesulfonic acid, 2-amino-5,7-naphthalenedisulfonic acid, tert-butylphenyliodonium salt perfluorooctanesulfonic acid, triphenylsulfonium perfluorobutanesulfonic acid, triphenylsulfonium perfluorobutyl and triphenylsulfonium trifluorosulfonic acid.

[0070] Furthermore, the organic dispersing solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-methoxy-2-propanol, propylene glycol mono-n-propyl ether, propylene glycol butyl ether, 1-ethoxy-2-propanol, methanol, ethanol, and propanol. The solvent is preferably 1-ethoxy-2-propanol.

[0071] Some embodiments of the present invention provide a method for patterning Ag organic coordinated nanoparticle photoresist, using the above-mentioned photoresist composition, dropping the photoresist composition onto a substrate by spin coating, heating it on a hot plate, and then exposing it to electron beam or mid-ultraviolet, deep ultraviolet, or extreme ultraviolet light, and developing it with a developer.

[0072] Furthermore, the spin coating speed is 1000-6000 rpm; the heating temperature of the hot stage is controlled at 50-110° C., and the heating time is controlled at 30-900 s.

[0073] Furthermore, the exposure dose is 50 to 8000 mJ / cm 2 .

[0074] Furthermore, the developer is selected from a mixture of any one or more of decahydronaphthalene, tetrahydronaphthalene, indene, indane, quinoline, 1-methylnaphthalene, toluene, o-xylene, m-xylene, ethyl acetate, butyl acetate, ethanol, n-propanol, isopropanol, n-butanol, n-hexane and cyclohexane, and the developing temperature is room temperature or 20°C to 50°C.

[0075] The thickness of the pre-film layer after removing the organic dispersing solvent may be 10 nm to 100 nm. Specifically, the thickness of the pre-film layer may be 10 nm to 20 nm, 20 nm to 30 nm, 30 nm to 40 nm, 40 nm to 50 nm, 50 nm to 60 nm, 60 nm to 70 nm, 70 nm to 80 nm, 80 nm to 90 nm, or 90 nm to 100 nm.

[0076] The substrate is selected from a silicon plate. Other substrates that are insoluble in developer can also be selected according to actual needs.

[0077] Furthermore, the aforementioned nanoparticles can be used in the field of photoresists, particularly electron beam, mid-UV, deep UV, extreme UV, and / or EUV photoresists. Regarding the mask, deep UV and longer wavelength light sources are used as transmissive masks, while extreme UV is used as reflective masks. Electron beam exposure is performed according to a pattern set by software.

[0078] Example 1

[0079] 0.769 g of bis(diphenylphosphino)methane was dissolved in 20 mL of dichloromethane, 0.884 g of silver trifluoroacetate was added, and the mixture was stirred for 12 hours. The mixture was filtered and the solvent was evaporated to obtain a white solid product. The product was recrystallized from dichloromethane and dried under vacuum at room temperature. A sample was taken for H NMR analysis (see Figure 2, where δ 3.26 (CH2), δ 7.26, 7.40 (C6H5)). The crystalline structure is shown in Figure 1, with a molecular formula of Ag4(dppm)2(CF3COO)4.

[0080] 0.5 g of Ag4(dppm)2(CF3COO)4 and 0.05 g of N-hydroxynaphthalimide trifluoromethanesulfonate were weighed and dissolved in 0.945 g of propylene glycol monomethyl ether acetate. The solution was filtered three times with a 0.22 μm filter to obtain a photoresist composition. Dynamic light scattering particle size testing showed that the average particle size was 1.7 nm (see Figure 3). The spin coater was set to 2000 rpm for 1 minute, and a uniform photoresist film was spin-coated on a silicon wafer. The wafer was then placed on a hot plate at 80°C and heated for 1 minute. The wafer was exposed to a 254 nm wavelength mercury lamp at a dose of 1260 mJ / cm 2 , using m-xylene as a developer, developing for 10 seconds to obtain a line pattern with a half-pitch of 10 μm (see FIG4 ).

[0081] Example 2

[0082] 0.157 g of bis(diphenylphosphino)methane was dissolved in 16 mL of dichloromethane, 0.136 g of silver acetate was added, and the mixture was stirred until a clear solution was obtained. The mixture was filtered, concentrated, and cooled to produce a white precipitate. The precipitate was isolated and recrystallized from dichloromethane / n-hexane. The crystals were sampled and tested for hydrogen nuclear magnetic resonance (HNMR) (see Figure 6, HNMR spectrum δ 2.02 (CH3), δ 3.31 (CH2), δ 7.0-7.5 (C6H5)). The crystalline structure is shown in Figure 5, with a molecular formula of Ag4(dppm)2(CH3COO)4, and dried in vacuo at room temperature.

[0083] Weigh 0.5g Ag4(dppm)2(CH3COO)4 and 0.05g N-hydroxynaphthalimide trifluoromethanesulfonate, dissolve them in 0.945g propylene glycol monomethyl ether acetate, and filter the solution three times with a 0.22μm filter. Dynamic light scattering particle size test showed that the average particle size was 1.7nm (see Figure 7). Set the spin coater speed to 2000rpm for 1min, spin coat a uniform photoresist film on the silicon wafer, and then place the wafer on a hot plate at 80℃ and heat for 1min. Expose the above wafer to a 254nm wavelength mercury lamp light source with a dose of 2000mJ / cm 2 , using o-xylene as a developer, developing for 15 seconds to obtain a line pattern with a half-pitch of 10 μm (see Figure 8).

[0084] Example 3

[0085] 0.104 g of Ag4(dppm)2(CH3COO)4 crystals were dissolved in 30 mL of methanol, 0.056 g of bis(diphenylphosphino)methane was added, and the mixture was stirred until a clear solution was obtained. The mixture was filtered, concentrated, and cooled to form a precipitate. The precipitate was separated and recrystallized from dichloromethane / n-hexane. The precipitate was separated and sampled for H NMR spectrum testing (see Figure 10, wherein the H NMR spectrum is δ2.12 (CH3), δ3.36 (CH2), δ6.95-7.45 (C6H5)). The crystalline structure is shown in Figure 9, with a molecular formula of Ag2(dppm)2(CH3COO)2, and the mixture was dried in vacuo at room temperature.

[0086] Weigh 0.5g Ag2(dppm)2(OAc)2 and 0.05g N-hydroxynaphthalimide trifluoromethanesulfonate, dissolve them in 0.945g propylene glycol monomethyl ether acetate, and filter the solution three times with a 0.22μm filter. Dynamic light scattering particle size test showed that the average particle size was 1.3nm (see Figure 11). Set the spin coater speed to 2000rpm for 1min, spin coat a uniform photoresist film on the silicon wafer, and then place the wafer on a hot plate at 80℃ and heat for 1min. Expose the above wafer to a 254nm wavelength mercury lamp light source with a dose of 270mJ / cm 2 , using m-xylene as a developer, developing for 30 seconds to obtain a line pattern with a half-pitch of 10 μm (see Figure 12).

[0087] In summary, the present invention has obtained a variety of effective nanoparticles and corresponding compositions, which have verified that the structure has good lithography performance under mid-ultraviolet and electron beam conditions, and can achieve better lithography performance such as high resolution, high sensitivity, and low line roughness.

Claims

1. An Ag-based organic coordination nanoparticle, characterized in that: The general formula is: [Ag m (R) n (Q) x ] y , the ranges of m, n, x, and y are all 1-4; Wherein, R is selected from bis(diphenylphosphino)methane (dppm), bis(dicyclohexylphosphino)methane (abbreviated dcpm), bis(diphenylamino)methane, N,N-bis(diphenylphosphino)amine (abbreviated dppa), N,N,N',N'-tetramethyldiaminomethane, N,N,N',N'-tetraethyldiaminomethane; Q is selected from CH3COO, C2H5COO, C3H7COO, i-C3H7COO, C4H9COO, C6H 13 COO, C9H 19 COO, C6H5COO, CF3COO, C2F5COO, C3F7COO, i-C3F7COO, C4F9COO, C6F 13 COO, C9F 19 COO, C6H5COO.

2. The Ag-based organic coordination nanoparticles according to claim 1, characterized in that: Its specific structure is: Ag2(dppm)2(CH3COO)2; Ag4(dppm)2(CH3COO)4; Ag4(dppm)2(CF3COO)4; Ag2(dppm)2(C2H5COO)2; Ag4(dppm)2(C2F5COO)4; Ag4(dppm)2(C4F9COO)4; Ag2(dcpm)2(CH3COO)2; Ag4(dppa)2(CH3COO)4.

3. The Ag-based organic coordination nanoparticles according to claim 1, characterized in that: The size of the Ag-based organic coordination nanoparticle crystal is 1nm-4nm.

4. The method for preparing Ag-based organic coordination nanoparticles according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: adding silver salt and a first organic ligand into a sample bottle respectively, adding an organic solvent to dissolve them, stirring for a certain time under certain temperature conditions, filtering, concentrating, cooling crystallization or evaporation crystallization, and finally recrystallizing in an organic solvent to obtain Ag-based organic coordination nanoparticles, wherein the ratio of the silver salt to the first organic ligand is 1:(0.5-1).

5. The method for preparing Ag-based organic coordination nanoparticles according to claim 4, characterized in that: The organic solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-ethoxy-2-propanol, tetrahydrofuran, methanol, ethanol, propanol, dichloromethane and chloroform.

6. The method for preparing Ag-based organic coordination nanoparticles according to claim 4, characterized in that: The stirring temperature is controlled at 0-120°C.

7. A photoresist composition comprising the Ag-based organic coordination nanoparticles according to any one of claims 1 to 3, and further comprising a photoinitiator and an organic dispersing solvent, wherein: The photoinitiator occupies 0.1 wt%-10 wt% of the composition, and the Ag-based organic coordination nanoparticles occupies 1 wt%-20 wt% of the composition.

8. The photoresist composition according to claim 7, characterized in that The photoinitiator is selected from any one or more of N-hydroxynaphthaleneimide trifluoromethanesulfonic acid, 1,4-aminonaphthalenesulfonic acid, 2-amino-5,7-naphthalene disulfonic acid, tert-butylphenyl iodonium salt perfluorooctanesulfonic acid, triphenylsulfonium perfluorobutanesulfonic acid, triphenylsulfonium perfluorobutyl and triphenylsulfonium trifluorosulfonic acid.

9. The photoresist composition according to claim 7, characterized in that: The organic dispersing solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-methoxy-2-propanol, propylene glycol mono-n-propyl ether, propylene glycol butyl ether, 1-ethoxy-2-propanol, methanol, ethanol, and propanol.

10. A method for patterning Ag organic coordinated nanoparticle photoresist, comprising: using the photoresist composition as claimed in any one of claims 7 to 9, dripping the photoresist composition onto a substrate by spin coating, heating it on a hot stage, exposing it to electron beam or mid-ultraviolet, deep ultraviolet or extreme ultraviolet light, and developing it with a developer, wherein the spin coating speed is 1000 to 6000 rpm; the heating temperature of the hot stage is controlled at 50 to 110° C., the heating time is controlled at 30 to 900 s, and the exposure dose is 50 to 8000 mJ / cm 2 The developer is selected from a mixture of any one or more of decahydronaphthalene, tetrahydronaphthalene, indene, indane, quinoline, 1-methylnaphthalene, toluene, o-xylene, m-xylene, ethyl acetate, butyl acetate, ethanol, n-propanol, isopropanol, n-butanol, n-hexane and cyclohexane, and the developing temperature is room temperature or 20°C to 50°C; the thickness of the pre-film layer after removing the organic dispersing solvent can be 10nm to 100nm.

11. Use of the Ag-based organic coordination nanoparticles according to any one of claims 1 to 3 for electron beam, mid-ultraviolet, deep ultraviolet and / or extreme ultraviolet photoresists.

Citation Information

Patent Citations

  • Metal peroxo compounds with organic co-ligands for electron beam, deep uv and extreme uv photoresist applications

    CN104145217A

  • Photoactive, inorganic ligand-capped inorganic nanocrystals

    CN110832618A

  • Photoresist composition and method of forming thin film pattern and array substrate using same

    CN111766762A

  • Photoresist and patterning method of imine material

    CN111880371A

  • Photoresist composition based on metal nanoparticles and application thereof

    CN114089599A

Cited By

  • Preparation method of luminescent material for epoxy negative photoresist

    CN121537955A

  • A method for preparing a luminescent material for epoxy negative photoresist

    CN121537955B