Martensitic stainless seamless steel pipe

The seamless martensitic stainless steel pipe with a tailored composition and microstructure addresses the challenges of high strength, low-temperature toughness, and corrosion resistance, ensuring effective performance in harsh CCS environments.

WO2024236897A1PCT designated stage expired Publication Date: 2024-11-21JFE STEEL CORP

Patent Information

Application Number
PCT/JP2024/009910
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-03-14
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Martensitic stainless steel pipes used in oil country tubular goods and carbon capture and storage (CCS) applications face challenges in achieving high strength, low-temperature toughness, and corrosion resistance, particularly in environments with high CO2 and chloride ions at elevated temperatures and pressures.

Method used

A seamless martensitic stainless steel pipe composition with specific ranges of Cr, Ni, and other elements is developed, including 15.0-17.5% Cr and 6.0-9.0% Ni, to enhance yield strength, low-temperature toughness, and corrosion resistance, with a microstructure predominantly composed of martensite and optional additional elements to satisfy specific relational expressions for optimal properties.

Benefits of technology

The solution provides a seamless martensitic stainless steel pipe with a yield stress of 758 MPa or more, absorbed energy of 100 J or more at -80°C, and excellent corrosion resistance, suitable for demanding CCS press-fit pipe applications and potentially cheaper than duplex stainless steel alternatives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a martensitic stainless seamless steel pipe which has a yield stress of 758 MPa or more, has an absorption energy of 100 J or more in a Charpy impact test at -80°C, and has excellent corrosion resistance. This martensitic stainless seamless steel pipe comprises, in terms of mass%, 0.005%-0.100% of C, 0.05%-1.00% of Si, 0.05%-1.00% of Mn, 0.05% or less of P, 0.005% or less of S, 6.0%-9.0% of Ni, 15.0%-17.5% of Cr, 0.001%-0.10% of Al, 0.001%-0.20% of Nb, 0.1% or less of N, 0.01% or less of O, 3.5% or less of Cu, less than 1.0% of Mo, and 1.0% or less of W, with the balance being Fe and inevitable impurities, and has a component composition that satisfies predetermined formulae (1) and (2).
Need to check novelty before this filing date? Find Prior Art

Description

Martensitic stainless steel seamless pipe

[0001] The present invention relates to a martensitic stainless steel seamless pipe.

[0002] In conventional oil and gas fields, martensitic stainless steel pipes such as 13% Cr steel (steel containing approximately 13% by mass of Cr) and 17% Cr steel (steel containing approximately 17% by mass of Cr) are widely used as oil country tubular goods for mining. Furthermore, in recent years, carbon dioxide capture and storage (CCS) technology has been promoted worldwide in order to achieve carbon neutrality. In CCS, martensitic stainless steel pipes are also used for injection pipes (hereinafter also referred to as CCS injection pipes) used to inject captured carbon dioxide into aquifers or depleted oil fields.

[0003] Oil country tubular goods and CCS injection pipes are steel pipes that are connected to depths of several thousand meters underground, so they must be strong enough to withstand their own weight. Furthermore, both oil country tubular goods and CCS injection pipes must be corrosion resistant in environments where high-temperature, high-pressure carbon dioxide and chloride ions are present. In particular, CCS sometimes injects carbon dioxide containing highly corrosive impurities such as oxygen, sulfur oxides, and nitrogen oxides, so the material for the CCS injection pipes must be highly corrosion resistant.

[0004] Furthermore, when oil country tubular goods and CCS injection pipes are used in cold regions, they must not become embrittled even at low temperatures, and therefore low-temperature toughness is required. In particular, in the case of CCS injection pipes, the pressure of the fluid passing through the steel pipe is high, so there is a concern that if a sudden pressure drop occurs due to a leak or other reason, the temperature will drop due to the Joule-Thomson effect. Therefore, toughness at even lower temperatures may be required.

[0005] Patent Document 1 proposes a high-strength, high-toughness seamless steel pipe having a chemical composition with a Cr content of 14% by mass or less. Patent Documents 2 to 4 propose high-strength, high-toughness, and high-corrosion-resistant seamless steel pipes having a chemical composition with a Cr content of about 17% by mass and a Ni content of 6.0% by mass or less, and a structure containing a certain amount of ferrite phase.

[0006] International Publication No. 2009 / 004741 Japanese Patent Application Laid-Open No. 2017-14543 International Publication No. 2019 / 035329 International Publication No. 2020 / 202957

[0007] The technology described in Patent Document 1 involves the use of a 20 mass % NaCl aqueous solution at a liquid temperature of 80°C and CO at 30 atmospheres. 2 Although corrosion tests have been conducted for one week in atmospheric conditions, it may not be said that the material has sufficient corrosion resistance in the more severe corrosive environments of oil country tubular goods and CCS injection pipes.

[0008] In Patent Documents 2 and 3, excellent low-temperature toughness is defined as an absorbed energy of 80 J or more at −60° C. and an absorbed energy of 40 J or more at −40° C. in a Charpy impact test, respectively. Furthermore, in Patent Document 4, excellent low-temperature toughness is defined as an absorbed energy of 300 J or more at −10° C. in a Charpy impact test and a ductile-brittle transition temperature of −40° C. or less. However, in applications for CCS press-fitted pipes, the use environment may be −60° C. or less, and therefore toughness at even lower temperatures may be required.

[0009] Thus, martensitic stainless steels containing about 13% by mass of Cr can achieve high strength and high toughness, but may not have sufficient corrosion resistance.On the other hand, martensitic stainless steels containing about 17% by mass of Cr, which have relatively high corrosion resistance, have the problem of reduced low-temperature toughness due to the inclusion of a ferrite phase.

[0010] An object of the present invention is to provide a martensitic stainless steel seamless pipe having a yield stress of 758 MPa or more, an absorbed energy of 100 J or more in a Charpy impact test at −80° C., and excellent corrosion resistance.

[0011] In the present invention, "having excellent corrosion resistance" means that the corrosion resistance is high enough to withstand 30 atmospheres of CO 2 This refers to a corrosion rate of 0.127 mm / y or less when a test piece is immersed in a 20 mass % NaCl aqueous solution at a liquid temperature of 200°C for 336 hours in a gas atmosphere.

[0012] To achieve the above-mentioned objectives, the present inventors conducted extensive research into the composition of martensitic stainless steels that combine high strength, high toughness, and high corrosion resistance. As a result, they discovered that increasing the Ni content to 6-9 mass% and reducing the ferrite phase compared to conventional 17% Cr steels can improve toughness at lower temperatures while maintaining high corrosion resistance. However, increasing the content of alloys such as Cr and Ni can lower the Ms point, the temperature at which martensitic transformation begins, to below room temperature, potentially preventing sufficient strength from being achieved even after quenching. Therefore, they discovered that by defining C, Cu, Ni, Cr, Mo, Nb, N, and W in an appropriate relationship and further adjusting the composition so that the value calculated by the relationship falls within a predetermined range, a martensitic stainless steel seamless pipe with the desired strength, excellent low-temperature toughness, and excellent corrosion resistance can be obtained.

[0013] The present invention was completed based on these findings and further investigations. That is, the gist of the present invention is as follows. [1] A martensitic stainless steel seamless pipe containing, by mass%, C: 0.005 to 0.100%, Si: 0.05 to 1.00%, Mn: 0.05 to 1.00%, P: 0.05% or less, S: 0.005% or less, Ni: 6.0 to 9.0%, Cr: 15.0 to 17.5%, Al: 0.001 to 0.10%, Nb: 0.001 to 0.20%, N: 0.1% or less, O: 0.01% or less, Cu: 3.5% or less, Mo: less than 1.0%, and W: 1.0% or less, with the balance being Fe and unavoidable impurities, and having a chemical composition that satisfies the following formulas (1) and (2): 1001-2172C-17.35Cu-44.95Ni-34.45Cr-22.15Mo+60.96Nb-978.3N-18.57W>50.00 (1) Cr+0.65Ni+0.6Mo+0.3W+0.55Cu-20C>20.00 (2) Here, each element symbol in formula (1) and formula (2) indicates the content (mass%) of the corresponding element, and if the element is not contained, it is set to 0. [2] The martensitic stainless steel seamless pipe according to [1], wherein the chemical composition further contains, in mass %, one or more elements selected from the group consisting of Co: 1% or less, V: 0.1% or less, Ti: 0.1% or less, Zr: 0.2% or less, Ta: 0.2% or less, Hf: 0.2% or less, Ca: 0.01% or less, REM: 0.01% or less, Mg: 0.01% or less, B: 0.01% or less, Sn: 0.2% or less, and Sb: 0.2% or less. [3] The martensitic stainless steel seamless pipe according to [1] or [2], which has a yield strength of 758 MPa or more and an absorbed energy of 100 J or more in a Charpy impact test at -80°C.

[0014] According to the present invention, it is possible to provide a martensitic stainless steel seamless pipe having a yield stress of 758 MPa or more, an absorbed energy of 100 J or more in a Charpy impact test at −80° C., and excellent corrosion resistance.

[0015] According to the present invention, martensitic stainless steel seamless pipes can be used for CCS press-fit pipe applications, which require superior low-temperature toughness and high corrosion resistance compared to conventional oil country tubular goods applications. Furthermore, according to the present invention, it is possible to provide martensitic stainless steel seamless pipes that are less expensive and have superior toughness, even for applications in which duplex stainless steels such as 25% Cr steel are used.

[0016] The martensitic stainless steel seamless pipe of the present invention (hereinafter also simply referred to as the seamless steel pipe of the present invention) contains, in mass%, C: 0.005 to 0.100%, Si: 0.05 to 1.00%, Mn: 0.05 to 1.00%, P: 0.05% or less, S: 0.005% or less, Ni: 6.0 to 9.0%, Cr: 15.0 to 17.5%, Al: 0.001 to 0.10%, Nb: 0.001 to 0.20%, N: 0.1% or less, O: 0.01% or less, Cu: 3.5% or less, Mo: less than 1.0%, and W: 1.0% or less, with the balance being Fe and unavoidable impurities, and has a component composition that satisfies the following formulas (1) and (2). 1001-2172C-17.35Cu-44.95Ni-34.45Cr-22.15Mo+60.96Nb-978.3N-18.57W>50.00 (1) Cr+0.65Ni+0.6Mo+0.3W+0.55Cu-20C>20.00 (2) Here, each element symbol in the above formulas (1) and (2) indicates the content (mass%) of the corresponding element, and if no element is contained, it is set to 0.

[0017] The reasons for limiting the chemical composition of the seamless steel pipe of the present invention will be explained below. Hereinafter, unless otherwise specified, mass % will simply be abbreviated as %.

[0018] C: 0.005 to 0.100% C improves hardenability and increases the strength of the steel. To achieve this effect, the C content is set to 0.005% or more. On the other hand, if the C content is too high, the Ms point decreases, martensitic transformation does not occur at room temperature, and strength cannot be ensured. Therefore, the C content is set to 0.100% or less. The C content is preferably 0.007% or more. Furthermore, the C content is preferably 0.050% or less, more preferably 0.030% or less, and even more preferably 0.020% or less.

[0019] Si: 0.05 to 1.00% Si acts as a deoxidizer. To obtain this effect, the Si content is set to 0.05% or more. On the other hand, a Si content exceeding 1.00% reduces corrosion resistance and hot workability due to the precipitation of δ-ferrite. Therefore, the Si content is set to 1.00% or less. The Si content is preferably 0.50% or less. On the other hand, from the viewpoint of ensuring stable strength, the Si content is preferably 0.10% or more.

[0020] Mn: 0.05 to 1.00% Mn is an element that improves hot workability and strength. To achieve this effect, the Mn content is set to 0.05% or more. On the other hand, excessive Mn content causes MnS to precipitate, reducing sulfide stress corrosion cracking resistance. Therefore, the Mn content is set to 1.00% or less. The Mn content is preferably 0.50% or less. Furthermore, the Mn content is preferably 0.10% or more.

[0021] P: 0.05% or less P is an unavoidable impurity. P is an element that reduces corrosion resistance, and in the present invention, it is desirable to reduce it as much as possible. However, an extreme reduction in P increases production costs. Therefore, the P content is limited to 0.05% or less, as a range that does not result in an extreme deterioration in properties and is industrially feasible at low cost. The P content is preferably 0.03% or less. Furthermore, although there is no particular lower limit for the P content, excessive dephosphorization increases production costs, so from the viewpoint of production costs, the P content is preferably 0.005% or more.

[0022] S: 0.005% or less S is an unavoidably contained impurity. Since S is an element that significantly reduces hot workability, it is desirable to reduce it as much as possible. Reducing the S content to 0.005% or less makes it possible to manufacture pipes using the Mannesmann method, so the S content in the present invention is limited to 0.005% or less. The S content is preferably 0.002% or less. Furthermore, although there is no particular restriction on the lower limit of the S content, excessive desulfurization increases manufacturing costs, so from the viewpoint of manufacturing costs, the S content is preferably 0.0005% or more.

[0023] Ni: 6.0 to 9.0% Ni is an element that strengthens the protective coating, improving corrosion resistance, and further increases the strength of the steel by dissolving. Furthermore, since Ni is an element that stabilizes the austenite phase at quenching temperatures, the Ni content is set to 6.0% or more. If the Ni content is less than 6.0%, the amount of ferrite increases and toughness decreases. On the other hand, if the Ni content exceeds 9.0%, the Ms point decreases and strength decreases. Therefore, the Ni content is limited to 6.0 to 9.0%. The Ni content is preferably 6.5% or more. Furthermore, the Ni content is preferably 8.0% or less, and more preferably 7.5% or less.

[0024] Cr: 15.0 to 17.5% Cr is an element that forms a protective film to improve corrosion resistance, and a content of 15.0% or more can achieve the target corrosion resistance. On the other hand, if Cr is contained in excess of 17.5%, the Ms point decreases and the amount of ferrite increases, making it impossible to achieve both strength and low-temperature toughness. Therefore, the Cr content is limited to 15.0 to 17.5%. The Cr content is preferably 15.5% or more, and more preferably 16.0% or more. Furthermore, the Cr content is preferably 17.0% or less.

[0025] Al: 0.001 to 0.10% Al acts as a deoxidizer. To achieve this effect, the Al content is set to 0.001% or more. However, an Al content exceeding 0.10% adversely affects toughness due to the precipitation of excess oxides, so the Al content in the present invention is limited to 0.10% or less. The Al content is preferably 0.01% or more. Furthermore, the Al content is preferably 0.04% or less.

[0026] Nb: 0.001 to 0.20% Nb forms carbides, thereby reducing solute carbon and improving the Ms point. To achieve this effect, the Nb content is set to 0.001% or more. On the other hand, an Nb content of more than 0.20% may precipitate coarse carbides and reduce toughness. Therefore, the Nb content is set to 0.20% or less. The Nb content is preferably 0.01% or more. Furthermore, the Nb content is preferably 0.10% or less.

[0027] N: 0.1% or less N is an unavoidably contained impurity. N has the effect of dissolving in steel and increasing strength. However, if the N content exceeds 0.1%, various nitride-based inclusions are formed in large amounts, reducing corrosion resistance. Therefore, the N content in the present invention is limited to 0.1% or less. The N content is preferably 0.005% or more. The N content is also preferably 0.05% or less, more preferably 0.03% or less.

[0028] O: 0.01% or less O is an unavoidably contained impurity. O exists as an oxide in steel and therefore has an adverse effect on various properties. Therefore, in the present invention, it is desirable to reduce the O content as much as possible. In particular, if the O content exceeds 0.01%, the hot workability, corrosion resistance, and toughness decrease. Therefore, the O content is set to 0.01% or less. The O content is preferably 0.005% or less. There is no particular restriction on the lower limit of the O content, but since excessive deoxidation increases production costs, from the viewpoint of production costs, the O content is preferably set to 0.001% or more.

[0029] Cu: 3.5% or less Cu strengthens the protective coating and improves corrosion resistance. However, a Cu content exceeding 3.5% reduces hot workability due to the precipitation of metallic Cu. Therefore, the Cu content is set to 3.5% or less. The Cu content is preferably 3.0% or less. The seamless steel pipe of the present invention does not necessarily need to contain Cu. The Cu content is preferably 0.5% or more.

[0030] Mo: Less than 1.0% Mo is an element that improves corrosion resistance. On the other hand, an excessive Mo content of 1.0% or more leads to a decrease in the Ms point, which reduces hardenability and makes ferrite more likely to form, thereby reducing toughness. Therefore, in the present invention, the Mo content is limited to less than 1.0%. The Mo content is preferably 0.8% or less. Note that the seamless steel pipe of the present invention does not necessarily need to contain Mo. The Mo content is preferably 0.1% or more.

[0031] W: 1.0% or less W is an element that improves corrosion resistance. On the other hand, an excessive W content of more than 1.0% leads to a decrease in the Ms point, so in the present invention, the W content is limited to 1.0% or less. The W content is preferably 0.8% or less. Note that the seamless steel pipe of the present invention does not necessarily need to contain W. The W content is preferably 0.1% or more.

[0032] The chemical composition of the seamless steel pipe of the present invention further contains each element so as to satisfy the following formula (1): 1001-2172C-17.35Cu-44.95Ni-34.45Cr-22.15Mo+60.96Nb-978.3N-18.57W>50.00 (1) Here, each element symbol in formula (1) indicates the content (mass%) of the corresponding element, and if the element is not contained, it is set to 0. Formula (1) correlates with the Ms point, and when the value calculated on the left side of formula (1) is greater than 50.00, martensitic transformation occurs even when cooled to room temperature, ensuring sufficient strength. Therefore, the value calculated on the left side of formula (1) is set to greater than 50.00. The value calculated on the left side of formula (1) is preferably 55.00 or greater. Furthermore, the value calculated on the left side of formula (1) is preferably 300.00 or less.

[0033] The seamless steel pipe of the present invention further contains each element so as to satisfy the following formula (2): Cr+0.65Ni+0.6Mo+0.3W+0.55Cu-20C>20.00 (2) Here, each element symbol in formula (2) indicates the content (mass%) of the corresponding element, and if the element is not contained, it is set to 0. Formula (2) is an equation relating to corrosion resistance. When the value calculated on the left side of formula (2) exceeds 20.00, the seamless steel pipe can withstand 30 atmospheres of CO 2 When a test piece is immersed in a 20 mass % NaCl aqueous solution at a liquid temperature of 200°C for 336 hours in a gas atmosphere, a corrosion rate of 0.127 mm / y or less can be obtained. Therefore, the value calculated on the left side of equation (2) is set to be greater than 20.00. The value calculated on the left side of equation (2) is preferably 20.50 or more, and more preferably 21.00 or more. Furthermore, because excessive alloy addition promotes the precipitation of intermetallic compounds, the value calculated on the left side of equation (2) is preferably 30.00 or less.

[0034] The balance other than the above components may be Fe and unavoidable impurities.

[0035] The chemical composition of the seamless steel pipe of the present invention may further contain, as optional elements, one or more selected from Co: 1% or less, V: 0.1% or less, Ti: 0.1% or less, Zr: 0.2% or less, Ta: 0.2% or less, Hf: 0.2% or less, Ca: 0.01% or less, REM: 0.01% or less, Mg: 0.01% or less, B: 0.01% or less, Sn: 0.2% or less, and Sb: 0.2% or less. Note that the chemical composition of the seamless steel pipe of the present invention may not contain these optional elements (it may be 0%).

[0036] Co: 1% or less Co is an element that improves corrosion resistance and hardenability. On the other hand, a Co content exceeding 1% reduces low-temperature toughness. Therefore, when Co is contained, the Co content is set to 1% or less. The Co content is preferably 0.5% or less. Furthermore, when Co is contained, the Co content is preferably 0.01% or more.

[0037] V: 0.1% or less V is an element that increases the strength of steel through precipitation strengthening. On the other hand, a V content exceeding 0.1% reduces low-temperature toughness. Therefore, when V is contained, the V content is set to 0.1% or less. The V content is preferably 0.08% or less. Furthermore, when V is contained, the V content is preferably 0.01% or more.

[0038] Ti: 0.1% or less Ti is an element that forms carbonitrides and increases the strength of steel. On the other hand, a Ti content exceeding 0.1% reduces low-temperature toughness. Therefore, when Ti is contained, the Ti content is set to 0.1% or less. The Ti content is preferably 0.02% or less. Furthermore, when Ti is contained, the Ti content is preferably 0.001% or more.

[0039] Zr: 0.2% or less Zr is an element that forms carbonitrides and increases the strength of steel. On the other hand, a Zr content exceeding 0.2% reduces low-temperature toughness. Therefore, when Zr is contained, the Zr content is set to 0.2% or less. The Zr content is preferably 0.15% or less. Furthermore, when Zr is contained, the Zr content is preferably 0.01% or more.

[0040] Ta: 0.2% or less Ta is an element that forms carbonitrides and increases the strength and corrosion resistance of steel. On the other hand, a Ta content of more than 0.2% reduces low-temperature toughness. Therefore, when Ta is contained, the Ta content is set to 0.2% or less. The Ta content is preferably 0.15% or less. Furthermore, when Ta is contained, the Ta content is preferably 0.01% or more.

[0041] Hf: 0.2% or less Hf is an element that forms carbonitrides and increases the strength of steel. On the other hand, a Hf content exceeding 0.2% reduces low-temperature toughness. Therefore, when Hf is contained, the Hf content is set to 0.2% or less. The Hf content is preferably 0.15% or less. Furthermore, when Hf is contained, the Hf content is preferably 0.01% or more.

[0042] Ca: 0.01% or less Ca is an element that improves the hot workability of steel by fixing S in the steel as sulfides. On the other hand, a Ca content exceeding 0.01% coarsens inclusions, reducing toughness and corrosion resistance. Therefore, when Ca is contained, the Ca content is set to 0.01% or less. The Ca content is preferably 0.005% or less. Furthermore, when Ca is contained, the Ca content is preferably 0.0001% or more.

[0043] REM: 0.01% or less. REM (rare earth metal) is an element that improves the hot workability of steel by fixing S in the steel as sulfides. On the other hand, a REM content exceeding 0.01% coarsens inclusions, reducing toughness and corrosion resistance. Therefore, when REM is contained, the REM content is set to 0.01% or less. The REM content is preferably 0.005% or less. Furthermore, when REM is contained, the REM content is preferably 0.0001% or more. In the present invention, REM refers collectively to 17 elements, including Sc (atomic number 21), Y (atomic number 39), and 15 elements from La (atomic number 57) to Lu (atomic number 71). Furthermore, the REM content refers to the total content of these elements.

[0044] Mg: 0.01% or less Mg is an element that improves the hot workability of steel by fixing S in the steel as sulfides. On the other hand, a Mg content exceeding 0.01% coarsens inclusions, reducing toughness and corrosion resistance. Therefore, when Mg is contained, the Mg content is set to 0.01% or less. The Mg content is preferably 0.005% or less. Furthermore, when Mg is contained, the Mg content is preferably 0.0001% or more.

[0045] B: 0.01% or less B is an element that improves the hot workability of steel by suppressing the segregation of S to grain boundaries in the steel material. On the other hand, a B content exceeding 0.01% forms coarse nitrides, reducing the toughness of the steel. Therefore, when B is contained, the B content is set to 0.01% or less. The B content is preferably 0.005% or less. Furthermore, when B is contained, the B content is preferably 0.0001% or more.

[0046] Sn: 0.2% or less Sn is an element that enhances the corrosion resistance of steel. On the other hand, a Sn content exceeding 0.2% reduces the hot workability of steel. Therefore, when Sn is contained, the Sn content is set to 0.2% or less. The Sn content is preferably 0.1% or less. Furthermore, when Sn is contained, the Sn content is preferably 0.01% or more.

[0047] Sb: 0.2% or less Sb is an element that improves the corrosion resistance of steel. On the other hand, an Sb content exceeding 0.2% reduces the hot workability of steel. Therefore, when Sb is contained, the Sb content is set to 0.2% or less. The Sb content is preferably 0.1% or less. Furthermore, when Sb is contained, the Sb content is preferably 0.01% or more.

[0048] Next, a preferred method for manufacturing the seamless steel pipe of the present invention will be described. In the present invention, a steel pipe material having the above-mentioned chemical composition is used, but the method for manufacturing the seamless steel pipe does not need to be particularly limited, and any known method for manufacturing a seamless steel pipe can be used, for example. It is preferable to melt molten steel having the above-mentioned chemical composition using a melting method such as a converter, and form it into a steel pipe material such as a billet using a method such as a continuous casting method or an ingot-making and blooming rolling method. Next, the steel pipe material is heated and hot worked and formed into a pipe in a pipe-making process using a Mannesmann plug mill method or a Mannesmann mandrel mill method, which are known pipe-making methods, and then quenched and tempered to form a seamless steel pipe having the above-mentioned chemical composition.

[0049] The microstructure of the seamless steel pipe of the present invention has martensite as the main phase. In this specification, having martensite as the main phase means that the volume fraction of martensite in the microstructure is 60% or more. The balance can be one or two selected from a volume fraction of 0 to 40% retained austenite and a volume fraction of 0 to 10% ferrite. The volume fraction of martensite is preferably 80% or more, and more preferably 90% or more. The microstructure of the seamless steel pipe of the present invention may be a single martensite phase.

[0050] The seamless steel pipe of the present invention preferably has a yield strength of 758 MPa or more. The yield strength is more preferably 792 MPa or more, and even more preferably 827 MPa or more. Although not particularly limited, as an example, the yield strength is 1034 MPa or less.

[0051] The seamless steel pipe of the present invention preferably has an absorbed energy of 100 J or more in a Charpy impact test at −80° C. The absorbed energy is preferably 150 J or more, and more preferably 180 J or more.

[0052] 50 kg of molten steel having the chemical composition shown in Table 1 was melted in a vacuum furnace, and an ingot was produced by ingot casting. The following processing was then carried out, simulating the manufacturing process of a martensitic stainless steel seamless pipe. The ingot was heated at 1250°C for 60 minutes and rolled to a thickness of 105 mm. It was then heated again at 1250°C for 60 minutes and rolled to a thickness of 15 mm to produce a plate. The plate was quenched by heating at 1000°C for 20 minutes and then water-cooled to 25°C, and then tempered by heating at 570°C for 30 minutes and then air-cooled to room temperature, to obtain a test material (plate).

[0053] Tensile test: A round bar tensile test specimen with a parallel portion diameter of 6 mm and a parallel portion length of 25 mm was taken from the center of the plate thickness of each test material (corresponding to the center of the wall thickness of a seamless steel pipe) in accordance with API regulations. The longitudinal direction of the parallel portion of this test specimen was the rolling direction of the plate material. Using this test specimen, a tensile test was performed at room temperature (25°C) to determine the yield strength YS (MPa). The yield strength YS was defined as the 0.2% proof stress. A yield strength YS of 758 MPa or more was considered to be pass, and a yield strength YS of less than 758 MPa was considered to be fail.

[0054] Impact test: V-notch test pieces (full size) were taken from the center of the plate thickness of each test material so that the longitudinal direction of the test piece was perpendicular to the rolling direction, and a Charpy impact test was performed in accordance with the provisions of JIS Z 2242: 2018. The test temperature was -80 ° C, and those with an absorbed energy of 100 J or more were considered to have passed, and those with an absorbed energy of less than 100 J were considered to have failed.

[0055] Corrosion Resistance Test: A test specimen measuring 30 mm x 40 mm x 3 mm was taken from each test material. The test specimen was immersed in a test liquid held in an autoclave: a 20 mass% NaCl aqueous solution (liquid temperature: 200°C, CO 30 atmospheres) 2 The corrosion test was performed by immersing the specimens in a gas atmosphere for 336 hours. After the test, the specimens were weighed, and the corrosion rate was calculated from the difference in weight before and after the corrosion test. A corrosion rate of 0.127 mm / y or less was deemed to be acceptable, and a corrosion rate of more than 0.127 mm / y was deemed to be unacceptable.

[0056] Microstructural observation: Test specimens for microstructural observation and X-ray diffraction were taken from the center of the plate thickness (corresponding to the center of the wall thickness of a seamless steel pipe) from each test material. A cross section of the test specimen for microstructural observation, perpendicular to the longitudinal direction (rolling direction) of the steel material, was etched using a Villela etching solution. The cross section was then observed using an optical microscope at an appropriate magnification between 100 and 1000 times. The obtained images were analyzed to calculate the area fraction of the ferrite phase. This area fraction was considered to be the volume fraction of the ferrite phase. The volume fraction of the retained austenite phase was determined by X-ray diffraction after chemically polishing a cross section of the X-ray diffraction test specimen perpendicular to the thickness direction of the steel material. A Co-Kα radiation source was used for incident X-rays, and the area fraction of the retained austenite phase was calculated from the intensity ratio of the (200) and (211) planes of ferrite to the (200), (220), and (311) planes of austenite. This area ratio was regarded as the volume ratio of the retained austenite phase. The results are shown in Table 2. In Table 2, the remainder other than the ferrite phase and the retained austenite phase was regarded as the martensite phase. In the present invention, the martensite phase may contain a precipitate phase in a volume ratio of 5% or less in addition to the ferrite phase and the retained austenite phase.

[0057]

[0058]

[0059] All of the examples of the present invention have high strength with a yield strength YS of 758 MPa or more, high toughness with an absorbed energy of 100 J or more in a Charpy impact test at -80°C, and 2 , Cl - The samples had excellent corrosion resistance in a high-temperature corrosive environment containing ions at 200°C. On the other hand, the comparative examples outside the scope of the present invention did not achieve the desired values ​​for at least one of the yield strength YS, absorbed energy in a Charpy impact test at -80°C, and corrosion resistance.

[0060] The embodiments of the present invention have been described above. However, the above-described embodiments are merely examples for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiments, and the above-described embodiments can be appropriately modified and carried out without departing from the spirit of the present invention.

[0061] The martensitic stainless steel seamless pipe of the present invention is useful as oil country tubular goods and CCS press-in pipes, which require high strength, excellent low-temperature toughness, and excellent corrosion resistance, and is particularly suitable as CCS press-in pipes.

Claims

1. A martensitic stainless steel seamless pipe containing, by mass, the following: C: 0.005-0.100%, Si: 0.05-1.00%, Mn: 0.05-1.00%, P: 0.05% or less, S: 0.005% or less, Ni: 6.0-9.0%, Cr: 15.0-17.5%, Al: 0.001-0.10%, Nb: 0.001-0.20%, N: 0.1% or less, O: 0.01% or less, Cu: 3.5% or less, Mo: less than 1.0%, and W: 1.0% or less, with the balance being Fe and unavoidable impurities, and having a component composition that satisfies the following formulas (1) and (2). 1001-2172C-17.35Cu-44.95Ni-34.45Cr-22.15Mo+60.96Nb-978.3N-18.57W>50.00 ... (1) Cr+0.65Ni+0.6Mo+0.3W+0.55Cu-20C>20.00 ... (2) Here, each element symbol in formula (1) and formula (2) indicates the content (mass%) of the corresponding element, and 0 is set when the element is not contained.

2. A martensitic stainless steel seamless steel pipe as described in claim 1, wherein the chemical composition further contains, in mass%, one or more elements selected from the following: Co: 1% or less, V: 0.1% or less, Ti: 0.1% or less, Zr: 0.2% or less, Ta: 0.2% or less, Hf: 0.2% or less, Ca: 0.01% or less, REM: 0.01% or less, Mg: 0.01% or less, B: 0.01% or less, Sn: 0.2% or less, and Sb: 0.2% or less.

3. A martensitic stainless steel seamless pipe as claimed in claim 1 or 2, having a yield strength of 758 MPa or more and an absorbed energy in a Charpy impact test at -80°C of 100 J or more.

Citation Information

Patent Citations

  • Stainless steel for oil well and stainless steel pipe for oil well

    JP2017014543A

  • Martensitic stainless-steel seamless pipe for oil well pipe and process for producing the same

    WO2009004741A1

  • High strength stainless seamless steel pipe for oil wells, and method for producing same

    WO2019035329A1

  • Stainless seamless steel pipe

    WO2020202957A1

  • Martensitic welded stainless steel pipe and producing method therefor

    JP2001179485A

Cited By

  • Stainless steel

    JP2025110965A

  • Stainless Steel

    JP7678375B1