Method for processing lithium-ion battery waste
The method improves the recovery rate of cobalt and nickel from lithium-ion battery waste by using ammonia and amine compounds in wet processing, followed by solid-liquid separation with specific acids, effectively reducing unwanted metal residues and achieving high recovery rates of cobalt and nickel.
Patent Information
- Application Number
- PCT/JP2024/014200
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-04-08
- Publication Date
- 2024-11-21
AI Technical Summary
Existing methods for recovering valuable metals like cobalt and nickel from lithium-ion battery waste face inefficiencies in removing aluminum and iron, leading to suboptimal leaching rates and co-recovery of undesired metals.
A method involving wet processing of lithium-ion battery waste with ammonia and amine compounds, followed by solid-liquid separation, using specific acids and chelate amine compounds to selectively dissolve and separate cobalt and nickel, while removing aluminum, iron, and manganese.
This approach enhances the recovery rate of cobalt and nickel to 50% or more, significantly reducing the residual rates of unwanted metals like aluminum, iron, and manganese, enabling selective recovery of valuable metals.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
How to dispose of lithium-ion battery waste
[0001] The present invention relates to a method for treating lithium ion battery waste.
[0002] From the perspective of the SDGs, the recovery and reuse of valuable metals such as cobalt and nickel from lithium-ion battery waste is being widely considered.
[0003] To recover valuable metals such as cobalt and nickel from lithium-ion battery waste, the lithium-ion battery waste is roasted, crushed, and other processes. The resulting lithium-ion battery powder is added to an acidic solution to obtain a leachate containing dissolved lithium, copper, cobalt, nickel, iron, aluminum, manganese, and other metals. Next, solid-liquid separation and solvent extraction are repeatedly performed to obtain a solution containing the desired valuable metals, such as cobalt and nickel. Finally, nickel and cobalt are recovered from each solution by electrolysis or other methods.
[0004] For example, Patent Document 1 listed below describes a method for treating lithium ion battery waste, which includes a first-stage neutralization step in which an acidic solution obtained by subjecting lithium ion battery waste to wet processing and in which at least cobalt, nickel, manganese, and aluminum are dissolved is neutralized to a pH of 4.0 to 6.0, a portion of the aluminum is precipitated, and the portion of the aluminum is removed by solid-liquid separation; and a second-stage neutralization step in which, after the first-stage neutralization step, the pH is neutralized to 11.0 or higher, the remainder of the aluminum is left in the liquid, and a neutralization residue containing cobalt, nickel, and manganese is obtained by solid-liquid separation.
[0005] Japanese Patent Application Laid-Open No. 2020-180362
[0006] The present inventors have conducted extensive research into the treatment method described in Patent Document 1 and have found that it is difficult to efficiently remove aluminum and iron, which are the targets of removal, from the leachate, and that there is room for further improvement in order to leach desired valuable metals such as nickel and cobalt at a high leaching rate.
[0007] In view of the above, an object of the present invention is to provide a method for treating lithium ion battery waste that has an excellent recovery rate of desired valuable metals such as nickel and cobalt.
[0008] The above-mentioned problems can be solved by the following configuration: That is, the present invention relates to a method for treating lithium-ion battery waste by wet treating the lithium-ion battery waste to obtain a leachate in which at least cobalt and nickel are dissolved, the method comprising: a wet treatment step of adding at least one compound (1) selected from the group consisting of ammonia and its salts, and amine compounds and their salts to the lithium-ion battery waste and mixing them to obtain the leachate in which at least the cobalt and the nickel are dissolved; and a solid-liquid separation step of removing at least a portion of the metal that is not dissolved in the leachate by solid-liquid separation after the wet treatment step.
[0009] In the method (1) for treating lithium ion battery waste, a method (2) for treating lithium ion battery waste is preferred, in which an acid is added in addition to the compound (1) in the wet treatment step, and the mixture is mixed.
[0010] In the above-mentioned method (2) for treating lithium ion battery waste, a method (3) for treating lithium ion battery waste is preferred, in which the acid is at least one compound (2) selected from the group consisting of monocarboxylic acid-based organic acids and inorganic acids.
[0011] In any of the above-mentioned methods for treating lithium ion battery waste (1) to (3), a method for treating lithium ion battery waste (4) is preferred, in which the compound (1) is at least one compound selected from the group consisting of amine compounds having an amino group and salts thereof.
[0012] In any of the above-mentioned methods for treating lithium ion battery waste (1) to (4), a method for treating lithium ion battery waste (5) is preferred, in which the compound (1) is at least one compound selected from the group consisting of chelate amine compounds having two or more amino groups and salts thereof.
[0013] In any of the above-mentioned methods for treating lithium-ion battery waste (1) to (5), the lithium-ion battery waste contains aluminum, and in the solid-liquid separation step, at least a part of the aluminum is removed.
[0014] In any of the above-mentioned methods for treating lithium-ion battery waste (1) to (6), the lithium-ion battery waste contains iron, and in the solid-liquid separation step, at least a part of the iron is removed.
[0015] In any of the above-mentioned methods for treating lithium-ion battery waste (1) to (7), the lithium-ion battery waste contains manganese, and in the solid-liquid separation step, at least a part of the manganese is removed.
[0016] The method for treating lithium ion battery waste according to the present invention includes a wet treatment step in which at least one compound selected from the group consisting of ammonia and its salts, and amine compounds and their salts is added and mixed to obtain a leachate in which at least cobalt and nickel are dissolved. This makes it possible to remove aluminum, iron, manganese, and other elements other than at least cobalt and nickel that are not the target of recovery by a simple operation such as solid-liquid separation, and therefore makes it possible to recover desired valuable metals such as nickel and cobalt at a high recovery rate.
[0017] The present invention provides a method for treating lithium ion battery waste, which involves wet treating the lithium ion battery waste to obtain a leachate containing at least cobalt and nickel dissolved therein, and which includes at least a wet treatment step and a solid-liquid separation step.
[0018] Lithium-ion battery waste is waste from lithium-ion batteries used in various devices such as electric vehicles, mobile phones, and personal computers. Lithium-ion batteries typically consist of a positive electrode with lithium cobalt oxide as the main active material, a negative electrode with special carbon as the main active material, a separator, and other components stacked or spirally wound together while containing an electrolyte, and then placed inside an exterior material such as aluminum.
[0019] Lithium-ion battery waste is usually subjected to pretreatment such as roasting and crushing before the wet treatment step. In the roasting step, the lithium-ion batteries are heated and held at a temperature in the range of 500 to 1000°C for several hours. The heating and holding may be carried out in a furnace or in the air. In the crushing step, a crusher such as a sample mill, hammer mill, or hammer crusher is used. In the present invention, pretreatment other than roasting and crushing may be carried out before the wet treatment step, as necessary. For example, lithium-ion battery waste may be converted into finely powdered lithium-ion battery powder through pretreatment such as roasting and crushing, and then the lithium-ion battery powder may be contacted with, for example, ion-exchanged water to recover a certain amount of lithium from the lithium-ion battery powder.
[0020] Lithium-ion battery waste contains lithium, copper, cobalt, nickel, iron, aluminum, manganese, and other metals. The concentrations of each metal contained in lithium-ion battery waste can be measured, for example, by the following method. Specifically, lithium-ion battery waste is subjected to pretreatment such as roasting and pulverization to produce a finely powdered lithium-ion battery powder. The lithium-ion battery powder is then added to, for example, aqua regia (a solution of hydrochloric acid and nitric acid in a ratio of 3:1) to obtain a leachate containing dissolved lithium, copper, cobalt, nickel, iron, aluminum, manganese, and other metals. The leachate is preferably prepared by leaching lithium-ion battery powder with an acidic solution such as aqua regia. The pH of the leachate after the addition of aqua regia is preferably 0.0 to 1.0. Examples of conditions for obtaining the leachate include adding 1.0 to 10.0 g of lithium-ion battery powder per 50.0 to 500.0 g of aqua regia, and leaching at 25 to 80°C for 1 to 72 hours with a stirring speed of 250 to 1500 rpm. After leaching, solid-liquid separation is performed using a suction filter or the like, and the concentration of each metal in the resulting filtrate is measured. The concentration of each metal in the leachate can be measured, for example, using an ICP optical emission spectrometer (ICP-OES). In the present invention, the recovery rates of cobalt, nickel, and the like are calculated based on the leachate (filtrate) after adding aqua regia to the lithium-ion battery waste. This point will be described later.
[0021] (Wet Treatment Step) In the wet treatment step, at least one compound (1) selected from the group consisting of ammonia and its salts, and amine compounds and their salts is added to and mixed with lithium ion battery waste to obtain a leachate in which at least cobalt and nickel are dissolved.
[0022] Compound (1) is at least one compound selected from the group consisting of ammonia and its salts, and amine compounds and their salts. Examples of ammonia salts (ammonium salts) include ammonium chloride. Examples of amine compounds include ethylenediamine, tris(2-ethylamino)amine, imidazole, 2-piperazine, triethanolamine, L-lysine, and aminoguanidine. Examples of amine compound salts include ethylenediamine dihydrochloride, 2-piperazine hydrochloride, 2-piperazine hydrochloride monohydrate, cysteamine hydrochloride, triethanolamine hydrochloride, L-lysine hydrochloride, and aminoguanidine hydrochloride. Ammonia and its salts, and amine compounds and their salts may be used alone or in combination. For example, an ammonium salt may be combined with ammonia, or an amine compound salt may be combined with ammonia. More specifically, for example, a combination of ammonium chloride and ammonia may be used, a combination of 2-piperazine hydrochloride monohydrate and ammonia may be used, a combination of cysteamine hydrochloride and ammonia may be used, a combination of ethylenediamine dihydrochloride and ammonia may be used, a combination of triethanolamine hydrochloride and ammonia may be used, a combination of L-lysine hydrochloride and ammonia may be used, or a combination of aminoguanidine hydrochloride and ammonia may be used.
[0023] In the present invention, among the compounds (1), at least one compound selected from the group consisting of amine compounds having an amino group and salts thereof is preferred, and at least one compound selected from the group consisting of chelating amine compounds having two or more amino groups and salts thereof is more preferred. Specifically, for example, ethylenediamine, tris(2-ethylamino)amine, 2-piperazine hydrochloride monohydrate, ethylenediamine dihydrochloride, and L-lysine hydrochloride are preferably used, since they can further increase the recovery rate of desired valuable metals such as nickel and cobalt.
[0024] To increase the recovery rate of desired valuable metals such as nickel and cobalt, the wet treatment step preferably involves adding an acid to the lithium-ion battery waste in addition to compound (1) and mixing the mixture to remove at least a portion of the metals other than cobalt and nickel. It is even more preferable to add at least one compound (2) selected from the group consisting of monocarboxylic organic acids and inorganic acids as the acid and mix the mixture to remove at least a portion of the metals other than cobalt and nickel. Examples of monocarboxylic organic acids include formic acid and acetic acid. Examples of inorganic acids include hydrochloric acid and hydrobromic acid.
[0025] When compound (2) is added in addition to compound (1) in the wet treatment step, the molar ratio of compound (2):compound (1) is preferably 1:1 to 1:6, more preferably 1:1 to 1:2. By setting the ratio within this range, the recovery rate of desired valuable metals such as nickel and cobalt can be further increased.
[0026] To increase the recovery rate of desired valuable metals such as nickel and cobalt, the pH of the leachate after addition of compound (1) alone or after addition of compound (1) and compound (2) in the hydroprocessing step is preferably adjusted to 3.0 to 12.5, more preferably 9.5 to 11.0. The temperature of the leachate is preferably set to 25 to 80°C, and the leachate is preferably stirred at a stirring speed of 500 to 1,000 rpm for 8 to 24 hours.
[0027] (Solid-Liquid Separation Step) A method for removing at least a portion of the insoluble metals from the leachate obtained in the wet treatment step includes, for example, a method of separating the leachate containing at least cobalt and nickel dissolved therein from the target precipitates, such as aluminum and iron, by solid-liquid separation. The method for treating lithium-ion battery waste according to the present invention makes it possible to recover desired valuable metals, such as nickel and cobalt, at a high recovery rate. Specifically, for example, when a solid-liquid separation step is performed after the wet treatment step, the recovery rate of the cobalt and nickel obtained thereafter is 50% or more, and more preferably 70% or more. In the present invention, the recovery rates of cobalt, nickel, and the like can be calculated using the following formula (1): (Recovery rate (%) of each metal) = (Metal concentration in the leachate (filtrate) obtained after the wet treatment step) / (Metal concentration in the leachate (filtrate) after adding aqua regia to the lithium-ion battery waste) × 100 ... Formula (1)
[0028] In the method for treating lithium-ion battery waste according to the present invention, when the lithium-ion battery waste contains aluminum, removing at least a portion of the aluminum in the solid-liquid separation step is preferable because the aluminum recovery rate calculated by formula (1) is low, i.e., the amount of remaining aluminum is small. Specifically, for example, the aluminum remaining rate after the wet treatment step is 30% or less, and more preferably 10% or less.
[0029] In the method for treating lithium-ion battery waste according to the present invention, when the lithium-ion battery waste contains iron, removing at least a portion of the iron in the solid-liquid separation step is preferable because the iron recovery rate calculated by formula (1) is low, i.e., the residual iron rate is low. Specifically, for example, the residual iron rate after the wet treatment step is 30% or less, and more preferably 10% or less.
[0030] In the method for treating lithium-ion battery waste according to the present invention, the lithium-ion battery waste contains manganese, and removing at least a portion of the manganese in the solid-liquid separation step is preferable because the manganese recovery rate calculated by formula (1) is low, that is, the manganese residual rate is low. Specifically, for example, the manganese residual rate after the wet treatment step is 30% or less, and more preferably 10% or less.
[0031] The method for treating lithium-ion battery waste according to the present invention is preferable because, even when the lithium-ion battery waste contains lithium, the recovery rate of lithium calculated by formula (1) in the solid-liquid separation step is relatively high. Specifically, for example, the recovery rate of lithium after the wet treatment step is 10% or more, and more preferably 35% or more.
[0032] The method for treating lithium-ion battery waste according to the present invention is preferable because, even when the lithium-ion battery waste contains copper, the recovery rate of copper calculated by formula (1) in the solid-liquid separation step is relatively high. Specifically, for example, the recovery rate of copper after the wet treatment step is 10% or more, and more preferably 35% or more.
[0033] In the method for treating lithium-ion battery waste according to the present invention, if a solid-liquid separation step is performed after the wet treatment step, the recovery rate of cobalt and nickel among the metals contained in the leachate (filtrate) obtained thereafter is high, and the remaining rate of unnecessary metals, particularly aluminum and iron, is low. Therefore, the method for treating lithium-ion battery waste according to the present invention is particularly useful as a method for recovering cobalt and nickel from lithium-ion battery waste. For example, by performing an extraction operation using an extractant known to those skilled in the art, it is possible to recover only cobalt or only nickel from the filtrate finally obtained after the wet treatment step.
[0034] An example of an embodiment of the present invention will be described below, but the present invention is not limited to this description in any way.
[0035] (Measurement of the concentration of each metal contained in lithium-ion battery waste) 1.0 g of lithium-ion battery powder obtained by roasting and crushing lithium-ion battery waste was added to 50.0 g of aqua regia (hydrochloric acid / nitric acid = 3 / 1), and mixed at 25°C for 24 hours at a stirring speed of 500 to 750 rpm to obtain a leachate. Solid-liquid separation of the leachate was performed using a suction filter, and the metal concentration of the obtained filtrate was measured. ICP was used to measure the metal concentration. The results are shown in Table 1.
[0036]
[0037] (Wet Treatment Step / Solid-Liquid Separation Step) 1.0 g of lithium ion battery powder was added to and mixed with 50.0 g of treated water. The treated water consisted of ion-exchanged water and compound (1) alone, or ion-exchanged water, compound (1), and compound (2) adjusted in the ratios shown in Tables 2 and 3. The lithium battery powder and treated water were mixed at 25°C for 24 hours at a stirring speed of 500 to 750 rpm (wet treatment step), followed by solid-liquid separation using a suction filter (solid-liquid separation step), and the metal concentrations of the resulting filtrate were measured. ICP was used to measure the concentrations. The results are shown in Tables 2 and 3. The recovery rates of each metal in Tables 2 and 3 were calculated using the formula (1) and evaluated according to the following criteria.
[0038] The recovery rate of target metals (cobalt (Co) and nickel (Ni)) was evaluated as "Good" if it was 70% or more, "Good" if it was 50% or more but less than 70%, and "Poor" if it was 50% or less. The recovery rate of non-target metals (iron (Fe), aluminum (Al), and manganese (Mn)) was evaluated as "Good" if it was 10% or less, "Good" if it was 10% or more but less than 30%, and "Poor" if it was 30% or more. Note that the higher the recovery rate of non-target metals, the more likely they are to remain in the filtrate and be recovered together with the target metals, which is undesirable because it means that the target metals are not selectively recovered. The recovery rate of other metals (lithium (Li) and copper (Cu)) was evaluated as "Good" if it was 35% or more, "Good" if it was 10% or more but less than 35%, and "Poor" if it was 10% or less.
[0039]
[0040] Comparative Examples 1-3 are conventional treatment methods using organic or inorganic acids, and not only the target metals cobalt and nickel but also the non-target metals aluminum, iron, and manganese are simultaneously recovered, indicating that cobalt and nickel cannot be selectively recovered. On the other hand, Examples 1-9 are treatment methods for lithium-ion battery waste according to the present invention, and indicate that the target metals cobalt and nickel can be selectively recovered while reducing the recovery rates of the non-target metals aluminum, iron, and manganese. In particular, Examples 3, 4, 6, and 8, which used a chelating amine compound having two or more amino groups as compound (1) and a monocarboxylic acid organic acid or inorganic acid as compound (2), showed particularly excellent recovery rates of desired valuable metals such as nickel and cobalt.
[0041]
[0042] Examples 10-19 show the method for treating lithium-ion battery waste according to the present invention, which demonstrates that the recovery rates of target metals, cobalt and nickel, can be selectively recovered while reducing the recovery rates of metals not targeted for recovery, such as aluminum, iron, and manganese. In particular, Example 10, which used ammonium chloride in combination with ammonia, Example 12, which used 2-piperazine hydrochloride monohydrate in combination with ammonia, Example 13, which used cysteamine hydrochloride in combination with ammonia, Example 15, which used ethylenediamine dihydrochloride in combination with ammonia, and Example 18, which used L-lysine hydrochloride in combination with ammonia, all showed particularly excellent recovery rates of desired valuable metals, such as nickel and cobalt.
Claims
1. A method for treating lithium ion battery waste, which comprises wet treating the lithium ion battery waste to obtain a leachate in which at least cobalt and nickel are dissolved, the method comprising: a wet treatment step of adding at least one compound (1) selected from the group consisting of ammonia and its salts, and amine compounds and their salts to the lithium ion battery waste and mixing the resulting leachate in which at least the cobalt and the nickel are dissolved; and a solid-liquid separation step of removing at least a portion of the metal that is not dissolved in the leachate by solid-liquid separation after the wet treatment step.
2. The method for treating lithium ion battery waste according to claim 1, wherein in the wet treatment step, an acid is added in addition to the compound (1) and mixed.
3. The method for treating lithium ion battery waste according to claim 2, wherein the acid is at least one compound (2) selected from the group consisting of monocarboxylic organic acids and inorganic acids.
4. The method for treating lithium ion battery waste according to claim 1, wherein the compound (1) is at least one compound selected from the group consisting of amine compounds having an amino group and salts thereof.
5. A method for treating lithium ion battery waste according to claim 1, wherein the compound (1) is at least one compound selected from the group consisting of chelating amine compounds having two or more amino groups and salts thereof.
6. A method for treating lithium ion battery waste as described in claim 1, wherein the lithium ion battery waste contains aluminum, and at least a portion of the aluminum is removed in the solid-liquid separation step.
7. A method for treating lithium ion battery waste as described in claim 1, wherein the lithium ion battery waste contains iron, and at least a portion of the iron is removed in the solid-liquid separation step.
8. A method for treating lithium ion battery waste as described in claim 1, wherein the lithium ion battery waste contains manganese, and at least a portion of the manganese is removed in the solid-liquid separation step.
Citation Information
Patent Citations
Method for treating lithium-ion battery waste and method for producing sulfate
JP2020180362A
Method for extracting lithium from lithium containing ore
CN108277367A
Method for separating cobalt from material containing cobalt and nickel
CN109468472A
Preparation method of nickel-cobalt binary oxide positive electrode material precursor of lithium-ion battery
CN111129488A
Process for recycling waste lithium batteries
CN111600090A