Method for dispersing organic modified nanoparticles in solvent, and liquid dispersion of organic modified nanoparticles

By adding a molecule with a smaller van der Waals volume as a third component and applying pressure, organically modified nanoparticles can be dispersed in solvents with large molecular weights, overcoming aggregation issues and enhancing solvent selection options.

WO2024237072A1PCT designated stage expired Publication Date: 2024-11-21TOHOKU UNIV +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016455
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-04-26
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional methods struggle to disperse organically modified nanoparticles in solvents with large molecular weights due to poor chemical affinity and high surface energy, leading to aggregation and limited solvent selection options.

Method used

Incorporating a specific molecule as a third component with a smaller van der Waals volume than the solvent and organic modifying group, which coordinates with the nanoparticles to increase the free volume of the organic layer, improving the affinity with the solvent and preventing aggregation, and applying pressure to enhance dispersion.

Benefits of technology

This approach allows for the effective dispersion of organically modified nanoparticles in solvents with large molecular weights, increasing the degree of freedom in solvent selection and maintaining dispersibility for an extended period.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016455_21112024_PF_FP_ABST
    Figure JP2024016455_21112024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To enable organic modified nanoparticles to be dispersed even in a solvent having a relatively high molecular weight, and to enable an increase in the freedom of choice of solvents. [Solution] The present invention is a method for dispersing organic modified nanoparticles in a solvent, and includes a dispersion step for dispersing organic modified nanoparticles, each having an organic modification group on the surface thereof, in a solvent. The solvent comprises: a poorly dispersible solvent which is poorly dispersible with respect to the organic modified nanoparticles; and a predetermined molecule. With respect to the van der Waals volume, the van der Waals volume of the predetermined molecule under a temperature / pressure in a dispersion treatment step is smaller than that of the solvent and is also smaller than that of the organic modification group. With respect to a dispersion force component δD of Hansen solubility parameters, the absolute value of the difference between the value for the organic modified nanoparticles and the value for the predetermined molecule under the above-mentioned pressure is 1.2 MPa1 / 2 or less, and the difference between the value for the organic modified nanoparticles and the value for a poorly dispersible mixture solvent containing the predetermined molecule under the above-mentioned pressure is 1.2 MPa1 / 2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Method for dispersing organically modified nanoparticles in a solvent and organically modified nanoparticle dispersion

[0001] The present invention relates to a method for dispersing organically modified nanoparticles in a solvent and to an organically modified nanoparticle dispersion.

[0002] Fine particles, particularly nanometer-sized particles (nanoparticles), exhibit a variety of unique and excellent properties, characteristics, and functions. They are expected to realize technologies that meet the demands for higher precision, smaller size, and lighter weight for all materials and products. Nanoparticles have thus attracted attention as a promising material for achieving high functionality, high performance, high density, and high precision in industrial and technological materials, such as nanostructure modifiers for ceramics, optical functional coatings, electromagnetic wave shielding materials, secondary battery materials, fluorescent materials, electronic component materials, magnetic recording materials, and abrasives, as well as pharmaceutical and cosmetic materials. Recent fundamental research on nanoparticles has led to a succession of discoveries, including ultra-high functionality and the emergence of new physical properties due to the quantum size effect of nanoparticles, as well as the synthesis of new materials, attracting great interest from the industrial sector.

[0003] To maintain these properties, nanoparticles must maintain their individual structure. However, because nanoparticles are often handled in solvents, it is important to prevent aggregation in the solution phase due to their high surface energy. Controlling the viscosity caused by aggregation will facilitate unit operations of nanoparticles.

[0004] Therefore, there is a method for changing the intermolecular interaction between nanoparticles and a solvent by surface modification of nanoparticles. This method can prevent aggregation by promoting dispersion of nanoparticles in the target solvent. As a method for continuously synthesizing organically modified nanoparticles in large quantities, a recovery or collection method for metal oxide nanoparticles has been proposed (Patent Document 1). This method involves using high-temperature, high-pressure water as a reaction field to react the metal oxide nanoparticle surface with an organic modifier, thereby organically modifying the nanoparticle surface by bonding a hydrocarbon group, which may be substituted or unsubstituted, to the nanoparticle surface via a covalent bond or a bond selected from the group consisting of an ether bond, an ester bond, a bond via an N atom, a bond via an S atom, a metal-C- bond, a metal-C= bond, and a metal-(C=O)- bond. The method is characterized by: (1) precipitating and recovering the metal oxide nanoparticles dispersed in an aqueous solution; (2) transferring the metal oxide nanoparticles dispersed in an aqueous solution into an organic solvent and recovering them; or (3) collecting the metal oxide nanoparticles at the organic solvent phase-aqueous phase interface.

[0005] Patent No. 3925936

[0006] In any dispersion method for organically modified nanoparticles, it is important to increase the affinity between the organic modification group and the solvent. To improve chemical affinity, it is important to reduce the difference in Hansen solubility parameters (HSP) between the organic modification molecule and the solvent molecule. However, this alone does not predict the dispersibility of nanoparticles. Recent research has shown that the molecular volume of the solvent molecule is also an important factor. Furthermore, recent computational science calculations have shown that the formation of a self-ordering structure of the organic modification group ultimately reduces chemical interaction with the solvent.

[0007] Considering these effects, it is understandable that conventional techniques can only disperse organically modified nanoparticles in solvents with high chemical affinity and relatively small molecular weights, but cannot disperse organically modified nanoparticles in solvents with relatively large molecular weights. In other words, there is a need to provide a technique that can disperse organically modified nanoparticles even in solvents with relatively large molecular weights and low dispersibility. If this becomes possible, it will increase the freedom of solvent selection.

[0008] The present invention has been made in view of such problems, and aims to make it possible to disperse organically modified nanoparticles even in solvents with relatively large molecular weights, thereby increasing the degree of freedom in solvent selection.

[0009] As a result of extensive research, the present inventors discovered that organically modified nanoparticles can be dispersed by adding a specific molecule as a third component to a solvent that has a relatively large molecular weight and is difficult to disperse, and this led to the completion of the present invention. Specifically, the present invention provides the following.

[0010] The invention according to a first aspect includes a dispersing step of dispersing organically modified nanoparticles having organic modifying groups on their surfaces in a solvent, the solvent containing a poorly dispersible solvent in which the organically modified nanoparticles are poorly dispersible, and a predetermined molecule as a third component, and the method further includes the step of: dispersing the organically modified nanoparticles in a solvent; and dispersing the organically modified nanoparticles in a solvent containing a poorly dispersible solvent in which the organically modified nanoparticles are poorly dispersible; the method further includes the step of dispersing the organically modified nanoparticles in a solvent containing a poorly dispersible solvent and a predetermined molecule as a third component ... D With respect to the dispersion force term δ of the organic modifying group at the temperature and pressure D and the dispersion force term δ of the given molecule D The absolute value of the difference between the values ​​is 1.2 MPa. 1 / 2 and the dispersion force term δ of the given molecule at the temperature and pressure is less than or equal to D The value of the dispersion force term δ of the poorly dispersible solvent D The absolute value of the difference between the values ​​is 1.2 MPa. 1 / 2The present invention provides a method for dispersing organically modified nanoparticles in a solvent, which method induces an increase in the free volume of the organically modified layer.

[0011] It is not possible to disperse organically modified nanoparticles in a poorly dispersible solvent that does not contain a specific molecule as a third component. This is because the van der Waals volume of the poorly dispersible solvent is larger than the volume of the voids created by the organic modification group, or the free volume of the organic modification layer is too small to contain the solvent molecules, making it impossible to dissolve organically modified nanoparticles easily, or the dispersion force term δ of the Hansen solubility parameters D Regarding the dispersion force term δ of the organic modifying group under the dispersion treatment temperature and pressure D The value of and the dispersion term δ of poorly dispersible solvents D The absolute value of the difference between the values ​​is 1.2 MPa 1 / 2 It means exceeding.

[0012] According to the first aspect of the present invention, the van der Waals volume of the predetermined molecule as the third component is smaller than the van der Waals volume of the solvent and also smaller than the van der Waals volume of the modifying group of the organically modified nanoparticles. Therefore, when the predetermined molecule is added to the solvent, the predetermined molecule coordinates with the modifying group of the organically modified nanoparticles, and the dispersion force terms δ of the mixed solvent and the organically modified nanoparticles are D The absolute value of the difference between the values ​​is 1.2 MPa. 1 / 2 If the third component coordinates to the modified organic molecules, the self-organization of the modified organic molecules can be suppressed, thereby increasing the free volume of the organic molecule layer and promoting the coordination of solvent molecules, thereby dramatically improving the affinity of the organically modified nanoparticles with the solvent.

[0013] According to the first aspect of the invention, organically modified nanoparticles can be dispersed even in solvents with relatively large molecular weights, which results in greater freedom in the selection of solvents.

[0014] The second aspect of the invention provides a method according to the first aspect of the invention, wherein the dispersion step includes a step of accelerating dispersion of the organically modified nanoparticles in the solvent by increasing the concentration of the third component while the organically modified nanoparticles are in the solvent. This method corresponds to providing a method in which, as a pre-processing step of the dispersion step, the organically modified nanoparticles are brought into contact with a high concentration of the third component in advance, thereby enabling good dispersion of the organically modified nanoparticles in the solvent for a certain period of time. In other words, while the first aspect of the invention is an equilibrium-based invention, the second aspect of the invention is an invention relating to a kinetic dispersion step.

[0015] By contacting the organically modified nanoparticles with a high concentration of the third component in advance, the third component is coordinated to the organically modified layer of the organically modified nanoparticles. The dispersion force term δ of the Hansen solubility parameter of the organic modifying group containing the third component is D and the dispersion term δ of the solvent molecules D The absolute value of the difference between the molecular weight and the molecular weight can be significantly reduced, which makes it possible to disperse organically modified nanoparticles in a solvent with a relatively large molecular weight that would otherwise not be able to disperse organically modified nanoparticles.

[0016] In the dispersion step, if a new dispersion solvent or a temperature and pressure different from those in the adjustment step is used, the equilibrium-coordinated third component will be desorbed, diffused, and released, resulting in a decrease in dispersibility. However, since the dispersibility can be maintained within the time constant, the effectiveness of the dispersion step can be improved in a kinetic sense.

[0017] A third aspect of the invention is the method according to the first or second aspect of the invention, wherein the dispersion step includes a step of dispersing the organically modified nanoparticles in the solvent by pressurizing the solvent to a predetermined pressure, and the temperature and pressure of the gas in contact with the surface of the solvent are the predetermined temperature and the predetermined pressure.

[0018] By pressurizing a poorly dispersible solvent and a solvent containing a third component to a predetermined pressure in the presence of a predetermined gas, the gas dissolves in the solvent, and the free volume of the mixed solvent increases compared to before pressure. In addition, the gas is distributed to the modifying groups of the organically modified nanoparticles, increasing the free volume of the organically modified layer and the dispersion force term δ of the Hansen solubility parameter of the modifying group. D and the dispersion term of the mixed solvent δ D The absolute value of the difference between the two also becomes lower. As a result, it becomes possible to disperse organically modified nanoparticles in a solvent that would not normally be able to disperse them. At normal pressure (0.1 MPa), the gas desorbs and diffuses out, but high dispersibility can be maintained for 1 to 14 hours or more.

[0019] A fourth aspect of the invention provides the method according to the third aspect of the invention, wherein the organically modified nanoparticles are purified nanoparticles.

[0020] Generally, in the synthesis process of organically modified nanoparticles, even after the cleaning process, some impurities and unmodified modifying molecules often remain physically adsorbed. However, in the process of the invention relating to the fourth feature, these impurities are replaced and separated by high-pressure gas, thereby significantly reducing the load of the precision cleaning process.

[0021] According to the fourth aspect of the invention, better dispersion is possible than dispersion of poorly purified organically modified nanoparticles, and the dispersed state can be maintained for 14 hours or more even after decompression to normal pressure (0.1 MPa).

[0022] A fifth aspect of the invention provides a method according to the third or fourth aspect of the invention, wherein the predetermined molecule is a gas or liquefied gas selected from carbon dioxide, a hydrocarbon compound, a nitrogen oxide compound, or a chlorofluorocarbon gas, and the predetermined pressure is a pressurized state of 0.5 MPa or more, or a pressure equal to or greater than the saturated vapor pressure at the dispersion treatment temperature (however, if the dispersion treatment temperature is equal to or greater than the critical temperature, the pressure is equal to or greater than the critical pressure).

[0023] A solution containing organically modified nanoparticles may contain impurities or unreacted modifying molecules, which may reduce the dispersibility of the organically modified nanoparticles. According to the fifth aspect of the invention, when the high-pressure gas has sufficient pressure and is in a liquefied gas state or a supercritical fluid at or above its critical pressure, the gas becomes dissolving power, and impurities contained in the solution are extracted by the high-pressure gas such as carbon dioxide, thereby increasing the dispersibility of the organically modified nanoparticles in nonpolar solvents and, as a result, increasing the freedom of solvent selection.

[0024] The sixth aspect of the invention is the invention according to any one of the first to fifth aspects, wherein the solvent is a mixed solvent containing the poorly-dispersible solvent and the specified molecule, the poorly-dispersible solvent is a main solvent, and the specified molecule is a co-solvent.

[0025] The poorly dispersible solvent is poorly dispersible in the organically modified nanoparticles, and the organically modified nanoparticles cannot be dispersed in the poorly dispersible solvent.

[0026] In molecular dissolution systems, the addition of a small amount of co-solvent improves the affinity between the main solvent and the solute, as typified by the entrainer effect. According to the sixth aspect of the invention, the addition of a co-solvent to a poorly dispersible solvent increases the dispersion power term δ of the Hansen solubility parameter of the mixed solvent. D and the dispersion force term δ of the organic modifying group under the dispersion treatment temperature and pressure D The absolute value of the difference with the value of δ becomes smaller. The cosolvent is also coordinated and distributed to the organic modifying group, and the dispersion term δ D The absolute value of the difference is even lower, at 1.2 MPa. 1 / 2 As a result, it becomes possible to disperse organically modified nanoparticles in a solvent that would not normally be able to disperse organically modified nanoparticles.

[0027] According to the sixth feature of the invention, organically modified nanoparticles can be dispersed even in solvents with a relatively large molecular weight and low dispersibility, resulting in increased freedom in solvent selection.

[0028] A seventh aspect of the invention is the invention according to any one of the first to sixth aspects, wherein the organically modified nanoparticles have multiple types of organic modifying groups on their surfaces as the predetermined molecules, and the free volume of the organically modified molecule layer under the temperature and pressure in the dispersion step is larger than the free volume of a single type of organically modified molecule layer, and the free volume of the organically modified molecule layer is smaller than the van der Waals volume of the solvent molecules.

[0029] When there is only one type of modifying group, the controlling factor for the dispersibility of organically modified nanoparticles is the chemical affinity between the solvent molecules and the modifying molecule layer. For example, if the Hansen solubility parameter δ D Even if the absolute value of the difference between the Hansen solubility parameter of the solvent is small, if the van der Waals volume of the solvent is larger than the range in which the organically modified nanoparticles are dispersible, the organically modified nanoparticles cannot be dispersed in the solvent.

[0030] According to the seventh feature of the invention, the dispersibility of the organically modified nanoparticles is further determined by controlling the free volume of the organically modified layer.

[0031] When the surface is modified with multiple types of organic modifiers, and the van der Waals volumes of the first and second modifying groups are larger than the van der Waals volume of the solvent, and the volume of the void (molecular pocket) formed between these modifying groups or other modifying groups is larger than the van der Waals volume of the solvent, solvent molecules with large van der Waals volumes are also incorporated into the organically modified nanoparticles, resulting in the properties of the organically modified nanoparticles becoming closer to those of the solvent molecules and significantly improving affinity. This makes it possible to disperse organically modified nanoparticles in solvents with relatively large molecular weights that would normally not be able to disperse organically modified nanoparticles.

[0032] Recent molecular theory research, such as computational science, has revealed that the dispersibility of organically modified nanoparticles is highly dependent on the self-ordering of the organic modification groups or solvent molecules.

[0033] It is well known that self-ordering corresponds to the formation of a solid-phase-like structure by molecules, and that the solubility of solidified molecules in a solvent is significantly reduced. The release of self-ordering is equivalent to a change from a solid phase to a liquid phase, which increases the freedom of molecular motion and promotes the incorporation of solvent molecules, thereby improving the dispersibility of particles in the solvent. The effect of adding a third component according to the first invention also changes the freezing point. The addition of a third component lowers the melting point, and the fact that a liquid phase can be formed at the same temperature is well known, for example, from the snow-melting effect. In addition to the physical effect of the third component entering the liquid phase, it also leads to a freezing point effect on the organic molecular layer, i.e., the release of self-ordering, i.e., an increase in the freedom of movement of organic molecules (liquid-phase transition).

[0034] As in the seventh aspect of the invention, suppression of self-ordering can also be achieved by structural design of the organic molecular layer. By modifying with multiple types of molecules, the modified molecules become less susceptible to self-ordering. To achieve this, domain structures are formed for each molecule, allowing self-ordering to proceed within the domains. However, random modification suppresses the formation of self-ordered structures. This can be determined by the size of the free volume of the modified molecules; the larger the free volume, the less likely they are to crystallize. For random modification, a process such as supercritical hydrothermal synthesis, in which the modified molecules form a homogeneous phase and undergo repeated adsorption and desorption on the surface, resulting in bond formation on the surface, is effective. Since the structure is formed through the free movement of molecules, it is only natural that the free volume increases. In contrast, organic modification under conditions that favor self-ordering at lower temperatures results in a lower free volume, even with the same amount of modification.

[0035] As for the organic modification of multiple types of molecules, by optimizing both the effects of forming a void structure that facilitates physical solvent incorporation, as explained above, and the effect of forming a structure that increases free volume, it is possible to greatly improve the affinity with the solvent.

[0036] An eighth aspect of the invention provides an organically modified nanoparticle dispersion liquid in which organically modified nanoparticles having organic modifying groups on the surface thereof are dispersed in a solvent, the solvent containing a poorly dispersible solvent in which the organically modified nanoparticles are poorly dispersible, and a predetermined molecule as a third component, and the transmittance at a wavelength of 450 nm when the concentration of the organically modified nanoparticles is 1 wt % is 0.8 or more.

[0037] The eighth aspect of the invention corresponds to a different category (product invention) of the first aspect of the invention (process invention). This organically modified nanoparticle dispersion has a transparency of 0.8 or more at a wavelength of 450 nm when the concentration of organically modified nanoparticles is 1 wt%. Therefore, the eighth aspect of the invention can provide a dispersion of organically modified nanoparticles dispersed in a solvent with a relatively large molecular weight.

[0038] A ninth aspect of the invention is the eighth aspect of the invention, wherein the predetermined molecule is a gas or liquefied gas selected from carbon dioxide, a hydrocarbon compound, a nitrogen oxide compound, and a chlorofluorocarbon gas, and the organically modified nanoparticle dispersion is contained in a pressure vessel pressurized to a predetermined pressure of 0.5 MPa or more.

[0039] When the pressure is reduced during use, the gas distributed in the modifying molecules and solvent is desorbed, diffused, and released, gradually reducing the dispersibility. However, the dispersibility is maintained within the time constant of desorption, i.e., for 1 to 14 hours or more, making dispersion possible even in cases where dispersion is normally difficult.

[0040] In a solution containing organically modified nanoparticles, impurities and unreacted modifiers are physically adsorbed, which may reduce the dispersibility of the organically modified nanoparticles. According to the ninth feature of the invention, the impurities contained in the solution are replaced and separated by a high-pressure gas such as carbon dioxide, thereby increasing the dispersibility of the organically modified nanoparticles in a nonpolar solvent, thereby increasing the freedom of solvent selection.

[0041] The invention according to the tenth feature is the invention according to the eighth or ninth feature, wherein the dispersion power term δ of the Hansen solubility parameters at the temperature and pressure of the dispersion liquid to be provided, including the dispersion liquid containing a gas, isD With respect to the dispersion force term δ of the organically modified nanoparticles containing the predetermined molecule or gas, D The value of the dispersion force term δ of the mixed solvent at the enclosed temperature and pressure D The absolute value of the difference between the values ​​is 1.2 MPa. 1 / 2 A dispersion is provided, which is:

[0042] According to the tenth feature of the invention, it is possible to provide a dispersion liquid of organically modified nanoparticles dispersed in a solvent having a relatively large molecular weight.

[0043] The invention according to an eleventh feature is the invention according to any one of the eighth to tenth features, wherein the solvent is a mixed solvent containing a first solvent and a second solvent, the first solvent is a main solvent that is poorly dispersible in the organically modified nanoparticles, and the second solvent, including the case of a gas, has a van der Waals volume at the temperature and pressure of the dispersion liquid that is smaller than the van der Waals volume of the organically modified molecular layer of the organically modified nanoparticles, and the dispersion force term δ of the Hansen solubility parameters D The dispersion force term δ of the organically modified nanoparticles at the temperature and pressure D The absolute value of the difference between the values ​​is 1.2 MPa. 1 / 2 The following cosolvents, dispersions are provided:

[0044] According to the eleventh aspect of the present invention, it is possible to provide a dispersion of organically modified nanoparticles dispersed in a solvent that has a relatively large molecular weight and is generally difficult to disperse.

[0045] The invention according to a twelfth feature is the invention according to the eighth or ninth feature, in which the organically modified nanoparticles have on their surfaces multiple types of organic modifying groups as the predetermined molecules, and the free volume of the organically modified molecule layer is larger than the van der Waals volume of the solvent molecules, and the free volume of each of the organically modified molecule layers is larger than the free volume of a single type of organically modified molecule layer.

[0046] The van der Waals volume of the solvent is greater than the range in which the first modifying group, which is one of the multiple types of organic modifying groups, is easily soluble. Therefore, for organically modified nanoparticles having only the first modifying group, the Hansen solubility parameter δ of the organic modifying group is D and the Hansen solubility parameter δ of the solvent moleculeD Even if the absolute value of the difference between the above is small, the organically modified nanoparticles cannot be dispersed in the solvent.

[0047] According to a twelfth aspect of the invention, the surface has multiple types of organic modifying groups, and the van der Waals volume of the second modifying group is larger than the van der Waals volume of the solvent. This creates a modified chain configuration (molecular pocket) that easily interacts with solvent molecules with large van der Waals volumes, making it possible to disperse organically modified nanoparticles even in solvents with relatively high molecular weights that would otherwise not be able to disperse them. Furthermore, the coexistence of multiple molecules in the modified layer makes self-organization less likely to occur compared to a single molecule, increasing the free volume, which facilitates coordination of solvent molecules and improves dispersibility. As a result, the twelfth aspect of the invention can provide a dispersion of organically modified nanoparticles dispersed in a solvent with a relatively high molecular weight.

[0048] According to the present invention, organically modified nanoparticles can be dispersed even in solvents with relatively large molecular weights, thereby increasing the degree of freedom in solvent selection.

[0049] Fig. 1 is a schematic diagram of the apparatus used in Test Example 1. Fig. 2 is a diagram showing the pressure setting conditions in Test Example 1. Fig. 3 is a diagram showing the test results of Example 1. Fig. 4 is a diagram showing the polar term δ of the Hansen solubility parameters for various solvents. P and the dispersion force term δ D Figure 5 is a visualization of the correlation between the van der Waals volume and the dispersion force term δ of the Hansen solubility parameter for various solvents. D 6 is a visualization of the correlation between the pressure of carbon dioxide and the dispersion force term δ of the Hansen solubility parameter in a mixture of decane or cyclohexane and carbon dioxide. Dand van der Waals volume. Fig. 7 is a schematic diagram of the apparatus used in Test Example 2 etc. Fig. 8 is a diagram showing the pressure setting conditions in Test Example 2. Fig. 9 is a diagram showing the relationship between the wavelength of light irradiated by a spectrophotometer and the absorbance of a measurement sample (Example 2). Fig. 10 is a diagram showing the relationship between the wavelength of light irradiated by a spectrophotometer and the absorbance of a measurement sample (Example 1). Fig. 11 is a diagram showing the relationship between the wavelength of light irradiated by a spectrophotometer and the absorbance of a measurement sample (Example 1) when the measurement sample is the washed decanoic acid-modified nanoparticles used in Example 2. 2 12 shows the relationship between the wavelength of irradiated light and the absorbance of the measurement sample when the measurement sample is the unwashed decanoic acid-modified nanoparticles used in Example 1. FIG. 13 shows the test results of Example 3, i.e., CO 2 14 is a TEM image of composite organically modified nanoparticles modified with both decanoic acid and stearic acid.

[0050] Specific embodiments of the present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be implemented with appropriate modifications within the scope of the object of the present invention.

[0051] <Method for Dispersing Organically Modified Nanoparticles in a Solvent> The invention described in this embodiment is a method for dispersing organically modified nanoparticles obtained by a known method (for example, the method described in Japanese Patent No. 4336856) even in a solvent with a relatively large molecular weight. The invention described in this embodiment includes a dispersion step of dispersing organically modified nanoparticles having organic modifying groups on their surfaces in a solvent.

[0052] [Organically Modified Nanoparticles] The type of organically modified nanoparticles is not particularly limited, and examples thereof include organically modified nanoparticles obtained by the method described in Japanese Patent No. 4,336,856.

[0053] The type of organic modifying group is not particularly limited, and examples thereof include an optionally substituted linear or branched alkyl group, an optionally substituted cyclic alkyl group, an optionally substituted aryl group, an optionally substituted aralkyl group, and an optionally substituted saturated or unsaturated heterocyclic group.

[0054] Examples of the substituent include a carboxy group, a cyano group, a nitro group, a halogen atom, an ester group, an amide group, a ketone group, a formyl group, an ether group, a hydroxyl group, an amino group, a sulfonyl group, -O-, -NH-, and -S-.

[0055] The organically modified nanoparticles may have one type of organic modifying group on the surface, or may have multiple types of organic modifying groups.

[0056] [Solvent] The solvent contains a poorly dispersible solvent in which the organically modified nanoparticles are poorly dispersible, and a predetermined molecule as a third component.

[0057] [Difficult-to-Disperse Solvent] In this embodiment, the term "difficult-to-disperse" refers to a solvent in which turbidity can be visually confirmed when the organically modified nanoparticles are dispersed in the solvent.

[0058] The poorly dispersible solvent is not particularly limited as long as it is poorly dispersible in the organically modified nanoparticles at the dispersion treatment temperature and pressure. If the dispersion treatment temperature is room temperature, the dispersion treatment temperature is room temperature (25°C), and if the dispersion treatment pressure is normal pressure, the dispersion treatment pressure is normal pressure (0.1 MPa).

[0059] As a poorly dispersible solvent, for example, the polar term δ P 0. Specific examples of the nonpolar solvent include cyclohexane, cyclopentane, hexane, octane, bicyclohexyl, decane, decalin, and dodecane.

[0060] [Predetermined Molecule] The van der Waals volume of the predetermined molecule as the third component is smaller at the dispersion treatment temperature and pressure than the van der Waals volume of the poorly dispersible solvent at the dispersion treatment temperature and pressure, and is also smaller than the free volume of the organic modification layer.

[0061] When the solvent is under atmospheric pressure, the dispersion process pressure, i.e., the pressure of the gas in contact with the surface of the solvent, is normal pressure (0.1 MPa). When the solvent is under pressure, the temperature and pressure of the dispersion process are measured.

[0062] The van der Waals volume refers to the volume of the region occupied by the target molecule at a given temperature and pressure. The free volume refers to the volume obtained by subtracting the van der Waals volume from the volume of space in which the molecules can move freely at that temperature and pressure.

[0063] A solvent that does not contain a specific molecule as a third component is poorly dispersible in organically modified nanoparticles, and the organically modified nanoparticles cannot be dispersed in the solvent. This is because the van der Waals volume of the solvent is larger than the range in which the organically modified nanoparticles are easily soluble, or the dispersion force term δ of the Hansen solubility parameters is D With respect to the dispersion force term δ of the organically modified nanoparticles, D The value of and the dispersion term δ of a nonpolar solvent D The absolute value of the difference between the values ​​is 1.2 MPa. 1 / 2 It means exceeding.

[0064] The Hansen solubility parameter is a value used to predict the solubility of a substance, published by Charles M. Hansen in 1967. It is the intermolecular energy due to the dispersion force between molecules per molecular volume (dispersion force term δ D ), the energy due to intermolecular dipole interactions (polar term δ P ) and the energy due to intermolecular hydrogen bonds (hydrogen bond term δ H ) is composed of

[0065] In this embodiment, the van der Waals volume of the predetermined molecule as the third component is smaller than the van der Waals volume of the solvent, and the dispersion force term δ of the modifying group of the organically modified nanoparticles is D and the dispersion term δ for a given molecule D The absolute value of the difference between the values ​​is 1.2 MPa. 1 / 2 Therefore, by adding a predetermined molecule to the solvent, a good mixed state can be obtained, and the average van der Waals volume of the mixed solvent can be kept lower than the van der Waals volume of the solvent, and the dispersion force term δ D Regarding the organically modified nanoparticles, the affinity with the mixed solvent can be dramatically improved by coordinating a specific molecule to the modifying group of the organically modified nanoparticles. As a result, the dispersion force terms δ of the mixed solvent and the organically modified nanoparticles can be improved. D Furthermore, the coordination of the third component suppresses the self-ordering of the organically modified layer, thereby increasing the free volume of the organically modified layer and further improving the affinity with solvent molecules and, in turn, the dispersibility of the organically modified nanoparticles in the solvent.

[0066] (First Aspect) In a first aspect, the dispersing step preferably includes, prior to the dispersing step, a step of increasing the concentration of a third component in a state in which the organically modified nanoparticles are placed in a solvent, thereby accelerating the dispersion of the organically modified nanoparticles in the solvent.

[0067] By increasing the concentration of the third component and coordinating it with the organic modification group, the self-ordering of the organic molecular layer is suppressed, the free volume increases, and the coordination of the solvent can be improved. The coordination of the third component reduces the Hansen solubility parameter dispersion term δ of the organically modified nanoparticles. D and the dispersion term of the solvent δ D This makes it possible to disperse organically modified nanoparticles in a poorly dispersible solvent in which they would not normally be dispersed.

[0068] The type of the predetermined molecule is not particularly limited, but it is desirable that the van der Waals volume is smaller than the free volume of the organic molecule layer, and it may be a bidispersible solvent molecule.It may also be a gas, such as a gas or liquefied gas selected from carbon dioxide, a hydrocarbon compound, a nitrogen oxide compound, and a chlorofluorocarbon gas.

[0069] The type of hydrocarbon compound is not particularly limited, but typically includes one or more light hydrocarbon compounds in the group including methane, ethane, ethylene, propane, and butane.

[0070] The type of nitrogen oxide compound is not particularly limited, but generally includes one or more of the group including nitric oxide, nitrogen dioxide, nitrogen trioxide, nitrous oxide, dinitrogen trioxide, dinitrogen tetroxide, and dinitrogen pentoxide.

[0071] When the predetermined molecules are gases or liquefied gases, the dispersion step preferably involves dispersing the organically modified nanoparticles in the solvent by pressurizing them to a predetermined pressure. By pressurizing the poorly dispersible solvent to a predetermined temperature and pressure in the presence of the predetermined gas, the gas molecules dissolve in the solvent and are distributed to the organic modification groups. Therefore, the Hansen solubility parameter of the mixed solvent is close to the solubility parameter of the organically modified layer. The dispersion force term δ of the modified layer is D The value of and the dispersion term δ of the mixed solvent D This makes it possible to disperse organically modified nanoparticles in a solvent with a relatively large molecular weight that would normally not be able to disperse organically modified nanoparticles.

[0072] The pressure applied is preferably equal to or higher than the saturated vapor pressure at the dispersion treatment temperature (however, if the dispersion treatment temperature is equal to or higher than the critical temperature, equal to or higher than the critical pressure), but is not particularly limited as long as it is capable of dispersing the organically modified nanoparticles in a poorly soluble solvent or a mixed solvent with a predetermined molecule. For example, the lower limit of the pressure is preferably 0.5 MPa or higher, and although higher pressures are effective, the optimum pressure is determined based on operability.

[0073] The upper limit of the pressure is not particularly limited, but in consideration of ease and safety of operation and the costs of the pressure vessel and compressor of the equipment, the upper limit of the pressure is preferably 20 MPa or less, and more preferably 10 MPa or less.

[0074] By pressurizing a poorly soluble solvent or a mixed solvent with a specific molecule to a specific temperature and pressure in the presence of gas, the Hansen solubility parameter dispersion power term δ of the mixed solvent can be calculated. D and the dispersion force term δ of organically modified nanoparticles D The absolute value of the difference from the value of also becomes lower. Furthermore, the coexistence of gas further increases the free volume of the organic molecular layer, and further increases the affinity with the solvent.

[0075] Solutions containing organically modified nanoparticles contain impurities and unreacted modifying molecules, which may reduce the dispersibility of the organically modified nanoparticles. When a high-pressure gas has sufficient pressure and is in a liquefied gas state or a supercritical fluid above its critical pressure, the gas acquires dissolving power, and impurities contained in the solution are extracted by the high-pressure gas, such as carbon dioxide, thereby increasing the dispersibility of the organically modified nanoparticles in poorly soluble solvents, thereby increasing the freedom of solvent selection.

[0076] The organically modified nanoparticles are preferably purified nanoparticles.

[0077] In general, purification of organically modified nanoparticles is carried out to make the physical properties of the organically modified nanoparticles uniform by fractionating them based on particle size and modification rate, and to remove unreacted organic molecules used during the organic modification and cleaning solvents used in the cleaning process. The purification method is not particularly limited, and may be any of centrifugation, membrane purification, solvent extraction, chromatography, etc.

[0078] The van der Waals volume and free volume can be evaluated in both the liquid and gas phases using the van der Waals equation of state and various other real gas equations of state. The physical properties and critical constants of any substance can be obtained from physical property evaluations. Even for unknown substances, the group contribution method can be used to estimate the physical properties of the constituent molecules. When a third component, including a gas, is present, partitioning into organically modified molecules or solvents—that is, phase equilibrium prediction—requires intermolecular interaction parameters, which can be evaluated from a database or from the difference in Hansen solubility parameters. This allows the volume fraction φi to be evaluated for each component, allowing the average solubility parameter, average van der Waals volume, and free volume to be evaluated when multiple components coexist. In the formula, φ is the volume fraction in the liquid phase, the subscript 1 indicates carbon dioxide, and the subscript 2 indicates the solvent.

[0079] When the mixed solvent is pressurized, the van der Waals volume of the mixed solvent at a given pressure falls within the range in which the organically modified nanoparticles are readily soluble, and the dispersion force term δ of the organically modified nanoparticles at 0.1 MPa is D The value of and the dispersion force term δ of the mixed solvent at a given pressure D The difference between the values ​​of is less than 1. This makes it possible to disperse organically modified nanoparticles in a solvent with a relatively large molecular weight, which would normally not be able to disperse organically modified nanoparticles.

[0080] According to the first aspect of the invention, organically modified nanoparticles can be dispersed even in solvents with relatively large molecular weights, resulting in increased freedom in solvent selection.

[0081] (Second Aspect) In the second aspect, organically modified nanoparticles are dispersed in a mixed solvent containing a poorly dispersible solvent as the main solvent and a predetermined molecule as the co-solvent.

[0082] The main solvent is a poorly dispersible solvent that has low chemical affinity, i.e., has a large difference between its Hansen solubility parameter and the solubility parameter of the organic modifying group, or has a van der Waals volume at the temperature and pressure of the dispersion process that is greater than the range in which the organic modifying group is easily soluble.

[0083] The cosolvent has a van der Waals volume within a range in which the organically modified nanoparticles are readily soluble, and the dispersion force term δ D With respect to the dispersion force term δ of the organically modified nanoparticles at the pressure D The absolute value of the difference between the values ​​is 1.2 MPa 1 / 2 The following co-solvents:

[0084] The cosolvent is the van der Waals volume and the dispersion term δ D In the case where a mixed solvent is dispersed in organically modified nanoparticles modified with decanoic acid, specific examples of the co-solvent include cyclohexane, bicyclohexyl, decane, decalin, and dodecane.

[0085] The volume ratio of the co-solvent to the main solvent is not particularly limited, but is preferably 0.1 parts by volume or more, more preferably 0.5 parts by volume or more, and even more preferably 1.0 parts by volume or more, relative to 100 parts by volume of the main solvent. Furthermore, since the original purpose is to use the main solvent, the volume ratio of the co-solvent is preferably 20 parts by volume or less, more preferably 10 parts by volume or less, relative to 100 parts by volume of the main solvent.

[0086] In molecular solution systems, the addition of a small amount of cosolvent improves the affinity between the main solvent and the solute, as exemplified by the entrainer effect. According to the second aspect of the invention, a cosolvent is added whose van der Waals volume is smaller than the void volume of the organic modification group and is within a range in which it is readily soluble in the organic modification group. This makes it possible to disperse organically modified nanoparticles in solvents that would otherwise be unable to disperse them, despite their low affinity for the organically modified nanoparticles and relatively large molecular weight. This is thought to be due to the molecules of the highly dispersible solvent, with their small van der Waals volume, preferentially acting on the surface-modified chains, resulting in high dispersibility of the entire organically modified nanoparticles, including the cosolvent molecules coordinated to the surface, in the main solvent.

[0087] According to the second aspect of the invention, the organically modified nanoparticles can be dispersed even in a solvent that has a low affinity for the organically modified nanoparticles and a relatively large molecular weight, resulting in an increased degree of freedom in the selection of the solvent.

[0088] (Third Aspect) As described above, the organically modified nanoparticles may have one type of organic modifying group on the surface, or may have multiple types of organic modifying groups. When the organically modified nanoparticles have multiple types of organic modifying groups, these multiple types of organic modifying groups are treated as a predetermined molecule.

[0089] Organically modified nanoparticles having multiple types of organic modifying groups can be obtained by using a mixture of multiple types of organic modifying agents as a modifying agent in a known method (for example, the method described in Japanese Patent No. 4336856). For example, Ce(OH) 4 Using the precursor as a compound, and a mixture of decanoic acid (DA, carbon number: 10) and stearic acid (SA, carbon number: 18) as a modifier, composite organic modified CeO was synthesized by supercritical hydrothermal synthesis. 2 Nanoparticles can be synthesized.

[0090] When the organically modified nanoparticles have multiple types of organic modifying groups on their surfaces, the free volume of the organically modified molecular layer under the temperature and pressure conditions in the dispersion step is preferably larger than the free volume of a single type of organically modified molecular layer, and the free volume of the organically modified molecular layer under the temperature and pressure conditions in the dispersion step is preferably smaller than the van der Waals volume of the solvent molecules.

[0091] The van der Waals volume of the solvent is greater than the range in which the first modifying group, which is one of the multiple types of organic modifying groups, is readily soluble, and therefore, organically modified nanoparticles in which the first modifying group is the only modifier cannot be dispersed in the solvent.

[0092] The surface is modified with multiple types of organic modifiers, and the volume of the voids (molecular pockets) formed in these modified base layers is larger than the van der Waals volume of the solvent, regardless of the van der Waals volume of the solvent. This allows solvent molecules with large van der Waals volumes to be incorporated into the organically modified nanoparticles, resulting in the properties of the organically modified nanoparticles becoming closer to those of the solvent molecules and significantly improving affinity. In other words, it is now possible to disperse organically modified nanoparticles in solvents with relatively large molecular weights that would normally not be able to disperse them.

[0093] According to recent molecular theory research, such as computational science, adding multiple types of organic modification groups to the surface significantly changes the self-ordering of the organic modification groups or solvent molecules, which in turn significantly changes the dispersibility of the organically modified nanoparticles. In other words, we can expect to see an improvement in dispersibility based on a completely different principle.

[0094] It is well known that self-ordering corresponds to the formation of a solid phase by molecules, and that the solubility of solidified molecules in a solvent is significantly reduced. The release of self-ordering is equivalent to a change from a solid to a liquid phase, which increases the freedom of molecular movement, promoting the incorporation of solvent molecules, thereby improving the dispersibility of particles in the solvent. The addition of a third component also creates a freezing point. The addition of a third component lowers the melting point, and the fact that a liquid phase can be formed at the same temperature is well known from the deicing agent effect, etc. In addition to the physical effect of the third component entering the liquid phase, it also leads to a freezing point effect on the organic molecular layer, i.e., the release of self-ordering, i.e., an increase in the freedom of movement of organic molecules (liquid-phase transition).

[0095] Self-ordering can also be suppressed by structural design of the organic molecular layer. By modifying with multiple types of molecules, the modified molecules become less susceptible to self-ordering. To achieve this, domain structures are formed for each molecule, allowing self-ordering to proceed within the domains. However, random modification suppresses the formation of self-ordered structures. This is determined by the size of the free volume of the modified molecules; the larger the free volume, the less likely they are to crystallize. Random modification is effective, for example, in supercritical hydrothermal synthesis, where the modified molecules form a homogeneous phase and undergo repeated adsorption and desorption on the surface, resulting in bond formation on the surface. In principle, the molecules form structures while moving freely, so naturally, the free volume increases. In contrast, organic modification under conditions that favor self-ordering at lower temperatures results in a lower free volume, even with the same amount of modification.

[0096] As for the organic modification of multiple types of molecules, by optimizing both the effects of forming a void structure that facilitates physical solvent incorporation and the effect of forming a structure that increases free volume, as explained above, it is possible to greatly improve the affinity with the solvent.

[0097] [Product: Organically Modified Nanoparticle Dispersion] The particles obtained by the method described in this embodiment are preferably supplied in a state dispersed in a solvent. The solvent contains a poorly dispersible solvent in which the organically modified nanoparticles are poorly dispersible and a predetermined molecule as a third component, and when the concentration of the organically modified nanoparticles is 1 wt %, the transmittance at a wavelength of 450 nm is 0.8. The transmittance is the value obtained by subtracting the absorbance from 1. Therefore, "a transmittance of 0.8 or more" can also be rephrased as "an absorbance of 0.2 or less."

[0098] The organically modified nanoparticle dispersion obtained by the above-described method has a transparency of 0.8 or more at a wavelength of 450 nm when the concentration of the organically modified nanoparticles is 1 wt %. Therefore, the invention described in this embodiment can provide a dispersion of organically modified nanoparticles dispersed in a solvent with a relatively large molecular weight.

[0099] In this embodiment, the transmittance is a measure of dispersibility, and the higher the transmittance, the better. The transmittance is 0.8 or more, more preferably 0.9 or more, and even more preferably 0.95 or more.

[0100] Examples of the predetermined molecule as the third component include a gas or liquefied gas selected from carbon dioxide, a hydrocarbon compound, a nitrogen oxide compound, and a chlorofluorocarbon gas. The organically modified nanoparticle dispersion is preferably contained in a pressure vessel pressurized to a predetermined pressure of 0.5 MPa or more.

[0101] A solution containing organically modified nanoparticles may contain unreacted modifiers and impurities, which may inhibit dispersibility. According to the invention described in this embodiment, the unreacted modifiers and impurities contained in the solution are extracted by a high-pressure gas such as carbon dioxide, thereby increasing the dispersibility of the organically modified nanoparticles in nonpolar solvents, thereby increasing the freedom of solvent selection.

[0102] Furthermore, when the gas pressure is released and returned to normal pressure (0.1 MPa), the absorbance increases over time, making it impossible to maintain the dispersion state of the organically modified nanoparticles in the poorly dispersible nonpolar solvent. According to the invention described in this embodiment, the gas pressure is maintained, so the dispersion state can be maintained for a long period of time.

[0103] Alternatively, the particles obtained by the method according to the present embodiment are preferably supplied in a state dispersed in a mixed solvent containing a first solvent and a second solvent. The first solvent is a main solvent that is poorly dispersible in the organically modified nanoparticles. The second solvent has a van der Waals volume at a temperature and pressure of the gas in contact with the surface of the mixed solvent that is smaller than the void volume formed in the organic modifying group, and the dispersion force term δ of the Hansen solubility parameters is D Regarding the dispersion force term δ of the organically modified nanoparticles at the temperature and pressure of the gas in contact with the surface of the mixed solvent, D The absolute value of the difference between the values ​​is 1.2 MPa. 1 / 2 The following co-solvents:

[0104] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these examples.

[0105] Test Example 1: Dispersion of organically modified nanoparticles in a solvent Example 1: Dispersion of organically modified nanoparticles in a solvent in decane (with additives) [Preparation of organically modified nanoparticles using decanoic acid] In this test, CeO 2 Using decanoic acid (DA) as a modifier, organically modified CeO nanoparticles were synthesized by supercritical hydrothermal synthesis. 2 Nanoparticles (hereinafter also referred to as "OM nanoparticles") were synthesized.

[0106] Ce(OH) 4 was dispersed in distilled water by ultrasonic treatment, and 0.1 M Ce(OH) 4 Then, 0.10 M Ce(OH) 4 The aqueous suspension (2.5 mL) and DA (molar ratio 1:3) were placed in a 5 mL Hastelloy tubular batch reactor. The reactor was placed in a furnace and heated at 150 °C for 20 minutes, then at 400 °C for 10 minutes. The reactor was then rapidly cooled to terminate the reaction, after which the product was recovered using hexane and the aqueous layer was removed. An equal volume of ethanol was added to the remaining organic layer, and the mixture was centrifuged (9600 rpm, 20 minutes) to remove unreacted materials, yielding OM nanoparticles.

[0107] [Dispersion of OM Nanoparticles in Decane] The solvent dispersion was carried out under the following conditions using the apparatus shown in FIG. 1. Nanoparticles: the above-mentioned decanoic acid-modified CeO 2 Nanoparticles (OM nanoparticles) Nanoparticle concentration: 1 wt% Solvent: Decane Temperature: 40°C Additive: Carbon dioxide gas Pressure: As shown in Figure 2 (2, 4, 6 MPa)

[0108] [Results] The results are shown in Figure 3. When the carbon dioxide gas pressure was 2 MPa, the OM nanoparticles were not dispersed in the solvent (decane), but when the pressure was 4 MPa, the OM nanoparticles were uniformly dispersed in the solvent (decane). This uniform dispersion state was maintained even when the pressure was increased to 6 MPa, and was also maintained when the pressure was subsequently returned to normal pressure.

[0109] Comparative Example 1 Except for not adding carbon dioxide gas, an attempt was made to disperse OM nanoparticles in decane using the same method as in Example 1. However, it was not possible to uniformly disperse the OM nanoparticles in decane.

[0110] [Discussion] Figure 4 shows the polarity term δ of the Hansen solubility parameters for various solvents. P and the dispersion force term δ D As shown in Figure 4, the dispersion force term δ of the Hansen solubility parameters between the solvent and the organically modified nanoparticles is basically D The difference is 1.2 MPa 1 / 2 or less, and both the solvent and the organically modified nanoparticles have a polarity term δ P is 0 MPa 1 / 2 For example, the dispersion force term δ of cyclohexane is D is 16.8 MPa 1 / 2 and decanoic acid-modified CeO 2 Dispersion force term δ of nanoparticles (OM nanoparticles) D is 15.7 MPa 1 / 2 Therefore, between the two, the dispersion force term δ D The difference is 1.2 MPa 1 / 2 The polarity terms δ of cyclohexane and OM nanoparticles are as follows: P are all 0 MPa 1 / 2 Therefore, the OM nanoparticles can be dispersed in cyclohexane.

[0111] In addition, the dispersion force term δ of decane D is 16 MPa 1 / 2 and the dispersion force term δ between decane and OM nanoparticles is D The difference is 1.2 MPa 1 / 2 The polarity term of decane is δ P is 0 MPa 1 / 2 Therefore, it seems possible to disperse OM nanoparticles in decane, but in reality, it is not possible to disperse OM nanoparticles in decane under normal temperature and pressure conditions.

[0112] Figure 5 shows the relationship between the van der Waals volume and the dispersion term δ of the Hansen solubility parameter for various solvents. D As shown in Figure 5, the OM nanoparticles were prepared by the decanoic acid-modified CeO 2 If the nanoparticles have a van der Waals volume of 89 cm 3 mol -1 OM nanoparticles can be dispersed in a non-polar solvent if the volume is less than 0.01 mm. For example, the van der Waals volume of cyclohexane is 61.4 cm. 3 mol -1 and 89 cm 3 mol -1 Therefore, the OM nanoparticles can be dispersed in cyclohexane.

[0113] In comparison, the van der Waals volume of decane is 129.6 cm 3 mol -1 The van der Waals volume range (89 cm) indicates that OM nanoparticles are easily soluble. 3 mol -1 Therefore, decane is out of the dispersion force term δ D The difference is 1.2 MPa 1 / 2 is less than or equal to, and the polar term δ P is 0 MPa 1 / 2 Despite this, it is believed that OM nanoparticles cannot be dispersed in decane under normal temperature and pressure conditions.

[0114] Here, the van der Waals volume of carbon dioxide at 25 °C and 0.1 MPa is 19.7 cm 3 mol -1 This is significantly smaller than the van der Waals volume of OM nanoparticles. Therefore, the present inventor hypothesized that if carbon dioxide could be added to decane as an additive to bring the van der Waals volume of the mixture closer to the van der Waals volume of OM nanoparticles, it might be possible to disperse OM nanoparticles in decane, which is incapable of dispersing OM nanoparticles at room temperature and pressure. This example supports the validity of this hypothesis.

[0115] FIG. 6 shows the relationship between the pressure of carbon dioxide and the dispersion force term δ of the Hansen solubility parameter in a mixture of decane or cyclohexane and carbon dioxide. D and van der Waals volume.

[0116] The van der Waals volume and free volume can be evaluated in both the liquid and gas phases using the van der Waals equation of state and other equations of state for real gases. The physical properties and critical constants of any substance can be obtained from property evaluations. For unknown substances, the group contribution method can be used to estimate the physical properties of the constituent molecules. When a third component, including a gas, coexists, the partitioning to organically modified molecules or solvents, i.e., phase equilibrium estimation, requires further intermolecular interaction parameters, which can be evaluated from a database or from the difference in Hansen solubility parameters. This allows the volume fraction φ for each component to be calculated. i Therefore, it is possible to evaluate the average solubility parameter, average van der Waals volume, and free volume when multiple components coexist. In the formula, φ is the volume fraction in the liquid phase, the subscript 1 indicates carbon dioxide, and the subscript 2 indicates the solvent.

[0117] We focus on the case where the solvent is a mixture of decane and carbon dioxide. When the pressure is close to 0 MPa, the van der Waals volume is 89 cm 3 mol -1 Therefore, the dispersion force term δ of the Hansen solubility parameters D is the dispersion force term δ of the OM nanoparticles D Even if the concentration is close to 0.1, the OM nanoparticles cannot be dispersed in the mixed solvent.

[0118] On the other hand, as the pressure increases, the van der Waals volume of the mixed solvent decreases. At a pressure of 4 MPa, the van der Waals volume of the mixed solvent is 89 cm 3 mol -1 As a result, although OM nanoparticles could not be dispersed in decane alone due to the large molecular weight of the solvent, by mixing it with carbon dioxide, it became possible to disperse OM nanoparticles.

[0119] Next, we will focus on the case where the solvent is a mixed solvent of cyclohexane and carbon dioxide. As mentioned above, cyclohexane is a solvent that can disperse OM nanoparticles even when used alone. However, when the solvent is a mixed solvent of cyclohexane and carbon dioxide and the pressure of carbon dioxide is increased, the dispersion force term δ of the Hansen solubility parameter D decreases, and the dispersion force term δ of the OM nanoparticles D Therefore, even if a solvent is capable of dispersing OM nanoparticles by itself, it is technically significant to mix the solvent with carbon dioxide.

[0120] Test Example 2: Dispersion of washed organically modified nanoparticles in a solvent Example 2: Dispersion of washed organically modified nanoparticles in a solvent in decane (with additives) Preparation of washed OM nanoparticles The washed OM nanoparticles obtained in Example 1 were dispersed in cyclohexane, and the suspension was slowly added dropwise. Washing was performed with stirring using acetone in an amount 20 times the amount of cyclohexane. The particles were then recovered by centrifugation, washed again in the same manner, and then redispersed in cyclohexane. The particles were then allowed to stand at room temperature for one day and subjected to size classification. After size classification, the supernatant was recovered and vacuum freeze-dried to obtain washed OM nanoparticles.

[0121] The average primary particle diameter of the washed OM nanoparticles was measured using a transmission electron microscope (TEM, H-7650; Hitachi, Ltd.) and found to be 5.8 nm. 2 The decanoic acid modification rate on the nanoparticle surface was 4.9 molecules / nm 2 It was.

[0122] [Dispersion of washed OM nanoparticles in decane] In Example 1, dispersibility was evaluated visually, but in order to quantify this, solvent dispersion was performed using the apparatus shown in Figure 7. The apparatus configuration in Figure 7 differs from that in Figure 1 in that a UV-visible spectrophotometer V-750 (manufactured by JASCO Corporation) was added. The conditions for solvent dispersion were as follows: Nanoparticles: Decanoic acid-modified CeO after the above-mentioned washing 2Nanoparticles (OM nanoparticles after washing) Nanoparticle concentration: 1 wt% Solvent: Decane Temperature: 40°C Additive: Carbon dioxide gas Pressure: As shown in Figure 8 (2, 4, 6 MPa)

[0123] [Dispersibility when pressure is returned to normal] Decane-CO 2 After dispersion in the mixed solvent, CO 2 After the pressure was released, the dispersibility of the washed OM nanoparticles in the decane solvent was evaluated for 14 hours from the start of pressure release.

[0124] [Results] After washing, the OM nanoparticles were 2 The results when dispersed in a mixed solvent are shown in Figure 9. Figure 9 shows the wavelength of the irradiated light measured by a spectrophotometer and the measurement sample (OM nanoparticles after washing were dissolved in decane-CO 2 The graph shows the relationship between the absorbance of OM nanoparticles (dispersed in a mixed solvent) and the absorbance of OM nanoparticles (dispersed in a mixed solvent). Focusing on the absorbance at an irradiation wavelength of 450 nm, it is suggested that in Example 1, OM nanoparticles could not be dispersed in a solvent at a pressure of 2 MPa, but in Example 2, even at a pressure of 2 MPa, the washed OM nanoparticles can be dispersed in a solvent. Example 2 indicates that the use of washed OM nanoparticles can reduce the carbon dioxide pressure required to disperse the OM nanoparticles in a mixed solvent.

[0125] 10 shows the relationship between the wavelength of light irradiated by a spectrophotometer and the absorbance of the measurement sample when the measurement sample was the OM nanoparticles used in Example 1, i.e., OM nanoparticles before cleaning. Focusing on the absorbance at a wavelength of 450 nm of irradiated light, it is clear that the absorbance remains high at a pressure of 2 MPa, but is low at pressures of 4 MPa or higher, suggesting that the OM nanoparticles can be dispersed in a solvent.

[0126] FIG. 11 shows the CO 2 11 is a graph showing the relationship between the time elapsed since the start of decompression and the absorbance at a wavelength of 450 nm. According to FIG. 11, even after 14 hours have passed since the start of decompression, the absorbance remains at approximately 0.85. 2It can be said that the dispersibility of the OM nanoparticles in the solvent after washing is sufficiently guaranteed, even though the pressure was reduced.

[0127] 12 shows the relationship between the wavelength of the irradiated light and the absorbance of the measurement sample when the measurement sample is the unwashed OM nanoparticles used in Example 1. 2 The graphs show the results at the start of decompression, 1 to 60 minutes after the start of decompression, and 150 minutes after the start of decompression. Focusing on the absorbance at a wavelength of 450 nm, the absorbance at the start of decompression is less than 0.5, indicating sufficient solvent dispersibility, but 60 minutes after the start of decompression, the absorbance is about 3, indicating poor solvent dispersibility. Therefore, it can be said that whether or not washing is performed when obtaining OM nanoparticles significantly affects the solvent dispersibility after decompression of additives such as carbon dioxide.

[0128] Test Example 3 Relationship between pressurization time and solvent dispersibility of additive Example 3 Solvent dispersion of washed OM nanoparticles in decane Using the apparatus shown in Figure 7, the washed OM nanoparticles used in Example 2 were dispersed in a decane-carbon dioxide mixed solvent. The solvent dispersion conditions were as follows: Nanoparticles: the same washed OM nanoparticles as in Example 2 Nanoparticle concentration: 1 wt% Solvent: decane Temperature: 40°C Additive: carbon dioxide gas Pressure: 0.8, 1, 2, 6 MPa

[0129] [Results] Figure 13 shows the results of CO 2 13 is a graph showing the relationship between the time elapsed since the start of the addition of CO and the absorbance at a wavelength of 450 nm. 2 Even if the pressure is 0.8 MPa, a CO permeability of 0.8 or more, which is an index of sufficient dispersibility, can be achieved in about 17 minutes after the start of addition. 2 The higher the pressure, the better. 2 If the pressure is 1.2 MPa or more, a permeability of 0.8 or more can be achieved in less than 10 minutes after the start of addition.

[0130] Test Example 4 Dispersion of Decanoic Acid-Modified Nanoparticles Washed OM nanoparticles (decanoic acid-modified nanoparticles) prepared in the same manner as in Example 2 were wetted with cyclohexane and then dispersed in toluene, a poor solvent.

[0131] Although aggregation progressed over time, good dispersibility was achieved immediately after dispersion. This is because cyclohexane coordinates with the decane organic modification layer, increasing the free volume of the organic modification layer and suppressing self-ordering (solidification of the organic phase). In equilibrium, the third component, cyclohexane, desorbs and diffuses into the solvent molecules, ultimately decreasing affinity and promoting aggregation. Being able to maintain a dispersed state for some time is extremely useful in the processing and handling of nanoparticles, which involve many processes. These can also be provided as wet nanoparticles.

[0132] Test Example 5: Dispersion of OM Nanoparticles in a Mixed Solvent Example 5-1: Dispersion of OM Nanoparticles in a Mixed Solvent (Decane + Cyclohexane) One part by mass of washed OM nanoparticles prepared using the same method as in Example 2 was added to 100 parts by mass of a mixed solvent consisting of 100 parts by volume of decane and 1 part by volume of cyclohexane, and the mixture was sonicated for 30 minutes and then allowed to stand overnight at room temperature. Dispersibility was then evaluated by visual observation and dynamic light scattering (DLS) using a Zetasizer Nano ZS (Malvern Instruments). Visual observation determined the nanoparticles to be "dispersed" if there was no precipitation or cloudiness. Dynamic light scattering observation determined the nanoparticles to be "dispersed" if they were monodispersed with an average hydrodynamic diameter of 10 nm or less.

[0133] As a result, it was confirmed by both visual observation and dynamic light scattering observation that the OM nanoparticles were properly dispersed.

[0134] Example 5-2: Dispersion of OM nanoparticles in a mixed solvent (decane + hexane) The dispersibility of OM nanoparticles was evaluated using the same method as in Example 5-1, except that 1 part by volume of cyclohexane was replaced by 1 part by volume of hexane. As a result, it was confirmed that the OM nanoparticles were properly dispersed by both visual observation and dynamic light scattering observation.

[0135] Example 5-3 Dispersion of OM nanoparticles in a mixed solvent (decalin + cyclohexane) The dispersibility of OM nanoparticles was evaluated using the same method as in Example 4-1, except that 100 parts by volume of decane was replaced with 100 parts by volume of decalin (also known as decahydronaphthalene). As a result, it was confirmed that the OM nanoparticles were properly dispersed by both visual observation and dynamic light scattering observation.

[0136] Example 5-4 Dispersion of OM nanoparticles in a mixed solvent (decalin + hexane) The dispersibility of OM nanoparticles was evaluated using the same method as in Example 4-1, except that 100 parts by volume of decane was replaced by 100 parts by volume of decalin, and 1 part by volume of cyclohexane was replaced by 1 part by volume of hexane. As a result, it was confirmed that the OM nanoparticles were properly dispersed by both visual observation and dynamic light scattering observation.

[0137] Comparative Example 5-1: Dispersion of OM nanoparticles in a single solvent (decane) The dispersibility of OM nanoparticles was evaluated using the same method as in Example 5-1, except that the mixed solvent consisting of 100 parts by volume of decane and 1 part by volume of cyclohexane was the single solvent consisting of decane. As a result, both visual observation and dynamic light scattering observation confirmed that the OM nanoparticles were not properly dispersed.

[0138] Comparative Example 5-2: Dispersion of OM nanoparticles in a single solvent (decalin) The dispersibility of OM nanoparticles was evaluated in the same manner as in Example 5-1, except that the mixed solvent consisting of 100 parts by volume of decalin and 1 part by volume of cyclohexane was a single solvent consisting of decalin. As a result, both visual observation and dynamic light scattering observation confirmed that the OM nanoparticles were not properly dispersed.

[0139] [Discussion] The van der Waals volume of the primary solvent, decane or decalin (first solvent), is greater than the range in which OM nanoparticles are readily soluble, making it impossible to disperse organically modified nanoparticles in the first solvent alone.

[0140] In molecular dissolution systems, as exemplified by the entrainer effect, adding a small amount of co-solvent (second solvent) improves the affinity between the main solvent and the solute, increasing solubility. According to the invention described in this embodiment, the addition of a co-solvent (hexane) whose van der Waals volume is within the range in which the organic modification group is easily soluble to the first solvent makes it possible to disperse OM nanoparticles, even in solvents with relatively large molecular weights that would not normally disperse OM nanoparticles. This is thought to be due to the molecules of the highly dispersible solvent with a small van der Waals volume preferentially acting on the surface-modified chains, resulting in the entire organically modified nanoparticles, including the co-solvent molecules coordinated to the surface, exhibiting high dispersibility in the main solvent.

[0141] Test Example 6: Dispersion of composite OM nanoparticles in a solvent Example 6: Dispersion of composite OM nanoparticles in a solvent using decanoic acid and stearic acid Preparation of composite OM nanoparticles Ce(OH) 4 Using the precursor as a compound, and a mixture of decanoic acid (DA, carbon number: 10) and stearic acid (SA, carbon number: 18) as a modifier, composite organic modified CeO was synthesized by supercritical hydrothermal synthesis. 2 Nanoparticles were synthesized.

[0142] Ce(OH) 4 was dispersed in distilled water by ultrasonic treatment, and 0.10 M Ce(OH) 4 Then, 0.10 M Ce(OH) 4The aqueous suspension (2.5 mL), DA, and SA (molar ratio 1:1.5:1.5) were placed in a 5 mL Hastelloy tubular batch reactor. The reactor was placed in a heating furnace and heated first at 150 °C for 20 minutes, then at 400 °C for 10 minutes. The reactor was rapidly cooled to terminate the reaction, and the product was recovered using hexane, and the aqueous layer was removed. An equal volume of ethanol was added to the remaining organic layer, and unreacted materials were removed by centrifugation (9600 rpm, 20 minutes). The recovered particles were then dispersed in cyclohexane, and the suspension was slowly added dropwise. The particles were then washed with acetone (20 times the volume of cyclohexane) while stirring. The particles were then recovered by centrifugation, washed again in the same manner, redispersed in cyclohexane, and left at room temperature for 1 day for size classification. After size classification, the supernatant was recovered and vacuum freeze-dried to obtain the composite organic-modified CeO. 2 Nanoparticles (hereinafter also referred to as "composite OM nanoparticles") were obtained.

[0143] Figure 14 shows a TEM image of composite OM nanoparticles modified with both DA and SA. The gaps between the particles indicate that the particles are well modified and dispersed in the solvent (cyclohexane). The average primary particle diameter of the composite OM nanoparticles was 5.2 nm.

[0144] [Dispersibility in Solvent] 1 part by mass of the above-described composite OM nanoparticles was added to 100 parts by mass of a single solvent consisting of 100 parts by volume of dodecane, and the mixture was ultrasonicated for 30 minutes and then left overnight at room temperature. The dispersibility was then evaluated by visual observation and by the dynamic light scattering method described above. Both visual observation and dynamic light scattering observation confirmed that the OM nanoparticles were properly dispersed.

[0145] Comparative Example 6-1 Dispersion of OM Nanoparticles with Decanoic Acid in Solvent The dispersibility of the OM nanoparticles with decanoic acid was evaluated in the same manner as in Example 6-1, except that the composite OM nanoparticles were replaced with OM nanoparticles with decanoic acid similar to those in Example 2. As a result, it was confirmed that the OM nanoparticles were not properly dispersed by both visual observation and observation by dynamic light scattering.

[0146] [Comparative Example 6-2] Dispersion of OM nanoparticles in a solvent using stearic acid [Preparation of organically modified nanoparticles using stearic acid] OM nanoparticles using stearic acid were obtained in the same manner as in Example 2, except that the modifier was stearic acid (SA).

[0147] [Dispersibility in Solvent] Except that the composite OM nanoparticles were replaced with OM nanoparticles made from stearic acid, the dispersibility of the OM nanoparticles made from decanoic acid was evaluated in the same manner as in Example 5. As a result, it was confirmed that the OM nanoparticles were not properly dispersed by both visual observation and observation by dynamic light scattering.

[0148] [Discussion] The surface of OM nanoparticles is densely covered with organic modifiers, which prevents solvents with large molecular sizes from penetrating. Even if the solvent has a high affinity for alkyl chains, it does not penetrate, resulting in poor dispersibility.

[0149] According to Test Example 6, copolymerization of carboxylic acids with different chain lengths causes geometric changes in the modifier shell surface, creating additional space at the end of the modifier, the area exposed to the solvent. The difference in chain length creates depressions on the modifier shell surface, creating space to accommodate penetration, which is thought to enable penetration of solvents with large molecular weights.

[0150] Although the Hansen solubility parameter (HSP) values ​​of dodecane are similar to those of DA- and SA-modified nanoparticles, these two monomolecular systems do not disperse in dodecane at concentrations as high as 1 wt%. This is likely due to the size of dodecane preventing efficient penetration of the modifier into the shell. In contrast, the two composite OM nanoparticles were monodispersed at 1 wt%, indicating enhanced interaction between the modifier and the solvent. While the molecular arrangement of the two modifiers within the modifier shell, which affects solvent penetration, has not yet been fully elucidated, this result is likely due to the penetration of larger solvent molecules into the cavity created by the difference in chain length between DA and SA.

[0151] In this way, by adding multiple types of organic modifying groups to the surface, voids are created, and the solvent is trapped within these voids, thereby increasing the apparent solvent affinity of the organically modified nanoparticles, which is effective in improving their dispersibility. However, this is not all. Recent molecular theory research, such as computational science, has revealed that the dispersibility of organically modified nanoparticles is highly dependent on the self-ordering of the organic modifying groups or solvent molecules. In other words, it is expected that dispersibility will be improved based on a principle completely different from that previously known.

[0152] Self-ordering corresponds to the formation of a solid-phase-like structure by molecules, and it is well known that the solubility of solidified molecules in solvents is significantly reduced. The release of self-ordering is equivalent to a change from solid to liquid phase, which increases the degree of freedom of molecular movement, promoting the incorporation of solvent molecules, thereby improving the dispersibility of particles in the solvent. The addition of a third component also creates a freezing point. The addition of a third component lowers the melting point, and the fact that a liquid phase can be formed at the same temperature is well known from the snow-melting effect, etc. This not only has a physical effect, such as the penetration of a third component into the liquid phase, but also leads to a freezing point effect on the organic molecular layer, i.e., the release of self-ordering, i.e., an increase in the degree of freedom of movement of organic molecules (liquid-phase transition).

[0153] Self-ordering can also be suppressed by structural design of the organic molecular layer. By modifying the layers with multiple types of molecules, the modified molecules are less susceptible to self-ordering. To achieve this, domain structures are formed for each molecule, allowing self-ordering to proceed within the domains. However, random modification suppresses the formation of self-ordered structures. The degree of self-ordering suppression is determined by the free volume of the modified molecules; the larger the free volume, the less likely crystallization occurs. Random modification is effectively achieved by a process in which the modified molecules form a homogeneous phase and undergo repeated adsorption and desorption on the surface, as in supercritical hydrothermal synthesis. In principle, the molecules move freely while forming structures, so naturally the free volume increases. In contrast, organic modification under conditions that favor self-ordering at lower temperatures results in a lower free volume, even with the same amount of modification.

[0154] According to Example 6, it is believed that the organic modification of multiple types of molecules can significantly improve the affinity with the solvent by optimizing both the effects of forming a void structure that facilitates physical solvent incorporation and the effect of forming a structure that increases free volume.

Claims

1. A method for producing a nanoparticle dispersion comprising a dispersion step of dispersing an organically modified nanoparticle having an organic modifying group on its surface in a solvent, the solvent containing a poorly dispersible solvent that is poorly dispersible in the organically modified nanoparticle and a predetermined molecule as a third component, with respect to van der Waals volume, at a dispersion treatment temperature and pressure, the van der Waals volume of the predetermined molecule in contact with the surface of the solvent is smaller than the van der Waals volume of the poorly dispersible solvent at said temperature and pressure, the van der Waals volume of the predetermined molecule at said temperature and pressure is smaller than the van der Waals volume of the organic modifying group at said temperature and pressure, with respect to the dispersion power term δD of the Hansen solubility parameters, the absolute value of the difference between the value of the dispersion power term δD of the organic modifying group and the value of the dispersion power term δD of the predetermined molecule at said temperature and pressure is 1.2 MPa1 / 2 or less, and the absolute value of the difference between the value of the dispersion power term δD of the predetermined molecule and the value of the dispersion power term δD of the poorly dispersible solvent at said temperature and pressure is 1.2 MPa1 / 2 or less, A method for dispersing organically modified nanoparticles in a solvent, which induces an increase in the free volume of the organically modified layer.

2. The method according to claim 1, wherein the dispersion step includes a step of accelerating the dispersion of the organically modified nanoparticles in the solvent by increasing the concentration of the third component while the organically modified nanoparticles are in the solvent.

3. The method according to claim 1, wherein the dispersion step includes a step of dispersing the organically modified nanoparticles in the solvent by pressurizing the organically modified nanoparticles to a predetermined pressure, and the temperature and pressure of the gas in contact with the surface of the solvent are the predetermined temperature and the predetermined pressure.

4. The method of claim 3, wherein the organically modified nanoparticles are purified nanoparticles.

5. The method according to claim 3 or 4, wherein the predetermined molecule is a gas or liquefied gas selected from carbon dioxide, a hydrocarbon compound, a nitrogen oxide compound, or a fluorocarbon gas, and the predetermined pressure is a pressurized state of 0.5 MPa or more, or a pressure equal to or higher than the saturated vapor pressure at the dispersion treatment temperature (however, if the dispersion treatment temperature is equal to or higher than the critical temperature, then the pressure equal to or higher than the critical pressure).

6. The method according to claim 1, wherein the solvent is a mixed solvent containing the poorly dispersible solvent and the specific molecule, the poorly dispersible solvent being a main solvent and the specific molecule being a co-solvent.

7. The method according to claim 1, wherein the organically modified nanoparticles have a plurality of types of organic modifying groups on their surfaces as the predetermined molecules, and the free volume of the organically modified molecular layer under the temperature and pressure in the dispersion step is larger than the free volume of a single type of organically modified molecular layer, and the free volume of the organically modified molecular layer is smaller than the van der Waals volume of the solvent molecules.

8. An organically modified nanoparticle dispersion liquid, in which organically modified nanoparticles having organic modifying groups on the surface are dispersed in a solvent, the solvent containing a poorly dispersible solvent in which the organically modified nanoparticles are poorly dispersible and a specified molecule as a third component, and the transmittance at a wavelength of 450 nm when the concentration of the organically modified nanoparticles is 1% by weight is 0.8 or more.

9. The dispersion liquid according to claim 8, wherein the predetermined molecule is a gas or liquefied gas selected from the group consisting of carbon dioxide, a hydrocarbon compound, a nitrogen oxide compound, and a fluorocarbon gas, and the organically modified nanoparticle dispersion liquid is contained in a pressure vessel pressurized to a predetermined pressure of 0.5 MPa or more.

10. The dispersion liquid described in claim 9, wherein, with respect to the dispersion force term δD of the Hansen solubility parameters, the absolute value of the difference between the value of the dispersion force term δD of the chemically modified nanoparticles containing the specified molecules and the molecules of the solvent under the temperature and pressure of the dispersion liquid and the value of the dispersion force term δD of the mixed solvent at the specified pressure is 1.2 MPa1 / 2 or less.

11. The dispersion liquid according to claim 8, wherein the solvent is a mixed solvent containing a first solvent and a second solvent, the first solvent is a main solvent that is poorly dispersible in the organically modified nanoparticles, and the second solvent, including the case of a gas, is a co-solvent whose van der Waals volume at the temperature and pressure of the dispersion liquid is smaller than the van der Waals volume of the organically modified molecular layer of the organically modified nanoparticles, and whose absolute value of the difference between the dispersion force term δD of the Hansen solubility parameters of the organically modified nanoparticles at the temperature and pressure is 1.2 MPa1 / 2 or less.

12. The dispersion liquid described in claim 8, wherein the organically modified nanoparticles have a plurality of types of organic modifying groups on the surface as the predetermined molecules, the free volume of the organically modified molecule layer is larger than the van der Waals volume of the solvent molecules, and the free volume of each of the organically modified molecule layers is larger than the free volume of a single type of organically modified molecule layer.

Citation Information

Patent Citations

  • METHOD OF RECOVERING OR COLLECTION OF METAL OXIDE NANOPARTICLES

    JP3925936B2

  • organically modified microparticles

    JP4336856B2