Resin composition, resin film, prepreg, laminate, printed wiring board, and semiconductor package
The resin composition, combining styrene elastomer, maleimide compounds, and inorganic fillers, addresses the challenge of high-frequency characteristics and surface depressions in printed wiring boards, enhancing their performance and adhesion.
Patent Information
- Application Number
- PCT/JP2024/016783
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-01
- Publication Date
- 2024-11-21
AI Technical Summary
Printed wiring boards face challenges in achieving high-frequency characteristics and preventing surface depressions after desmear treatment, which affects their performance and adhesion with conductors.
A resin composition comprising a styrene elastomer, a maleimide compound, and an inorganic filler, along with a polyphenylene ether derivative and a curing accelerator, is used to enhance high-frequency properties and suppress surface depression formation during desmear treatment.
The resin composition effectively improves high-frequency characteristics and prevents surface depressions, ensuring excellent adhesion and performance in printed wiring boards and semiconductor packages.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resin compositions, resin films, prepregs, laminates, printed wiring boards, and semiconductor packages
[0001] The present disclosure relates to a resin composition, a resin film, a prepreg, a laminate, a printed wiring board, and a semiconductor package.
[0002] Mobile communication devices such as mobile phones, their base station equipment, servers, routers, and other network infrastructure devices, and large-scale computers are increasingly using faster and larger-capacity signals. Accordingly, printed wiring boards used in these electronic devices must be compatible with higher frequencies, and substrate materials with excellent dielectric properties (low dielectric constant and low dielectric loss tangent; hereinafter, sometimes referred to as "high-frequency properties") in high-frequency bands (e.g., 10 GHz or higher) that enable reduced transmission loss are in demand. In recent years, in addition to the electronic devices mentioned above, new systems using high-frequency wireless signals have been planned and put into practical use in the fields of ITS (automotive and transportation systems) and indoor short-range communications. Therefore, it is expected that low-transmission-loss substrate materials will also be required for printed wiring boards used in these devices in the future.
[0003] Under these circumstances, a resin composition containing a specific polyphenylene ether derivative, a specific thermosetting resin, and a styrene-based thermoplastic elastomer (see Patent Document 1) has been proposed, with the objective of providing a resin composition that has particularly good compatibility and also has high-frequency characteristics, high adhesion to conductors, excellent heat resistance, a high glass transition temperature, a low thermal expansion coefficient, and high flame retardancy.
[0004] International Publication No. 2016 / 175326
[0005] In the manufacturing process of printed wiring boards, a desmear treatment is performed on an insulating layer with an aqueous oxidizing agent solution to remove residual components after drilling holes in the insulating layer or to roughen the surface to improve adhesion between the insulating layer and a conductor layer. According to the investigations of the present inventors, it has been found that in copper-clad laminates using a resin composition containing a styrene-based elastomer, depressions with a diameter exceeding approximately 1 μm may occur on the surface of the insulating layer after the desmear treatment.
[0006] In view of the current situation, an object of the present disclosure is to provide a resin composition capable of forming a cured product that has excellent high-frequency characteristics and that suppresses the occurrence of depressions on the surface after desmearing, and to provide a resin film, a prepreg, a laminate, a printed wiring board, and a semiconductor package that use the resin composition.
[0007] As a result of extensive research, the present inventors have found that the resin composition of the present disclosure can achieve the above-mentioned object. The present disclosure includes the following embodiments [1] to
[11] . [1] A resin composition containing a styrene-based elastomer (A) and a maleimide compound (B), wherein the component (A) contains structural units derived from the styrene-based compound in an amount of 5 to 15 mass % or 40 mass % or more based on the total structural units of the component (A). [2] The resin composition according to the above [1], wherein the content of the component (A) is 1 to 50 mass parts per 100 mass parts of the solid content of the resin composition. [3] The resin composition according to the above [1] or [2], wherein the component (B) is one or more selected from the group consisting of maleimide compounds having two or more N-substituted maleimide groups and derivatives thereof. [4] The resin composition according to any one of the above [1] to [3], further containing an inorganic filler (C). [5] The resin composition according to any one of [1] to [4] above, further comprising a polyphenylene ether derivative (D) having an ethylenically unsaturated bond-containing group. [6] The resin composition according to any one of [1] to [5] above, further comprising a curing accelerator (E). [7] A resin film containing the resin composition according to any one of [1] to [6] above or a semi-cured product of the resin composition. [8] A prepreg containing the resin composition according to any one of [1] to [6] above or a semi-cured product of the resin composition. [9] A laminate having a cured product of the resin composition according to any one of [1] to [6] above or a cured product of the prepreg according to [8] above, and a metal foil.
[10] A printed wiring board having one or more members selected from the group consisting of a cured product of the resin composition according to any one of [1] to [6] above, a cured product of the prepreg according to [8] above, and the laminate according to [9] above.
[11] A semiconductor package having the printed wiring board according to
[10] above and a semiconductor element.
[0008] According to the present disclosure, it is possible to provide a resin composition capable of forming a cured product that has excellent high-frequency characteristics and in which the generation of depressions on the resin layer surface after desmearing is suppressed, and to provide a resin film, a prepreg, a laminate, a printed wiring board, and a semiconductor package using the resin composition.
[0009] In the numerical ranges described in this disclosure, the upper or lower limit of the numerical range may be replaced with the values shown in the examples. Furthermore, the lower and upper limits of a numerical range can be arbitrarily combined with the lower or upper limit of another numerical range. In the expression "AA to BB," the numerical values AA and BB at both ends are included as the lower and upper limits, respectively, of the numerical range. In this disclosure, for example, the expression "10 or more" means 10 and a numerical value greater than 10, and this also applies when the numerical values differ. Furthermore, for example, the expression "10 or less" means a numerical value less than 10 and a numerical value less than 10, and this also applies when the numerical values differ. Furthermore, unless otherwise specified, each component and material exemplified in this disclosure may be used alone or in combination of two or more types. In this disclosure, when multiple substances corresponding to each component are present in the resin composition, the content of each component in the resin composition refers to the total amount of the multiple substances present in the resin composition, unless otherwise specified.
[0010] In the present disclosure, the term "resin component" refers to all components of the solid content constituting the resin composition, excluding inorganic compounds such as inorganic fillers, which will be described later. In the present disclosure, the term "solid content" refers to components in the resin composition other than the organic solvent, which will be described later. The expression "containing XX" described in the present disclosure may mean that XX is contained in a reacted state if XX is reactive, or may simply mean that XX is contained as is, or may include both of these aspects. Any combination of the items described in the present disclosure is also included in the present disclosure and the present embodiment.
[0011] [Resin Composition] The resin composition of this embodiment is a resin composition containing a styrene-based elastomer (A) [hereinafter also referred to as component (A)] and a maleimide compound (B) [hereinafter also referred to as component (B)], wherein component (A) contains structural units derived from the styrene-based compound in an amount of 5 to 15 mass % or 40 mass % or more based on the total structural units of component (A). Each component contained in the resin composition of this embodiment will be described below.
[0012] <Styrene-Based Elastomer (A)> The resin composition of this embodiment contains a styrene-based elastomer containing structural units derived from a styrene-based compound in an amount of 5 to 15% by mass or 40% by mass or more, based on all structural units of component (A). The inclusion of a styrene-based elastomer improves high-frequency characteristics, and the presence of the structural units derived from a styrene-based compound in the above-mentioned predetermined amount suppresses the formation of depressions on the surface of the resin layer after desmearing. From the viewpoint of suppressing the formation of depressions on the surface of the resin layer after desmearing, the content of the structural units derived from a styrene-based compound is preferably 7 to 15% by mass or 40 to 55% by mass, more preferably 10 to 15% by mass or 40 to 50% by mass, and even more preferably 10 to 15% by mass or 40 to 45% by mass, based on all structural units of component (A). That is, the "5 to 15% by mass" may independently be 7 to 15% by mass or 10 to 15% by mass, and the "40% by mass or more" may independently be 40 to 55% by mass, 40 to 50% by mass, or 40 to 45% by mass.
[0013] Component (A) is preferably a styrene-based thermoplastic elastomer. As described above, component (A) contains structural units derived from a styrene-based compound, and is preferably a copolymer having structural units derived from a styrene-based compound and structural units derived from a conjugated diene compound. Examples of the styrene-based compound include styrene, α-methylstyrene, p-methylstyrene, and p-tert-butylstyrene. Among these, from the viewpoints of availability and productivity, styrene, α-methylstyrene, and 4-methylstyrene are preferred, and styrene is more preferred. Examples of the conjugated diene compound include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 1,3-pentadiene (piperylene), 1-phenyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-methyl-1,3-pentadiene, 3,4-dimethyl-1,3-hexadiene, and 4,5-diethyl-1,3-octadiene. Among these, from the viewpoints of availability and productivity, 1,3-butadiene and isoprene are preferred, and 1,3-butadiene is more preferred.
[0014] Component (A) may be a hydrogenated styrene-based elastomer in which at least a portion of the structural units derived from the conjugated diene compound are hydrogenated. In this disclosure, the term "styrene-based elastomer" simply refers to a hydrogenated styrene-based elastomer. The hydrogenation rate of the hydrogenated styrene-based elastomer is not particularly limited, but is preferably 50 to 100 mol%, more preferably 70 to 100 mol%, even more preferably 80 to 100 mol%, and particularly preferably 90 to 100 mol%, and may even be 95 to 100 mol%. Examples of hydrogenated styrene-based elastomers include hydrogenated styrene-butadiene-styrene block copolymers (SEBS) and hydrogenated styrene-isoprene-styrene block copolymers (SEPS). Among these, SEBS is preferred. Commercially available SEBS products include the Tuftec (registered trademark) H series and M series manufactured by Asahi Kasei Corporation, the Septon (registered trademark) series manufactured by Kuraray Co., Ltd., and the Kraton (registered trademark) G Polymer series manufactured by Kraton Polymer Japan Co., Ltd.
[0015] The styrene-based elastomer may be modified with a compound having a functional group such as maleic anhydride. For example, the styrene-based elastomer modified with maleic anhydride may be produced by reacting a styrene-based elastomer or a hydrogenated styrene-based elastomer with maleic anhydride, or a commercially available product may be used.
[0016] The styrene-based elastomer preferably has a number average molecular weight of 5,000 to 200,000, more preferably 10,000 to 150,000, and even more preferably 50,000 to 100,000. In the present disclosure, the number average molecular weight is a value determined in terms of standard polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent.
[0017] (Content of Component (A)) The content of the component (A) in the resin composition of the present embodiment is not particularly limited, but from the viewpoint of high-frequency characteristics and suppressing the occurrence of depressions on the surface of the resin layer after desmearing, the content is preferably 1 to 50 parts by mass, more preferably 3 to 40 parts by mass, even more preferably 3 to 35 parts by mass, particularly preferably 3 to 25 parts by mass, and most preferably 3 to 15 parts by mass, relative to 100 parts by mass of the solid content in the resin composition.
[0018] <Maleimide Compound (B)> The resin composition of this embodiment contains a maleimide compound as component (B). By containing a maleimide compound, the resin composition of this embodiment becomes a resin composition with excellent heat resistance and low thermal expansion. The maleimide compound is preferably one or more selected from the group consisting of maleimide compounds having two or more N-substituted maleimide groups [hereinafter, sometimes simply referred to as "maleimide compound (b1)" or "component (b1)"] and derivatives thereof. Examples of the "derivatives thereof" include addition reaction products of maleimide compounds having two or more N-substituted maleimide groups with amine compounds such as diamine compounds described below.
[0019] Specific examples of the maleimide compound (b1) are not particularly limited as long as they are maleimide compounds having two or more N-substituted maleimide groups, and include aromatic maleimide compounds such as bis(4-maleimidophenyl)methane, polyphenylmethane maleimide, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, m-phenylene bismaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, and indane ring-containing aromatic bismaleimide; and aliphatic maleimide compounds such as 1,6-bismaleimido-(2,2,4-trimethyl)hexane and pyrophosphate binder-type long-chain alkyl bismaleimide. Among these, from the viewpoints of adhesion to conductors and mechanical properties, aromatic maleimide compounds are preferred, aromatic bismaleimide compounds are more preferred, and 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane and 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide are even more preferred. Note that an aromatic maleimide compound refers to a compound in which a maleimide group is directly bonded to an aromatic hydrocarbon group, and an aliphatic maleimide compound refers to a compound in which a maleimide group is directly bonded to an aliphatic hydrocarbon group.
[0020] From the viewpoints of solubility in organic solvents, compatibility, adhesion to conductors, and high-frequency characteristics, the maleimide compound is preferably a derivative of maleimide compound (b1). The derivative of maleimide compound (b1) is preferably a modified maleimide compound (hereinafter sometimes abbreviated as "modified maleimide compound (X)" or "component (X)") having a structural unit derived from maleimide compound (b1) and a structural unit derived from an amine compound having a primary amino group (hereinafter sometimes abbreviated as "component (b2)"). The structural unit derived from component (b1) and the structural unit derived from component (b2) contained in modified maleimide compound (X) may each be one type, or a combination of two or more types.
[0021] The modified maleimide compound (X) is preferably a compound having a structure represented by the following formula (B-1), which is formed by an addition reaction between a maleimide group in the component (b1) and a primary amino group in the component (b2): (* indicates the bond position to other structures.)
[0022] The amine compound (b2) is preferably a compound having two or more amino groups, and more preferably a diamine compound having two amino groups. Examples of the amine compound (b2) include 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-dimethyldiphenylmethane, 4,4'-diamino-3,3'-diethyldiphenylmethane, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ketone, 4,4'-diaminobiphenyl, and 3,3'-dimethyl-4,4'-diaminodiphenyl. Aminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diaminodiphenylmethane, 2,2-bis(4-aminophenyl)propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis(3-aminophenoxy)benzene, 1 ,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 1,3-bis[1-[4-(4-aminophenoxy)phenyl]-1-methylethyl]benzene, 1,4-bis[1-[4-(4-aminophenoxy)phenyl]-1-methylethyl]benzene, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, Examples of aromatic diamine compounds include 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline, 3,3'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, and 9,9-bis(4-aminophenyl)fluorene; and amine-modified siloxane compounds having primary amino groups. Here, the aromatic diamine compound refers to a compound in which two amino groups are directly bonded to an aromatic hydrocarbon group.
[0023] Among these, 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-dimethyldiphenylmethane, 4,4'-diamino-3,3'-diethyldiphenylmethane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, and 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline are preferred as component (b2) from the viewpoints of excellent solubility in organic solvents, reactivity with component (b1), and heat resistance. Furthermore, 3,3'-dimethyl-5,5'-diethyl-4,4'-diaminodiphenylmethane is preferred from the viewpoints of excellent high-frequency characteristics and low water absorption. Furthermore, 2,2-bis[4-(4-aminophenoxy)phenyl]propane is preferred from the viewpoints of excellent mechanical properties such as high adhesion to conductors, elongation, and breaking strength. Furthermore, from the viewpoints of excellent solubility in organic solvents, reactivity during synthesis, heat resistance, high adhesion to conductors, as well as excellent high-frequency characteristics and low moisture absorption, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline and 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline are preferred. Furthermore, from the viewpoint of low thermal expansion, amine-modified siloxane compounds are preferred.
[0024] The functional group equivalent weight of the amine-modified siloxane compound is not particularly limited, but is preferably 300 to 3,000 g / mol, more preferably 400 to 2,000 g / mol, and even more preferably 600 to 1,000 g / mol.
[0025] From the viewpoints of heat resistance and low thermal expansion, it is preferable to use a combination of an aromatic diamine compound and an amine-modified siloxane compound as component (b2). The ratio of the aromatic diamine compound and the amine-modified siloxane compound used [aromatic diamine compound / amine-modified siloxane compound] is not particularly limited, but is preferably 20 / 80 to 80 / 20, more preferably 40 / 60 to 70 / 30, and even more preferably 50 / 50 to 65 / 35 by mass ratio.
[0026] The content of the structural units derived from component (b2) in the modified maleimide compound (X) is not particularly limited, but is preferably 5 to 50 mass%, more preferably 8 to 30 mass%, and even more preferably 10 to 15 mass%. When the content of the structural units derived from component (b2) is within this range, excellent high-frequency characteristics, as well as better heat resistance, flame retardancy, and glass transition temperature, tend to be obtained.
[0027] The total content of the structural units derived from the component (b1) and the structural units derived from the component (b2) in the modified maleimide compound (X) is not particularly limited, but is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 100% by mass (i.e., consisting solely of structural units derived from the component (b1) and structural units derived from the component (b2)).
[0028] The content ratio of the structural unit derived from the component (b1) and the structural unit derived from the component (b2) in the modified maleimide compound (X) is not particularly limited. 2 Group derived from the group (-NH 2 The content ratio is such that the equivalent ratio (Ta1 / Ta2) of the total equivalent (Ta1) of groups (including maleimide groups) derived from component (b1) to the total equivalent (Ta2) of groups (including maleimide groups) derived from maleimide groups is preferably 0.05 to 10, more preferably 1 to 5. When the equivalent ratio (Ta1 / Ta2) is within the above range, excellent high-frequency characteristics, and better heat resistance, flame retardancy, and glass transition temperature tend to be obtained.
[0029] (Method for Producing Modified Maleimide Compound (X)) Component (X) can be obtained as a reaction product between component (b1) and component (b2), and can be produced, for example, by reacting component (b1) with component (b2) in an organic solvent. Specifically, a reactor is charged with predetermined amounts of components (b1), (b2), and, if necessary, other components, and the components (b1) and (b2) are subjected to a Michael addition reaction (hereinafter, sometimes abbreviated as "pre-reaction") to obtain modified maleimide compound (X). The reaction conditions for the pre-reaction are not particularly limited, but from the viewpoint of obtaining good reactivity and workability while suppressing gelation, a reaction temperature of 50 to 160°C and a reaction time of 1 to 10 hours are preferred.
[0030] In the pre-reaction, a reaction catalyst may be used as necessary. Examples of the reaction catalyst include acidic catalysts such as p-toluenesulfonic acid; amines such as triethylamine, pyridine, and tributylamine; imidazole compounds such as methylimidazole and phenylimidazole; and phosphorus-based catalysts such as triphenylphosphine. These may be used alone or in combination of two or more. There are no particular restrictions on the amount of the reaction catalyst used, but it is, for example, 0.01 to 5 parts by mass per 100 parts by mass of the total amount of component (b1) and component (b2).
[0031] The weight-average molecular weight (Mw) of the modified maleimide compound (X) is not particularly limited, but is preferably 400 to 10,000, more preferably 1,000 to 5,000, even more preferably 1,500 to 4,000, and particularly preferably 2,000 to 3,000. In the present disclosure, the weight-average molecular weight is a value calculated by gel permeation chromatography (GPC) from a calibration curve using standard polystyrene, and more specifically, a value determined by the measurement method described in the Examples.
[0032] (Content of Component (B)) The content of the thermosetting resin (B) in the resin composition of the present embodiment is not particularly limited, but from the viewpoints of high-frequency characteristics, heat resistance, low thermal expansion, and moldability, it is preferably 10 to 70 parts by mass, more preferably 15 to 60 parts by mass, even more preferably 20 to 50 parts by mass, and particularly preferably 25 to 45 parts by mass, relative to 100 parts by mass of the solid content in the resin composition.
[0033] <Inorganic Filler (C)> The resin composition of this embodiment may contain an inorganic filler as component (C). By including component (C) in the resin composition of this embodiment, the thermal expansion coefficient, heat resistance, and flame retardancy tend to be improved. Examples of component (C) include, but are not limited to, silica, alumina, titanium oxide, mica, beryllia, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay (e.g., calcined clay), molybdenum compounds (e.g., zinc molybdate), talc, aluminum borate, and silicon carbide. One type of component (C) may be used alone, or two or more types may be used in combination. Among these, silica, alumina, mica, and talc are preferred from the viewpoints of thermal expansion coefficient, heat resistance, and flame retardancy, with silica and alumina being more preferred, and silica being even more preferred. Examples of silica include crushed silica, fumed silica, and fused silica (fused spherical silica).
[0034] The shape and particle size of component (C) are not particularly limited, but the particle size is preferably 0.01 to 20 μm, more preferably 0.1 to 10 μm, even more preferably 0.2 to 1 μm, and particularly preferably 0.3 to 0.8 μm. Here, particle size refers to the average particle size, and is the particle size at the point corresponding to 50% volume when a cumulative frequency distribution curve of particle sizes is calculated, with the total volume of particles being 100%. The particle size of component (C) can be measured using a particle size distribution measuring device using a laser diffraction scattering method, for example.
[0035] (Content of Component (C)) When the resin composition of the present embodiment contains the component (C), the content of the component (C) is not particularly limited, but from the viewpoints of the thermal expansion coefficient, heat resistance, and flame retardancy, it is preferably 5 to 70 parts by mass, more preferably 15 to 65 parts by mass, even more preferably 20 to 60 parts by mass, and particularly preferably 30 to 55 parts by mass, per 100 parts by mass of the solid content in the resin composition.
[0036] Furthermore, when component (C) is used, a coupling agent may be used in combination, if necessary, to improve the dispersibility of component (C) and the adhesion between component (C) and the organic components in the resin composition. The coupling agent is not particularly limited, and, for example, a silane coupling agent or a titanate coupling agent can be appropriately selected and used. One coupling agent may be used alone, or two or more coupling agents may be used in combination. The amount of coupling agent used is also not particularly limited. When a coupling agent is used, a so-called integral blending method may be used in which the coupling agent is added after blending component (C) into the resin composition. However, a method in which an inorganic filler is previously surface-treated with a coupling agent by dry or wet processing is preferred. By adopting this method, the characteristics of component (C) can be more effectively expressed.
[0037] When the component (C) is used in this embodiment, in order to improve the dispersibility of the component (C) in the resin composition, the component (C) may be used as a slurry in which the component (C) is dispersed in an organic solvent in advance, as necessary. Examples of the organic solvent include the same organic solvents as those described below.
[0038] <Polyphenylene Ether Derivative (D) Having an Ethylenically Unsaturated Bond-Containing Group> The resin composition of this embodiment may contain a polyphenylene ether derivative having an ethylenically unsaturated bond-containing group as component (D) (hereinafter, simply referred to as "polyphenylene ether derivative (D)"). When the resin composition of this embodiment contains component (D), the high-frequency characteristics are further improved, and the compatibility between components (A) and (B) tends to be improved. Component (D) is preferably a polyphenylene ether derivative having an ethylenically unsaturated bond-containing group at its terminal, and more preferably a polyphenylene ether derivative having ethylenically unsaturated bond-containing groups at both terminals. In the present disclosure, the term "ethylenically unsaturated bond-containing group" refers to a substituent containing a carbon-carbon double bond capable of addition reaction, and does not include a double bond in an aromatic ring. The polyphenylene ether derivative (D) may be used singly or in combination of two or more types.
[0039] Examples of the ethylenically unsaturated bond-containing group include unsaturated aliphatic hydrocarbon groups such as vinyl, allyl, 1-methylallyl, isopropenyl, 2-butenyl, 3-butenyl, and styryl groups; maleimide groups; and groups containing a heteroatom and an ethylenically unsaturated bond, such as groups represented by the following general formula (D-1). Among these, from the viewpoints of high-frequency characteristics, adhesion to conductors, and compatibility between components (A) and (B), the ethylenically unsaturated bond-containing group is preferably a group represented by the following general formula (D-1).
[0040] (In the formula, R d1 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.
[0041] R d1The alkyl group having 1 to 20 carbon atoms represented by may be any of a linear alkyl group, a branched alkyl group, or a cyclic alkyl group, and is preferably a linear alkyl group. The number of carbon atoms in the alkyl group is preferably 1 to 10, more preferably 1 to 5, even more preferably 1 to 3, and particularly preferably 1. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a decyl group, a pentadecyl group, a hexadecyl group, and a heptadecyl group, and among these, a methyl group is preferred. From the viewpoints of high-frequency characteristics, adhesion to a conductor, and compatibility between component (A) and component (B), the group represented by general formula (D-1) is preferably a (meth)acryloyl group (i.e., R d1 is a hydrogen atom or a methyl group), and more preferably a methacryloyl group.
[0042] In the present disclosure, groups that partially contain an unsaturated aliphatic hydrocarbon group, such as a maleimide group and a group represented by the general formula (D-1), but cannot be considered to be an unsaturated aliphatic hydrocarbon group when viewed as a whole, are not included in the "unsaturated aliphatic hydrocarbon group".
[0043] The polyphenylene ether derivative (D) preferably has a group represented by the general formula (D-1) at one end or both ends. When the polyphenylene ether derivative (D) has an ethylenically unsaturated bond-containing group at one end or both ends, it may further have an ethylenically unsaturated bond-containing group at an end other than one end or both ends, but it is preferable that the polyphenylene ether derivative (D) has an ethylenically unsaturated bond-containing group only at both ends. The polyphenylene ether derivative (D) is preferably a polyphenylene ether having methacryloyl groups at both ends.
[0044] The number of ethylenically unsaturated bond-containing groups that the polyphenylene ether derivative (D) has in one molecule is not particularly limited, but is preferably 2 to 5, more preferably 2 to 3, and even more preferably 2. When the number of ethylenically unsaturated bond-containing groups is at least the above-mentioned lower limit, excellent heat resistance and compatibility between the (A) and (B) components tend to be obtained, while when the number is at most the above-mentioned upper limit, excellent flowability and moldability tend to be obtained.
[0045] The polyphenylene ether derivative (D) has a phenylene ether bond and preferably has a structural unit represented by the following general formula (D-2).
[0046] (In the formula, R d2 represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. d1 represents an integer from 0 to 4.)
[0047] R in the general formula (D-2) d2 Examples of the aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by n include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. As the aliphatic hydrocarbon group, an aliphatic hydrocarbon group having 1 to 3 carbon atoms is preferred, an alkyl group having 1 to 3 carbon atoms is more preferred, and a methyl group is even more preferred. d1 represents an integer of 0 to 4, preferably 1 or 2, and more preferably 2. d1 When R is 1 or 2, d2 is preferably substituted at the ortho position on the benzene ring (based on the substitution position of the oxygen atom). d1 is an integer of 2 or more, a plurality of R d2 The structural unit represented by the general formula (D-2) is preferably a structural unit represented by the following general formula (D-2'):
[0048]
[0049] From the viewpoints of high-frequency characteristics, adhesion to a conductor, and compatibility between components (A) and (B), the polyphenylene ether derivative (D) is preferably a compound represented by the following general formula (D-3):
[0050] (In the formula, R d2 and n d1 is as explained in the general formula (D-2). d3 and R d4 Each of n independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. d2 and n d3 Each independently represents an integer of 0 to 4. d4 and n d5 each independently represents an integer of 0 to 20, d4 and n d5 The sum of X is an integer from 1 to 30. d1 represents an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, or a single bond. d1 and Y d2 each independently represents the ethylenically unsaturated bond-containing group.
[0051] R in the general formula (D-3) d3 and R d4 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by R in the general formula (D-2) is explained below. d2 The same applies to the aliphatic hydrocarbon group having 1 to 5 carbon atoms as shown by n d2 and n d3 represents an integer of 0 to 4, preferably an integer of 0 to 3, and more preferably 2 or 3. d2 or n d3 is an integer of 2 or more, a plurality of R d3 R d4 may be the same or different. d4 and n d5 represents an integer of 0 to 20, preferably an integer of 1 to 20, more preferably an integer of 2 to 15, and even more preferably an integer of 3 to 10. d4 or n d5is an integer of 2 or more, d1 They may be the same or different. d4 and n d5 The sum of these is an integer of 1 to 30, preferably an integer of 2 to 25, more preferably an integer of 5 to 20, and even more preferably an integer of 7 to 15.
[0052] X in the general formula (D-3) d1 Examples of the alkylene group having 1 to 5 carbon atoms represented by X include a methylene group, a 1,2-dimethylene group, a 1,3-trimethylene group, a 1,4-tetramethylene group, and a 1,5-pentamethylene group. d1 Examples of the alkylidene group having 2 to 5 carbon atoms represented by X include an ethylidene group, a propylidene group, an isopropylidene group, a butylidene group, an isobutylidene group, a pentylidene group, and an isopentylidene group. d1 Among the groups represented by the formula (I), an isopropylidene group is preferred from the viewpoints of high frequency characteristics, adhesion to a conductor, and compatibility between the components (A) and (B). d1 and Y d2 The preferred embodiment of the ethylenically unsaturated bond-containing group represented by formula (D-3) is as described above. From the viewpoints of high-frequency characteristics, adhesion to a conductor, and compatibility between components (A) and (B), the compound represented by formula (D-3) is preferably a compound represented by formula (D-4) below.
[0053] (In the formula, n d4 and n d5 is as explained in the general formula (D-3). d5 and R d6 Each of X independently represents a hydrogen atom or a methyl group. d2 represents a methylene group or an isopropylidene group.
[0054] [Weight-average molecular weight (Mw) of polyphenylene ether derivative (D)] The weight-average molecular weight (Mw) of the polyphenylene ether derivative (D) is not particularly limited, but is preferably 500 to 7,000, more preferably 800 to 5,000, even more preferably 1,000 to 3,000, and particularly preferably 1,200 to 2,500. When the weight-average molecular weight (Mw) of the (D) component is at least the above-mentioned lower limit, a cured product having the excellent dielectric properties of polyphenylene ether and excellent heat resistance tends to be obtained, while when it is at most the above-mentioned upper limit, excellent moldability tends to be obtained.
[0055] The method for synthesizing the polyphenylene ether derivative (D) is not particularly limited, and known methods for synthesizing and modifying polyphenylene ethers can be applied.
[0056] (Content of Component (D)) When the resin composition of the present embodiment contains component (D), the content of component (D) is not particularly limited, but is preferably 0.1 to 40 parts by mass, more preferably 0.5 to 20 parts by mass, even more preferably 1 to 15 parts by mass, and particularly preferably 2 to 10 parts by mass, per 100 parts by mass of the solid content in the resin composition. When the content of component (D) is equal to or greater than the lower limit, better high-frequency characteristics and compatibility tend to be obtained, and when it is equal to or less than the upper limit, better heat resistance, moldability, and processability tend to be obtained.
[0057] <Curing Accelerator (E)> The resin composition of this embodiment further contains a curing accelerator as component (E), which tends to improve curability and provide better high-frequency characteristics, heat resistance, adhesion to conductors, elastic modulus, and glass transition temperature. When the resin composition of this embodiment contains a curing accelerator (E), a suitable curing accelerator (E) may be appropriately selected depending on the type of thermosetting resin (B) component used. The curing accelerator (E) may be used alone or in combination of two or more types.
[0058] Examples of component (E) include amine-based curing accelerators, imidazole-based curing accelerators, phosphorus-based curing accelerators, organometallic salts, acidic catalysts, and organic peroxides. In this embodiment, imidazole-based curing accelerators are not classified as amine-based curing accelerators. Examples of amine-based curing accelerators include amine compounds having primary to tertiary amines, such as triethylamine, pyridine, tributylamine, dicyandiamide, and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane; and quaternary ammonium compounds. Examples of imidazole-based curing accelerators include imidazole compounds such as methylimidazole, phenylimidazole, 2-undecylimidazole, and isocyanate-masked imidazole (e.g., an addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole). Examples of phosphorus-based curing accelerators include tertiary phosphines such as triphenylphosphine; and quaternary phosphonium compounds such as the addition product of p-benzoquinone and tri-n-butylphosphine. Examples of organic metal salts include carboxylates of manganese, cobalt, zinc, etc. Examples of acidic catalysts include p-toluenesulfonic acid. Examples of organic peroxides include dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3,2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, t-butylperoxyisopropyl monocarbonate, and α,α'-di(t-butylperoxy)diisopropylbenzene. Among these, from the viewpoint of obtaining better high frequency characteristics, heat resistance, adhesion to conductors, elastic modulus, and glass transition temperature, amine-based curing accelerators, imidazole-based curing accelerators, and phosphorus-based curing accelerators are preferred, and dicyandiamide, imidazole-based curing accelerators, and quaternary phosphonium compounds are more preferred, and it is even more preferred to use these in combination. In this case, an organic peroxide may also be used in combination, but from the viewpoint of the physical properties of the cured product, it is preferable not to contain an organic peroxide.
[0059] (Content of Component (E)) When the resin composition of the present embodiment contains the component (E), the content of the component (E) is not particularly limited, but is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, still more preferably 0.1 to 4 parts by mass, and particularly preferably 0.5 to 3 parts by mass, per 100 parts by mass of the resin component. When the content of the curing accelerator (E) is within the above range, better high-frequency characteristics, heat resistance, storage stability, and moldability tend to be obtained.
[0060] <Other Components> The resin composition of this embodiment may further contain one or more optional components, such as resin materials other than the above-mentioned components, flame retardants, flame retardant assistants, antioxidants, heat stabilizers, antistatic agents, UV absorbers, pigments, colorants, lubricants, and silane coupling agents, as necessary. Each of the optional components may be used alone or in combination of two or more. Examples of resin materials other than the above-mentioned components include thermosetting resins other than maleimide compounds. The thermosetting resin preferably contains one or more selected from the group consisting of epoxy resins, phenolic resins, polyimide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, and melamine resins.
[0061] When the resin composition of this embodiment contains the optional components, their contents are not particularly limited, and may be 0.01 parts by mass or more, 0.1 parts by mass or more, 0.5 parts by mass or more, or 30 parts by mass or less, 10 parts by mass or less, 5 parts by mass or less, or 1 part by mass or less, per 100 parts by mass of the total of the resin components. Furthermore, the resin composition of this embodiment may not contain the optional components, depending on the desired performance.
[0062] The total content of components (A) to (E) in the resin components contained in the resin composition of the present embodiment is not particularly limited, but is preferably 80 parts by mass or more, more preferably 90 parts by mass or more, and even more preferably 95 parts by mass or more, per 100 parts by mass of the solid content in the resin composition, and may be 100 parts by mass.
[0063] (Organic Solvent) The resin composition of this embodiment may be a varnish-like resin composition containing an organic solvent, from the viewpoint of ease of handling and ease of production of the prepreg described below. Examples of the organic solvent include alcohol-based solvents such as ethanol, propanol, butanol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based solvents such as tetrahydrofuran; aromatic solvents such as toluene, xylene, and mesitylene; nitrogen-containing solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; sulfur-containing solvents such as dimethyl sulfoxide; and ester-based solvents such as γ-butyrolactone. These organic solvents may be used alone or in combination of two or more.
[0064] When the resin composition of this embodiment contains an organic solvent, its content is not particularly limited, but is preferably an amount such that the solids concentration of the resin composition of this embodiment is 30 to 90 mass%, more preferably 40 to 80 mass%, and even more preferably 50 to 70 mass%. When the organic solvent content is within the above range, the resin composition is easy to handle, and the impregnation into the substrate and the appearance of the produced prepreg are good. Furthermore, this makes it easy to adjust the solids concentration of the resin in the prepreg, as described below, and tends to make it easier to produce a prepreg with a desired thickness.
[0065] <Dielectric Properties> When a test specimen is prepared from the resin composition of this embodiment by the method described in the Examples below, the dielectric constant (Dk) at 10 GHz is not particularly limited, but is preferably 4.0 or less, more preferably 3.7 or less, even more preferably 3.3 or less, and can even be 3.1 or less. The smaller the dielectric constant (Dk), the better. There is no particular restriction on the lower limit of the dielectric constant (Dk). However, taking into account the balance with other physical properties, the dielectric constant (Dk) may be, for example, 2.5 or more, or even 2.8 or more. That is, the dielectric constant (Dk) may be 2.5 to 4.0. When a test specimen is prepared from the resin composition of this embodiment by the method described in the Examples below, the dielectric loss tangent (Df) at 10 GHz is not particularly limited, but is preferably 0.0040 or less, more preferably 0.0038 or less, even more preferably 0.0035 or less, particularly preferably 0.0034 or less, most preferably 0.0033 or less, and can even be 0.0032 or less. The smaller the dielectric loss tangent (Df), the better. There is no particular restriction on the lower limit of the dielectric loss tangent (Df). However, taking into consideration the balance with other physical properties, the dielectric loss tangent (Df) may be, for example, 0.0020 or more, 0.0025 or more, 0.0028 or more, or 0.0029 or more. In other words, the dielectric loss tangent (Df) may be 0.0025 to 0.0040. The dielectric constant (Dk) and the dielectric loss tangent (Df) are values measured in accordance with the cavity resonator perturbation method, and more specifically, are values measured by the method described in the examples. In addition, in the present disclosure, when simply referring to dielectric constant, it means relative dielectric constant.
[0066] The resin composition of this embodiment can be produced by mixing components (A) and (B) and, if necessary, other components, using a known method. In this process, each component may be dissolved or dispersed in the organic solvent while stirring. The mixing order, temperature, time, and other conditions are not particularly limited and can be set as desired.
[0067] [Resin Film] The resin film of this embodiment is a resin film containing the resin composition of this embodiment or a semi-cured product of the resin composition. The resin film of this embodiment can be produced, for example, by applying a resin composition containing an organic solvent, i.e., a varnish, to a support, drying it by heating, and semi-curing (B-staging) as needed. The thickness of the resin film is not particularly limited, but is preferably 1 to 100 μm, more preferably 3 to 70 μm, and even more preferably 5 to 35 μm. Examples of the support include plastic film, metal foil, and release paper. The drying temperature and drying time can be determined appropriately depending on the amount of organic solvent used, the boiling point of the organic solvent, and the like. However, a resin film can be suitably formed by drying at 50 to 200°C for about 1 to 10 minutes.
[0068] [Prepreg] The prepreg of this embodiment is a prepreg containing the resin composition of this embodiment or a semi-cured product of the resin composition. The prepreg of this embodiment contains, for example, the resin composition of this embodiment or a semi-cured product of the resin composition and a sheet-like fiber substrate. The prepreg is formed using the resin composition of this embodiment or the resin film and a sheet-like fiber substrate. For example, the prepreg can be obtained by impregnating a sheet-like fiber substrate with the resin composition of this embodiment or the resin film, followed by heating and drying to semi-cure (B-staging) as needed. More specifically, the prepreg of this embodiment can be produced by, for example, heating and drying in a drying oven, typically at 80 to 200°C for 1 to 30 minutes to semi-cure (B-staging). Here, in this disclosure, B-staging refers to achieving a B-stage state as defined in JIS K6900 (1994). The amount of resin composition used can be determined appropriately so that the solids concentration derived from the resin composition in the prepreg after drying is 30 to 90% by mass. By setting the solid content concentration within the above range, better moldability tends to be obtained when the laminate is formed.
[0069] As the sheet-like fiber substrate for the prepreg, known materials used in various laminates for electrical insulating materials are used. Examples of materials for the sheet-like fiber substrate include inorganic fibers such as E-glass, D-glass, S-glass, and Q-glass; organic fibers such as polyimide, polyester, and tetrafluoroethylene; and mixtures thereof. These sheet-like fiber substrates have shapes such as woven fabric, nonwoven fabric, roving, chopped strand mat, and surfacing mat. The thickness of the sheet-like fiber substrate is not particularly limited, but may be 1 to 100 μm, 3 to 70 μm, 5 to 55 μm, 15 to 55 μm, or 25 to 55 μm.
[0070] [Laminate] The laminate of this embodiment is a laminate having a cured product of the resin composition of this embodiment or a cured product of the prepreg of this embodiment and a metal foil. The laminate of this embodiment can be produced, for example, by placing a metal foil on one or both sides of a resin film of this embodiment, or by placing a metal foil on one or both sides of a laminate obtained by stacking two or more resin films of this embodiment, followed by hot-press molding. In the laminate obtained by this production method, the resin film of this embodiment is C-staged. Another embodiment of the laminate of this embodiment can be produced, for example, by placing a metal foil on one or both sides of a prepreg of this embodiment, or by placing a metal foil on one or both sides of a laminate obtained by stacking two or more prepregs of this embodiment, followed by hot-press molding. In the laminate obtained by this production method, the prepreg of this embodiment is C-staged. In the present disclosure, C-staging refers to achieving the C-stage state defined in JIS K6900 (1994). A laminate having a metal foil is sometimes referred to as a metal-clad laminate. The metal of the metal foil is not particularly limited, but from the viewpoint of electrical conductivity, it may be copper, gold, silver, nickel, platinum, molybdenum, ruthenium, aluminum, tungsten, iron, titanium, chromium, or an alloy containing one or more of these metal elements. Copper and aluminum are preferred, and copper is more preferred. The method for carrying out the hot-press molding is not particularly limited, but can be carried out, for example, under conditions of a temperature of 100 to 300°C, a pressure of 0.2 to 10 MPa, and a time of 0.1 to 5 hours. Furthermore, the hot-press molding can be carried out using a vacuum press or the like to maintain a vacuum state for 0.5 to 5 hours.
[0071] [Printed Wiring Board] The printed wiring board of this embodiment has a cured product of the resin composition of this embodiment. It can also be said that the printed wiring board of this embodiment is a printed wiring board having one or more materials selected from the group consisting of a cured product of the thermosetting resin composition of this embodiment, a cured product of the prepreg of this embodiment, and a laminate of this embodiment. The printed wiring board of this embodiment can be manufactured by performing circuit formation processing such as drilling, metal plating, and etching of metal foil using one or more materials selected from the group consisting of the prepreg of this embodiment, the resin film of this embodiment, and the laminate of this embodiment, using a known method. Furthermore, a multilayer printed wiring board can also be manufactured by further performing multilayer adhesive processing as necessary. In the printed wiring board of this embodiment, the prepreg of this embodiment and the resin film of this embodiment are C-staged.
[0072] [Semiconductor Package] The semiconductor package of this embodiment is a semiconductor package including the printed wiring board of this embodiment and a semiconductor element. The semiconductor package of this embodiment can be manufactured by mounting semiconductor elements such as semiconductor chips and memories at predetermined positions on the printed wiring board of this embodiment.
[0073] The resin composition, resin film, prepreg, laminate, printed wiring board, and semiconductor package of the present embodiment can be suitably used in electronic devices that handle high-frequency signals of 10 GHz or more. In particular, the printed wiring board is useful as a printed wiring board for millimeter-wave radar.
[0074] Although preferred embodiments have been described above, these are merely examples for the purpose of explaining the present disclosure, and the scope of the present disclosure is not intended to be limited to these embodiments. The present disclosure also includes various aspects that differ from the above-described embodiments without departing from the gist of the disclosure.
[0075] The present embodiment will be described in more detail below with reference to examples, although the present disclosure is not limited to the following examples.
[0076] In each example, the weight average molecular weight (Mw) was measured by the following method. It was calculated by gel permeation chromatography (GPC) from a calibration curve using standard polystyrene. The calibration curve was approximated by a cubic equation using standard polystyrene: TSKstandard POLYSTYRENE (Types: A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40) [manufactured by Tosoh Corporation, trade name]. The GPC measurement conditions are shown below. Apparatus: Pump: L-6200 type [manufactured by Hitachi High-Technologies Corporation] Detector: L-3300 type RI [manufactured by Hitachi High-Technologies Corporation] Column oven: L-655A-52 [manufactured by Hitachi High-Technologies Corporation] Column: Guard column; TSK Guard column HHR-L + column; TSKgel G4000HHR + TSKgel G2000HHR (all manufactured by Tosoh Corporation, trade names) Column size: 6.0 x 40 mm (guard column), 7.8 x 300 mm (column) Eluent: tetrahydrofuran Sample concentration: 30 mg / 5 mL Injection volume: 20 μL Flow rate: 1.00 mL / min Measurement temperature: 40°C
[0077] [Production Example 1: Production of Modified Maleimide Compound (X-1) (Component (B))] 100 parts by mass of 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, 5.6 parts by mass of a siloxane compound (functional group equivalent: 750 g / mol) having amino groups at both ends, 7.9 parts by mass of 3,3'-diethyl-4,4'-diaminodiphenylmethane, and 171 parts by mass of propylene glycol monomethyl ether were added to a 5 L reactor equipped with a thermometer, a stirrer, and a reflux condenser and moisture content monitor, and the mixture was allowed to react under reflux for 2 hours. The mixture was concentrated at reflux temperature for 3 hours to produce a modified maleimide compound (X-1) solution with a solids concentration of 65% by mass. The weight-average molecular weight (Mw) of the resulting modified maleimide compound (X-1) was approximately 2,700.
[0078] Examples 1-2, Comparative Examples 1-3 (Preparation of Resin Composition) The components listed in Table 1 were mixed with 58 parts by weight of toluene and 10 parts by weight of methyl isobutyl ketone at room temperature, stirring to prepare a resin composition with a solids concentration of 55-65% by weight. (Production of Resin Film) The resin composition was applied to a 0.050 mm-thick PET film using a coating machine, and the film was dried by heating at 120°C for 3 minutes to produce a resin-coated PET film with a resin thickness of 25 μm. (Production of Double-Sided Copper-Clad Laminate) The resin surfaces of the resin-coated PET films were bonded together using vacuum pressure lamination (temperature 110°C, pressure 0.5 MPa). The process of peeling one side of the PET film and bonding the resin surface of another resin-coated PET film to the exposed resin surface was repeated until the resin thickness reached 325 μm. The double-sided PET film of this 325 μm thick resin-coated PET film was peeled off, and 18 μm thick low-profile copper foil (BF-ANP18, M-side Rz: 1.5 μm, manufactured by CIRCUIT FOIL) was laminated on top and bottom of the resin so that the M-side was in contact with the resin, and this laminate was placed in a 300 μm thick mold. Next, it was heated and press-molded at a temperature of 230°C, a pressure of 3.0 MPa, and a time of 90 minutes to produce a double-sided copper-clad laminate.
[0079] [Evaluation Method] The double-sided copper-clad laminate obtained in each example was evaluated according to the following methods. The results are shown in Table 1.
[0080] (1. Confirmation of Presence or Absence of Depressions) The double-sided copper-clad laminate obtained in each example was immersed in a copper etching solution to remove the copper foil, and a desmear treatment was carried out by carrying out the following steps (1) to (4) in order to prepare a resin board. (1) The board was immersed in a swelling solution (manufactured by Atotech Japan Co., Ltd., product name "Swelling Dip Securigant P", glycol ethers, aqueous solution of sodium hydroxide) at 60°C for 10 minutes, and then washed with water. (2) The board was immersed in a roughening solution (manufactured by Atotech Japan Co., Ltd., product name "Concentrate Compact P", KMnO 4(3) The plate was immersed in a neutralizing solution (aqueous solution of sulfuric acid, "Reduction Showreusin Securigant P" manufactured by Atotech Japan Co., Ltd.) at 40°C for 5 minutes, and then washed with water. (4) The plate was dried at 80°C for 10 minutes.
[0081] The surface of the resin plate (resin layer) after the desmear treatment obtained above was observed using a scanning electron microscope (SEM) (manufactured by Hitachi High-Technologies Corporation, product name: SV-4700) under conditions of secondary electron mode, accelerating voltage 10 kV, and observation magnification 5,000 times. In the obtained surface SEM image, a depression having a size exceeding 1.0 μm on the surface of the resin plate (resin layer) was designated as "present," and a depression having no size exceeding 1.0 μm on the surface of the resin plate (resin layer) was designated as "absent." Note that the size of the depression here means the length of the longest straight line that can be drawn within the depression area in a planar view of the resin plate.
[0082] (2. High-Frequency Characteristics) A resin plate was prepared under the same conditions as in the above "Confirmation of the Presence or Absence of Depressions" and cut into a length of 60 mm and a width of 2 mm to serve as a test piece, and the dielectric constant and dielectric loss tangent were measured by the cavity resonator perturbation method. The measuring instrument used was a vector network analyzer "N5227A" manufactured by Agilent Technologies, the cavity resonator was "CP129" (10 GHz band resonator) manufactured by Kanto Electronics Application Development Co., Ltd., and the measurement program was "CPMA-V2". The measurement was carried out under conditions of a frequency of 10 GHz and a measurement temperature of 25°C.
[0083] (3. Evaluation of Copper Foil Peel Strength) The copper foil peel strength of the double-sided copper-clad laminate obtained in each example was measured by peeling the copper foil in a 90° direction in accordance with JIS C6481 (1996). The pulling speed was 50 mm / min. The copper foil peel strength was sufficient if it was 0.5 kN / m or more.
[0084]
[0085] The abbreviations for each material in Table 1 are as follows: [Component (A)] SEBS_A-1: Hydrogenated styrene-based elastomer (manufactured by Asahi Kasei Corporation, trade name "Tuftec (registered trademark) H1221"), styrene content 12% SEBS_A-2: Hydrogenated styrene-based elastomer (manufactured by Asahi Kasei Corporation, trade name "Tuftec (registered trademark) H1517"), styrene content 43% [Component (A'): Styrenic elastomer other than component (A)] SEBS_A'-3: Hydrogenated styrene-based elastomer (manufactured by Asahi Kasei Corporation, trade name "Tuftec (registered trademark) H1052"), styrene content 20% SEBS_A'-4: Hydrogenated styrene-based elastomer (manufactured by Asahi Kasei Corporation, trade name "Tuftec (registered trademark) H1041"), styrene content 30% SEBS_A'-5: maleic anhydride-modified hydrogenated styrene-based elastomer (manufactured by Asahi Kasei Corporation, product name "Tuftec (registered trademark) M1913"), acid value 10 mg CH 3 ONa / g, styrene content 30%
[0086] [Component (B)] Modified maleimide compound: modified maleimide compound (X-1) prepared in Production Example 1. [Component (C)] Silica: spherical fused silica, average particle size: 0.5 μm, 70% by mass slurry of methyl isobutyl ketone.
[0087] [Component (D)] Polyphenylene ether derivative having an ethylenically unsaturated bond-containing group: polyphenylene ether having methacryloyl groups at both ends (weight average molecular weight (Mw): 1,700) [Component (E)] Curing accelerator E-1: p-benzoquinone and tri-n-butylphosphine addition product Curing accelerator E-2: 2-undecylimidazole Curing accelerator E-3: N-2-(aminoethyl)-3-aminopropyltrimethoxysilane
[0088] As is clear from the results shown in Table 1, the copper-clad laminates of Examples 1 and 2, which were produced using the resin composition of this embodiment, had excellent high-frequency characteristics, but did not suffer from the depressions on the resin layer that occurred in the copper-clad laminates of Comparative Examples 1 to 3. The copper-clad laminates of Examples 1 and 2 also had excellent copper foil peel strength.
Claims
1. A resin composition containing a styrene-based elastomer (A) and a maleimide compound (B), wherein the (A) component contains 5 to 15 mass % or 40 mass % or more of structural units derived from a styrene-based compound, based on the total structural units of the (A) component.
2. The resin composition according to claim 1, wherein the content of said component (A) is 1 to 50 parts by mass per 100 parts by mass of the solid content in the resin composition.
3. The resin composition according to claim 1, wherein the component (B) is at least one member selected from the group consisting of maleimide compounds having two or more N-substituted maleimide groups and derivatives thereof.
4. The resin composition according to claim 1, further comprising an inorganic filler (C).
5. The resin composition according to claim 1, further comprising a polyphenylene ether derivative (D) having an ethylenically unsaturated bond-containing group.
6. The resin composition according to claim 1, further comprising a curing accelerator (E).
7. A resin film containing the resin composition according to claim 1 or a semi-cured product of said resin composition.
8. A prepreg containing the resin composition according to claim 1 or a semi-cured product of said resin composition.
9. A laminate comprising a cured product of the resin composition according to claim 1 or a cured product of the prepreg according to claim 8, and a metal foil.
10. A printed wiring board having a cured product of the resin composition according to claim 1.
11. A semiconductor package comprising the printed wiring board according to claim 10 and a semiconductor element.
Citation Information
Patent Citations
Thermosetting resin composition, prepreg, copper-clad laminate and printed wiring board
JP2017149859A
Resin varnish, resin composition, prepreg, laminate sheet, multilayer printed wiring board and preservation method of resin varnish
JP2019006878A
Resin composition, prepreg, laminate sheet, multilayer printed wiring board and semiconductor package
JP2019006879A
Maleimide resin composition, prepreg, resin film, laminate, multilayer printed wiring board, and semiconductor package
JP2022122542A
Resin composition, prepreg, laminate, resin film, multilayer printed wiring board, semiconductor package, method for producing resin composition and modified conjugated diene polymer
JP2022162795A