Iron-containing FER-type zeolite and method for producing same
The direct crystallization of iron-containing FER type zeolite without expensive organic agents addresses the industrial impracticality and efficiency limitations of conventional methods, achieving improved nitrogen oxide reduction and reduced oxygen production at low temperatures.
Patent Information
- Application Number
- PCT/JP2024/017079
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional iron-containing FER type zeolites used for nitrogen oxide reduction are expensive due to the requirement of expensive organic structure directing agents like hexamethylimine, making them industrially impractical, and they have limited nitrogen oxide reduction efficiency at low temperatures with high production of oxygen by-products.
An iron-containing FER type zeolite is developed through direct crystallization without expensive organic structure directing agents, with controlled raw materials and conditions, achieving higher iron dispersion and reduced oxygen production, and improved nitrogen oxide reduction properties at low temperatures.
The method allows for the production of an industrially applicable FER type zeolite with enhanced nitrogen oxide reduction capabilities at low temperatures while minimizing oxygen production, using a cost-effective process without expensive organic agents.
Smart Images

Figure JP2024017079_21112024_PF_FP_ABST
Abstract
Description
Iron-containing FER-type zeolite and method for producing the same
[0001] The present disclosure relates to an iron-containing FER-type zeolite and a method for producing the same.
[0002] FER-type zeolite containing iron as a transition metal element is 2 It has been investigated as a transition metal-containing zeolite that can be used as a nitrogen oxide reduction catalyst in which the by-production of O is suppressed (for example, Patent Documents 1 to 4).
[0003] For example, Patent Documents 1 to 3 report that iron can be incorporated into FER zeolite by post-treatment by mixing FER zeolite with an aqueous solution containing an iron salt such as iron nitrate. Patent Document 4 reports that iron-containing FER zeolite can be directly obtained by crystallizing a raw material containing iron.
[0004] Japanese Patent Publication No. 2017-510437 Japanese Patent Publication No. 2017-512630 Japanese Patent Publication No. 2007-537858 Chinese Patent Publication No. 114345402
[0005] Catalysis Communications, 2017, 89, 133-147 Journal of Catalysis, 2009, 261, 27-34
[0006] Compared with the FER zeolites containing iron by post-treatment disclosed in Patent Documents 1 to 3, the directly crystallized iron-containing FER zeolite disclosed in Patent Document 4 has high nitrogen oxide reduction properties. However, the crystallization in Patent Document 4 requires expensive hexamethylimine as an essential raw material, and therefore the resulting FER zeolite is also expensive, making it difficult to apply industrially.
[0007] The present disclosure provides a novel method for reducing nitrogen oxides using iron-containing FER-type zeolites, which has a higher N 2 The present invention aims to provide at least one of a FER-type zeolite that produces little O and is industrially applicable, a method for producing the same, and a nitrogen oxide reduction catalyst containing the same.
[0008] In the present disclosure, an improvement in the nitrogen oxide reduction properties of iron-containing FER zeolite was investigated. As a result, it was found that iron-containing FER zeolite can be directly crystallized without requiring an expensive organic structure-directing agent such as hexamethylimine by controlling the raw materials and conditions for crystallization. Furthermore, such iron-containing FER zeolite has a different state of iron existence and a high degree of iron dispersion compared to conventional iron-containing FER zeolites, and also has a higher N reduction property in nitrogen oxide reduction at low temperatures compared to conventional iron-containing FER zeolites. 2 It was found that the generation of O can be further suppressed.
[0009] That is, the present invention is as described in the claims, and the gist of the present disclosure is as follows. [1] A FER zeolite containing iron, wherein the area ratio of a spectral peak having a wavelength of 300 nm or more and 600 nm or less to the peak having a wavelength of 190 nm or more and 600 nm or less in a UV-VIS spectrum is 20% or less. [2] The FER zeolite according to the above [1], wherein the area ratio of a spectral peak having a wavelength of more than 400 nm and 600 nm or less to the peak having a wavelength of 190 nm or more and 600 nm or less in a UV-VIS spectrum is 20% or less. [3] The FER zeolite according to the above [1] or [2], wherein the area ratio of a spectral peak having a wavelength of 190 nm or more and less than 300 nm to the peak having a wavelength of 190 nm or more and 600 nm or less in a UV-VIS spectrum is 80% or more. [4] The FER zeolite according to any one of [1] to [3] above, having an iron content of 5 mass% or less. [5] The FER zeolite according to any one of [1] to [4] above, having a molar ratio of silica to alumina of 5 or more and 50 or less. [6] The FER zeolite according to any one of [1] to [5] above, containing one or more elements selected from the group consisting of copper (Cu), manganese (Mn), zirconium (Zr), yttrium (Y), cerium (Ce), lanthanum (La), and calcium (Ca). [7] A FER zeolite according to any one of [1] to [5] above, containing a silica-alumina source, an iron source, an alkali source, water, and seed crystals, and containing SiO 2[8] The method for producing FER-type zeolite according to any one of [1] to [6] above, comprising a step of crystallizing a composition having a molar ratio of iron to silicon converted of less than 0.1. [9] The method for producing FER-type zeolite according to [7] above, wherein the alkali source includes at least a sodium source or a potassium source.
[0010] [9] The method for producing a FER-type zeolite according to the above [7] or [8], wherein the composition has the following molar composition: In the following molar composition, M is an alkali metal: SiO 2 / Al 2 O 3 =5 or more and 50 or less Fe / SiO 2 = More than 0 and less than 0.1 M / SiO 2 = 0.05 or more and less than 0.40 K / M = 0 or more and 0.9 or less H 2 O / SiO 2 = 5 or more and 50 or less
[10] The production method according to any one of [7] to [9] above, wherein the seed crystals are one or more selected from the group consisting of CHA type zeolite, AEI type zeolite, MOR type zeolite, FER type zeolite, and AFX type zeolite.
[11] The production method according to any one of [7] to
[10] above, wherein the content of seed crystals in the raw material composition is more than 0 mass% and 10 mass% or less.
[12] The production method according to at least one of [7] to
[11] above, which does not contain an organic structure-directing agent source.
[13] The production method according to at least one of [7] to
[11] above, which contains one or more organic structure-directing agent sources selected from the group consisting of pyridine, pyrrolidine, cyclohexylamine, and butylamine.
[14] A nitrogen oxide reduction catalyst comprising the FER type zeolite according to any one of [1] to [6] above.
[15] A method for reducing nitrogen oxides, comprising a step of contacting a nitrogen oxide-containing gas with a nitrogen oxide reduction catalyst containing the FER-type zeolite according to any one of [1] to [6] above.
[0011] According to the present disclosure, the N zeolite containing iron has a higher efficiency in reducing nitrogen oxides than conventional iron-containing FER-type zeolites. 2The present invention provides at least one of a FER-type zeolite that produces little O and is industrially applicable, a method for producing the same, and a nitrogen oxide reduction catalyst containing the same.
[0012] UV-VIS spectrum of the iron-containing FER type zeolite of Example 1UV-VIS spectrum of the iron-containing FER type zeolite of Example 1 (after waveform separation)UV-VIS spectrum of the iron-containing FER type zeolite of Example 3UV-VIS spectrum of the iron-containing FER type zeolite of Example 3 (after waveform separation)UV-VIS spectrum of the iron-containing FER type zeolite of Comparative Example 1UV-VIS spectrum of the iron-containing FER type zeolite of Comparative Example 1 (after waveform separation)
[0013] Hereinafter, the present disclosure will be described with reference to an example of an embodiment.
[0014] "Zeolite" is a compound having a regular structure in which skeleton atoms (hereinafter also referred to as "T atoms") are connected via oxygen (O), and the T atoms are at least one of metal atoms and / or metalloid atoms. The metal atoms include one or more selected from the group consisting of aluminum (Al), titanium (Ti), iron (Fe), zinc (Zn), gallium (Ga), and tin (Sn), with at least one of aluminum and iron being preferred, and aluminum being more preferred. The metalloid atoms include one or more selected from the group consisting of boron (B), silicon (Si), germanium (Ge), arsenic (As), antimony (Sb), and tellurium (Te), with silicon being preferred.
[0015] A "zeolite-like substance" is a compound having a regular structure in which T atoms are oxygen-mediated, and the T atoms contain at least an atom other than a metal or a metalloid (hereinafter also referred to as a "non-metal atom"). An example of a non-metal atom is phosphorus (P). Examples of zeolite-like substances include complex phosphorus compounds containing phosphorus (P) as the T atom, such as aluminophosphate (AlPO) and silicoaluminophosphate (SAPO). For clarity, in this embodiment, zeolite does not include zeolite-like substances.
[0016] The "ordered structure (hereinafter also referred to as "zeolite structure")" of zeolite and zeolite-like substances is a skeletal structure specified by a structure code (hereinafter also simply referred to as "structure code") defined by the Structure Commission of the International Zeolite Association. For example, the FER structure is a skeletal structure specified by the structure code "FER." Identification of a zeolite structure can be performed by comparing it with an XRD pattern (hereinafter also referred to as a "reference pattern") described in the CHA section of Zeolite Framework Types on the IZA Structure Commission's website, http: / / www.iza-structure.org / databases / . In the present embodiment, the terms zeolite structure, skeletal structure, crystalline structure, and crystalline phase are used interchangeably.
[0017] In the present embodiment, "-type zeolite" such as "FER-type zeolite" means a zeolite having a zeolite structure of the corresponding structure code.
[0018] An "aluminosilicate" is a composite oxide having a structure consisting of a repeating network of aluminum (Al) and silicon (Si) via oxygen (O). Among aluminosilicates, those that have a crystalline XRD peak in their powder X-ray diffraction (hereinafter also referred to as "XRD") pattern are called "crystalline aluminosilicates," and those that do not have a crystalline XRD peak are called "amorphous aluminosilicates."
[0019] The XRD pattern in this embodiment is an XRD pattern obtained by XRD measurement under the following conditions: Acceleration current / voltage: 40 mA / 40 kV Radiation source: CuKα radiation (λ=1.5405 Å) Measurement mode: Step scan Scan condition: 40° / min Measurement time: 3 seconds Measurement range: 2θ=3° to 43° Divergence vertical limiting slit: 10 mm Divergence / entrance slit: 1° Receiving slit: open Receiving solar slit: 5° Detector: Semiconductor detector (D / teX Ultra) Filter: Ni filter
[0020] The XRD pattern can be measured using a general powder X-ray diffractometer (for example, UltimaIV Protectus, manufactured by Rigaku Corporation). A crystalline XRD peak is a peak whose peak top 2θ is identified and detected in an analysis of an XRD pattern using general analysis software, and in particular, an XRD peak whose half-width is 2θ=0.50° or less. [Iron-Containing FER-Type Zeolite] This embodiment is a FER-type zeolite that contains iron and in which the area ratio of the peak in the spectrum having a wavelength of 300 nm or more and 600 nm or less to the peak in the wavelength of 190 nm or more and 600 nm or less in the UV-VIS spectrum is 20% or less.
[0021] This embodiment relates to a FER-type zeolite containing iron (hereinafter also referred to as "iron-containing FER-type zeolite"), which is a zeolite having a crystal structure consisting of only the FER structure, and further, a FER-type crystalline aluminosilicate. By containing iron (Fe), it exhibits nitrogen oxide reduction properties. Furthermore, compared to FER-type zeolite containing copper, it exhibits nitrogen oxide reduction properties. 2 Nitrogen oxides can be reduced while suppressing the generation of O.
[0022] In the iron-containing FER-type zeolite of this embodiment, the peak top of the XRD peak of the (200) plane in the XRD pattern is 2θ=9.5±0.2°.
[0023] In the iron-containing FER zeolite of this embodiment, the area ratio of the peaks in the spectrum with wavelengths of 300 nm or more and 600 nm or less to the peaks in the wavelengths of 190 nm or more and 600 nm or less in the UV-VIS spectrum (hereinafter also referred to as the "300 nm-600 nm spectral intensity ratio") is 20% or less. In the UV-VIS spectrum of the iron-containing FER zeolite, the presence of iron can be confirmed by the presence of peaks with wavelengths of 190 nm or more and 600 nm or less, and the more highly dispersed the iron, the more it can be confirmed as a peak with a lower wavelength. In the iron-containing FER zeolite of this embodiment, the iron is isolated iron (Fe 3+ ), iron clusters (Fe x O y ), and iron oxide (Fe 2 O 3 In this embodiment, the peaks at wavelengths of 190 nm or more and less than 300 nm are included as isolated iron (Fe) particles. 3+ ), and the peaks at wavelengths of 300 nm to 400 nm are iron clusters (Fe x O y ) and the peak corresponding to a wavelength of more than 400 nm and less than 600 nm are iron oxide (Fe 2 O 3) particles. When the 300 nm-600 nm spectral intensity ratio exceeds 20%, even in the case where isolated iron is contained, the proportion of iron oxide and iron clusters in the iron contained in the FER zeolite increases, and only nitrogen oxide reduction properties comparable to those of conventional iron-containing FER zeolites can be obtained. In the iron-containing FER zeolite of the present embodiment, the area ratio of peaks having wavelengths of 190 nm or more and less than 300 nm to peaks having wavelengths of 190 nm or more and less than 600 nm in the UV-VIS spectrum (hereinafter also referred to as the "190 nm-300 nm spectral intensity ratio") is 70% or more, 80% or more, or 90% or more, and is preferably 100% or less, less than 100%, or 99% or less, and examples thereof include 70% or more and 100% or less, 80% or more and less than 100%, or 90% or more and 99% or less. In the iron-containing FER-type zeolite of the present embodiment, the area ratio of peaks having a wavelength of 300 nm or more and 400 nm or less to peaks having a wavelength of 190 nm or more and 600 nm or less in a UV-VIS spectrum (hereinafter also referred to as "300 nm-400 nm spectral intensity ratio") is 20% or less, 5.0% or less, 3.0% or less, or 1.0% or less, and is preferably 0% or more, more than 0%, or 0.1% or more, and examples thereof include 0% or more and 20% or less, 0% or more and 5.0% or less, 0% or more and 3.0% or less, more than 0% and 3.0% or less, or 0.1% or more and 1.0% or less. In the iron-containing FER type zeolite of this embodiment, the area ratio of the peak having a wavelength of more than 400 nm and less than 600 nm to the peak having a wavelength of 190 nm or more and less than 600 nm in the UV-VIS spectrum (hereinafter also referred to as the "400 nm-600 nm spectral intensity ratio") is 20% or less, 5.0% or less, 3.0% or less, or 1.0% or less, and is preferably 0% or more, more than 0%, or 0.1% or more, and examples thereof include 0% or more and less than 20%, 0% or more and less than 5.0%, 0% or more and less than 3.0%, more than 0% and less than 3.0%, or 0.1% or more and less than 1.0%. These spectral intensity ratios [%] correspond to the abundance ratio [%] of iron species in the iron-containing FER type zeolite, and the 190 nm-300 nm spectral intensity ratio corresponds to the abundance ratio [%] of isolated iron (Fe 3+ ), the 300 nm-400 nm spectral intensity ratio is iron cluster (Fe x Oy ), and the 400 nm-600 nm spectral intensity ratio is iron oxide particles (Fe 2 O 3 ) is present in the iron-containing FER zeolite of the present embodiment. Therefore, the iron-containing FER zeolite of the present embodiment can also be regarded as a FER zeolite that contains iron and in which the abundance ratio of iron clusters and iron oxide particles is 20% or less, or as a FER zeolite that contains iron and in which the abundance ratio of isolated iron particles is 80% or more. Furthermore, in the iron-containing FER-type zeolite of the present embodiment, the total abundance ratio of isolated iron, iron clusters, and iron oxide particles is 100%, and the abundance ratio of isolated iron is 70% or more, 80% or more, or 90% or more, and is preferably 100% or less, less than 100%, or 99% or less, and is 70% or more and 100% or less, 80% or more and less than 100%, or 90% or more and 99% or less, and the abundance ratio of iron clusters is 20% or less, 5.0% or less, 3.0% or less, or 1.0% or less, and is preferably 0% or more, more than 0%, or 0.1% or more, and is 0% or more and 20% or less, 0% or more and 5.0% or less, 0% or more and 3.0% or less, more than 0% and 3.0% or less, or 0.1% or more and 1.0% or less, and The iron-containing FER-type zeolite has an iron-containing content of 20% or less, 5.0% or less, 3.0% or less, or 1.0% or less, and is preferably 0% or more, more than 0%, or 0.1% or more. The iron-containing FER-type zeolite can also be considered to have an iron-containing FER-type zeolite having an iron oxide particle content of 0% or more and 20% or less, 0% or more and 5.0% or less, 0% or more and 3.0% or less, more than 0% and 3.0% or less, or 0.1% or more and 1.0% or less.
[0024] The UV-VIS spectrum in this embodiment may be measured using a general UV-visible spectrophotometer (for example, UV-visible spectrophotometer V-770, manufactured by JASCO Corporation) under the following conditions: Integrating sphere unit: ISN-923 (manufactured by JASCO Corporation) Measurement mode: Diffuse reflectance method Wavelength: 190 to 700 nm Temperature: Room Slit width: 5 nm Background: Barium sulfate
[0025] The obtained UV-VIS spectrum is corrected so that the reflectance of the iron-containing FER-type zeolite of this embodiment relative to the reflectance of barium sulfate at a wavelength of 700 nm (hereinafter also referred to as "γ∞" or "relative reflectance") is 1, and then the corrected UV-VIS spectrum is subjected to KM (Kubelka-Munk) transformation using the KM function (f(γ∞)) of the following equation: f(γ∞) = (1 - γ∞) 2 / 2γ∞
[0026] The UV-VIS spectrum after KM conversion is fitted and separated using general analysis software (e.g., Fityk 0.9.8) with a Gaussian fitting function, and then the peak areas are determined for wavelengths of 190 nm or more and less than 300 nm, 300 nm or more and 400 nm or less, and more than 400 nm and 600 nm or less, and the sum of these peak areas is taken as the peak area for wavelengths of 190 nm or more and 600 nm or less. The area ratio can be calculated from the ratio of the peak area for each wavelength range to the obtained peak area for wavelengths of 190 nm or more and 600 nm or less.
[0027] In order to facilitate the exhibiting of practical nitrogen oxide reduction properties, the iron content is, for example, 0.1 mass% or more, 0.5 mass% or more, or 1.0 mass% or more, and 5.0 mass% or less, or 3.5 mass% or less, and is preferably 0.1 mass% or more and 5.0 mass% or less, or 1.0 mass% or more and 5.0 mass% or less, or 1.0 mass% or more and 3.5 mass% or less.
[0028] In the present embodiment, the "iron content" refers to the mass ratio [mass %] of iron (Fe) relative to the mass of the iron-containing FER zeolite. 2 O 3 Converted aluminum, SiO 2 The mass of the iron-containing FER zeolite can be determined by measuring the mass after treating it in an air atmosphere at 100°C for 2 hours.
[0029] The iron-containing FER zeolite of this embodiment preferably contains a large amount of isolated iron, and the content of isolated iron in the iron content (hereinafter referred to as “isolated Fe 3+ The content of isolated Fe is preferably 1.0 mass % or more, 1.2 mass % or more, or 1.5 mass % or more. 3+ The content is preferably high, but in that case, isolated Fe 3+ The content is the same as the upper limit of the iron content, and may be, for example, 5.0 mass % or less or 3.5 mass % or less. 3+ The content may be 1.0 mass% or more and 5.0 mass% or less, 1.2 mass% or more and 3.5 mass% or less, or 1.5 mass% or more and 3.5 mass% or less. 3+ The content can be calculated by the following formula: Isolated Fe 3+ Content [mass %] = iron content [mass %] × abundance ratio of isolated iron particles [%] = iron content [mass %] × 190 nm - 300 nm spectrum intensity ratio [%] Similarly, the content of iron clusters in the iron content (hereinafter also referred to as "cluster content") and the content of iron oxide particles in the iron content (hereinafter also referred to as "iron oxide content") can be calculated using the following formulas: Cluster content [mass %] = iron content [mass %] × abundance ratio of isolated iron particles [%] = iron content [mass %] × 300 nm - 400 nm spectrum intensity ratio [%] Iron oxide content [mass %] = iron content [mass %] × abundance ratio of isolated iron particles [%] = iron content [mass %] × 400 nm - 600 nm spectrum intensity ratio [%]
[0030] In the iron-containing FER zeolite of this embodiment, iron is contained in a state where it functions as an active metal, and is present on the surface, in pores, and at ion exchange sites of the FER zeolite, and preferably present at least in the pores. Note that, in the iron-containing FER zeolite of this embodiment, iron does not have to be substituted into the framework structure.
[0031] The iron-containing FER-type zeolite of the present embodiment may contain iron as an active metal, but may also contain an active metal other than iron, for example, one or more elements selected from the group consisting of copper (Cu), manganese (Mn), zirconium (Zr), yttrium (Y), cerium (Ce), lanthanum (La), and calcium (Ca), and further at least one of copper and manganese, or even copper.
[0032] The molar ratio of silica to alumina in the iron-containing FER zeolite of this embodiment (hereinafter referred to as "SiO 2 / Al 2 O 3 The crystalline porosity (ratio) may be any value that makes it difficult for crystal collapse to occur when exposed to a high-temperature, high-humidity atmosphere, and may be 5 or more, 10 or more, or 15 or more, and 50 or less, 30 or less, or 20 or less, and is preferably 5 or more and 50 or less, 10 or more and 30 or less, or 15 or more and 20 or less.
[0033] The iron-containing FER zeolite of the present embodiment preferably does not substantially contain fluorine (F), and further preferably has a fluorine content of 0 ppm by mass. Taking measurement error into consideration, the fluorine content of the iron-containing FER zeolite of the present embodiment may be equal to or less than the measurement limit, and is, for example, preferably from 0 ppm by mass to 100 ppm by mass, further preferably from 0 ppm by mass to 50 ppm by mass, and further preferably from 0 ppm by mass to 5 ppm by mass.
[0034] The shape of the iron-containing FER-type zeolite of this embodiment may be any shape depending on the application, and examples thereof include at least one of a powder and a molded body. In the case of a powder, the zeolite may be applied or wash-coated onto a substrate such as a honeycomb to form a catalyst member. In the case of a molded body, the zeolite may have any initial shape depending on the application, and may be one or more shapes selected from the group consisting of spherical, approximately spherical, elliptical, disk-like, cylindrical, polyhedral, irregular, and petal-like.
[0035] The iron-containing FER-type zeolite of the present embodiment can be used in known applications of zeolites, and can be used for, for example, one or more selected from the group consisting of catalysts, adsorbents, and carriers thereof, and can also be used as at least one of a catalyst and a catalyst carrier.
[0036] The iron-containing FER-type zeolite of this embodiment is suitable for use as at least one of a nitrogen oxide reduction catalyst and a support thereof, and further as a nitrogen oxide reduction catalyst, and further as a nitrogen oxide reduction catalyst by selective catalytic reduction.
[0037] For example, when the iron-containing FER type zeolite of this embodiment is used as a nitrogen oxide reduction catalyst, it may be used as a method for reducing nitrogen oxides, which includes a step of contacting the iron-containing FER type zeolite of this embodiment with a nitrogen oxide-containing gas (hereinafter also referred to as a "contact step").
[0038] The nitrogen oxide-containing gas may be any gas containing nitrogen oxide (NOx), and may contain at least nitrous oxide (N 2 The nitrogen oxide-containing gas is preferably a gas containing one or more selected from the group consisting of nitric oxide, nitrogen dioxide, dinitrogen trioxide, dinitrogen tetroxide, and dinitrogen monoxide, and more preferably a gas containing one or more selected from the group consisting of nitric oxide, nitrogen dioxide, and dinitrogen monoxide. The nitrogen oxide-containing gas may contain components other than nitrogen oxides, and may contain one or more selected from the group consisting of hydrocarbons, carbon monoxide, carbon dioxide, hydrogen, nitrogen, oxygen, sulfur oxides, and water. Specific examples of nitrogen oxide-containing gases include waste gases emitted from internal combustion engines, and waste gases emitted from one or more selected from the group consisting of automobiles, ships, boilers, and gas turbines.
[0039] In the contact step, any conditions may be used so long as the iron-containing FER-type zeolite of this embodiment comes into contact with the nitrogen oxide-containing gas, but examples of the contact conditions include the following: Space velocity: 500 to 500,000 h -1 , preferably 2,000 to 300,000 hours -1 Contact temperature: 120°C or higher and 600°C or lower, preferably 150°C or higher and 550°C or lower
[0040] The contact in the contact step is preferably carried out in the presence of a reducing agent. Examples of the reducing agent include one or more selected from the group consisting of ammonia, urea, organic amines, hydrocarbons, alcohols, ketones, carbon monoxide, and hydrogen, and further include at least one of ammonia, hydrocarbons, urea, and organic amines, and further include at least one of ammonia and hydrocarbons, and further include ammonia. [Method for Producing Iron-Containing FER-Type Zeolite] A preferred method for producing the iron-containing FER-type zeolite of this embodiment is a method for producing an iron-containing FER-type zeolite containing a silica-alumina source, an iron source, an alkali source, and water, and further including SiO 2 and a step of crystallizing a composition having a molar ratio of iron to silicon converted of less than 0.1.
[0041] Conventionally, methods for producing iron-containing FER-type zeolite have been used.
[0042] The production method of this embodiment is a method for producing a silica-alumina powder containing a silica-alumina source, an iron source, an alkali source, and water, and further containing SiO 2 The method includes a step of crystallizing a composition (hereinafter also referred to as a "raw material composition") having a molar ratio of iron to silicon converted to less than 0.1 (hereinafter also referred to as a "crystallization step").
[0043] The silica-alumina source is a compound containing aluminum (Al) and silicon (Si), and is preferably an amorphous compound containing aluminum and silicon. Specific examples of the silica-alumina source include amorphous aluminosilicates. In this embodiment, it is believed that crystallization proceeds in a state where iron dispersion is promoted, compared to when an aluminum source and a silicon source are separately contained.
[0044] The iron source is a compound containing iron, and may be any iron compound that is uniformly dispersed in the raw material composition. Specific examples of the iron compound include one or more selected from the group consisting of iron nitrate, iron sulfate, iron oxide, iron chloride, and iron oxyhydroxide, further one or more selected from the group consisting of iron hydroxide, iron sulfate, and iron nitrate, further at least one of iron sulfate and iron nitrate, and further iron sulfate.
[0045] The alkali source is a compound containing an alkali metal element, and examples thereof include compounds containing one or more selected from the group consisting of sodium, potassium, rubidium, and cesium, compounds containing one or more selected from the group consisting of sodium, potassium, and cesium, compounds containing at least one of sodium and potassium, and compounds containing sodium. Examples of the alkali source (hereinafter, when the alkali metal is sodium or the like, these will also be referred to as "sodium source" or the like) include one or more selected from the group consisting of hydroxides, fluorides, bromides, iodides, sulfates, nitrates, and carbonates containing the above-mentioned alkali metal elements, one or more selected from the group consisting of hydroxides, bromides, and iodides, or hydroxides.
[0046] Since the FER zeolite becomes more likely to crystallize without using an expensive organic structure-directing agent, the alkali source preferably contains at least a sodium source or a potassium source, more preferably contains at least a potassium source, even more preferably contains a sodium source and a potassium source, and even more preferably contains a sodium source and a potassium source.
[0047] The water in the raw material composition may include not only pure water and ion-exchanged water, but also structural water, hydration water, and water contained in other starting materials such as solvents.
[0048] When a starting material such as an iron source contains an alkali metal element, the starting material can also be considered as an alkali source. Similarly, when an iron source contains aluminum, the iron source can also be considered as an alumina source.
[0049] Because the resulting FER zeolite would be expensive, the raw material composition preferably does not contain a source of an organic structure-directing agent (hereinafter also referred to as "SDA"), and particularly preferably does not contain hexamethyleneimine. On the other hand, in order to promote crystallization, the raw material composition may contain an SDA source. The organic structure-directing agent source is at least one of an SDA capable of directing FER zeolite and a compound thereof, and may be an amine compound capable of directing FER zeolite. In order to facilitate industrial application of the production method of this embodiment, the SDA source is preferably an inexpensive amine compound, and examples thereof include amines other than hexamethyleneimine, as well as one or more selected from the group consisting of pyridine, pyrrolidine, cyclohexylamine, and butylamine, and further one or more selected from the group consisting of pyridine, pyrrolidine, and butylamine.
[0050] Al in the raw material composition 2 O 3 SiO relative to converted aluminum 2 The molar ratio of iron to silicon (hereinafter referred to as "SiO 2 / Al 2 O 3 ") is 5 or more, 10 or more, or 15 or more, and 50 or less, 30 or less, 25 or less, or 18 or less, and is preferably 5 or more and 50 or less, 10 or more and 30 or less, or 15 or more and 25 or less.
[0051] SiO of the raw material composition 2 The molar ratio of iron to silicon (hereinafter referred to as "Fe / SiO 2 ") is less than 0.1, and preferably 0.05 or less, or 0.03 or less. 2 If the Fe / SiO ratio exceeds 0.1, iron will aggregate and be incorporated into the FER zeolite in a low activity state. 2 The lower limit may be greater than 0, 0.001 or greater, or 0.01 or greater, and examples include greater than 0 but less than 0.1, greater than 0 but 0.5, 0.001 or greater but 0.5, 0.01 or greater but 0.05, or 0.01 or greater but 0.03.
[0052] SiO of the raw material composition 2The total molar ratio of alkali metal elements to silicon (hereinafter referred to as "M / SiO 2 ") is preferably less than 0.40, 0.38 or less, or 0.30 or less, and is preferably 0.05 or more, 0.20 or more, or 0.25 or more. 2 Examples of the α-value include 0.05 or more and less than 0.40, 0.20 or more and 0.38 or less, and 0.25 or more and 0.30 or less.
[0053] SiO of the raw material composition 2 The total molar ratio of potassium to silicon (hereinafter referred to as "K / SiO 2 ") is less than 0.40, 0.30 or less, or 0.15 or less, and may be 0 or more, more than 0, or 0.1 or more, and is preferably more than 0 but less than 0.40, 0.1 or more and 0.30 or less, or 0.1 or more and 0.15 or less.
[0054] Since the iron-containing FER-type zeolite in which the iron is more dispersed is more likely to crystallize, the SiO 2 Water (H 2 O) molar ratio (hereinafter referred to as "H 2 O / SiO 2 ") is sufficient as long as it is 50 or less, and preferably 40 or less or 25 or less. 2 O / SiO 2 is sufficient if it is 5 or more, 10 or more, or 13 or more, and is preferably 5 or more and 40 or less, 10 or more and 40 or less, or 13 or more and 25 or less.
[0055] Preferred compositions of the raw material composition include the following molar compositions: In the following molar compositions, M is an alkali metal, and when the alkali metals are sodium and potassium, for example, M can be considered as (Na+K).
[0056] SiO 2 / Al 2 O 3 = 5 or more, 10 or more, or 15 or more, 50 or less, 30 or less, 25 or less, or 18 or less, Fe / SiO 2M / SiO = more than 0, 0.001 or more, 0.01 or more, or 0.02 or more, less than 0.1, 0.05 or less, or 0.03 or less 2 = 0.05 or more, 0.20 or more, or 0.25 or more, less than 0.40, 0.38 or less, or 0.30 or less, K / M = 0 or more, more than 0, 0.10 or more, or 0.30 or more, 0.9 or less, 0.7 or less, or 0.5 or less, H 2 O / SiO 2 = 5 or more, 10 or more, or 13 or more, 50 or less, 40 or less, or 25 or less
[0057] More preferred compositions of the raw material composition include the following molar compositions: SiO 2 / Al 2 O 3 =5 or more and 50 or less Fe / SiO 2 = More than 0 and less than 0.1 M / SiO 2 = 0.05 or more and less than 0.40 K / M = 0 or more and 0.9 or less H 2 O / SiO 2 = 5 or more and 50 or less Particularly preferred compositions of the raw material composition include the following molar compositions: SiO 2 / Al 2 O 3 =10 or more, 30 or less Fe / SiO 2 =0.01 or more and 0.05 or less M / SiO 2 =0.20 or more and 0.38 or less K / M =0.10 or more and 0.7 or less H 2 O / SiO 2 = 5 or more and 25 or less
[0058] In order to facilitate application of production equipment made of general-purpose materials, the raw material composition preferably does not contain fluorine (F) or phosphorus (P), and the fluorine content is preferably 100 ppm by mass or less, and further preferably below the detection limit (10 ppm by mass or less).Similarly, the phosphorus content is preferably 100 ppm by mass or less, and further preferably below the detection limit (0.01 ppm by mass or less).
[0059] The raw material composition may contain seed crystals to promote crystallization of the raw material composition. The seed crystals may be any zeolite that promotes crystallization of FER zeolite, and are preferably one or more selected from the group consisting of CHA zeolite, AEI zeolite, MOR zeolite, FER zeolite, and AFX zeolite, with FER zeolite being more preferred.
[0060] In the crystallization step, the raw material composition is crystallized. As a result, iron-containing FER-type zeolite can be obtained as a crystallized product. The crystallization may be performed by hydrothermal treatment under conditions that allow the iron-containing FER-type zeolite to crystallize. Preferred crystallization conditions include the following: Pressure: autogenous pressure Crystallization temperature: 100°C or higher, 160°C or higher, or 175°C or higher, and 200°C or lower, or 190°C or lower
[0061] The crystallization time may be any time that allows the iron-containing FER zeolite to be sufficiently crystallized, and may be appropriately set depending on the amount of the raw material composition to be subjected to the crystallization and the crystallization method. Examples of the crystallization time include 4 hours or more, 8 hours or more, 24 hours or more, or 48 hours or more, and 150 hours or less, 100 hours or less, or 80 hours or less. In order to produce the iron-containing FER zeolite with practical productivity, the crystallization time is preferably 4 hours or more and 150 hours or less, 8 hours or more and 100 hours or less, or 24 hours or more and 48 hours or less.
[0062] In order to allow the crystallization to proceed more uniformly, it is preferable to carry out the crystallization while stirring the raw material composition. The stirring may be performed by directly stirring the raw material composition, or by stirring a container containing the raw material composition.
[0063] The crystallized product (iron-containing FER-type zeolite) may be recovered by any method, for example, by solid-liquid separation, washing, drying, and then recovering the product.
[0064] The solid-liquid separation may be any method capable of separating the raw material composition after crystallization into a solid component (crystallized material) and a liquid phase, and examples thereof include one or more methods selected from the group consisting of filtration, decantation, and centrifugation.
[0065] The washing may be carried out by any method that can remove impurities contained in the recovered crystallized product, for example, washing with pure water.
[0066] The drying may be carried out by any method capable of removing moisture physically adsorbed on the crystallized product, for example, by at least one of static drying and spray drying, in an air atmosphere at 100°C or higher and 120°C or lower.
[0067] In order to remove the SDA contained in the iron-containing FER-type zeolite (crystallized product after crystallization), the production method of this embodiment may include a step of removing an organic structure-directing agent from the crystallized product (hereinafter also referred to as an "SDA removal step"). In the SDA removal step, any SDA removal method may be used, and examples thereof include one or more selected from the group consisting of liquid phase treatment with an acidic aqueous solution, exchange treatment with a resin, pyrolysis treatment, and calcination treatment. From the viewpoint of production efficiency, the SDA removal step is preferably at least one of pyrolysis treatment and calcination treatment, and calcination treatment is more preferred. Examples of preferred calcination conditions include the following conditions. Calcination atmosphere: air atmosphere Calcination temperature: 400°C or higher or 560°C or higher, and 700°C or lower or 650°C or lower
[0068] The calcination time may be appropriately set depending on the crystallized material to be calcined and the calcination method, and may be, for example, from 1 hour to 10 hours, from 2 hours to 8 hours, or from 3 hours to 5 hours.
[0069] The production method of this embodiment may include a step of ion-exchanging the iron-containing FER zeolite (hereinafter also referred to as an "ion exchange step") in order to reduce the alkali metal content of the iron-containing FER zeolite. The ion exchange may be any method that reduces the alkali metal content, and an example of the ion exchange method is mixing the iron-containing FER zeolite with an ammonium chloride aqueous solution.
[0070] If necessary, the iron-containing FER-type zeolite after ion exchange may be calcined.
[0071] The production method of the present embodiment may include, in addition to or instead of the ion exchange step, a step of mixing the iron-containing FER zeolite with a metal compound (hereinafter also referred to as a "metal supporting step"). This makes it possible to support any metal element depending on the purpose on the iron-containing FER zeolite.
[0072] The mixing method may be any method that can support a metal compound on the iron-containing FER-type zeolite, and may include one or more methods selected from the group consisting of ion exchange, impregnation, evaporation to dryness, precipitation, and physical mixing.
[0073] The present disclosure will be described below with reference to examples. However, the present disclosure is not limited to the following. The evaluation method is described below. (Crystal Identification) XRD measurement of the sample was performed using a powder X-ray diffractometer (device name: Ultima IV, manufactured by Rigaku Corporation). The measurement conditions are as follows: Radiation source: CuKα radiation (λ=1.5405 Å) Measurement mode: Step scan Scanning conditions: 40° / min Measurement time: 3 seconds Measurement range: 2θ=5° to 43°
[0074] (Composition analysis) A sample solution was prepared by dissolving the sample in a mixed aqueous solution of hydrofluoric acid and nitric acid. The sample solution was measured by inductively coupled plasma atomic emission spectroscopy (ICP-AES) using an ICP device (device name: OPTIMA 5300DV, manufactured by PerkinElmer). (Measurement of iron dispersibility) The UV-Vis spectrum of the sample was measured using an ultraviolet-visible spectrophotometer (device name: UV-visible spectrophotometer V-770, manufactured by JASCO Corporation). The measurement conditions were as follows: Integrating sphere unit: ISN-923 (JASCO Corporation) Measurement mode: Diffuse reflectance method Wavelength: 190-700 nm Temperature: Room temperature Slit width: 5 nm Background: Barium sulfate The obtained UV-Vis spectrum was fitted and separated using general analysis software (software name: Fityk 0.9.8) with a Gaussian fitting function, and then the peak areas of wavelengths 190 nm or more and less than 300 nm, wavelengths 300 nm or more and 400 nm or less, and wavelengths over 400 nm and 600 nm or less were calculated, and the 300 nm-600 nm spectral intensity ratio [%] and the 190 nm-300 nm spectral intensity ratio (isolated iron (Fe 3+ ) abundance ratio) [%], 300 nm-400 nm spectrum intensity ratio (cluster iron (Fe x O y ) content ratio [%], and 400 nm-600 nm spectral intensity ratio (iron oxide particles (Fe 2 O 3 The content of each iron species was calculated from the content of isolated iron and the iron content calculated by the composition analysis using the following formula: 3+ Content [mass%] = Iron content [mass%] × Isolated iron (Fe 3+) abundance ratio [%] = iron content [mass %] × 190 nm - 300 nm spectrum intensity ratio [%] Cluster content [mass %] = iron content [mass %] × abundance ratio of isolated iron [%] = iron content [mass %] × 300 nm - 400 nm spectrum intensity ratio [%] Iron oxide content [mass %] = iron content [mass %] × abundance ratio of isolated iron [%] = iron content [mass %] × 400 nm - 600 nm spectrum intensity ratio [%]
[0075] Example 1 A 48% by mass aqueous solution of sodium hydroxide, a 48% by mass aqueous solution of potassium hydroxide, iron (III) nitrate nonahydrate, pure water, and amorphous aluminosilicate (SiO 2 / Al 2 O 3 = 17.9) were mixed to obtain a raw material composition having the following molar composition:
[0076] SiO 2 / Al 2 O 3 =17.9 Fe / SiO 2 =0.016 (Na+K) / SiO 2 =0.280 (Na / SiO 2 =0.163, K / SiO 2 =0.117) K / (Na+K) =0.418H 2 O / SiO 2 = 16 The obtained raw material composition was added with FER type zeolite (SiO 2 / Al 2 O 3 = 18.0) were mixed. The mixed raw material composition was filled into an 80 mL sealed container, which was rotated at 55 rpm and subjected to hydrothermal treatment at 180°C for 40 hours to obtain a crystallized product. The obtained crystallized product was subjected to solid-liquid separation, washed with pure water, and then dried at 110°C in the air and collected. The crystallized product was a zeolite consisting of a single phase of FER-type zeolite, and SiO 2 / Al 2 O 3 was 18.0.
[0077] The obtained crystallized product was calcined in the air at 600° C. for 2 hours and then subjected to ion exchange with a 20 mass % aqueous ammonium chloride solution at 60° C. The crystallized product after ion exchange was washed with a sufficient amount of pure water and dried in the air at 110° C., thereby obtaining an iron-containing FER-type zeolite of this example.
[0078] The iron-containing FER-type zeolite of this example is a zeolite consisting of a single phase of FER-type zeolite, and SiO 2 / Al 2 O 3 The 190 nm-300 nm spectral intensity ratio (proportion of isolated iron) was 99.8%, the 300 nm-400 nm spectral intensity ratio (proportion of iron clusters) was 0.2%, the 400 nm-600 nm spectral intensity ratio (proportion of iron oxide particles) was 0%, and the 300 nm-600 nm spectral intensity ratio was 0.2%, indicating that the isolated Fe 3+ The content was 1.4% by mass. The 2θ angle of the peak top of the XRD peak of the (200) plane was 9.3.
[0079] Example 2 The iron-containing FER-type zeolite of this example was obtained in the same manner as in Example 1, except that the raw material composition had the following molar composition: SiO 2 / Al 2 O 3 =17.9 Fe / SiO 2 =0.024 (Na+K) / SiO 2 =0.305 Na / SiO 2 =0.177, K / SiO 2 =0.128) K / (Na+K) =0.420H 2 O / SiO 2 =16
[0080] The iron-containing FER-type zeolite of this example is a zeolite consisting of a single phase of FER-type zeolite, and SiO 2 / Al 2 O 3The SiO2 content was 18.2, the alkali metal content was less than 0.1 mass %, and the Fe content was 2.0 mass %. The 2θ angle of the peak top of the XRD peak of the (200) plane was 9.3.
[0081] Example 3 The iron-containing FER-type zeolite of this example was obtained in the same manner as in Example 1, except that the raw material composition had the following molar composition: SiO 2 / Al 2 O 3 =17.9 Fe / SiO 2 =0.037 (Na+K) / SiO 2 =0.350 (Na / SiO 2 =0.203, K / SiO 2 =0.147) K / (Na+K) =0.420H 2 O / SiO 2 =16
[0082] The iron-containing FER-type zeolite of this example is a zeolite consisting of a single phase of FER-type zeolite, and SiO 2 / Al 2 O 3 The 190 nm-300 nm spectral intensity ratio (proportion of isolated iron) was 99.7%, the 300 nm-400 nm spectral intensity ratio (proportion of iron clusters) was 0.3%, the 400 nm-600 nm spectral intensity ratio (proportion of iron oxide particles) was 0%, and the 300 nm-600 nm spectral intensity ratio was 0.3%, indicating that the isolated Fe 3+ The content was 3.0% by mass. The 2θ angle of the peak top of the XRD peak of the (200) plane was 9.3.
[0083] Comparative Example 1 Crystallization, solid-liquid separation, washing and drying were carried out in the same manner as in Example 1, except that the raw material composition was changed to the following composition, to obtain a crystallized product. 2 / Al 2 O 3 =19.0 (Fe / SiO 2 =0) (Na+K) / SiO2 =0.19 (Na / SiO 2 =0.114, K / SiO 2 =0.076) K / (Na+K) =0.400H 2 O / SiO 2 =16
[0084] The obtained crystallized product is a zeolite consisting of a single phase of FER type zeolite, and SiO 2 / Al 2 O 3 was 18.7.
[0085] The obtained crystallized product was calcined in air at 600°C for 2 hours. The calcined solid was exchanged with a 20% by mass aqueous ammonium chloride solution at 60°C (weight of the aqueous ammonium chloride solution: weight of the zeolite = 1.0), washed with a large amount of water, and dried at 110°C. The alkali metal content in the dried sample was less than 0.1% by mass. Next, 7.0 g of the dried sample, 1.6 g of iron (III) nitrate nonahydrate, and 2.4 g of pure water were mixed in a mortar. Finally, the homogeneously mixed sample was dried in air at 110°C for 5 hours and then calcined at 500°C for 2 hours to obtain the iron-containing FER-type zeolite of this comparative example.
[0086] The iron-containing FER zeolite of this comparative example is a zeolite consisting of a single phase of FER zeolite, and SiO 2 / Al 2 O 3 The 190 nm-300 nm spectral intensity ratio (proportion of isolated iron) was 29.6%, the 300 nm-400 nm spectral intensity ratio (proportion of iron clusters) was 23.2%, the 400 nm-600 nm spectral intensity ratio (proportion of iron oxide particles) was 47.2%, and the 300 nm-600 nm spectral intensity ratio was 70.4%, indicating that the isolated Fe 3+ The content was 0.9% by mass.
[0087] The iron-containing FER zeolite of this comparative example has an iron content similar to that of the iron-containing FER zeolite of Example 3, but has a lower proportion of isolated iron, and has a higher proportion of isolated Fe than the iron-containing FER zeolite of Example 1. 3+ The content was confirmed to be low.
[0088]
[0089] According to this example, it was confirmed that iron-containing FER zeolite containing dispersed iron, that is, iron-containing FER zeolite having a low 300 nm-600 nm spectral intensity ratio, can be obtained without requiring expensive SDA.
[0090] Measurement Example <Hydrothermal Durability Treatment> The iron-containing FRR-type zeolites obtained in the Examples and Comparative Examples were each molded and pulverized to form agglomerated particles having an agglomeration diameter of 12 to 20 mesh. 3 mL of the obtained agglomerated particles were packed into an atmospheric pressure fixed-bed flow reactor, and then a hydrothermal durability treatment was carried out by flowing air containing 20% by volume of moisture under the following conditions: Air flow rate: 300 mL / min Treatment temperature: 700°C Treatment time: 20 hours
[0091] <Nitrogen oxide reduction treatment> 1.5 mL of the sample in the form of agglomerated particles was packed into an atmospheric pressure fixed-bed flow-type reactor, and a nitrogen oxide-containing gas was passed through the reactor while maintaining the temperature at the following measurement temperature, and the nitrogen oxide concentrations at the inlet and outlet of the atmospheric pressure fixed-bed flow-type reactor were measured. The flow conditions for the nitrogen oxide-containing gas were as follows:
[0092] Composition of nitrogen oxide-containing gas: NO 200 ppm by volume NH 3 200 ppm by volume O 2 10% by volume H 2 O 3 vol% N 2 Remainder: Flow rate of nitrogen oxide-containing gas: 1.5 L / min Space velocity: 60,000 hr -1Measurement temperature: 150°C, 200°C, 300°C, 500°C, 550°C or 600°C
[0093] The nitrogen oxide reduction rate was calculated from the obtained nitrogen oxide concentrations using the following formula: Nitrogen oxide reduction rate (%) = {([NOx] in - [NOx] out) / [NOx] in} × 100, where [NOx] in is the nitrogen oxide concentration of the nitrogen oxide-containing gas at the inlet of the atmospheric pressure fixed-bed flow-type reactor tube, and [NOx] out is the nitrogen oxide concentration of the nitrogen oxide-containing gas at the outlet of the atmospheric pressure fixed-bed flow-type reactor tube.
[0094] In addition, the nitrogen oxide-containing gas at the outlet of the atmospheric pressure fixed-bed flow reactor 2 The amount of O was measured, and N 2 The amount of O produced was considered to be
[0095] Hereinafter, the N content of iron-containing FER-type zeolite before hydrothermal durability treatment in nitrogen oxide reduction treatment at 150°C to 300°C will be 2 The evaluation results of the amount of O produced are shown in Table 2. The amount of N produced by the iron-containing FER-type zeolite after hydrothermal durability treatment in the nitrogen oxide reduction treatment at 150°C to 300°C is also shown in Table 2. 2 The evaluation results of the amount of O produced are shown in Table 3.
[0096]
[0097] The iron-containing FER-type zeolite of the example exhibited excellent nitrogen oxide reduction properties in the nitrogen oxide reduction treatment at low temperatures of 150°C to 200°C and at medium temperatures of 300°C. 2 It was confirmed that the generation of O was suppressed. In particular, the iron-containing FER zeolite of Example 3 and the iron-containing FER zeolite of Comparative Example 1 both have an iron content of 3 mass%. However, compared with the iron-containing FER zeolite of Comparative Example 1 obtained by the post-loading method, the iron-containing FER zeolite of Example 3 produced less N in the nitrogen oxide reduction treatment in the low temperature range of 150°C to 200°C and the medium temperature range of 300°C. 2 It was confirmed that the generation of O was significantly suppressed.
[0098]
[0099] Compared with the iron-containing zeolite of Comparative Example 1, the iron-containing FER-type zeolite of the Example exhibited a higher nitrogen oxide reduction rate in the nitrogen oxide reduction treatment at a low temperature range of 150°C to 300°C, even after the hydrothermal durability treatment. 2 It was confirmed that the generation of O was suppressed.
[0100] Next, the N content of iron-containing FER-type zeolite before hydrothermal durability treatment in the high-temperature nitrogen oxide reduction treatment was 2 The evaluation results of the amount of O produced are shown in Table 4. The amount of N produced by the iron-containing FER-type zeolite after hydrothermal durability treatment in the nitrogen oxide reduction treatment at high temperatures is also shown in Table 5. 2 The evaluation results of the amount of O produced are shown in Table 5.
[0101]
[0102] In the nitrogen oxide reduction treatment at high temperatures of 500°C or higher, the iron-containing FER-type zeolite of Example 1 not only contains iron, which is an active component, but also iron clusters, which are considered to be active species in high temperatures, but also substantially reduces the amount of N 2 It was confirmed that no O was produced.
[0103]
[0104] Compared with the iron-containing zeolite of Comparative Example 1, the iron-containing FER-type zeolite of Example 3 was found to have a low nitrogen oxide reduction rate in a high-temperature range of 500°C or higher even after hydrothermal durability treatment. 2 It was confirmed that the generation of O was suppressed.
[0105] Next, the ratio of the nitrogen oxide reduction rate (%) after the hydrothermal durability treatment to the nitrogen oxide reduction rate (%) before the hydrothermal durability treatment (maintenance rate of the nitrogen oxide reduction rate) is shown.
[0106]
[0107] It was confirmed that, compared to the iron-containing FER-type zeolite of Comparative Example 1, the iron-containing FER-type zeolite of the Example exhibited stable nitrogen oxide reduction properties over a wide temperature range of the nitrogen oxide reduction treatment from low to high temperatures.
[0108] Furthermore, the nitrogen oxide reduction rate after hydrothermal durability treatment in a nitrogen oxide reduction treatment at 550°C was 75% for the iron-containing FER-type zeolite of Comparative Example 1, whereas Examples 1 to 3 were 77%, 73%, and 81%, respectively. From this, it was confirmed that the iron-containing FER-type zeolite of this example, despite substantially not containing iron clusters, which are considered to be active species in high-temperature ranges, exhibited a nitrogen oxide reduction rate after hydrothermal durability treatment in a nitrogen oxide reduction treatment in a high-temperature range that was equal to or higher than that of conventional iron-containing FER-type zeolites containing iron clusters. The entire contents of the specification, claims, and abstract of Japanese Patent Application No. 2023-79261, filed on May 12, 2023, are hereby incorporated by reference herein as the disclosure of the specification of the present disclosure.
Claims
1. A FER-type zeolite which contains iron and in which the area ratio of the peak in the UV-VIS spectrum having a wavelength of 300 nm or more and 600 nm or less to the peak in the wavelength range of 190 nm or more and 600 nm or less is 20% or less.
2. The FER type zeolite according to claim 1, in which the area ratio of the peak having a wavelength of more than 400 nm and not more than 600 nm to the peak having a wavelength of 190 nm or more and not more than 600 nm in the UV-VIS spectrum is 20% or less.
3. A FER type zeolite according to claim 1 or 2, in which the area ratio of the peak in the UV-VIS spectrum having a wavelength of 190 nm or more and less than 300 nm to the peak having a wavelength of 190 nm or more and 600 nm or less is 80% or more.
4. A FER type zeolite according to any one of claims 1 to 3, having an iron content of 5 mass% or less.
5. A FER type zeolite according to any one of claims 1 to 4, wherein the molar ratio of silica to alumina is 5 or more and 50 or less.
6. A FER type zeolite according to any one of claims 1 to 5, containing one or more elements selected from the group consisting of copper (Cu), manganese (Mn), zirconium (Zr), yttrium (Y), cerium (Ce), lanthanum (La) and calcium (Ca).
7. A catalyst containing a silica alumina source, an iron source, an alkali source, water, and seed crystals, and further containing SiO 2 A method for producing a FER type zeolite according to any one of claims 1 to 6, comprising a step of crystallizing a composition having a molar ratio of iron to silicon converted of less than 0.
1.
8. The method according to claim 7, wherein the alkali source comprises at least a sodium source or a potassium source.
9. The method for producing FER type zeolite according to claim 7 or 8, wherein the composition has the following molar composition: In the following molar composition, M is an alkali metal. SiO 2 / Al 2 O 3 =5 or more and 50 or less Fe / SiO 2 = More than 0 and less than 0.1 M / SiO 2 = 0.05 or more and less than 0.40 K / M = 0 or more and 0.9 or less H 2 O / SiO 2 =5 or more and 50 or less 10. The method according to any one of claims 7 to 9, wherein the seed crystals are one or more selected from the group consisting of CHA type zeolite, AEI type zeolite, MOR type zeolite, FER type zeolite and AFX type zeolite.
11. A method for producing a semiconductor device according to any one of claims 7 to 10, wherein the content of seed crystals in the raw material composition is greater than 0% by mass and is not more than 10% by mass.
12. The process according to any one of claims 7 to 11, which does not include a source of organic structure directing agent.
13. The process according to any one of claims 7 to 12, further comprising a source of one or more organic structure directing agents selected from the group consisting of pyridine, pyrrolidine, cyclohexylamine and butylamine.
14. A nitrogen oxide reduction catalyst comprising the FER type zeolite according to any one of claims 1 to 6.
15. A method for reducing nitrogen oxides, comprising a step of contacting a nitrogen oxide-containing gas with a nitrogen oxide reduction catalyst containing the FER zeolite according to any one of claims 1 to 6.
Citation Information
Patent Citations
Preparation method of iron-based molecular sieve catalyst
CN114345402A
Method for decomposing n2o, catalyst therefor and method for producing this catalyst
JP2007537858A
Protector, wire harness, and lock mechanism
JP2023079261A
Scr catalyst with improved low temperature performance and method of making and using same
JP2017510437A
SCR Catalyst with Improved Low-Temperature Performance, and Method for Manufacturing and Using the Same
JP2017512630A