Electrode for secondary battery and secondary battery comprising same
The electrode for lithium secondary batteries, featuring a functional layer with expanded graphite, addresses safety and thermal stability issues by increasing resistance at high temperatures, thereby enhancing safety and energy density.
Patent Information
- Application Number
- PCT/KR2024/006025
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-05-03
- Publication Date
- 2024-11-21
AI Technical Summary
Lithium secondary batteries face challenges in achieving high energy density while maintaining safety and thermal stability, particularly due to the low thermal stability of high Ni-based anode materials, which can reduce safety and capacity.
An electrode for secondary batteries is developed with a functional layer containing expanded graphite and an auxiliary binder, applied to the electrode current collector, which increases resistance at high temperatures, enhancing safety and stability without compromising energy density.
The electrode effectively prevents ignition by expanding to separate the active material layer from the current collector at high temperatures, improving safety and maintaining high energy density, as demonstrated by increased resistance and stable electrochemical performance.
Smart Images

Figure KR2024006025_21112024_PF_FP_ABST
Abstract
Description
Electrode for secondary battery and secondary battery including same
[0001] The present invention relates to an electrode for a secondary battery and a secondary battery including the same, and more specifically, to an electrode for a secondary battery having improved safety by further including a functional layer and a secondary battery including the same.
[0002] The development of portable electronic devices such as smartphones, MP3 players, and tablet PCs has led to an explosive increase in demand for secondary batteries capable of storing electrical energy. In particular, the emergence of electric vehicles, medium- to large-scale energy storage systems, and portable devices requiring high energy density is driving the demand for secondary batteries.
[0003] Lithium secondary batteries are a type of secondary battery that can be charged using an external power source. They boast numerous advantages, including high energy density and long lifespan. These batteries typically use lithium transition metal oxides as the positive electrode active material and graphite-based materials as the negative electrode active material. Charging and discharging occur through repeated intercalation / deintercalation of lithium ions from the positive electrode to the negative electrode.
[0004] Lithium secondary batteries are the most widely used energy storage devices due to their high energy density, excellent output characteristics, high charge / discharge efficiency, and stable cycle life. Recently, with carbon emission regulations and the development of the electric vehicle industry, active research is being conducted on cathode and anode materials that can improve the energy density and output characteristics of lithium secondary batteries. The conventional lithium cobalt oxide (LCO) cathode material has a low discharge capacity, limiting its ability to achieve high energy density. To address this issue, high-nickel (Ni) cathode materials with high discharge capacity are being used. However, the inherent low thermal stability of these materials compromises the safety of lithium secondary batteries. Therefore, various studies are being conducted to improve the safety of lithium secondary batteries.
[0005] Prior literature: Korean Patent No. 10-1517043 (April 27, 2015)
[0006] The technical problem to be solved by the present application is to provide an electrode for a secondary battery and a secondary battery including the same, which not only has excellent battery capacity and initial charge / discharge efficiency, but also can control resistance at high temperatures.
[0007] Another technical problem that the present application seeks to solve is to provide an electrode for a secondary battery with improved safety by including novel functionality, and a secondary battery including the same.
[0008] The technical problems that this application seeks to solve are not limited to those described above.
[0009] To solve the above technical problem, the present invention provides an electrode for a secondary battery and a secondary battery including the same.
[0010] In one embodiment, an electrode for a secondary battery according to an embodiment of the present invention includes: an electrode current collector; a functional layer coated on at least a portion of the electrode current collector; and an electrode active material layer provided on the functional layer; wherein the functional layer may include expanded graphite and an auxiliary binder.
[0011] In one embodiment, the expanded graphite and the auxiliary binder in the functional layer may be included in a ratio of 50:50 to 99:1.
[0012] In one embodiment, the expanded graphite may have a particle size of 500 nm to 7 μm, and the expanded graphite may have an expansion ratio of 200% to 600% at 140°C.
[0013] In one embodiment, the functional layer may include an opening to expose at least a portion of the surface of the electrode collector.
[0014] In one embodiment, the functional layer is provided on one surface of the electrode collector, and may be provided in a patterned form so as to expose a portion of the surface of the electrode collector.
[0015] In one embodiment, the thickness of the functional layer may be 2 μm to 20 μm, and the thickness of the electrode active material layer may be 50 μm to 150 μm.
[0016] In one embodiment, the functional layer may be heat-treated at 100°C to 160°C for 30 seconds to 10 minutes after being coated on the electrode collector.
[0017] In one embodiment, the electrode active material layer includes a negative electrode active material and a negative electrode binder, and the negative electrode binder and the auxiliary binder are each independently selected from the group consisting of poly(vinylidene fluoride-co-hexafluoropropylene), PVDF-co-HFP, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, and polytetrafluoroethylene (PTFE). It may be at least one selected from the group consisting of an aqueous binder of acrylonitrile-butadiene rubber, styrene-butadiene rubber (SBR) or acrylic rubber; and a polymer resin of hydroxyethyl cellulose, carboxymethyl cellulose or polyvinylidene fluoride.
[0018] In one embodiment, the expanded graphite may be included in an amount of 0.1 to 1 part by weight based on 100 parts by weight of the electrode active material.
[0019] In one embodiment, the electrode active material layer includes a negative electrode active material and a negative electrode binder, and the negative electrode active material may include natural graphite or artificial graphite.
[0020] In one embodiment, the negative electrode binder is provided in an amount of 2 to 6 parts by weight based on 100 parts by weight of the negative electrode active material, and the negative electrode binder includes a first binder and a second binder, and the first binder and the second binder may be included in a ratio of 30:70 to 70:30.
[0021] In one embodiment, the first binder may include carboxyl methyl cellulose (CMC), the second binder may include styrene-butadiene rubber (SBR), and the auxiliary binder may include styrene-butadiene rubber (SBR).
[0022] In one embodiment, the electrode current collector includes a negative current collector or a positive current collector, and the negative current collector includes at least one of copper (Cu), nickel-coated copper (Ni coated Cu), stainless steel (SUS), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), carbon, and carbon fiber, and the positive current collector may include at least one of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), and lithium (Li).
[0023] In one embodiment, the present invention includes a lithium secondary battery comprising a negative electrode; a positive electrode; and an electrolyte interposed therebetween, wherein the negative electrode or the positive electrode may be the electrodes described above.
[0024] In one embodiment, the method for manufacturing an electrode for a secondary battery may include the steps of: preparing an electrode current collector; coating a mixture including expanded graphite and an auxiliary binder on one surface of the electrode current collector, and heat-treating the mixture at 100° C. to 160° C. to form a functional layer; and forming an electrode active material layer on the functional layer.
[0025] In one embodiment, the expanded graphite and the auxiliary binder in the functional layer may be included in a ratio of 50:50 to 99:1.
[0026] In one embodiment, the expanded graphite may have a particle size of 500 nm to 7 μm, and the expanded graphite may have an expansion ratio of 200% to 600% at 140°C.
[0027] In one embodiment, the expanded graphite may be manufactured by adding natural graphite or artificial graphite to a reactor equipped with an acidic solution, performing a first mixing at room temperature for 0.5 to 2 hours, adding an oxidizing agent to the reactor after the first mixing is completed, performing a second mixing at 30°C to 45°C for 6 to 30 hours, adding deionized water to the reactor after the second mixing is completed, performing a third mixing at 80°C to 100°C for 10 minutes to 1 hour, adding deionized water and hydrogen peroxide to the reactor after the third mixing is completed, performing a fourth mixing at room temperature for 1 to 30 minutes, and washing and drying after performing the fourth mixing.
[0028] In one embodiment, the acidic solution has a pH of 0.1 to 5 and SO4 2- , Cl - , and NO3 - Including at least one of the following, wherein the oxidizing agent may include at least one of potassium permanganate (KMnO4), hydrogen peroxide (H2O2), ozone (O3), peroxydisulfuric acid (H2S2O8), peroxymonosulfuric acid (H2SO5), potassium nitrate (KNO3), and sodium hypochlorite (NaClO).
[0029] According to the present invention, an electrode for a secondary battery and a secondary battery including the same can be provided with improved safety by controlling the resistance of the electrode at high temperatures.
[0030] In addition, according to the present invention, it is possible to provide an electrode for a secondary battery having improved high-temperature stability of a secondary battery having a high energy density without reducing the capacity of the secondary battery, and a secondary battery including the same.
[0031] Figure 1 is a cross-sectional view of an electrode for a secondary battery according to one embodiment of the present invention.
[0032] Figure 2 is a drawing showing a functional layer of an electrode for a secondary battery from above according to another embodiment of the present invention.
[0033] Figure 3 is a schematic drawing of a negative electrode for a secondary battery according to one embodiment of the present invention.
[0034] FIG. 4 is a drawing schematically showing the operation of a functional layer at high temperature in a negative electrode for a secondary battery according to one embodiment of the present invention.
[0035] Figure 5 is a graph showing the expansion rate of manufactured expanded graphite according to the heat treatment temperature.
[0036] Figure 6 shows SEM photographs of the manufactured expanded graphite before and after heat treatment.
[0037] Figure 7 is a graph comparing the adhesive strength before and after heat treatment in a cathode according to a comparative example and an embodiment of the present invention.
[0038] Figure 8 is a graph comparing the resistance values before and after heat treatment in a cathode according to comparative examples and embodiments of the present invention.
[0039] Figure 9 is a graph confirming the safety of the cathode according to comparative examples and embodiments of the present invention.
[0040] Figure 10 is a graph showing the electrochemical characteristics of a half-cell using a cathode according to comparative examples and examples of the present invention.
[0041] Figure 11 is a graph showing the electrochemical characteristics of a full cell using a cathode according to comparative examples and examples of the present invention.
[0042] Figure 12 is a graph confirming the safety of the anode according to comparative examples and embodiments of the present invention.
[0043] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. However, the technical concept of the present invention is not limited to the embodiments described herein and may be embodied in other forms. Rather, the embodiments introduced herein are provided to ensure that the disclosure is thorough and complete and to sufficiently convey the spirit of the present invention to those skilled in the art.
[0044] In this specification, when a component is referred to as being on another component, it means that it can be formed directly on the other component, or a third component may be interposed between them. In addition, in the drawings, the thicknesses of films and regions are exaggerated for the purpose of effectively explaining the technical contents.
[0045] Also, although terms such as first, second, and third have been used to describe various components in various embodiments of this specification, these components should not be limited by these terms. These terms are only used to distinguish one component from another. Thus, what is referred to as a first component in one embodiment may be referred to as a second component in another embodiment. Each embodiment described and illustrated herein also includes its complementary embodiments. Also, the term "and / or" has been used herein to mean including at least one of the components listed before and after.
[0046] In the specification, singular expressions include plural expressions unless the context clearly dictates otherwise. Furthermore, terms such as "comprises" or "has" are intended to specify the presence of a feature, number, step, component, or combination thereof described in the specification, but should not be construed as excluding the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0047] In addition, when describing the present invention below, if it is determined that a detailed description of a related known function or configuration may unnecessarily obscure the gist of the present invention, the detailed description will be omitted.
[0048] Figure 1 is a cross-sectional view of an electrode for a secondary battery according to one embodiment of the present invention.
[0049] An electrode (100) for a secondary battery according to one embodiment of the present invention may include an electrode current collector (110); a functional layer (120) coated on at least a portion of the electrode current collector (110); and an electrode active material layer (130) provided on the functional layer (120).
[0050] The functional layer (120) includes expanded graphite and an auxiliary binder, and the secondary battery electrode (100) may include a functional layer (120) formed by coating a mixture of the expanded graphite and the auxiliary binder on the electrode current collector (110). The electrode current collector (110), the functional layer (120), and the electrode active material layer (130) may be provided in a sequentially laminated form.
[0051] Typically, secondary batteries generate electrochemical energy through charging and discharging. However, safety concerns arise when operating at temperatures exceeding a certain threshold, so flame retardants have been introduced and used. Because flame retardants function to extinguish fire, the problem arises when the anode and cathode are short-circuited, causing a rapid temperature rise, followed by thermal runaway and subsequent fire.
[0052] The electrode for a secondary battery according to an embodiment of the present invention can prevent problems such as ignition by rapidly increasing the resistance of the secondary battery at a predetermined temperature before a fire occurs. Specifically, the negative electrode for a secondary battery according to the present embodiment further includes a functional layer, thereby preventing the secondary battery from rising above a predetermined temperature, thereby further improving safety.
[0053] Specifically, when the temperature of the secondary battery increases due to a short circuit or the like, the expanded graphite included in the functional layer (120) expands and can separate the electrode active material layer (130) from the electrode current collector (110) by a predetermined distance. The functional layer (120) operates at approximately 140°C or higher to increase the resistance of the secondary battery, thereby improving the safety of the secondary battery.
[0054] The secondary battery electrode (100) may have a functional layer (120) interposed between the electrode current collector (110) and the electrode active material layer (130), and the expanded graphite and the auxiliary binder may be included in the functional layer (120) at a ratio of 50:50 to 99:1. If the expanded graphite and the auxiliary binder are outside the above-described range, it is difficult for the functional layer (120) to be uniformly coated on the surface of the negative electrode current collector (110), and the function of the functional layer (120) operating at high temperatures is not sufficiently performed, which is problematic.
[0055] The expanded graphite may have a particle size of 500 nm to 7 μm. If the particle size of the expanded graphite is less than 500 nm, the expanded graphite does not expand sufficiently, which causes a problem. If the particle size exceeds 7 μm, the distance between the negative electrode current collector (110) and the negative electrode active material (130) increases, which causes a problem in that the charge transfer efficiency decreases.
[0056] The above-mentioned expanded graphite may have an expansion rate of 200% to 600% at 140°C. Since the above-mentioned expanded graphite has an expansion rate within the aforementioned range at 140°C, it can effectively improve the resistance of a secondary battery at high temperatures.
[0057] The functional layer (120) may include an opening to expose at least a portion of the surface of the electrode current collector (110). When the functional layer (120) is provided on the surface of the electrode current collector (110), the electrode active material layer (130) may be inserted through the opening to expose at least a portion of the electrode current collector (110). In the opening, the electrode current collector (110) and the electrode active material layer (130) are in direct contact, thereby allowing the performance of the functional layer (120) to be sufficiently exhibited without lowering the charge transfer efficiency of the secondary battery.
[0058] The thickness of the functional layer (120) may be 2 µm to 20 µm, and the thickness of the electrode active material layer (130) may be 50 µm to 150 µm. If the thickness of the functional layer (120) is less than 2 µm, the functional layer (120) may not be sufficient to operate, which may be problematic, and if it is more than 20 µm, the specific capacity of the secondary battery may be reduced, which may be problematic. In addition, the electrode active material layer (130) is provided with the aforementioned thickness, so that it can effectively affect the electrochemical performance and safety of the secondary battery together with the thickness of the functional layer (120).
[0059] The functional layer (120) may be heat-treated at 100°C to 160°C for 30 seconds to 10 minutes after being coated on the electrode current collector (110). The functional layer (120) may further include heat-treating after coating a mixture of the expanded graphite and the auxiliary binder on the electrode current collector (110). By heat-treating in the temperature range described above, the functional layer (120) may be more firmly attached.
[0060] The expanded graphite may be included in an amount of 0.1 to 1 part by weight based on 100 parts by weight of the electrode active material. If the expanded graphite is included in an amount of less than 0.1 part by weight, the electrode active material layer (130) may not be sufficiently detached at high temperatures, and if the expanded graphite is included in an amount of more than 1 part by weight, the distance between the electrode active material layer (130) and the negative electrode current collector (110) may increase, resulting in an increase in initial resistance and a decrease in specific capacity.
[0061] FIG. 2 is a drawing showing the functional layer of a negative electrode for a secondary battery from above according to another embodiment of the present invention.
[0062] Referring to FIG. 2, in the negative electrode for a secondary battery according to the present embodiment, the functional layer (120a, 120b, 120c) is provided on one surface of the negative electrode collector (110), and may be provided in a pattern shape so as to expose a portion of the surface of the negative electrode collector (110). Specifically, the functional layer (120a, 120b, 120c) may be provided in one or more of a striped shape (120a), a grid pattern (120b), and a wave pattern (120c).
[0063] In the functional layer (120a, 120b, 120c), by exposing a part of the surface of the negative electrode collector (110), the negative electrode collector (110) and the negative electrode active material layer can be brought into direct contact, thereby improving charge transfer efficiency. In addition, by providing the functional layer (120a, 120b, 120c) in a patterned form, the contact area with the negative electrode active material layer increases, so that the functional layer (120a, 120b, 120c) can stably fix the negative electrode active material layer, and when the expanded graphite expands, the negative electrode active material layer can be separated from the negative electrode collector (110) in a short period of time.
[0064] The secondary battery electrode (100) may include a negative electrode or a positive electrode. Specifically, when the secondary battery electrode (100) is a negative electrode, the electrode current collector (110) may be a negative electrode current collector, and the electrode active material layer (130) may be a negative electrode active material layer. In addition, when the secondary battery electrode (110) is a positive electrode, the electrode current collector (110) may be a positive electrode current collector, and the electrode active material layer (130) may be a positive electrode active material layer. The functional layer (120) may be provided by being coated on the negative electrode current collector or the positive electrode current collector.
[0065] Fig. 3 is a schematic drawing of a negative electrode for a secondary battery according to one embodiment of the present invention. Fig. 4 is a schematic drawing of the function of a functional layer at high temperatures in a negative electrode for a secondary battery according to one embodiment of the present invention.
[0066] Referring to FIGS. 3 and 4, the function of the functional layer (120) in the secondary battery electrode (100) will be described in detail. Since the function of the functional layer (120) is similar in the negative electrode and the positive electrode, the description will be focused on the case of the negative electrode.
[0067] The above electrode active material layer may be a negative electrode active material including a negative electrode active material and a negative electrode binder. The negative electrode active material layer may be prepared by coating a mixture of the negative electrode active material and the negative electrode binder on a functional layer composed of the expanded graphite and an auxiliary binder.
[0068] The above negative electrode active material may include natural graphite or artificial graphite. The natural graphite may include at least one of flake graphite, vein graphite, and amorphous graphite, and may be provided in various formations. Specifically, the natural graphite may be amorphous graphite. The natural graphite may have a tap density of 0.9 g / cc to 1.3 g / cc, and specifically, 0.92 g / cc to 1.15 g / cc. The average particle diameter (D50) of the natural graphite may be 5 μm to 30 μm.
[0069] The above artificial graphite may be in the form of powder, flakes, blocks, plates, or rods, and specifically, may be in the form of flakes or plates. The above artificial graphite has a specific surface area (BET) of 0.5 m in a range smaller than that of natural graphite. 2 / g to 5m 2 / g can be, specifically 0.6m 2 / g to 4m 2 / g. In addition, the artificial graphite may have a tap density of 0.7 g / cc to 1.1 g / cc, and specifically, 0.8 g / cc to 1.05 g / cc.
[0070] Alternatively, the negative electrode active material may include both the natural graphite and the artificial graphite, and the natural graphite and the artificial graphite may be included in a weight ratio of 10:90 to 90:10. Specifically, the weight ratio of the natural graphite and the artificial graphite may be 30:70 to 45:65.
[0071] The artificial graphite described above exhibits lower capacity than the natural graphite, has low manufacturing processability due to low electrode slurry and electrode adhesion, and has poor electrode rolling characteristics. The natural graphite exhibits poor swelling and rapid charging performance, and has a problem in that it has relatively more functional groups on its surface than the artificial graphite, resulting in poor high-temperature characteristics.
[0072] Therefore, the negative electrode for a secondary battery according to the present embodiment can improve the specific capacity of the secondary battery while improving high-temperature characteristics, etc., by including the negative electrode active material in the negative electrode active material layer as natural graphite and artificial graphite within the aforementioned range.
[0073] The above negative electrode binder and the auxiliary binder are each independently a non-aqueous binder of polyvinylidene fluoride-co-hexafluoropropylene (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, and polytetrafluoroethylene (PTFE); It may be at least one selected from the group consisting of an aqueous binder of acrylonitrile-butadiene rubber, styrene-butadiene rubber (SBR) or acrylic rubber; and a polymer resin of hydroxyethyl cellulose, carboxymethyl cellulose or polyvinylidene fluoride.
[0074] The negative electrode binder may be provided in an amount of 2 to 6 parts by weight based on 100 parts by weight of the negative electrode active material. In addition, the negative electrode binder may include a first binder and a second binder, and the first binder and the second binder may be included in a ratio of 30:70 to 70:30. If the content ratio of the second binder exceeds 70, the resistance of the secondary battery may increase, thereby reducing the specific capacity, and if it is less than 30, the adhesive strength between the negative electrode active material and the negative electrode current collector may decrease.
[0075] The first binder may include carboxyl methyl cellulose (CMC), and the second binder may include styrene-butadiene rubber (SBR). In addition, the auxiliary binder may include styrene-butadiene rubber (SBR).
[0076] The negative electrode binder provided in the negative electrode active material layer may be provided by mixing two types of first and second binders, and the auxiliary binder provided in the functional layer may be provided with the same material as the second binder. By providing the auxiliary binder and the second binder with the same material, the adhesive strength between the functional layer (120) and the negative electrode active material layer can be improved and the process efficiency can be increased.
[0077] The above negative electrode current collector may include at least one of a copper current collector, a copper composite current collector, a nickel current collector, a nickel composite current collector, a carbon paper current collector, and a carbon fiber current collector, copper (Cu), nickel coated copper (Ni coated Cu), stainless steel (SUS), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), carbon, and carbon fiber.
[0078] The above negative electrode is manufactured by applying, drying, and pressing a negative electrode active material onto a negative electrode current collector, and the conductive material, filler, etc. may be optionally further included as needed.
[0079] In another embodiment of the present invention, the secondary battery electrode may be a positive electrode. Specifically, the electrode current collector may be a positive electrode current collector, and the electrode active material layer may be a positive electrode active material layer. The functional layer may include expanded graphite and an auxiliary binder, and may be interposed between the positive electrode current collector and the positive electrode active material layer.
[0080] The above positive electrode active material layer may include a positive electrode active material, a conductive material, and a positive electrode binder.
[0081] The above cathode active material can be any cathode active material that is commonly used, and lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or a lithium composite oxide combining these can be used, but is not limited thereto.
[0082] The above conductive material can be used to improve the electrical conductivity of the anode, and at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fiber can be used.
[0083] The above-described positive electrode binder may include at least one resin selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As an example, the binder may include polyvinylidene fluoride.
[0084] The above cathode current collector may include one or more of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), and lithium (Li).
[0085] The above positive electrode can be manufactured by coating a positive electrode active material and conductive binder mixed in a slurry form on a positive electrode current collector and going through processes such as pressing and drying.
[0086] According to another aspect of the present invention, an embodiment of the present invention relates to a lithium secondary battery comprising a negative electrode; a positive electrode; and an electrolyte interposed therebetween, wherein the negative electrode or the positive electrode may include the negative electrode for a secondary battery described above.
[0087] According to another aspect of the present invention, an embodiment of the present invention includes a method for manufacturing an electrode for a secondary battery as described above, and the method for manufacturing an electrode for a secondary battery may include a step of preparing an electrode current collector; a step of coating a mixture including expanded graphite and an auxiliary binder on one surface of the electrode current collector and heat-treating at 100° C. to 160° C. to form a functional layer; and a step of forming an electrode active material layer on the functional layer.
[0088] In the step of forming the functional layer, the functional layer may include expanded graphite and the auxiliary binder in a ratio of 50:50 to 99:1. The expanded graphite and the auxiliary binder may be first mixed to prepare a mixture, and then the mixture may be formed by coating the mixture on the negative electrode current collector. The expanded graphite may have a particle size of 500 nm to 7 μm, and the expanded graphite may have an expansion ratio of 200% to 600% at 140°C.
[0089] In the step of forming the functional layer, the step of producing the expanded graphite may further include. The producing of the expanded graphite may include adding natural graphite or artificial graphite to a reactor equipped with an acidic solution and performing a first mixing at room temperature for 0.5 to 2 hours, adding an oxidizing agent to the reactor after the first mixing is completed and performing a second mixing at 30°C to 45°C for 6 to 30 hours, adding deionized water to the reactor after the second mixing is completed and performing a third mixing at 80°C to 100°C for 10 minutes to 1 hour, adding deionized water and hydrogen peroxide to the reactor after the third mixing is completed and performing a fourth mixing at room temperature for 1 to 30 minutes, and washing and drying after performing the fourth mixing.
[0090] When performing the above first mixing, the acidic solution has a pH of 0.1 to 5 and SO4 2- , Cl - , and NO3 -It may include one or more of the following. Specifically, the acidic solution may have a pH of 1 to 4, or 2 to 4, or 2.5 to 3.5.
[0091] When performing the above secondary mixing, the oxidizing agent may include one or more of potassium permanganate (KMnO4), hydrogen peroxide (H2O2), ozone (O3), peroxydisulfuric acid (H2S2O8), peroxymonosulfuric acid (H2SO5), potassium nitrate (KNO3), and sodium hypochlorite (NaClO).
[0092] When the electrode for the secondary battery is a negative electrode, the electrode current collector may be manufactured by including a negative electrode current collector, coating a functional layer on the negative electrode current collector, and then coating a negative electrode active material layer on the functional layer.
[0093] When the electrode for the secondary battery is a positive electrode, the electrode current collector may be manufactured by including a positive electrode current collector, coating a functional layer on the positive electrode current collector, and then coating a positive electrode active material layer on the functional layer.
[0094]
[0095] Hereinafter, examples and comparative examples of the present invention are described. However, the following examples are only preferred embodiments of the present invention and the scope of the present invention is not limited by the following examples.
[0096]
[0097] Preparation of Examples and Comparative Examples
[0098]
[0099] 1. Manufacturing of expanded graphite
[0100] 2 g of natural graphite (043480, Alfa Aesar) was placed in a reactor containing 82.8 g of H2SO4 (98 wt% in H2O) (112080, Merck) at room temperature, 1 g of NaNO3 (S5506, Sigma-Aldrich), and stirred for 1 hour. Subsequently, 6 g of KMnO4 (223468, Sigma-Aldrich) was added, and the temperature was heated to 35°C and stirred overnight. After stirring was completed, 92 g of deionized water (DIW) was added, the temperature was raised to 98°C, and the mixture was stirred for 30 minutes. After lowering the temperature to room temperature, 214.4 g of H2O2 (30 wt% in H2O) (H1009, Sigma-Aldrich) and 280 mL of deionized water were added, and the mixture was stirred for 5 minutes. After the second stirring was completed, the mixture was washed several times with deionized water and dried to produce expanded graphite.
[0101]
[0102] 2. Manufacturing of cathode according to comparative example 1 (Ref.)
[0103] A negative electrode slurry was prepared by mixing 97.8 wt% of natural graphite (043480, Alfa Aesar), 1.0 wt% of carboxymethyl cellulose (CMC) (419281, Sigma-Aldrich), and 1.2 wt% of styrene-butadiene rubber (SBR) (432490, Sigma-Aldrich) with deionized water, and having a solid content ratio ((graphite + binder) / (graphite + binder + solvent)) of 47.4% by weight. At this time, the solid content and solvent ratio in the negative electrode slurry was 53:47 by weight. The prepared negative electrode slurry was coated on a copper current collector with a thickness of 6 ㎛ to prepare a negative electrode. The prepared negative electrode had a loading level of 10.8 mg / cm 2 , the composite density was 1.6 g / cc, as shown in Table 1 below.
[0104]
[0105] 3. Preparation of cathode according to Example 1 (EG coated anode)
[0106] The previously manufactured expanded graphite and styrene butadiene rubber (SBR) (432490, Sigma-Aldrich) were mixed at a weight ratio of 50:50 to prepare a mixture, and then the prepared mixture was coated on a copper current collector with a thickness of 6 μm using a bar-coater (RDS3, CORETECH) to form a functional layer. At this time, the thickness of the functional layer was 3 μm, and the loading level of the functional layer (expanded graphite and SBR) was 0.044 mg / cm 2 And, the loading level of expanded graphite alone within the functional layer is 0.022 mg / cm 2 Here, 97.6 wt% of natural graphite (043480, Alfa Aesar), 1.0 wt% of carboxymethyl cellulose (CMC) (419281, Sigma-Aldrich), and 1.0 wt% of styrene butadiene rubber (SBR) (432490, Sigma-Aldrich) were mixed with deionized water to prepare a negative electrode slurry having a solid content ratio ((graphite + binder) / (graphite + binder + solvent)) of 47.4% by weight. At this time, the solid content and solvent ratio in the negative electrode slurry was 53:47 by weight. The negative electrode slurry was coated on the functional layer to prepare the negative electrode. The loading level of the prepared negative electrode was 10.8 mg / cm 2 , the composite density was 1.6 g / cc, as shown in Table 1 below.
[0107]
[0108] 4. Manufacturing of cathode according to comparative example 2 (EG added anode)
[0109] The previously manufactured expanded graphite 0.2 wt%, natural graphite 97.6 wt% (043480, Alfa Aesar), carboxymethyl cellulose (CMC) 1.0 wt% (419281, Sigma-Aldrich), and styrene butadiene rubber (SBR) 1.2 wt% (432490, Sigma-Aldrich) were mixed with deionized water to prepare an anode slurry with a solid content ratio ((graphite + binder) / (graphite + binder + solvent)) of 47.4% by weight. At this time, the solid content and solvent ratio in the anode slurry was 53:47 by weight. The manufactured anode slurry was coated on a copper current collector with a thickness of 6 ㎛ to prepare an anode. The manufactured anode had a loading level of 10.8 mg / cm 2 , the composite density was 1.6 g / cc, as shown in Table 1 below.
[0110]
[0111] Category 1 Category 2 Functional layer (wt%) Negative active material layer (wt%) SBR Expanded graphite Graphite CMC SBR Expanded graphite Comparative example 1 Ref. 0097.8 11.20 Example 1 EG coated anode 0.2 0.2 9 7.6 110 Comparative example 2 EG added anode 0097.6 11.2 0.2
[0112]
[0113] 5. Manufacturing of anode according to Comparative Example 3 (Ref.)
[0114] LiCoO2 (442704, Sigma-Aldrich), poly(vinylidene fluoride) (182702, Sigma-Aldrich), and carbon black (702102, Sigma-Aldrich) were added to N-methyl2-pyrrolidone (443778, Sigma-Aldrich) at a weight ratio of 98:1:1, respectively, to prepare a cathode slurry. At this time, the solid content and solvent ratio in the cathode slurry was 70:30 by weight. The prepared cathode slurry was coated on an aluminum current collector with a thickness of 10 ㎛, and after roll pressing, vacuum drying was performed to prepare a cathode. The manufactured positive electrode had a loading level of 20 mg / ㎠ (meaning that when aluminum foil coated with the positive electrode active material is sampled in a square of 1㎠, the weight of the positive electrode active material alone in the positive electrode composition is 20 mg), as shown in Table 2 below.
[0115]
[0116] 6. Manufacturing of anode according to Example 2 (EG coated cathode)
[0117] The previously manufactured expanded graphite and styrene butadiene rubber (SBR) (432490, Sigma-Aldrich) were mixed at a weight ratio of 50:50 to prepare a mixture, and then the prepared mixture was coated on an aluminum current collector, which is a positive electrode current collector with a thickness of 10 ㎛, using a bar-coater (RDS3, CORETECH) to form a functional layer. At this time, the thickness of the functional layer was 3 ㎛, and the loading level of the functional layer (expanded graphite and SBR) was 0.044 mg / cm 2 And, the loading level of expanded graphite alone within the functional layer is 0.022 mg / cm 2Here, LiCoO2 (442704, Sigma-Aldrich), poly(vinylidene fluoride) (182702, Sigma-Aldrich), and carbon black (702102, Sigma-Aldrich) were added to N-methyl2-pyrrolidone (443778, Sigma-Aldrich) at a weight ratio of 98:1:1, respectively, to prepare a cathode slurry. At this time, the solid content and solvent ratio in the cathode slurry was 70:30 by weight. The prepared cathode slurry was coated on a functional layer to prepare a cathode. The manufactured positive electrode had a loading level of 20 mg / ㎠ (meaning that when aluminum foil coated with the positive electrode active material is sampled in a square of 1㎠, the weight of the positive electrode active material alone in the positive electrode composition is 20 mg), as shown in Table 2 below.
[0118]
[0119] Functional layer (wt%) Cathode active material layer (wt%) Category 1 Category 2 SBR Expanded graphite LiCoO2 Carbon black PVdF Comparative example 3 Ref. 009811 Example 2 EG coated cathode 0.10.197.811
[0120]
[0121] Evaluation of Examples and Comparative Examples
[0122]
[0123] 1. Evaluation of high-temperature properties of expanded graphite
[0124] Figure 5 is a graph showing the expansion rate of manufactured expanded graphite according to the heat treatment temperature. Figure 6 is an SEM photograph of manufactured expanded graphite before and after heat treatment.
[0125] The expansion rate according to the heat treatment temperature was investigated using the previously manufactured expanded graphite. The device used was a tube furnace device (1100 Mini-mite Tube Furnace, FINETHERM), and the temperature was increased from 0℃ to 300℃ at a rate of 10℃ / min.
[0126] Referring to Fig. 5, it was confirmed that the expanded graphite manufactured according to the example did not expand during heat treatment and remained stable up to approximately 140°C, and then expanded by more than 600% in volume at 142°C. That is, the expanded graphite according to the present example rapidly expanded in volume at temperatures exceeding approximately 140°C.
[0127] Referring to Fig. 6, expanded graphite before heat treatment was compared with expanded graphite after heat treatment at 140°C. It was confirmed that the expanded graphite before heat treatment had a layered structure in which multiple layers were overlapped and attached to each other. On the other hand, it was confirmed that the expanded graphite after heat treatment had a layered structure in which the layers were spaced apart from each other and the interlayer distance increased. In other words, the expanded graphite was formed in a layered structure and was densely packed in an attached form until heat treatment at 140°C, whereas after heat treatment at 140°C, the layers were separated from each other, forming an air layer, which increased the volume.
[0128]
[0129] 2. Evaluation of cathode according to comparative examples and examples
[0130] Figure 7 is a graph comparing the adhesive strength before and after heat treatment in the negative electrode according to comparative examples and examples of the present invention. After fixing the negative electrode active material layer to the upper grip and the negative electrode current collector to the lower grip, respectively, the peel strength was analyzed by peeling them by pulling them in the 180° direction at a peel speed of 100 mm / min using a peel strength measuring device (AGS-J, SHIMADZU). At this time, the peel strength (unit: gf / mm), which is the required force, was measured.
[0131] Figure 8 is a graph comparing the resistance values before and after heat treatment in a cathode according to comparative examples and embodiments of the present invention. The manufactured cathode was placed between two measuring pins located above and below a potentiostat (XPF60-20DPMHV, IVSOLUTION), and a current of 10 mA was applied to measure the resistance value.
[0132] Table 3 below shows the results of the adhesive strength and resistance values of the negative electrode according to comparative examples and examples of the present invention. Here, the heat treatment temperature was 170°C.
[0133]
[0134] Classification 1 Classification 2 Adhesive strength (gf / mm) Resistance (Ω) Before heat treatment After heat treatment Before heat treatment After heat treatment Comparative example 1 Ref. 1.0 10.9 2 1.4 3.7 4 Example 1 EG coated anode 1.1 2 0.1 5 2.5 2 16.4 Comparative example 2 EG added anode 1.0 2 0.4 3 1.5 17.3 0
[0135]
[0136] Referring to FIGS. 7 and 8 and Table 2, it was confirmed that the adhesive strength of Comparative Example 1 did not change significantly before and after heat treatment, but the adhesive strength of Example 1 and Comparative Example 2 decreased significantly after heat treatment at 170°C compared to Comparative Example 1. In particular, it was confirmed that Example 1 decreased to half of the value of Comparative Example 2. This is because Example 1 has a functional layer, and the volume of the expanded graphite included in the functional layer increases due to heat treatment, and the negative electrode active material layer is detached from the negative electrode current collector by the expanded graphite. In addition, Comparative Example 2 does not have a functional layer and includes expanded graphite in the negative electrode active material layer, and it was confirmed that the volume of the expanded graphite included in the negative electrode active material layer expanded, resulting in a decrease in the overall adhesive strength. On the other hand, it was confirmed that Comparative Example 1, which does not include expanded graphite, maintains an adhesive strength that does not significantly differ before and after heat treatment because the negative electrode active material layer is firmly attached to the negative electrode current collector even when heat treated at a high temperature.
[0137] In addition, when checking the resistance before and after heat treatment at 170℃, it was confirmed that the resistance before and after heat treatment of Comparative Example 1 was maintained almost similarly, but the resistance of Example 1 and Comparative Example 2 increased significantly after heat treatment. In particular, the resistance of Example 1 increased more significantly than that of Comparative Example 1, and this is because, as described above, the negative electrode active material layer was detached from the negative electrode current collector due to the increase in the volume of the expanded graphite included in the functional layer.
[0138] That is, when using the negative electrode according to Example 1, the expanded graphite expands in volume at a high temperature of 170°C or higher, thereby causing the negative electrode active material to fall off from the negative electrode current collector, thereby preventing short circuits or ignition from occurring.
[0139] Figure 9 is a graph confirming the safety of the negative electrode according to comparative examples and examples of the present invention. To confirm the safety of the negative electrode, a positive electrode manufactured under the following conditions was utilized as a counter electrode. As a positive electrode active material, LiCoO2 (442704, Sigma-Aldrich), poly(vinylidene fluoride) (182702, Sigma-Aldrich), and carbon black (702102, Sigma-Aldrich) were added to N-methyl2-pyrrolidone (443778, Sigma-Aldrich) at a weight ratio of 98:1:1, respectively, to prepare a positive electrode slurry. At this time, the ratio of solid content to solvent in the positive electrode slurry was 70:30 by weight. The manufactured positive electrode slurry was coated on aluminum foil, and after roll pressing, vacuum drying was performed to manufacture a positive electrode having a loading level of 20 mg / ㎠ (meaning that when aluminum foil coated with the positive electrode active material is sampled in a square of 1㎠, the weight of the positive electrode active material alone in the positive electrode composition is 20 mg).
[0140] The positive electrode manufactured in this manner and the negative electrode according to Example 1 were brought into contact with each other while applying a constant pressure of 20 MPa, and then a constant voltage of 20 V was applied using a potentiostat (XPF60-20DPMHV, IVSOLUTION). At this time, the temperature change over time in the short-circuit region where the positive and negative electrodes were in contact was measured using a data logger (LR8431-20, HIOKI).
[0141] Referring to Fig. 9, it was confirmed that Comparative Example 1 (ref.) was short-circuited and the temperature rose to and was maintained at 351°C, whereas the temperatures of Example 1 and Comparative Example 2 rose to 164°C and 167°C, respectively, and then were maintained at a somewhat lowered state. In particular, it was confirmed that Example 1 had high stability even in a short-circuit as the temperature was maintained at a lowered state from 164°C to 95°C.
[0142]
[0143] 3. Evaluation of secondary batteries using cathodes according to comparative examples and examples
[0144] Half-cells and full-cells were manufactured using the negative electrode according to the manufacturing example described above.
[0145] The electrolyte was used by uniformly dissolving 5 wt% of fluoroethylene carbonate (FEC) as an additive and 1.2 mol / L LiPF6 as a lithium salt in ethylene carbonate and ethyl methyl carbonate (EC:EMC = 3:7 v / v) as a solvent.
[0146] The half-cell was manufactured as a 2032-coin-type half-cell (hereinafter, coin cell) using lithium metal (200 μm, Welcos) and an electrolyte as a negative electrode according to the examples and comparative examples.
[0147] The full cell was manufactured by using the cathode according to the examples and comparative examples in the anode and electrolyte described above, and inserting a separator (Celgard, model 2320) between the anode and cathode to manufacture an electrode assembly, and then adding it together with the electrolyte to a pouch-type case.
[0148]
[0149] Fig. 10 is a graph showing the electrochemical characteristics of a half-cell using a cathode according to comparative examples and examples of the present invention. Fig. 11 is a graph showing the electrochemical characteristics of a full-cell using a cathode according to comparative examples and examples of the present invention.
[0150] The electrochemical characteristics of the half-cell were confirmed by charging to 1.2 V and discharging to 0.01 V at a constant current of 0.2 C (1 C is 350 mA / g) at room temperature. The electrochemical characteristics of the full-cell were confirmed by charging to 4.35 V and discharging to 2.75 V at a constant current of 0.2 C (1 C is 150 mA / g) at room temperature.
[0151] Referring to FIGS. 10 and 11, it was confirmed that the charge / discharge profiles of Comparative Example 1, Example 1, and Comparative Example 2 were all similar. That is, it was confirmed that even when a functional layer including expanded graphite is provided, the electrochemical characteristics are not significantly affected.
[0152]
[0153] 4. Bipolar evaluation according to comparative examples and examples
[0154] Figure 12 is a graph confirming the safety of the anode according to comparative examples and embodiments of the present invention.
[0155] To verify the safety of the positive electrode, a negative electrode manufactured under the following conditions was utilized. 97.8 wt% of natural graphite (043480, Alfa Aesar), 1.0 wt% of carboxymethyl cellulose (CMC) (419281, Sigma-Aldrich), and 1.2 wt% of styrene butadiene rubber (SBR) (432490, Sigma-Aldrich) were mixed with deionized water to prepare a negative electrode slurry. The solid and solvent ratio in the negative electrode slurry was 53:47 by weight. The prepared negative electrode slurry was coated on a copper current collector, roll-pressed, and vacuum-dried to obtain a loading level of 10.8 mg / cm. 2 A human negative electrode was manufactured.
[0156] The cathode manufactured in this manner and the anode according to Example 2 were brought into contact with each other while applying a constant pressure of 20 MPa, and then a constant voltage of 20 V was applied using a potentiostat (XPF60-20DPMHV, IVSOLUTION). At this time, the temperature change over time in the short-circuit region where the anode and cathode were in contact was measured using a data logger (LR8431-20, HIOKI).
[0157] Referring to Fig. 12, it was confirmed that Comparative Example 3 (ref.) was short-circuited and the temperature rose to and was maintained at 351°C, whereas Example 2 was short-circuited and the temperature rose to 172°C and then maintained at a somewhat lower temperature of 104°C. It was confirmed that Example 2, which is an anode including a functional layer, had higher stability even in a short-circuit than Comparative Example 3, which does not have a functional layer.
[0158]
[0159] Those skilled in the art will appreciate that the present invention can be implemented in other specific forms without altering its technical spirit or essential characteristics. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. The scope of the present invention is defined by the claims below rather than the detailed description above, and all changes or modifications derived from the meaning and scope of the claims and their equivalents should be construed as being included within the scope of the present invention.
Claims
1. Electrode collector; A functional layer coated on at least a portion of the above electrode collector; and Including an electrode active material layer provided on the above functional layer; An electrode for a secondary battery, wherein the functional layer comprises expanded graphite and an auxiliary binder.
2. In paragraph 1, An electrode for a secondary battery, wherein the expanded graphite and the auxiliary binder are included in the functional layer in a ratio of 50:50 to 99:
1.
3. In paragraph 1, An electrode for a secondary battery, wherein the expanded graphite has a particle size of 500 nm to 7 μm and an expansion rate of the expanded graphite at 140°C of 200% to 600%.
4. In paragraph 1, An electrode for a secondary battery, wherein the functional layer includes an opening to expose at least a portion of the surface of the electrode collector.
5. In paragraph 4, An electrode for a secondary battery, wherein the functional layer is provided on one surface of the electrode collector, and is provided in a patterned form so as to expose a portion of the surface of the electrode collector.
6. In paragraph 1, The thickness of the above functional layer is 2㎛ to 20㎛, An electrode for a secondary battery, wherein the thickness of the electrode active material layer is 50 ㎛ to 150 ㎛.
7. In paragraph 1, An electrode for a secondary battery, wherein the functional layer is coated on the electrode collector and then heat-treated at 100°C to 160°C for 30 seconds to 10 minutes.
8. In paragraph 1, The above electrode active material layer includes a negative electrode active material and a negative electrode binder, The above negative electrode binder and the auxiliary binder are each independently a non-aqueous binder of polyvinylidene fluoride-co-hexafluoropropylene (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, and polytetrafluoroethylene (PTFE); An electrode for a secondary battery, comprising at least one selected from the group consisting of an aqueous binder of acrylonitrile-butadiene rubber, styrene-butadiene rubber (SBR), or acrylic rubber; and a polymer resin of hydroxyethyl cellulose, carboxymethyl cellulose, or polyvinylidene fluoride.
9. In paragraph 1, An electrode for a secondary battery, wherein the expanded graphite is included in an amount of 0.1 to 1 part by weight relative to 100 parts by weight of the electrode active material.
10. In paragraph 1, The above electrode active material layer includes a negative electrode active material and a negative electrode binder, The above negative electrode active material is an electrode for a secondary battery including natural graphite or artificial graphite.
11. In paragraph 10, The above negative electrode binder is provided in an amount of 2 to 6 parts by weight per 100 parts by weight of the negative electrode active material. The above negative binder includes a first binder and a second binder, An electrode for a secondary battery, wherein the first binder and the second binder are included in a ratio of 30:70 to 70:
30.
12. In paragraph 11, The first binder comprises carboxyl methyl cellulose (CMC), and the second binder comprises styrene-butadiene rubber (SBR). An electrode for a secondary battery, wherein the auxiliary binder comprises styrene-butadiene rubber (SBR).
13. In paragraph 1, The above electrode collector includes a negative electrode collector or a positive electrode collector, The above negative electrode collector comprises at least one of copper (Cu), nickel-coated copper (Ni coated Cu), stainless steel (SUS), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), carbon, and carbon fiber. An electrode for a secondary battery, wherein the positive electrode current collector comprises at least one of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), and lithium (Li).
14. In a lithium secondary battery including a cathode; an anode; and an electrolyte interposed therebetween, A lithium secondary battery, characterized in that the negative electrode or positive electrode is an electrode according to any one of claims 1 to 13.
15. Step for preparing the electrode collector; A step of coating a mixture containing expanded graphite and an auxiliary binder on one surface of the electrode collector and heat-treating at 100°C to 160°C to form a functional layer; and A method for manufacturing an electrode for a secondary battery according to any one of claims 1 to 13, comprising a step of forming an electrode active material layer on the functional layer.
16. In paragraph 15, A method for manufacturing an electrode for a secondary battery, wherein the expanded graphite and the auxiliary binder in the functional layer are included in a ratio of 50:50 to 99:
1.
17. In paragraph 15, A method for manufacturing an electrode for a secondary battery, wherein the expanded graphite has a particle size of 500 nm to 7 μm and an expansion rate of the expanded graphite at 140°C of 200% to 600%.
18. In paragraph 15, The above expanded graphite is, Natural graphite or artificial graphite is added to a reactor equipped with an acid solution and primary mixing is performed at room temperature for 0.5 to 2 hours. After the above first mixing is completed, an oxidizing agent is added to the reactor and a second mixing is performed at 30°C to 45°C for 6 to 30 hours. After the above secondary mixing is completed, deionized water is added to the reactor and a third mixing is performed at 80°C to 100°C for 10 minutes to 1 hour. After the above 3rd mixing is completed, deionized water and hydrogen peroxide are added to the reactor and the 4th mixing is performed at room temperature for 1 to 30 minutes. A method for manufacturing an electrode for a secondary battery, which is manufactured by performing the above 4th mixing, then washing and drying.
19. In paragraph 18, The above acidic solution has a pH of 0.1 to 5 and SO4 2- , Cl - , and NO3 - Contains one or more of the following: A method for manufacturing an electrode for a secondary battery, wherein the oxidizing agent comprises at least one of potassium permanganate (KMnO4), hydrogen peroxide (H2O2), ozone (O3), peroxydisulfuric acid (H2S2O8), peroxymonosulfuric acid (H2SO5), potassium nitrate (KNO3), and sodium hypochlorite (NaClO).
Citation Information
Patent Citations
Electrode for battery and battery using the same
JP2004030998A
Nonaqueous electrolyte secondary battery
KR1020080092281A
Cathode for battery, method for manufacturing thereof, and lithium secondary battery comprising the same
KR1020090076277A
Electromagnetic-wave-absorbing composite sheet
KR102123786B1
KR20190081771A