Sodium-ion battery positive electrode precursor, preparation method therefor, and use thereof

By covering the surface of the nickel-ferromanganese precursor of the sodium ion battery positive electrode material with infinite order, the problems of low energy density and poor cycle stability of the sodium ion battery positive electrode material are solved, and the problem of low energy density and poor cycle stability of the sodium ion battery positive electrode material is improved The material's cycle stability and rate performance enable high capacity and long life sodium ion batteries.

WO2024239458A1PCT designated stage expired Publication Date: 2024-11-28JINGMEN GEM NEW MATERIAL CO LTD +1

Patent Information

Application Number
PCT/CN2023/111981
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2023-08-09
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing sodium ion battery positive electrode materials have problems with low energy density and poor cycle stability, mainly because the large radius of sodium leads to the deintercalation of Na+, causing the transition metal layer to slip, and the elements precipitation are uneven during the co-precipitation preparation process. Causes rapid attenuation of battery capacity.

Method used

An infinitely ordered metal organic framework compound (Y-MOF) is coated on the surface of the nickel-ferromanganese precursor through nano-wet coating technology. The Y-MOF is coordinated and synthesized by metal and organic carboxylic acid to form a tight and uniform The porous conductive adsorption structure overcomes the problem of uneven coating elements and improves cycle stability and rate performance.

Benefits of technology

The cycle stability and rate performance of sodium electropositive electrode materials are improved, ensuring rapid de-embedding of Na+, avoiding resistance increase and rate performance reduction, and the reversible capacity of the battery can reach more than 136.28mA/hg, and 0.1C cycle The capacity retention rate after 100 turns can reach more than 85.16%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023111981_28112024_PF_FP_ABST
    Figure CN2023111981_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A sodium-ion battery positive electrode precursor, a preparation method therefor, and the use thereof. The preparation method comprises the following steps: (1) mixing a nickel source, a manganese source and an iron source to obtain a ternary salt solution, and adding in parallel the ternary salt solution, an alkali solution and a complexing agent to a substrate solution to undergo a coprecipitation reaction, so as to obtain a ternary precursor; and (2) by using the ternary precursor as a matrix, adding in parallel a carboxylic acid solution and a metal salt solution to a reaction vessel to perform a coating reaction on the matrix, and aging same to obtain the sodium-ion battery positive electrode precursor. The outer layer of the precursor is coated with a Y-MOF by means of a nano wet-coating process, wherein the Y-MOF is synthesized by coordination of a metal and an organic carboxylic acid, is an infinitely-ordered layered structure compound and is highly-ordered in the nano-level; thus, said Y-MOF can compactly and uniformly coat the surface of nickel-iron-manganese, so that the problem of non-uniformity of coating elements is solved, thereby improving the cycling stability and the rate capability of sodium-electric positive electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

A sodium cathode precursor and its preparation method and application

[0001] The present application belongs to the technical field of sodium ion batteries and relates to a sodium battery positive electrode precursor and its preparation method and application. Background Art

[0002] Lithium-ion batteries, due to their high energy density and long cycle life, have dominated the secondary battery market. Currently, most advanced energy storage systems utilize lithium-ion battery technology. However, the development of lithium-ion batteries faces certain limitations, particularly due to price fluctuations and the depletion and future shortage of lithium resources. Consequently, sodium, a resource-rich substance, has garnered significant attention. Sodium and lithium are members of the same family, sharing similar electrochemical properties. Compared to lithium-ion batteries, sodium-ion batteries offer numerous potential advantages, including abundant resources and low cost, making them suitable for large-scale energy storage and poised to become a promising new type of green and environmentally friendly energy storage battery.

[0003] In the positive electrode materials of sodium ion batteries, the diffusion barrier of sodium ions migrating in layered materials is lower than that of lithium ions. Layered compounds are very advantageous as sodium storage materials because the interlayer spacing perpendicular to the c-axis can be adjusted during the sodium ion deintercalation process. Therefore, when studying the positive electrode materials of sodium ion batteries, layered transition metal oxides are usually the first choice. On the other hand, layered oxides are widely studied due to their easy synthesis, high energy / power density, and environmental friendliness. Its general chemical formula can be expressed as Na x TMO2 (x≤1, TM is Ni, Mn, Fe, Co, Cu, etc.). In addition, layered oxides are prepared using a co-precipitation-high-temperature solid-phase sintering method, which is similar to the preparation method of lithium battery positive electrode materials, and the process equipment is basically the same. Therefore, sodium battery layered oxide positive electrode materials are considered to be the most suitable sodium battery material for large-scale production.

[0004] CN103985851A discloses a type of sodium ion battery positive electrode material and a sodium ion battery comprising the positive electrode material. The preparation method comprises: mixing sodium carbonate, M oxide and L oxide according to a stoichiometric ratio, ball milling, calcining, and ball milling to obtain the sodium ion battery positive electrode material.

[0005] CN109638278A discloses a sodium ion battery positive electrode material and a sodium ion battery, comprising granular Na x MnO2 material, where 0<x≤1, Na x Each particle of the MnO2 material contains randomly stacked MnO2 nanosheets, and a staggered stacking structure is formed between multiple MnO2 nanosheets.

[0006] The sodium cathode material described in the above scheme has the problems of low energy density and poor cycle stability. The main reason is that the radius of sodium is larger than that of lithium. + The deintercalation and insertion of the transition metal layer causes slippage, which leads to the O3-P2 phase transition and deteriorates the cycle stability. At the same time, the co-precipitation preparation process may lead to uneven element precipitation. As a result, sodium branched crystals are generated during the cycle of the sodium ion battery, resulting in rapid battery capacity decay.

[0007] Summary of the Invention

[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0009] The purpose of this application is to provide a sodium cathode precursor and its preparation method and application. This application uses a nano-wet coating technology to coat a metal organic framework compound (Y-MOF) on the outer layer of the precursor. The Y-MOF is synthesized by coordination of metal and organic carboxylic acid. It is an infinitely ordered layered structure compound with high order at the nanometer level and can be tightly and evenly coated on the surface of nickel iron manganese. This overcomes the problem of uneven coating elements, thereby improving the cycle stability and rate performance of the sodium cathode material.

[0010] To achieve this goal, this application adopts the following technical solutions:

[0011] In a first aspect, an embodiment of the present application provides a method for preparing a sodium cathode precursor, the preparation method comprising the following steps:

[0012] (1) mixing a nickel source, a manganese source, and an iron source to obtain a ternary salt solution, and adding the ternary salt solution, an alkali solution, and a complexing agent to a bottom liquid in parallel for a coprecipitation reaction to obtain a ternary precursor;

[0013] (2) Using the ternary precursor as a matrix, adding a carboxylic acid solution and a metal salt solution into a reaction vessel in parallel to carry out a coating reaction with the matrix, and obtaining the sodium cathode precursor after aging.

[0014] The embodiment of the present application adopts a co-precipitation method with a relatively stable reaction system to prepare nickel-iron-manganese hydroxide precursor, with uniform spherical particle size, while ensuring that nickel-iron-manganese hydroxide is completely precipitated, and no nickel-iron-manganese elements are present in the supernatant. The metal salt reacts with the carboxylic acid solution under certain conditions to form Y-MOFs. Y-MOF is an infinitely ordered layered structure compound that ensures the uniformity of the Y element coating at the atomic level of the shell, solving the problem of uneven solid phase coating at the positive electrode material end. The porous conductive adsorption structure coated on the surface can achieve Na + The rapid deintercalation alleviates the problem of increased resistance caused by conventional coating and avoids a significant decrease in rate performance after coating.

[0015] In one embodiment, the nickel source in step (1) includes any one of nickel sulfate, nickel nitrate or nickel chloride, or a combination of at least two of them.

[0016] In one embodiment, the manganese source includes any one of manganese sulfate, manganese nitrate, or manganese chloride, or a combination of at least two thereof.

[0017] In one embodiment, the iron source includes any one of ferrous sulfate, ferrous nitrate or ferrous chloride, or a combination of at least two thereof.

[0018] In one embodiment, the concentration of the ternary salt solution is 2 to 4 mol / L, for example, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L or 4 mol / L.

[0019] In one embodiment, the alkali solution in step (1) comprises any one of sodium hydroxide solution, sodium carbonate solution or potassium hydroxide solution, or a combination of at least two thereof.

[0020] In one embodiment, the concentration of the alkali solution is 2 to 4 mol / L, for example, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L or 4 mol / L.

[0021] In one embodiment, the complexing agent comprises aqueous ammonia.

[0022] In one embodiment, the concentration of the ammonia solution is 1 to 3 mol / L, for example, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L or 3 mol / L.

[0023] In one embodiment, the base solution includes a complexing agent, an alkali solution and water.

[0024] In one embodiment, the pH of the base solution is 10-12, for example, 10, 10.5, 11, 11.5 or 12.

[0025] In one embodiment, the concentration of the complexing agent in the base solution is 7 to 11 g / L, for example, 7 g / L, 8 g / L, 9 g / L, 10 g / L or 11 g / L.

[0026] In one embodiment, the flow rate of the ternary salt solution in step (1) is 30 to 60 kg / h, for example, 30 kg / h, 35 kg / h, 40 kg / h, 50 kg / h or 60 kg / h.

[0027] In one embodiment, the flow rate of the alkali solution is 3 to 8 kg / h, for example, 3 kg / h, 4 kg / h, 5 kg / h, 6 kg / h, 7 kg / h or 8 kg / h.

[0028] In one embodiment, the flow rate of the complexing agent is 10 to 20 kg / h, for example, 10 kg / h, 12 kg / h, 15 kg / h, 18 kg / h or 20 kg / h.

[0029] In one embodiment, the coprecipitation reaction temperature is 45-70°C, for example, 45°C, 50°C, 55°C, 60°C or 70°C.

[0030] In one embodiment, the coprecipitation reaction time is 50 to 70 hours, for example, 50 hours, 55 hours, 60 hours, 65 hours or 70 hours.

[0031] In one embodiment, the stirring speed of the coprecipitation reaction is 120-400 rpm, for example, 120 rpm, 150 rpm, 200 rpm, 300 rpm or 400 rpm.

[0032] In one embodiment, the solute of the carboxylic acid solution in step (2) includes any one of 5-hydroxyisophthalic acid, trimesic acid, or 1,2,4,5-benzenetetracarboxylic acid, or a combination of at least two thereof.

[0033] In one embodiment, the solvent of the carboxylic acid solution includes any one of N,N-dimethylformamide, N,N-diethylformamide, methanol, ethanol or propanol, or a combination of at least two thereof.

[0034] In one embodiment, the concentration of the carboxylic acid solution is 1.8 to 2.2 mol / L, for example, 1.8 mol / L, 1.9 mol / L, 2 mol / L, 2.1 mol / L or 2.2 mol / L.

[0035] In one embodiment, the metal salt solution includes any one of aluminum salt solution, magnesium salt solution, zirconium salt solution, calcium salt solution, titanium salt solution or tungsten salt solution, or a combination of at least two thereof.

[0036] In one embodiment, the concentration of the metal salt solution is 1 to 3 mol / L, for example, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L or 3 mol / L.

[0037] In one embodiment, the flow rate of the carboxylic acid solution in step (2) is 1 to 3 L / h, for example, 1 L / h, 1.5 L / h, 2 L / h, 2.5 L / h or 3 L / h.

[0038] In one embodiment, the flow rate of the metal salt solution is 8 to 16 L / h, for example, 8 L / h, 10 L / h, 12 L / h, 14 L / h or 16 L / h.

[0039] In one embodiment, the pH of the coating reaction in step (2) is 7 to 8, for example, 7, 7.2, 7.5, 7.8 or 8.

[0040] In one embodiment, the coating reaction temperature is 50-65°C, for example, 50°C, 52°C, 55°C, 60°C or 65°C.

[0041] In one embodiment, the coating reaction time is 2 to 8 hours, for example, 2 hours, 3 hours, 5 hours, 6 hours or 8 hours.

[0042] In one embodiment, the stirring speed of the coating reaction is 250-350 rpm, for example, 250 rpm, 280 rpm, 300 rpm, 320 rpm or 350 rpm.

[0043] In one embodiment, the aging time is 2 to 5 hours, for example, 2 hours, 3 hours, 4 hours or 5 hours.

[0044] In the second aspect, an embodiment of the present application provides a sodium cathode precursor, which is prepared by the method described in the first aspect. In the sodium cathode precursor, the content of the coating metal is 1000 to 10000 ppm, for example: 1000 ppm, 2000 ppm, 5000 ppm, 8000 ppm or 10000 ppm, etc.

[0045] The surface coating Y-MOF of the sodium cathode precursor in the embodiment of the present application is a porous conductive adsorption layer, which can ensure the Na + The deintercalation solves the problem of poor rate performance of conventional coating element materials.

[0046] In a third aspect, an embodiment of the present application provides a sodium cathode material, which is obtained by sintering the sodium cathode precursor as described in the second aspect in one step, mixing it with a sodium source, and then sintering it in two steps.

[0047] In one embodiment, the one-step sintering temperature is 400-600°C, for example, 400°C, 450°C, 500°C, 550°C or 600°C.

[0048] In one embodiment, the one-step sintering time is 3 to 6 hours, for example, 3 hours, 4 hours, 5 hours or 6 hours.

[0049] In one embodiment, the sodium source comprises sodium carbonate.

[0050] In one embodiment, the temperature of the two-step sintering is 800-1200°C, for example, 800°C, 900°C, 1000°C, 1100°C or 1200°C.

[0051] In one embodiment, the two-step sintering time is 10 to 20 hours, for example, 10 hours, 12 hours, 15 hours, 18 hours or 20 hours.

[0052] In a fourth aspect, an embodiment of the present application provides a sodium ion battery, which comprises the sodium cathode material as described in the third aspect.

[0053] Compared with the prior art, this application has the following beneficial effects:

[0054] (1) This application uses nano-wet coating technology to coat a metal organic framework compound (Y-MOF) on the outer layer of the precursor. The Y-MOF is synthesized by coordination of metal and organic carboxylic acid. It is an infinitely ordered layered structure compound with high order at the nanometer level and can be tightly and evenly coated on the surface of nickel iron manganese. It overcomes the problem of uneven coating elements, thereby improving the cycle stability and rate performance of sodium positive electrode materials. The Y-MOF coated on the surface of the precursor is a porous conductive adsorption layer that can ensure the Na + The deintercalation solves the problem of poor rate performance of conventional coating element materials.

[0055] (2) The coating method described in this application is a continuous reaction synthesis based on the original nickel-iron-manganese precursor system, which is simple to operate and can provide the possibility for subsequent pilot production and even mass production.

[0056] (3) The precursor described in this application is made into a sodium battery positive electrode material, and the reversible capacity of the battery produced can reach more than 136.28 mA / hg, and the capacity retention rate after 100 cycles at 0.1C can reach more than 85.16%.

[0057] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.

[0059] FIG1 is a SEM image of the sodium cathode precursor described in Example 3 of the present application. DETAILED DESCRIPTION

[0060] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.

[0061] Example 1

[0062] This embodiment provides a sodium battery cathode precursor, and the preparation method of the sodium battery cathode precursor is as follows:

[0063] (1) nickel sulfate, ferrous sulfate and manganese sulfate solutions were prepared in a molar ratio of 0.25:0.5:0.25 to prepare a 2 mol / L nickel-iron-manganese mixed metal salt A solution; a 1 mol / L ammonia solution and a 2 mol / L liquid alkali solution were prepared in a 1 m 3 Ammonia complexing agent, liquid alkali, and pure water were added to the reactor as the base liquid, and inert gas was introduced as a protective gas to prevent oxidation of Mn and Fe during the reaction. When the pH of the base liquid reached 11.2 and the ammonia concentration reached 7 g / L, solution A, ammonia complexing agent, and sodium hydroxide solution were added to the reactor at a flow rate of 30 kg / h for solution A, 3 kg / h for ammonia, and 10 kg / h for liquid alkali. The reaction was carried out at 52° C. and a stirring speed of 350 rpm for 50 hours to obtain a Ni-2O3 with a particle size of 2.5 μm. 0.25 Fe 0.5 Mn 0.25 (OH)2 spherical particles;

[0064] (2) 5-Hydroxyisophthalic acid was dissolved in methanol to prepare a 2 mol / L solution B, and zirconium sulfate tetrahydrate was dissolved in deionized water to prepare a zirconium salt solution with a concentration of 1 mol / L. The precursor particles in the reactor were used as the matrix, and solution B and zirconium sulfate solution were continuously added to the reactor at a feed rate of 1 L / h and 8 L / h, respectively, to react with the precursor matrix. During the reaction, the pH of the reaction was maintained between 7 and 7.5. The reaction was carried out at 50 ° C for 3 h, the stirring speed was 350 pm, and then aged for 2 h to obtain Zr-MOF@Ni 0.25 Fe 0.5 Mn 0.25 (OH)2 sodium cathode precursor, wherein the Zr content is 1000ppm.

[0065] Example 2

[0066] This embodiment provides a sodium battery cathode precursor, and the preparation method of the sodium battery cathode precursor is as follows:

[0067] (1) nickel sulfate, ferrous sulfate and manganese sulfate solutions were prepared in a molar ratio of 0.34:0.33:0.33 to prepare a 2 mol / L nickel-iron-manganese mixed metal salt A solution; a 2 mol / L ammonia solution and a 2 mol / L liquid alkali solution were prepared in a 1 m 3 Ammonia complexing agent, liquid alkali, and pure water are added to the reactor as the base liquid, and inert gas is introduced as a protective gas to prevent oxidation of Mn and Fe during the reaction. When the pH of the base liquid reaches 10.5 and the ammonia concentration reaches 8 g / L, solution A, ammonia complexing agent, and sodium hydroxide solution are added to the reactor at a feed rate of 40 kg / h for solution A, 4 kg / h for ammonia, and 15 kg / h for liquid alkali. The reaction is carried out at 58° C. and a stirring speed of 320 rpm for 60 hours to obtain a Ni-N-Ni ... 0.34 Fe 0.33 Mn 0.33 (OH)2 spherical particles;

[0068] (2) Trimellitic acid was dissolved in methanol to prepare a 2 mol / L solution B, and magnesium sulfate was dissolved in deionized water to prepare a 2 mol / L magnesium sulfate solution. The precursor particles in the reactor were used as the matrix, and solution B and magnesium sulfate solution were continuously added to the reactor at a feed rate of 2 L / h and 10 L / h, respectively, to react with the precursor matrix. During the reaction, the pH of the reaction was maintained between 7.5 and 8. The reaction was carried out at 55 ° C for 3 h, the stirring speed was 300 pm, and then aged for 2 h to obtain Mg-MOF@Ni 0.34 Fe 0.33 Mn 0.33 (OH)2 sodium cathode precursor with a Mg content of 5000ppm.

[0069] Example 3

[0070] This embodiment provides a sodium battery cathode precursor, and the preparation method of the sodium battery cathode precursor is as follows:

[0071] (1) nickel sulfate, ferrous sulfate and manganese sulfate solutions were prepared in a molar ratio of 0.6:0.2:0.2 to prepare a 3 mol / L nickel-iron-manganese mixed metal salt A solution; a 2 mol / L ammonia solution and a 4 mol / L liquid alkali solution were prepared in a 1 m 3Ammonia complexing agent, liquid alkali, and pure water are added to the reactor as the base liquid, and inert gas is introduced as a protective gas to prevent oxidation of Mn and Fe during the reaction. When the pH of the base liquid reaches 11.5 and the ammonia concentration reaches within the range of 10 g / L, solution A, ammonia complexing agent, and sodium hydroxide solution are added to the reactor at a feed rate of 60 kg / h for solution A, 8 kg / h for ammonia, and 20 kg / h for liquid alkali. The reaction is carried out at 60° C. and a stirring speed of 350 rpm for 70 hours to obtain a Ni-N-Ni ... 0.6 Fe 0.2 Mn 0.2 (OH)2 spherical particles;

[0072] (2) 1,2,4,5-benzenetetracarboxylic acid was dissolved in methanol to prepare a 2 mol / L solution B, and aluminum sulfate 18hydrate was dissolved in deionized water to prepare an aluminum salt solution with a concentration of 3 mol / L. The precursor particles in the reactor were used as the matrix, and solution B and aluminum sulfate solution were continuously added to the reactor at a feed rate of 3 L / h and 16 L / h, respectively, to react with the precursor matrix. During the reaction, the pH of the reaction was maintained between 7 and 7.5. The reaction was carried out at 65 ° C for 8 h, the stirring speed was 250 pm, and then aged for 5 h to obtain Al-MOF@Ni 0.6 Fe 0.2 Mn 0.2 (OH)2 sodium cathode precursor, wherein the Al content is 10000 ppm. The SEM image of the sodium cathode precursor is shown in FIG1 .

[0073] Example 4

[0074] The only difference between this embodiment and embodiment 1 is that the concentration of the metal salt solution is 0.5 mol / L, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0075] Example 5

[0076] The only difference between this embodiment and embodiment 1 is that the concentration of the metal salt solution is 4 mol / L, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0077] Example 6

[0078] The only difference between this embodiment and embodiment 1 is that the pH of the reaction in step (2) is 6.5, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0079] Example 7

[0080] The only difference between this embodiment and embodiment 1 is that the pH of the reaction in step (2) is 8.5, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0081] Example 8

[0082] The only difference between this embodiment and embodiment 1 is that the reaction temperature in step (2) is 45° C., and the other conditions and parameters are exactly the same as those in embodiment 1.

[0083] Example 9

[0084] The only difference between this embodiment and embodiment 1 is that the reaction temperature in step (2) is 70° C., and the other conditions and parameters are exactly the same as those in embodiment 1.

[0085] Comparative Example 1

[0086] The only difference between this comparative example and Example 1 is that Zr-MOFs are not coated, and other conditions and parameters are exactly the same as those in Example 1.

[0087] Performance testing:

[0088] The precursors prepared in the examples and comparative examples were pre-calcined in a muffle furnace at 400° C. for 4 h to obtain nickel-iron-manganese oxide. The nickel-iron-manganese oxide was mixed with sodium carbonate in a mortar and then calcined at 900° C. for 10 h to obtain a nickel-iron-manganese sodium cathode material with a metal outer layer. The cathode materials prepared in the examples and comparative examples were assembled into button batteries for electrochemical testing. The performance test parameters were as follows:

[0089] Reversible capacity test: The half-cell was initially charged and discharged at a current density of 0.1C with a voltage range of 2-4.2V.

[0090] Cycling performance test: half cell was cycled 100 times at 1C with a voltage range of 2-4.2V.

[0091] The test results are shown in Table 1:

[0092] Table 1

[0093] As can be seen from Table 1, from Examples 1-3, the reversible capacity of the battery prepared by making the precursor described in this application into a sodium battery positive electrode material can reach more than 136.28 mA / hg, and the capacity retention rate after 100 cycles at 0.1C can reach more than 85.16%.

[0094] By comparing Example 1 with Examples 4-5, it can be seen that during the preparation of the sodium cathode precursor described in this application, the concentration of the metal salt solution affects its performance. When the concentration of the metal salt solution is controlled at 1 to 3 mol / L, the performance of the sodium cathode precursor is better. If the concentration of the metal salt solution is too high, the particle growth rate during the reaction is too fast, resulting in poor sphericity and dispersibility. If the concentration of the metal salt solution is too low, new crystal nuclei are easily formed during the growth of the precursor particles, resulting in poor particle uniformity and consistency.

[0095] From the comparison between Example 1 and Example 6-7, it can be seen that in the preparation process of the sodium cathode precursor of the present application, the pH of the reaction in step (2) will affect its performance. The performance of the sodium cathode precursor prepared by controlling the pH of the reaction at 7 to 8 is better. If the pH of the reaction is too high, the precipitation rate of the metal ions is too fast during the coprecipitation process, and the Ni 2+ 、Co 2+ and Mn 2+ If the pH of the reaction is too low, the particles will grow too fast during the reaction and easily agglomerate, resulting in poor sphericity and dispersion of the sample.

[0096] From the comparison between Example 1 and Example 8-9, it can be seen that in the preparation process of the sodium cathode precursor of the present application, the temperature of the reaction in step (2) will affect its performance. When the reaction temperature is controlled at 50-65°C, the performance of the sodium cathode precursor is better. If the reaction temperature is too high, Mn(OH)2, Co(OH)2 and Co(NH3)6 2+ The oxidation tendency of the metal ions increases, and the ammonia in the precipitation is more volatile. The loss of ammonia can easily reduce the coordination effect of the metal ions in the system, resulting in an accelerated precipitation rate. If the reaction temperature is too low, the adsorption of impurity ions by the precipitate will increase, and the "thermal motion" of the ions in the solution will be reduced, making it difficult to obtain high-purity and large-sized particles.

[0097] As can be seen from the comparison between Example 1 and Comparative Example 1, this application mainly uses a nano-wet coating technology to coat a metal organic framework compound (Y-MOF) on the outer layer of the precursor. The Y-MOF is synthesized by coordination of metal and organic carboxylic acid. It is an infinitely ordered layered structure compound that is highly ordered at the nanometer level and can be tightly and evenly coated on the surface of nickel iron manganese. This overcomes the problem of uneven coating elements, thereby improving the cycle stability and rate performance of the sodium cathode material.

[0098] The applicant declares that the above is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Technical personnel in the relevant technical field should understand that any changes or substitutions that can be easily thought of by technical personnel in the relevant technical field within the technical scope disclosed in this application fall within the protection scope and disclosure scope of this application.

Claims

1. A method for preparing a sodium cathode precursor, the method comprising the following steps: (1) mixing a nickel source, a manganese source and an iron source to obtain a ternary salt solution, and adding the ternary salt solution, an alkali solution and a complexing agent to a base liquid in parallel for a co-precipitation reaction to obtain a ternary precursor; (2) Using the ternary precursor as a matrix, adding a carboxylic acid solution and a metal salt solution in parallel into a reaction container to carry out a coating reaction with the matrix, and obtaining the sodium positive electrode precursor after aging.

2. The preparation method according to claim 1, wherein The nickel source in step (1) comprises any one of nickel sulfate, nickel nitrate or nickel chloride, or a combination of at least two thereof; Optionally, the manganese source includes any one or a combination of at least two of manganese sulfate, manganese nitrate or manganese chloride; Optionally, the iron source includes any one of ferrous sulfate, ferrous nitrate or ferrous chloride, or a combination of at least two of them.

3. The preparation method according to claim 1 or 2, wherein: The concentration of the ternary salt solution is 2-4 mol / L.

4. The preparation method according to any one of claims 1 to 3, wherein The alkali solution in step (1) comprises any one of sodium hydroxide solution, sodium carbonate solution or potassium hydroxide solution or a combination of at least two thereof; Optionally, the concentration of the alkali solution is 2 to 4 mol / L; Optionally, the complexing agent includes aqueous ammonia; Optionally, the concentration of the ammonia water is 1 to 3 mol / L. Optionally, the base solution includes a complexing agent, an alkali solution and water; Optionally, the pH of the base solution is 10 to 12; Optionally, the concentration of the complexing agent in the base solution is 7 to 11 g / L.

5. The preparation method according to any one of claims 1 to 4, wherein: The flow rate of the ternary salt solution in step (1) is 30-60 kg / h; Optionally, the flow rate of the alkali solution is 3 to 8 kg / h; Optionally, the flow rate of the complexing agent is 10 to 20 kg / h; Optionally, the coprecipitation reaction temperature is 45 to 70°C; Optionally, the coprecipitation reaction time is 50 to 70 hours; Optionally, the stirring speed of the coprecipitation reaction is 120-400 rpm.

6. The preparation method according to any one of claims 1 to 5, wherein: The solute of the carboxylic acid solution in step (2) includes any one of 5-hydroxyisophthalic acid, trimesic acid or 1,2,4,5-benzenetetracarboxylic acid or a combination of at least two thereof; Optionally, the solvent of the carboxylic acid solution includes any one or a combination of at least two of N,N-dimethylformamide, N,N-diethylformamide, methanol, ethanol or propanol; Optionally, the concentration of the carboxylic acid solution is 1.8 to 2.2 mol / L; Optionally, the metal salt solution includes any one of an aluminum salt solution, a magnesium salt solution, a zirconium salt solution, a calcium salt solution, a titanium salt solution or a tungsten salt solution, or a combination of at least two thereof; Optionally, the concentration of the metal salt solution is 1 to 3 mol / L.

7. The preparation method according to any one of claims 1 to 6, wherein: The flow rate of the carboxylic acid solution in step (2) is 1 to 3 L / h; Optionally, the flow rate of the metal salt solution is 8 to 16 L / h.

8. The preparation method according to any one of claims 1 to 7, wherein: The pH of the coating reaction in step (2) is 7 to 8; Optionally, the coating reaction temperature is 50-65°C; Optionally, the coating reaction time is 2 to 8 hours; Optionally, the stirring speed of the coating reaction is 250-350 rpm; Optionally, the aging time is 2 to 5 hours.

9. A sodium-based positive electrode precursor, wherein the sodium-based positive electrode precursor is prepared by the method according to any one of claims 1 to 8, wherein the content of the coating metal in the sodium-based positive electrode precursor is 1000 to 10000 ppm.

10. A sodium positive electrode material, the sodium positive electrode material being obtained by sintering the sodium positive electrode precursor as claimed in claim 9 in one step, mixing it with a sodium source, and then sintering it in two steps; Optionally, the one-step sintering temperature is 400-600° C.; Optionally, the one-step sintering time is 3 to 6 hours; Optionally, the sodium source comprises sodium carbonate; Optionally, the temperature of the second-step sintering is 800-1200°C; Optionally, the two-step sintering time is 10 to 20 hours.

11. A sodium ion battery, comprising the sodium positive electrode material according to claim 10.

Citation Information

Patent Citations

  • MOF-coated single crystal ternary positive electrode material and preparation method of precursor of MOF-coated single crystal ternary positive electrode material

    CN111129463A

  • High-nickel ternary precursor with core-shell structure, preparation method of high-nickel ternary precursor, and hollow doped high-nickel ternary positive electrode material

    CN111525113A

  • Preparation method of nickel-aluminum coated nickel-iron-manganese sodium ion precursor material

    CN114291852A

  • Sodium battery positive electrode composite material and preparation method thereof

    CN115440955A

  • Nickel-manganese-iron-sodium ion battery positive electrode material precursor and preparation method thereof

    CN115991503A

Cited By

  • Method for preparing copper element doped nickel-iron-manganese precursor material and sodium battery positive electrode material thereof