Binder, negative electrode sheet, battery, and electric device

The 'spring mesh' adhesive obtained through cross-linking polymerization uses hydrogen bonds and covalent bonds to bind the silicon-based negative electrode material, solving the problem of battery performance degradation caused by expansion of the silicon-based negative electrode material, and significantly improving the cycling stability of the battery and service life.

WO2024239463A1PCT designated stage expired Publication Date: 2024-11-28CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/113602
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2023-08-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The volume expansion of the silicon-based negative electrode material during the cycle charging and discharge process is severe, resulting in loosening of the electrode structure and deteriorating the conductivity, reducing the cycling efficiency and service life of the battery. It is difficult for existing adhesives to effectively suppress this problem.

Method used

Using a 'spring mesh' adhesive obtained by cross-polymerization of the first polymer and the second polymer, the first polymer provides high strength and bonding properties, the second polymer has elasticity and self-healing ability, through hydrogen The bonds and covalent bonds form a cross-linked network structure, which binds the negative electrode material and inhibits expansion.

Benefits of technology

It significantly improves the cycle stability and service life of the battery, effectively suppresses the expansion of the negative electrode material, and improves the mechanical strength and conductive properties of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023113602_28112024_PF_FP_ABST
    Figure CN2023113602_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application discloses a binder, a negative electrode sheet, a battery, and an electric device. The binder comprises a copolymer of a first polymer and a second polymer. The structural formula of the first polymer is formula (1); the second polymer is a copolymer of a first monomer and a second monomer; the first monomer comprises at least one of urethane, a compound of which the structural formula is formula (2), tris(2-hydroxyethyl)isocyanurate triacrylate, and (2-hydroxyethyl)methacrylate; the second monomer comprises at least one of an ester obtained by dehydration of a compound of which the structural formula is formula (3) and alkenoic anhydride, 4-amino-catechol alkenate, dopamine hydrochloride alkenate, 1-aminocatechol alkenate, and 3,4-dihydroxyphenylalanine alkenate; the weight average molecular weight of the binder ranges from 200,000 to 3,000,000.
Need to check novelty before this filing date? Find Prior Art

Description

Binder, negative electrode sheet, battery and electrical device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the priority benefit of Chinese patent application No. 202310578399.0 filed on May 22, 2023, and incorporates the entirety of the application into this document. Technical Field

[0003] The present application relates to the field of battery technology, and in particular to a binder, a negative electrode sheet, a battery, and an electrical device. Background Art

[0004] Silicon-based anode materials have high capacity, but they experience significant volume expansion during cyclic charge and discharge, loosening the negative electrode structure and reducing battery conductivity. Furthermore, this process continuously damages the SEI (solid electrolyte interface) film on the negative electrode surface and consumes electrolyte, thereby reducing battery cycle efficiency and lifespan. However, current binders have a poor ability to inhibit the expansion of silicon-based materials, making it difficult to mitigate the technical issues associated with this expansion, such as reduced battery cycle performance and shortened lifespan.

[0005] Therefore, current binders, negative electrode sheets, batteries and electrical devices still need to be improved.

[0006] Summary of the Invention

[0007] In view of the above problems, the present application proposes a binder, a negative electrode plate, a battery and an electrical device, aiming to at least to some extent alleviate or even solve the technical problems such as poor battery cycle performance and short service life caused by the expansion of the negative electrode material.

[0008] In one aspect of the present application, a binder is provided. In some embodiments of the present application, the binder comprises a copolymer of a first polymer and a second polymer, wherein the first polymer has a structural formula of formula (1), and the second polymer is a copolymer of a first monomer and a second monomer, wherein the first monomer comprises at least one of urethane, a compound having a structural formula of formula (2), tris(2-hydroxyethyl)isocyanuric acid triacrylate, and (2-hydroxyethyl)methacrylate, and the second monomer comprises at least one of an ester obtained by dehydrating a compound having a structural formula of formula (3) and olefinic anhydride, 4-amino-catechol olefinic acid ester, dopamine hydrochloride olefinic acid ester, 1-aminocatechol olefinic acid ester, and 3,4-dihydroxyphenylalanine olefinic acid ester.

[0009] Wherein, X includes at least one of a hydroxyl group and a thiol group, and the number of carbon atoms in X is not greater than 3, Y includes at least one of a hydroxyl group and a thiol group, and the number of carbon atoms in Y is not greater than 3, Z includes at least one of an amino group and a thiol group, and the number of carbon atoms in Z is not greater than 3, and the weight average molecular weight of the binder is 200,000-3,000,000.

[0010] The binder has a three-dimensional network structure. The first polymer can provide sufficient adhesion and mechanical strength, and the second polymer has good elasticity and self-healing properties, so that the binder can at least to a certain extent inhibit the expansion of the negative electrode material, thereby improving the cycle performance of the battery and extending the service life of the battery. In addition, the binder has a suitable molecular weight. When the binder is added to the negative electrode slurry and left to stand for a period of time after stirring, it is not easy to agglomerate, and is suitable for large-scale production of batteries.

[0011] In some embodiments of the present application, the first polymer includes at least one of the following polymers:

[0012] In some embodiments of the present application, the first monomer includes at least one of the compounds of the following structural formulas:

[0013] In some embodiments of the present application, the second monomer comprises at least one of the esters obtained by dehydration of a compound of the following structural formula and an olefinic anhydride:

[0014] In some embodiments of the present application, the binder satisfies at least one of the following conditions: X is a hydroxyl group; the first monomer comprises 2-hydroxyethyl acrylate; the second monomer comprises at least one of 4-amino-catechol methacrylate, 4-amino-catechol crotonate, and 4-amino-catechol pentenoate; and the olefinic anhydride comprises at least one of methacrylic anhydride, crotonic anhydride, and 4-pentenoic anhydride. Thus, the binder can effectively inhibit the expansion of the negative electrode material, thereby improving the cycling performance of the battery.

[0015] In some embodiments of the present application, the weight average molecular weight of the binder is 1 million to 2 million. Thus, the weight average molecular weight of the binder is within a suitable range, which can more effectively inhibit the expansion of the negative electrode material, thereby improving the cycle performance and service life of the battery.

[0016] In some embodiments of the present application, X is a hydroxyl group, the first monomer is 2-hydroxyethyl acrylate, and the second monomer is 4-amino-catechol methacrylate.

[0017] In some embodiments of the present application, X is a hydroxyl group, the first monomer is tris(2-hydroxyethyl)isocyanurate triacrylate, and the second monomer is 4-amino-catechol methacrylate.

[0018] In some embodiments of the present application, X is a hydroxyl group, the first monomer is a compound of structural formula (2-6), and the second monomer is 4-amino-catechol methacrylate.

[0019] In some embodiments of the present application, X is a hydroxyl group, the first monomer is 2-hydroxyethyl acrylate, and the second monomer is 1-aminocatechol methacrylate.

[0020] In some embodiments of the present application, the structural formula of the first polymer is formula (1-6), the first monomer is 2-hydroxyethyl acrylate, and the second monomer is 4-amino-catechol methacrylate.

[0021] In another aspect of the present application, the present application proposes a negative electrode plate. In some embodiments of the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer, the negative electrode active material layer is located on at least one side surface of the negative electrode current collector, and the negative electrode active material layer includes: a negative electrode active material and the aforementioned binder, and the negative electrode active material includes a silicon-based material and graphite. Therefore, the negative electrode plate has all the characteristics and advantages of the binder described above, which will not be repeated here. In general, the negative electrode active material layer of the negative electrode plate has a high bonding strength with the negative electrode current collector, and the negative electrode plate has good cycle stability during the cyclic charge and discharge process.

[0022] In some embodiments of the present application, the negative electrode active material layer further includes at least one of a viscous material and a conductive agent. The addition of the viscous material can further improve the bonding strength between the negative electrode active material layer and the negative electrode current collector; the addition of the conductive agent can reduce the resistance of the battery.

[0023] In some embodiments of the present application, the negative electrode plate satisfies at least one of the following conditions: the silicon-based material includes at least one of pre-lithiated silicon oxide, silicon oxide and silicon carbon; the graphite includes at least one of natural graphite and artificial graphite; the viscous material includes at least one of styrene-butadiene rubber, polyamide-imide, polyvinyl alcohol, polyethylene imine, polyimide and poly(tert-butyl acrylate-triethoxyvinylsilane); the weight-average molecular weight of the viscous material is 40,000-2 million; the conductive agent includes at least one of carbon nanotubes, carbon black, carbon fiber and graphene; the negative electrode active material also includes at least one of hard carbon, soft carbon, Ketjen black, mesophase carbon microbeads, graphene and carbon fiber. The above-mentioned silicon-based materials have a higher capacity, which is beneficial to improving the capacity of the battery; artificial graphite and natural graphite have good cycle stability, which is beneficial to improving the cycle performance of the battery; the above-mentioned viscous material can further improve the bonding performance between the negative electrode active material layer and the negative electrode current collector, which is beneficial to reducing the risk of the negative electrode active material layer on the negative electrode current collector falling off; the molecular weight of the viscous material is between 40,000 and 2 million, which can further improve the bonding strength between the negative electrode current collector and the negative electrode active material layer; the above-mentioned conductive agent has good conductivity, and adding the above-mentioned conductive agent is beneficial to reducing the resistance of the battery; adding one or more materials such as hard carbon, soft carbon, Ketjen black, mesophase carbon microbeads, graphene and carbon fiber to the negative electrode active material can further improve the cycle stability or conductivity of the battery.

[0024] In some embodiments of the present application, based on the total mass of the negative electrode active material layer, the negative electrode active material layer includes: a silicon-based material having a mass content of 0.85 wt% to 59.82 wt%; graphite having a mass content of 34 wt% to 98.75 wt%; a conductive agent having a mass content of 0.1 wt% to 5 wt%; a binder having a mass content of 0.1 wt% to 5 wt%; and a viscous material having a mass content of 0.1 wt% to 5 wt%. The appropriate proportions of the components in the negative electrode active material layer further improve the overall performance of the negative electrode sheet.

[0025] In some embodiments of the present application, the negative electrode active material is composed of a silicon-based material and graphite, with the mass ratio of the silicon-based material to the graphite being 1:99 to 3:2. A silicon-based material to graphite mass ratio within this range can result in a battery having both excellent cycle stability and high capacity.

[0026] In another aspect of the present application, a battery is provided. In some embodiments of the present application, the battery comprises a positive electrode sheet, a negative electrode sheet, and an electrolyte, wherein the negative electrode sheet is the negative electrode sheet described above. Thus, the battery possesses all the features and advantages of the negative electrode sheet described above, which will not be further elaborated here. Overall, the battery has a high capacity and good cycling stability.

[0027] In another aspect of the present application, an electrical device is provided. In some embodiments of the present application, the electrical device includes the aforementioned battery. Thus, the electrical device has all the features and advantages of the aforementioned battery, which will not be further elaborated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0029] FIG1 shows a schematic structural diagram of a battery according to an embodiment of the present application;

[0030] Figure 2 shows an exploded view of the battery in Figure 1;

[0031] FIG3 shows a schematic structural diagram of a battery module according to an embodiment of the present application;

[0032] FIG4 shows a schematic structural diagram of a battery pack according to an embodiment of the present application;

[0033] FIG5 shows an exploded view of the battery pack in FIG4 ;

[0034] FIG6 shows a schematic structural diagram of an electrical device using a battery as a power source according to an embodiment of the present application.

[0035] Explanation of the reference numerals: 1: battery pack; 2: upper case; 3: lower case; 4: battery module; 5: battery; 51: housing; 52: electrode assembly; 53: cover plate. DETAILED DESCRIPTION

[0036] The following embodiments of the technical solution of the present application are described in detail. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only used as examples and are not intended to limit the scope of protection of the present application.

[0037] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0038] For the sake of clarity, only some numerical ranges are specifically disclosed herein. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.

[0039] In the description of this application, regardless of whether the word "about" or "approximately" is used, all numbers disclosed herein are approximate values. The value of each number may vary by less than 10% or by a reasonable difference considered by a person skilled in the art, such as 1%, 2%, 3%, 4% or 5%.

[0040] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.

[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0042] As one of the most promising anode materials for high-energy-density lithium-ion batteries, silicon-based anode materials offer high theoretical specific capacity and low redox electrode potential. However, silicon-based anode materials experience significant volume changes during cyclic charge and discharge, loosening the electrode structure and degrading the battery's conductivity. They also continuously damage the SEI film on the electrode surface and consume electrolyte, forming more and thicker SEI films, thereby reducing the battery's cycle efficiency and service life. Composite anodes made from silicon-based materials and graphite also suffer from technical issues such as reduced battery cycle stability and shortened service life due to the expansion of the anode material.

[0043] In order to at least alleviate or even solve at least one of the above-mentioned technical problems to a certain extent, a "spring net" binder can be added to the negative electrode. The binder is obtained by cross-linking and polymerization of two polymers, wherein the first polymer can provide higher strength and bonding properties, and the second polymer has certain elasticity and self-healing ability. The "spring net" binder contains a large number of hydrogen bonding sites such as amino, hydroxyl, and thiol groups, which can form hydrogen bonds with surrounding hydroxyl groups, carboxyl groups, amino groups, etc. The second polymer has certain elasticity and self-healing ability and can stretch and shrink during the cyclic charge and discharge process. Moreover, the second polymer itself carries catechol functional groups, and the two hydroxyl groups of the catechol functional groups can also dehydrate with silicon-based materials such as silicon oxide to form covalent bonds, thereby forming a cross-linked network structure. During the cyclic charge and discharge process, the "spring net" binder can restrain the negative electrode material and improve the expansion problem of the negative electrode material, thereby alleviating technical problems such as decreased battery cycle stability and shortened service life caused by the expansion of the negative electrode material.

[0044] The "spring mesh" binder can be used as a binder for lithium-ion battery negative electrode materials. For example, it can be applied to a composite negative electrode material system comprising pre-lithiated silicon oxide and graphite, a composite negative electrode material system comprising silicon oxide and graphite, a composite negative electrode material system comprising silicon carbon and graphite, etc.

[0045] Lithium-ion batteries with the "spring net" binder added to the battery negative electrode material system can be used in electrical devices that use batteries as power sources or various energy storage systems that use batteries as energy storage elements. Electrical devices may include, but are not limited to, mobile phones, tablets, laptops, electric toys, power tools, battery-powered vehicles, electric vehicles, ships, spacecraft, and the like. Electric toys may include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, and spacecraft may include airplanes, rockets, space shuttles, and spacecraft, and the like.

[0046] In one aspect of the present application, the present application proposes a binder. In some embodiments of the present application, the binder may include a copolymer of a first polymer and a second polymer. The structural formula of the first polymer may be formula (1), the second polymer may be a copolymer of a first monomer and a second monomer, the first monomer may include at least one of urethane, a compound having the structural formula (2), tris(2-hydroxyethyl)isocyanuric acid triacrylate and (2-hydroxyethyl)methacrylate, etc., and the second monomer may include at least one of an ester obtained by dehydrating a compound having the structural formula (3) and an olefinic anhydride, 4-amino-catechol olefinate (an ester obtained by dehydrating 4-amino-1,2-catechol hydrochloride and an olefinic anhydride), dopamine hydrochloride olefinate (an ester obtained by dehydrating dopamine hydrochloride and an olefinic anhydride), 1-aminocatechol olefinate (an ester obtained by dehydrating aminocatechol and an olefinic anhydride), 3,4-dihydroxyphenylalanine olefinate (an ester obtained by dehydrating dopa(3,4-dihydroxyphenylalanine) and an olefinic anhydride), etc.

[0047] In formula (1), X may include at least one of a hydroxyl group, a thiol group, etc., and the number of carbon atoms in X is not greater than 3. For example, the number of carbon atoms in X may be 0, 1, 2, or 3, and n is the degree of polymerization. In some specific embodiments of the present application, formula (1) may be the following structural formula:

[0048] X includes at least one of a hydroxyl group and a thiol group. These groups can form hydrogen bonds with carboxyl, hydroxyl, and amino groups in external materials, promoting the formation of a three-dimensional network structure. Furthermore, the thiol group can form an inorganic lithium salt (e.g., lithium sulfide) with good lithium conductivity, thereby improving the lithium conductivity of the negative electrode. The number of carbon atoms in X is no greater than 3, and X can rotate through a large angle, thereby enhancing the flexibility of the binder.

[0049] In formula (2), Y may include at least one of a hydroxyl group, a thiol group, etc., and the number of carbon atoms in Y is not greater than 3. For example, the number of carbon atoms in Y may be 0, 1, 2, or 3. In some specific embodiments of the present application, formula (2) may be the following structural formula:

[0050] Y includes at least one of a hydroxyl group and a thiol group. These groups contain hydrogen and possess lone pairs of electrons, which can form hydrogen bonds with carboxyl, hydroxyl, and amino groups in external materials, promoting the formation of a three-dimensional network structure. Furthermore, thiol groups can form inorganic lithium salts such as lithium sulfide, which have good lithium conductivity, thereby enhancing the lithium conductivity of the negative electrode. The number of carbon atoms in Y is no greater than 3, and Y can rotate through a large angle, thereby improving the flexibility of the binder.

[0051] In formula (3), Z may include at least one of an amino group, a thiol group, etc., and the number of carbon atoms in Z is not greater than 3. For example, the number of carbon atoms in Z may be 0, 1, 2, or 3. In some specific embodiments of the present application, formula (3) may be the following structural formula:

[0052] Z includes at least one of an amino group and a thiol group. These groups can form hydrogen bonds with carboxyl, hydroxyl, and amino groups in the external material, promoting the formation of a three-dimensional network structure. The thiol group can form an inorganic lithium salt (such as lithium sulfide) with good lithium conductivity, thereby improving the lithium conductivity of the negative electrode. The number of carbon atoms in Z is no more than 3, allowing for wide rotation and resisting breakage.

[0053] Herein, the copolymer of the first polymer and the second polymer refers to a polymer obtained by cross-linking and polymerization of the first polymer and the second polymer. The copolymer of the first monomer and the second monomer refers to a polymer obtained by copolymerization of the first monomer and the second monomer.

[0054] In some embodiments of the present application, the weight-average molecular weight of the binder can be 200,000-3,000,000. For example, the weight-average molecular weight of the binder can be 200,000, 500,000, 700,000, 1,000,000, 1,500,000, 1,700,000, 2,000,000, 2,600,000, 3,000,000, etc. The binder has a suitable weight-average molecular weight, can provide good bonding properties, and is not easy to agglomerate during the preparation of the negative electrode slurry. After stirring, the negative electrode slurry can be left for 24 hours or even longer without agglomeration, which is conducive to the large-scale production of negative electrode sheets or batteries. The weight-average molecular weight of the binder can be adjusted by controlling the reaction time, reaction temperature, the ratio of the reaction raw materials, etc. The first polymer serves as the main body of the binder. The higher its content, the greater the weight-average molecular weight of the binder. When the weight-average molecular weight is too large, the binding force of the binder is very strong, and agglomeration will occur when stirring the slurry (here refers to stirring the negative electrode slurry). The negative electrode slurry sticks together, the fluidity is very poor, and there is no way to form an electrode sheet; if the weight-average molecular weight is too small, the binder cannot provide sufficient bonding strength, and the bonding force between the binder and the negative electrode active material and the negative electrode current collector is relatively weak. During the cyclic charge and discharge process, the negative electrode active material layer is easy to fall off from the negative electrode current collector, resulting in a decrease in the battery cycle stability.

[0055] It should be noted that the negative electrode slurry is a slurry obtained by dispersing the negative electrode active material, binder, conductive agent, etc. in a dispersant such as water. The negative electrode slurry is coated on at least one side of the negative electrode collector and dried to form a negative electrode active material layer on the surface of the negative electrode collector.

[0056] Herein, the olefinic anhydride has a carbon-carbon double bond and an acid anhydride group.

[0057] In some embodiments of the present application, the olefinic anhydride may include at least one of methacrylic anhydride, crotonic anhydride, and 4-pentenoic anhydride. Methacrylic anhydride has the structural formula of Formula (4), crotonic anhydride has the structural formula of Formula (5), and 4-pentenoic anhydride has the structural formula of Formula (6).

[0058] In some embodiments of the present application, the olefinic anhydride may include methacrylic anhydride, and the second monomer may include at least one of an ester obtained by dehydrating a compound having the structural formula (3) and methacrylic anhydride, 4-amino-catechol methacrylate (an ester obtained by dehydrating 4-amino-1,2-catechol hydrochloride and methacrylic anhydride), dopamine hydrochloride methacrylate (an ester obtained by dehydrating dopamine hydrochloride and methacrylic anhydride), 1-aminocatechol methacrylate (an ester obtained by dehydrating aminocatechol and methacrylic anhydride), 3,4-dihydroxyphenylalanine methacrylate (an ester obtained by dehydrating dopamine (3,4-dihydroxyphenylalanine) and methacrylic anhydride), and the like.

[0059] In some embodiments of the present application, the olefinic anhydride may include crotonic anhydride, and the second monomer may include at least one of an ester obtained by dehydrating a compound having the structural formula (3) and crotonic anhydride, 4-amino-catechol crotonic ester (an ester obtained by dehydrating 4-amino-1,2-catechol hydrochloride and crotonic anhydride), dopamine hydrochloride crotonic ester (an ester obtained by dehydrating dopamine hydrochloride and crotonic anhydride), 1-aminocatechol crotonic ester (an ester obtained by dehydrating aminocatechol and crotonic anhydride), 3,4-dihydroxyphenylalanine crotonic ester (an ester obtained by dehydrating dopa (3,4-dihydroxyphenylalanine) and crotonic anhydride), etc.

[0060] In some embodiments of the present application, the enoic anhydride may include 4-pentenoic anhydride, and the second monomer may include at least one of an ester obtained by dehydration of a compound having the structural formula (3) and 4-pentenoic anhydride, 4-amino-catechol pentenoate (an ester obtained by dehydration of 4-amino-1,2-catechol hydrochloride and 4-pentenoic anhydride), dopamine hydrochloride pentenoate (an ester obtained by dehydration of dopamine hydrochloride and 4-pentenoic anhydride), 1-aminocatechol pentenoate (an ester obtained by dehydration of aminocatechol and 4-pentenoic anhydride), 3,4-dihydroxyphenylalanine pentenoate (an ester obtained by dehydration of dopa (3,4-dihydroxyphenylalanine) and 4-pentenoic anhydride), etc.

[0061] The first polymer alone has certain bonding properties and can provide a strong bonding effect for the negative electrode active material layer and the negative electrode current collector, but its flexibility is poor, its side chains are difficult to rotate at a large angle, and the inhibitory effect on the expansion of the negative electrode material is poor; the second polymer alone has insufficient bonding force to the negative electrode active material layer and the negative electrode current collector, and is highly swollen in the electrolyte, which has an adverse effect on the cycle stability of the battery. The binder proposed in the present application includes a copolymer of a first polymer and a second polymer. The part corresponding to the first polymer serves as the main body of the binder, which can provide higher mechanical strength and better bonding performance. The part corresponding to the second polymer has certain elasticity and self-healing properties, and can be stretched and contracted during the charging and discharging process. The binder is obtained by cross-linking and polymerization of the first polymer and the second polymer, has high mechanical strength, and can prevent flow and creep. At the same time, the binder has a large number of repetitive hydrogen bonds and catechol functional groups in each local area, which can produce self-healing ability and enhance the microscopic stability of the three-dimensional network structure. The binder of the three-dimensional network structure has certain shrinkage properties and can effectively restrain the expanded negative electrode active material. The binder has excellent self-healing properties, can maintain good stability, and is not prone to bond breaking due to mechanical fatigue, thereby effectively inhibiting the volume expansion of the negative electrode active material, thereby significantly improving the cycle performance of the battery and extending the battery life.

[0062] In some embodiments of the present application, the weight-average molecular weight of the binder may be 1 million to 2 million. For example, the weight-average molecular weight of the binder may be 1 million, 1.2 million, 1.4 million, 1.5 million, 1.8 million, 2 million, etc. When the weight-average molecular weight of the binder is within the above range, the binder can provide sufficient bonding strength between the negative electrode active material and the negative electrode current collector, and the negative electrode slurry can remain uniformly dispersed for a long time after stirring; moreover, when the weight-average molecular weight of the binder is within the above range, it can provide a stronger bonding force between the negative electrode active material layer and the negative electrode current collector, and the negative electrode slurry can remain uniformly dispersed for a long time after stirring; moreover, during the charge and discharge cycle, the binder can effectively inhibit the expansion of the negative electrode active material, so that the battery has excellent cycle stability and a longer service life.

[0063] In some embodiments of the present application, X may be a hydroxyl group, as shown in formula (1-1). In this case, the first polymer is polyacrylic acid (PAA). Polyacrylic acid has high strength and adhesive properties, and cross-linking with the second polymer can significantly improve the mechanical strength and adhesive properties of the adhesive.

[0064] In some embodiments of the present application, the first monomer may include 2-hydroxyethyl acrylate, as shown in formula (2-1). The polymer of 2-hydroxyethyl acrylate has good elasticity, and the hydroxyl groups contained in 2-hydroxyethyl acrylate can provide hydrogen bonding sites, which is conducive to forming a three-dimensional network structure adhesive with a certain elasticity.

[0065] In some embodiments of the present application, the second monomer may include an ester obtained by dehydrating 4-amino-1,2-catechol hydrochloride and an olefinic anhydride, for example, 4-amino-catechol methacrylate (an ester obtained by dehydrating 4-amino-1,2-catechol hydrochloride and methacrylic anhydride), 4-amino-catechol crotonate (an ester obtained by dehydrating 4-amino-1,2-catechol hydrochloride and crotonic anhydride), and 4-amino-catechol pentenoate (an ester obtained by dehydrating 4-amino-1,2-catechol hydrochloride and 4-pentenoic anhydride). The second monomer contains a catechol functional group, which has a certain degree of elasticity. In addition, the two hydroxyl groups of the functional group can form a covalent bond with the negative electrode active material by dehydration, and can also form hydrogen bonds with surrounding hydroxyl groups, amino groups, etc., to form a cross-linked network structure, thereby inhibiting the expansion of the negative electrode active material.

[0066] In some embodiments of the present application, X may be a hydroxyl group, the first monomer may be 2-hydroxyethyl acrylate, and the second monomer may be 4-amino-catechol methacrylate.

[0067] In some embodiments of the present application, X can be a hydroxyl group, the first monomer can be 2-hydroxyethyl acrylate, the second monomer can be 4-amino-catechol methacrylate, and the weight-average molecular weight of the binder is 1.7 million. It can not only provide a strong bonding effect between the negative electrode active material layer and the negative electrode current collector, but also maintain a high mechanical strength, effectively inhibit the expansion of the negative electrode active material during the cyclic charge and discharge process, so as to avoid the battery capacity "diving", and can also enable the battery to maintain good dynamic performance, so that the battery has excellent cycle stability and a long service life.

[0068] In some embodiments of the present application, X may be a hydroxyl group, the first monomer may be 2-hydroxyethyl acrylate, the second monomer may be 4-amino-catechol methacrylate, and the molar ratio of X, Y, and Z in the binder is 32:8:1. Thus, the binder has a weight-average molecular weight of approximately 1.7 million, which provides a strong bond between the negative electrode active material layer and the negative electrode current collector while maintaining high mechanical strength and effectively suppressing the expansion of the negative electrode active material during cyclic charge and discharge, thereby providing the battery with excellent cycle stability and a long service life.

[0069] In some specific embodiments of the present application, X may be a hydroxyl group, the first monomer may be tris(2-hydroxyethyl)isocyanurate triacrylate, and the second monomer may be 4-amino-catechol methacrylate.

[0070] In some specific embodiments of the present application, X may be a hydroxyl group, the first monomer may be a compound of structural formula (2-6), and the second monomer may be 4-amino-catechol methacrylate.

[0071] In some specific embodiments of the present application, X may be a hydroxyl group, the first monomer may be 2-hydroxyethyl acrylate, and the second monomer may be 1-aminocatechol methacrylate.

[0072] In some specific embodiments of the present application, the structural formula of the first polymer may be formula (1-6), the first monomer may be 2-hydroxyethyl acrylate, and the second monomer may be 4-amino-catechol methacrylate.

[0073] The use of the above materials to form a binder with a suitable molecular weight can effectively inhibit the expansion of the negative electrode active material during the charge and discharge process, thereby improving the cycle performance of the battery.

[0074] In another aspect of the present application, a negative electrode sheet is provided. In some embodiments of the present application, the negative electrode sheet may include a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer is located on at least one surface of the negative electrode current collector. The negative electrode active material layer may include a negative electrode active material and the aforementioned binder. The negative electrode active material may include a silicon-based material and graphite. Thus, the negative electrode active material can combine the high capacity of the silicon-based material with the good cycle stability and excellent conductivity of graphite.

[0075] The negative electrode active material layer in the negative electrode sheet includes the negative electrode active material and the aforementioned binder. As a result, the negative electrode sheet possesses all the characteristics and advantages of the aforementioned binder, which will not be elaborated upon here. In general, the negative electrode active material layer in the negative electrode sheet has a high bond strength with the negative electrode current collector. When this negative electrode sheet is used in a battery, the binder can effectively inhibit the expansion of the silicon-based material during cyclic charge and discharge, thereby significantly improving the battery's cycling stability.

[0076] In some embodiments of the present application, the graphite may include at least one of natural graphite and artificial graphite. For example, the graphite may be natural graphite, artificial graphite, or a mixture of natural graphite and artificial graphite. Both natural graphite and artificial graphite have good stability and excellent conductivity. Adding graphite to the negative electrode active material can help improve the conductivity and stability of the negative electrode active material layer.

[0077] In some embodiments of the present application, the silicon-based material may include at least one of pre-lithiated silicon oxide, silicon oxide, and silicon carbon. All of these silicon-based materials have high specific capacities, and adding silicon-based materials to the negative electrode active material can help increase the capacity of the battery. In some embodiments of the present application, the silicon-based material may be pre-lithiated silicon oxide, silicon oxide, or silicon carbon; in other embodiments of the present application, the silicon-based material may be a mixture of two or three of pre-lithiated silicon oxide, silicon oxide, and silicon carbon.

[0078] In some embodiments of the present application, in addition to silicon-based materials and graphite, the negative electrode active material may also include at least one of hard carbon, soft carbon, Ketjen black, mesophase carbon microbeads, graphene and carbon fiber, etc. Adding at least one of the above materials to the negative electrode active material can improve the capacity, conductivity and / or cycle stability of the negative electrode to a certain extent.

[0079] In some embodiments of the present application, in addition to silicon-based materials and graphite, the negative electrode active material may further include hard carbon, soft carbon, Ketjen black, mesophase carbon microbeads, graphene, or carbon fiber. In other embodiments of the present application, in addition to silicon-based materials and graphite, the negative electrode active material may further include two or more of hard carbon, soft carbon, Ketjen black, mesophase carbon microbeads, graphene, and carbon fiber.

[0080] In some embodiments of the present application, the negative electrode active material layer may further include at least one of a viscous material and a conductive agent. According to some embodiments of the present application, the negative electrode active material layer may further include a viscous material or a conductive agent; in other embodiments of the present application, the negative electrode active material layer may further include a viscous material and a conductive agent.

[0081] The adhesive material can further enhance the bonding strength between the negative electrode active material layer and the negative electrode current collector, thereby further improving the stability of the negative electrode sheet. The conductive agent can further enhance the conductivity of the negative electrode active material layer, thereby further reducing the resistance of the battery.

[0082] In some embodiments of the present application, the viscous material may include at least one of styrene-butadiene rubber (SBR), polyamide-imide (PAI), polyvinyl alcohol (PVA), polyethylene imine (PEI), polyimide (PI), and poly(tert-butyl acrylate-triethoxyvinylsilane) (TBATEVS). In some embodiments of the present application, the viscous material may be composed of one of the above materials; in other embodiments of the present application, the viscous material may be composed of two or more of the above materials.

[0083] In some embodiments of the present application, the adhesive material may include styrene-butadiene rubber, which can provide a stronger adhesive force for graphite and the negative electrode current collector (eg, copper foil).

[0084] The above-mentioned viscous material has good bonding properties and can form a strong bonding effect between the graphite and the negative electrode current collector, thereby further improving the bonding strength between the negative electrode active material layer and the negative electrode current collector.

[0085] In some embodiments of the present application, the weight average molecular weight of the viscous material can be 40,000-2 million. For example, the weight average molecular weight of the viscous material can be 40,000, 100,000, 300,000, 500,000, 800,000, 1 million, 1.2 million, 1.5 million, 1.7 million, 2 million, etc.

[0086] When the weight average molecular weight of the viscous material is within the above range, a stronger bonding effect can be formed between the graphite and the negative electrode current collector, thereby further improving the structural stability of the negative electrode sheet.

[0087] In some embodiments of the present application, the conductive agent may include at least one of carbon nanotubes, carbon black, carbon fibers, and graphene. In some embodiments of the present application, the conductive agent may be carbon nanotubes, carbon black, carbon fibers, or graphene. In other embodiments of the present application, the conductive agent may be a mixture of two or more of carbon nanotubes, carbon black, carbon fibers, and graphene.

[0088] The above conductive agents all have good conductivity. Adding the above conductive agents to the negative electrode active material layer can improve the conductivity of the negative electrode active material layer.

[0089] In some embodiments of the present application, based on the total mass of the negative electrode active material layer, the negative electrode active material layer may include: a silicon-based material with a mass content of 0.85wt% to 59.82wt%; a graphite with a mass content of 34wt% to 98.75wt%; a conductive agent with a mass content of 0.1wt% to 5wt%; a binder with a mass content of 0.1wt% to 5wt%; and a viscous material with a mass content of 0.1wt% to 5wt%.

[0090] In some embodiments of the present application, based on the total mass of the negative electrode active material layer, the negative electrode active material layer may include: a silicon-based material with a mass content of 0.85wt%, 1wt%, 5wt%, 10wt%, 15wt%, 20wt%, 40wt%, 50wt% or 59.82wt%; a graphite with a mass content of 34wt%, 36wt%, 40wt%, 50wt%, 60wt%, 70wt%, 80wt%, 90wt% or 98.75wt%; a conductive agent with a mass content of 0.1wt%, 0.5wt%, 1wt%, 3wt% or 5wt%; a binder with a mass content of 0.1wt%, 0.5wt%, 1.5wt%, 4wt% or 5wt%; and a viscous material with a mass content of 0.1wt%, 0.3wt%, 0.5wt%, 2wt% or 5wt%.

[0091] The appropriate content of each component in the negative electrode active material layer is beneficial to increasing the capacity of the battery, reducing the resistance of the battery, and further improving the cycle stability of the battery.

[0092] In some embodiments of the present application, the negative electrode active material is composed of a silicon-based material and graphite, wherein the mass ratio of the silicon-based material to the graphite is 1:99 to 3:2. For example, the mass ratio of the silicon-based material to the graphite can be 1:99, 1:19, 1:9, 3:17, 1:4, 1:2, 1:1, 3:2, etc. Therefore, when the mass ratio of the silicon-based material to the graphite in the negative electrode active material is within the above range, the negative active material layer can have a high capacity, good conductivity, and good cycle stability.

[0093] In some embodiments of the present application, the negative electrode current collector may be copper foil.

[0094] In some embodiments of the present application, a negative electrode active material layer can be formed on one or both surfaces of the negative electrode current collector by coating a negative electrode slurry on the negative electrode current collector and drying the negative electrode slurry.

[0095] In another aspect, the present application provides a battery. In some embodiments of the present application, the battery may include a positive electrode sheet, a negative electrode sheet, and an electrolyte, wherein the negative electrode sheet may be the negative electrode sheet described above. Thus, the battery has good cycle stability and a long service life.

[0096] A battery is a battery that can be recharged to activate the active materials after discharge and continue to be used.

[0097] In some embodiments of the present application, the battery may be a lithium-ion battery.

[0098] In some embodiments of the present application, the battery includes a positive electrode sheet, a negative electrode sheet and an electrolyte. During the charging and discharging process of the battery, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet, and the electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet.

[0099] In some embodiments of the present application, the electrolyte may be a solid electrolyte, a gel electrolyte, or an electrolyte solution.

[0100] Typically, when the electrolyte is an electrolyte solution, the battery may further include a separator, which is disposed between the positive electrode sheet and the negative electrode sheet to separate the positive electrode sheet from the negative electrode sheet.

[0101] In some embodiments of the present application, the isolation membrane may include but is not limited to a polyethylene porous film, a polypropylene porous film, a polypropylene-polyethylene copolymer porous film, and the like.

[0102] In some embodiments of the present application, the electrolyte may include an organic solvent and a lithium salt. The organic solvent may include but is not limited to ethylene carbonate (EC), ethyl methyl carbonate (EMC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), etc., and the lithium salt may include but is not limited to lithium hexafluorophosphate, etc.

[0103] In some embodiments of the present application, the positive electrode sheet may include a positive electrode current collector and a positive electrode active material layer, and the positive electrode active material layer is located on at least one side surface of the positive electrode current collector.

[0104] In some embodiments of the present application, the positive electrode current collector may be aluminum foil.

[0105] In some embodiments of the present application, the positive electrode active material layer may include a positive electrode active material, a positive electrode binder, a positive electrode conductive agent, etc. In some embodiments of the present application, the positive electrode active material may include one or more of lithium iron phosphate, nickel-cobalt-manganese ternary material, lithium cobaltate, lithium manganate, lithium nickelate, lithium vanadate, etc. In some embodiments of the present application, the positive electrode binder may include one or more of styrene-butadiene rubber, polyamide-imide, polyvinyl alcohol, polyethyleneimine, polyimide, and poly(tert-butyl acrylate-triethoxyvinylsilane). In some embodiments of the present application, the positive electrode conductive agent may include one or more of carbon nanotubes, carbon black, carbon fiber, and graphene.

[0106] In some embodiments of the present application, the battery may be cylindrical, square (a battery 5 with a square structure is shown in FIG1 ) or any other shape.

[0107] In some embodiments, the battery may include an outer packaging. This outer packaging is used to encapsulate the positive electrode sheet, the negative electrode sheet, and the electrolyte. Specifically, referring to Figure 2 , the outer packaging of the battery 5 may include a housing 51 and a cover plate 53 . The housing 51 may include a bottom plate and side plates connected to the bottom plate, which together form a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 may be positioned over the opening to seal the receiving cavity.

[0108] As an example, the positive electrode sheet, the negative electrode sheet, and the separator can be wound or laminated to form an electrode assembly 52. ​​The electrode assembly 52 is encapsulated in a housing cavity, and the electrolyte fills the interior space of the electrode assembly 52. ​​The battery 5 can contain one or more electrode assemblies 52, and those skilled in the art can select the number based on specific practical needs.

[0109] In some embodiments, the outer packaging of the battery may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell.

[0110] In other embodiments, the outer packaging of the battery may also be a soft bag, such as a bag-type soft bag. The material of the soft bag may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0111] As an example, batteries can be assembled into battery modules, and the number of batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module. Figure 3 is a battery module 4 as an example. Referring to Figure 3, in the battery module 4, multiple batteries 5 can be arranged in sequence along the length direction of the battery module 4. Of course, they can also be arranged in any other manner. The multiple batteries 5 can further be fixed by fasteners. The battery module 4 can also include a shell having a storage space, and the multiple batteries 5 are accommodated in the storage space.

[0112] As an example, the above-mentioned battery modules can also be assembled into a battery pack. The number of battery modules contained in the battery pack can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery pack. Figures 4 and 5 are a battery pack 1 as an example. Referring to Figures 4 and 5, the battery pack 1 may include a battery box and a plurality of battery modules 4 arranged in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can be covered on the lower box body 3 to form a closed space for accommodating the battery module 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0113] In another aspect of the present application, an electrical device is provided. In some embodiments of the present application, the electrical device includes the aforementioned battery. Thus, the electrical device has all the features and advantages of the aforementioned battery, which will not be further elaborated here.

[0114] In some embodiments of the present application, the electrical device may include at least one of a battery, a battery module, and a battery pack. The battery, battery module, or battery pack may serve as a power source for the electrical device, or may serve as an energy storage unit for the electrical device. The electrical device may be a mobile device (e.g., a mobile phone, a laptop computer), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck), an electric train, a ship, a satellite, or an energy storage system, but is not limited thereto.

[0115] The electrical device can select batteries, battery modules or battery packs according to its usage requirements.

[0116] As an example, a power-consuming device can be a vehicle, as shown in Figure 6. This power-consuming device includes a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the power-consuming device's requirements for high power and high energy density, a battery pack or battery module can be used.

[0117] As another example, electric devices may include mobile phones, tablet computers, and laptop computers. These electric devices are generally required to be lightweight and thin, and may use batteries as power sources.

[0118] The present application will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are merely for illustrative purposes and are not intended to limit the scope of the present application in any way. In addition, in the following examples, unless otherwise specified, the materials and equipment employed are all commercially available. If, in the following examples, specific processing conditions and treatment methods are not clearly described, then conditions and methods well known in the art may be used to process.

[0119] Example 1

[0120] [Preparation of Second Monomer]

[0121] Sodium tetraborate (Na2B4O7, 10g) and sodium bicarbonate (NaHCO3, 4g) were dissolved in 100mL of deionized water and purged with argon for 20 minutes to remove oxygen from the solution. To a solution containing 4-amino-1,2-catechol hydrochloride (10g, 29.1mmol) and 25mL of tetrahydrofuran, 4.7mL of methacrylic anhydride (4.5g, 29.1mmol) was slowly added dropwise. During this time, the pH of the solution was adjusted to above 8 by continuous addition of 1M NaOH solution. The reaction system was stirred at room temperature overnight and purged with Ar (argon) to protect the reaction system. The aqueous solution was washed twice with 50mL of ethyl acetate, at which point the pH dropped below 2, and then extracted three times with 50mL of ethyl acetate. The resulting ethyl acetate solutions were combined, dried over anhydrous magnesium sulfate (MgSO4), and concentrated to approximately 30 mL using a rotary evaporator. After vigorous stirring, 250 mL of n-hexane was added to obtain a suspension. The suspension was allowed to stand overnight at 40°C and filtered to obtain a gray powder. This powder was recrystallized from n-hexane and dried to obtain 4.0 g of a gray product, 4-amino-catechol methacrylate, the second monomer.

[0122] [Preparation of Second Polymer]

[0123] Purified 2-hydroxyethyl acrylate (5.22 g, 43.1 mmol), 4-amino-catechol methacrylate (0.66 g, 2.87 mmol), azobisisobutyronitrile (AIBN) (76 mg, 0.46 mmol), and 20 mL of N,N-dimethylformamide (DMF) solvent were added sequentially to a sealed tube to obtain a solution. The solution was subjected to vacuum rotary evaporation three times, then sealed under vacuum, heated to 60°C, and stirred overnight. After the reaction was completed, the reaction mixture was diluted with 50 mL of methanol, precipitated in 400 mL of diethyl ether, and filtered. The product was then washed and precipitated twice in a dichloroethane / diethyl ether mixture and vacuum dried to obtain 3.5 g of a white, viscous solid, the second polymer, a copolymer of 2-hydroxyethyl acrylate and 4-amino-catechol methacrylate.

[0124] [Preparation of binder]

[0125] The first polymer is commercially available polyacrylic acid (PAA), and PAA and the second polymer are mixed in a mass ratio of 4:1. Thereafter, the mixture is heated, dehydrated, and polycondensed to obtain the adhesive.

[0126] Testing method for weight average molecular weight of binder: Use gel permeation chromatography to test weight average molecular weight of binder, and use tetrahydrofuran or N,N-dimethylformamide to dissolve binder.

[0127] The weight average molecular weight of the binder in Example 1 is 1,000,000.

[0128] [Preparation of positive electrode sheet]

[0129] Cathode active material lithium nickel cobalt manganese oxide (NCM523 LiNi 0.5 Co 0.2 Mn 0.3 O2), binder polyvinylidene fluoride PVDF, conductive agent Super P were mixed in a mass ratio of 98:1:1, N-methylpyrrolidone (NMP) was added as a dispersant, and stirred in a vacuum state until uniform to obtain a slurry. The obtained slurry was heated at 13.7 mg / cm 2 The surface density was coated on a 13 μm thick aluminum foil with a doctor blade, and then dried at 140° C., cold pressed, and cut to obtain the positive electrode sheet of Example 1.

[0130] [Preparation of negative electrode sheet]

[0131] Pre-lithiated silicon oxide, artificial graphite, conductive agent acetylene black, binder prepared in Example 1, and SBR were dispersed in deionized water as a dispersant in a mass ratio of 14.55:82.45:1:1:1, stirred, and mixed to obtain a negative electrode slurry. The negative electrode slurry was heated to 9.7 mg / cm 2The surface density is evenly coated on the 7μm thick negative electrode current collector copper foil, and the negative electrode sheet is obtained after drying, cold pressing and slitting. Among them, the Dv50 of pre-lithiated silicon oxide is 3μm-20μm, and its composition includes lithium metasilicate. In the particles of pre-lithiated silicon oxide, pure silicon grains are mixed with silicon dioxide and lithium metasilicate, and the outer side is wrapped with a carbon layer. The diameter of the pure silicon grains is 1nm~20nm (the diameter of the pure silicon grains is obtained by XRD testing); the Dv50 of artificial graphite is 5μm~20μm, and the specific surface area is 0.5m 2 / g~4m 2 / g.

[0132] [Electrolyte]

[0133] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), the organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 3:7, and 12.5wt% (based on the total mass of ethylene carbonate and ethyl methyl carbonate solvents) of LiPF6 was added to the mixed solvent and stirred evenly to dissolve LiPF6 in the above organic solvent to obtain an electrolyte.

[0134] [Isolation film]

[0135] The separator used was a commercially available PP-PE copolymer microporous film (from Zhuogao Electronic Technology Co., Ltd., Model 20) with a thickness of 7 μm and an average pore size of 80 nm.

[0136] [Preparation of lithium-ion batteries]

[0137] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator positioned between the positive and negative electrodes to isolate them. The sheets are then wound to form a bare cell. The bare cell is then placed in an outer packaging, injected with the aforementioned electrolyte, and packaged to form a lithium-ion battery.

[0138] Example 2

[0139] The difference from Example 1 is that the weight average molecular weight of the binder is 1.7 million. The remaining parameters and steps are the same as those in Example 1.

[0140] Example 3

[0141] The difference from Example 1 is that the weight average molecular weight of the binder is 2,000,000. The remaining parameters and steps are the same as those in Example 1.

[0142] Example 4

[0143] The difference from Example 1 is that the weight average molecular weight of the binder is 3,000,000. The remaining parameters and steps are the same as those in Example 1.

[0144] Example 5

[0145] Unlike Example 2, when preparing the negative electrode sheet, pre-lithiated silicon oxide, artificial graphite, conductive agent acetylene black, binder, and SBR were dispersed in deionized water as a dispersant at a mass ratio of 4.85:92.15:1:1:1 and mixed evenly to obtain a negative electrode slurry. The remaining parameters and steps were the same as in Example 2.

[0146] Example 6

[0147] Different from Example 5, when preparing the negative electrode sheet, silicon oxide, artificial graphite, conductive agent acetylene black, binder, and SBR are dispersed in deionized water as a dispersant in a mass ratio of 4.85:92.15:1:1:1, and mixed evenly to obtain a negative electrode slurry. Among them, the Dv50 of silicon oxide is 1 μm to 12 μm, and the specific surface area is 0.5 m 2 / g~8m 2 / g, in the silicon-oxygen particles, pure silicon grains are mixed with silicon dioxide and coated with carbon on the outside, and the diameter of the pure silicon grains is 1nm to 20nm. The remaining parameters and steps are the same as those in Example 5.

[0148] Example 7

[0149] Different from Example 5, when preparing the negative electrode sheet, silicon carbon, artificial graphite, conductive agent acetylene black, binder, and SBR are dispersed in deionized water as a dispersant in a mass ratio of 4.85:92.15:1:1:1, and mixed evenly to obtain a negative electrode slurry. Among them, the Dv50 of silicon carbon is 3μm to 15μm, and the specific surface area is 1m 2 / g~12m 2 The remaining parameters and steps are the same as those in Example 5.

[0150] Example 8

[0151] The difference from Example 1 is that the weight average molecular weight of the prepared binder is 200,000. The remaining parameters and steps are the same as those in Example 1.

[0152] Example 9

[0153] Unlike Example 2, when preparing the negative electrode sheet, silica, artificial graphite, conductive agent acetylene black, binder, and SBR were dispersed in deionized water (dispersant) at a mass ratio of 14.55:82.45:1:1:1 and mixed evenly to obtain a negative electrode slurry. The remaining parameters and steps were the same as in Example 2.

[0154] Example 10

[0155] The difference from Example 2 is that the first monomer used in preparing the adhesive material is tris(2-hydroxyethyl)isocyanurate triacrylate. The remaining parameters and steps are the same as those in Example 2.

[0156] Example 11

[0157] The difference from Example 2 is that the first monomer used to prepare the binder material is the compound of structural formula (2-6). The remaining parameters and steps are the same as those in Example 2.

[0158] Example 12

[0159] The difference from Example 2 is that the second monomer is 1-aminocatechol methacrylate (an ester obtained by dehydrating aminocatechol and methacrylic anhydride). The remaining parameters and steps are the same as those in Example 2.

[0160] Example 13

[0161] The difference from Example 2 is that the structural formula of the first polymer used in preparing the binder material is (1-6). The remaining parameters and steps are the same as those in Example 2.

[0162] Comparative Example 1

[0163] The difference from Example 9 is that the molecular weight of the binder is 100,000. The remaining parameters and steps are the same as those of Example 9.

[0164] Comparative Example 2

[0165] The difference from Example 9 is that the molecular weight of the binder is 3.5 million. The remaining parameters and steps are the same as those of Example 9.

[0166] Comparative Example 3

[0167] Unlike Example 1, when preparing the negative electrode sheet, the binder prepared in Example 1 was not added to the negative electrode slurry of Example 1. Instead, the binder was replaced with SBR. Specifically, pre-lithiated silica, artificial graphite, conductive agent acetylene black, and SBR were dispersed in deionized water (dispersant) at a mass ratio of 14.55:82.45:1:2, stirred, and mixed until uniformly mixed to obtain the negative electrode slurry. The remaining parameters and steps were the same as in Example 1.

[0168] The lithium ion battery samples in each embodiment and comparative example were subjected to cycle performance tests, and the cycle performance test results are recorded in Table 1.

[0169] Cycling performance test method: At 25°C, the lithium-ion batteries prepared in each embodiment and comparative example were charged at a 4C rate and discharged at a 1C rate, and continuous cycling tests were performed in the range of 3%-97% SOC (State of Charge) until the capacity of the lithium-ion battery was less than 80% of the initial capacity. The number of cycles was recorded and recorded as the cycle life.

[0170] Material Specific Surface Area Testing Method: The silicon oxide, artificial graphite, silicon carbon, and other materials in the Examples and Comparative Examples can be tested using methods known in the art. For example, the specific surface area analysis method using nitrogen adsorption can be used in accordance with GB / T 19587-2017.

[0171] The particle size Dv50 (Dv50) of a material is tested using the laser diffraction method for particle size distribution according to GB / T 19077.1-2009. When a particle is irradiated by a laser beam, the angle of scattered light is inversely proportional to its diameter, while the intensity of the scattered light decays logarithmically with increasing angle. The energy distribution of the scattered light is directly related to the distribution of particle diameters. By receiving and measuring the energy distribution of the scattered light, the particle size distribution characteristics can be determined.

[0172] Table 1 Cyclic performance test results of various embodiments and comparative examples

[0173] It should be noted that the mass contents of pre-lithiated silicon oxide, silicon oxide and artificial graphite in Table 1 are based on the total mass of the negative electrode active material.

[0174] As can be seen from Table 1, adding the binder proposed in this application to different negative electrode active material systems, and the weight average molecular weight of the binder is between 200,000 and 3,000,000, can improve the cycle performance of the battery and extend the service life of the battery. The binder is added to a composite negative electrode system of pre-lithiated silicon oxygen and graphite, a composite negative electrode system of silicon oxygen and graphite, or a composite negative electrode system of silicon carbon and graphite, which can significantly improve the cycle stability of the battery. Taking Example 1 and Comparative Example 3 as examples for illustration, compared with Comparative Example 3, the binder proposed in this application is added to the negative electrode active material layer of Example 1, and the binder can effectively suppress the expansion effect of the negative electrode material during the charge and discharge process, and its number of cycles is significantly increased, and the cycle stability is significantly improved. It should be noted that for the composite negative electrodes of the above-mentioned different systems, changing the mass ratio of silicon-based material and graphite in the negative electrode active material, for example, when the mass ratio of silicon-based material and graphite in the negative electrode active material is less than 1:19 or greater than 3:17, adding a binder with a weight average molecular weight of 200,000 to 3 million proposed in this application can also improve the cycle performance of the battery.

[0175] It should also be noted that binders with a weight-average molecular weight of 200,000 to 3,000,000, all within this range, have the effect of improving battery cycle performance. In Comparative Example 1, the weight-average molecular weight of the binder was too low. The cycle performance test used a small battery cell. The small battery cell itself is a small stack, so the risk of the negative electrode active material layer falling off is relatively low. There is no clamp on the outside, so the small battery cell can expand. For mass production, it will be made into a large battery cell and need to be rolled up. The large battery cell is clamped by two hard clamps on the outside, which is very stressful and can easily cause the negative electrode active material layer to fall off. The weight-average molecular weight of the binder in Comparative Example 2 is too large, the viscosity of the binder is very high, and agglomeration will occur during slurry stirring. In experimental testing, small battery cells are made, and the negative electrode slurry is placed in a small tank and stirred continuously to reduce the risk of slurry agglomeration so as to complete the small battery cell test; in mass production, a large stirring tank is used for stirring. After the slurry is stirred, the slurry comes out of the stirring tank and is finally coated. It may be placed on the mass production line for a period of time, for example, about 24 hours. The slurry is likely to agglomerate in the pipeline. The pipeline is very long, and the slurry is difficult to flow after agglomeration, and subsequent operations cannot be performed. The weight-average molecular weight of the binder is too large to meet the needs and indicators of mass production.

[0176] Rebound rate of fully charged electrode:

[0177] The rebound rate of the negative electrode sheet samples of Example 1 and Comparative Example 3 was tested. The thickness of the negative electrode sheet was obtained by testing with a vernier caliper. The thickness d of the negative electrode sheet after cold pressing was used as a reference. The thickness of the negative electrode sheet after full charge was D. The rebound rate of the fully charged sheet = [(Dd) / d] × 100%. Among them, the rebound rate of the fully charged sheet of the negative electrode sheet of Comparative Example 3 was as high as 42%, which greatly limited the improvement of the energy density of the graphite and silicon-based composite materials and also had an adverse effect on the cycle stability of the battery. After the binder proposed in this application was added to Example 1, the rebound rate of the fully charged sheet can be reduced to 30%, which can significantly reduce the rebound rate of the fully charged sheet and improve the cycle performance of the battery.

[0178] In the description of this specification, the descriptions with reference to the terms "one embodiment", "another embodiment", "some embodiments", "other embodiments", etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present application. In this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are mutually inconsistent. In addition, it should be noted that in this specification, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated.

[0179] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A binder, wherein: The binder comprises a copolymer of a first polymer and a second polymer, wherein the first polymer has a structural formula of formula (1), and the second polymer is a copolymer of a first monomer and a second monomer, wherein the first monomer comprises at least one of carbamate, a compound having a structural formula of formula (2), tris(2-hydroxyethyl)isocyanuric acid triacrylate and (2-hydroxyethyl)methacrylate, and the second monomer comprises at least one of an ester obtained by dehydrating a compound having a structural formula of formula (3) and olefinic anhydride, 4-amino-catechol olefinic acid ester, dopamine hydrochloride olefinic acid ester, 1-aminocatechol olefinic acid ester and 3,4-dihydroxyphenylalanine olefinic acid ester. Wherein, X includes at least one of a hydroxyl group and a thiol group, and the number of carbon atoms in X is not greater than 3, Y includes at least one of a hydroxyl group and a thiol group, and the number of carbon atoms in Y is not greater than 3, Z includes at least one of an amino group and a thiol group, and the number of carbon atoms in Z is not greater than 3, and the weight average molecular weight of the binder is 200,000-3,000,000.

2. The adhesive according to claim 1, wherein At least one of the following conditions is met: The first polymer includes at least one of the following polymers: The first monomer includes at least one of the compounds of the following structural formulas: The second monomer comprises at least one of the esters obtained by dehydrating a compound of the following structural formula and an olefinic anhydride:

3. The adhesive according to claim 1 or 2, wherein At least one of the following conditions is met: X is a hydroxyl group; The first monomer includes 2-hydroxyethyl acrylate; The second monomer includes at least one of 4-amino-catechol methacrylate, 4-amino-catechol crotonate, and 4-amino-catechol pentenoate; The olefinic anhydride includes at least one of methacrylic anhydride, crotonic anhydride and 4-pentenoic anhydride.

4. The binder according to any one of claims 1 to 3, wherein The weight average molecular weight of the binder is 1 million to 2 million.

5. The binder according to any one of claims 1 to 4, wherein The binder satisfies one of the following conditions: X is a hydroxyl group, the first monomer is 2-hydroxyethyl acrylate, and the second monomer is 4-amino-catechol methacrylate; X is a hydroxyl group, the first monomer is tris(2-hydroxyethyl)isocyanuric acid triacrylate, and the second monomer is 4-amino-catechol methacrylate; X is a hydroxyl group, the first monomer is a compound of structural formula (2-6), and the second monomer is 4-amino-catechol methacrylate; X is a hydroxyl group, the first monomer is 2-hydroxyethyl acrylate, and the second monomer is 1-aminocatechol methacrylate; The structural formula of the first polymer is formula (1-6), the first monomer is 2-hydroxyethyl acrylate, and the second monomer is 4-amino-catechol methacrylate.

6. A negative electrode sheet, wherein: The invention comprises a negative electrode current collector and a negative electrode active material layer, wherein the negative electrode active material layer is located on at least one side surface of the negative electrode current collector, and the negative electrode active material layer comprises: A negative electrode active material, the negative electrode active material comprising a silicon-based material and graphite; and The adhesive according to any one of claims 1 to 5.

7. The negative electrode sheet according to claim 6, wherein: The negative electrode active material layer further includes at least one of a viscous material and a conductive agent.

8. The negative electrode sheet according to claim 7, wherein: At least one of the following conditions is met: The silicon-based material includes at least one of pre-lithiated silicon oxygen, silicon oxygen and silicon carbon; The graphite includes at least one of natural graphite and artificial graphite; The viscous material includes at least one of styrene-butadiene rubber, polyamide-imide, polyvinyl alcohol, polyethylene imine, polyimide and poly(tert-butyl acrylate-triethoxyvinylsilane); The weight average molecular weight of the viscous material is 40,000-2,000,000; The conductive agent includes at least one of carbon nanotubes, carbon black, carbon fibers and graphene; The negative electrode active material further includes at least one of hard carbon, soft carbon, Ketjen black, mesophase carbon microbeads, graphene and carbon fiber.

9. The negative electrode sheet according to claim 7, wherein: Based on the total mass of the negative electrode active material layer, the negative electrode active material layer includes: Silicon-based material with a mass content of 0.85wt% to 59.82wt%; Graphite with a mass content of 34wt% to 98.75wt%; A conductive agent having a mass content of 0.1wt% to 5wt%; A binder having a mass content of 0.1wt% to 5wt%; The mass content of the viscous material is 0.1wt% to 5wt%.

10. The negative electrode sheet according to any one of claims 6, 7 and 9, wherein: The negative electrode active material is composed of silicon-based material and graphite, and the mass ratio of the silicon-based material to the graphite is 1:99 to 3:

2.

11. A battery, wherein: It comprises a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the negative electrode sheet is the negative electrode sheet according to any one of claims 6 to 10.

12. An electrical device, wherein: Comprising the battery of claim 11.

Citation Information

Patent Citations

  • Binder, negative pole piece, battery and electric device

    CN116285882A

  • Negative electrode active material for lithium ion secondary battery, lithium ion secondary battery negative electrode arranged by use thereof, and lithium ion secondary battery arranged by use thereof

    JP2017183051A

  • Aqueous binder and secondary battery

    WO2019120140A1