Method for producing steel strip for battery case
By optimizing the chemical composition and process flow of steel for battery shells, the problem of uneven wall thickness reduction and inclusions in stamped components of steel for battery shells is solved, and a steel belt with high cleanliness and high performance uniformity is achieved Production to meet the needs of rapid stamping forming.
Patent Information
- Application Number
- PCT/CN2023/119274
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2023-09-18
- Publication Date
- 2024-11-28
AI Technical Summary
During the stamping process of existing battery shell steel, the wall thickness is uneven, and the defects such as ear making and burrs are prone to occur. The inclusions are large in size and large in quantity, which affects the continuous casting performance of the steel liquid, resulting in the surface being curled. , sand holes, holes and other defects, and the formation performance of low-carbon battery shell steel is poor, making it difficult to meet the requirements of rapid stamping and thinning.
By optimizing the chemical composition and process flow of steel strips, the content of carbon, manganese, titanium, aluminum, phosphorus, sulfur and nitrogen is controlled, and the converter → LF refining → RH treatment → continuous casting process is used to combine carbon, ferromanganese and metal manganese Coordinated use can achieve the improvement of the cleanliness and stamping performance of the steel, and reduce the inclusions of the shallow surface layer of the casting billet through the immersion port insertion depth and the plug-in rod blowing argon flow design.
High cleanliness, high surface quality and high performance uniformity steel strips are obtained, which reduces the anisotropy and reduces the appearance of defects such as squids, sand holes, and holes, meeting the requirements of rapid stamping and forming.
Smart Images

Figure PCTCN2023119274-FTAPPB-I100001 
Figure PCTCN2023119274-FTAPPB-I100002 
Figure PCTCN2023119274-FTAPPB-I100003
Abstract
Description
Production method of steel strip for battery casing Technical Field
[0001] The invention relates to a production method of a steel strip for a battery shell, belonging to the technical field of metallurgy. Background Art
[0002] Battery casing steel is a high-end cold-rolled steel grade with extremely high comprehensive performance requirements. The steel strip is required to have high cleanliness, high surface quality, high performance uniformity, and excellent processing properties. Therefore, during the manufacturing process, it is required to reduce the anisotropy of the steel strip (Δr ≤ 0.15) to ensure its stamping performance, reduce the number of endogenous inclusions such as deoxidation products and foreign inclusions such as secondary oxidation, and reduce defects such as sand holes, warping, holes, and stamping cracks to ensure surface quality.
[0003] Common defects in battery case steel include slag inclusions, warping, pinholes, holes, and cracks. These defects are primarily caused by non-metallic inclusions generated during the steelmaking process. During the stamping process, battery case steel components must be uniformly thinned and free of defects such as earing and burrs. Therefore, the manufacturing process for battery case steel requires extremely low anisotropy, and the size of non-metallic inclusions must be as small as possible.
[0004] In the existing technology, the steel used in battery cases has the following main problems: 1) The strip steel has poor anisotropy. During the stamping process into components, the wall thickness is unevenly thinned, which easily leads to defects such as ears and burrs; 2) The strip steel has large inclusions in large numbers, which affects the continuous casting performance of the molten steel and causes defects such as warping, sand holes, and holes on the strip steel surface.
[0005] For example, the patent document with publication number CN109136444A discloses a steel for new energy vehicle battery shells for rapid and thinning stamping processing and a production method. This invention ensures the cleanliness and performance of the steel strip through reasonable composition design and optimized design of processes such as steelmaking, refining, continuous casting, hot rolling, coiling, cold rolling, and continuous annealing. It not only has higher strength than commercial ultra-low carbon steel, but also overcomes the problem of poor forming performance of low-carbon battery shell steel, and adapts to the processing requirements of rapid stamping and thinning stamping. However, this method requires a high temperature for steel tapping from the converter, resulting in large refractory material loss in the converter and high smelting costs; the RH decarburization process produces a large number of inclusions due to oxygen blowing and temperature increase, which affects the casting performance of the molten steel, and ultimately causes defects such as sand holes and warping in the steel strip. The patent document with authorization announcement number CN100560770C discloses a battery shell steel with excellent planar isotropy and a manufacturing method thereof. The patent adopts a low-carbon aluminum-killed steel composition system to produce battery shell steel, with a carbon mass percentage of 0.01 to 0.05%. The annealing process is hood annealing. This composition system has low production difficulty and low manufacturing cost, but because it is a low-carbon steel composition, the stamping processing performance is poor, and it is difficult to meet the requirements of rapid stamping and thinning of battery shell steel.
[0006] Summary of the Invention
[0007] The object of the present invention is to provide a method for producing a steel strip for a battery casing, wherein the obtained steel strip has high cleanliness, high surface quality, high performance uniformity and excellent processing performance.
[0008] To achieve the above object, the technical solution of the present invention is:
[0009] A method for producing a steel strip for a battery case, wherein the chemical composition and mass percentage of the steel strip for the battery case are: carbon: 0.003-0.006%, silicon ≤0.03%, manganese: 0.35-0.45%, titanium: 0.040-0.050%, aluminum: 0.040-0.060%, phosphorus ≤0.020%, sulfur ≤0.012%, nitrogen ≤0.0040%, and the balance is iron and unavoidable impurities, wherein 7>Ti / (C+N)>5.
[0010] The composition control principle of the steel strip for battery casing of the present invention is as follows:
[0011] Carbon (C): A strengthening element in steel, it increases its strength and decreases its plasticity. To ensure that the steel used in battery housings for new energy vehicles possesses a certain strength to withstand the internal pressure of the battery after filling, the C content must be controlled. Furthermore, interstitial carbon atoms can reduce the stamping performance of the steel strip. Therefore, the present invention controls the C content to 0.0030-0.0060%, improving the stamping performance while maintaining the strength of the steel strip.
[0012] Manganese (Mn): A steel-strengthening element. A certain manganese content can increase the strength of the steel strip. Mn combines with sulfur to form MnS, which prevents hot brittleness caused by sulfur in the steel. However, excessive manganese content in ultra-low carbon steel can be detrimental to stamping processes, so the Mn content is controlled at 0.35-0.45%.
[0013] Titanium (Ti): Ti is used to fix C and N atoms, so that the steel strip reaches an interstitial atom-free (IF) state, and the steel strip has good stamping forming performance. Ti mainly exists in the form of precipitated phases such as TiN, which precipitates in ferrite, hinders grain growth, and improves strength. The C content in the present invention is specially designed, and the Ti content needs to ensure the effect of fixing C and N to improve the stamping forming performance while meeting the need for isotropy. In addition, too high Ti has an adverse effect on the casting performance of molten steel. Therefore, the Ti content is designed accordingly and controlled at 0.04-0.05%. At the same time, 7>Ti / (C+N)>5 is controlled. While fixing C and N, there is an appropriate amount of dissolved Ti content in the steel, which increases the r value to a certain extent, reduces the anisotropy of the steel strip, and ensures high-speed stamping forming performance.
[0014] Aluminum (Al): Aluminum is used in the steelmaking process for deoxidation, removing oxygen from the molten steel during smelting to form easily removable inclusions such as alumina. However, too low an Al content in the molten steel results in poor deoxidation and difficulty ensuring molten steel cleanliness. Furthermore, the addition of aluminum to steel forms acid-soluble aluminum (Als), which reacts with nitrogen to form AlN, promoting interstitial atomization. The finely dispersed AlN precipitates inhibit austenite grain growth, refine grains, and promote microstructure homogenization. However, excessively high Als levels significantly increase the difficulty of controlling smelting and casting. Therefore, the Al content is controlled between 0.04 and 0.06%.
[0015] Silicon (Si): It is a strengthening element, but has a great influence on stamping performance and is controlled at ≤0.03%.
[0016] Phosphorus (P) also has a strengthening effect, but it will increase the brittleness of steel plate processing and damage the stamping performance, so it needs to be removed. However, too low P content increases the difficulty of steelmaking and smelting, so it is controlled at ≤0.020%.
[0017] Sulfur (S): It is a harmful element for steel strips, affecting toughness and stamping performance, and needs to be removed. Considering the difficulty of control, it is controlled at ≤0.012%.
[0018] Nitrogen (N): Excessive content will lead to a significant decrease in the stamping performance of the steel strip and should be controlled at ≤0.0040%.
[0019] The process (production method) is as follows: hot metal pretreatment → converter smelting → LF refining → RH treatment → continuous pouring → hot rolling → pickling → cold rolling → continuous annealing → finishing. Hot metal pretreatment: The hot metal is stirred and desulfurized. After desulfurization, the sulfur content of the hot metal is ≤0.0050%. The hot metal temperature is 1300-1330°C.
[0020] Converter smelting: at least 2 clearly visible bottom blowing holes, argon gas is blown at the bottom during the entire blowing process, and the argon gas flow rate is ≥300Nm 3 / h, converter blowing end temperature 1640 ~ 1660 ℃, converter end carbon content 0.03 ~ 0.04%, converter end free oxygen content 0.06 ~ 0.08%, converter final slag T.Fe 15 ~ 18%, converter tapping slag amount 2 ~ 4 kg / t.
[0021] LF refining: After the ladle is placed in the heating position, power is turned on and heating begins. During this heating process, the ladle bottom blowing flow rate is controlled at 300-500 nL / min. This flow rate ensures temperature uniformity of the molten steel while maximizing heating efficiency. When the molten steel temperature reaches the target temperature of 1618-1635°C, the temperature and oxygen content of the molten steel are measured and determined. The free oxygen content of the molten steel is 0.06-0.07%. This free oxygen content meets the requirements of natural decarburization during the RH decarburization process, while also reducing the free oxygen content before deoxidation and alloying, reducing the amount of primary deoxidation products in the molten steel and improving the cleanliness of the molten steel. The ladle bottom blowing flow rate is adjusted to 100-200 nL / min. This flow rate is intended to provide the necessary kinetic conditions to promote the melting of modifiers and lime, while preventing surface exposure of the molten steel and the risk of secondary oxidation. According to the free oxygen content of the molten steel, add 400-500kg of slag modifier and 400-500kg of lime. The slag modifier composition is Al 45-50%, CaO 20-25%, Al2O3 10-15%, CaCO3 10-15%, and other unavoidable impurities. CaCO3 is a diffusing agent to promote the dispersion of the modifier.
[0022] RH treatment: The RH arrival temperature is 1610-1630°C. Due to the temperature drop during the RH treatment process, the temperature requirements for continuous pouring are met, and decarburization is relatively fast at this temperature. The arrival free oxygen content is 0.06-0.07%, meeting the natural decarburization requirements of the RH decarburization process. This also reduces the free oxygen content before deoxidation and alloying, minimizing the amount of primary deoxidation products in the molten steel and improving the cleanliness of the molten steel. The arrival carbon content is 0.025-0.035% (the decarburization capacity of the converter blowing process is limited, resulting in a carbon content of this level at the RH arrival point. Furthermore, after RH decarburization within this control range, the free oxygen content in the molten steel is low, primary deoxidation products are minimal, and the cleanliness of the molten steel is high). The T.Fe content of the ladle slag at the RH arrival point is 5-8%. RH decarburization takes 15-18 minutes. Once the temperature, final carbon, and final oxygen requirements are met, decarburization for 15-18 minutes is sufficient. Decarburization for longer periods of time will result in unnecessary temperature drops, leading to increased temperatures from RH oxygen and aluminum blowing, which can affect the cleanliness of the molten steel. After RH decarburization, the free oxygen content of the molten steel is 0.025-0.030%. Aluminum granules, carbon-containing ferromanganese, metallic manganese, and titanium-containing alloy are added in sequence, depending on the composition. The carbon-containing ferromanganese addition rate is 2.3-2.7 kg / t of steel, and the manganese addition rate is 1.1-1.3 kg / t of steel. After the addition of the aluminum granules and manganese-containing alloy (carbon-containing ferromanganese and metallic manganese), the titanium-containing alloy is added in a cycle (e.g., 3 minutes). After alloying and circulating for 5-8 minutes, the steel is tapped from the RH ladle. The carbon content of carbon-containing ferromanganese is 0.8-1.2%, and the titanium content of the titanium-containing alloy is ≥99.6%. The RH ladle slag composition is T.Fe ≤ 5%. The time between RH breaking and continuous pouring is 10 to 15 minutes. During this period, there is a secondary oxidation process of slag on molten steel. The time interval should be minimized as much as possible. However, due to the limitation of production rhythm, the time cannot be compressed indefinitely, so this time range is selected.
[0023] Continuous pouring: The tundish superheat is 25-35°C. High superheat pouring reduces inclusions in the molten steel and improves cleanliness. The mold cross-section is 220mm (thickness) x 1000-1400mm (width), and the submerged nozzle insertion depth is 160-200mm. Too deep an insertion depth will result in a low mold surface temperature, while too shallow will cause large mold level fluctuations. The opening angle is 20°, and this angle and insertion depth are coordinated. This angle and corresponding insertion depth can reduce the number and density of subsurface inclusions while ensuring the required mold surface temperature, thereby reducing or eliminating the need for stripping. The argon flow rate for the stopper during continuous casting (i.e., continuous pouring) is 8-12 L / min. This flow reduces the adhesion of inclusions to the nozzle inner wall and prevents bubble defects in the cast strand. Inclusions in the final product are all ≤15μm, and total oxygen is ≤15ppm.
[0024] Others: Qualified continuous casting (i.e., continuous pouring) billets undergo hot rolling, pickling, cold rolling, sequential annealing, and finishing to produce battery case steel strips. These processes are known in the art and will not be described in detail.
[0025] The present invention reduces the Δr value of the steel strip, increases the isotropy of the steel strip, and improves its processing performance through the chemical composition design of the battery shell steel; through the "converter → LF refining → RH treatment → continuous casting" process, precise control of the steel composition and effective control of the number and size of inclusions in the steel are achieved, wherein the coordinated use of carbon-containing ferromanganese and metallic manganese achieves precise targeting of extremely low carbon elements and manganese elements in the molten steel; through LF heating, slag making and fine-tuning of the molten steel composition, low-quantity control of the free oxygen in the molten steel is achieved at the end of RH decarburization; through the optimization of the insertion depth of the submerged nozzle and the design of the stopper rod argon blowing flow process, the number of inclusions in the shallow surface layer of the ingot is reduced, the peeling depth is reduced or no peeling is performed, and the yield rate is improved. DETAILED DESCRIPTION
[0026] The chemical composition of the steel strip for battery casing is shown in Table 1, with the remainder being iron and unavoidable impurities.
[0027] Table 1 Chemical composition of steel for battery shell
[0028] The production method of steel strip for battery case has the following process flow: molten iron pretreatment → converter smelting → LF refining → RH treatment → continuous casting → hot rolling → pickling → cold rolling → continuous annealing → finishing.
[0029] Hot metal pretreatment: blast furnace hot metal is desulfurized by adding desulfurizer and stirring at the pretreatment position. After desulfurization, the sulfur content of hot metal is ≤0.0050% and the temperature of hot metal is ≥1300℃.
[0030] Converter smelting: Desulfurized molten iron and scrap steel are added to the converter for smelting. There are four clearly visible bottom blowing holes at the bottom of the converter. Argon is blown throughout the blowing process, with an argon flow rate of 300-350 Nm 3 / h, converter blowing end temperature 1640-1660°C, converter end carbon content 0.03-0.04%, converter end free oxygen content 0.06-0.08%, converter final slag T.Fe 15-18%, converter slag blocking using slag plugs or slides, and converter tapping slag rate 2-4 kg / t. Heat parameters are shown in Table 2.
[0031] Table 2 Converter endpoint conditions
[0032] LF refining: After the ladle is placed in the heating station, the ladle car is moved to the power-on heating position and heating begins. During this heating process, the ladle bottom blowing flow rate is controlled at 300-500 nL / min. When the molten steel temperature reaches the target, the temperature and oxygen content of the molten steel are measured and determined. The free oxygen content of the molten steel is 0.06-0.07%. The ladle bottom blowing flow rate is adjusted to 100-200 nL / min. Depending on the free oxygen content of the molten steel, 400-500 kg of slag modifier and 400-500 kg of lime are added. After stirring for 3-5 minutes, the molten steel is hoisted to the RH vacuum station. The slag surface modifier composition is 48.3% Al, 23.3% CaO, 13.3% Al2O3, 12.5% CaCO3, and the remainder is impurities. The CaCO3 is used as a diffusion agent.
[0033] RH treatment: The RH arrival temperature is 1610-1630°C, the arrival free oxygen content is 0.06-0.07%, the arrival carbon content is 0.025-0.035%, and the arrival ladle slag has a T / Fe content of 5-8%. After RH decarburization for 15-18 minutes, the free oxygen content of the molten steel is 0.025-0.030%. Aluminum granules, carbon-containing ferromanganese, manganese metal, and titanium-containing alloy are added in sequence, depending on the composition requirements. The carbon-containing ferromanganese addition rate is 2.5 kg / t steel, and the manganese metal addition rate is 1.2 kg / t steel. The manganese-containing alloy is added 3 minutes after the Al granules are added, and the titanium-containing alloy is added 3 minutes after the manganese-containing alloy is added. After alloying, the steel is then circulated for 5-8 minutes before RH tapping. The carbon content of the carbon-containing ferromanganese is 1.1%, and the titanium content of the titanium-containing alloy is 99.8%. The T / Fe content of the RH ladle slag is ≤5%. The time between RH breaking and continuous pouring is 10 to 15 minutes. See Table 3 for details.
[0034] Table 3 RH treatment parameters
[0035] Continuous casting: Ingot cross-section: 220mm x 1260mm. Tundish superheat: 25-35°C. Submerged nozzle insertion depth: 160-200mm, opening angle: 20°. Argon flow rate for continuous casting stopper: 8-12 L / min. Inclusions in the final product are all ≤15μm, and total oxygen concentration is ≤15ppm. See Table 4 for details.
[0036] Table 4 Continuous casting parameters and inclusion levels of finished products
[0037] The qualified continuous casting billets are subjected to existing processes such as hot rolling, pickling, cold rolling, continuous annealing, and finishing to obtain strip steel for battery shells.
[0038] The surface quality of the battery case steel produced by the method of the present invention meets the O5 requirement, without defects such as warping, scarring, sand holes, holes, etc., and the isotropy is well controlled, and Δr is less than 0.15. Detailed data are shown in Table 5, which meets the requirements of rapid stamping.
[0039] Table 5 Δr of steel strip for battery case (Δr=(r0+r 90 -2r 45 ) / 2)
[0040] The calculation formula of Δr (Δr=(r0+r 90 -2r 45 ) / 2) The calculation formula published in the national standard "Determination of plastic strain ratio (r value) of metal sheets and strips" (GB / T 5027-2016) is used, where r0 is the plastic strain ratio at an angle of 0°, r 45 is the plastic strain ratio at an angle of 45°, r 90 is the plastic strain ratio at an angle of 90°. r0, r 90 、r 45 The value is obtained by measuring the value using the measurement method in the national standard "Determination of the plastic strain ratio (r value) of metal sheets and strips" (GB / T 5027-2016).
[0041] The above embodiments do not limit the present invention in any way, and any technical solutions obtained by equivalent replacement or equivalent transformation fall within the protection scope of the present invention.
Claims
1. A method for producing a steel strip for a battery case, comprising the steps of molten iron pretreatment, converter smelting, LF refining, RH treatment, and continuous casting, characterized in that: LF refining: After the ladle is placed, turn on the power-on heating position and start heating. During the heating process, the ladle bottom blowing flow rate is controlled at 300-500NL / min. When the molten steel temperature reaches the target temperature of 1618-1635℃, the temperature and oxygen are measured and the free oxygen content of the molten steel is 0.06-0.07%. The ladle bottom blowing flow rate is adjusted to 100-200NL / min, and slag modifier and lime are added according to the free oxygen content of the molten steel. RH treatment: RH arrival temperature is 1610-1630℃, arrival free oxygen is 0.06-0.07%, arrival carbon content is 0.025-0.035%, arrival ladle slag T.Fe is 5-8%; after RH decarburization for 15-18min, the free oxygen content of molten steel is 0.025-0.030%, according to the composition requirements, aluminum particles, carbon-containing ferromanganese, metallic manganese, titanium-containing alloy are added in sequence, among which the amount of carbon-containing ferromanganese added is 2.3-2,7kg / t steel, the amount of metallic manganese added is 1.1-1.3kg / t steel, and titanium-containing alloy is added after Al particles and manganese-containing alloy are added; the time from RH breaking to continuous pouring is 10-15min; the carbon content of carbon-containing ferromanganese is 0.8-1.2%, and the titanium content of titanium-containing alloy is ≥99.6%; Continuous casting: tundish superheat 25-35°C, immersion nozzle insertion depth 160-200mm, opening angle 20°, continuous casting stopper argon flow 8-12L / min; The chemical composition and mass percentage of the steel strip for battery shell are: carbon: 0.003-0.006%, silicon ≤0.03%, manganese: 0.35-0.45%, titanium: 0.040-0.050%, aluminum: 0.040-0.060%, phosphorus ≤0.020%, sulfur ≤0.012%, nitrogen ≤0.0040%, and the balance is iron and unavoidable impurities, wherein 7>Ti / (C+N)>5.
2. The method for producing a steel strip for a battery case according to claim 1, characterized in that: Hot metal pretreatment: Hot metal is stirred and desulfurized. The sulfur content of hot metal after desulfurization is ≤0.0050%.
3. The method for producing a steel strip for a battery case according to claim 1, characterized in that: Converter smelting: at least 2 clearly visible bottom blowing holes, argon gas is blown at the bottom during the whole blowing process, and the argon gas flow rate is ≥300Nm 3 / h, the final temperature of the converter blowing is 1640-1660℃, the final carbon content of the converter is 0.03-0.04%, the final free oxygen content of the converter is 0.06-0.08%, the final slag T.Fe is 15-18%, and the slag amount of the converter tapping is 2-4kg / t.
4. The method for producing a steel strip for a battery case according to claim 1, characterized in that: After continuous casting, the steps of hot rolling, pickling, cold rolling, continuous annealing and finishing are also included.
5. The method for producing a steel strip for a battery case according to claim 1, characterized in that: In the LF refining step, 400-500 kg of slag modifier and 400-500 kg of lime are added.
6. The method for producing a steel strip for a battery case according to claim 5, characterized in that: The slag modifier comprises 45-50% Al, 20-25% CaO, 10-15% Al2O3, 10-15% CaCO3, and the rest are inevitable impurities.
7. The method for producing a steel strip for a battery case according to claim 1, characterized in that: In the RH treatment step, the RH hollow ladle slag has a composition of T.Fe≤5%.
8. The method for producing a steel strip for a battery case according to claim 1, characterized in that: In the RH treatment step, after the Al particles and the manganese-containing alloy are added, the titanium-containing alloy is added after a 3-min cycle.
9. The method for producing a steel strip for a battery case according to claim 1, characterized in that: In the continuous pouring step, the size of inclusions in the final product is all ≤15μm, and the total oxygen is ≤15ppm.
Citation Information
Patent Citations
Steel for battery shell with excellent planar isotropism and its production
CN100560770C
Production method for steel for deep drawing of battery case
CN106148803A
Cold-rolled steel plate for ultra-low-carbon battery shell, and production method thereof
CN108728737A
Quick and thinning stamping processing new energy automobile battery shell steel and method for producing same
CN109136444A