Separator and preparation method therefor, secondary battery and preparation method therefor, and electric device

By using a separator film with a lithium-ion particle content in lithium-ion batteries, the ratio of its particle size to coating thickness is controlled, and the problems of resource waste and environmental pollution during the recycling process of lithium-ion batteries are solved, and the dynamics and circulation performance of the battery are improved. , achieving more efficient resource recycling and security performance.

WO2024239552A1PCT designated stage expired Publication Date: 2024-11-28CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/129679
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2023-11-03
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

In the recycling process of existing lithium-ion batteries, traditional methods have high energy consumption and cumbersome steps, and the treatment of used battery poles is not ideal enough, resulting in waste of resources and environmental pollution, and the circulation and safety performance of secondary batteries need to be improved.

Method used

Using a separator film with a lithium-rich particle content, by controlling the ratio of the average particle size and coating thickness of the lithium-rich particles to the range of 1:(1-15), to ensure that the separator film does not destroy the base film during charging and discharging, and passes through the separator The oxidative decomposition of lithium particles increases porosity and lithium ion supplementation, improving the dynamics and cycling performance of the battery.

Benefits of technology

It improves the dynamic performance and cycling performance of secondary batteries, enhances safety performance, reduces the internal resistance of lithium-ion batteries, extends the service life of the battery, and provides more efficient resource recycling and environmentally friendly recycling methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023129679_28112024_PF_FP_ABST
    Figure CN2023129679_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present application are a separator and a preparation method therefor, an electrode assembly, a secondary battery, a battery module, a battery pack and an electric device. The separator comprises: a first microporous base membrane, a second microporous base membrane, and a coating disposed between the first microporous base membrane and the second microporous base membrane, wherein the coating comprises lithium-rich particles, and the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating is 1:(1-15).
Need to check novelty before this filing date? Find Prior Art

Description

Separator and preparation method thereof, secondary battery and preparation method thereof, and electric device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 202310600998.8, filed on May 25, 2023, entitled “Isolation membrane and preparation method thereof, secondary battery and preparation method thereof, and electrical device”, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application belongs to the field of battery technology, and specifically relates to an isolation membrane and a preparation method thereof, a secondary battery and a preparation method thereof, and an electrical device. Background Art

[0004] As the production of lithium-ion batteries continues to expand, the number of discarded / used lithium-ion batteries is also increasing. Waste batteries are not only rich in valuable metal elements, but also retain residual energy inside the battery. In addition, if not handled properly, batteries will face serious resource shortages, and waste batteries will bring risks and pollution to the environment we live in. Pyrometallurgical / hydrometallurgical methods have been proven to be an effective strategy for extracting key metals and are currently widely used in the recycling of waste battery electrodes. However, high energy consumption or cumbersome steps undoubtedly increase the cost of the entire recycling process. Traditional recycling processes may not be the best choice for processing waste battery electrodes. Recycling some structurally stable waste positive electrode electrodes by replenishing lithium through diaphragms is a new solution.

[0005] The battery separator is an insulating film with a porous structure and is an important component of the battery. It can block the positive electrode and the negative electrode to prevent the positive electrode and the negative electrode from short-circuiting inside the battery.

[0006] Battery separators contain nanoscale pores that allow active ions, including lithium ions, to pass freely during the charge and discharge process, providing a pathway for the rapid transfer of active ions between the positive and negative electrodes. Multilayer composite separators offer the advantages of multiple materials and, compared to composites of several different separators, achieve complementary performance between the various layers. By sandwiching an intermediate functional layer within a multilayer separator, separator functionality can be achieved and its thickness reduced. In recent years, with the widespread use of secondary batteries and the increasing demand for their performance, higher requirements have been placed on the performance of separators.

[0007] Summary of the Invention

[0008] The purpose of this application is to provide an isolation membrane that can improve the kinetic performance and cycle performance of a secondary battery containing it; the purpose of this application is also to provide a secondary battery and an electrical device containing the above-mentioned isolation membrane, so as to obtain improved secondary battery kinetic performance and cycle performance.

[0009] In a first aspect, an embodiment of the present application provides an isolation film, comprising:

[0010] The first microporous base membrane,

[0011] a second microporous base membrane, and

[0012] A coating layer is provided between the first microporous base membrane and the second microporous base membrane, the coating layer comprising lithium-rich particles, wherein the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating layer is 1:(1-15).

[0013] According to the technical solution of the embodiment of the present application, the coating of the isolation membrane contains lithium-rich particles, and the average particle size Dv50 of the lithium-rich particles and the thickness of the coating are within the above-specified ranges. When the isolation membrane is in the winding process or even when subjected to mechanical compression, the lithium-rich particles will not damage or pierce the first microporous base membrane and the second microporous base membrane, which is beneficial to improving the safety performance of the secondary battery containing the isolation membrane. In addition, during the formation and subsequent charge and discharge processes of the secondary battery containing the isolation membrane of the embodiment of the present application, on the one hand, the lithium-rich particles can undergo oxidative decomposition or dissolution, and the vacancies generated by the decomposition increase the porosity of the isolation membrane, which is beneficial to improving the liquid absorption capacity and active ion permeability of the isolation membrane, reducing the internal resistance of the battery cell, and enhancing the dynamic performance of the secondary battery containing the isolation membrane; on the other hand, the lithium ions generated after the decomposition of the lithium-rich particles can replenish the lithium ions consumed during, for example, the formation and subsequent charge and discharge processes, which is beneficial to maintaining the capacity of the battery, thereby enhancing the cycle performance of the secondary battery containing the isolation membrane.

[0014] In addition, when the isolation membrane of the embodiment of the present application is combined with the positive electrode sheet obtained by disassembling the recycled battery and being charged and discharged, an electrode assembly comprising the isolation membrane and the positive electrode sheet that has been charged and discharged is obtained. The lithium ions generated after the decomposition of the lithium-rich particles in the isolation membrane can replenish the lithium ions consumed by the recovered positive electrode sheet after discharge, which is beneficial to restoring the capacity of the secondary battery, thereby reactivating the positive electrode active material and enhancing the cycle performance of the secondary battery comprising the isolation membrane.

[0015] In any embodiment of the present application, the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating is 1:1:(1.5-10). The average particle size Dv50 of the lithium-rich particles and the thickness of the coating are within the above-specified ranges, further improving the safety performance of a secondary battery containing the separator. Furthermore, during the formation and subsequent charge-discharge processes of a secondary battery containing the separator according to an embodiment of the present application, the kinetic performance of the secondary battery containing the separator is further enhanced; on the other hand, the cycling performance of the secondary battery containing the separator is further enhanced.

[0016] In any embodiment of the present application, the average particle size Dv50 of the lithium-rich particles is 0.2μm to 3μm, and can be optionally 0.25μm to 1μm. When the average particle size Dv50 of the lithium-rich particles is within the above range, when the isolation membrane containing the lithium-rich particles is formed and charged and discharged, the lithium-rich particles are oxidatively decomposed or dissolved to form voids, which can improve the distribution of voids in the coating layer of the isolation membrane and form voids with a particle size within the above range. The vacancies are beneficial to increase the porosity of the isolation membrane, reduce the internal ionic resistance of the battery cell, and enhance the dynamic performance of the secondary battery containing the isolation membrane. When the average particle size Dv50 of the lithium-rich particles is within the above range, it can reduce or avoid damage to the coating layer of the isolation membrane after the decomposition of the lithium-rich particles, thereby improving the safety performance of the secondary battery containing the isolation membrane.

[0017] In any embodiment of the present application, the average particle size Dv90 of the lithium-rich particles is 0.5 to 2.5 μm, optionally 0.5 to 2.0 μm. When the average particle size Dv90 of the lithium-rich particles is within this range, when the volume expansion of the negative electrode material squeezes the separator during the charge and discharge process of the secondary battery, the lithium-rich particles can further reduce or avoid squeezing or puncturing the first microporous base membrane or the second microporous base membrane, thereby improving the safety performance of the secondary battery including the separator.

[0018] In any embodiment of the present application, the average particle size Dv99 of the lithium-rich particles is 1 to 20 μm. When the average particle size Dv99 of the lithium-rich particles is within this range, when the volume expansion of the negative electrode material squeezes the separator during the charge and discharge process of the secondary battery, the lithium-rich particles can further reduce or avoid squeezing or puncturing the first microporous base membrane or the second microporous base membrane, thereby improving the safety performance of the battery.

[0019] In any embodiment of the present application, the mass percentage of lithium-rich particles in the coating is 10% to 80%, optionally 25% to 75%. When the separator containing the lithium-rich particles is charged and discharged, the lithium-rich particles oxidatively decompose to form voids. The mass percentage of lithium-rich particles in the coating within the above range can improve the distribution of voids in the separator coating, increase the porosity of the separator, reduce the internal resistance of the battery cell, and improve the dynamic performance of the secondary battery containing the separator. In addition, the mass percentage of lithium-rich particles in the coating within the above range can avoid or reduce damage to the separator coating after the decomposition of the lithium-rich particles, further improving the safety performance of the secondary battery containing the separator.

[0020] In any embodiment of the present application, the lithium-rich particles comprise a lithium salt or lithium-containing composite oxide having a layered, spinel, or olivine structure. The lithium-rich particles having the above-described structure can effectively maintain the structure of the coating, avoid structural collapse caused by vacancies resulting from oxidative decomposition of the lithium-rich particles, increase the porosity and permeability of the coating, reduce the internal ionic resistance of the battery cell, and improve the dynamic performance of the secondary battery containing the separator.

[0021] In any embodiment of the present application, the lithium-rich particles comprise one or more of Li2C2O4, LiOH, Li15Si4, and Li4Sn. The lithium-rich particles of the above structure can decompose during battery formation, which helps to increase the porosity and permeability of the coating, reduce the internal ionic resistance of the battery cell, and improve the dynamic performance of the secondary battery containing the separator.

[0022] In any embodiment of the present application, the lithium-rich particles have a core-shell structure, wherein the core comprises a layered lithium salt or a lithium-containing composite oxide; and the shell comprises one or more of carbon and silicon oxides. The lithium-rich particles have a core-shell structure, and the shell comprises one or more of carbon and silicon oxides. The shell has a certain degree of flexibility, encapsulating the lithium salt or composite oxide, thereby preventing the edges of the lithium salt or composite oxide from scratching or puncturing the first and second microporous base membranes, further preventing short circuits in secondary batteries containing the separators and improving their safety.

[0023] In any embodiment of the present application, the lithium salt or lithium-containing composite oxide having a layered structure includes Li x MO y , Li x [M b A d ]O y One or more of the following, wherein M includes one or more of Mn, Co, and Ni metals, A includes one or more of Al, Fe, V, Mg, Ca, Sr, and Ga elements, x is 0.8 to 2.2, y is 1.8 to 3.2, b>0, d>0, and b+d=1.

[0024] During the formation and charge / discharge process of the battery having the separator according to this embodiment, the battery containing Li x MO y He Li x [M b A d ]O y The lithium-rich particles of this type of lithium salt will undergo oxidative decomposition, and no decomposition products that are harmful to battery performance will remain; the vacancies produced by the decomposition increase the porosity of the isolation membrane, and can effectively maintain the structure of the coating in the isolation membrane, reduce the internal resistance of the battery cell, and thus improve the kinetic performance of the secondary battery containing the isolation membrane; in addition, the lithium ions produced after the decomposition of the lithium-rich particles are beneficial to maintaining or restoring the capacity of the battery and maintaining the lithium content of the electrode, thereby enhancing the cycle performance of the secondary battery containing the isolation membrane.

[0025] In any embodiment of the present application, the first microporous base membrane and the second microporous base membrane each comprise one or more of a polyolefin membrane, a non-woven fabric membrane, a polyester membrane, a polyether membrane, a polyetherimide membrane, and a fluorinated polyetherimide membrane. The materials of the first microporous base membrane and the second microporous base membrane are selected from the above materials and have good strength and toughness, thereby providing the separator with a high resistance to penetration by foreign particles or lithium-rich particles, thereby improving the safety performance of the secondary battery including the separator.

[0026] In any embodiment of the present application, the thickness of the first microporous base membrane and the second microporous base membrane are respectively 3 μm to 20 μm. The first and second microporous base membranes have appropriate thicknesses, thereby providing a suitable total thickness for the separator. This helps reduce the volume and weight of the secondary battery and improves the safety of the secondary battery containing the separator.

[0027] In any embodiment of the present application, the porosity of the first microporous base membrane and the second microporous base membrane is 30% to 70%, respectively. The first microporous base membrane and the second microporous base membrane have the above-mentioned porosity, which allows the first microporous base membrane and the second microporous base membrane to fully absorb and penetrate the electrolyte, so that the coating between the first microporous base membrane and the second microporous base membrane can be in full contact with the electrolyte, and the lithium-rich particles can be rapidly oxidized and decomposed in the presence of the electrolyte to form vacancies. Therefore, the separator according to this embodiment can ensure the rapid transmission of active ions including lithium ions, thereby improving the dynamic performance of the secondary battery containing the separator.

[0028] In any embodiment of the present application, the coating has a thickness of 0.5 to 20 μm. The coating thickness within this range can provide the separator with a suitable total thickness and effectively embed the added lithium-rich particles even when a large amount of lithium-rich particles are added to the coating, thereby achieving a better lithium replenishment effect on the electrode.

[0029] In any embodiment of the present application, the coating layer includes a binder and ceramic particles. The coating layer including ceramic particles and a binder provides the separator with good mechanical strength and a "thermal shutdown" function, thereby improving the safety performance of the secondary battery including the separator.

[0030] In any embodiment of the present application, the ceramic particles have an average particle size (Dv50) of 0.2 μm to 6 μm. The average particle size of the ceramic particles within the above range can improve the uniformity of the coating surface in the separator, maintain the stability of the coating structure, and enhance the safety performance of the secondary battery including the separator.

[0031] In any embodiment of the present application, the mass content of the ceramic particles in the coating is 20% to 60%. The mass content of the ceramic particles in the above range can maintain the stability of the coating structure and improve the safety performance of the secondary battery including the separator.

[0032] In any embodiment of the present application, the binder content in the coating is 10% to 20% by weight. The binder content in the coating within the above range is conducive to maintaining the stability of the coating structure, enhancing the adhesion between the first microporous base membrane and the second microporous base membrane and the coating, and preventing the decomposition of lithium-rich particles during the charge and discharge process of the secondary battery including the separator from causing vacancies in the coating and separating the first microporous base membrane from the second microporous base membrane.

[0033] In any embodiment of the present application, the porosity of the separator is 25% to 65%. The porosity of the separator is within an appropriate range, which helps the separator to have an appropriate electrolyte retention capacity, thereby improving the dynamic performance of the secondary battery including the separator.

[0034] In any embodiment of the present application, under the condition of testing at 130°C for 1h, the thermal shrinkage of the separator in the longitudinal direction (MD) is ≤5.0%, and the thermal shrinkage in the width direction (TD) is ≤5.0%. The test of thermal shrinkage in the longitudinal (Machine Direction, abbreviated as MD) direction and the transverse (Transverse Direction, abbreviated as TD) direction can refer to the national standard GB / T 36363-2018. The separator according to the embodiment of the present application has a composite structure of multiple film layers, which can enable the separator to have a smaller thermal shrinkage in the MD or TD direction. Therefore, even if the separator is damaged, the pore expansion rate of the damaged part under heating conditions is low. Therefore, even when the secondary battery containing the separator is subjected to mechanical damage such as nail penetration, the separator can still maintain a good isolation effect, thereby reducing the risk of thermal runaway of the secondary battery and improving safety performance.

[0035] In any embodiment of the present application, the separator has an air permeability of 300 s / 100 cc to 500 s / 100 cc. When the air permeability of the separator is within an appropriate range, ions can pass through the separator, thereby helping the secondary battery to have higher capacity performance and cycle performance.

[0036] In any embodiment of the present application, the tensile strength of the separator in transverse direction (TD) is 1000 to 2000 kg / cm 2 The tensile strength of the separator in the transverse (TD) direction is within an appropriate range, and it has high toughness and strength in this direction. Even when a secondary battery with this separator is subjected to mechanical damage such as nail penetration, the separator can still play a good isolation role, thereby reducing the risk of secondary thermal runaway and improving safety performance.

[0037] In any embodiment of the present application, the longitudinal tensile strength of the separator is 1200 to 1800 kg / cm 2 The tensile strength of the separator in the longitudinal direction (MD) is within an appropriate range, and it has high toughness and strength in this direction. Even when a secondary battery with this separator is subjected to mechanical damage such as nail penetration, the separator can still play a good isolation role, thereby reducing the risk of secondary thermal runaway and improving safety performance.

[0038] In a second aspect, an embodiment of the present application provides an isolation film, comprising:

[0039] a first microporous base membrane and a second microporous base membrane, a first coating layer disposed between the first microporous base membrane and the second microporous base membrane,

[0040] a third microporous base membrane, disposed on a side of the second microporous base membrane away from the first microporous base membrane; and

[0041] a second coating layer disposed between the second microporous base membrane and the third microporous base membrane;

[0042] Wherein, the first coating layer and / or the second coating layer contains lithium-rich particles, wherein the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating layer is 1:(1-15), and can be optionally 1:(1.5-10).

[0043] In a third aspect, an embodiment of the present application provides a method for preparing an isolation membrane, comprising:

[0044] providing a slurry comprising lithium-rich particles;

[0045] providing a coating of the slurry between a first microporous base membrane and a second microporous base membrane;

[0046] The slurry is dried so that the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the dried coating layer is 1:(1-15) to produce the separator of the first aspect.

[0047] According to the preparation method of the present application, the isolation membrane is obtained, wherein the average particle size Dv50 of the lithium-rich particles and the thickness of the coating are within the above-mentioned ranges. During the winding process of the isolation membrane, the lithium-rich particles will not damage or pierce the first microporous base membrane and the second microporous base membrane; when the isolation membrane is in the formation and subsequent charging and discharging process, on the one hand, the lithium-rich particles are oxidatively decomposed, and the vacancies generated by the decomposition are beneficial to increase the porosity of the isolation membrane, reduce the internal resistance of the battery cell, and enhance the liquid absorption capacity and the permeability of active ions, thereby enhancing the kinetic performance of the secondary battery containing the isolation membrane; in addition, the lithium ions generated after the decomposition of the lithium-rich particles are beneficial to maintaining or restoring the capacity of the battery, and are beneficial to maintaining the lithium content of the electrode, thereby enhancing the cycle performance of the secondary battery containing the isolation membrane.

[0048] In a fourth aspect, an embodiment of the present application provides a secondary battery, comprising the isolation membrane of the first aspect or the second aspect, or the isolation membrane prepared by the preparation method of the third aspect.

[0049] In any embodiment of the present application, the secondary battery includes a recycled positive electrode sheet, and the recycled positive electrode sheet includes a positive electrode active material film layer that has been charged and discharged, and the positive electrode active material film layer includes a lithium-containing positive electrode active material. When the positive electrode sheet in the electrode assembly is a positive electrode sheet that has been charged and discharged, it can come from the positive electrode sheet in the recycled battery. Compared with the normal positive electrode sheet, the active lithium ions in the positive electrode sheet in the recycled battery have a certain lithium loss. Using the isolation membrane of the embodiment of the present application, during the formation and subsequent charge and discharge process of the secondary battery containing the electrode assembly, the lithium ions generated after the decomposition of the lithium-rich particles can supplement the lithium ions consumed by the positive electrode active material film layer in the recycled battery, which is beneficial to restore the capacity of the battery, thereby enhancing the cycle performance of the secondary battery containing the isolation membrane.

[0050] In any embodiment of the present application, the lithium-containing positive electrode active material includes a lithium iron phosphate material, and the capacity of the secondary battery, when discharged to 0%, includes a mixed crystal phase of LFP and FPO, and the molar ratio of the LFP crystal phase to the FPO crystal phase is 97:(3-97). In the recovered positive electrode plate, there is a certain amount of loss of lithium element in the lithium-containing positive electrode active material, and the structural phase change of the lithium-containing positive electrode active material is within the above range. It can be combined with the isolation membrane containing lithium-rich particles of the embodiment of the present application, and the recovered positive electrode plate can be utilized. The isolation membrane of the embodiment of the present application is combined with the recovered positive electrode plate, which is also conducive to enhancing the cycle performance of the secondary battery including the isolation membrane and the positive electrode plate.

[0051] In any embodiment of the present application, after formation of the secondary battery, the ratio of the molar amount n1 of the lithium-containing positive electrode active material in the positive electrode active material film layer to the molar amount n2 of the lithium element in the coating layer of the lithium-rich particles is (0.2-50):1, and can optionally be (20-40):1. By adding lithium-rich particles, the molar amount n1 of the positive electrode active material film layer and the molar amount n2 of the lithium element therein in the coating layer are within the above range, which is beneficial for replenishing lithium in the recovered positive electrode sheets and is beneficial to the cycle performance of the secondary battery.

[0052] In a fifth aspect, an embodiment of the present application provides a method for preparing a secondary battery, the method comprising:

[0053] Provided is a separator according to the first aspect or a separator obtained by the method of the second aspect or the third aspect, the separator comprising a first microporous base membrane and a second microporous base membrane, and a coating disposed between the first microporous base membrane and the second microporous base membrane, the coating comprising lithium-rich particles, wherein a ratio of an average particle size Dv50 of the lithium-rich particles to a thickness of the coating is 1:(1-15);

[0054] A secondary battery comprising the separator and the recovered positive electrode sheet is prepared.

[0055] Compared to normal positive electrode sheets, the active lithium ions in the recovered battery's positive electrode sheets exhibit a certain amount of lithium loss. In a secondary battery produced using the preparation method of an embodiment of the present application, during the formation and subsequent charge and discharge processes of a secondary battery containing the electrode assembly, the lithium ions generated by the decomposition of the lithium-rich particles can replenish the lithium ions consumed by the positive electrode active material film layer in the recovered battery, facilitating the recovery of the battery's capacity and thereby enhancing the cycle performance of the secondary battery containing the separator.

[0056] In any embodiment of the present application, the positive electrode plate includes a lithium-containing positive electrode active material, and the ratio of the total molar amount n3 of the lithium-containing positive electrode active material in the positive electrode active material film layer to the total molar amount n4 of the lithium element in the coating layer of the lithium-rich particles is (0.2-1.5):1, and can optionally be (0.5-1.2):1. By adding lithium-rich particles, the molar amount n1 in the positive electrode active material film layer and the molar amount n2 of the lithium element therein in the coating layer are within the above range, which is beneficial for replenishing lithium in the recycled positive electrode plate and is beneficial to the cycle performance of the secondary battery.

[0057] In a sixth aspect, an embodiment of the present application provides an electrical device comprising the secondary battery of the fifth aspect.

[0058] The technical solution of the embodiment of the present application, by controlling the average particle size Dv50 of the lithium-rich particles in the separator and the thickness of the coating within the above range, can increase the porosity of the separator, reduce the ionic resistance of the battery cell, and enhance the dynamic performance of the secondary battery by oxidatively decomposing the lithium-rich particles during formation and subsequent charge and discharge processes. In addition, the lithium ions generated after the decomposition of the lithium-rich particles are beneficial for maintaining the lithium content of the electrode and the capacity of the secondary battery, thereby enhancing the cycle performance of the secondary battery containing the separator. The electrical device of the present application includes the secondary battery provided by the present application, and thus has at least the same advantages as the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.

[0060] FIG1 shows a schematic diagram of an embodiment of an isolation membrane of the present application.

[0061] FIG2 shows a schematic diagram of another embodiment of the isolation membrane of the present application.

[0062] FIG3 shows a schematic diagram of an embodiment of a secondary battery of the present application.

[0063] FIG. 4 is an exploded schematic diagram of the secondary battery shown in FIG. 3 .

[0064] FIG5 is a schematic diagram showing an embodiment of an electric device including the secondary battery of the present application as a power source.

[0065] In the accompanying drawings, the drawings are not necessarily drawn to scale. DETAILED DESCRIPTION

[0066] Below, the electrode assembly and its preparation method, secondary battery, battery module, battery pack and electric device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0067] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0068] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.

[0069] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.

[0070] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0071] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0072] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0073] Unless otherwise specified, the terms "connected" and "connection" in this application should be understood broadly. For example, they can refer to fixed connection, detachable connection, or integral connection; they can refer to direct connection, indirect connection through an intermediate medium, or internal communication between two components. Those skilled in the art will understand the specific meanings of the above terms in this application based on specific circumstances.

[0074] If not otherwise specified, in this application, the term "attach" refers to connection by adhesion, coating, etc.

[0075] Unless otherwise specified, in this application, the terms "first", "second", "third", "fourth", etc. are used to distinguish different objects rather than to describe a specific order or a primary-secondary relationship.

[0076] Unless otherwise specified, in this application, the term "active ions" refers to ions that can be intercalated and extracted between the positive and negative electrodes of a secondary battery, including but not limited to lithium ions.

[0077] The term "plurality" used in this application refers to two or more (including two).

[0078] In this application, the secondary battery may include a lithium-ion battery, which is not limited in the embodiments of this application. The secondary battery may be an aqueous battery or an oil-based battery, which is not limited in the embodiments of this application. The secondary battery may be flat, rectangular, or in other shapes, which is not limited in the embodiments of this application.

[0079] Secondary batteries, also known as rechargeable batteries or storage batteries, are batteries that can be recharged after discharge to activate the active materials and continue to be used. Typically, a secondary battery comprises an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator. The positive electrode sheet comprises a positive current collector and a positive active material film layer, which is coated on the surface of the positive current collector and contains the positive active material. The negative electrode sheet comprises a negative current collector and a negative active material film layer, which is coated on the surface of the negative current collector and contains the negative active material. During the battery's charge and discharge processes, active ions move back and forth between the positive and negative electrode sheets (including insertion and deinsertion, adsorption, etc.). The separator is positioned between the positive and negative electrode sheets to prevent short circuits between the positive and negative electrodes while allowing the active ions to pass through. Therefore, the separator is a crucial component of lithium-ion batteries. Its performance determines the battery's electrode interface structure, internal resistance, and other factors, affecting the battery's capacity, cycle life, and safety.

[0080] After repeated charge-discharge cycles, secondary batteries gradually consume active ions. For example, lithium ions released from the positive electrode active material film gain electrons at the negative electrode, potentially reducing them to form metallic dendrites, which are no longer able to participate in the charge-discharge cycle. This gradually deactivates the positive electrode active material and reduces its capacity, rendering the battery unusable after a certain number of charge-discharge cycles. To improve the cycle performance of secondary batteries, it is necessary to effectively replenish the active ions consumed during the charge-discharge process.

[0081] On the other hand, as the use of secondary batteries becomes more and more common, a large number of waste secondary batteries, such as waste power batteries, are generated. From an economic and environmental perspective, it is very necessary to safely and effectively recycle the positive electrode materials and the like in waste power batteries. The conventional method for recycling positive electrode materials is to remove the positive electrode sheets from waste secondary batteries, separate the active materials from the positive electrode sheets, and then regenerate them; the regenerated positive electrode materials can be used to prepare new positive electrode sheets. However, such a positive electrode material recycling method can actually be considered as a process of using deactivated positive electrode materials as raw materials and re-preparing positive electrode active materials, which still has large environmental and economic costs. If the positive electrode sheets with reduced capacity in waste secondary batteries can be directly recycled and used to prepare secondary batteries with an acceptable cycle life, it will be a more cost-effective recycling method.

[0082] In view of this, embodiments of the present application provide a separator that can at least reduce or avoid the adverse effects of lithium-deficient positive electrode sheets on the cycle performance of a secondary battery during the charge and discharge process, thereby improving the cycle performance of the secondary battery containing the separator. In addition, when the separator provided in embodiments of the present application is used to prepare a secondary battery, the positive electrode sheet can be directly recycled from a secondary battery that has reached the end of its cycle life.

[0083] Isolation film

[0084] The following describes an embodiment of the isolation membrane according to the first aspect of the present application with reference to FIG1 . As shown in FIG1 , the isolation membrane 1 includes:

[0085] The first microporous base membrane 10,

[0086] The second microporous base membrane 20, and

[0087] The coating layer 30 is disposed between the first microporous base membrane 10 and the second microporous base membrane 20 , and the coating layer comprises lithium-rich particles, wherein the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating layer is 1:(1-15).

[0088] Optionally, the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating is 1:(1.5-10), further optionally 1:(1.2-3), for example 1:(1.5-2.5). In some embodiments, the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating is any ratio of 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, or 1:15.

[0089] According to the technical solution of the embodiment of the present application, the coating of the isolation membrane contains lithium-rich particles, and the average particle size Dv50 of the lithium-rich particles and the thickness of the coating are within the above-specified ranges. When the isolation membrane is in the winding process or even when subjected to mechanical compression, the lithium-rich particles will not damage or pierce the first microporous base membrane and the second microporous base membrane, which is beneficial to improving the safety performance of the secondary battery containing the isolation membrane. In addition, during the formation and subsequent charge and discharge processes of the secondary battery containing the isolation membrane of the embodiment of the present application, on the one hand, the lithium-rich particles can undergo oxidative decomposition or dissolution, and the vacancies generated by the decomposition increase the porosity of the isolation membrane, which is beneficial to improving the liquid absorption capacity and active ion permeability of the isolation membrane, reducing the internal resistance of the battery cell, and enhancing the dynamic performance of the secondary battery containing the isolation membrane; on the other hand, the lithium ions generated after the decomposition of the lithium-rich particles can replenish the lithium ions consumed during, for example, the formation and subsequent charge and discharge processes, which is beneficial to maintaining the capacity of the battery, thereby enhancing the cycle performance of the secondary battery containing the isolation membrane.

[0090] In addition, when the isolation membrane of the embodiment of the present application is combined with the positive electrode sheet obtained by disassembling the recycled battery and undergoing charge and discharge, an electrode assembly comprising the isolation membrane and the positive electrode sheet undergoing charge and discharge is obtained. The lithium ions generated by the decomposition of the lithium-rich particles in the isolation membrane can replenish the lithium ions consumed by the positive electrode sheet undergoing charge and discharge, which is beneficial to restoring the capacity of the secondary battery, thereby enhancing the cycle performance of the secondary battery comprising the isolation membrane.

[0091] In addition, the vacancies generated by the decomposition of lithium-rich particles can still maintain the pore structure in the coating unchanged in a 105°C environment, which is beneficial to the stability of the battery during long-term use.

[0092] The average particle size Dv50 of the lithium-rich particles, also known as the mean volume particle size or median particle size, represents the particle size corresponding to 50% of the volume distribution of the particles. Dv50 can be measured using instruments and methods known in the art, for example, using a laser particle size analyzer, such as the Mastersizer 3000 laser particle size analyzer available from Malvern Instruments Ltd. in the United Kingdom.

[0093] In some embodiments, the average particle size Dv50 of the lithium-rich particles is 0.2 μm to 3 μm, optionally 0.25 μm to 1 μm. In some embodiments, the average particle size Dv50 of the lithium-rich particles can be any value or range of 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2.0 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, 2.5 μm, 2.6 μm, 2.7 μm, 2.8 μm, 2.9 μm, 3.0 μm. When the average particle size Dv50 of the lithium-rich particles is within the above range, when the isolation membrane containing the lithium-rich particles is formed and charged and discharged, the lithium-rich particles are oxidized and decomposed or dissolved to form voids, which can improve the void distribution of the coating in the isolation membrane and form voids with a particle size within the above range. The vacancies are beneficial to increase the porosity of the isolation membrane, reduce the internal ionic resistance of the battery cell, and enhance the kinetic performance of the secondary battery containing the isolation membrane; when the average particle size Dv50 of the lithium-rich particles is within the above range, it can reduce or avoid the damage to the coating of the isolation membrane after the decomposition of the lithium-rich particles, thereby improving the safety performance of the secondary battery containing the isolation membrane.

[0094] In some embodiments, the average particle size Dv90 of the lithium-rich particles is 0.5 to 2.5 μm, optionally 0.5 to 2.0 μm. The average particle size Dv90 of the lithium-rich particles can also be any value or range thereof selected from 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2.0 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, and 2.5 μm. The average particle size Dv90 of the lithium-rich particles is within the above range. When the volume expansion of the negative electrode material squeezes the isolation membrane during the charge and discharge process of the secondary battery, the extrusion or puncture of the first microporous base membrane or the second microporous base membrane by the lithium-rich particles can be further reduced or avoided, thereby improving the safety performance of the secondary battery containing the isolation membrane.

[0095] In some embodiments, the average particle size Dv99 of the lithium-rich particles is 1 to 4 μm. In some embodiments, the average particle size Dv99 of the lithium-rich particles can be any value selected from the group consisting of 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2.0 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, 2.5 μm, 2.6 μm, 2.7 μm, 2.8 μm, 2.9 μm, 3.0 μm, 3.1 μm, 3.2 μm, 3.3 μm, 3.4 μm, 3.5 μm, 3.6 μm, 3.7 μm, 3.8 μm, 3.9 μm, and 4.0 μm, or a range thereof. The average particle size Dv99 of the lithium-rich particles is within the above range. When the volume expansion of the negative electrode material squeezes the isolation membrane during the charge and discharge process of the secondary battery, the extrusion or puncture of the first microporous base membrane or the second microporous base membrane by the lithium-rich particles can be further reduced or avoided, thereby improving the safety performance of the battery.

[0096] The particle size distributions Dv99 and Dv90 of lithium-rich particles are both well-known in the art. The particle size distribution Dv99 represents the particle size corresponding to the 99th percentile volume distribution of the positive electrode active material particles; the particle size distribution Dv90 represents the particle size corresponding to the 90th percentile volume distribution of the positive electrode active material particles. Each of the above particle size distributions can be measured using instruments and methods well-known in the art. For example, a laser particle size analyzer, such as the Mastersizer 3000 laser particle size analyzer available from Malvern Instruments Ltd. in the UK, can be used.

[0097] In some embodiments, the mass percentage of lithium-rich particles in the coating is 5% to 90%, optionally 25% to 75%. In some embodiments, the mass percentage of lithium-rich particles in the coating is any value selected from 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, and 80%, or a range thereof. When the separator containing lithium-rich particles is charged and discharged, the lithium-rich particles are oxidized and decomposed to form voids. The mass percentage of lithium-rich particles in the coating within the above range can improve the distribution of voids in the separator, increase the porosity of the separator, reduce the internal resistance of the battery cell, and improve the dynamic performance of the secondary battery containing the separator. In addition, the mass percentage of lithium-rich particles in the coating within the above range can avoid or reduce damage to the separator coating after the decomposition of the lithium-rich particles, further improving the safety performance of the secondary battery containing the separator.

[0098] The mass percentage of lithium-rich particles in the coating can be determined based on the element content test method, including:

[0099] The membrane sample was immersed in an acetone solution and ultrasonically separated from the coating at 40°C for 3 hours. The acetone mixture containing the coating was collected. The element content in the mixture was measured using inductively coupled plasma optical emission spectrometry (ICP-OES). The mass percentage of each element was output.

[0100] In some embodiments, the volume percentage of lithium-rich particles in the coating is 10% to 90%. When the isolation membrane containing lithium-rich particles is charged and discharged, the lithium-rich particles are oxidatively decomposed or dissolved to form voids. The volume percentage of lithium-rich particles in the coating is within the above range, which can increase the corresponding porosity of the isolation membrane coating, reduce the internal resistance of the battery cell, and improve the dynamic performance of the secondary battery containing the isolation membrane.

[0101] In some embodiments, the lithium-rich particles comprise a lithium salt or lithium-containing composite oxide having a layered, spinel, or olivine structure. Lithium-rich particles with such structures can effectively maintain the structure of the coating, avoiding structural collapse caused by vacancies resulting from oxidative decomposition of the lithium-rich particles. This improves coating stability, porosity, and permeability, thereby reducing the internal ionic resistance of the battery cell and enhancing the kinetic performance of secondary batteries containing such separators.

[0102] In any embodiment of the present application, the lithium-rich particles comprise one or more of Li2C2O4, LiOH, Li15Si4, and Li4Sn. The lithium-rich particles of the above structure can decompose during battery formation, which helps to increase the porosity and permeability of the coating, reduce the internal ionic resistance of the battery cell, and improve the dynamic performance of the secondary battery containing the separator.

[0103] In some embodiments, the lithium-rich particles can have a layered structure, allowing lithium ions to diffuse in two dimensions, or a spinel structure, allowing lithium ions to diffuse in three dimensions. Alternatively, the lithium-rich particles can be selected from one or more of lithium transition metal oxides and compounds formed by adding other transition metals, non-transition metals, or non-metals to lithium transition metal oxides.

[0104] In some embodiments, the lithium-rich particles have a core-shell structure, wherein the core comprises a layered lithium salt or lithium-containing composite oxide, and the shell comprises one or more of carbon and silicon oxides. The shell of the lithium-rich particles, comprising one or more of carbon and silicon oxides, exhibits a degree of flexibility, encapsulating the lithium salt or composite oxide. This prevents the edges of the lithium salt or composite oxide from scratching or puncturing the first and second microporous base membranes, further preventing short circuits in secondary batteries containing such separators and improving their safety.

[0105] In some embodiments, the lithium salt or lithium-containing composite oxide having a layered structure includes Li x MO y , Li x [M b A d ]O y One or more of the following, wherein M includes one or more of Mn, Co, and Ni metals, A includes one or more of Al, Fe, V, Mg, Ca, Sr, and Ga elements, x is 0.8 to 2.2, y is 1.8 to 3.2, b>0, d>0, and b+d=1.

[0106] During the formation and charge / discharge process of the battery with the separator according to this embodiment, A can be present as a doping element in the Li x [M b A d ]O y This type of lithium salt can be used as an element that can change the valence state of layered metal oxides. The layered structure of lithium salts or lithium-containing composite oxides contains Li x MO y He Li x [M b A d ]O y The lithium-rich particles of this type of lithium salt will undergo oxidative decomposition, and no decomposition products that are harmful to battery performance will remain; the vacancies produced by the decomposition increase the porosity of the isolation membrane, and can effectively maintain the structure of the coating in the isolation membrane, reduce the internal resistance of the battery cell, and thus improve the kinetic performance of the secondary battery containing the isolation membrane; in addition, the lithium ions produced after the decomposition of the lithium-rich particles are beneficial to maintaining or restoring the capacity of the battery and maintaining the lithium content of the electrode, thereby enhancing the cycle performance of the secondary battery containing the isolation membrane.

[0107] In some embodiments, the lithium-rich particles may be selected from one or more of lithium cobalt oxide, lithium silver oxide, lithium manganese oxide, lithium silver manganese oxide, lithium silver cobalt manganese oxide, lithium silver cobalt aluminum oxide, and lithium-containing phosphate with an olivine structure.

[0108] In some embodiments, the lithium salt or composite oxide with an olivine structure contains lithium phosphate, and its general formula may be LiFe1−nMnmNTnPO4, where m is 0 to 1, n is 0 to 1, 0 < x + y < 1, and NT may be selected from one or more of other transition metal elements or non-transition metal elements except Fe and 1 M. 1 M' may be selected from one or more of Cr, Mg, Ti, Al, Zn, W, Nb, and Zr. More preferably, the lithium-containing phosphate with an olivine structure may be selected from one or more of lithium iron phosphate, lithium manganese phosphate, and lithium zinc iron phosphate.

[0109] There is no particular limitation on the specific type of the lithium-rich particles, as long as they can embed and extract lithium ions and can form vacancies under a relatively low voltage window. In some embodiments, the lithium-rich particles may be lithium-containing compounds such as C2H3LiO4, Li3N, Li2O2, Li2S, and -OLi.

[0110] In some embodiments, the first microporous base film and the second microporous base film respectively include one or more of a polyolefin film, a non-woven fabric film, a polyester film, a polyether film, a polyetherimide film, and a fluorinated polyetherimide film. The materials of the first microporous base film and the second microporous base film are selected from the above materials, having good strength and toughness, enabling the separator to have a high resistance to being pierced by foreign particles or lithium-rich particles, thereby improving the safety performance of the secondary battery including the separator.

[0111] In some embodiments, the thicknesses of the first microporous base film and the second microporous base film are respectively 3 μm to 20 μm. The thicknesses of the first microporous base film and the second microporous base film can be respectively any value or the range composed thereof among 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, and 20 μm. Having an appropriate thickness makes the separator have a suitable total thickness; it helps to reduce the volume and weight of the secondary battery and can improve the safety performance of the secondary battery including the separator.

[0112] In some embodiments, the porosity of the first microporous base membrane and the second microporous base membrane is 30% to 70%, respectively. The aforementioned porosity allows the first microporous base membrane and the second microporous base membrane to fully absorb and permeate the electrolyte, thereby allowing the coating between the first microporous base membrane and the second microporous base membrane to fully contact the electrolyte and allowing the lithium-rich particles to be rapidly oxidized and decomposed in the presence of the electrolyte to form vacancies. Therefore, the separator according to this embodiment can ensure the rapid transmission of active ions including lithium ions, thereby improving the dynamic performance of the secondary battery containing the separator.

[0113] In some embodiments, the coating has a thickness of 0.5 μm to 20 μm. The coating may have a thickness of 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2.0 μm, 5.0 μm, 6.0 μm, 7.0 μm, 8.0 μm, 9.0 μm, 10.0 μm, 12.0 μm, 15.0 μm, 18.0 μm, 19.0 μm, or 20.0 μm, or a range consisting of any of the following values: The thickness of the coating is within the above range, which can make the isolation membrane have a suitable total thickness; it can allow a large amount of lithium-rich particles to be added to the coating while still effectively embedding the added lithium-rich particles, thereby better achieving the lithium replenishment effect on the electrode.

[0114] In some embodiments, the coating layer includes a binder and ceramic particles. The coating layer including ceramic particles and a binder provides the separator with good mechanical strength and a "thermal shutdown" function, thereby improving the safety performance of the secondary battery including the separator.

[0115] In some embodiments, the ceramic particles have an average particle size Dv50 of 0.2 μm to 6 μm. The ceramic particles having an average particle size within the above range can improve the uniformity of the coating surface in the separator, maintain the stability of the coating structure, and enhance the safety performance of the secondary battery including the separator.

[0116] In some embodiments, the mass content of the ceramic particles in the coating is 20% to 60%. The mass content of the ceramic particles in the above range can maintain the stability of the coating structure and improve the safety performance of the secondary battery including the separator.

[0117] In some embodiments, the ceramic particles may have a "hair"-like structure in microstructure, which has a certain degree of flexibility and elasticity and can enhance the liquid absorption capacity of the isolation membrane.

[0118] In some embodiments, the binder content in the coating is 10% to 20% by weight. The binder content in the coating within the above range is beneficial for maintaining the stability of the coating structure, enhancing the adhesion between the first microporous base membrane and the second microporous base membrane, and preventing the decomposition of lithium-rich particles during the charge and discharge process of a secondary battery including a separator from creating vacancies in the coating and causing separation of the first microporous base membrane and the second microporous base membrane.

[0119] The thicknesses of the first microporous base membrane and the second microporous base membrane, the isolation membrane and the coating are all well known in the art and can be tested using instruments and methods known in the art. An exemplary test method for the thickness of the isolation membrane is as follows: take a sample of 500 mm in length and 100 mm in width; take 5 points evenly on the sample (for example, take a point every 100 mm along the length of the sample), use a 10,000-point thickness gauge to test the thickness of the isolation membrane at the 5 different positions, and take the average value as the thickness of the isolation membrane. The length direction of the sample is parallel to the TD direction of the isolation membrane. The thickness of the first microporous base membrane and the second microporous base membrane can be tested with reference to the above method. If a coating is provided on one side of the isolation membrane, the thickness of the isolation membrane minus the thickness of the base membrane is the thickness of the coating. If the opposite sides of the isolation membrane are provided with a coating to be tested and a coating on the opposite side of the coating to be tested, the thickness of the isolation membrane minus the sum of the thickness of the base membrane and the coating on the opposite side is the thickness of the coating to be tested.

[0120] In some embodiments, the porosity of the separator is 25% to 65%. A suitable porosity range of the separator helps the separator to have a suitable electrolyte retention capacity, thereby improving the dynamic performance of the secondary battery including the separator.

[0121] The porosity of the isolation membrane is well known in the art and can be tested using instruments and methods known in the art. An exemplary test method is as follows:

[0122] The porosity of the separator is measured using a Micromeritics AUTOPOREV 9620 mercury intrusion porosimeter. Under compression, a certain amount of mercury liquid is filled into the separator, and the ratio of the volume occupied by the mercury liquid to the volume of the material is measured to obtain the separator porosity.

[0123] In some embodiments, under the condition of testing at 130°C for 1 hour, the thermal shrinkage of the isolation membrane in the longitudinal direction (MD) is ≤5.0%, and the thermal shrinkage in the width direction (TD) is ≤5.0%. The test of thermal shrinkage in the longitudinal (Machine Direction, abbreviated as MD) direction and the transverse (Transverse Direction, abbreviated as TD) direction can refer to the national standard GB / T 36363-2018. The isolation membrane according to the embodiment of the present application has a composite structure of multiple film layers, which can enable the isolation membrane to have a smaller thermal shrinkage in the MD or TD direction. Therefore, even if the isolation membrane is damaged, the pore expansion rate of the damaged part under heating conditions is low. Therefore, even when the secondary battery containing the isolation membrane is subjected to mechanical damage such as nail penetration, the isolation membrane can still maintain a good isolation effect, thereby reducing the risk of thermal runaway of the secondary battery and improving safety performance.

[0124] As an example, the test method involves cutting the separator into a specimen with a MD length lM0 of 100 mm and a TD length lT0 of 100 mm, with the MD direction of the specimen parallel to the MD direction of the separator, and the TD direction of the specimen parallel to the TD direction of the separator. The specimen is then heated in a 130°C oven for one hour. The MD length lM or TD length lT of the heated specimen is then measured, and the thermal shrinkage in the MD or TD direction is calculated. The test method can refer to the national standard GB / T 36363-2018.

[0125] In some embodiments, the permeability of the separator is 300 s / 100 cc to 500 s / 100 cc. The permeability of the separator is within an appropriate range, which facilitates ions to pass through the separator, thereby helping the secondary battery to have higher capacity performance and cycle performance.

[0126] The air permeability of a barrier membrane refers to the degree to which an object or medium allows gas to pass through it. Under stable pressure, the time required for a certain volume of gas (25 cubic centimeters (cc) to 300 cc) to flow through a sample of a specified area is measured. In the examples of this application, the air permeability of the barrier membrane was tested using a Gurley 4110N air permeability tester manufactured in the United States. The test method is to measure the time (in seconds) required for 100 cc of air to pass through a 3-inch diameter circular membrane at a high pressure of 4.88 inches of water column.

[0127] In some embodiments, the transverse direction (TD) tensile strength of the separator is 1000 to 2000 kg / cm 2The tensile strength of the isolation membrane in the transverse (TD) direction is within an appropriate range, and it has high toughness and strength in this direction. Even when the secondary battery with the isolation membrane is subjected to mechanical damage such as nail penetration, the isolation membrane can still play a good isolation role, thereby reducing the risk of secondary thermal runaway and improving safety performance.

[0128] In some embodiments, the separator has a tensile strength in the machine direction (MD) of 1200 to 1800 kg / cm². A separator with a tensile strength in the MD within an appropriate range provides high toughness and strength in this direction. Even when mechanically damaged, such as by nail penetration, secondary batteries equipped with such separators can still effectively isolate the battery due to the separator, thereby reducing the risk of thermal runaway and improving safety.

[0129] In some embodiments, the method for testing the longitudinal (MD) tensile strength of a separator includes: taking five specimens, each 100 mm long and 15 mm wide, along the MD direction of the base film, with the length of the specimens parallel to the MD direction of the base film; clamping each specimen in two opposing fixtures of a tensile testing machine, setting the specimen gauge length to 40 mm (i.e., the distance between the fixtures), and conducting a tensile test at a constant speed of 50 mm / min. The force F and tensile displacement ΔL at the moment of tensile rupture are read. The unit thickness tensile strength of each specimen is calculated using the unit thickness tensile energy calculation formula.

[0130] In some embodiments, the peel strength between the coating and the first microporous base membrane is ≥50N / m, (50-1500N / m) optionally any one of 50N / m to 1200N / m, 150N / m to 1000N / m, 200N / m to 800N / m, 400N / m to 700N / m, and 500N / m to 600N / m. The higher the peel strength between the coating and the first microporous base membrane, the better the interlayer adhesion of the isolation membrane. Therefore, the performance of the isolation membrane is further improved. Instruments and methods known in the art can be used for testing. An exemplary test method is as follows: bond the green glue to the surface of the coating of the isolation membrane; then cut it into a width w of 15mm; peel the coating and the base membrane 180° at 50mm / min; read the maximum tensile force x (N) according to the data graph of tension and displacement, and calculate the peel strength F' (N / m) between the coating and the base membrane according to F'=x / w. The stretching equipment may be a tensile testing machine from a high-speed rail testing instrument company, such as the AI-3000-S model.

[0131] FIG2 shows another embodiment of the isolation membrane according to the first aspect of the present application. As shown in FIG2 , the isolation membrane 1 includes a first microporous base membrane 10, a second microporous base membrane 20, a first coating layer 30a disposed between the first microporous base membrane 10 and the second microporous base membrane 20, and further includes a third microporous base membrane 40 disposed on the side of the second microporous base membrane 20 facing away from the first microporous base membrane 10, and a second coating layer 30b disposed between the second microporous base membrane 20 and the third microporous base membrane 40. The description of any embodiment of the first microporous base membrane 10 and the second microporous base membrane 20 described above is independently applicable to the first microporous base membrane 10, the second microporous base membrane 20 and the third microporous base membrane 40 in this embodiment, and will not be repeated here. The description of any embodiment of the coating layer 30 described above is independently applicable to the first coating layer 30a and the second coating layer 30b in this embodiment, and will not be repeated here.

[0132] Preparation method of isolation film

[0133] In a second aspect, an embodiment of the present application provides a method for preparing an isolation membrane, comprising:

[0134] providing a slurry comprising lithium-rich particles;

[0135] providing a coating of the slurry between a first microporous base membrane and a second microporous base membrane;

[0136] The slurry is dried so that the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the dried coating layer is 1:(1-15) to produce the separator of the first aspect.

[0137] According to the preparation method of the present application, the isolation membrane is obtained, wherein the average particle size Dv50 of the lithium-rich particles and the thickness of the coating are within the above-mentioned ranges. During the winding process of the isolation membrane, the lithium-rich particles will not damage or pierce the first microporous base membrane and the second microporous base membrane; when the isolation membrane is in the formation and subsequent charging and discharging process, on the one hand, the lithium-rich particles are oxidatively decomposed, and the vacancies generated by the decomposition are beneficial to increase the porosity of the isolation membrane, reduce the internal resistance of the battery cell, and enhance the liquid absorption capacity and the permeability of active ions, thereby enhancing the kinetic performance of the secondary battery containing the isolation membrane; in addition, the lithium ions generated after the decomposition of the lithium-rich particles are beneficial to maintaining or restoring the capacity of the battery, and are beneficial to maintaining the lithium content of the electrode, thereby enhancing the cycle performance of the secondary battery containing the isolation membrane.

[0138] secondary batteries

[0139] Fourthly, embodiments of the present application provide a secondary battery comprising the separator of the first or second aspect, or the separator prepared by the preparation method of the third aspect. This application does not particularly limit the type of secondary battery; for example, the secondary battery may be a lithium-ion battery.

[0140] In some embodiments, a secondary battery includes a positive electrode sheet including a positive electrode active material film layer, the positive electrode active material film layer including a lithium-containing positive electrode active material; the ratio of the mass percentage W1 of the lithium-containing positive electrode active material in the positive electrode active material film layer to the mass percentage W2 of the lithium-rich particles in the coating layer is (1.01-1.5):1. In the electrode assembly of the embodiment of the present application, by controlling the ratio of W1 to W2 within the above range, during the formation of the secondary battery, the lithium ions generated by the decomposition of the lithium-rich particles can participate in the pre-lithiation of the negative electrode sheet and the formation of the SEI film, thereby reducing the consumption of lithium ions in the positive electrode active material film layer; during the formation and subsequent charge and discharge processes of the secondary battery, the lithium ions generated by the decomposition of the lithium-rich particles can replenish the lithium ions consumed by the positive electrode active material film layer during the formation and subsequent charge and discharge processes, which is beneficial to maintaining the capacity of the battery, thereby enhancing the cycle performance of the secondary battery including the separator.

[0141] In some embodiments, the ratio of the mass percentage W1 of the lithium-containing positive electrode active material in the positive electrode active material film layer to the mass percentage W3 of the lithium element in the lithium-rich particles in the coating layer is (1.34-1.82):1.

[0142] The secondary battery of the embodiment of the present application controls the ratio of W1 and W3 within the above range. When the secondary battery is formed, the lithium ions generated after the decomposition of the lithium-rich particles can participate in the pre-lithiation of the negative electrode plate and the formation of the SEI film, thereby reducing the consumption of lithium ions in the positive electrode active material film layer; during the formation and subsequent charge and discharge processes of the secondary battery, the lithium ions generated after the decomposition of the lithium-rich particles can supplement the lithium ions consumed in the positive electrode active material film layer during the formation and subsequent charge and discharge processes, which is beneficial to maintaining the capacity of the battery, thereby enhancing the cycle performance of the secondary battery containing the isolation membrane.

[0143] In some embodiments, the mass percentage W1 of the lithium-containing positive electrode active material in the positive electrode active material film layer is 70% to 95%. The mass percentage W1 of the lithium-containing positive electrode active material in the positive electrode active material film layer within the above range is beneficial to the cycle performance of the secondary battery.

[0144] In some embodiments, the secondary battery includes a positive electrode sheet and a negative electrode sheet, and the ratio of the area capacity of the positive electrode sheet to the negative electrode sheet is (1.02-1.12): 1. In some embodiments, the ratio of the area capacity of the positive electrode sheet to the negative electrode sheet can be any one of 1.03:1, 1.04:1, 1.05:1, 1.06:1, 1.07:1, 1.08:1, 1.09:1, 1.1:1, 1.11:1, and 1.12:1. In this embodiment, by designing the ratio of the area capacity of the positive electrode sheet to the negative electrode sheet to be within the above range, the ratio of the area capacity of the positive electrode sheet to the negative electrode sheet to be within the above range, when the secondary battery including the electrode assembly is formed, it helps the negative electrode sheet to achieve pre-lithiation, promotes the formation of the SEI film of the negative electrode sheet, and is beneficial to improving the cycle stability and safety of the secondary battery.

[0145] In some embodiments, the secondary battery includes a positive electrode sheet and a negative electrode sheet, and the ratio of the gram capacity of the positive electrode sheet to the negative electrode sheet is (0.45-0.72):1. In some embodiments, the ratio of the gram capacity of the positive electrode sheet to the negative electrode sheet can be any one of 0.46:1, 0.47:1, 0.48:1, 0.49:1, 0.50:1, 0.55:1, 0.60:1, 0.65:1, 0.70:1, 0.71:1, and 0.72:1. By designing the ratio of the gram capacity of the positive electrode sheet to the negative electrode sheet to be within the above range, it is helpful to combine the active ions in the positive electrode sheet with the negative electrode material in the negative electrode sheet, thereby improving the kinetic performance of the secondary battery comprising the positive electrode sheet and the negative electrode sheet.

[0146] In some embodiments, the secondary battery includes a recycled positive electrode. The recycled positive electrode is a directly recycled positive electrode from a secondary battery that has reached its service life after a long cycle. Since the capacity decay of the secondary battery includes multiple reasons such as the loss of active lithium, structural defects of the negative electrode, and structural defects of the positive electrode, in view of the high value of the positive electrode, some structurally stable positive electrode sheets are treated with the lithium-supplementing separator of the embodiment of the present application. During the formation and subsequent charge and discharge process of the secondary battery containing the electrode assembly, the lithium ions generated after the decomposition of the lithium-rich particles can replenish the lithium ions consumed by the positive electrode active material film layer in the recycled battery, which is beneficial to restoring the capacity of the battery, thereby obtaining a secondary battery with acceptable cycle performance.

[0147] In any embodiment of the present application, the secondary battery includes a recycled positive electrode sheet, and the recycled positive electrode sheet includes a positive electrode active material film layer that has been charged and discharged, and the positive electrode active material film layer includes a lithium-containing positive electrode active material. When the positive electrode sheet in the electrode assembly is a positive electrode sheet that has been charged and discharged, it can come from the positive electrode sheet in the recycled battery. Compared with the normal positive electrode sheet, the active lithium ions in the positive electrode sheet in the recycled battery have a certain lithium loss. Using the isolation membrane of the embodiment of the present application, during the formation and subsequent charge and discharge process of the secondary battery containing the electrode assembly, the lithium ions generated after the decomposition of the lithium-rich particles can supplement the lithium ions consumed by the positive electrode active material film layer in the recycled battery, which is beneficial to restore the capacity of the battery, thereby enhancing the cycle performance of the secondary battery containing the isolation membrane.

[0148] In any embodiment of the present application, the lithium-containing positive electrode active material includes a lithium iron phosphate material, and the lithium iron phosphate material includes a mixed crystal phase of LFP and FPO when discharged to 0%, and the molar ratio of the LFP crystal phase to the FPO crystal phase is 97:(3-97).

[0149] According to the embodiment of the present application, the LFP crystal phase can be Li X Fe y PO4 normal crystalline phase 0<x≤1, 0<x≤1. As an example, the LFP crystalline phase can be the crystalline phase of LiFePO4 that can normally deintercalate active lithium ions, and the FPO crystalline phase is Li X Fe y Defective crystal phase of PO4, Li-ion battery caused by the collapse of the iron-lithium structure after long cycles x Fe y PO4 cannot insert lithium normally.

[0150] In the recycled positive electrode sheet, there is a certain amount of loss of lithium elements in the lithium-containing positive electrode active material. The structural phase change of the lithium-containing positive electrode active material is within the above-mentioned range, and can be combined with the isolation membrane containing lithium-rich particles in the embodiment of the present application. The recycled positive electrode sheet can be utilized, and the isolation membrane of the embodiment of the present application is combined with the recycled positive electrode sheet, which is also beneficial to enhancing the cycle performance of the secondary battery containing the isolation membrane and the positive electrode sheet.

[0151] The molar ratio of the LFP crystalline phase to the FPO crystalline phase can be determined using commonly used methods in the art. For example, if the lithium iron phosphate material is LiFePO4, the valence state of the Fe element in the crystalline phase, which can normally deintercalate active lithium ions, is different from the valence state of the Fe element in the FPO crystalline phase. The molar ratio of the elements of different valence states can be determined by measuring the content of the elements of different valence states using inductively coupled plasma optical emission spectrometry (ICP-OES). The molar ratio of the LFP crystalline phase to the FPO crystalline phase can be determined based on the molar ratio of the elements of different valence states.

[0152] In some embodiments, the recovered positive electrode sheet comprises a charged and discharged positive electrode active material film layer, wherein the positive electrode active material film layer comprises a lithium-containing positive electrode active material; the mass percentage W1 of the lithium-containing positive electrode active material in the charged and discharged positive electrode active material film layer is 5% to 90%. The mass percentage W1 of the lithium-containing positive electrode active material in the charged and discharged positive electrode active material film layer is any one of 5%, 6%, 7%, 8%, 9%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 86%, 87%, 88%, 89%, and 90%, or a range thereof. In the positive electrode plate after charge and discharge, there is a certain amount of loss of lithium elements in the lithium-containing positive electrode active material. The mass percentage W1 of the lithium-containing positive electrode active material in the positive electrode active material film layer after charge and discharge is within the above range, which can be combined with the isolation membrane containing lithium-rich particles in the embodiment of the present application to enhance the cycle performance of the secondary battery comprising the isolation membrane and the positive electrode plate.

[0153] In some embodiments, the recovered positive electrode sheet comprises a charged and discharged positive electrode active material film layer, the positive electrode active material film layer comprising a lithium-containing positive electrode active material; the ratio of the mass percentage W1 of the lithium-containing positive electrode active material in the charged and discharged positive electrode active material film layer to the mass percentage W2 of the lithium-rich particles in the coating layer is (0.09-1.5):1. The ratio of W1 to W2 can be any one of 0.09:1, 0.1:1, 0.5:1, 0.8:1, 1.03:1, 1.04:1, 1.05:1, 1.06:1, 1.07:1, 1.08:1, 1.09:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, and 1.5:1. In the recycled positive electrode sheet, there is a certain amount of loss of lithium elements in the lithium-containing positive electrode active material. The ratio of W1 and W2 is within the above range, which can be combined with the isolation membrane of the embodiment of the present application. During the formation and subsequent charging and discharging process of the secondary battery containing the electrode assembly, the lithium ions generated after the decomposition of the lithium-rich particles in the isolation membrane can supplement the lithium ions consumed by the positive electrode active material film layer in the recycled battery, which is beneficial to restoring the battery capacity, thereby enhancing the cycle performance of the secondary battery containing the isolation membrane and the positive electrode sheet.

[0154] In some embodiments, after formation of the secondary battery, the ratio of the molar amount n1 of the lithium-containing positive electrode active material in the positive electrode active material film layer to the molar amount n2 of the lithium element in the coating layer of the lithium-rich particles is (0.2-2):1, optionally (0.2-50):1, or optionally (20-40):1. By adding lithium-rich particles, the molar amount n1 of the positive electrode active material film layer and the molar amount n2 of the lithium element therein in the coating layer are within the above range, which is beneficial for replenishing lithium in the recycled positive electrode sheets and is beneficial for the cycle performance of the secondary battery.

[0155] In a fifth aspect, an embodiment of the present application provides a method for preparing a secondary battery, the method comprising:

[0156] Provided is a separator according to the first aspect or a separator obtained by the method of the second aspect or the third aspect, the separator comprising a first microporous base membrane and a second microporous base membrane, and a coating disposed between the first microporous base membrane and the second microporous base membrane, the coating comprising lithium-rich particles, wherein a ratio of an average particle size Dv50 of the lithium-rich particles to a thickness of the coating is 1:(1-15);

[0157] A secondary battery comprising the separator and the recovered positive electrode sheet is prepared.

[0158] Compared to normal positive electrode sheets, the active lithium ions in the recovered battery's positive electrode sheets exhibit a certain amount of lithium loss. In a secondary battery produced using the preparation method of an embodiment of the present application, during the formation and subsequent charge and discharge processes of a secondary battery containing the electrode assembly, the lithium ions generated by the decomposition of the lithium-rich particles can replenish the lithium ions consumed by the positive electrode active material film layer in the recovered battery, facilitating the recovery of the battery's capacity and thereby enhancing the cycle performance of the secondary battery containing the separator.

[0159] In some embodiments, the positive electrode plate includes a lithium-containing positive electrode active material, and the ratio of the total molar amount n3 of the lithium-containing positive electrode active material in the positive electrode active material film layer to the total molar amount n4 of the lithium element in the coating layer of the lithium-rich particles is (0.2-1.5):1, and can optionally be (0.5-1.2):1. By adding lithium-rich particles, the molar amount n1 in the positive electrode active material film layer and the molar amount n2 of the lithium element therein in the coating layer are within the above range, which is beneficial for replenishing lithium in the recycled positive electrode plate and improving the cycle performance of the secondary battery.

[0160] In addition to the above technical features, the secondary battery may have related features as described below.

[0161] [Negative electrode]

[0162] The specific composition and structure of the negative electrode plate can be selected according to the type of battery cell, and the embodiments of the present application are not limited thereto.

[0163] For example, when the battery cell is a lithium-ion battery cell, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and comprising a negative electrode active material. For example, the negative electrode current collector has two opposing surfaces in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.

[0164] The negative electrode active material is a material that can extract and embed active ions (such as lithium ions, etc.), and the negative electrode active material can adopt materials well known in the art. As an example, the negative electrode active material includes but is not limited to one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate. Silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite and silicon alloy materials. Tin-based materials may include one or more of elemental tin, tin oxide and tin alloy materials. The present application is not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials may also be used.

[0165] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. The present application does not particularly limit the type of the negative electrode conductive agent. For example, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0166] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. The present application does not particularly limit the type of the negative electrode binder. As examples, the negative electrode binder may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).

[0167] In some embodiments, the negative electrode film layer may optionally include other additives. For example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC-Na), a PTC thermistor material, and the like.

[0168] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0169] The negative electrode film layer is typically formed by coating the negative electrode slurry onto the negative electrode current collector, drying it, and cold pressing it. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.

[0170] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate of the present application may further include a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector; in some embodiments, the negative electrode plate of the present application may further include a protective layer covering the surface of the negative electrode film layer.

[0171] When the battery cell is a lithium metal battery cell, the negative electrode plate may not include a negative electrode active material capable of extracting and inserting active ions. For example, in some embodiments, the negative electrode plate may include a lithium plate or a lithium alloy plate; in other embodiments, the negative electrode plate includes a mesh or foam-like three-dimensional skeleton layer, such as copper foam (or copper alloy), nickel foam (or nickel alloy), copper (or copper alloy) mesh, nickel (or nickel alloy) mesh, etc.

[0172] [Positive electrode]

[0173] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector and comprising a positive electrode active material. For example, the positive electrode current collector has two opposing surfaces in the thickness direction of the positive electrode current collector, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.

[0174] The positive electrode film layer includes a positive electrode active material, and the positive electrode active material can be a positive electrode active material for battery cells known in the art.

[0175] For example, when the battery cell is a lithium-ion battery cell or a lithium metal battery cell, the positive electrode active material may include one or more of a lithium transition metal oxide, an olivine-structured lithium-containing phosphate, and their respective modified compounds. Examples of lithium transition metal oxides may include one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of lithium phosphates containing an olivine structure may include one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds. The present application is not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials may also be used.

[0176] In some embodiments, in order to further improve the energy density of the battery cell, the positive electrode active material may include a general formula of Li a Ni b Co c M d O e A f One or more lithium transition metal oxides and modified compounds thereof. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M comprises one or more selected from Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, and B, and A comprises one or more selected from N, F, S, and Cl.

[0177] As an example, the positive electrode active material may include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.85 Co 0.15 Al 0.05 One or more of O2, LiFePO4 and LiMnPO4.

[0178] The modified compounds of the above-mentioned positive electrode active materials may be used to perform doping modification and / or surface coating modification on the positive electrode active materials.

[0179] In some embodiments, the positive electrode film layer may further include a positive electrode conductive agent. The present application does not particularly limit the type of the positive electrode conductive agent. For example, the positive electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0180] In some embodiments, the positive electrode film layer may further optionally include a positive electrode binder. This application does not particularly limit the type of positive electrode binder. As an example, the positive electrode binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.

[0181] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0182] The positive electrode film is typically formed by coating a positive electrode slurry onto a positive electrode current collector, drying it, and cold pressing it. The positive electrode slurry is typically formed by dispersing the positive electrode active material, an optional conductive agent, an optional binder, and any other components in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP).

[0183] [Preparation method]

[0184] The preparation method of the battery of the present application is well known. In some embodiments, the positive electrode sheet, the separator, the negative electrode sheet and the electrolyte can be assembled to form a secondary battery cell. As an example, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process, and the electrode assembly is placed in an outer package, and the electrolyte is injected after drying. After packaging, standing, forming, shaping and other processes, a battery cell is obtained. Multiple battery cells can also be further connected in series, in parallel or in a mixed connection to form a battery module. Multiple battery modules can also be connected in series, in parallel or in a mixed connection to form a battery pack. In some embodiments, multiple battery cells can also directly form a battery pack.

[0185] [Electrolytes]

[0186] In some embodiments, a secondary battery includes an electrolyte. The electrolyte conducts active ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte, and the electrolyte may be selected based on needs. For example, the electrolyte may be selected from at least one of a solid electrolyte and a liquid electrolyte (i.e., an electrolyte solution).

[0187] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.

[0188] The type of electrolyte salt is not specifically limited and can be selected according to actual needs. For example, the electrolyte salt includes a lithium salt selected from lithium salts used in lithium-ion batteries. As an example, the lithium salt includes one or more selected from lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP), lithium tetrafluorooxalatophosphate (LiTFOP). As an example, the sodium salt includes one or more selected from NaPF6, NaClO4, NaBCl4, NaSO3CF3, Na(CH3)C6H4SO3.

[0189] The type of solvent is not specifically limited and can be selected according to actual needs. In some embodiments, as an example, the solvent may include one or more selected from ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0190] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature power performance.

[0191] In addition, secondary batteries can have various outer packaging and existing forms.

[0192] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly including the positive electrode sheet, the negative electrode sheet, and the separator, and the electrolyte.

[0193] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0194] The present application has no particular limitation on the shape of the secondary battery, which can be a flat body, a rectangular parallelepiped, or other shapes. FIG3 shows a secondary battery 5 with a rectangular parallelepiped structure as an example.

[0195] In some embodiments, as shown in Figure 4, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate together form a accommodating cavity. The shell 51 has an opening connected to the accommodating cavity, and the cover plate 53 is used to cover the opening to close the accommodating cavity. The electrode assembly 52 of the first aspect of the embodiment of the present application or the electrode assembly 52 prepared by the method according to the second aspect of the embodiment of the present application is encapsulated in the accommodating cavity. The electrolyte is impregnated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, which can be adjusted according to demand.

[0196] The preparation method of the secondary battery of the present application is well known. In some embodiments, the electrode assembly can be placed in an outer package, dried, injected with electrolyte, and then vacuum packaged, allowed to stand, formed, and shaped to obtain a secondary battery.

[0197] In some embodiments, the secondary battery can be assembled into any one or more of a battery cell, a battery module, or a battery pack.

[0198] In some embodiments of the present application, the secondary batteries according to the present application can be assembled into a battery module. The battery module can contain multiple secondary batteries, and the specific number can be adjusted according to the application and capacity of the battery module.

[0199] Optionally, the battery module may further include a housing having an accommodation space, and the plurality of secondary batteries are accommodated in the accommodation space.

[0200] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0201] In some embodiments, secondary batteries can be assembled into battery cells, which can be assembled into battery modules, which can be assembled into battery packs.

[0202] In some embodiments, secondary batteries may be assembled into battery cells, and the battery cells may be assembled into a battery pack.

[0203] Electrical devices

[0204] In a sixth aspect, the present invention provides an electric device, including the secondary battery of the fifth aspect. The present invention provides an electric device, which may include at least one of the above-mentioned battery cells, battery modules and battery packs.

[0205] By controlling the average particle size Dv50 of the lithium-rich particles in the isolation membrane and the thickness of the coating within the above-mentioned range, the porosity of the isolation membrane can be increased, the ionic resistance can be reduced, and the kinetic performance and cycle performance of the secondary battery can be enhanced. Under the combined influence of many properties such as the thermal shrinkage and permeability of the isolation membrane, the thermal stability and safety of the battery cell, the lithium-ion secondary battery and electrical device containing the isolation membrane of the present application can obtain excellent performance.

[0206] Secondary batteries can be used as power sources or energy storage units for electrical devices. These devices include, but are not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, and energy storage systems.

[0207] Figure 5 is a schematic diagram of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.

[0208] As another example, the electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a secondary battery as a power source.

[0209] Example

[0210] The following examples describe the present disclosure in more detail. These examples are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are commercially available.

[0211] Example 1

[0212] Preparation of isolation membrane

[0213] The first microporous base membrane and the second microporous base membrane were made by cutting commercial 5μm PE base membrane and 6μm PP base membrane purchased from Ningde Zhuogao New Material Technology Co., Ltd., and the porosity thereof was 30%.

[0214] Preparation of coating film:

[0215] Lithium oxalate, aluminum oxide, polyacrylate, and carboxymethyl cellulose were mixed in a solvent (deionized water) at a mass ratio of 2.5:6.5:0.5:0.5 to form an aqueous slurry with a solid content of 25 wt% and a viscosity of 100 mPa·s. The lithium-replenishing slurry was then coated onto a 5 μm polyethylene (PE) film using a coating machine. A separate unwinding roll was used for a 6 μm polypropylene (PP) film. The slurry was extruded onto one surface of the PE film to form a wet coating approximately 15 μm thick. The film was then transferred to an oven and dried at 60°C for 2 minutes. The rolls were then reversed and the PP film was pressed onto the wet coating at a pressure of 1000 MPa to produce a composite separator.

[0216] Preparation of positive electrode

[0217] It uses a 60Ah LFP square hard-shell battery cell from CATL. The positive LFP pole piece, which is fully discharged after 3,000 cycles, contains lithium iron phosphate positive active material with the structural formula LiFePO4.

[0218] Preparation of negative electrode sheet

[0219] 97.5 parts by weight of artificial graphite as the negative electrode active material, 1.5 parts by weight of SBR as the binder, and 1 part by weight of CMC-Na as the thickener were added to deionized water, stirred and mixed evenly, and then coated on the surface of Cu foil. After drying, cold pressing, and stripping, the negative electrode sheet was obtained.

[0220] Preparation of electrolyte

[0221] 11.9 parts by weight of lithium hexafluorophosphate were added to 88.1 parts by weight of a solution of EC and DEC (mass ratio of 1:1), and the mixture was stirred uniformly to fully dissolve, thereby obtaining an electrolyte solution.

[0222] Preparation of lithium-ion secondary batteries

[0223] The positive electrode sheet, separator and negative electrode sheet obtained above are assembled into a laminated bare cell, placed in an aluminum-plastic film, vacuum-baked at 80°C for 8 hours, injected with the above-mentioned electrolytic solution for infiltration and activation, thereby completing the preparation of the lithium-ion secondary battery.

[0224] Examples 2 to 14

[0225] The preparation method was similar to that of Example 1, except that the content and type of lithium-rich particles, as well as the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating were different, as shown in Table 1. When the content of the lithium-rich particles varied, the content of alumina in the coating was adjusted so that the sum of the content of the lithium-rich particles and alumina in the coating was 90%.

[0226] Example 15

[0227] The difference between this embodiment and embodiment 1 lies in the preparation of the positive electrode plate, wherein the positive electrode active material is LiFePO4, and the positive electrode plate is a freshly prepared positive electrode plate.

[0228] 94 parts by weight of lithium iron phosphate (LiFePO4), a positive electrode active material, 3 parts by weight of conductive carbon, and 3 parts by weight of PVDF, a binder, were added to the solvent NMP, stirred and mixed evenly, and then coated on the surface of Al foil. After drying, cold pressing, and slitting, the positive electrode sheet was obtained, as shown in Table 4.

[0229] Examples 16-24

[0230] This embodiment differs from Example 1 in that, during the preparation process before formation of the secondary battery, the ratio of the total amount of lithium-rich particles in the coating to the total amount of positive electrode active material in the positive electrode active material film layer is controlled, as shown in Table 3.

[0231] Comparative Example 1

[0232] This comparative example provides a two-layer composite separator using a 5μm thick PE microporous film and a 6μm thick PP microporous film as the substrate layers. Polycarbosilane (PCS) was sprayed onto one side of the 5μm thick PE surface to produce a polymer coating at a rate of 0.5mg / m². To ensure consistency with the examples, the separator was baked at 60°C for 2 minutes and then pressed against the PP base film on the other side at a pressure of 1 MPa to produce a coated composite separator free of lithium-rich particles.

[0233] Comparative Example 2

[0234] The preparation method is similar to that of Example 1, except that there are no lithium-rich particles and the particles are partially supplemented by alumina.

[0235] Comparative Examples 3-6

[0236] The difference from Example 1 is that, before the secondary battery is formed, the ratio of the total amount of the lithium-rich particles in the coating to the total amount of the positive electrode active material in the positive electrode active material film layer is controlled during the preparation process, as shown in Table 3.

[0237] Test section

[0238] 1) Test method for average particle size Dv50, Dv90, and Dv99 of lithium-rich particles: The particle size distribution of lithium-rich particles is measured using a laser particle size analyzer according to GB / T 19077-2016. The procedure is as follows: Place an appropriate amount of the sample to be tested in a clean beaker, add a surfactant dropwise, and then add a dispersant. The beaker is operated at a speed exceeding 120W / 5 minutes to ensure complete dispersion of the sample in the dispersant. The sample is then poured into the injection tower and circulated with the solution into the test optical system. The particles are illuminated by a laser beam, and the energy distribution of the scattered light is measured to determine the particle size distribution (shading: 8-12%).

[0239] 2) Test method for isolation film and coating thickness: Use a thickness gauge to test according to GB / T6672-2001 Film and Sheet Thickness Determination Method; First, the thickness of the isolation film base film is defined as W1, and the thickness of the coating film after coating is defined as W1. The coating thickness W3 = W1-W2.

[0240] 3) Thermal Shrinkage Test Method for Isolator Films: Cut the film into 100 x 50 mm pieces and place it in an oven at 130°C for 1 hour. Use a vernier caliper to measure the shrinkage of the film in the longitudinal direction (MD) and transverse direction (TD). The film of the example was subjected to the above test, and its structure is shown in Table 2.

[0241] 4) Separator Tensile Strength Test Method: Separator films were cut in both the MD and TD directions to obtain multiple 15 mm x 50 mm samples. These samples were stretched using a tensile machine until they broke, and the tensile strength of the samples was recorded. Separator films from the examples were subjected to the aforementioned tests, and their structures are shown in Table 2.

[0242] 5) Test Method for Liquid Absorption of Isolator Membrane: Cut the isolator membrane sample into a 5cm x 5cm square and weigh it. Then, soak the isolator membrane in electrolyte for 30 minutes, remove it, gently blot the electrolyte on the membrane surface with a dust-free paper, and weigh it. The electrolyte used was a 1 mol / L LiPF6 ethylene carbonate (EC) solution. Liquid Absorption = (Weight after Soaking - Weight Before Soaking) / Weight Before Soaking × 100%. The isolator membrane of the embodiment was subjected to the above test, and its structure is shown in Table 2.

[0243] 6) Air Permeability Test Method for Separator Membranes: The air permeability of the separator membranes was tested using a Gurley 4110N air permeability tester. The test method measured the time required for 100cc of air to pass through a 3cm diameter circular separator membrane at a pressure of 4.88 inches of water column (in seconds). Separator membranes from the examples were subjected to the above test, and their structures are shown in Table 2.

[0244] 7) Test method for the surface density of the isolation film: Cut the isolation film into a circle with a radius R of 50 mm, weigh it using an electronic balance, and then calculate its surface density. The isolation film of the embodiment was subjected to the above test, and its structure is shown in Table 2.

[0245] 8) The method for detecting the amount of Li element in the separator coating of lithium-rich particles includes: washing the separator coating, mixing and grinding the material to be tested with conductive carbon and PVDF in a mass ratio of 8:1:1, preparing a positive electrode slurry, coating it on aluminum foil, and assembling it with a Li sheet into a button half-cell. By charging and discharging the button half-cell assembled with the positive electrode lithium-rich material to be tested, measuring the battery's capacity and discharge time, the charge of the positive electrode active material in a single cell is calculated, Q = It, where Q is the charge of the active material, I is the current intensity, and t is the discharge time. According to the stoichiometric relationship of the electrochemical equation, the charge of the active material is converted to the amount of the active material, thereby calculating the content of the active material, such as n = Q / FM, where n is the amount of active material, F is the Faraday constant, and M is the relative molecular mass of the active material.

[0246] 9) The method for detecting the amount of Li substance in the positive electrode active material is similar to that of the lithium-rich coating material.

[0247] 10) Capacity recovery rate calibration and initial coulombic efficiency test method for secondary batteries: Place an unactivated battery in the test channel of a Chenhua electrochemical workstation and charge it at a constant current rate of 0.1C to a charge cut-off voltage of 3.65V. After standing for 5 minutes, discharge it at a constant current rate of 1C to a discharge cut-off voltage of 2.25V. Discharge capacity / charge capacity = initial coulombic efficiency. Then charge it at a constant current rate of 0.1C to a charge cut-off voltage of 3.65V. Record the reversible battery capacity after activation. The capacity recovery rate is the final discharge capacity of the secondary battery before the positive electrode sheet is disassembled / the discharge capacity of the secondary battery with the positive electrode sheet newly assembled.

[0248] 11) Testing of the kinetic performance of secondary batteries: Constant-voltage AC impedance spectroscopy (CES) was performed on the separator using a Chenhua electrochemical workstation. The intercept of the impedance curve on the Nyquist plot, where the real part intersects with the real part, was taken as Rs. Ionic conductivity was then determined by comparing the Rs parameter with that of a known standard conductivity sample.

[0249] 12) Test method for the cycling performance of secondary batteries: Place the battery in the test channel of a Chenhua electrochemical workstation and charge it at a constant current rate of 1C to a charge cut-off voltage of 3.65V. After 5 minutes of rest, discharge it at a constant current rate of 1C to a discharge cut-off voltage of 2.25V. Record the discharge capacity and let it rest for another 5 minutes. Repeat this cycle. Cycle capacity retention = capacity after cycle / capacity after first cycle × 100%. This is generally the ratio of the capacity after 500 cycles to the capacity after first cycle.

[0250] Based on the test results of Examples 1-14, it can be seen that under the lithium replenishment condition where the ratio of the amount of lithium-rich material Li to the amount of LFP material is 1:1, the old positive electrode sheet is successfully activated and can achieve a capacity retention rate of 94% after 500 cycles, which proves that the structure of the LFP positive electrode sheet is relatively stable under long cycles, and the waste positive electrode can be recycled through lithium replenishment of the diaphragm.

[0251] From the test results in Table 1, it can be seen that when the separator is wound or even mechanically squeezed, the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating is within the above range, and the lithium-rich particles will not damage or pierce the first microporous base membrane and the second microporous base membrane, which is beneficial to improving the safety performance of the secondary battery containing the separator. The separator includes a coating containing lithium-rich particles. During the charge and discharge process of the battery containing the separator, the lithium-rich particles gradually reach the decomposition voltage under the action of the electrolyte and decompose. The vacancies generated by the decomposition are beneficial to increasing the porosity of the separator, enhancing the liquid absorption capacity of the separator and the permeability of active ions, reducing the internal resistance of the battery cell, and enhancing the dynamic performance of the secondary battery containing the separator. In addition, the lithium ions generated after the decomposition of the lithium-rich particles are beneficial to maintaining or restoring the capacity of the battery and maintaining the lithium content of the electrode, thereby enhancing the cycle performance of the secondary battery containing the separator.

[0252] According to Table 1, compared with Comparative Example 1-2, Example 1-6 consumes a large amount of lithium salt in the electrolyte, resulting in an increase in the internal resistance of the battery and a deterioration in the cycle. As the amount of lithium replenished in the examples increases, the first coulombic efficiency gradually increases. Since the lithium-rich particles not only replenish lithium for the positive electrode sheet, but also supplement the active lithium ions consumed in the formation of the SEI film, it is possible to recover the positive electrode sheet while pre-lithiating the negative electrode.

[0253] According to Table 1, compared with Comparative Examples 1-2, Examples 7-10 have different decomposition effects due to different decomposition voltages of different lithium-rich particles. However, all of them improve the first efficiency and ionic conductivity while supplementing lithium to the positive electrode.

[0254] According to Table 1, compared with Comparative Examples 1-2, Examples 11-14 have lithium-rich coatings with different thicknesses and aluminum oxide contents. Under the same capacity recovery effect, the thinner the coating, the higher the ionic conductivity, which is beneficial to the long cycle performance of the battery.

[0255] The results of Comparative Examples 1-2 in Table 1 show that the positive electrode sheets in Comparative Examples 1-2 were recycled and lacked lithium. When directly assembled into secondary batteries using conventional separators, they failed to charge properly. Table 2 shows that, compared to Comparative Examples 1-2, the separators coated with aluminum oxide in Examples 1-6 exhibited improved heat resistance, mechanical properties, and electrolyte affinity.

[0256] According to Table 2, compared with Comparative Examples 1-2, the diaphragms in Examples 7-10 whose lithium-rich particles are lithium silicide (Li2Si) have better air permeability, corresponding to the high ionic conductivity in Table 1, thanks to their lower decomposition voltage and pore-forming effect.

[0257] According to Table 2, compared with Comparative Examples 1-2, the increase in coating thickness in Examples 11-14 is beneficial to improving the mechanical strength of the isolation membrane.

[0258] The ratio of the total amount of Li element in the coating of the lithium-rich particles to the total amount of the positive electrode active material in the positive electrode active material film layer in Tables 2 and 3 was measured before the battery was formed. In Table 3, in the Examples, before the secondary battery was formed, the ratio of the total amount of Li element in the coating of the lithium-rich particles to the total amount of the positive electrode active material in the positive electrode active material film layer was between (0.2-2):1, and the resulting battery capacity met the requirements. However, in Comparative Examples 3-6, the ratio of the amount of material was larger, and the resulting battery capacity did not meet the requirements, such as 500 cycles / 7% SOC, or caused a short circuit.

[0259] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and within the scope of the technical solution of the present application, embodiments having substantially the same structure as the technical concept and performing the same function are all included in the technical scope of the present application. In addition, without departing from the scope of the subject matter of the present application, other methods of constructing the embodiments by applying various modifications that can be conceived by those skilled in the art and combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A separation film, comprising: The first microporous base membrane, a second microporous base membrane, and A coating layer is disposed between the first microporous base membrane and the second microporous base membrane, wherein the coating layer contains lithium-rich particles, wherein the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating layer is 1:(1-15).

2. The isolation film according to claim 1, wherein: The ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating is 1:(1.5-10).

3. The isolation film according to claim 1 or 2, wherein: The average particle size Dv50 of the lithium-rich particles is 0.2 μm to 3 μm, and can be 0.25 μm to 1 μm; and / or, The average particle size Dv90 of the lithium-rich particles is 0.5 μm to 5 μm, and can be 0.5 μm to 2.0 μm; and / or, The average particle size Dv99 of the lithium-rich particles is 1 μm to 20 μm; and / or, The mass percentage of the lithium-rich particles in the coating is 10% to 80%, and optionally 25% to 75%.

4. The isolation film according to any one of claims 1 to 3, wherein: The lithium-rich particles contain a lithium salt or a lithium-containing composite oxide having a layered structure, a spinel structure or an olivine structure; and / or, The lithium-rich particles include Li2C2O4, LiOH, Li 15 One or more of Si4, Li4Sn.

5. The isolation film according to any one of claims 1 to 4, wherein: The lithium-rich particles have a core-shell structure, wherein the core comprises a lithium salt or a lithium-containing composite oxide having a layered structure; and the shell comprises one or more of carbon and silicon oxide.

6. The isolation film according to claim 4 or 5, wherein: The lithium salt or lithium-containing composite oxide having a layered structure includes Li x MO y , Li x [M b A d ]O y One or more of the following: M includes one or more of Mn, Co, and Ni metals; A includes one or more of Al, Fe, V, Mg, Ca, Sr, and Ga elements; x is 0.8 to 2.2; y is 1.8 to 3.2; b>0; d>0; and b+d=1.

7. The isolation film according to any one of claims 1 to 7, wherein: The isolation film satisfies at least one of the following conditions: The first microporous base membrane and the second microporous base membrane respectively include one or more of a polyolefin membrane, a non-woven fabric membrane, a polyester membrane, a polyether membrane, a polyetherimide membrane, and a fluorinated polyetherimide membrane; The thickness of the first microporous base membrane and the second microporous base membrane are respectively 3 μm to 20 μm; The porosity of the first microporous base membrane and the second microporous base membrane is 30% to 70% respectively; The coating has a thickness of 0.5 μm to 20 μm; The coating includes a binder and ceramic particles.

8. The isolation film according to claim 7, wherein: The average particle size Dv50 of the ceramic particles is 0.2 μm to 6 μm; and / or, The ceramic particles have a mass content of 20% to 60% in the coating.

9. The isolation film according to claim 7 or 8, wherein: The binder has a mass content of 10% to 20% in the coating.

10. The isolation film according to any one of claims 1 to 9, wherein: The isolation film satisfies at least one of the following conditions: The porosity of the isolation membrane is 25% to 65%; Under the condition of testing at 130° C. for 1 hour, the thermal shrinkage of the isolation film in the longitudinal direction (MD) is ≤5.0%, and the thermal shrinkage in the width direction (TD) is ≤5.0%; The air permeability of the isolation film is 300s / 100cc to 500s / 100cc; The transverse direction (TD) tensile strength of the separator is 1000 kg / cm 2 Up to 2000kg / cm 2 ; The longitudinal tensile strength of the separator is 1200 kg / cm 2 Up to 1800kg / cm 2 .

11. A separation film comprising: a first microporous base membrane and a second microporous base membrane, a first coating layer disposed between the first microporous base membrane and the second microporous base membrane, A third microporous base membrane is disposed on a side of the second microporous base membrane away from the first microporous base membrane; as well as A second coating layer disposed between the second microporous base membrane and the third microporous base membrane; Wherein, the first coating and / or the second coating contains lithium-rich particles, wherein the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating is 1:(1-15), and can be optionally 1:(1.5-10).

12. A method for preparing an isolation film, comprising: providing a slurry comprising lithium-rich particles; providing a coating of the slurry between a first microporous base membrane and a second microporous base membrane; The slurry is dried so that the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the dried coating is 1:(1-15), thereby obtaining the isolation film according to any one of claims 1-9.

13. A secondary battery comprising the separator according to any one of claims 1 to 10 or the separator prepared by the preparation method according to claim 11 or 12.

14. The secondary battery according to claim 13, wherein The positive electrode sheet includes a recycled positive electrode sheet, wherein the recycled positive electrode sheet comprises a charged and discharged positive electrode active material film layer, wherein the positive electrode active material film layer comprises a lithium-containing positive electrode active material.

15. The secondary battery according to claim 14, wherein The lithium-containing positive electrode active material includes lithium iron phosphate material. The capacity of the secondary battery, when discharged to 0%, includes a mixed crystal phase of LFP and FPO, and the molar ratio of the LFP crystal phase to the FPO crystal phase is 97:(3-97).

16. The secondary battery according to any one of claims 13 to 15, wherein: After the secondary battery is formed, the ratio of the molar amount n1 of the lithium-containing positive electrode active material in the positive electrode active material film layer to the molar amount n2 of the lithium element in the lithium-rich particles in the coating layer is (0.2-50):1, and can be optionally (20-40):

1.

17. A method for preparing a secondary battery, the method comprising: Provided is an isolation membrane according to any one of claims 1 to 11 or an isolation membrane obtained by the preparation method according to claim 11 or 12, wherein the isolation membrane comprises a first microporous base membrane and a second microporous base membrane and a coating disposed between the first microporous base membrane and the second microporous base membrane, the coating comprising lithium-rich particles, wherein the ratio of the average particle size Dv50 of the lithium-rich particles to the thickness of the coating is 1:(1-15); A secondary battery comprising the separator and the recovered positive electrode sheet is prepared.

18. The preparation method according to claim 17, wherein: The positive electrode plate includes a lithium-containing positive electrode active material, and the ratio of the total molar amount n3 of the lithium-containing positive electrode active material in the positive electrode active material film layer to the total molar amount n4 of the lithium element in the lithium-rich particles in the coating is (0.2-1.5):1, which can be optionally (0.5-1.2):

1.

19. An electrical device comprising the secondary battery according to any one of claims 13 to 16 or the secondary battery prepared by the preparation method according to claim 17 or 18.

Citation Information

Patent Citations

  • Battery diaphragm, preparation method of battery diaphragm, and lithium ion battery

    CN109428034A

  • Novel lithium battery isolation film and lithium ion battery including isolation film

    CN110085792A

  • Lithium-supplementing functional electrolyte membrane for solid-state lithium battery

    CN113764667A

  • Preparation method of lithium-supplementing functional electrolyte membrane for solid-state lithium battery

    CN113782823A

  • Lithium-supplementing composite isolating membrane as well as preparation method and application thereof

    CN115051109A

Cited By

  • Water-based lithium-supplementing diaphragm and preparation method and application thereof

    CN119905772A