Composite water-based binder and preparation method therefor, and lithium-ion battery
By combining PAA water-based binder with organic lithium, a composite water-based binder with high adhesion and low swelling properties is solved, and the problems of low adhesion and poor flexibility in lithium-ion batteries are improved, and the first charging of the battery is improved Discharge efficiency.
Patent Information
- Application Number
- PCT/CN2023/141495
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2023-12-25
- Publication Date
- 2024-11-28
AI Technical Summary
The adhesives in existing lithium-ion batteries have low adhesion, poor flexibility and low conductivity during charging and discharging, resulting in an increase in lithium ion loss and affecting the battery's first charging and discharging efficiency.
A composite water-based binder is used to combine PAA water-based binder with organic lithium to form a binder with high bonding force, good flexibility and low swelling, reducing lithium ion losses.
The bonding force and flexibility of the negative electrode adhesive of lithium-ion battery is improved, the loss of lithium ions during the charging and discharging process is reduced, and the first charging and discharging efficiency of the battery is improved.
Smart Images

Figure CN2023141495_28112024_PF_FP_ABST
Abstract
Description
Composite water-based binder, preparation method thereof, and lithium-ion battery
[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on May 22, 2023, with application number 202310587986.6 and application name “A composite aqueous binder, its preparation method and lithium-ion battery”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present invention belongs to the technical field of water-based binders, and in particular relates to a composite water-based binder, a preparation method thereof, and a lithium-ion battery. Background Art
[0003] Lithium-ion batteries, as secondary batteries, are widely used in various fields due to their advantages, including high energy conversion rate, high energy density, high charge and discharge rate, no memory effect, and environmental friendliness. Polymer binders, with their excellent bonding properties, can bind various particles together and tightly bond them to the current collector, making them an indispensable component of lithium-ion batteries. In addition to high adhesion, high-performance binders also require the following properties: good flexibility, electrolyte resistance, compactness, chemical and electrochemical stability, low cost, and environmental friendliness.
[0004] Currently, industrial binders used in lithium-ion batteries fall into three main categories: polyvinylidene fluoride (PVDF), styrene-butadiene rubber latex and carboxymethyl cellulose (SBR / CMC), and polyacrylic acid (PAA). All of these have promising applications in lithium-ion batteries. PAA, with its strong adhesion, excellent stability, low cost, and environmental friendliness, is a hot topic in negative electrode binder research.
[0005] Commonly used negative electrode graphite materials have good processing properties and high-temperature stability, but their capacity is relatively low. During the charge and discharge process of lithium-ion batteries, graphite particles also easily absorb lithium ions, resulting in a decrease in the battery's initial charge and discharge efficiency.
[0006] Therefore, in this field, developing a binder with better performance to improve the initial charge and discharge efficiency of lithium-ion batteries while ensuring adhesion, electrochemical stability, flexibility, etc. is a research focus in this field.
[0007] Summary of the Invention
[0008] To address the shortcomings of the prior art, the present invention provides a composite water-based binder, a preparation method thereof, and a lithium-ion battery. The composite water-based binder of the present invention is a PAA water-based binder with high bonding strength, good flexibility, and low swelling. It also reduces lithium ion loss during charge and discharge, allowing the binder to play a greater role in lithium-ion batteries.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In one aspect, the present invention provides a composite aqueous binder comprising a PAA aqueous binder represented by Formula I and organic lithium;
[0011] wherein R1 is hydrogen or methyl; R2 is C1-C12 (e.g., C1, C2, C3, C4, C5, C6, C7, C8, C9, C10, C11, or C12) alkyl; x = 100-4300 (e.g., 105, 407, 800, 1204, 1636, 2270, 2400, 2800, 3200, 3600, 4083, or 4300 ), y=an integer from 100 to 4000 (e.g., 100, 401, 805, 1211, 1646, 2000, 2400, 2838, 3205, 3606, 4000), and z=an integer from 10 to 750 (e.g., 10, 55, 90, 150, 204, 307, 400, 500, 623, 650, 702, or 750).
[0012] In the present invention, the PAA aqueous binder of the structure is compounded with organic lithium to obtain a composite aqueous binder having high bonding strength, good flexibility and low swelling, thereby reducing the loss of lithium ions during the charge and discharge process, and allowing the binder to play a greater role in lithium-ion batteries.
[0013] Preferably, the weight-average molecular weight of the PAA aqueous binder represented by Formula I is 50,000 to 500,000, for example, 50,000, 100,000, 150,000, 200,000, 250,000, 300,000, 350,000, 400,000, 450,000, or 500,000. In the present invention, if the weight-average molecular weight of the PAA aqueous binder is less than 50,000, the solvent resistance of the adhesive may be affected. If the weight-average molecular weight of the PAA aqueous binder is greater than 500,000, the adhesive performance may be affected.
[0014] Preferably, the monomers for preparing the PAA aqueous binder represented by Formula I include acrylate monomers and styrene monomers;
[0015] Preferably, the acrylic acid ester monomer includes any one or a combination of at least two of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, isopropyl methacrylate, butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, isobornyl methacrylate, n-octyl acrylate, isooctyl acrylate, lauric acid acrylate, 2-ethylhexyl acrylate, hexyl methacrylate or vinyl acetate.
[0016] Preferably, the preparation method of the PAA aqueous binder represented by Formula I comprises the following steps:
[0017] (1) adding acrylate monomer, styrene monomer and persulfate initiator to an emulsifier aqueous solution, mixing, and causing polymerization reaction to obtain a polyacrylate copolymer emulsion;
[0018] (2) adding an alkaline compound to the polyacrylate copolymer emulsion obtained in step (1) to adjust the pH of the reaction system to 7 to 10 (e.g., 7, 7.5, 8, 8.5, 9, 9.5 or 10) to obtain the PAA aqueous binder.
[0019] Preferably, the emulsifier in step (1) is selected from any one of allyloxy fatty alcohol polyoxyethylene ether ammonium sulfate, sodium allyl hydroxypropyl sulfonate, sodium lauryl sulfate, sodium dodecylphenyl cyclate or disodium succinate polyoxyethylene ether monoester sulfonate or a combination of at least two thereof.
[0020] Preferably, the mass percentage concentration of the emulsifier in the emulsifier aqueous solution in step (1) is 0.05%-10%, for example, 0.05%, 0.08%, 0.1%, 0.5%, 1%, 2%, 3%, 5%, 7%, 9% or 10%.
[0021] Preferably, the molar ratio of the acrylate monomer to the styrene monomer in step (1) is 1:0.1-2, for example, 1:0.1, 1:0.3, 1:0.5, 1:0.7, 1:1, 1:1.3, 1:1.5, 1:1.8 or 1:2.
[0022] Preferably, the persulfate initiator in step (1) is selected from any one of potassium persulfate, ammonium persulfate or sodium persulfate, or a combination of at least two thereof.
[0023] Preferably, the polymerization reaction temperature in step (1) is 35-100° C. (e.g., 35° C., 38° C., 40° C., 50° C., 60° C., 70° C., 80° C., 90° C., or 100° C.), and the polymerization reaction time is 2.5-12 hours (e.g., 2.5 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, or 12 hours). In the present invention, at a relatively high temperature (60-100° C.), the persulfate decomposes into free radicals and introduces free radicals into the micelles, thereby initiating the polymerization of the acrylate to form a polyacrylate copolymer emulsion.
[0024] Preferably, the alkaline compound in step (2) is selected from any one or a combination of at least two of ammonia water, sodium hydroxide, potassium hydroxide or lithium hydroxide.
[0025] In the present invention, since the acidity of the reaction system after the reaction is relatively strong, which may have an adverse effect on the performance of the lithium-ion battery, it is necessary to adjust the pH value of the reaction system.
[0026] In the present invention, the solid content of the PAA aqueous binder is 10%-60%, for example, 10%, 15%, 18%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%.
[0027] Preferably, the organic lithium is selected from one or a combination of at least two of lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium trifluoromethanesulfonate, lithium bis(difluorosulfonylimide), and lithium bis(trifluoromethanesulfonylimide).
[0028] Preferably, the composite aqueous binder comprises 90-100 parts (e.g., 90 parts, 93 parts, 95 parts, 97 parts, 99 parts or 100 parts) of the PAA aqueous binder represented by Formula I and 0.1-10 parts (e.g., 0.1 parts, 0.5 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts) of organolithium, in parts by weight.
[0029] In the present invention, if the amount of the PAA aqueous binder represented by Formula I in the composite aqueous binder is less than 90 parts, optimal adhesion cannot be provided. If the amount of the PAA aqueous binder represented by Formula I in the composite aqueous binder is greater than 100 parts, the effect of the organic lithium cannot be significantly manifested.
[0030] In the present invention, if the amount of organic lithium in the composite aqueous adhesive is less than 0.1 parts, its function cannot be well demonstrated. If the amount of organic lithium is greater than 10 parts, the bonding ability of the adhesive will be reduced.
[0031] In another aspect, the present invention provides a method for preparing the composite water-based binder as described above, the method comprising the following steps:
[0032] The PAA aqueous binder represented by formula I and organic lithium are mixed to obtain the composite aqueous binder.
[0033] Preferably, the mixing is performed under stirring.
[0034] Preferably, the stirring speed is 100-500 rpm, for example, 100 rpm, 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm or 500 rpm.
[0035] Preferably, the mixing is carried out at a temperature of 5-55°C (e.g. 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C or 55°C).
[0036] Preferably, the mixing time is more than 10 min, for example, 10 min, 15 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min or 100 min.
[0037] In another aspect, the present invention provides a negative electrode plate for a lithium ion battery, comprising the composite aqueous binder as described above.
[0038] In another aspect, the present invention provides a lithium-ion battery, comprising the lithium-ion battery negative electrode sheet as described above.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] In the present invention, the PAA aqueous binder with the structure is compounded with organic lithium to obtain a composite aqueous binder having high bonding strength, good flexibility and low swelling properties, thereby solving the problems of low bonding strength, poor flexibility and low conductivity currently encountered in binders used for negative electrodes of lithium-ion batteries. In addition, the loss of lithium ions during the charge and discharge process is reduced, allowing the binder to play a greater role in lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] FIG1 is an infrared spectrum of the PAA aqueous binder prepared in Preparation Example 1.
[0042] FIG2 is a gel permeation chromatogram of the PAA aqueous binder prepared in Preparation Example 1. DETAILED DESCRIPTION
[0043] The technical solution of the present invention is further described below by way of specific embodiments. It should be understood by those skilled in the art that the embodiments are merely to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0044] Preparation Example 1
[0045] This preparation example provides the preparation of a PAA aqueous binder represented by Formula I, which specifically includes the following steps:
[0046] (1) First, dissolve 1.875 g of sodium allyl hydroxypropyl sulfonate in 375 mL of water and stir thoroughly to obtain a transparent emulsifier aqueous solution;
[0047] (2) adding 4 g of methacrylic acid, 28.5 g of isopropyl methacrylate, 25 g of butyl acrylate, 42.5 g of styrene monomer, and 0.6 g of ammonium persulfate initiator to the above-mentioned emulsifier aqueous solution, stirring and mixing uniformly, and then heating to 65° C. to initiate polyacrylate emulsion polymerization for 11 h to form a polyacrylate copolymer emulsion;
[0048] (3) NaOH was added to the polyacrylate copolymer emulsion to adjust the pH of the reaction system to 7.5 to obtain the PAA aqueous binder.
[0049] The prepared PAA binder was characterized by infrared spectroscopy (Tianjin Gangdong Technology Co., Ltd., FTIR-650S), and the results are shown in Figure 1. -1 、2871cm -1 The stretching vibration peak of the methyl group (-CH3) is at 1727cm -1 The characteristic peak of ester group is at 1493cm -1 、1452cm -1 , 760cm -1 、699cm -1 It is the characteristic peak of benzene ring, indicating that we have successfully synthesized PAA binder.
[0050] The molecular weight of the PAA adhesive was characterized by gel permeation chromatography (GPC). The characterization results are shown in FIG2 . The weight average molecular weight of the PAA adhesive of this embodiment is 178,000.
[0051] Preparation Example 2
[0052] (1) First, dissolve 12 g of allyloxy fatty alcohol polyoxyethylene ether ammonium sulfate in 600 mL of water and stir thoroughly to obtain a transparent emulsifier aqueous solution;
[0053] (2) adding 30 g of ethyl acrylate, 8 g of acrylic acid, 25.9 g of isooctyl acrylate, 36.1 g of styrene monomer, and 0.6 g of ammonium persulfate initiator to the above-mentioned emulsifier aqueous solution, stirring and mixing uniformly, and then heating to 75° C. to initiate polyacrylate emulsion polymerization for 8 hours to form a polyacrylate copolymer emulsion;
[0054] (3) LiOH was added to the polyacrylate copolymer emulsion to adjust the pH of the reaction system to 7.5, thereby obtaining the PAA aqueous binder.
[0055] Gel permeation chromatography analysis showed that the weight average molecular weight of the PAA aqueous binder obtained in this example was 390,400.
[0056] Preparation Example 3
[0057] (1) First, dissolve 50g of disodium succinate polyoxyethylene ether sulfonate in 1000mL of water and stir thoroughly to obtain a transparent emulsifier aqueous solution;
[0058] (2) adding 27 g of vinyl acetate, 36 g of lauric acid acrylate, 37 g of styrene monomer and 0.6 g of ammonium persulfate initiator to the above-mentioned emulsifier aqueous solution, stirring and mixing uniformly, and then heating to 85° C. to initiate polyacrylate emulsion polymerization for 6 hours to form a polyacrylate copolymer emulsion;
[0059] (3) Adding ammonia water to the polyacrylate copolymer emulsion to adjust the pH of the reaction system to 9 to obtain the PAA aqueous binder.
[0060] Gel permeation chromatography analysis showed that the weight average molecular weight of the PAA aqueous binder obtained in this example was 62,100.
[0061] Example 1
[0062] At a temperature of 20° C., 100 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by addition of 1 part of lithium bis(trifluoromethanesulfonyl)imide, and the mixture was stirred evenly for 30 minutes to obtain a composite water-based binder.
[0063] Example 2
[0064] At a temperature of 10° C., 100 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by 3 parts of lithium bis(trifluoromethanesulfonyl)imide. The mixture was stirred evenly for 30 minutes to obtain a composite water-based binder.
[0065] Example 3
[0066] At a temperature of 20° C., 100 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by 5 parts of lithium bis(trifluoromethanesulfonyl)imide. The mixture was stirred evenly for 30 minutes to obtain a composite water-based binder.
[0067] Example 4
[0068] At a temperature of 15° C., 95 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by 3 parts of lithium bis(oxalatoborate) and stirred evenly for 1 hour to obtain a composite water-based binder.
[0069] Example 5
[0070] At a temperature of 25° C., 92 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by 7 parts of lithium difluorooxalatoborate. The mixture was stirred evenly for 45 minutes to obtain a composite water-based binder.
[0071] Example 6
[0072] At a temperature of 30° C., 100 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by 9 parts of lithium trifluoromethanesulfonate. The mixture was stirred evenly for 1.5 hours to obtain a composite water-based binder.
[0073] Example 7
[0074] At a temperature of 45° C., 97 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by addition of 1 part of lithium bis(difluorosulfonyl)imide. The mixture was stirred evenly for 20 minutes to obtain a composite water-based binder.
[0075] Example 8
[0076] At a temperature of 55° C., 98 parts of the PAA binder prepared in Preparation Example 2 were added to a container, followed by 1 part of lithium bis(difluorosulfonyl)imide. The mixture was stirred evenly for 30 minutes to obtain a composite water-based binder.
[0077] Example 9
[0078] At a temperature of 5° C., 90 parts of the PAA binder prepared in Preparation Example 2 were added to a container, followed by 1 part of lithium bis(oxalatoborate) and stirred evenly for 40 minutes to obtain a composite water-based binder.
[0079] Example 10
[0080] At a temperature of 10° C., 90 parts of the PAA binder prepared in Preparation Example 3 were added to a container, followed by 5 parts of lithium bis(oxalatoborate) and stirred evenly for 40 minutes to obtain a composite water-based binder.
[0081] Example 11
[0082] At a temperature of 10° C., 100 parts of the PAA binder prepared in Preparation Example 3 were added to a container, followed by 10 parts of lithium bis(trifluoromethanesulfonyl)imide. The mixture was stirred evenly for 40 minutes to obtain a composite water-based binder.
[0083] Example 12
[0084] At a temperature of 40° C., 95 parts of the PAA binder prepared in Preparation Example 3 were added to a container, followed by 0.1 parts of lithium bis(difluorosulfonyl)imide. The mixture was stirred evenly for 50 minutes to obtain a composite water-based binder.
[0085] Comparative Example 1
[0086] The PAA aqueous binder obtained in Preparation Example 1 was used as a comparative example without any organic lithium compound.
[0087] Comparative Example 2
[0088] The PAA aqueous binder obtained in Preparation Example 2 was used as a comparative example without any organic lithium compound.
[0089] Comparative Example 3
[0090] The PAA aqueous binder obtained in Preparation Example 3 was used as a comparative example without any organic lithium compound.
[0091] Comparative Example 4
[0092] The only difference from Example 1 is that the amount of the PAA binder prepared in Preparation Example 1 is 110 parts.
[0093] At a temperature of 20° C., 110 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by 1 part of lithium bis(trifluoromethanesulfonyl)imide. The mixture was stirred evenly for 30 minutes to obtain a composite water-based binder.
[0094] Comparative Example 5
[0095] The only difference from Example 1 is that the amount of the PAA binder prepared in Preparation Example 1 is 80 parts.
[0096] At a temperature of 20° C., 80 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by addition of 1 part of lithium bis(trifluoromethanesulfonyl)imide. The mixture was stirred evenly for 30 minutes to obtain a composite water-based binder.
[0097] Comparative Example 6
[0098] The only difference from Example 1 is that the amount of lithium bis(trifluoromethanesulfonyl)imide used is 0.05 parts.
[0099] At a temperature of 20° C., 100 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by 0.05 parts of lithium bis(trifluoromethanesulfonyl)imide. The mixture was stirred evenly for 30 minutes to obtain a composite water-based binder.
[0100] Comparative Example 7
[0101] The only difference from Example 1 is that the amount of lithium bis(trifluoromethanesulfonyl)imide used is 15 parts.
[0102] At a temperature of 20° C., 100 parts of the PAA binder prepared in Preparation Example 1 were added to a container, followed by 15 parts of lithium bis(trifluoromethanesulfonyl)imide. The mixture was stirred evenly for 30 minutes to obtain a composite water-based binder.
[0103] The adhesives obtained in the examples and comparative examples were subjected to performance tests, and the test methods were as follows:
[0104] (1) Take graphite slurry without adding adhesive, then add adhesive in an amount of 2% of the solid component of the graphite slurry to the solid component of the adhesive, stir evenly to obtain a mixed slurry. Take 8g of the mixed slurry, evenly apply it on the copper foil with a 200μm thick applicator, and then bake it in a 75℃ oven for 20min to obtain an electrode. Cut the electrode into 30mm wide strips, use 3M tape to stick the strips to the plywood, use a 2kg standard rolling wheel to roll the strips back and forth 3 times to compact them, and then stretch the strips at a stretching speed of 50mm / min to obtain the peel strength;
[0105] (2) The water-based adhesives prepared in the above examples and comparative examples were dried at 65°C to form films. 1.5 g of the film sample was cut and immersed in an electrolyte at 65°C for 3 days. The film sample was weighed and the swelling ratio was calculated: swelling ratio = (weight after swelling - weight before swelling) / weight before swelling × 100%;
[0106] The test results are shown in Table 1.
[0107] Table 1
[0108] It can be seen that the composite water-based adhesive of the present invention has a relatively high peel strength (above 5.25 N / m) and a relatively low expansion rate (below 51%).
[0109] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the composite water-based binder, its preparation method, and lithium-ion battery of the present invention. However, the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent replacements of various raw materials in the products of the present invention, addition of auxiliary ingredients, and selection of specific methods, etc., are all within the scope of protection and disclosure of the present invention.
Claims
1. A composite water-based adhesive, characterized in that: The composite aqueous binder comprises a PAA aqueous binder as shown in Formula I and organic lithium; Wherein R1 is hydrogen or methyl; R2 is C1-C12 alkyl; x=an integer of 100-4300, y=an integer of 100-4000, and z=an integer of 10-750.
2. The composite water-based adhesive according to claim 1, characterized in that: The weight average molecular weight of the PAA aqueous binder shown in Formula I is 50,000 to 500,000.
3. The composite water-based adhesive according to claim 1 or 2, characterized in that: The monomers for preparing the PAA aqueous binder represented by Formula I include acrylic monomers, acrylic ester monomers and styrene monomers; Preferably, the acrylic monomer comprises acrylic acid and / or methacrylic acid; Preferably, the acrylic acid ester monomer includes any one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, isopropyl methacrylate, butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, isobornyl methacrylate, n-octyl acrylate, isooctyl acrylate, lauric acid acrylate, 2-ethylhexyl acrylate, hexyl methacrylate or vinyl acetate, or a combination of at least two thereof.
4. The composite water-based adhesive according to any one of claims 1 to 3, characterized in that: The preparation method of the PAA aqueous binder shown in Formula I comprises the following steps: (1) adding acrylate monomer, styrene monomer and persulfate initiator to an emulsifier aqueous solution, mixing, and causing polymerization reaction to obtain a polyacrylate copolymer emulsion; (2) adding an alkaline compound to the polyacrylate copolymer emulsion obtained in step (1) to adjust the pH of the reaction system to 7-10, thereby obtaining the PAA aqueous binder.
5. The composite water-based adhesive according to claim 4, characterized in that: The emulsifier in step (1) is selected from any one of ammonium allyloxy fatty alcohol polyoxyethylene ether sulfate, sodium allyl hydroxypropyl sulfonate, sodium dodecyl sulfate, sodium dodecylbenzene ring acid or disodium succinic acid nonylphenol polyoxyethylene ether monoester sulfonate or a combination of at least two thereof; Preferably, the mass percentage concentration of the emulsifier in the emulsifier aqueous solution in step (1) is 0.05%-10%; Preferably, the molar ratio of the acrylic acid ester monomer to the styrene monomer in step (1) is 1:0.1-2; Preferably, the persulfate initiator in step (1) is selected from any one of potassium persulfate, ammonium persulfate or sodium persulfate, or a combination of at least two thereof; Preferably, the polymerization reaction temperature in step (1) is 35 to 100° C., and the polymerization reaction time is 2.5 to 12 hours.
6. The composite water-based adhesive according to claim 4 or 5, characterized in that: The alkaline compound in step (2) is selected from any one of ammonia, sodium hydroxide, potassium hydroxide or lithium hydroxide, or a combination of at least two thereof; Preferably, the solid content of the PAA aqueous binder is 10%-60%.
7. The composite water-based adhesive according to any one of claims 1 to 6, characterized in that: The organic lithium is selected from one or a combination of at least two of lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium trifluoromethanesulfonate, lithium bis(difluorosulfonylimide), and lithium bis(trifluoromethanesulfonylimide); Preferably, the composite aqueous binder comprises 90-100 parts of the PAA aqueous binder of Formula I and 0.1-10 parts of organic lithium, in parts by weight.
8. The method for preparing the composite water-based adhesive according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: Mixing the PAA aqueous binder shown in Formula I and organic lithium to obtain the composite aqueous binder; Preferably, the mixing is carried out under stirring; Preferably, the stirring speed is 100-500 rpm; Preferably, the mixing is carried out at a temperature of 5-55°C; Preferably, the mixing time is more than 10 minutes.
9. A negative electrode plate for a lithium ion battery, characterized in that: The negative electrode plate of the lithium-ion battery comprises the composite aqueous binder as described in any one of claims 1 to 7.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises a lithium-ion battery negative electrode sheet as claimed in any one of claims 1 to 7.
Citation Information
Patent Citations
Lithium ion battery silicon-based cathode composite binder, preparation method and application thereof
CN110071289A
Low-porosity positive pole piece, preparation method thereof and application of low-porosity positive pole piece in solid-state lithium metal battery
CN111276690A
Negative plate and battery
CN114141976A
Binder for lithium ion battery and lithium ion battery using same
CN115386033A
Acrylic resin, binder composition using the same and secondary battery using the same