Solar cell, solar cell module, and electric device
Through contactless sealed annealing and optimizing the grain structure, the grain boundary defects caused by heat inhomogeneity of perovskite photovoltaic cells during the annealing process are solved, and the energy conversion efficiency and stability of solar cells are improved.
Patent Information
- Application Number
- PCT/CN2024/074374
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-01-29
- Publication Date
- 2024-11-28
AI Technical Summary
The heat inhomogeneity of existing perovskite photovoltaic cells during annealing leads to different grain sizes, increasing grain boundary defects, reducing energy conversion efficiency and open circuit voltage.
The light absorption layer is prepared by contactless sealed annealing container, and the overall particle size of perovskite-type compound grains is controlled from 1 μm to 6 μm, reducing the number of grain boundaries, adopting a grain structure that penetrates the grain and polygonal shapes, combined with the passivation layer To reduce interface defects and improve carrier transmission efficiency.
It improves the light capture capability and carrier transport speed, reduces interface defects, improves the energy conversion efficiency and open circuit voltage of solar cells, and enhances the stability of the equipment.
Smart Images

Figure CN2024074374_28112024_PF_FP_ABST
Abstract
Description
Solar cells, solar cell modules and electrical devices
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 202310587850.5, filed on May 23, 2023, entitled “Solar Cell, Solar Cell Module and Electrical Device,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the technical field of solar cell devices, and in particular to a solar cell, a solar cell assembly and an electrical device. Background Art
[0004] Green, environmentally friendly, recycled, and renewable energy is a key area of future energy technology development. Perovskite photovoltaic cells, which directly convert solar energy into electricity when exposed to sunlight, are a new energy technology receiving increasing attention.
[0005] For perovskite photovoltaic cells, how to improve the overall performance is the key research direction.
[0006] Summary of the Invention
[0007] The purpose of the present application is to provide a solar cell that can improve the internal electric field strength of the solar cell, increase the open circuit voltage, and improve its energy conversion efficiency; the purpose of the present application is also to provide a solar cell module and an electrical device containing the solar cell, so that it can obtain improved internal electric field strength, open circuit voltage, and improve its energy conversion efficiency.
[0008] In a first aspect, an embodiment of the present application provides a solar cell comprising a light absorbing layer,
[0009] The light absorbing layer comprises a plurality of perovskite compound grains, wherein in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1 μm to 6 μm is ≥90%.
[0010] According to the technical solution of the embodiment of the present application, the light absorbing layer contains perovskite compound grains with a long diameter of 1 μm to 6 μm in at least one cross section perpendicular to the layer thickness direction, and the cumulative distribution rate of the perovskite compound grains is ≥90%.
[0011] The crystallization quality of the perovskite compound grains in the light absorption layer, including the overall particle size, is improved, and properties such as efficient light capture capability, ultrafast carrier transport capability, and ion migration inhibition can be obtained; during the power generation process of the solar cell, the overall particle size of the perovskite compound grains is larger, which reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, and promotes charge separation at the interface, thereby improving the comprehensive performance of the solar cell, including energy conversion efficiency.
[0012] Furthermore, open-circuit voltage is influenced by the minimum energy required to excite electrons and the energy gap of the semiconductor material itself. A higher energy gap increases the open-circuit voltage, while the number of photons required decreases. During solar cell power generation, larger perovskite-type compound grains favor a suitable energy gap, improving light capture and reducing the number of photons required, thus increasing the open-circuit voltage.
[0013] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 2.0 μm to 5.0 μm is ≥75%.
[0014] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 2.0 μm to 3.5 μm is ≥50%.
[0015] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D greater than or equal to 3.5 μm is 5%-30%.
[0016] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 2.5 μm to 3.0 μm is ≥60%.
[0017] In any embodiment of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 1.0 μm to 2.5 μm is 20%-40%.
[0018] In any embodiment of the present application, in at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of less than or equal to 1.0 μm is ≤8%. According to an embodiment of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1.0 μm to 2.5 μm is within the above range, indicating that the proportion of perovskite compound grains of the above particle size in the entire cross-section is within an appropriate range, with smaller grains accounting for a smaller proportion, thereby improving the uniformity of the grain size of the entire light absorbing layer; during the power generation process of the solar cell, the uniformity of the grain size is beneficial to the stability of the solar cell operation.
[0019] In any embodiment of the present application, in at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction, the perovskite compound grains having a major diameter D of 1 μm to 6 μm are polygonal. These shapes provide good contact between the grains and low porosity, which helps improve carrier transport efficiency and reduce defects between grains. This also contributes to the stability of solar cell operation and energy conversion efficiency during solar cell power generation.
[0020] In any embodiment of the present application, in at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction, the perovskite compound grains having a major diameter D of 1 μm to 4 μm are N-polygonal, where N is a positive integer greater than 5; N can be 6-9. According to the embodiments of the present application, the close contact between the polygonal perovskite compound grains is beneficial for improving the carrier transport efficiency and reducing the impact of grain boundary defects; this is beneficial for the stability of the solar cell operation and the energy conversion efficiency during the power generation process.
[0021] In any embodiment of the present application, the light absorbing layer includes perovskite compound grains extending through the light absorbing layer in at least one cross-section along the thickness direction of the layer. The perovskite compound grains extending through the light absorbing layer may be in direct contact with the first carrier transport layer and the second carrier transport layer, thereby reducing interface defects between the light absorbing layer and the first and second carrier transport layers, reducing non-radiative recombination losses at the interfaces, reducing or avoiding current transmission limitations, and improving the current intensity and energy conversion efficiency of the battery.
[0022] In any embodiment of the present application, the ratio of the perovskite compound grains extending through the light absorbing layer to the total number of grains in the light absorbing layer is 50% to 90%, and optionally 60% to 85%. The ratio of the perovskite compound grains extending through the light absorbing layer to the total number of grains in the light absorbing layer being within the above range can further reduce interface defects between the light absorbing layer and the first and second carrier transport layers, respectively, reduce non-radiative recombination losses at the interfaces, reduce or avoid current transmission limitations, and improve the current intensity and energy conversion efficiency of the battery.
[0023] In any embodiment of the present application, the perovskite compound grains include primary grains and secondary grains, and the number of the secondary grains accounts for 80%-100% of the total number of the perovskite compound grains, and can be optionally 65%-95%.
[0024] In any embodiment of the present application, the solar cell includes a first carrier transport layer and a second carrier transport layer, and the solar cell includes:
[0025] A passivation layer located between the light absorbing layer and the first carrier transport layer and / or between the light absorbing layer and the second carrier transport layer; wherein the passivation layer is used to reduce defects at the interface between the two. The passivation layer facilitates ohmic transport of carriers, reduces interfacial charge transport barriers caused by poor contact between the light absorbing layer and the carrier transport layer due to polarity differences, reduces defect density, optimizes energy levels, promotes internal charge transfer, and improves the energy conversion efficiency of perovskite solar cells.
[0026] In a second aspect, an embodiment of the present application provides a method for preparing a solar cell, the method comprising:
[0027] The light absorbing layer comprising a plurality of perovskite compound grains of the first aspect is prepared by a non-contact sealed annealing container, wherein, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains having a long diameter D of 1 μm to 6 μm is ≥90%.
[0028] According to the embodiments of the present application, the light absorption layer prepared by a contactless sealed annealing container improves the crystallization quality of the perovskite compound grains in the light absorption layer, including the overall particle size, and can obtain properties such as efficient light capture capability, ultrafast carrier transport capability, and inhibition of ion migration. During the power generation process of the solar cell, the overall particle size of the perovskite compound grains is larger, which reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, and promotes charge separation at the interface, thereby improving the comprehensive performance of the solar cell, including energy conversion efficiency.
[0029] In any embodiment of the present application, the method includes at least one of the following conditions:
[0030] 1) A sealed annealing container contains an annealing atmosphere, wherein the annealing atmosphere includes a polar aprotic solvent; optionally, the polar aprotic solvent includes at least one of N,N-dimethylformamide, 1-methyl-2-pyrrolidone, dimethyl sulfoxide, and dimethylacetamide;
[0031] 2) The annealing temperature in the sealed annealing container is 100-180°C, and can be optionally 120-160°C;
[0032] 3) The annealing time in the sealed annealing container is 8 to 30 minutes, and can be optionally 10 to 20 minutes.
[0033] According to the embodiments of the present application, by regulating the annealing atmosphere, annealing temperature and annealing time in a closed annealing container, the crystallization quality of the perovskite compound grains, including the overall particle size, is comprehensively controlled, thereby improving the comprehensive performance of the solar cell, including the energy conversion efficiency.
[0034] In a third aspect, an embodiment of the present application provides a solar cell assembly, comprising the solar cell of the second aspect.
[0035] In a fourth aspect, an embodiment of the present application provides an electrical device, comprising a solar cell assembly according to any one of the embodiments of the third aspect of the present application, wherein the solar cell assembly is used to provide electrical energy.
[0036] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiments below. The accompanying drawings are for illustration purposes only and are not to be construed as limiting the present application. The same reference numerals are used throughout the accompanying drawings to represent the same components.
[0038] In the attached figure:
[0039] FIG1 is a schematic diagram showing the measurement of the major diameter, minor diameter and height of the cross section of the light absorbing layer according to an embodiment of the present application;
[0040] FIG2 shows a schematic cross-sectional structure diagram of a solar cell provided in an embodiment of the present application;
[0041] FIG3 shows a schematic cross-sectional structure diagram of a solar cell provided in an embodiment of the present application;
[0042] FIG4 shows a microscopic image of the long diameter of perovskite compound grains in a light absorbing layer of a solar cell provided by an embodiment of the present application;
[0043] FIG5 shows a microscopic image of the long diameter of perovskite compound grains in a light absorbing layer of a solar cell provided in another embodiment of the present application;
[0044] FIG6 shows a microscopic image of the long diameter of perovskite compound grains in a light absorbing layer of a solar cell provided in another embodiment of the present application;
[0045] FIG7 shows a microscopic image of the height of perovskite compound grains in a light absorption layer of a solar cell provided in an embodiment of the present application.
[0046] The drawings in this application are not necessarily drawn to scale. DETAILED DESCRIPTION
[0047] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.
[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.
[0049] In the description of the embodiments of this application, the technical terms "first," "second," etc. are used only to distinguish different objects and should not be understood to indicate or imply relative importance or to implicitly indicate the quantity, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise specifically defined.
[0050] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0051] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.
[0052] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0053] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they should not be understood as limiting the embodiments of the present application.
[0054] In the description of the embodiments of the present application, unless otherwise expressly specified or limited, technical terms such as "installed," "connected," "connected," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; and internal connections between two components or interactions between two components. Those skilled in the art can understand the specific meanings of the above terms in the embodiments of the present application based on specific circumstances.
[0055] A solar cell is a device that converts light energy directly into electrical energy through the photoelectric effect or photochemical reaction. Examples of solar cells include perovskite solar cells, which use perovskite-type compound semiconductors as light-absorbing materials and are considered third-generation solar cells.
[0056] The perovskite compound in a perovskite solar cell absorbs photons of a certain energy, causing its valence band electrons to transition to the conduction band, while leaving holes in the valence band, forming bound electron-hole pairs. These electron-hole pairs can separate into free carriers and be transported to the corresponding electrodes, achieving photoelectric conversion. The crystallization quality of the perovskite compound directly affects the initial efficiency and stability of the perovskite solar cell, and the crystallization quality is largely affected by the annealing process. In the process of engineering mass production of perovskite solar cells, how to ensure the consistency of the annealing temperature for the perovskite compound and the uniformity of the heated area are key issues in ensuring crystallization quality.
[0057] Currently, the most widely used annealing process is contact hot plate annealing, which primarily relies on heat conduction or radiation. This involves heating the hot plate surface with a heating wire, which then transfers heat to the perovskite solar cell substrate (primarily glass or flexible substrates), and finally conducts heat upward to the perovskite. This process raises the following issues: 1. Uniform heating across a large area of the perovskite layer. Traditional annealing is mainly based on hot plate annealing, and the uniformity of perovskite heating is restricted in multiple ways. One is the uniformity of the hot plate. The larger the heating area, the more difficult it is to control the temperature between different areas. Another difficult-to-control factor is that the substrate material of the perovskite solar cell, especially glass, deforms during the heating process. This deformation directly leads to large differences in the heating rate of different areas of the perovskite layer. Due to uneven heating and large temperature differences in the body, the perovskite compound grains often have different sizes and uneven size distribution, which further introduces grain boundary defects. When a solar cell containing these perovskite compound grains with different sizes and uneven size distribution is used, it affects the transport of carriers. The grain boundary defects with more water reduce the energy conversion efficiency of the solar cell. Secondly, the perovskite grains prepared by the above annealing process are small (generally less than 500nm). Small perovskite crystals inevitably produce a large number of grain boundaries. There are often unavoidable defects at the grain boundaries, which directly cause the open circuit voltage of the perovskite solar cell to drop, the energy conversion efficiency is low, and the performance of the perovskite solar cell is seriously affected.
[0058] In related technologies, a fluctuating thermal annealing process is used to strictly control the annealing temperature and annealing cycle of the perovskite photoactive layer. The growth time of the crystallization is controlled through a short heating process, so that the grains of the perovskite active layer grow relatively orderly. In the slow growth stage, the perovskite grains can self-assemble, making the contact between the grains denser and more uniform. However, it solves the problem of large differences in perovskite grain size or uniformity. Based on the traditional contact hot plate annealing preparation, the perovskite grains produced are small (generally less than 500nm), and a large number of grain boundaries will still be produced, which will inevitably bring many defects, resulting in low efficiency and poor stability of perovskite solar cells.
[0059] In view of this, the technical solution of the embodiment of the present application provides a solar cell, which can at least improve the adverse effects of a large number of grain boundaries and grain boundary defects caused by the grain size of perovskite compound grains during the solar cell power generation process, thereby improving the energy conversion efficiency of the solar cell.
[0060] solar cells
[0061] In a first aspect, an embodiment of the present application provides a solar cell comprising a light absorbing layer,
[0062] The light absorbing layer comprises a plurality of perovskite compound grains, wherein in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1 μm to 6 μm is ≥90%.
[0063] According to an embodiment of the present application, the long diameter D of the perovskite compound grains is measured on a cross section perpendicular to the thickness direction of the light absorbing layer, and optionally the short diameter b of the perovskite compound grains can be measured. The thickness h of the perovskite compound grains can be measured on a cross section perpendicular to the thickness direction of the light absorbing layer, so the long diameter D reflects the actual long diameter of the perovskite compound grains. The long diameter can be understood as the longest measured particle size of the perovskite compound grains. This is shown in Figure 1.
[0064] According to the embodiments of the present application, the cumulative distribution rate of the number of perovskite compound grains represents the percentage of perovskite compound grains with a specific particle size out of the total number of perovskite compound grains in the cross-section. The percentage is calculated based on the number of grains. The cumulative distribution rate of the number of perovskite compound grains = the number of perovskite grains within the corresponding size range in the SEM image / the total number of perovskite grains in the corresponding SEM image × 100%.
[0065] According to the technical solution of the embodiment of the present application, the crystal defects of the perovskite compound grains themselves in the light absorption layer of the solar cell can cause non-radiative recombination of carriers, thereby causing a certain amount of energy loss and reducing the photoelectric conversion efficiency of the solar cell. The cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1 μm to 6 microns in the present application is within the above range, which improves the crystal quality of the perovskite compound grains in the light absorption layer, including the overall particle size, and can obtain high-efficiency light capture capability, ultra-fast carrier transport capability, and ion migration inhibition performance. During the power generation process of the solar cell, the overall particle size of the perovskite compound grains is larger, which reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, and can promote charge separation at the interface, thereby improving the comprehensive performance of the solar cell, including energy conversion efficiency.
[0066] Furthermore, open-circuit voltage is influenced by the minimum energy required to excite electrons and the energy gap of the semiconductor material itself. A higher energy gap increases the open-circuit voltage, while the number of photons required decreases. During solar cell power generation, larger perovskite-type compound grains favor a suitable energy gap, improving light capture and reducing the number of photons required, thus increasing the open-circuit voltage.
[0067] Optionally, the long diameter D of the perovskite compound grains may be any value among 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, 4.5 μm, 4.6 μm, 4.7 μm, 4.8 μm, 4.9 μm, 5.0 μm, 5.1 μm, 5.2 μm, 5.3 μm, 5.4 μm, 5.5 μm, 5.6 μm, 5.7 μm, 5.8 μm, 5.9 μm, 6.0 μm, or a range thereof. The cumulative distribution rate of the number of perovskite compound grains having a long diameter D of 1 μm to 6 μm may be any value among 90%, 91%, 92%, 93%, 94%, 95%, 96%, or 97%, or a range thereof. The long diameter D of the perovskite compound grains is within the above-mentioned range, further increasing the overall particle size of the perovskite compound grains in the light absorption layer. The cumulative distribution ratio of the number of perovskite compound grains with a long diameter D of 1 μm to 6 μm is within the above-mentioned range. During the power generation process of the solar cell, the overall particle size of the perovskite compound grains is larger, further reducing the number of grain boundaries between the perovskite compound grains, reducing or avoiding interference from interface defects, and improving energy conversion efficiency.
[0068] In some embodiments, at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction may be a cross-section along the thickness direction of the light absorbing layer and near the surface layer. Alternatively, the cross-section may be a cross-section of an end face along the thickness direction of the light absorbing layer. The thickness of the surface layer may be ≤ 100 nm, and may optionally be ≤ 50 nm.
[0069] In some optional embodiments of the present application, in at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 5.0 μm is ≥ 75%. Optionally, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 5.0 μm can be any value selected from 75%, 76%, 77%, 78%, 79%, 80%, 85%, 90%, and 95%, or a range thereof. The cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 5.0 μm within the above range increases the overall particle size of the perovskite compound grains; the long diameter D of 2.0 μm to 5.0 μm improves the uniformity of the perovskite compound grain size; and during the power generation process of the solar cell, the number of grain boundaries between the perovskite compound grains is reduced, the interference of interface defects is reduced or avoided, and the energy conversion efficiency is improved.
[0070] Perovskite compound grains with a long diameter D of 2.0 μm to 5.0 μm have a suitable energy gap. When the cumulative distribution rate of the number of perovskite compound grains is within the above range, the light capture capability can be improved and the open circuit voltage of the solar cell can be increased.
[0071] In some optional embodiments of the present application, in at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 3.5 μm is ≥ 50%. Optionally, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 3.5 μm can be any value selected from or a range of combinations thereof, such as 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 65%, 70%, 75%, 80%, 90%, or 95%.
[0072] According to the embodiments of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 3.5 μm is within the above range, which improves the uniformity of the perovskite compound grain size and the overall particle size; during the power generation process of the solar cell, the number of grain boundaries between the perovskite compound grains is reduced, the interference of interface defects is reduced or avoided, and the energy conversion efficiency is improved.
[0073] In some optional embodiments of the present application, in at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D greater than or equal to 3.5 μm is 5%-30%. Optionally, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D greater than or equal to 3.5 μm can be any value or a range composed of 5%, 6%, 7%, 8%, 9%, 10%, 15%, 20%, 25%, 26%, 27%, 28%, 29%, 30%. According to the embodiment of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D greater than or equal to 3.5 μm is within the above range, indicating that the proportion of perovskite compound grains of the above particle size in the entire cross-section is within an appropriate range, and the proportion of larger grains is relatively small, thereby improving the uniformity of the grain size of the entire light absorbing layer; during the power generation process of the solar cell, the uniformity of the grain size is beneficial to the stability of the solar cell operation.
[0074] In some optional embodiments of the present application, in at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.5 μm to 3.0 μm is ≥ 60%. Optionally, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.5 μm to 3.0 μm can be any value or range of its composition among 60%, 61%, 62%, 63%, 64%, 65%, 70%, 75%, 80%, 81%, 82%, 83%, 84%, 90%, 95%. According to the embodiment of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.5 μm to 3.0 μm is within the above range, which improves the uniformity of the perovskite compound grain size and the overall particle size; during the power generation process of the solar cell, the number of grain boundaries between the perovskite compound grains is reduced, the interference of interface defects is reduced or avoided, and the energy conversion efficiency is improved.
[0075] In some optional embodiments of the present application, in at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1.0 μm to 2.5 μm is 20%-40%. The cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1.0 μm to 2.5 μm can be any value or range of 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 32%, 35%, 36%, 37%, 38%, 39%, or 40%. According to the embodiments of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 1.0 μm to 2.5 μm is within the above range, indicating that the proportion of perovskite compound grains with the above particle size in the entire cross-section is within an appropriate range, and the proportion of smaller grains is relatively small, thereby improving the uniformity of the grain size of the entire light absorption layer; during the power generation process of the solar cell, the uniformity of the grain size is beneficial to the stability of the operation of the solar cell.
[0076] In some optional embodiments of the present application, in at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D less than or equal to 1.0 μm is ≤8%. The cumulative distribution rate of the number of perovskite compound grains with a long diameter D less than or equal to 1.0 μm can be any value of 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, or a range composed thereof. According to the embodiment of the present application, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D less than or equal to 1.0 μm is within the above range, indicating that the proportion of perovskite compound grains of the above particle size in the entire cross-section is within a suitable range, and the proportion of smaller grains is relatively small, thereby improving the uniformity of the grain size of the entire light absorbing layer; during the power generation process of the solar cell, the uniformity of the grain size is beneficial to the stability of the solar cell operation.
[0077] In some optional embodiments of the present application, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the perovskite compound grains with a long diameter D of 1 μm to 6 μm are polygonal.
[0078] According to the embodiments of the present application, defects in porosity or adhesion between the perovskite compound grains in the light absorption layer of the solar cell can cause non-radiative recombination of carriers, resulting in a certain amount of energy loss and reducing the photoelectric conversion efficiency of the solar cell. The above-mentioned shape has better contact between the grains and lower porosity, which is conducive to improving the transmission efficiency of carriers and reducing defects between the grains; this is beneficial to the stability of the solar cell operation and the energy conversion efficiency during the power generation process.
[0079] As an example, perovskite compound grains with a long diameter D of 1 μm to 6 μm are polygonal as shown in FIG. 4-6 .
[0080] In some optional embodiments of the present application, in at least one cross-section of the light absorbing layer perpendicular to the layer thickness direction, the perovskite compound grains with a long diameter D of 1 μm to 4 μm are N-gons, where N is a positive integer and N is greater than 5; it can be optionally 6-9.
[0081] According to the embodiments of the present application, the polygonal perovskite compound grains are closely connected to each other, which is beneficial to improving the carrier transmission efficiency and reducing the impact of grain boundary defects; during the power generation process of the solar cell, it is beneficial to the stability of the solar cell operation and the energy conversion efficiency.
[0082] In some optional embodiments of the present application, the light absorbing layer comprises perovskite compound grains running through the light absorbing layer in at least one cross section in the thickness direction of the light absorbing layer.
[0083] In the embodiment of the present application, the perovskite compound grains extending through the light absorbing layer can be measured from a cross section parallel to the thickness direction of the light absorbing layer, i.e., the height h of the perovskite compound grains can be measured, as shown in FIG1 . As an example, the perovskite compound grains extending through the light absorbing layer are shown in FIG7 .
[0084] The carriers formed by the photoexcitation of the perovskite compound in the solar cell diffuse within the light-absorbing layer. When they reach the interface between the electron transport layer / hole transport layer and the light-absorbing layer, if the energy levels of the two functional layers are matched, free electrons and holes are formed under the action of the interface barrier. Defects within the perovskite compound and at the interface between the two transport layers can cause non-radiative recombination of carriers, resulting in a certain amount of energy loss and reducing the photoelectric conversion efficiency of the perovskite solar cell. Therefore, the perovskite compound grains that penetrate the light-absorbing layer can directly contact the first carrier transport layer and the second carrier transport layer, which can reduce the interface defects between the light-absorbing layer and the first carrier transport layer and the second carrier transport layer, reduce non-radiative recombination losses between the interfaces, reduce or avoid current transmission restrictions, and improve the current intensity and energy conversion efficiency of the battery.
[0085] In some optional embodiments of the present application, the ratio of perovskite compound grains extending through the light absorbing layer to the total number of grains in the light absorbing layer is 50% to 90%, and optionally 60% to 85%. The ratio of perovskite compound grains extending through the light absorbing layer to the total number of grains in the light absorbing layer being within the above range further reduces interface defects between the light absorbing layer and the first and second carrier transport layers, further reducing or avoiding current transmission limitations, and improving the current intensity and energy conversion efficiency of the battery.
[0086] In some optional embodiments of the present application, the perovskite compound grains include primary grains and secondary grains, and the number of secondary grains accounts for 80%-100% of the total number of perovskite compound grains, and optionally 65%-95%.
[0087] According to the embodiments of the present application, primary grains refer to the dense, small and uniform grains obtained in the early stage of annealing of the perovskite compound. Secondary grains refer to the primary grains that continue to anneal in a trace solvent atmosphere. According to the Oswald ripening effect, small grains are continuously dissolved to form a solute atmosphere that is absorbed by slightly larger grains due to the chemical kinetic process, gradually forming a large grain structure, that is, large grains with small surface energy swallow up small grains with large surface energy. Such grown grains are called secondary grains. Generally speaking, the major diameter of the primary grains ranges from about 100nm to 800nm, and the volume of the secondary grains can reach 1μm to 6μm.
[0088] In some optional embodiments of the present application, the perovskite-type compound grains contain an organic-inorganic perovskite compound represented by the general formula ABX3, where A is an organic cation, B is a metal cation, and X is a halogen anion or SCN - . In some embodiments of the present application, the halogen X includes at least one of chlorine, bromine, and iodine.
[0089] It can be understood that: Perovskite materials with different halogen ions have different bandgaps. The perovskite material with halogen ion I- has the smallest bandgap (generally about 1.5 electron volts), and the perovskite material with halogen ion Cl- has the largest bandgap (generally about 3 electron volts). Moreover, the perovskite material can contain two mixed halogen ions, and the mixing ratio can be continuously adjusted. Therefore, the bandgap of the perovskite material can be continuously adjusted within the range of 1.5 - 3 electron volts, corresponding to the wavelength range of the light that can be absorbed of about 414 - 820 nanometers, which basically covers the entire visible light spectrum. Carriers are generated in the light absorption layer.
[0090] For example: A in ABX3 can include at least one of CH3NH 3+ and HC(NH2) 2+ ; in other words, A can be CH3NH 3+ , HC(NH2) 2+ or a mixture of the two in any proportion. It can be understood that A can also include metal ions, such as Cs + , Rb + and K + at least one of them.
[0091] For example: B in ABX3 can be at least one of Pb 2+ , Sn 2+ and Ge 2+ at least one of them.
[0092] For example, ABX3 can be CH3NH3PbI3; CH3NH3SnI3; CH3NH3PbI2Cl; CH3NH3PbI2Br; CH3NH3Pb(I 1-x Br x )3 (where 0 < x < 1), etc.
[0093] In some embodiments, the organic cation A includes at least one of an amine group and an amine group derivative. In some examples, the amine group can be an alkylamine group.
[0094] In some embodiments, the amine group includes at least one of methylamine group, ethylamine group, propylamine group, butylamine group, pentylamine group, hexylamine group, and formamidine group. The amine group derivative can include an imidazole group.
[0095] In some embodiments, the metal in the metal cation B includes at least one of lead (Pb), cesium (Cs), tin (Sn), zinc (Zn), titanium (Ti), antimony (Sb), bismuth (Bi), nickel (Ni), iron (Fe), cobalt (Co), silver (Ag), copper (Cu), gallium (Ga), germanium (Ge), magnesium (Mg), calcium (Ca), indium (In), aluminum (Al), manganese (Mn), chromium (Cr), molybdenum (Mo), and europium (Eu). B in the general formula ABX3 is selected from the above metal cations, which can help improve the photoelectric conversion efficiency of the light absorbing layer.
[0096] Figure 2 shows a schematic cross-sectional view of a solar cell according to an embodiment of the present application. As shown in Figure 2, a solar cell 10 includes the following structures stacked in sequence: a first electrode layer 11; a first carrier transport layer 13; a light absorbing layer 15; a second carrier transport layer 14; and a second electrode layer 12.
[0097] In some embodiments of the present application, the first electrode layer 11 may be made of a conductor having a high work function to facilitate hole injection. For example, the conductor may be a metal, a metal oxide, and / or a conductive polymer.
[0098] Exemplarily, the first electrode layer 11 may be made of a metal, for example, the material of the first electrode 11 includes at least one of nickel (Ni), platinum (Pt), vanadium (V), chromium (Cr), copper (Cu), zinc (Zn), gold (Au), silver (Ag), or alloys thereof. The first electrode 131 may also be made of a metal oxide, for example, the material of the first electrode 131 includes at least one of zinc oxide (ZnO), indium oxide (In2O3), fluorine-doped tin oxide (FTO), indium tin oxide (ITO), nickel oxide (NiO), aluminum zinc oxide (AZO), indium zinc oxide (IZO), and gallium zinc oxide (GZO). The first electrode 131 may also be made of a conductive polymer, for example, the material of the first electrode 131 includes at least one of poly(3-methylthiophene), poly(3,4-(ethylene-1,2-dioxy)thiophene) (PEDOT), polypyrrole, and polyaniline.
[0099] In an embodiment of the present application, the second electrode layer 12 may also be made of a conductor having a low work function to facilitate electron injection. Exemplarily, the material of the second electrode 12 includes at least one of copper (Cu), magnesium (Mg), aluminum (Al), nickel (Ni), silver (Ag), tin (Sn), chromium (Cr), bismuth (Bi), platinum (Pt), molybdenum (Mo), tungsten (W), or alloys thereof, carbon (C), graphene, carbon nanotubes, fluorine-doped tin oxide (FTO), indium tin oxide (ITO), aluminum zinc oxide (AZO), indium zinc oxide (IZO), and gallium zinc oxide (GZO).
[0100] In some embodiments, the solar cell includes a first carrier transport layer 13 and a second carrier transport layer 14 disposed on both sides of the light absorbing layer 15. The first carrier transport layer 13 and the second carrier transport layer 14 are associated with each other.
[0101] The first carrier transport layer 13 and the second carrier transport layer 14 have opposite carrier selectivities. If the first carrier transport layer 13 has electron selectivity and the second carrier transport layer 14 has hole selectivity, then after the light absorption layer 15 absorbs sunlight and generates carriers, the electrons in the carriers are selected by the first carrier transport layer 13 and transported to the first electrode layer 11, and then collected by the first electrode layer 11. The holes that have lost the electrons are selected by the second carrier transport layer 15 and their electrical properties are transferred to the second electrode layer 12, and then collected by the second electrode layer 12, thereby achieving the separation of carriers in the perovskite compound in the light absorption layer 15.
[0102] If the first carrier transport layer 13 has hole selectivity and the second carrier transport layer 14 has electron selectivity, then after the light absorption layer 15 absorbs sunlight and generates carriers, the holes that lose electrons are selected by the first carrier transport layer 13 and their electrical properties are transferred to the first electrode layer 11, and then collected by the first electrode layer 11. The electrons in the carriers are selected by the second carrier transport layer 30 and transferred to the second electrode layer 12, and then collected by the second electrode layer 12, thereby realizing the separation of carriers in the light absorption layer 15.
[0103] Furthermore, the first carrier transport layer 13 is arranged on the light-facing surface of the light absorption layer 15, and the second carrier transport layer 14 is arranged on the backlight surface of the light absorption layer 15, and the carrier selectivities corresponding to the first carrier transport layer 13 and the second carrier transport layer 15 are opposite, and the first electrode layer 11 is arranged on the side of the first carrier transport layer 13 away from the light absorption layer 15, and the second electrode layer 12 is arranged on the side of the second carrier transport layer 14 away from the light absorption layer 15, and the second electrode layer 12 and the second carrier transport layer 14 are electrically connected.
[0104] According to the embodiment of the present application, the first carrier transport layer 13 and the second carrier transport layer 14 can be a single-layer structure or a multi-layer structure respectively.
[0105] In some embodiments of the present application, the hole-selective material includes at least one of thiophene, phthalocyanine, porphyrin, 2,2',7,7'-tetrakis(N,N-di-p-methoxyaniline)-9,9'-spirobifluorene, molybdenum oxide (MoO3), vanadium oxide (V2O5), tungsten oxide (WO3 and / or WO2), nickel oxide (NiO), copper oxide (CuO), tin oxide (SnO2), molybdenum sulfide (MoS2), tungsten sulfide (WS2), copper sulfide (CuS), tin sulfide (SnS), cuprous thiocyanate (CuSCN), copper iodide (CuI), fluorine-containing phosphonic acid, carbonyl-containing phosphonic acid, carbon nanotubes and graphene.
[0106] In some embodiments of the present application, the electron-selective material includes at least one of [6,6]-phenyl-C61-butyric acid isomethyl ester, C60, cyano-containing polyphenylene vinylene, boron-containing polymer, bathocuproine, bathophenanthroline, hydroxyquinoline aluminum, oxadiazole compounds, benzimidazole compounds, naphthalenetetracarboxylic acid compounds, perylene derivatives, phosphine oxide compounds, phosphorus sulfide compounds, fluorine-containing phthalocyanine, titanium oxide (TiO2), zinc oxide (ZnO), tin oxide (SnO2), indium oxide (In2O3), gallium oxide (Ga2O3), tin sulfide (SnS), indium sulfide (In2O3), lithium fluoride (LiF), sodium fluoride (NaF), magnesium fluoride (MgF2) and zinc sulfide (ZnS).
[0107] In some optional embodiments of the present application, the solar cell includes a first carrier transport layer and a second carrier transport layer, and the solar cell includes:
[0108] A passivation layer located between the light absorbing layer and the first carrier transport layer and / or a passivation layer located between the light absorbing layer and the second carrier transport layer. The passivation layer is used to reduce defects when the two interfaces contact each other.
[0109] Figure 3 shows a schematic cross-sectional structure of a solar cell according to an embodiment of the present application. As shown in Figure 3, the solar cell 10 includes the following structures stacked in sequence: a first electrode layer 11; a first carrier transport layer 13; a first passivation layer 16; a light absorbing layer 15; a second passivation layer 17; a second carrier transport layer 14; and a second electrode layer 12.
[0110] According to an embodiment of the present application, the passivation layer can be made of a material commonly used in the art. For example, the material can be methyl-substituted carbazole molecules (Me-4PACz). Methyl-substituted carbazole molecules (Me-4PACz) can be understood as a self-assembled molecular layer. The thickness can be 1 to 5 nm.
[0111] The light-absorbing layer in a solar cell absorbs energy and releases carriers that diffuse within the perovskite. When these carriers reach the interface between the electron transport layer / hole transport layer and the light-absorbing layer, defects at the interface between the perovskite compound and the two transport layers cause non-radiative recombination of the carriers, resulting in a certain amount of energy loss and reducing the photoelectric conversion efficiency of the perovskite solar cell. The aforementioned passivation layer facilitates ohmic transport of carriers, reduces interfacial charge transport barriers caused by poor interface contact due to the polarity difference between the light-absorbing layer and the carrier transport layer, reduces defect density, optimizes energy levels, promotes internal charge transfer, and helps improve the energy conversion efficiency of perovskite solar cells.
[0112] In some embodiments, the solar cell includes a substrate disposed on a side of the first electrode layer facing away from the second electrode layer. The substrate is made of glass or a mixture of one or more transparent organic polymers, including one or more of PET (polyethylene terephthalate) and PI (polyimide).
[0113] [Method for producing solar cells]
[0114] In the embodiment of the present application, the solar cell 10 may be manufactured using methods known in the art.
[0115] In some embodiments of the present application, a method for preparing a solar cell includes:
[0116] S10: providing a first electrode layer;
[0117] S20: forming a first carrier transport layer on one side of the first electrode layer;
[0118] S30: forming a light absorbing layer on a side of the first carrier transport layer away from the first electrode layer;
[0119] S40: forming a second carrier transport layer on a side of the light absorbing layer away from the first carrier transport layer;
[0120] S50: forming a second electrode layer on a side of the second carrier transport layer away from the light absorption layer.
[0121] Exemplarily, a method for manufacturing a solar cell device 10 may include forming a first carrier transport layer 13, a light absorbing layer 15, a second carrier transport layer 14, and a second electrode layer 12 in order from bottom to top on a transparent or opaque first electrode layer 11. The light absorbing layer 15 may be formed using known film-forming methods such as evaporation, sputtering, spin coating, dipping, and ion plating.
[0122] The preparation process of the light absorbing layer includes three steps: wet film coating, solvent quenching and annealing.
[0123] The wet film coating includes: in the wet film coating state, the perovskite is in a colloidal state, and ABX3 is distributed in a precursor solvent and coated on a substrate.
[0124] Solvent quenching involves rapidly removing the bulk of the organic solvent from the perovskite precursor solution, leaving only a small amount of solvent to complex with the perovskite components. At this point, the perovskite is in an intermediate state, typically with the general formula AX·BX2·organic solvent. This process is the process by which a portion of the solute forms seed crystals.
[0125] Annealing involves the gradual loss of solvent molecules from the organic solvent AX·BX2, resulting in the formation of complete ABX3. During the annealing process, seed crystals absorb the remaining solute, which has been stripped of solvent molecules, and grow into perovskite grains. Generally, given a fixed solute content, the number of seed crystals is inversely proportional to grain size.
[0126] In a second aspect, an embodiment of the present application provides a method for preparing a solar cell, the method comprising:
[0127] The light absorbing layer comprising a plurality of perovskite compound grains of the first aspect is prepared by a non-contact sealed annealing container, wherein, in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains having a long diameter D of 1 μm to 6 μm is ≥90%.
[0128] In related technologies, contact hot plate annealing is an annealing process achieved through heat conduction. When preparing perovskite layers on a large scale, the temperature rises unevenly due to the warping of the glass, resulting in inconsistent seed crystal growth rates and different grain sizes. In addition, the number of seed crystals is large and irreversible, resulting in generally small grains (the maximum width of the grains is less than 500nm).
[0129] According to the embodiments of the present application, the light absorption layer prepared by a contactless sealed annealing container improves the crystallization quality of the perovskite compound grains in the light absorption layer, including the overall particle size, and can obtain properties such as efficient light capture capability, ultrafast carrier transport capability, and inhibition of ion migration. During the power generation process of the solar cell, the overall particle size of the perovskite compound grains is larger, which reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, and promotes charge separation at the interface, thereby improving the comprehensive performance of the solar cell, including energy conversion efficiency.
[0130] In the embodiment of the present application, the contactless closed annealing container leukemia adopts a contactless closed oven for annealing to achieve uniform temperature rise of the seed crystal, and the volatile organic solvent molecules will accumulate in the annealing atmosphere to form a specific solvent annealing atmosphere, which gradually dissolves the small grains. Through the Ostwald ripening effect, the large grains absorb these dissolved small grains and gradually grow into larger perovskite compound grains, with a reduced number of grain boundaries and defects. The Ostwald ripening effect is a phenomenon that can be observed in solid solutions or liquid sols. It describes the changes that occur in a non-uniform structure over time: smaller crystals or sol particles in the solute dissolve and redeposit on larger crystals or sol particles. It relies on the reduction of the specific interfacial energy per unit mass, the reduction of the total free energy of the system, and the spontaneous reaction.
[0131] In any embodiment of the present application, the method includes at least one of the following conditions:
[0132] 1) A sealed annealing container contains an annealing atmosphere, wherein the annealing atmosphere includes a polar aprotic solvent; optionally, the polar aprotic solvent includes at least one of N,N-dimethylformamide, 1-methyl-2-pyrrolidone, dimethyl sulfoxide, and dimethylacetamide;
[0133] 2) The annealing temperature in the sealed annealing container is 100-180°C, and can be optionally 120-160°C;
[0134] 3) The annealing time in the sealed annealing container is 8 to 30 minutes, and can be optionally 10 to 20 minutes.
[0135] According to the embodiments of the present application, by regulating the annealing atmosphere, annealing temperature and annealing time in a closed annealing container, the crystallization quality of the perovskite compound grains, including the overall particle size, is comprehensively controlled, thereby improving the comprehensive performance of the solar cell, including the energy conversion efficiency.
[0136] In some embodiments, the closed oven has a first heating source and a second heating source. In some embodiments, the first heating source and the second heating source can be arranged opposite to each other, and the space in between is used to accommodate the structure to be prepared. The structure to be prepared can be a stacked first electrode layer, a first carrier layer and a mixture coated on the first carrier layer, and the mixture is used to prepare a light absorption layer. The first heating source and the second heating source can themselves heat the closed oven, and can also conduct heat from the heat source. In some embodiments, the closed oven includes a carrier, which contacts the edge of the structure to be prepared, and the middle of the structure to be prepared is suspended in the air. The position where the carrier contacts the structure to be prepared is ≤5mm away from the edge of the prepared structure. In some embodiments, along the direction of the first heating source and the second heating source arranged opposite to each other, the width of the cross section of the first heating substrate and the second heating substrate can be 5 to 100mm, preferably 20 to 80mm. In some embodiments, the surfaces of the first heating source and the second heating source are 28-32mm, optionally 30mm, away from the surface of the structure to be prepared.
[0137] Solar cell modules
[0138] The solar cell assembly provided in the embodiments of the present application may include one solar cell 10 according to the first aspect, or may include multiple solar cells according to the first aspect. If there are multiple solar cells, the multiple solar cells may be connected in series, in parallel, or in a hybrid connection. A hybrid connection refers to a connection of multiple solar cells in both series and parallel.
[0139] In some embodiments, the solar cell assembly includes a protective layer and / or an encapsulation layer.
[0140] [Protective layer]
[0141] A protective layer is disposed between the encapsulation layer and the solar cell and contains metal halides and / or organic halides. The metal halides and organic halides in the protective layer absorb infiltrating water and oxygen, reducing the erosion of the organic and inorganic perovskite compounds in the light-absorbing layer by water and oxygen, thereby improving the stability of the solar cell and thus helping to extend the service life of the solar cell.
[0142] In some optional embodiments of the present application, the metal halide has a general formula of BXk, wherein the value of k is in the range of 1 to 3. The organic halide has a general formula of AX.
[0143] In the above embodiments, the metal halide and the organic halide respectively have the above general formula, which can enable the protective layer to absorb water and oxygen while also generating substances similar to or identical to the precursor substances of the organic-inorganic perovskite compounds. These substances can react to generate perovskite compounds with functions similar to those of the organic-inorganic perovskite compounds, thereby allowing the solar cell to have a longer service life even when water and oxygen penetrate into it.
[0144] In some optional embodiments of the present application, the organic cation in the organic-inorganic perovskite compound and the organic cation in the organic halide are the same or are homologous to each other.
[0145] In this application, homologues refer to organic compounds with similar structures and molecular compositions that differ by several "CH2" atomic groups.
[0146] In the above embodiments, the organic cations in the general formula ABX3 and the organic cations in the general formula AX are the same or homologous to each other, which can help the organic halide in the protective layer 15 and the precursor material to form an organic-inorganic perovskite compound.
[0147] In some optional embodiments of the present application, the organic cation includes at least one of an amine group and an amine derivative, such as an alkylamine group.
[0148] In some optional embodiments of the present application, the amino group includes at least one of methylamino, ethylamino, propylamino, butylamino, pentylamino, hexylamino, and formamidinyl. The amino derivative includes imidazole.
[0149] For example, when the organic cation in the organic-inorganic perovskite compound is the same as the organic cation in the organic halide, the organic cation in the organic-inorganic perovskite compound is methylamine (CH3NH - ), then the organic cation in the organic halide is also methylamine (CH3NH - ).
[0150] For example, when the organic cation in the general formula ABX3 and the organic cation in the general formula AX are homologous to each other, the organic cation in the organic-inorganic perovskite compound is methylamine (CH3NH - ), the organic cation in the organic halide can be an ethylamine group (CH3CH2NH - ), propylamine (CH3CH2CH2NH - ).
[0151] In the embodiments of the present application, the protective layer may be a single-layer structure or a multi-layer structure, and the specific number of layers may be designed according to requirements.
[0152] In some optional embodiments of the present application, the protective layer comprises at least one of MOF material, activated carbon, montmorillonite, diatomaceous earth, zeolite, molecular sieve, kaolin, ion exchange resin and 2-methylimidazole zinc salt MAF-4 to provide a porous structure.
[0153] [Encapsulation layer]
[0154] The encapsulation layer can encapsulate the solar cell between the cover plate and the substrate to protect the solar cell.
[0155] The material of some optional encapsulation layers in the present application includes at least one of a thermoplastic encapsulation adhesive, a heat-curing encapsulation adhesive, and a light-curing encapsulation adhesive.
[0156] Exemplary thermoplastic encapsulants include at least one of ethylene-vinyl acetate copolymer, polyvinyl butyral, ethylene octene copolymer, polyisobutylene, polyolefin encapsulants, and butyl rubber. Thermal curing encapsulants include at least one of epoxy encapsulants, silicone encapsulants, and polyurethane encapsulants. Curing encapsulants include at least one of UV-curing encapsulants and infrared-curing encapsulants.
[0157] Electrical devices
[0158] In a third aspect, an embodiment of the present application provides an electrical device, comprising the solar cell assembly of the second aspect, wherein the solar cell assembly is used to provide electrical energy.
[0159] Electrical devices can be used in, but are not limited to, construction, military, travel, national defense, power supply and other fields, such as: mobile phones, tablets, laptops, electric toys, power tools, battery vehicles, electric cars, ships, spacecraft, photovoltaic greenhouses, photovoltaic water heaters, etc.
[0160]
[0161] The following examples describe the present disclosure in more detail and are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise indicated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and used directly without further processing, and all instruments used in the examples are commercially available.
[0162] Example 1
[0163] The present invention provides a method for manufacturing a solar cell module, which comprises the following steps:
[0164] (1) Forming a solar cell device: A set of FTO conductive glass with a size of 30 cm × 30 cm was etched with P1 using an infrared laser. The width of P1 was about 30 μm. The entire piece of glass was divided into 44 sub-cells along the long side. The series resistance of different sub-cells was greater than 10 MΩ. 10 mm above and below were used as the component welding area. The etched conductive glass surface was cleaned twice with acetone and isopropyl alcohol, immersed in deionized water for ultrasonic treatment for 10 minutes, and then dried in a forced air drying oven. It was placed in a drying room (humidity less than 2%) and used as the first electrode.
[0165] The cleaned conductive glass was placed in a magnetron sputtering process to deposit a hole transport layer of nickel oxide with a thickness of about 15 nm.
[0166] Apply a layer of FA using slot coating 0.95 Cs 0.05 The PbI3 perovskite main layer is formed, and a heated substrate is obtained. The substrate is then transferred to a vacuum device and evacuated for 60 seconds to a vacuum degree of 15 Pa. At this time, the closed oven has a trace amount of N,N-dimethylformamide solvent atmosphere. A closed oven non-contact annealing method is used. The closed oven structure is as follows: a. The closed oven structure consists of an upper heating source hot plate and a lower heating source hot plate. The four walls have heat exhaust holes that can be controlled to open and close and adjust the exhaust rate. The perovskite substrate to be heated is heated upward, and the upper heating source hot plate and the lower heating source are respectively 30mm away from the substrate surface; b. The carrier structure of the substrate to be heated is non-contact in the middle of the substrate, with only insulating pins at the four corners contacting the substrate edge by 5mm, so that the substrate to be heated is suspended inside the closed oven.
[0167] The annealing process involves uniform heating and slow crystallization, followed by annealing at 150°C for 10 minutes to form a light absorption layer with a thickness of approximately 500 nm.
[0168] The prepared device was placed in a vacuum thermal evaporation device, vacuumed to 4×10-4Pa, and 30nm C60 and 8nm BCP were deposited as the charge transport layer of the device;
[0169] After the charge transfer layer was deposited in the vacuum thermal evaporation device, 10 nm Ag was deposited on the surface and then the vacuum was broken and taken out. P2 was laser etched. The width of P2 was 150 μm and the depth was etched to the surface of the FTO layer. The interval between P2 and P1 was 20 μm. Then the substrate was placed in the evaporation device again and vacuumed to 4×10 -4 After Pa, a layer of Ag is continuously deposited with a thickness of about 80 nm;
[0170] After cooling, the vacuum is broken and the P second green laser is used to etch P3. The width of P3 is 15 μm and the depth is etched to the surface of the FTO layer. The interval between P3 and P2 is 20 μm (the positions of the etched lines are P1 / P2 / P3 in sequence).
[0171] (3) Edge cleaning: Use a laser marking machine to clean the coating in the area extending inward from the edge of the solar cell device to 0.1 cm.
[0172] (4) Glue application: Apply the encapsulation glue to the clean edge area.
[0173] (5) Lamination: The substrate, the adhesive-coated solar cell device, the encapsulation layer with a protective layer, and the cover plate are bonded together and laminated to obtain a solar cell module.
[0174] Examples 2-6
[0175] The difference between this embodiment and embodiment 1 is that the perovskite components used in the light absorption layer are different, which are detailed in Table 1.
[0176] Comparative Examples 1-3
[0177] The manufacturing methods of Comparative Examples 1-3 are similar to those of Example 1, except that the annealing method is to use a hot plate for direct contact annealing at 150° C. for 10 min. For details, please refer to Table 1.
[0178] Test section
[0179] Using a Zeiss (Carl Zeiss Jena, ZEISS) Gemini 360 field emission electron scanning microscope at 3 kV, with the lens at a distance of 4.9 to 5.1 mm from the sample surface, the surface morphology of the perovskite layer was imaged at a magnification of 5k to 10k, and the cross-section was imaged at a magnification of 20k. Cross-sections of the light absorbing layers prepared in Examples 1-3 were examined, as shown in Figures 4-6. The perovskite compound grains therein were found to have a particle size distribution of 1 to 6 μm. As shown in Figure 7, perovskite compound grains were observed to extend through the light absorbing layer.
[0180] Photoelectric conversion efficiency testing: At room temperature and pressure, using a standard AM1.5G sunlight simulating light source, a four-channel digital source meter (Keithley 2440) was used to measure the volt-ampere characteristic curves of the solar cells prepared in the examples and comparative examples under the illumination of the light source. The open circuit voltage Voc, short circuit current density Jsc, fill factor FF (Fill Factor), and energy conversion efficiency Eff (Efficiency) of the solar cells were obtained. The test results are shown in Table 1.
[0181] According to Table 1, by comparing the test results of Examples 1-10 and Comparative Examples 1-3, it can be seen that in the solar cells provided by the embodiments of the present application, the overall particle size of the perovskite compound grains of the embodiments is larger than the grain size of the comparative examples, which reduces the number of grain boundaries between the perovskite compound grains, reduces or avoids the interference of interface defects, promotes charge separation at the interface, and increases the open circuit voltage of the solar cell, thereby improving the comprehensive performance of the solar cell, including the energy conversion efficiency.
[0182] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
[0183]
[0184]
Claims
1. A solar cell comprising a light absorbing layer, The light absorbing layer comprises a plurality of perovskite compound grains, wherein: In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 1 μm to 6 μm is ≥90%.
2. The solar cell according to claim 1, wherein: In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a long diameter D of 2.0 μm to 5.0 μm is ≥ 75%; 3. The solar cell according to claim 1 or 2, wherein: In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 2.0 μm to 3.5 μm is ≥50%.
4. The solar cell according to any one of claims 1 to 3, wherein: In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D greater than or equal to 3.5 μm is 5%-30%; and / or, In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 2.5 μm to 3.0 μm is ≥ 60%; and / or, In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 1.0 μm to 2.5 μm is 20%-40%; and / or, In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D of 1.0 μm to 2.0 μm is 16.69%-20.9%; and / or, In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains with a major diameter D less than or equal to 1.0 μm is ≤8%.
5. The solar cell according to any one of claims 1 to 4, wherein: In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, perovskite compound crystal grains having a long diameter D of 1 μm to 6 μm are polygonal.
6. The solar cell according to any one of claims 1 to 5, wherein: In at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the perovskite compound grains with a long diameter D of 1 μm to 4 μm are N-gonal, where N is a positive integer and greater than 5.
7. The solar cell according to any one of claims 1 to 6, wherein: The light absorbing layer includes perovskite compound crystal grains penetrating the light absorbing layer in at least one cross section in a layer thickness direction.
8. The solar cell according to claim 7, wherein: The ratio of the perovskite compound grains running through the light absorbing layer to the total number of grains in the light absorbing layer is 50% to 90%.
9. The solar cell according to claim 7 or 8, wherein: The ratio of the perovskite compound grains running through the light absorbing layer to the total number of grains in the light absorbing layer is 60% to 85%.
10. The solar cell according to any one of claims 7 to 9, wherein: The perovskite compound grains include primary grains and secondary grains, and the number of the secondary grains accounts for 80%-100% of the total number of the perovskite compound grains.
11. The solar cell according to any one of claims 7 to 10, wherein: The perovskite compound grains include primary grains and secondary grains, and the number of the secondary grains accounts for 65%-95% of the total number of the perovskite compound grains.
12. The solar cell according to any one of claims 7 to 11, wherein: The solar cell comprises a first carrier transport layer and a second carrier transport layer, and the solar cell comprises: A passivation layer located between the light absorbing layer and the first carrier transporting layer and / or a passivation layer located between the light absorbing layer and the second carrier transporting layer; wherein the passivation layer is used to reduce defects when two interfaces are in contact.
13. A method for preparing a solar cell, the method comprising: A light absorbing layer comprising a plurality of perovskite compound grains as described in any one of claims 1 to 12 is prepared by a contactless sealed annealing container, wherein in at least one cross section of the light absorbing layer perpendicular to the layer thickness direction, the cumulative distribution rate of the number of perovskite compound grains having a long diameter D of 1 μm to 6 μm is ≥90%.
14. The preparation method according to claim 13, wherein: The method comprises one or more of the following conditions: 1) The sealed annealing container contains an annealing atmosphere, and the annealing atmosphere includes a polar aprotic solvent; optionally, the polar aprotic solvent includes N,N-dimethylformamide, 1-methyl-2-pyrrolidine At least one of ketone, dimethyl sulfoxide, and dimethylacetamide; 2) The annealing temperature in the sealed annealing container is 100-180°C; 3) The annealing time in the sealed annealing container is 8 to 30 minutes.
15. A solar cell assembly, comprising the solar cell according to any one of claims 1 to 12 or the solar cell prepared by the preparation method according to claim 13 or 14.
16. An electrical device comprising the solar cell assembly according to claim 15, wherein the solar cell assembly is used to provide electrical energy.
Citation Information
Patent Citations
Thermally stable inorganic perovskite thin film and preparation method thereof
CN112968129A
Polymer perovskite thin film, preparation method, application and flexible solar cell
CN113948641A
Trans-solar cell preparation method based on seed crystal induced growth perovskite thin film
CN114649482A
Monodisperse particle film, forming method thereof and photovoltaic cell
CN115732581A
Solar cell and laminated solar cell
CN115799359A
Cited By
CuO composite material, immunosensor as well as preparation method and application of immunosensor