Slurry for negative electrode sheet, negative electrode sheet and electrochemical device

By coating the slurry containing conductive material and polyfluoroolefin polymer on the negative electrode sheet to form an elastic functional layer, the battery capacity attenuation and safety performance problems caused by volume expansion of the alloy negative electrode material are solved, and the circulation of lithium-ion batteries is improved Performance and safety performance.

WO2024239812A1PCT designated stage expired Publication Date: 2024-11-28HUAWEI TECH CO LTD

Patent Information

Application Number
PCT/CN2024/086774
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-04-09
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The alloy negative electrode material expands in volume during the lithium-ion battery circulation, resulting in the destruction and pulverization of active substance particles, the battery capacity decays rapidly, and the solid electrolyte interface repeatedly destroys, affecting the circulation and safety performance.

Method used

Provide a slurry for the negative electrode sheet, including conductive material, polyfluoroolefin polymer and modified hydrogenated nitrile rubber, to form an elastic functional layer, improve the adhesion between the negative electrode sheet and the separator, and to alleviate volume Expansion, promotes electron transport, reduces impedance and polarization.

Benefits of technology

It improves the circulation and safety performance of the negative electrode plate, extends the service life of the battery, reduces the expansion damage of the electrode plate and the electronic path failure, and enhances the flatness and lithium replenishment efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024086774_28112024_PF_FP_ABST
    Figure CN2024086774_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A slurry for a negative electrode sheet, a negative electrode sheet and an electrochemical device. The slurry comprises a conductive material, a polyfluoroalkene polymer, modified hydrogenated butadiene-acrylonitrile rubber and a solvent. The surface of a negative electrode active material layer of the negative electrode sheet is provided with an elastic functional layer, which comprises a conductive material, a polyfluoroalkene polymer and modified hydrogenated butadiene-acrylonitrile rubber; and the elastic functional layer has good cohesiveness and elasticity, can improve the interface bonding performance between the negative electrode sheet and a separator and relieve the volume expansion of the electrode sheet, and can further promote the electron transport and reduce the impedance and polarization of the negative electrode sheet, thereby further improving the cycle performance and safety performance of a battery during use.
Need to check novelty before this filing date? Find Prior Art

Description

Slurry for negative electrode sheet, negative electrode sheet and electrochemical device

[0001] This application claims priority to the Chinese patent application filed with the State Intellectual Property Office of China on May 22, 2023, with application number 202310582265.6 and application name “Slurry for negative electrode sheet, negative electrode sheet and electrochemical device”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of electrochemical technology, and in particular to a slurry for a negative electrode sheet, a negative electrode sheet, and an electrochemical device. Background Art

[0003] Lithium-ion batteries, with their high specific energy, long cycle life, high operating voltage, and wide operating temperature range, are widely used in portable electronic devices, electric vehicles, and other fields. With the rapid development of electric vehicles, demands for lithium-ion batteries' energy density and cycle performance are increasing. Alloy anode materials, with their higher specific capacities (Si ~4200mAh / g, P ~2760mAh / g), are considered a promising class of anode materials.

[0004] However, the volume expansion of alloy negative electrode materials during the cycle of lithium-ion batteries is large, which can easily cause the destruction and crushing of active material particles, resulting in rapid battery capacity decay; at the same time, the large volume expansion leads to repeated destruction and generation of the solid electrolyte interface film (SEI), resulting in an increase in by-products and high electrolyte consumption, and is more prone to gas production, thereby affecting the battery's cycle performance and safety performance.

[0005] Application Contents

[0006] The purpose of the present application is to provide a slurry for a negative electrode sheet, a negative electrode sheet and an electrochemical device. The slurry for a negative electrode sheet provided in the present application is coated on the surface of the negative electrode sheet to form an elastic functional layer. The elastic functional layer has excellent adhesion and elasticity, which can improve the interface adhesion performance between the negative electrode sheet and the separator, alleviate the volume expansion of the sheet, promote electron transmission, reduce the impedance and polarization of the negative electrode sheet, thereby further improving the cycle performance and safety performance of the battery during use.

[0007] In a first aspect, the present application provides a slurry for a negative electrode plate, the slurry comprising a conductive material, a polyfluoroolefin polymer, a modified hydrogenated nitrile rubber and a solvent.

[0008] In some embodiments, the polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of a monomer containing a polar functional group.

[0009] In some embodiments, the fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, ethylene fluoride, trifluoroethylene, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.

[0010] In some embodiments, the general structural formula of the polar functional group-containing olefin monomer is R1CH=CR1R2, wherein R1 is selected from H or CH3, and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3 or CN.

[0011] In some embodiments, based on the total mass of the components in the slurry excluding the solvent, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material is (2-4):(2-4):(2-4).

[0012] In some embodiments, the solid content of the slurry is 5 wt% to 10 wt%.

[0013] In some embodiments, the modified hydrogenated nitrile rubber contains acrylonitrile, and the mass content of acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%.

[0014] In some embodiments, the viscosity of the slurry is 100 cP to 2000 cP.

[0015] In some embodiments, the conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, and graphene.

[0016] In some embodiments, the solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, n-hexane, or N-methylpyrrolidone.

[0017] In a second aspect, the present application provides a negative electrode plate, the negative electrode plate comprising:

[0018] A negative electrode current collector, a negative electrode active material layer disposed on the negative electrode current collector; and

[0019] An elastic functional layer covers the surface of the negative electrode active material layer, and the elastic functional layer includes a conductive material, a polyfluoroolefin polymer and a modified hydrogenated nitrile rubber.

[0020] In some embodiments, the polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of a monomer containing a polar functional group.

[0021] In some embodiments, the fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, ethylene fluoride, trifluoroethylene (TrFE), tetrafluoroethylene (TFE), chlorotrifluoroethylene (CTFE), hexafluoropropylene (HFP), and the like.

[0022] In some embodiments, the general structural formula of the monomer containing a polar functional group is R1CH=CR1R2, wherein R1 is selected from H or CH3, and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3 or CN.

[0023] In some embodiments, the modified hydrogenated nitrile rubber is obtained by polymerizing ethylene and acrylonitrile.

[0024] In some embodiments, the molar ratio of the acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%.

[0025] In some embodiments, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber, and the conductive material is (2-4):(2-4):(2-4).

[0026] In some embodiments, the thickness of the negative electrode current collector is 5 μm to 15 μm.

[0027] In some embodiments, the thickness of the negative electrode active material layer is 10 μm to 70 μm.

[0028] In some embodiments, the elastic functional layer has a thickness of 1 μm to 5 μm.

[0029] In some embodiments, the negative electrode sheet includes a negative electrode active material.

[0030] In some embodiments, the negative electrode active material includes a silicon-based material, and the silicon-based material is selected from at least one of elemental silicon, silicon-oxygen compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys.

[0031] In some embodiments, the negative electrode active material includes a phosphorus-based material, and the phosphorus-based material includes at least one of elemental phosphorus and a phosphorus-carbon composite.

[0032] In some embodiments, the conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, and graphene.

[0033] In a third aspect, the present application provides an electrochemical device, comprising the negative electrode sheet described in the second aspect.

[0034] In a fourth aspect, the present application further provides an electronic device, which is the electrochemical device described in the third aspect.

[0035] Compared with the prior art, this application has at least the following beneficial effects:

[0036] The slurry for the negative electrode provided herein comprises a conductive material, a polyfluoroolefin polymer, a modified hydrogenated nitrile rubber, and a solvent. The polyfluoroolefin polymer can enhance the adhesion of the elastic functional layer formed by coating the slurry; it can form a miscible layer with polymer materials such as polyvinylidene fluoride (PVDF) in the separator coating during the shaping and hot pressing process, enhancing the adhesion between the separator and the negative electrode, thereby improving the contact interface; it also provides mechanical strength. The synergistic effect of the polyfluoroolefin polymer and the modified hydrogenated nitrile rubber can adjust the toughness and elasticity of the elastic functional layer, achieving a toughening effect.

[0037] Second, modified hydrogenated nitrile rubber is used as a dispersant to improve the uniformity of the dispersion of the conductive material in the slurry, inhibit the pulverization or agglomeration of the conductive material in the slurry, and make the slurry have both low solid content and high stability; thereby, the elastic functional layer formed by the slurry coating can buffer the volume expansion of the negative electrode plate, and its excellent elasticity can adapt to the extension of the plate caused by the volume expansion and prevent it from falling off the plate.

[0038] Third, the conductive material in the slurry is evenly dispersed, so that the elastic functional layer formed by the slurry coating has excellent conductivity and equipotentiality. When electrons come into contact with the elastic functional layer, the electric field on the surface of the electrode can be evenly dispersed, promoting the uniform deposition of ions, improving the cycle life and safety performance of the battery, and providing an electron path for the lithium insertion / extraction / replenishment process.

[0039] In the negative electrode provided by the present application, the elastic functional layer covers the surface of the negative electrode active material layer; first, the elastic functional layer can make the negative electrode plate and the diaphragm have an excellent bonding effect, which can improve the stress distribution of the plate, alleviate the problems of interface expansion and battery cell deformation, thereby further improving the cycle life and safety performance of the battery during actual use; second, the elastic functional layer has excellent elasticity and buffering performance (functional layer deformation force < plate adhesion force and plate expansion stress and interface shaping force), which can reduce the extrusion and expansion damage of particles to the negative electrode plate, alleviate the volume expansion of the negative electrode plate during the cycle, and also alleviate the shedding of some particles and the destruction of the electron path due to particle expansion and crushing, inhibiting the active material from falling off. The cycle capacity attenuation phenomenon caused by mass loss can improve the flatness of the negative electrode surface, thereby improving the cycle performance and safety performance of the battery; finally, the conductive material in the elastic functional layer makes the elastic functional layer have equipotentiality. When electrons contact the elastic functional layer, the electric field on the surface of the electrode can be dispersed, promoting electron transmission and reducing the impedance and polarization of the negative electrode; and acting as a lithium replenishment buffer layer, reducing the interfacial side reactions caused by direct contact between metallic lithium and the negative electrode active material layer during the metal lithium replenishment process, thereby improving the lithium replenishment efficiency; in the late cycle, the elastic functional layer can also ensure the complete electronic path of the electrode, so that the electric field on the surface of the electrode is dispersed, promoting the uniform deposition of lithium ions, thereby improving the cycle performance and safety performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The present application is further described below with reference to the accompanying drawings and examples.

[0041] FIG1 is a schematic diagram of a lithium-ion battery provided by the present application;

[0042] FIG2 is a schematic diagram of the structure of the negative electrode sheet provided in this application;

[0043] FIG3 is a schematic diagram of the bonding between the negative electrode sheet and the separator provided in the present application;

[0044] FIG4 is a schematic diagram of the surface flatness of the negative electrode plate after cycling provided by the present application;

[0045] FIG5 is a schematic diagram of the conductive performance of the elastic functional layer of the negative electrode provided by the present application;

[0046] FIG6 is a SEM image of the negative electrode sheet provided in Example 1 of the present application;

[0047] FIG7 a is a schematic diagram of the surface flatness of the negative electrode sheet after cycling provided in Example 1 of the present application;

[0048] FIG7 b is a partial SEM image of the negative electrode sheet provided in Example 1 of the present application after cycling;

[0049] FIG8a is a schematic diagram of the surface flatness of the negative electrode plate after cycling provided in Comparative Example 1 of the present application;

[0050] FIG8b is a partial SEM image of the negative electrode sheet provided in Comparative Example 1 of the present application after cycling;

[0051] FIG9 is a schematic diagram of the cycle capacity retention rate of the lithium-ion batteries provided in Example 1 and Comparative Example 1 of the present application.

[0052] In Figure 2:

[0053] 1- negative electrode current collector;

[0054] 2-negative electrode active material layer;

[0055] 3- Elastic functional layer. DETAILED DESCRIPTION

[0056] In order to better understand the technical solutions of this specification, the embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0057] It should be clear that the embodiments described are only part of the embodiments of this specification, not all of the embodiments. Based on the embodiments in this specification, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this specification.

[0058] The terms used in the examples of this application are for the purpose of describing specific embodiments only and are not intended to limit this specification. The singular forms "a," "an," "the," and "the" used in the examples of this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise.

[0059] Figure 1 is a schematic diagram of the lithium-ion battery provided by the present application. As shown in Figure 1, it includes a positive electrode sheet, a negative electrode sheet, an electrolyte, a diaphragm and a corresponding circuit, wherein the lithium-ion battery realizes energy storage and release by the intercalation and deintercalation of lithium ions between the positive and negative electrodes. The electrolyte is a carrier for the transmission of lithium ions between the positive and negative electrodes. The ion-conducting but electronically insulating diaphragm ensures the migration of lithium ions while separating the positive and negative electrodes to prevent short circuits. The positive and negative active materials are the main parts of the lithium battery that perform the energy storage function and determine the energy density, cycle performance and safety performance of the battery cell. After determining the positive electrode material system, the capacity of the negative electrode material is crucial to the improvement of the energy density of the entire battery cell.

[0060] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer located on the surface of the positive electrode current collector, and the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located on the surface of the negative electrode current collector.

[0061] Battery energy density is positively correlated with the negative electrode gram capacity. Compared with graphite materials (theoretical capacity 372 mAh / g), the use of alloy negative electrode materials with higher gram capacity (Si ~ 4200 mAh / g, P ~ 2760 mAh / g) is undoubtedly the preferred route to improve battery energy density. However, alloy negative electrode materials undergo a huge volume change (200% ~ 300%) during battery cycling. This dramatic volume change has the following negative effects: (1) The negative electrode sheet expands significantly, and the alloy particles are destroyed and crushed, resulting in rapid battery capacity decay; (2) The lithium intercalation alloying reaction rate is poor; (3) The first cycle coulombic efficiency is low, requiring additional active lithium to be supplemented; (4) The solid electrolyte interface (SEI) of the alloy negative electrode material is repeatedly destroyed and generated during cycling, resulting in a large number of by-products and high electrolyte consumption, and is more prone to gas generation, which will reduce the contact interface between the negative electrode sheet and the separator, and also have a significant impact on the interfacial bonding performance between the positive and negative electrode sheets and the separator, thereby affecting the battery's cycle performance and safety performance. The existence of these problems has hindered the commercialization of alloy negative electrode materials.

[0062] In some embodiments, the negative electrode plate includes a lithium metal layer or a current collector, and a functional layer is provided on the surface of the lithium metal layer, the functional layer including M conductive layers and N dielectric layers stacked in layers, the conductive layer including a lithium wetting material; wherein M ≥ 1, N ≥ 1. The dielectric layer can more effectively reduce the electron concentration on the surface of the functional layer, forcing lithium ions to enter the interior of the functional layer for deposition, reducing lithium deposition at the negative electrode interface, thereby inhibiting the formation of lithium dendrites at the negative electrode interface and improving the cycle life and safety performance of the electrochemical device. Although this approach can improve the cycle life and safety performance of the electrochemical device, the dielectric layer is an insulating layer, which will increase the contact impedance of the electrode interface, thereby increasing polarization, which will have a harmful effect on the cycle performance and capacity of the battery.

[0063] In other embodiments, the functional layer may also include a catechol-structured polymer compound. Such a compound can prevent oxidation of the current collector substrate and prevent dissolution or precipitation of the current collector substrate when charging the lithium-ion battery in an over-discharge state. Similarly, such a functional layer is an insulating layer and can increase the contact impedance of the electrode interface, thereby increasing polarization and adversely affecting the battery's cycle performance and capacity.

[0064] Therefore, how to make the electrochemical device have both excellent cycle performance and safety performance, improve the interfacial adhesion between the negative electrode plate and the separator, and at the same time reduce the impedance and polarization of the negative electrode plate, alleviate volume expansion, etc., is still the goal that has been explored.

[0065] Based on this, in a first aspect, the present application provides a slurry for a negative electrode plate, the slurry comprising a conductive material, a polyfluoroolefin polymer, a modified hydrogenated nitrile rubber and a solvent.

[0066] The slurry for the negative electrode provided herein comprises a conductive material, a polyfluoroolefin polymer, a modified hydrogenated nitrile rubber, and a solvent. The polyfluoroolefin polymer improves the adhesion of the elastic functional layer formed by coating the slurry. It also forms a miscible layer with polymers such as polyvinylidene fluoride in the separator coating during the hot-pressing process, enhancing the adhesion between the separator and the negative electrode, thereby improving the contact interface. The slurry also provides mechanical strength. The synergistic effect of the polyfluoroolefin polymer and the modified hydrogenated nitrile rubber adjusts the toughness and elasticity of the elastic functional layer, achieving a toughening effect.

[0067] Second, modified hydrogenated nitrile rubber is used as a dispersant to improve the uniformity of the dispersion of the conductive material in the slurry, inhibit the pulverization or agglomeration of the conductive material in the slurry, and make the slurry have both low solid content and high stability; thereby, the elastic functional layer formed by the slurry coating can buffer the volume expansion of the negative electrode plate, and its excellent elasticity can also adapt to the extension of the plate caused by the volume expansion and prevent it from falling off the plate.

[0068] Third, the conductive material in the slurry is evenly dispersed, so that the elastic functional layer formed by the slurry coating has excellent conductivity and equipotentiality. When electrons come into contact with the elastic functional layer, the electric field on the surface of the electrode can be evenly dispersed, promoting the uniform deposition of ions, improving the cycle life and safety performance of the battery, and providing an electron path for the lithium insertion / extraction / replenishment process.

[0069] In some embodiments, the polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of an olefin monomer containing a polar functional group.

[0070] In some embodiments, the fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, ethylene fluoride, trifluoroethylene (TrFE), tetrafluoroethylene (TFE), chlorotrifluoroethylene (CTFE), hexafluoropropylene (HFP), and the like.

[0071] In some embodiments, the polar functional group-containing monomer has a general structural formula of R1CH=CR1R2, wherein R1 is selected from H or CH3; and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3, or CN. It is understood that the polar functional group may be a carbonate group, carboxyl group, amino group, amide group, imide group, cyano group, or the like. Because these polar functional groups have good affinity with polymer materials such as polyvinylidene fluoride in the separator coating, during the hot pressing process, the separator coating and the polymer molecular chains in the elastic functional layer can be entangled and mutually dissolved. After hot pressing, the elastic functional layer can form a complete interface with the surface of the negative electrode active material layer and the negative electrode plate, thereby improving the contact interface and the interfacial adhesion between the negative electrode plate and the separator.

[0072] Optionally, the molar proportion of the fluorine-containing olefin monomer in the polyfluoroolefin polymer can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%, etc., and of course it can also be other values ​​between 20% and 60%, which is not limited here.

[0073] Optionally, the molar proportion of the polar functional group-containing olefin monomer in the polyfluoroolefin polymer can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%, etc., and of course it can also be other values ​​between 40% and 80%, which is not limited here.

[0074] It can be understood that the presence of polar functional groups in the polymer molecular chain can increase the adhesion of the polymer. The polyfluoroolefin polymer in the present application is obtained by copolymerization of fluorine-containing olefin monomers and olefin monomers containing polar functional groups. Therefore, the molecular chain structure of the polyfluoroolefin polymer in the present application contains polar functional groups, which can improve the adhesion of the polyfluoroolefin polymer; therefore, using it in the above-mentioned slurry can improve the adhesion between the negative electrode plate and the separator, thereby improving the cycle performance and safety performance of the battery.

[0075] In some embodiments, based on the total mass of the components in the slurry excluding the solvent, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber, and the conductive material is (2-4):(2-4):(2-4). Specifically, the mass ratio of the conductive material, the polyfluoroolefin polymer, and the modified hydrogenated nitrile rubber can be 2:2:4, 2:3:4, 2:4:4, 3:2:4, 3:3:4, 3:4:3, 4:2:4, or 4:4:2, etc., which are not limited here. Preferably, the mass ratio of the polyfluoroolefin polymer: the modified hydrogenated nitrile rubber: the conductive material is (2-3):(3-4):(3-4).

[0076] In some embodiments, the solid content of the slurry is 5wt% to 10wt%, specifically 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt% or 10wt%, etc. Of course, it can also be other values ​​within the above range, which is not limited here.

[0077] In some embodiments, the modified hydrogenated nitrile rubber contains acrylonitrile, and the mass content of the acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%. The mass content of the acrylonitrile in the modified hydrogenated nitrile rubber can specifically be 20%, 25%, 30%, 35%, 40%, 41%, 42%, 43%, 44% or 45%, etc., and of course it can also be other values ​​within the above range, which is not limited here. Controlling the acrylonitrile content within the above range is conducive to making the elastic functional layer formed by the slurry have excellent elasticity, while being able to adapt to the extension of the pole piece caused by volume expansion and not falling off the pole piece.

[0078] In some embodiments, the viscosity of the slurry is 100cP to 2000cP, specifically 100cP, 200cP, 300cP, 400cP, 500cP, 700cP, 800cP, 1000cP, 1500cP, 1800cP or 2000cP, etc., which are not limited here. It is understandable that a slurry with too high or too low viscosity is not conducive to electrode coating. A slurry with high viscosity is not easy to precipitate and has better dispersibility, but when the viscosity of the slurry is too high, it is not conducive to the leveling effect and is not conducive to electrode coating; when the slurry viscosity is low, although the slurry has good fluidity, it is difficult to dry, which reduces the drying efficiency of the coating, and may also cause problems such as coating cracking, slurry particle agglomeration, and poor surface density consistency.

[0079] In some embodiments, the conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, and graphene. The conductive material can be evenly dispersed in the elastic functional layer, imparting excellent conductivity and equipotentiality to the functional layer. When electrons contact the functional layer, the electric field on the electrode surface is evenly dispersed, promoting uniform ion deposition, improving the battery's cycle life and safety, and providing an electron pathway for lithium insertion / extraction and replenishment.

[0080] In some embodiments, the solvent is selected from at least one of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), dimethyl sulfoxide (DMSO), n-hexane, or N-methylpyrrolidone (NMP). It is understood that the polymer can be dissolved in the solvent.

[0081] In a second aspect, as shown in FIG2 , the present application provides a negative electrode plate, the negative electrode plate comprising:

[0082] A negative electrode current collector 1, a negative electrode active material layer 2 provided on the negative electrode current collector 1; and

[0083] The elastic functional layer 3 covers the surface of the negative electrode active material layer 2 . The elastic functional layer 3 includes a conductive material, a polyfluoroolefin polymer and a modified hydrogenated nitrile rubber.

[0084] In the negative electrode plate provided by the present application, the elastic functional layer covers the surface of the negative electrode active material layer; first, the elastic functional layer can make the negative electrode plate and the separator have an excellent bonding effect, which can improve the stress distribution of the plate, alleviate the problems of interface expansion and battery cell deformation, thereby further improving the cycle life and safety performance of the battery during actual use; second, the elastic functional layer has excellent elasticity and buffering performance (functional layer deformation force < plate adhesion force and plate expansion stress and interface shaping force), which can reduce the extrusion and expansion damage of particles to the negative electrode plate, alleviate the volume expansion of the negative electrode plate during the cycle, and also alleviate the shedding of some particles and the electric shock caused by particle expansion and crushing. The sub-pathway is destroyed, the cycle capacity attenuation phenomenon caused by the loss of active materials is suppressed, and the flatness of the surface of the negative electrode plate can be improved, thereby improving the cycle performance and safety performance of the battery; finally, the conductive material in the elastic functional layer makes the elastic functional layer have equipotentiality. When electrons contact the elastic functional layer, the electric field on the surface of the electrode plate can be dispersed, which promotes electron transmission and reduces the impedance and polarization of the negative electrode plate; and acts as a lithium replenishment buffer layer to reduce the side reaction of the lithium replenishment interface and improve the lithium replenishment efficiency; in the late cycle, the elastic functional layer can also ensure the complete electronic path of the electrode plate, so that the electric field on the surface of the electrode plate is dispersed, and promotes the uniform deposition of lithium ions, thereby improving the cycle performance and safety performance of the battery.

[0085] FIG2 is a schematic structural diagram of the negative electrode sheet provided in the present application. As shown in FIG2 , the negative electrode sheet has a negative electrode active material layer 2 and an elastic functional layer 3 on both sides.

[0086] When preparing the negative electrode sheet as shown in FIG2 , the preparation method includes the following steps:

[0087] Step S1: adding a conductive material, a polyfluoroolefin polymer, and a modified hydrogenated nitrile rubber into an organic solvent according to a preset ratio, and mixing them uniformly to obtain an elastic functional layer slurry;

[0088] Step S2: adding the negative electrode active material and the conductive material to the binder and mixing them uniformly to obtain a negative electrode active material slurry;

[0089] Step S3: coating the negative electrode active material slurry on the surface of the negative electrode current collector and drying to obtain a negative electrode sheet having a negative electrode active material layer;

[0090] Step S4: coating the elastic functional layer slurry on the surface of the negative electrode active material layer, and drying to obtain a negative electrode sheet having the negative electrode active material layer and the elastic functional layer.

[0091] Wherein, in step S4, the method of coating the elastic functional layer slurry on the surface of the negative electrode active material layer includes at least one of transfer coating or doctor blade coating.

[0092] In some embodiments, the material of the negative electrode current collector includes at least one of copper foil, copper mesh, carbon-coated copper foil, stainless steel foil, or carbon-coated stainless steel foil.

[0093] In some embodiments, the organic solvent includes at least one of N-methylpyrrolidone, ethanol, and acetone. Preferably, the organic solvent is N-methylpyrrolidone.

[0094] In some embodiments, the polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of a monomer containing a polar functional group.

[0095] Optionally, the molar proportion of the fluorine-containing olefin monomer in the polyfluoroolefin polymer can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%, etc., and of course it can also be other values ​​between 20% and 60%, which is not limited here.

[0096] Optionally, the molar proportion of the polar functional group-containing monomer in the polyfluoroolefin polymer can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%, etc., and of course it can also be other values ​​between 40% and 80%, which is not limited here.

[0097] In some embodiments, the fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, ethylene fluoride, trifluoroethylene (TrFE), tetrafluoroethylene (TFE), chlorotrifluoroethylene (CTFE), hexafluoropropylene (HFP), and the like.

[0098] In some embodiments, the general structural formula of the monomer containing a polar functional group is R1CH=CR1R2, wherein R1 is selected from H or CH3, and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3, or CN. It is understood that the polar functional group can be a carbonate group, a carboxyl group, an amino group, an amide group, an imide group, a cyano group, or the like. Since these polar functional groups have good affinity with polymer materials such as polyvinylidene fluoride in the separator coating, during the hot pressing process, the separator coating and the polymer molecular chains in the elastic functional layer can be entangled and mutually dissolved. After hot pressing, the elastic functional layer can form a complete interface with the surface of the negative electrode active material layer and the negative electrode plate, thereby improving the contact interface and improving the interfacial adhesion between the negative electrode plate and the separator.

[0099] In the above scheme, by introducing polar groups into the polyfluoroolefin polymer structure, the adhesion of the polyfluoroolefin polymer is further improved, so that the elastic functional layer and the separator have excellent bonding effect, thereby improving the adhesion between the negative electrode plate and the separator, and improving the cycle performance and safety performance of the battery; and the synergistic effect of the polyfluoroolefin polymer and the modified hydrogenated nitrile rubber can also adjust the balance between the toughness and elasticity of the elastic functional layer, thereby achieving a toughening effect.

[0100] Figure 3 is a schematic diagram of the adhesion between the negative electrode plate and the diaphragm provided in the present application. As shown in Figure 3, the elastic functional layer has good affinity with the diaphragm coating. During the hot pressing process, the polymer molecular chains in the diaphragm coating and the elastic functional layer can be entangled and dissolved. After hot pressing, the elastic functional layer can form a complete interface with the surface of the negative electrode plate of the negative electrode active material layer, thereby improving the contact interface, improving the interface adhesion between the negative electrode plate and the diaphragm, and then improving the interface adhesion between the negative electrode plate and the diaphragm.

[0101] In some embodiments, the modified hydrogenated nitrile rubber is obtained by polymerizing ethylene and acrylonitrile. The modified hydrogenated nitrile rubber of the present application, as a dispersant, can improve the uniformity of the dispersion of the conductive material in the slurry, inhibiting pulverization or agglomeration of the conductive material in the slurry, thereby achieving both low solid content and high stability in the slurry. Furthermore, the elastic functional layer formed by the slurry coating can buffer the volume expansion of the side near the negative electrode. Its excellent elasticity can adapt to the extension of the electrode due to volume expansion and prevent it from falling off the electrode.

[0102] Figure 4 is a schematic diagram of the surface flatness of the negative electrode plate after cycling provided by the present application. As shown in Figure 4, the elastic functional layer has excellent elasticity and buffering properties, and the deformation force of the elastic functional layer is smaller than the adhesion force, expansion stress and interface shaping force of the negative electrode plate, which can reduce the extrusion and expansion damage of the negative electrode active material particles to the negative electrode plate, alleviate the volume expansion of the negative electrode plate during the cycle, thereby improving the flatness of the negative electrode plate surface and the battery cell, and further improving the cycle performance and safety performance of the battery.

[0103] In some embodiments, the molar percentage of acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%. Specifically, the molar percentage of acrylonitrile in the modified hydrogenated nitrile rubber and / or its derivatives can be 20%, 25%, 30%, 35%, 40%, 41%, 42%, 43%, 44% or 45%, etc. Of course, other values ​​between 20% and 45% can also be used, which is not limited here.

[0104] In some embodiments, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber, and the conductive material is (2-4): (2-4): (2-4). Specifically, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber, and the conductive material can be 2:2:4, 2:3:4, 2:4:3, 2:4:4, 3:2:4, 3:3:4, 3:4:3, 4:2:4, or 4:4:2, etc., and is not limited here. Preferably, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber, and the conductive material is (2-3): (3-4): (3-4).

[0105] In some embodiments, the solid content of the elastic functional layer slurry is 5wt% to 10wt%, specifically 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt% or 10wt%, etc. Of course, it can also be other values ​​within the above range, which is not limited here.

[0106] In some embodiments, the conductive material of the elastic functional layer includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, and graphene.

[0107] Figure 5 is a schematic diagram of the conductive performance of the elastic functional layer of the negative electrode provided in the present application. As shown in Figure 5, it can be understood that the conductive material is evenly dispersed in the elastic functional layer, so that the elastic functional layer has excellent conductivity and equipotentiality. When electrons contact the elastic functional layer, the electric field on the surface of the electrode can be evenly dispersed, promoting the uniform deposition of ions, improving the cycle life and safety performance of the battery, and providing an electron path for the lithium insertion / extraction / lithium replenishment process; the conductive material can also improve the electronic conductivity of the electrode without providing additional capacity and causing additional chemical reactions; in addition, the conductive material can also reduce the impedance of the negative electrode and improve the battery rate performance.

[0108] In some embodiments, the thickness of the negative electrode current collector is 5 μm to 15 μm, specifically 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or 15 μm, etc. Of course, it can also be other values ​​within the above range, which is not limited here.

[0109] In some embodiments, the thickness of the negative electrode active material layer is 10 μm to 70 μm. Specifically, the thickness of the negative electrode active material layer can be 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, or 70 μm, etc., without limitation herein.

[0110] In some embodiments, the thickness of the elastic functional layer is 1 μm to 5 μm, specifically 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm or 5 μm, etc. Of course, it can also be other values ​​within the above range, which is not limited here. It can be understood that if the elastic functional layer is too thin, the elastic functional layer may not cover the negative electrode material layer perfectly, and it will not be able to buffer the volume expansion of the negative electrode sheet and improve the interface bonding performance between the negative electrode sheet and the separator; if the elastic functional layer is too thick, it is equivalent to increasing the thickness of the negative electrode sheet in disguise, which will cause the overall energy density of the battery cell to decrease, which is not conducive to improving the energy density of the lithium-ion battery. Therefore, controlling the thickness of the elastic functional layer within the above range can, on the one hand, alleviate the volume expansion of the negative electrode sheet during the cycle; on the other hand, it is also beneficial to improve the energy density of the lithium-ion battery. Preferably, the thickness of the elastic functional layer is 2 μm to 3 μm.

[0111] In some embodiments, the negative electrode active material layer includes a negative electrode active material. Specifically, the negative electrode active material includes a silicon-based material, and the silicon-based material is selected from at least one of elemental silicon, a silicon oxide, a silicon-carbon composite, a silicon-nitrogen composite, and a silicon alloy. Exemplarily, the silicon oxide may be silicon monoxide.

[0112] In some embodiments, the silicon-carbon composite can be a silicon-carbon composite material obtained by carbon coating a silicon material, a silicon-carbon composite material obtained by sintering a silicon material, a silicon-carbon composite material obtained by ball milling a silicon material and a carbon material, or a silicon-carbon composite material obtained by chemical vapor deposition a silicon material and a carbon material, etc., and is not limited here.

[0113] In some embodiments, the negative electrode active material may further include a phosphorus-based material, wherein the phosphorus-based material includes at least one of elemental phosphorus and a phosphorus-carbon composite. For example, the elemental phosphorus includes at least one of red phosphorus, black phosphorus, purple phosphorus, or blue phosphorus.

[0114] In some embodiments, the phosphorus-carbon composite is prepared by compounding elemental phosphorus and carbon material by ball milling or vapor deposition, and the carbon material includes at least one of graphite, carbon nanotubes, porous carbon, hard carbon, soft carbon or graphene, which is not limited here.

[0115] In some embodiments, the negative electrode active material further includes a carbon-based negative electrode material, the carbon-based negative electrode material includes at least one of graphite, hard carbon, soft carbon, carbon nanotubes and graphene, and the graphite includes at least one of natural graphite, artificial graphite and surface-modified natural graphite.

[0116] In some embodiments, the negative electrode active material layer further includes a binder, and the binder includes at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyimide, polyacrylic acid, polyacrylonitrile, and polyvinyl alcohol. It is understood that the binder can bond the negative electrode active material, the conductive material, and the negative electrode current collector, thereby enhancing contact between the negative electrode active material, the conductive material, and the negative electrode current collector, while also ensuring the integrity of the electrode structure and ensuring normal charge and discharge cycles of the battery.

[0117] In a third aspect, the present application provides an electrochemical device, comprising the negative electrode sheet described in the second aspect. It is understood that, in addition to the negative electrode sheet, the electrochemical device generally also includes a positive electrode sheet, a separator, and an electrolyte; the positive electrode sheet includes a positive electrode active material, a conductive material, and a binder, wherein the positive electrode active material includes at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, or a ternary material; the conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, and graphene; and the binder is polyvinylidene fluoride (PVDF).

[0118] In the above-mentioned electrochemical device, the electrolyte includes a lithium salt and a solvent. The lithium salt includes at least one of lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), and lithium trifluoromethanesulfonate (LiCF3SO3); and the solvent includes at least one of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). The electrolyte also includes additives. The type of additive is not particularly limited and can be a negative electrode film-forming additive, a positive electrode film-forming additive, or an additive capable of improving certain battery properties, such as an additive that improves battery overcharge performance, an additive that improves battery high-temperature performance, or an additive that improves battery low-temperature performance.

[0119] In a specific embodiment, the electrochemical device may be a primary battery, a secondary battery, a solid-state battery, or a lithium-ion battery, which is not limited here.

[0120] In a fourth aspect, the present application further provides an electronic device, comprising the electrochemical device described in the third aspect. The electrochemical device of the present application has excellent cycle performance and safety performance. Therefore, when the electrochemical device is used in an electronic device, the electronic device has excellent safety performance and can also extend the service life of the electronic device.

[0121] The electronic devices in this application can specifically be mobile phones, computers, tablet computers, smart bracelets, smart watches, etc., and are not limited here.

[0122] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application should be included in the scope of protection of the present application.

[0123] The present application will be further described below using lithium-ion batteries as an example through specific embodiments and comparative examples.

[0124] Example 1

[0125] (1) Preparation of slurry for negative electrode (elastic functional layer slurry)

[0126] 1.0 g of raw materials of polyfluoroolefin polymer (including 80 mol% of vinylidene fluoride and 20 mol% of monomer containing polar functional group: CH2=CHCOOCH3) and 2.0 g of modified hydrogenated nitrile rubber (including 36% of acrylonitrile) were added to 95 g of N-methylpyrrolidone (NMP) and stirred at room temperature until the reactants were completely dissolved; then 2.0 g of conductive carbon black was added and stirred at room temperature for 24 hours. After being evenly mixed, an elastic functional layer slurry with a solid content of 5 wt% was obtained.

[0127] (2) Preparation of negative electrode sheet

[0128] 80g SiO (Shin-Etsu Chemical) and 10g SP conductive carbon black were added to 70g modified polyacrylic acid binder solution (Chengdu Indile PAA, solid content 7wt%), stirred and mixed for 10 minutes, deionized water was added to adjust the solid content and viscosity, and stirred evenly to obtain a uniform negative electrode slurry; the negative electrode slurry was coated on one surface of a 10μm thick copper foil current collector and dried at 100°C for 12h to obtain a negative electrode active material layer. The above steps were then repeated on the other surface of the negative electrode sheet. After roller pressing, a negative electrode sheet with a negative electrode active material layer on both sides was obtained, wherein the negative electrode sheet compaction density was 1.2g / cm 3 , active material loading is 3 mg / cm 2 .

[0129] The elastic functional layer slurry is then applied to the surface of one of the negative electrode active material layers and dried at 85°C for 20 minutes to form an elastic functional layer with a thickness of 2μm on one side. The above steps are then repeated on the other surface of the negative electrode sheet, resulting in a negative electrode sheet with both a negative electrode active material layer and an elastic functional layer on both sides. The negative electrode sheet is then physically replenished with lithium. A metal lithium foil is rolled onto the surface of the elastic functional layer (the thickness of the metal lithium foil is adjustable and determined by the amount of lithium replenished) and allowed to stand.

[0130] (3) Production of positive electrode

[0131] 97g of lithium cobalt oxide, 0.5g of carbon nanotubes, and 2.5g of polyvinylidene fluoride (PVDF) were mechanically mixed, and then N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 65wt%, and stirred evenly to obtain a uniform positive electrode slurry. The positive electrode slurry was coated on one surface of an aluminum foil current collector with a thickness of 12μm and dried at 90°C. After the above steps were completed, the single-sided coating of the positive electrode sheet was completed. After that, the above steps were repeated on the other surface of the positive electrode sheet, and after roller pressing, a positive electrode sheet with a double-sided coating of positive electrode active material was obtained, wherein the compaction density of the positive electrode sheet was 4.0g / cm 3 , the active material loading matches the negative electrode active material loading, N / P = 1.1.

[0132] (4) Production of lithium-ion batteries

[0133] The prepared positive electrode sheet, separator (Celgard 2400), and negative electrode sheet were stacked in order to obtain a bare cell. The bare cell was placed in an aluminum-plastic film packaging bag, dried, and then injected with an electrolyte solution (a mixed solution of 1 mol / L LiPF6 in ethylene carbonate (EC) and diethyl carbonate (EMC) (v / v = 1:1, with an FEC addition of 10 wt%). After vacuum packaging, static standing, formation, and degassing, a lithium-ion battery was obtained.

[0134] The negative electrode sheet prepared in this embodiment includes a negative electrode current collector, a negative electrode active material layer arranged on the negative electrode current collector; and an elastic functional layer, wherein the elastic functional layer covers the surface of the negative electrode active material layer; as shown in Figure 6, it is an SEM image of the negative electrode sheet prepared in this embodiment.

[0135] Example 2

[0136] The preparation was carried out according to the preparation method of Example 1, except that:

[0137] During the preparation of the elastic functional layer slurry, the mass ratio of polyfluoroolefin polymer: modified hydrogenated nitrile rubber: conductive material is 3:2:4, and the rest is the same as in Example 1.

[0138] Example 3

[0139] The preparation was carried out according to the preparation method of Example 1, except that:

[0140] During the preparation of the elastic functional layer slurry, the mass ratio of polyfluoroolefin polymer: modified hydrogenated nitrile rubber: conductive material is 2:3:4. The olefin monomer of the polyfluoroolefin polymer is different, and the rest is the same as in Example 1.

[0141] Example 4

[0142] The preparation was carried out according to the preparation method of Example 1, except that:

[0143] The thickness of the elastic functional layer is 3 μm, and the rest is the same as in Example 1.

[0144] Example 5

[0145] The preparation was carried out according to the preparation method of Example 1, except that:

[0146] The thickness of the elastic functional layer is 1 μm. The amount of lithium supplementation in Example 5 is different, and the rest is the same as in Example 1.

[0147] Example 6

[0148] The preparation was carried out according to the preparation method of Example 1, except that:

[0149] The negative electrode active material is a black phosphorus-graphite composite (abbreviated as BP) with a mass ratio of 7:3. The amount of lithium supplement in Example 6 is different, and the rest is the same as that in Example 1.

[0150] Example 7

[0151] The preparation was carried out according to the preparation method of Example 6, except that:

[0152] During the preparation of the elastic functional layer slurry, the mass ratio of polyfluoroolefin polymer: modified hydrogenated nitrile rubber: conductive material is 3:2:4. The olefin monomer of the polyfluoroolefin polymer is different, and the rest is the same as Example 6.

[0153] Example 8

[0154] The preparation was carried out according to the preparation method of Example 6, except that:

[0155] The thickness of the elastic functional layer is 3 μm, and the rest is the same as in Example 6.

[0156] Example 9

[0157] The preparation was carried out according to the preparation method of Example 6, except that:

[0158] During the preparation of the elastic functional layer slurry, the mass ratio of polyfluoroolefin polymer: modified hydrogenated nitrile rubber: conductive material is 3:4:4, and the rest is the same as in Example 6.

[0159] Comparative Example 1

[0160] The difference from Example 1 is that:

[0161] In step (2), the elastic functional layer is not covered on the surface of the negative electrode active material layer during the production process of the negative electrode plate.

[0162] Comparative Example 2

[0163] The difference from Example 5 is that:

[0164] In step (2), the elastic functional layer is not covered on the surface of the negative electrode active material layer during the production process of the negative electrode plate.

[0165] Comparative Example 3

[0166] The difference from Example 6 is that:

[0167] In step (2), the elastic functional layer is not covered on the surface of the negative electrode active material layer during the production process of the negative electrode plate.

[0168] The specific parameter differences between Examples 1 to 9 and Comparative Examples 1 to 3 are shown in Table 1.

[0169] Table 1. Parameters of various embodiments and comparative examples

[0170] Performance testing:

[0171] (1) Testing the expansion rate of the negative electrode sheet: The lithium-ion batteries of Examples 1 to 9 and Comparative Examples 1 to 3 were subjected to 10 charge and discharge tests, and then charged to different battery states of charge (SOC) (50%, 100%). The batteries were then removed and the electrodes were disassembled. The surface of the negative electrode sheet was cleaned with dimethyl carbonate solvent and then dried. The thickness of different areas of the negative electrode sheet was measured using a micrometer, and the average value was taken. The difference between this average value and the initial thickness of the negative electrode sheet was divided by the initial thickness of the negative electrode sheet (the thickness of the remaining part after excluding the thickness of the current collector). The resulting value is the expansion rate of the negative electrode sheet.

[0172] (2) The first coulombic efficiency test of lithium-ion batteries:

[0173] The initial charge and discharge capacities of the soft-pack lithium-ion batteries of Examples 1 to 9 and Comparative Examples 1 to 3 were measured using a blue battery tester CT3001A, and the initial coulombic efficiency was calculated, where initial coulombic efficiency = initial discharge capacity / initial charge capacity×100%.

[0174] (3) Test of lithium-ion battery cycle capacity retention rate:

[0175] The capacity retention rates of the soft-pack lithium-ion batteries of Examples 1 to 9 and Comparative Examples 1 to 3 after 200 cycles at a charge and discharge rate of 0.5C / 0.7C, wherein 0.5C refers to a battery charge C rate (charge and discharge rate) of 0.5C, and 0.7C refers to a battery discharge C rate (charge and discharge rate) of 0.7C.

[0176] (4) Test of electrode peeling force:

[0177] The negative electrode sheets of Examples 1 to 9 and Comparative Examples 1 to 3 were cut into 2 cm × 10 cm strip test specimens. The electrode sheets were adhered to the side to be tested with 3M double-sided tape and compacted with a roller to ensure complete adhesion to the electrode sheets. The other side of the double-sided tape was then adhered to the surface of a stainless steel plate. One end of the specimen was bent in the opposite direction at a bending angle of 180 degrees. The specimen and the stainless steel plate were clamped and stretched using a universal material testing machine. The force required for stretching was recorded in real time. The average of all the forces was the peel force of the negative electrode sheet.

[0178] The performance test results of Examples 1 to 9 and Comparative Examples 1 to 3 are shown in Table 2.

[0179] Table 2. Performance test results of Examples 1 to 9 and Comparative Examples 1 to 3

[0180] According to the battery performance test results of Examples 1 to 9 and Comparative Examples 1 to 3 in Table 2, it can be seen that the battery pole piece expansion rate in Examples 1 to 9 is lower, and the first coulomb efficiency and capacity retention rate are higher, indicating that the elastic functional layer in the negative pole piece of the present application can inhibit the volume expansion of the pole piece and improve the cycle performance and safety performance of the lithium-ion battery. The reason is that, first, the elastic functional layer can make the negative pole piece and the diaphragm have an excellent bonding effect, which can improve the pole piece stress distribution, alleviate the problems of interface expansion and cell deformation, thereby further improving the cycle life and safety performance of the battery during actual use; second, the elastic functional layer has excellent elasticity and buffering properties (deformation force < pole piece adhesion and interface shaping force), which can reduce the extrusion and expansion damage of particles to the negative pole piece, alleviate the volume expansion of the negative pole piece during the cycle, and also alleviate the shedding of some particles and the destruction of the electron path due to particle expansion and crushing, and inhibit the cycle caused by the loss of active substances. The capacity attenuation phenomenon can improve the flatness of the surface of the negative electrode, thereby improving the cycle performance and safety performance of the battery; finally, the conductive material in the elastic functional layer makes the elastic functional layer have equipotentiality. When electrons contact the elastic functional layer, the electric field on the surface of the electrode can be dispersed, promoting electron transmission, reducing the impedance and polarization of the negative electrode; and acting as a lithium replenishment buffer layer, reducing the side reactions of the lithium replenishment interface, and improving the lithium replenishment efficiency; in the later stage of the cycle, the elastic functional layer can also ensure the complete electronic path of the electrode, so that the electric field on the surface of the electrode is dispersed, promoting the uniform deposition of lithium ions, thereby improving the cycle performance and safety performance of the battery.

[0181] Figure 7a is a schematic diagram of the surface flatness of the negative electrode plate provided in Example 1 of the present application after cycling; Figure 7b is an SEM image of the negative electrode plate provided in Example 1 of the present application after cycling. As shown in Figures 7a and 7b, it can be seen from the figures that the surface of the negative electrode plate in Example 1 after cycling is relatively flat, and the plate flatness is high; Figure 8a is a schematic diagram of the surface flatness of the negative electrode plate provided in Comparative Example 1 of the present application after cycling; Figure 8b is an SEM image of the negative electrode plate provided in Comparative Example 1 of the present application after cycling; as shown in Figures 8a and 8b, it can be seen from the figures that the surface of the negative electrode plate in Comparative Example 1 after cycling is uneven, and the plate flatness is low; it can be seen that adding an elastic functional layer to the negative electrode plate can reduce the extrusion and expansion damage of the negative electrode active material particles to the negative electrode plate, improve the flatness of the surface of the negative electrode plate, and keep the surface of the plate flat after cycling, thereby alleviating the volume expansion of the negative electrode plate during the cycle, and further improving the cycle performance of the lithium-ion battery.

[0182] Figure 9 is a schematic diagram of the cycle capacity retention rate of the lithium-ion batteries provided in Example 1 and Comparative Example 1 of the present application. As shown in Figure 9, and with reference to the battery performance test results of Example 1 and Comparative Example 1, it can be seen that since the lithium-ion soft-pack battery is hot-pressed and formed, the negative electrode sheet and the diaphragm have excellent bonding effect, and the cycle capacity retention rate of the battery in Example 1 is significantly higher than that in Comparative Example 1.

[0183] Further reference to the battery performance test results of Example 5 and Comparative Example 2 shows that for silicon-based anode systems, when the elastic functional layer is included in the negative electrode plate, the plate peeling force remains stable, the initial plate expansion rate of the negative electrode plate is reduced by approximately 10%, the cycle expansion rate of the negative electrode plate is reduced by approximately 15%, the first coulombic efficiency is increased by approximately 5% to 6%, and the capacity retention rate is increased by approximately 16% to 17%. This indicates that the elastic functional layer in the negative electrode plate can effectively mitigate the volume expansion of the negative electrode plate, thereby improving the cycling performance and safety of lithium-ion batteries.

[0184] According to the performance test results of Example 1 and Example 4, for the silicon-based negative electrode system, increasing the thickness of the elastic functional layer within a certain range is beneficial to improving the lithium replenishment efficiency of the negative electrode plate, while reducing the interfacial side reactions and thus reducing the cycle expansion rate of the plate, thereby improving the cycle performance of the battery.

[0185] According to the performance test results of Examples 1 and 5, there is a design space for the amount of lithium replenishment for the elastic functional layer. Reducing the amount of lithium replenishment is beneficial to reducing the initial and cyclic expansion rate of the negative electrode sheet, but the improvement in the cyclic capacity retention rate of the lithium-ion battery is limited.

[0186] The battery performance test results of Example 6 and Comparative Example 3 show that for phosphorus-based negative electrode systems, when the negative electrode sheet includes an elastic functional layer, the initial expansion rate of the negative electrode sheet is reduced by approximately 7%, the cycle expansion rate of the negative electrode sheet is reduced by approximately 10%, the initial coulombic efficiency is increased by approximately 5%, and the capacity retention rate after 200 cycles is improved by 17%. This indicates that the elastic functional layer can effectively mitigate the volume expansion of the negative electrode sheet, thereby improving the cycling performance and safety of lithium-ion batteries.

[0187] According to the battery performance test results of Example 6 and Example 8, for the phosphorus-based negative electrode system, increasing the thickness of the elastic functional layer is beneficial to reducing the cycle expansion rate of the electrode and improving the cycle capacity rate of the battery.

[0188] In summary, the elastic functional layer in the negative electrode can effectively alleviate the stress layout of the electrode and reduce the initial expansion rate of the electrode. At the same time, it can also reduce the side reaction of lithium replenishment and improve the efficiency of lithium replenishment. It can also reduce the interface side reaction during the battery cycle, balance polarization, reduce the cycle expansion rate of the electrode, and greatly improve the battery's cycle capacity retention rate, thereby improving the battery's cycle performance and safety performance.

Claims

1. A slurry for a negative electrode sheet, characterized in that: The slurry comprises a conductive material, a polyfluoroolefin polymer, a modified hydrogenated nitrile rubber and a solvent.

2. The slurry according to claim 1, characterized in that The polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of an olefin monomer containing a polar functional group.

3. The slurry according to claim 2, characterized in that The fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, ethylene fluoride, trifluoroethylene, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene; and / or, The general structural formula of the olefin monomer containing polar functional groups is R1CH=CR1R2, wherein R1 is selected from H or CH3, and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3 or CN.

4. The slurry according to any one of claims 1 to 3, characterized in that The slurry meets at least one of the following characteristics: (1) Based on the total mass of the components in the slurry excluding the solvent, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material is (2-4): (2-4): (2-4); (2) The solid content of the slurry is 5wt% to 10wt%; (3) The modified hydrogenated nitrile rubber contains acrylonitrile, and the mass content of acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%; (4) The viscosity of the slurry is 100 cP to 2000 cP; (5) The conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes and graphene; (6) The solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, n-hexane or N-methylpyrrolidone.

5. A negative electrode plate, characterized in that: The negative electrode plate comprises: A negative electrode current collector, a negative electrode active material layer disposed on the negative electrode current collector; and An elastic functional layer is covered on the surface of the negative electrode active material layer, and the elastic functional layer comprises a conductive material, a polyfluoroolefin polymer and a modified hydrogenated nitrile rubber.

6. The negative electrode sheet according to claim 5, characterized in that: The polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of an olefin monomer containing a polar functional group.

7. The negative electrode sheet according to claim 6, characterized in that: It meets at least one of the following characteristics: (1) The fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, ethylene fluoride, trifluoroethylene, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene; (2) The general structural formula of the olefin monomer containing a polar functional group is R1CH=CR1R2, wherein R1 is selected from H or CH3, and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3 or CN.

8. The negative electrode sheet according to claim 5, characterized in that: The modified hydrogenated nitrile rubber is obtained by polymerizing ethylene and acrylonitrile.

9. The negative electrode sheet according to claim 8, characterized in that: The molar proportion of the acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%.

10. The negative electrode sheet according to claim 5, characterized in that: The negative electrode plate meets at least one of the following characteristics: (1) The thickness of the negative electrode current collector is 5 μm to 15 μm; (2) The thickness of the negative electrode active material layer is 10 μm to 70 μm; (3) The thickness of the elastic functional layer is 1 μm to 5 μm; (4) The mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material is (2-4): (2-4): (2-4).

11. The negative electrode sheet according to claim 5, characterized in that: The negative electrode plate includes a negative electrode active material, which satisfies at least one of the following characteristics: (1) The negative electrode active material comprises a silicon-based material, wherein the silicon-based material is selected from at least one of elemental silicon, silicon-oxygen compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys; (2) The negative electrode active material includes a phosphorus-based material, and the phosphorus-based material includes at least one of elemental phosphorus and a phosphorus-carbon composite; (3) The conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes and graphene.

12. An electrochemical device, characterized in that The electrochemical device comprises the negative electrode sheet according to any one of claims 5 to 11.

13. An electronic device, characterized in that: The electronic device comprises the electrochemical device according to claim 12.

Citation Information

Patent Citations

  • Binder, electrode plate, battery and electric device

    CN115842095A

  • Nonaqueous electrolyte secondary battery

    JP1997063590A

  • Electrode binder composition, electrode slurry, electrode, and electrical storage device

    KR1020130099872A

  • Negative electrode plate and lithium-ion battery

    US20230135612A1

  • Slurry composition for secondary battery electrode and secondary battery electrode using same

    US20230139306A1

Cited By

  • Negative electrode active material powder supplemented with metal M as well as preparation method, preparation device and application of negative electrode active material powder

    CN120485802A