Sodium nickel iron manganese oxide composite material coated with hydrophobic coating and preparation method therefor
By combining oxalate coprecipitation and hydrophobic coating, the problems of uneven mixing and water absorption in sodium nickel iron manganese oxide cathode materials were solved, thereby improving the stability of the materials and battery performance.
Patent Information
- Application Number
- PCT/CN2024/087981
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-04-16
- Publication Date
- 2024-11-28
AI Technical Summary
In existing technologies, sodium-nickel-iron-manganese oxide cathode materials suffer from uneven mixing and high water absorption at high nickel content, leading to difficulties in battery processing and a decline in electrochemical performance.
Precursor materials were prepared by oxalate coprecipitation and coated with a hydrophobic coating. The hydrophobic materials, such as polyurethane, were then combined with sodium nickel iron manganese oxide to form a net-like structure, which reduced water absorption.
This improved the stability and electrochemical performance of sodium-nickel-iron-manganese oxide cathode materials, enhanced the battery's processing performance and cycle life, and achieved high energy density and good rate performance.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Sodium nickel iron manganese oxide composite material coated with hydrophobic coating and preparation method thereof Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium-nickel-iron-manganese oxide composite material coated with a hydrophobic coating and a preparation method thereof. Background Art
[0002] Due to the low cost and widespread availability of sodium resources, rechargeable sodium-ion batteries (SIBs) have attracted attention as an alternative to lithium-ion batteries (LIBs) in electrical energy storage applications. Research and development of SIBs focuses on developing high-capacity, high-potential cathode materials. Over the past decade, various cathode materials have been proposed, including layered oxides, polyanionic compounds, and Prussian blue analogs.
[0003] Layered sodium oxide materials are mainly used in small batteries, such as mobile phones and other digital products. They are usually characterized by high energy density. a Fe b Mn c O2) in particular can provide extremely high energy density.
[0004] For example, the Chinese invention patent application with publication number CN115692717A discloses a sodium ion battery mesh copper doped sodium nickel manganate positive electrode material, which uses mesh copper as a dopant to form a conductive network in the sodium nickel manganate positive electrode material. Its molecular formula is Na a Ni x Fe y Mn z Cu 1-x-y-z O2, where a is 0.6~07, x is 0.1~0.4, y is 0.2~0.6, z is 0.2~0.6, and x+y+z<1.
[0005] For example, the Chinese invention patent application with publication number CN112886084A discloses a method for repairing a sodium ion battery layered oxide positive electrode material, wherein the sodium ion battery layered oxide positive electrode material used can be a sodium nickel iron manganese ternary material, and the sodium nickel iron manganese ternary material is preferably NaNi p Fe q Mn r O2, 0.2≤p≤0.33, 0.11≤q≤0.5, 0.25≤r≤0.66, p+q+r=1, for example, NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, Na 0.6 Ni 0.22 Fe 0.11 Mn 0.66O2 or NaNi 0.25 Fe 0.5 Mn 0.25 O2.
[0006] Although the molar nickel content of sodium nickel iron manganese oxide cathode materials is high (NaNi a Fe b Mn c When a>0.6 in O2, the energy density can be further improved. However, the current methods for producing this material are limited. The technical problems are mainly manifested in:
[0007] (1) The solvent thermal reaction of nickel salt, iron salt and manganese salt mixed in deionized water is difficult to accurately mix due to their poor compatibility, which affects the synthesis quality of sodium nickel iron manganese oxide positive electrode materials.
[0008] (2) At high nickel molar ratios, significant water absorption occurs within the battery during and after battery production, which can lead to difficulties in battery processing and a decrease in the battery's electrochemical performance.
[0009] (3) The primary particles of the material synthesized by the oxalate co-precipitation method are small and evenly distributed, with good layered characteristics. However, due to the large specific surface area, significant water absorption will occur during and after the battery production process, which will also lead to difficulties in battery processing, a decrease in the electrochemical performance of the battery, and a shortened life cycle.
[0010] In view of the above background, it is necessary to design a method to reduce the water absorption and improve the overall stability of sodium layered oxide cathode materials with high nickel ion concentration. Summary of the Invention
[0011] The present invention addresses the above-mentioned technical problems existing in the prior art and provides a method for reducing water absorption and improving the overall stability of a sodium layered oxide positive electrode material having a high concentration of nickel ions.
[0012] A method for preparing a sodium nickel iron manganese oxide composite material coated with a hydrophobic coating, wherein the chemical formula of the sodium nickel iron manganese oxide composite material is Na 1+x Ni a Fe b Mn c M d (O2) 1+e , where M is a doping element, 0≤x≤0.1, 0.6≤a≤1, 0.01≤b≤0.40, 0.01≤c≤0.40, 0≤d≤0.05, 0≤e≤0.1,
[0013] The preparation method comprises the following steps:
[0014] S1: nickel salt, iron salt and manganese salt are weighed according to the stoichiometric ratio of each element and dissolved in deionized water; then an oxalate source is added to perform a solvothermal reaction to obtain an oxalate precipitate;
[0015] S2: mixing the oxalate precipitate obtained in step S1 with a sodium source and a dopant and then calcining the mixture to obtain a precursor sodium nickel iron manganese oxide material;
[0016] S3: The precursor sodium nickel iron manganese oxide material obtained in step S2 is mixed with the hydrophobic material, and then heated and dried to obtain the sodium nickel iron manganese oxide composite material coated with the hydrophobic coating.
[0017] Ni, Fe, and Mn are transition metal elements, with M being the element used to dope and replace transition metal sites in the oxide material structure. These ions at the transition metal sites form octahedral and tetrahedral structures with adjacent oxygen. A hydrophobic coating can reduce the material's hygroscopicity.
[0018] In step S1, after the oxalic acid source is added, a complexation reaction occurs and the pH of the solution becomes acidic. The pH can be adjusted to 3-4, preferably 3-3.5, by adding an alkali solution. The alkali solution used to adjust the pH is ammonia water.
[0019] Preferably, x=0, 0.6≤a≤0.8, 0.1≤b≤0.2, 0.1≤c≤0.2, 0.02≤d≤0.04, and e=0. The chemical formula of the sodium nickel iron manganese oxide composite material is NaNi a Fe b Mn c M d O2, among which, 0.6≤a≤0.8, 0.1≤b≤0.2, 0.1≤c≤0.2, 0.02≤d≤0.04.
[0020] Preferably, the nickel salt, iron salt, and manganese salt are each at least one of the following: sulfate, sulfite, chloride, nitrate, and acetate.
[0021] The oxalate source is at least one of the following: oxalic acid and ammonium oxalate.
[0022] The sodium source is at least one of the following: sodium carbonate, sulfate, sulfite, chlorate, nitrate, acetate, and citrate.
[0023] The hydrophobic material is at least one of the following: polyurethane, fluoropolyethylene, acrylic resin, epoxy resin, polyethylene, polystyrene, polydimethylsiloxane and polyester.
[0024] The doping element M in the dopant is at least one of the following: Mg 2+ 、Cu 2+ 、Al 3+ 、B3+ 、Co 3+ 、V 3+ 、Ti 4+ 、Zr 4+ 、F - The preferred dopant is at least one of the following: MgO, TiO2, aluminum fluoride, and vanadium fluoride. The amount of the dopant used is 0.1% to 0.3% of the theoretical mass of the iron manganese nickel oxalate in the solution.
[0025] Preferably, the amount of water used in step S1 is such that the mass percentage of water is 37.9% to 66.0% of the total mass of the system after the oxalate source is added.
[0026] Preferably, in step S1, the solvent thermal reaction temperature is 50-80°C and the reaction time is 6-12 hours. In step S2, the calcination temperature is 780-820°C and the time is 8-12 hours. In step S3, the heating and drying temperature is 200-220°C and the time is 2-5 hours.
[0027] Preferably, in step S1, the molar ratio of the oxalate source to the combination of nickel salt, iron salt and manganese salt is 1-1.2:1, preferably 1.1:1.
[0028] Preferably, in step S3, the mass of the added hydrophobic material is 1% to 4% of the precursor sodium nickel iron manganese oxide material obtained in step S2.
[0029] Preferably, ball milling is used for mixing in steps S2 and S3, the solvent medium used for ball milling is deionized water, and the slurry obtained after ball milling is spray dried.
[0030] The present invention further provides a sodium-nickel-iron-manganese oxide composite material coated with a hydrophobic coating prepared by the preparation method.
[0031] The present invention also provides a sodium ion battery electrode material, comprising the sodium nickel iron manganese oxide composite material coated with a hydrophobic coating.
[0032] The sodium-nickel-iron-manganese oxide composite material coated with a hydrophobic coating prepared by the present invention has high capacity and good rate capability, cycle life and material processing performance as a positive electrode material for a rechargeable sodium ion battery.
[0033] A large amount of nickel ions is introduced to provide charge compensation, and a small amount of doping elements is used to improve the stability of the crystal structure, thereby improving the reversible specific capacity and energy density of the oxide material.
[0034] The oxalate co-precipitation method usually involves mixing substances of different chemical compositions in a solution state, adding a precipitant to the mixed solution to prepare a precursor precipitate, and then drying or calcining the material to obtain the desired powder material; the material particles are fine, evenly distributed, and have good layered characteristics. Smaller material particle size means shorter Na + Migration path, making Na + The reversibility of crystal insertion and extraction enhances the material's electrochemical performance. Consequently, the resulting material exhibits improved electrochemical, cycling, and rate capabilities. The oxalate co-precipitation method allows for precise mixing of nickel, iron, and manganese salts in a solvothermal reaction in water, improving the quality of the synthesized sodium-nickel-iron-manganese oxide cathode material.
[0035] The hydrophobic coating prepared by the present invention forms a fishnet-like coating on the surface of the positive electrode material, overcoming the disadvantage of significant water absorption caused by the high molar ratio of nickel during and after the battery production process.
[0036] The disclosed synthesis process enables large-scale continuous production and maximizes economic advantages. The resulting sodium-ion full battery exhibits high average energy storage voltage, high energy density, and high power density. It can be used as a green and clean energy source for power generation, smart grid peak regulation, distributed power stations, backup power supplies, communication base stations, or energy storage for low-speed electric vehicles, with excellent safety, rate capability, and cycling performance. DETAILED DESCRIPTION
[0037] The present invention provides a sodium nickel iron manganese oxide composite material, the chemical formula of which is as follows: Na 1+x Ni a Fe b Mn c M d (O2) 1+e , wherein Ni, Fe and Mn are respective transition metal elements, and M is an element used to dope and replace transition metal positions in the oxide material structure. These ions at the transition metal sites form octahedral and tetrahedral structures with adjacent oxygen ions. Preferably, M is Mg 2+ 、Cu 2+ 、Al 3+ 、B 3+ 、Co 3+ 、V 3+ 、Ti 4+ 、Zr 4+, or a combination of two or more thereof. Preferably, x, a, b, c, d, and e are the molar percentages of the corresponding elements of each component in the chemical formula that satisfies charge conservation and stoichiometry conservation. Specifically, 0≤x≤0.1, 0.6≤a≤1, 0.01≤b≤0.40, 0.01≤c≤0.40, 0≤d≤0.05, and 0≤e≤0.1. The prepared sodium-nickel-iron-manganese oxide composite material contains a hydrophobic material coating on the surface of the sodium-nickel-iron-manganese oxide.
[0038] Sodium-nickel-iron-manganese oxide composite materials for sodium-ion batteries can be used as positive electrode active materials for sodium-ion secondary batteries. Sodium-nickel-iron-manganese oxide composite materials have the advantages of good reversible specific capacity, high energy density, and long cycle life.
[0039] In order to promote understanding of the present invention, the disclosure will be described in detail below with reference to preferred embodiments. It should be understood that the embodiments are merely illustrative and are not intended to limit the scope of the present invention. Any changes, modifications, and substitutions made by those skilled in the art without departing from the spirit of the disclosure shall fall within the scope of the disclosure defined by the appended claims.
[0040] Example 1
[0041] Sodium nickel iron manganese oxide composites (NaNi) coated with hydrophobic coating were prepared by solvothermal coprecipitation method. 0.6 Fe 0.2 Mn 0.2 Ti 0.02 O2). The method comprises the following specific steps:
[0042] (S1) 92.85 g of nickel (II) sulfate, 30.95 g of ferrous sulfate, and 31.00 g of manganese sulfate were placed in 500 mL of distilled water. 99.03 g of oxalic acid was added at 60°C, and the pH was adjusted to 3 with sodium hydroxide under rapid stirring. A solvothermal reaction was then carried out at 60°C for 10 hours. After the reaction, the precipitate was collected by filtration, washed with deionized water, and dried in air at 110°C to obtain nickel-iron-manganese oxalate.
[0043] (S2) The nickel iron manganese oxalate obtained in step S1 was added to 253.6 mL of deionized water, followed by the addition of 53.2 g of sodium carbonate and a dopant TiO2, wherein the amount of the dopant TiO2 was 0.1% of the theoretical mass of the nickel iron manganese oxalate in the solution. The mixture was then ball milled in a high-speed ball mill using 0.5 mm zirconium balls for 3 hours to obtain a slurry, which was then spray-dried in a spray dryer at an inlet temperature of 270°C and an outlet temperature of 90°C. The spray-dried material was then calcined in an oxygen atmosphere at 820°C for 8 hours and then cooled to room temperature to obtain a precursor sodium nickel iron manganese oxide (NaNi 0.6 Fe 0.2Mn 0.2 Ti 0.02 O2) materials.
[0044] (S3) The product obtained in step S2, polyurethane, and deionized water as a solvent are ball-milled in a high-speed ball mill, wherein the mass of the added polyurethane is 1% of the mass of the precursor sodium nickel iron manganese oxide obtained in step S2. The ball milling is carried out using 0.5 mm zirconium balls in a high-speed ball mill for 5 hours to obtain a slurry, which is then spray-dried in the spray dryer at an inlet temperature of 270°C and an outlet temperature of 90°C. The dried material is further dried at 200°C in a nitrogen atmosphere for 2 hours to obtain a sodium nickel iron manganese oxide composite material (NaNi) coated with a hydrophobic coating. 0.6 Fe 0.2 Mn 0.2 Ti 0.02 O2).
[0045] Example 2
[0046] Sodium nickel iron manganese oxide composites (NaNi) coated with hydrophobic coating were prepared by solvothermal coprecipitation method. 0.7 Fe 0.1 Mn 0.2 Al 0.01 O2F 0.03 ). The method comprises the following specific steps:
[0047] (S1) 108.33 g of nickel (II) sulfate, 15.47 g of ferrous sulfate, and 31.00 g of manganese sulfate were placed in 155 ml of deionized water. 99.03 g of ammonium oxalate was added at 60°C, and the pH was controlled to 3.5 with aqueous ammonia under rapid stirring. A solvothermal reaction was then carried out at 50°C for 12 hours. After the reaction, the precipitate was collected by filtration, washed with deionized water, and dried in air at 120°C to obtain nickel-iron-manganese oxalate.
[0048] (S2) adding the nickel iron manganese oxalate obtained in step S1 to 253.6 mL of deionized water, and then adding 53.2 g of sodium carbonate and dopant aluminum fluoride, wherein the amount of dopant aluminum fluoride is 0.3% of the theoretical mass of nickel iron manganese oxalate in the solution, and then ball milling with 0.5 mm zirconium balls in a high-speed ball mill for 3 hours to obtain a slurry, and then spray drying the slurry in the spray dryer at an inlet temperature of 270 ° C and an outlet temperature of 90 ° C, and then calcining the spray-dried material at 780 ° C in an oxygen atmosphere for 12 hours, and then cooling to room temperature to obtain a precursor sodium nickel iron manganese oxide (NaNi 0.7 Fe 0.1 Mn 0.2 Al 0.01 O2F 0.03 )Material.
[0049] (S3) The product obtained in step S2, polyurethane, and deionized water are ball-milled in a high-speed ball mill, wherein the mass of the added polyurethane is 3% of the mass of the precursor sodium nickel iron manganese oxide obtained in step S2. Ball milling is performed using 0.5 mm zirconium balls in a high-speed ball mill for 5 hours to obtain a slurry, which is then spray-dried. The dried material is further dried at 220°C in a nitrogen atmosphere for 5 hours to obtain a sodium nickel iron manganese oxide composite material (NaNi 0.7 Fe 0.1 Mn 0.2 Al 0.01 O2F 0.03 ).
[0050] Example 3
[0051] Sodium nickel iron manganese oxide composites (NaNi) coated with hydrophobic coating were prepared by solvothermal coprecipitation method. 0.8 Fe 0.1 Mn 0.1 Mg 0.02 O2). The method comprises the following specific steps:
[0052] (S1) 123.81 g of nickel (II) sulfate, 15.49 g of ferrous sulfate, and 15.50 g of manganese sulfate were placed in 155 ml of distilled water. 99.03 g of oxalic acid was added at 60°C in an air atmosphere. The pH was controlled to 3.5 with aqueous ammonia under rapid stirring, and then a solvothermal reaction was carried out at 80°C for 6 hours. After the reaction, the precipitate was collected by filtration, washed with deionized water, and dried in an oxygen atmosphere at 130°C to obtain nickel-iron-manganese oxalate.
[0053] (S2) The nickel iron manganese oxalate obtained in step S1 is added to 253.6 mL of deionized water, and then 53.2 g of sodium carbonate and a dopant of MgO are added, where the amount of the dopant MgO is 0.3% of the theoretical mass of the nickel iron manganese oxalate in the solution. The slurry is then ball milled in a high-speed ball mill with 0.5 mm zirconium balls for 3 hours to obtain a slurry, which is then spray-dried in a spray dryer at an inlet temperature of 270°C and an outlet temperature of 70°C. The spray-dried material is then calcined at 780°C in an oxygen atmosphere for 12 hours, and then cooled to room temperature to obtain a precursor sodium nickel iron manganese oxide (NaNi 0.8 Fe 0.1 Mn 0.1 Mg 0.02 O2) materials.
[0054] (S3) The product obtained in step S2, polyurethane, and deionized water as solvent are ball-milled in a high-speed ball mill, wherein the mass of the added polyurethane is 4% of the mass of the precursor sodium nickel iron manganese oxide obtained in step S2. The product is then spray-dried, and the dried material is further dried at 220°C in a nitrogen atmosphere for 5 hours to obtain a sodium nickel iron manganese oxide composite material (NaNi 0.8 Fe 0.1 Mn 0.1 Mg 0.02 O2).
[0055] Test Example 1
[0056] The performance of the products prepared in each example was tested.
[0057] By respectively adding 64 wt.% of NaNi coated with hydrophobic coating 0.6 Fe 0.2 Mn 0.2 Ti 0.02 O2 (Example 1), NaNi 0.7 Fe 0.1 Mn 0.2 Al 0.01 O 22 F 0.03 (Example 2) or NaNi 0.8 Fe 0.1 Mn 0.1 Mg 0.02 O2 (Example 3) was mixed with 1.4 wt.% Super-P, 2.7 wt.% PVDF5130 binder, and 32 wt.% NMP solvent. The mixture was homogenized and then coated onto an aluminum foil sheet. The sheet was dried in a vacuum oven at 80°C for 12 hours.
[0058] A 14 mm diameter disc was punched and a CR2032 coin cell was assembled using the prepared electrolyte, a sodium foil counter electrode, and a polyethylene separator. A 1.0 M NaPF6+EC-DMC-EMC (1:1:1 volume ratio) electrolyte containing 2% (volume ratio) fluorinated ethylene carbonate was injected into the cell.
[0059] The batteries corresponding to the products prepared in Example 1, Example 2, and Example 3 have discharge specific capacities of 167.3 mAh / g, 160.2 mAh / g, 158.3 mAh / g at 0.2C, 0.5C, and 1C, respectively; 172.6 mAh / g, 169.5 mAh / g, 162.4 mAh / g; 183.1 mAh / g, 175.2 mAh / g, and 171.3 mAh / g. In addition, the first efficiency measured at 1C was 89%, 87%, and 86.2%, respectively. Therefore, the sodium nickel iron manganese oxide composite material positive electrode coated with a hydrophobic coating prepared in this application has a high specific capacity, good first efficiency, and excellent rate performance.
[0060] Comparative Example 1
[0061] Compared with Example 1, the operation of step S3 is cancelled, and other technical solutions are the same as Example 1.
[0062] The sodium nickel iron manganese oxide composite material sample coated with a hydrophobic coating in Example 1 is marked as sample A1, and the sample not coated with a hydrophobic coating in Comparative Example 1 is marked as sample B1.
[0063] Samples A1 and B1 were vacuum dried at 250°C for 12 hours. After cooling to room temperature, the moisture content of both samples was measured using a coulometer. The initial moisture content of Samples A1 and B1 was 58 ppm and 67 ppm, respectively. Samples A1 and B1 were then left at room temperature for 48 hours, and their moisture content was measured again. The final moisture content of Samples A1 and B1 was 141 ppm and 1159 ppm, respectively, indicating that the hydrophobic coating inside the sodium nickel iron manganese oxide composite prevented water absorption.
[0064] Comparative Example 2
[0065] Compared with Example 2, the operation of step S3 is cancelled, and other technical solutions are the same as Example 2.
[0066] The sodium nickel iron manganese oxide composite material sample coated with a hydrophobic coating in Example 2 is marked as sample A2, and the sample not coated with a hydrophobic coating in Comparative Example 2 is marked as sample B2.
[0067] Samples A2 and B2 were vacuum dried at 250°C for 12 hours. After cooling to room temperature, the moisture content of the two samples was measured using a coulometer. The initial moisture content of sample A and sample B was 55ppm and 72ppm, respectively. Samples A2 and B2 were then left at room temperature for 48 hours and their moisture content was measured again. The final moisture content of sample A2 and sample B2 was 153ppm and 1262ppm, respectively, indicating that the hydrophobic coating inside the sodium nickel iron manganese oxide composite material prevented water absorption.
[0068] Comparative Example 3
[0069] Compared with Example 3, the operation of step S3 is cancelled, and other technical solutions are the same as Example 3.
[0070] The sodium nickel iron manganese oxide composite material sample coated with a hydrophobic coating in Example 3 is labeled as sample A3, and the sample not coated with a hydrophobic coating in Comparative Example 3 is labeled as sample B3.
[0071] Samples A3 and B3 were vacuum dried at 250°C for 12 hours. After cooling to room temperature, the moisture content of the two samples was measured using a coulometer. The initial moisture content of Samples A3 and B3 was 49 ppm and 83 ppm, respectively. Samples A3 and B3 were then left at room temperature for 48 hours, and their moisture content was measured again. The final moisture content of Samples A3 and B3 was 56 ppm and 1183 ppm, respectively, indicating that the hydrophobic coating inside the sodium nickel iron manganese oxide composite prevented water absorption.
Claims
1. A method for preparing a sodium-nickel-iron-manganese oxide composite material coated with a hydrophobic coating, characterized in that: The chemical formula of the sodium nickel iron manganese oxide composite material is Na 1+x Ni a Fe b Mn c M d (O2) 1+e , where M is a doping element, 0≤x≤0.1, 0.6≤a≤1, 0.01≤b≤0.40, 0.01≤c≤0.40, 0≤d≤0.05, 0≤e≤0.1, The preparation method comprises the following steps: S1: nickel salt, iron salt and manganese salt are weighed according to the stoichiometric ratio of each element and dissolved in deionized water; then an oxalate source is added to perform a solvothermal reaction to obtain an oxalate precipitate; S2: mixing the oxalate precipitate obtained in step S1 with a sodium source and a dopant and calcining the mixture to obtain a precursor sodium nickel iron manganese oxide material; S3: The precursor sodium nickel iron manganese oxide material obtained in step S2 is mixed with the hydrophobic material, and then heated and dried to obtain the sodium nickel iron manganese oxide composite material coated with the hydrophobic coating.
2. The preparation method according to claim 1, characterized in that: x=0, 0.6≤a≤0.8, 0.1≤b≤0.2, 0.1≤c≤0.2, 0.02≤d≤0.04, e=0.
3. The preparation method according to claim 1, characterized in that: The nickel salt, iron salt, and manganese salt are each at least one of the following: sulfate, sulfite, chloride, nitrate, acetate, citrate, and carbonate; The oxalate source is at least one of the following: oxalic acid and ammonium oxalate; The sodium source is at least one of the following: sodium carbonate, sulfate, sulfite, chlorate, nitrate, acetate, citrate and carbonate; The hydrophobic material is at least one of the following: polyurethane, fluoropolyethylene, acrylic resin, epoxy resin, polyethylene, polystyrene, polydimethylsiloxane and polyester; The doping element M in the dopant is at least one of the following: Mg 2+ , Cu 2+ 、Al 3+ , B 3+ 、Co 3+ 、V 3+ 、Ti 4+ 、Zr 4+ 、F - .
4. The preparation method according to claim 1, characterized in that: The amount of water used in step S1 is such that the mass percentage of water used is 37.9% to 66.0% of the total mass of the system after the oxalate source is added.
5. The preparation method according to claim 1, characterized in that: In step S1, the temperature of the solvent thermal reaction is 50-80°C, and the reaction time is 6-12h; In step S2, the calcination temperature is 780-820°C and the time is 8-12 hours; In step S3, the temperature of heating and drying is 200-220°C and the time is 2-5 hours.
6. The preparation method according to claim 1, characterized in that: In step S1, the molar ratio of the oxalate source to the combination of the nickel salt, the iron salt and the manganese salt is 1-1.2:
1.
7. The preparation method according to claim 1, characterized in that: In step S3, the mass of the hydrophobic material added is 1% to 4% of the precursor sodium nickel iron manganese oxide material obtained in step S2.
8. The preparation method according to claim 1, characterized in that: The mixing in steps S2 and S3 is performed by ball milling, the solvent medium used for the ball milling is deionized water, and the slurry obtained after the ball milling is spray dried.
9. A sodium-nickel-iron-manganese oxide composite material coated with a hydrophobic coating prepared by the preparation method according to any one of claims 1 to 8.
10. A sodium ion battery electrode material, characterized in that: A sodium-nickel-iron-manganese oxide composite material comprising the hydrophobic coating as claimed in claim 9.
Citation Information
Patent Citations
Method for preparing lithium-enriched lithium manganese oxide solid solution cathode material
CN102544475A
A lithium nickel cobalt manganate composite material and a preparation method thereof
CN109088066A
High-nickel layered oxide material for sodium-ion battery as well as preparation method and application thereof
CN113258060A
Sodium-nickel-iron-manganese oxide composite material coated with hydrophobic coating and preparation method of sodium-nickel-iron-manganese oxide composite material
CN116487518A
Sodium, manganese, titanium and nickel composite oxide, method for manufacturing the same, and sodium secondary battery using the same as member
JP2012206925A