Positive electrode material precursor for sodium ion battery, preparation method therefor, positive electrode material, and sodium ion battery
By using the secondary particle structure and co-precipitation method of disorderly core arrangement and staggered shell skeleton arrangement in the positive electrode material of sodium ion battery, the problem of poor element distribution uniformity is solved, and the capacity and cycle stability of sodium ion battery are improved , and through the use of sodium acetate and ammonium sulfate, the sintering process of the material is optimized, achieving high discharge capacity and air stability.
Patent Information
- Application Number
- PCT/CN2024/094485
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-28
AI Technical Summary
The distribution uniformity of the precursor elements of the existing sodium ion battery cathode material is poor, resulting in low material vibration, which restricts the improvement of the overall capacity and cycle stability of the sodium ion battery.
A secondary particle structure consisting of a core and a shell is adopted, where the primary particles of the core are arranged in an orderly manner, and the primary particles of the shell are arranged interlaced along the circumference of the secondary particles, and are filled with slender primary particles. The co-precipitation method is used to lie at high Preparation under pH conditions, sodium acetate and ammonium sulfate were used as complexing agents and additives to optimize precipitation rate and morphological uniformity.
The battery capacity and circulation performance of the positive electrode material are improved, the particle strength and volume energy density of the material are enhanced, the sintering temperature is reduced, and the copper-containing positive electrode material has good air stability and extends the circulation life.
Smart Images

Figure CN2024094485_28112024_PF_FP_ABST
Abstract
Description
A positive electrode material precursor for sodium ion battery and preparation method thereof, positive electrode material, and sodium ion battery
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This disclosure claims priority to Chinese patent application number 202310594291.0, filed with the Patent Office of China on May 23, 2023, entitled “A positive electrode material precursor for sodium ion battery and its preparation method, positive electrode material, sodium ion battery,” the entire contents of which are incorporated by reference into this disclosure. Technical Field
[0003] The present disclosure relates to the field of new energy technology, and in particular to a cathode material precursor for a sodium ion battery and a preparation method thereof, a cathode material, and a sodium ion battery. Background Art
[0004] Sodium-ion batteries, with their low cost, low-temperature resistance, safety, and convenience, are expected to see rapid development in a variety of fields, including electric vehicles, electric boats, home and industrial energy storage, 5G communication base stations, data centers, large-scale renewable energy access, and smart grids. Sodium is abundant in natural resources, and sodium-ion batteries can reduce or eliminate the use of expensive metals such as lithium, cobalt, and nickel, thereby lowering energy storage costs. Therefore, sodium-ion batteries are highly competitive in the energy storage field and are expected to become an excellent alternative to lithium-ion batteries.
[0005] The cycling stability, capacity, and other performance characteristics of sodium-ion batteries primarily depend on the properties of the cathode material, which inherits the morphology and structural characteristics of its precursor. Currently, sodium-ion batteries made from cathode materials prepared by mixed sintering of cathode material precursors suffer from low capacity and poor cycling performance. Cathode material precursors prepared by simple co-precipitation methods also suffer from poor elemental distribution uniformity and low material tap density, limiting improvements in the overall capacity and cycling stability of sodium-ion batteries.
[0006] Summary of the Invention
[0007] The present disclosure provides a cathode material precursor for a sodium ion battery, a preparation method thereof, a cathode material, and a sodium ion battery, aiming to solve the problems of poor element distribution uniformity and low material tap compaction in existing precursor materials, which restrict the improvement of the overall capacity and cycle stability of sodium ion batteries.
[0008] A first aspect of the present disclosure provides a cathode material precursor for a sodium ion battery, comprising secondary particles formed by aggregation of a plurality of primary particles, wherein the secondary particles comprise a core and a shell covering the core;
[0009] The primary particles of the inner core are arranged in disorder, and the primary particles of the outer shell include skeleton primary particles staggered along the circumference of the secondary particles and slender primary particles filled between the skeleton primary particles.
[0010] The uniform distribution of elements in the precursor of the positive electrode material for the sodium-ion battery is beneficial to improving the battery capacity and cycling performance of the positive electrode material. The primary particles in the core are arranged disorderly, which is beneficial to the diffusion of Na elements during the sintering process of the positive electrode material; the primary particles of the thick shell skeleton are arranged in a staggered manner along the circumference of the secondary particles, forming the outer skeleton structure of the secondary particles. The primary particles of the skeleton improve the particle strength of the secondary particles, making the positive electrode material not prone to structural collapse during the processes of Na doping and batch mixing and sintering, and capable of maintaining the structural stability; there are slender primary particles filled between the primary particles of the skeleton, which can improve the tap density of the precursor and the volumetric energy density of the material, enabling the battery to have a high discharge capacity and high charge-discharge efficiency; moreover, the precursor as a whole has many pores and uniform element distribution, which is beneficial to the infiltration of Na elements and other doping elements during the sintering process, reducing the sintering temperature; the positive electrode material containing copper prepared by sintering the precursor material of the positive electrode material for the sodium-ion battery has good air stability, which is beneficial to improving the cycle life.
[0011] Preferably, its chemical formula is (Ni ,
[0015] ,
[0014] , Cu y M 1-x-y )(OH)2, where 0 < x < 1, 0 < y ≤ 1, and M is one or more of the elements Mn, Fe, Ti, Zn, Mg, Ca, Al, Ag, Co, Cr, La, Ce.
[0012] Preferably, the precursor of the positive electrode material for the sodium-ion battery satisfies at least one of the following conditions (1) to (3):
[0013] (1) The thickness of the primary particles of the skeleton in the shell is 30 - 600 nm, for example, it can be 30 - 60 nm, or 50 - 100 nm, or 150 - 200 nm, or 70 - 120 nm, or 100 - 150 nm, or 20 - 300 nm, or 200 - 300 nm, or 200 - 400 nm, or 200 - 300 nm, or 200 - 600 nm; the length of the primary particles of the skeleton is 1.0 - 4.0 μm, for example, it can be 1.0 - 2.0 μm, or 1.1 - 1.9 μm, or 2.0 - 4.0 μm;
[0014] (2) The thickness of the slender primary particles in the shell is 5 - 80 nm, for example, it can be 5 - 20 nm, or 5 - 50 nm, or 5 - 80 nm, or 10 - 30 nm, or 10 - 50 nm, or 50 - 80 nm; the length of the slender primary particles is 0.(3) The thickness of the primary particles of the inner core is 10 to 50 nm, for example, 10 to 20 nm, or 15 to 30 nm, or 20 to 30 nm, or 15 to 25 nm, or 30 to 50 nm; the length of the primary particles of the inner core is 0.2 to 1.0 μm, for example, 0.2 to 0.4 μm, or 0.3 to 0.5 μm, or 0.2 to 0.6 μm, or 0.7 to 1.0 μm, or 0.5 to 0.8 μm.
[0016] It should be noted that the thickness or length of the primary particles in the core and shell in the present disclosure is obtained by taking a plurality of primary particles in the SEM image and calculating the average thickness or length of the plurality of primary particles.
[0017] Preferably, the area ratio of the skeleton primary particles in the shell to the secondary particles is greater than or equal to 10%, for example, it can be 10% to 20%, or 20% to 30%, or greater than 40%, or greater than 50%;
[0018] Preferably, the area ratio of the skeleton primary particles to the secondary particles in the shell is greater than 40%.
[0019] Preferably, the (D90-D10) / D50 ratio of the cathode material precursor for a sodium ion battery is 0.4-1.0, for example, 0.4-0.6, or 0.6-0.9, or 0.8-0.9, or 0.85-1.0. (D90-D10) / D50 is the span value. A small span value indicates a uniform secondary particle size, which allows for denser packing when used as a cathode material, thereby increasing the discharge capacity of the battery. Preferably, the (D90-D10) / D50 ratio of the cathode material precursor for a sodium ion battery is 0.6-0.9.
[0020] Preferably, the cathode material precursor satisfies at least one of the following conditions (4) to (5):
[0021] (4) The radius of the inner core is 1.0 to 2.0 μm, for example, 1.0 to 1.5 μm, or 1.5 to 1.6 μm, or 1.6 to 2.0 μm, or 1.5 to 2.0 μm; the thickness of the outer shell is 1.0 to 3.0 μm, for example, 1.0 to 1.5 μm, or 1.5 to 2.0 μm, or 2.0 to 3.0 μm, or 1.0 to 2.0 μm;
[0022] (5) The porosity of the inner core is in the range of 5-30%, for example, 5% to 10%, or 10% to 20%, or 20% to 30%, and the porosity of the outer shell is in the range of 20% to 45%, for example, 20% to 30%, or 30% to 40%, or 40% to 45%.
[0023] Preferably, the cathode material precursor for sodium ion batteries satisfies at least one of the following conditions (6) to (9):
[0024] (6) The D50 of the cathode material precursor for sodium ion batteries is 4 to 8 μm, for example, 4 to 6 μm, or 5 to 6 μm, or 5.5 to 6.5 μm, or 6 to 7 μm, or 7 to 8 μm;
[0025] (7) The TD of the cathode material precursor for sodium ion batteries is 1.0 to 1.5 g / cm 3 , for example, it can be 1.0 to 1.1 g / cm 3 , or 1.1~1.2g / cm 3 , or 1.2~1.5g / cm 3 ;
[0026] (8) The BET of the cathode material precursor for sodium ion batteries is 20 to 80 m 2 / g, for example, 20 to 40 m 2 / g, or 30-40m 2 / g, or 30-50m 2 / g, or 50-60m 2 / g, or 60-70m 2 / g, or 50-80m 2 / g;
[0027] (9) Preferably, the BET of the cathode material precursor for sodium ion batteries is 30 to 50 m 2 / g.
[0028] The present disclosure also provides a method for preparing the above-mentioned cathode material precursor for sodium ion batteries, comprising:
[0029] Adding water, a precipitant and a complexing agent into a reaction kettle and mixing them to obtain a reaction bottom liquid;
[0030] Adding a metal salt solution, a precipitant, and a complexing agent to the reaction base liquid to perform a coprecipitation reaction, and controlling the pH value of the reaction system to gradually decrease;
[0031] The coprecipitation reaction further comprises adding an additive during the reaction, and the additive comprises at least one of ammonium sulfate and dilute sulfuric acid.
[0032] During the preparation of the precursor material for the positive electrode material for sodium ion batteries, the precipitation rate of the metal is increased under high pH (11-12) conditions, so that the core primary particles become thinner and are arranged disorderly; by adding a chelating agent and an additive to reduce the surface potential energy of the shell primary particles and improve the growth consistency of the shell primary particles, while lowering the reaction pH (10-11) to achieve the effect of reducing the precipitation rate of the metal, thereby increasing the thickness of the shell primary particles, so that the shell forms a skeleton structure composed of thick sheet-like skeleton primary particles, and the skeleton primary particles are filled with slender primary particles that are tightly stacked.
[0033] Preferably, the preparation method of the positive electrode material precursor for sodium ion batteries satisfies at least one of the following conditions a to c:
[0034] a. The complexing agent includes one or more of ammonia solution, oxalic acid, sodium acetate, EDTA-2Na (disodium ethylenediaminetetraacetic acid);
[0035] b. A metal salt solution comprising Ni, Cu, and a metal salt solution of at least one element selected from Fe, Mn, Ti, Zn, Mg, Ca, Al, Ag, Co, Cr, La, and Ce;
[0036] c. The metal salt solution includes a metal salt solution containing Ni, Cu and at least one element selected from Fe, Mn and Mg.
[0037] Preferably, the complexing agent is sodium acetate. When sodium acetate is used as a complexing agent and ammonium sulfate is added, the complexing ability of the complexing agent for metal elements is less variable, resulting in smaller differences in precipitation rates, thereby optimizing morphological uniformity. Ammonium sulfate can further reduce the growth rate, resulting in thicker primary particles.
[0038] Preferably, the preparation method of the positive electrode material precursor for sodium ion batteries satisfies at least one of the following conditions d to g:
[0039] d. The concentration of the additive is 0.01 to 0.5 mol / L, for example, 0.01 to 0.05 mol / L, or 0.05 to 0.1 mol / L, or 0.1 to 0.5 mol / L, more specifically, for example, 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L or 0.5 mol / L;
[0040] e. The mass concentration of each metal ion in the metal salt solution is independently 10 to 50 g / L, for example, 10 to 30 g / L, or 20 to 40 g / L, or 30 to 50 g / L;
[0041] f. The mass concentration of the complexing agent is 60 to 100 g / L, for example, 60 to 90 g / L, or 70 to 100 g / L, or 70 to 90 g / L, more specifically, for example, 60 g / L, 65 g / L, 70 g / L, 72, 75 g / L, 77 g / L, 80 g / L, 82 g / L, 85 g / L, 88 g / L, 90 g / L, 95 g / L or 100 g / L;
[0042] g. The pH value of the reaction liquid is 11-12, and the pH value of the reaction system is reduced to 10-11.
[0043] The present disclosure also provides a sodium ion battery positive electrode material, which includes an inner layer and an outer layer. The outer layer is dense, the inner layer has a hollow structure, and the outer layer includes a plurality of flaky primary particles.
[0044] Preferably, the positive electrode material of the sodium ion battery satisfies at least one of the following conditions A to C:
[0045] A. The diameter of the inner layer of the sodium ion battery positive electrode material is 0.5-2.0 μm, for example, 0.5-1.0 μm, or 0.8-2.0 μm, or 0.6-1.2 μm, and the thickness of the outer layer of the sodium ion battery positive electrode material is 1.0-3.0 μm, for example, 1.0-2.0 μm, or 2.0-3.0 μm, or 1.0-1.5 μm;
[0046] B. The D50 of the sodium ion battery positive electrode material is 3.5 to 8 μm, for example, 3.5 to 5.0 μm, or 4.0 to 6.0 μm, or 5.0 to 8.0 μm, or 4.0 to 7.0 μm;
[0047] C. The (D90-D10) / D50 of the sodium ion battery positive electrode material is 0.4-1 μm, for example, 0.4-0.8 μm, or 0.5-1 μm, or 0.5-0.8 μm.
[0048] The present disclosure also provides a sodium ion battery, the raw materials of which include the above-mentioned sodium ion battery positive electrode material precursor or the above-mentioned sodium ion battery positive electrode material.
[0049] The primary particles in the inner core of the precursor of the positive electrode material for sodium ion batteries provided by the present invention are arranged in a disordered manner, which is conducive to the diffusion of the Na element during the sintering process of the positive electrode material; the skeleton primary particles with thicker shells are staggered along the circumference of the secondary particles to form the outer skeleton structure of the secondary particles. The skeleton primary particles improve the particle strength of the secondary particles, so that the positive electrode material is not prone to structural collapse during the process of Na doping, batch mixing and sintering, and can maintain structural stability; slender primary particles are filled between the skeleton primary particles, which can increase the tap density of the precursor and the volume energy density of the material, so that the battery has a high discharge capacity and high charge and discharge efficiency; and the precursor has more overall pores and uniform element distribution, which is conducive to the infiltration of Na and other doping elements during the sintering process to reduce the sintering temperature; the copper-containing positive electrode material prepared by sintering the positive electrode material precursor for sodium ion batteries has good air stability and is conducive to improving the cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope of the present disclosure.
[0051] FIG1 is a SEM image of a cathode material precursor for a sodium ion battery of Example 1;
[0052] FIG2 is a cross-sectional SEM image of the cathode material precursor for a sodium ion battery of Example 1;
[0053] FIG3 is a cross-sectional mapping diagram of the cathode material precursor for a sodium ion battery of Example 1;
[0054] FIG4 is a SEM image of the positive electrode material for a sodium ion battery of Example 1;
[0055] FIG5 is a cross-sectional SEM image of the positive electrode material for a sodium ion battery of Example 1;
[0056] FIG6 is a SEM image of the cathode material precursor for a sodium ion battery of Example 2;
[0057] FIG7 is a cross-sectional SEM image of a cathode material precursor for a sodium ion battery of Example 2;
[0058] FIG8 is a SEM image of the cathode material precursor for a sodium ion battery of Example 3;
[0059] FIG9 is a cross-sectional SEM image of a cathode material precursor for a sodium ion battery of Example 3;
[0060] FIG10 is a SEM image of the cathode material precursor for sodium ion batteries of Example 4;
[0061] FIG11 is an SEM image of the nickel-iron-manganese hydroxide precursor of Comparative Example 1;
[0062] FIG12 is an SEM image of the nickel-iron-manganese-copper hydroxide precursor of Comparative Example 2;
[0063] FIG13 is a cross-sectional SEM image of the nickel-iron-manganese-copper hydroxide precursor of Comparative Example 2;
[0064] FIG14 is a cross-sectional mapping diagram of the nickel-iron-manganese-copper hydroxide precursor of Comparative Example 2;
[0065] FIG15 is an SEM image of the positive electrode material for sodium ion battery of Comparative Example 2. DETAILED DESCRIPTION
[0066] As used herein:
[0067] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variations thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0068] The conjunction "consisting of" excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed, excluding materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim, rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0069] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed alone. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described herein, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0070] In these examples, parts and percentages are by mass unless otherwise indicated.
[0071] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0072] The embodiments of the present disclosure will be described in detail below with reference to specific examples. However, those skilled in the art will appreciate that the following examples are intended only to illustrate the present disclosure and should not be construed as limiting the scope of the present disclosure. Where specific conditions are not specified in the examples, conventional conditions or conditions recommended by the manufacturer were used. Reagents or instruments used where the manufacturer is not specified are conventional products that can be purchased commercially.
[0073] Example 1
[0074] Example 1 First, a D50 of 6.01 μm and a chemical formula of (Ni 0.23 Fe 0.33 Mn 0.34 Cu 0.10 The specific preparation method of the nickel-iron-manganese-copper hydroxide precursor of )(OH)2 is as follows:
[0075] ① Nickel sulfate, ferrous sulfate, manganese sulfate, and copper sulfate crystals are dissolved into metal salt solutions with a nickel ion concentration of 27.7 g / L, an iron ion concentration of 37.9 g / L, a manganese ion concentration of 37.3 g / L, and a copper ion concentration of 13.12 g / L, respectively. The concentration of the sodium hydroxide solution used is 21%, the complexing agent is sodium acetate, and its concentration is 82 g / L. The additives ammonium sulfate and dilute sulfuric acid have concentrations of 0.1 mol / L and 0.05 mol / L, respectively. Ammonium sulfate is added to the sodium acetate solution, and dilute sulfuric acid is added to the metal salt solution.
[0076] ② Add pure water, sodium acetate solution and sodium hydroxide solution to the reactor and mix to obtain a reaction base liquid. Control the pH value of the reaction base liquid to 11.40, introduce nitrogen protection, heat the reactor to 60°C, and control the stirring speed at 800 r / min.
[0077] ③ After the feeding conditions are met, metal salt solution, sodium hydroxide solution and sodium acetate solution are pumped into the reaction bottom liquid, and then the metal salt solution (flow rate is 8% of the total capacity of the reactor / h), sodium hydroxide solution (flow rate is 3.2% of the total capacity of the reactor / h) and sodium acetate solution (flow rate is 0.8% of the total capacity of the reactor / h) are introduced at a set flow rate, and the ammonium sulfate concentration in the reaction system is maintained at 0.025-0.01 mol / L, and the dilute sulfuric acid concentration in the reaction system is maintained at 0.01-0.05 mol / L, and the pH value of the reaction system is controlled, and the pH is gradually reduced from 11.40 in the nucleation period to 10.20 in the control period; the reaction obtains a nickel-iron-manganese-copper quaternary precursor precipitate.
[0078] ④ After the synthesis stage, the material was centrifuged, washed, dried, and demagnetized to obtain the nickel-iron-manganese-copper hydroxide precursor of Example 1, whose SEM image is shown in FIG1 , its cross-sectional SEM image is shown in FIG2 , and its cross-sectional mapping image is shown in FIG3 .
[0079] As can be seen from Figure 1, the secondary particles of the precursor prepared in Example 1 are uniform in size. This is mainly because sodium acetate is used as a chelating agent and ammonium sulfate is added as an additive. The chelating ability of the chelating agent for metals is relatively small, which reduces the difference in precipitation rate, thereby optimizing the uniformity of the morphology of the secondary particles of the precursor. The combined effect of ammonium sulfate and dilute sulfuric acid can further reduce the growth rate and make the primary particles thicker.
[0080] Combining Figures 1 and 2, it can be seen that the core of the precursor is composed of disordered arrangement of small primary particles. The thickness and length of the core primary particles are calculated through the cross-sectional SEM image. The small primary particles are conducive to the diffusion of Na element during the sintering process of the positive electrode material; the skeleton primary particles with thicker shells are staggered along the circumference of the secondary particles to form the outer skeleton structure of the secondary particles. The dotted line in the cross-sectional image is a partial schematic diagram of the skeleton primary particles. The thick skeleton primary particles improve the particle strength of the secondary particles, making it difficult for the positive electrode material to collapse during the process of Na doping, mixing and sintering, and can maintain The structure is stable; the skeleton primary particles are filled with slender primary particles, the thickness and length of the slender primary particles are calculated by cross-sectional SEM images, and the slender primary particles can increase the tap density of the precursor, increase the volume energy density of the material, and enable the battery to have a high discharge capacity and high charge and discharge efficiency; and the precursor has more overall pores and uniform element distribution, which is conducive to the infiltration of Na and other doping elements during the sintering process to reduce the sintering temperature; the copper-containing positive electrode material prepared by sintering the positive electrode material precursor material for sodium ion batteries has good air stability and is conducive to improving the cycle life.
[0081] According to Figure 3, it can be seen that the precursor elements prepared in Example 1 are well evenly distributed, which can effectively ensure the uniformity of element distribution of the positive electrode material prepared from the precursor material. Among them, the uniform distribution of the Cu element can effectively reduce the difficulty of sintering the positive electrode material and reduce the cost of material post-processing; at the same time, it is beneficial to improve the stability of the crystal structure. During the charge and discharge process of the positive electrode material, it can reduce the change of the crystal structure and reduce the dislocation of the layered oxide crystal plane, thereby improving the cycle performance.
[0082] Example 1 also prepares a positive electrode material for a sodium ion battery, which is prepared using the nickel-iron-manganese-copper hydroxide precursor obtained in Example 1. The preparation method is as follows: accurately weigh a certain weight of the precursor material and refined sodium carbonate (<100 mesh) at a mass ratio of 1:1.24, mix them evenly, and then transfer them to a mortar and spread them evenly. Finally, the mortar is transferred to a muffle furnace for sintering, and the temperature is increased at a heating curve of 1 ° C / min. After the temperature is kept at 500 ° C for 5-8h, it is heated to 950-1050 ° C at a heating curve of 1 ° C / min. After keeping warm for 10h, it is naturally cooled to obtain the positive electrode material for a sodium ion battery in Example 1.
[0083] Figure 4 is an SEM image of the positive electrode material for a sodium ion battery prepared in Example 1, and Figure 5 is a cross-sectional view of the positive electrode material for a sodium ion battery prepared in Example 1. It can be seen that the positive electrode material for a sodium ion battery includes an inner layer and an outer layer. By selecting multiple secondary particles in the cross-sectional SEM image and calculating the average values of the inner layer diameter and outer layer thickness of each secondary particle, the inner layer diameter is calculated to be 1.35 μm and the outer layer thickness is 1.83 μm. The inner layer is a fitted circle, and the area of the fitted circle is equivalent to the area of the hollow structure. The outer layer has a low porosity and is relatively dense relative to the inner layer. The outer layer includes multiple flaky primary particles, and the inner layer has a hollow structure, which is conducive to the infiltration of the electrolyte and increases the contact area between the electrolyte and the electrode material, thereby improving the electrochemical performance and available capacity of the material; the secondary particles are uniform in size, with a D50 of 5.85 μm and a span value of 0.78; the secondary particles have high strength and are not prone to producing fine powder during the mixed sintering process. The positive electrode material for a sodium ion battery can improve the capacity of the sodium ion battery.
[0084] Example 2
[0085] Example 2 First, a D50 of 6.17 μm and a chemical formula of (Ni 0.17 Fe 0.36 Mn 0.36 Cu 0.11 The specific preparation method of the nickel-iron-manganese-copper hydroxide precursor of )(OH)2 is as follows:
[0086] ① Nickel sulfate, ferrous sulfate, manganese sulfate, and copper sulfate crystals are dissolved into metal salt solutions with a nickel ion concentration of 20.3 g / L, an iron ion concentration of 41.0 g / L, a manganese ion concentration of 40.3 g / L, and a copper ion concentration of 14.3 g / L, respectively. The sodium hydroxide solution used has a concentration of 21%, the complexing agent is sodium acetate, and its concentration is 82 g / L. The additives ammonium sulfate and dilute sulfuric acid have concentrations of 0.1 mol / L and 0.05 mol / L, respectively. Ammonium sulfate is added to the sodium acetate solution, and dilute sulfuric acid is added to the metal salt solution.
[0087] ② Add pure water, sodium acetate solution and sodium hydroxide solution to the reactor and mix to obtain a reaction base liquid. Control the pH value of the reaction base liquid to 11.40, introduce nitrogen protection, heat the reactor to 60°C, and control the stirring speed at 800 r / min.
[0088] ③ After the feeding conditions are met, metal salt solution, sodium hydroxide solution and sodium acetate solution are pumped into the reaction bottom liquid, and then the metal salt solution (flow rate is 8% of the total capacity of the reactor / h), sodium hydroxide solution (flow rate is 3.2% of the total capacity of the reactor / h) and sodium acetate solution (flow rate is 0.8% of the total capacity of the reactor / h) are introduced at a set flow rate, and the ammonium sulfate concentration in the reaction system is maintained at 0.025-0.01 mol / L; the dilute sulfuric acid concentration in the reaction system is maintained at 0.01-0.05 mol / L, and the pH value of the reaction system is controlled, and the pH is gradually reduced from 11.40 in the nucleation period to 10.20 in the control period; the reaction obtains a nickel-iron-manganese-copper quaternary precursor precipitate.
[0089] ④ After the synthesis stage, the material was centrifuged, washed, dried, and demagnetized to obtain the nickel-iron-manganese-copper hydroxide precursor of Example 2. FIG6 is an SEM image of the nickel-iron-manganese-copper hydroxide prepared in Example 2, and its cross-sectional SEM image is shown in FIG7 . The primary particles of the core are arranged in a disordered manner. Changing the element ratio of nickel-iron-manganese-copper (Ni 0.17 Fe 0.36 Mn 0.36 Cu 0.11 The morphology of )(OH)2 remains stable, and it can be seen that the secondary particles of the precursor are uniform in size. In the cross-sectional view, the area of the thick flaky skeleton primary particles in the shell accounts for about 40% of the secondary particles. This shows that the stability and consistency of the precursor morphology prepared by this method can be guaranteed under different nickel content.
[0090] Example 2 also prepares a positive electrode material for a sodium ion battery, which is prepared using the nickel-iron-manganese-copper hydroxide precursor obtained in Example 2. The preparation method is carried out by referring to the preparation method of the positive electrode material for a sodium ion battery in Example 1.
[0091] Example 3
[0092] Example 3 First, a D50 of 5.99 μm and a chemical formula of (Ni 0.23 Fe 0.33 Mn 0.34 Cu 0.10 The specific preparation method of the nickel-iron-manganese-copper hydroxide precursor of )(OH)2 is as follows:
[0093] ① Nickel sulfate, ferrous sulfate, manganese sulfate, and copper sulfate crystals are dissolved into metal salt solutions with a nickel ion concentration of 27.7 g / L, an iron ion concentration of 37.9 g / L, a manganese ion concentration of 37.3 g / L, and a copper ion concentration of 13.1 g / L, respectively. The sodium hydroxide solution used has a concentration of 21%, the complexing agent is sodium acetate, and its concentration is 82 g / L. The additive ammonium sulfate has a concentration of 0.1 mol / L, wherein the ammonium sulfate is added to the sodium acetate solution.
[0094] ② Add pure water, sodium acetate solution and sodium hydroxide solution to the reactor and mix to obtain a reaction base liquid. Control the pH value of the reaction base liquid to 11.40, introduce nitrogen protection, heat the reactor to 60°C, and control the stirring speed at 800 r / min.
[0095] ③ After the feeding conditions are met, metal salt solution, sodium hydroxide solution and sodium acetate solution are pumped into the reaction bottom liquid, and then the metal salt solution (flow rate is 8% of the total capacity of the reactor / h), sodium hydroxide solution (flow rate is 3.2% of the total capacity of the reactor / h) and sodium acetate solution (flow rate is 0.8% of the total capacity of the reactor / h) are introduced at a set flow rate. The ammonium sulfate concentration in the reaction system is maintained at 0.025-0.01 mol / L, and the pH value of the reaction system is controlled, and the pH is gradually reduced from 11.40 in the nucleation period to 10.20 in the control period; the reaction obtains a nickel-iron-manganese-copper quaternary precursor precipitate.
[0096] ④ After the synthesis stage, the material is centrifuged, washed, dried, and demagnetized to obtain the nickel-iron-manganese-copper hydroxide precursor of Example 3.
[0097] Figure 8 is an SEM image of the nickel-iron-manganese-copper hydroxide precursor prepared in Example 3. It can be seen that the secondary particles of the precursor are uniform in size. This is mainly because sodium acetate is used as a chelating agent and ammonium sulfate is added. The chelating ability of the chelating agent for the metal is relatively small, which makes the precipitation rate difference smaller, thereby optimizing the uniformity of the secondary particle morphology of the precursor. Among them, ammonium sulfate can further reduce the growth rate and make the primary particles thicker.
[0098] Figure 9 is a cross-sectional view of the nickel-iron-manganese-copper hydroxide prepared in Example 3. It can be seen that the precursor prepared by this method has an inner layer composed of disordered small primary particles to form a dense structure, which is beneficial to the diffusion of Na element during the sintering process of the positive electrode material; the outer layer structure is loose and porous, and is composed of thick flake-like primary particles staggered along the circumference of the secondary particles to form the outer layer skeleton structure of the secondary particles. The thick flake skeleton primary particles in the outer shell account for about 40% of the area of the secondary particles.
[0099] Example 3 also prepares a positive electrode material for a sodium ion battery, which is prepared using the nickel-iron-manganese-copper hydroxide precursor obtained in Example 3. The preparation method is carried out by referring to the preparation method of the positive electrode material for a sodium ion battery in Example 1.
[0100] Example 4
[0101] Example 4 First, a D50 of 6.0±0.5μm and a chemical formula of (Ni 0.23 Fe 0.33 Mn 0.34 Cu 0.10 The specific preparation method of the nickel-iron-manganese-copper hydroxide precursor of )(OH)2 is as follows:
[0102] ① Nickel sulfate, ferrous sulfate, manganese sulfate, and copper sulfate crystals are dissolved into metal salt solutions with a nickel ion concentration of 27.7 g / L, an iron ion concentration of 37.9 g / L, a manganese ion concentration of 37.3 g / L, and a copper ion concentration of 13.1 g / L, respectively. The sodium hydroxide solution used has a concentration of 21%, the complexing agent is sodium acetate with a concentration of 82±2 g / L, and the additive dilute sulfuric acid has a concentration of 0.05 mol / L. The dilute sulfuric acid is added to the metal salt solution.
[0103] ② Add pure water, sodium acetate solution and sodium hydroxide solution to the reactor and mix to obtain a reaction base liquid. Control the pH value of the reaction base liquid to 11.40, introduce nitrogen protection, heat the reactor to 60°C, and control the stirring speed at 800 r / min.
[0104] ③ After the feeding conditions are met, metal salt solution, sodium hydroxide solution and sodium acetate solution are pumped into the reaction bottom liquid, and then the metal salt solution (the flow rate is 8% of the total capacity of the reactor / h), sodium hydroxide solution (the flow rate is 3.2% of the total capacity of the reactor / h) and sodium acetate solution (the flow rate is 0.8% of the total capacity of the reactor / h) are introduced at a set flow rate. The concentration of dilute sulfuric acid in the reaction system is maintained at 0.01-0.05 mol / L, and the pH value of the reaction system is controlled, and the pH is gradually reduced from 11.40 in the nucleation period to 10.20 in the control period; the reaction obtains a nickel-iron-manganese-copper quaternary precursor precipitate.
[0105] ④ After the synthesis stage, the material is centrifuged, washed, dried, and demagnetized to obtain the nickel-iron-manganese-copper hydroxide precursor of Example 4.
[0106] Figure 10 is an SEM image of the nickel-iron-manganese-copper hydroxide precursor prepared in Example 4. It can be seen that the precursor prepared by this method has uniform secondary particle size, a large number of primary skeleton particles, and a relatively thin thickness. This precursor uses sodium acetate as a complexing agent and adds dilute sulfuric acid to the metal salt solution. The complexing agent's ability to complex the metals is minimal, resulting in smaller differences in precipitation rates and optimized morphology uniformity.
[0107] Example 4 A positive electrode material for a sodium ion battery is also prepared, which is prepared using the nickel-iron-manganese-copper hydroxide precursor obtained in Example 4. The preparation method is carried out with reference to the preparation method of the positive electrode material for a sodium ion battery in Example 1.
[0108] The positive electrode material prepared from the nickel-iron-manganese-copper hydroxide precursor obtained in Example 4 has a lower compaction density than that of other examples, resulting in a slightly lower 1C capacity.
[0109] Comparative Example 1
[0110] Comparative Example 1: First, a D50 of 6.08 μm and a chemical formula of (Ni 0.33 Fe 0.33 Mn 0.34 The specific preparation method of the nickel-iron-manganese hydroxide precursor of (OH)2 is as follows:
[0111] ① Nickel sulfate, ferrous sulfate, and manganese sulfate crystals are dissolved into metal salt solutions with a nickel ion concentration of 39.8 g / L, an iron ion concentration of 37.9 g / L, and a manganese ion concentration of 37.3 g / L, respectively. The sodium hydroxide solution used has a concentration of 21%, the complexing agent is sodium acetate, and its concentration is 82 g / L. The additives ammonium sulfate and dilute sulfuric acid have concentrations of 0.1 mol / L and 0.05 mol / L, respectively. Ammonium sulfate is added to the sodium acetate solution, and dilute sulfuric acid is added to the metal salt solution.
[0112] ② Add pure water, sodium acetate solution and sodium hydroxide solution to the reactor and mix to obtain a reaction base liquid. Control the pH value of the reaction base liquid to 11.40, introduce nitrogen protection, heat the reactor to 60°C, and control the stirring speed at 800 r / min.
[0113] ③ After the feeding conditions are met, metal salt solution, sodium hydroxide solution and sodium acetate solution are pumped into the reaction bottom liquid, and then the metal salt solution (flow rate is 8% / h of the total capacity of the reactor), sodium hydroxide solution (flow rate is 3.2% / h of the total capacity of the reactor) and sodium acetate solution (flow rate is 0.8% / h of the total capacity of the reactor) are introduced at a set flow rate. The ammonium sulfate concentration in the reaction system is maintained at 0.025-0.01 mol / L; the dilute sulfuric acid concentration in the reaction system is maintained at 0.01-0.05 mol / L, and according to the control of the pH value of the reaction system, the pH is gradually reduced from 11.40 in the nucleation period to 10.20 in the control period; the reaction obtains a nickel-iron-manganese ternary precursor precipitate.
[0114] ④ After the synthesis stage, the material is centrifuged, washed, dried, and demagnetized to obtain the nickel-iron-manganese hydroxide precursor of Comparative Example 1.
[0115] FIG11 is an SEM image of the nickel-iron-manganese hydroxide precursor prepared in Comparative Example 1. Although the outer layer of the secondary particles of the precursor includes primary particles of two morphologies, the cross-section structure is quite different from that of the precursor prepared in Example.
[0116] Comparative Example 1 A positive electrode material for a sodium ion battery was also prepared using the nickel iron manganese hydroxide precursor obtained in Comparative Example 1. The preparation method was carried out with reference to the preparation method of the positive electrode material for a sodium ion battery in Example 1.
[0117] Comparative Example 2
[0118] Comparative Example 2: First, a D50 of 6.12 μm and a chemical formula of (Ni 0.23 Fe 0.33 Mn 0.34 Cu 0.10 The specific preparation method of the nickel-iron-manganese-copper hydroxide precursor of )(OH)2 is as follows:
[0119] ① Dissolve nickel sulfate, ferrous sulfate, manganese sulfate, and copper sulfate crystals into metal salt solutions with a nickel ion concentration of 27.7 g / L, an iron ion concentration of 37.9 g / L, a manganese ion concentration of 37.3 g / L, and a copper ion concentration of 13.1 g / L, respectively. The concentration of the sodium hydroxide solution used is 21%, and the complexing agent is ammonia water with a concentration of 19 g / L.
[0120] ② Add pure water and sodium hydroxide solution to the reactor and mix to obtain a reaction bottom liquid. Control the pH value of the reaction bottom liquid to 11.40, introduce nitrogen protection, heat the reactor to 60°C, and control the stirring speed at 800 r / min.
[0121] ③ After the feeding conditions are met, metal salt solution, sodium hydroxide solution and ammonia solution are pumped into the reaction bottom liquid, and then the metal salt solution (the flow rate is 8% / h of the total capacity of the reactor), sodium hydroxide solution (the flow rate is 3.2% / h of the total capacity of the reactor) and ammonia solution (the flow rate is 0.8% / h of the total capacity of the reactor) are introduced at a set flow rate, and according to the pH value of the reaction system, the pH is gradually reduced from 11.40 in the nucleation period to 10.20 in the control period; the reaction obtains a nickel-iron-manganese-copper quaternary precursor precipitate.
[0122] ④ After the synthesis stage, the material is centrifuged, washed, dried, and demagnetized to obtain the nickel-iron-manganese-copper hydroxide precursor of Comparative Example 2.
[0123] Figure 12 is an SEM image of the nickel-iron-manganese-copper hydroxide precursor prepared in Comparative Example 2. It can be seen that the secondary particle size uniformity of the precursor prepared by this method is poor, and the primary particles are uneven in thickness, with large morphological differences and disordered arrangement. This is mainly because the complexing agent used in the traditional method is ammonia water, and the large difference in the complexing ability of ammonia water for metals leads to large differences in precipitation rates, resulting in poor morphological uniformity. The precursor prepared by this method has low particle strength due to the lack of a skeleton structure, and the subsequent sintering process for preparing the positive electrode material oxide is difficult.
[0124] Figure 13 is a cross-sectional view of the nickel-iron-manganese-copper hydroxide precursor prepared in Comparative Example 2. It can be seen that the precursor shell prepared by this method is composed of disordered stacking of flaky primary particles, with a loose and porous structure, and is prone to structural collapse.
[0125] Figure 14 is a cross-sectional mapping diagram of the nickel-iron-manganese-copper hydroxide precursor prepared in Comparative Example 2. It can be seen that the element distribution uniformity of the precursor prepared by this method is poor, especially the Cu element distribution shows regional enrichment, which affects the capacitance and cyclability of the positive electrode material.
[0126] Comparative Example 2: A positive electrode material for a sodium ion battery is also prepared using the nickel-iron-manganese-copper hydroxide precursor obtained in Comparative Example 2. The preparation method is the same as that of the positive electrode material for a sodium ion battery in Example 1.
[0127] FIG15 is an SEM image of the positive electrode material for a sodium ion battery prepared in Comparative Example 2. It can be seen that the particle morphology of the positive electrode material is irregular and the sizes vary greatly.
[0128] The product parameters of the positive electrode material precursors for sodium ion batteries of Examples 1 to 4 and Comparative Examples 1 to 2 are shown in Table 1 (in order to evaluate the characteristics of the porosity, the present disclosure uses image analysis software (ImageJ) to directly calculate the pore area and cross-sectional area of each region, and the porosity of different regions is calculated by (porosity = pore area of each region / cross-sectional area of each region × 100%). The porosity of the present disclosure is characterized by this method).
[0129] Table 1 Parameters of cathode material precursor products
[0130] As shown in Table 1, compared with Comparative Examples 1-2, the precursors prepared in Examples 1-4 include a core and a shell, wherein the core is composed of a disordered arrangement of fine primary particles, and the skeleton primary particles with thicker shells are staggered along the circumference of the secondary particles to form an outer skeleton structure of the secondary particles, and the skeleton primary particles are filled with slender primary particles. Among them, the "skeleton" primary particles in the shells of Examples 1 and 2 account for more than 40% of the area of the secondary particles, and the "skeleton" primary particles in the shells of Examples 3-4 account for more than 30% of the area of the secondary particles. The slender primary particles filled between the "skeleton" primary particles can increase the tap density of the precursor, so Examples 1-4 all have a higher tap density.
[0131] The smaller Span values of Examples 1-4 indicate that the precursor secondary particles are relatively uniform in size, allowing for denser packing when used in the positive electrode, thereby improving the battery's discharge capacity. Furthermore, the precursors of Examples 1-4 have D50 and specific surface areas within appropriate ranges, and the precursor core and shell have thicknesses and porosities within appropriate ranges, enabling the cathode materials prepared from the precursors of Examples 1-4 to achieve both good capacity and cycle performance.
[0132] Sodium-ion batteries were prepared using the positive electrode materials prepared in Examples 1-4 and Comparative Examples 1-2. The positive electrode material, binder polyvinylidene fluoride (PVDF), and conductive agent (SuperP) were mixed uniformly in a mass ratio of 8:1:1. The mixture was evenly coated onto aluminum foil into a thin layer and, after drying, cut into discs as the positive electrode material. A sodium metal sheet served as the negative electrode, a Whatman glass fiber separator, and an electrolyte solution of 1.0 mol L⁻¹ NaClO⁻¹ / EC (ethylene carbonate) + DMC (dimethyl carbonate) + FEC (fluoroacetic acid ester) (EC:DMC volume ratio of 1:1, FEC accounting for 5% of the total volume) were used. CR2032 button cells were assembled in an argon glove box. The button cells were subjected to constant current charge and discharge tests with a charge and discharge voltage range of 2 to 4 V and continuous cycling of 50 cycles at a current density of 150 mA / g. The performance test results are shown in Table 2.
[0133] Table 2 Electrochemical performance
[0134] The batteries prepared from the precursors of Examples 1-4 have a high discharge capacity, all above 130mAh / g; the capacity retention rates of the batteries prepared from the precursors of Examples 1-4 are all above 82%, among which the capacity retention rates of the batteries prepared from the precursors of Examples 1-2 are all higher than those of Examples 3-4, reaching above 90%; the batteries prepared from the precursors of Example 1 not only have a high discharge capacity, but also have a high capacity retention rate. Comparative Example 1 has a high 1C discharge capacity and first efficiency due to its high nickel content, but due to the lack of copper elements and the inconsistency of its morphology and structure with the examples, its 50-week capacity retention rate is significantly lower than that of Examples 1-4; Comparative Example 2 has a relatively low 1C discharge capacity and 50-week capacity retention rate due to its inconsistency of its morphology and structure with the examples.
[0135] The sodium ion positive electrode materials prepared from the precursors obtained in different embodiments and comparative examples have a 50-week 1C capacity retention rate after exposure to air for different times, as shown in Table 3.
[0136] Table 3 50-week 1C capacity retention of different sodium ion cathode materials
[0137] When exposed to air, the sodium ion positive electrode material is highly active and easily reacts with moisture and carbon dioxide in the air, causing the transition metal oxide to easily undergo valence changes, resulting in phase changes and severe Na element precipitation, which in turn leads to poor capacity and cycle performance of the positive electrode material. In addition, poor air stability greatly increases the cost of material storage, transportation and battery manufacturing, thereby limiting the practical application of sodium ion positive electrode material oxides. It can be clearly seen from Table 3 that the sample of Comparative Example 1 does not contain copper and its internal structure is inconsistent with the embodiment. Its air stability is significantly worse than that of Examples 1-4 and Comparative Example 2, indicating that Cu-containing positive electrode materials can significantly improve the air stability of positive electrode materials. Example 1-2 has better cycle stability than Example 3-4 and Comparative Example 1, indicating that the morphology structure of Example 1-2 and the uniformity of the distribution of Cu elements are more conducive to the cycle stability of sodium ion battery materials. Compared with Example 1, the Cu content of Example 2 is 1% higher, and it can be seen that its cycle performance is significantly improved.
[0138] In summary, the primary particles in the inner core of the positive electrode material precursor for sodium ion batteries provided by the present invention are arranged in a disordered manner, which is beneficial to the diffusion of the Na element during the sintering process of the positive electrode material; the skeleton primary particles of the outer shell are staggered along the circumference of the secondary particles to form the outer skeleton structure of the secondary particles. The skeleton primary particles improve the particle strength of the secondary particles, so that the positive electrode material is not prone to structural collapse during the process of Na doping, batch mixing and sintering, and can maintain structural stability; the skeleton primary particles are filled with slender primary particles, which can increase the tap density of the precursor and the volume energy density of the material, so that the battery has a high discharge capacity and high charge and discharge efficiency; and the precursor has more overall pores and uniform element distribution, which is beneficial to the infiltration of Na and other doping elements during the sintering process, thereby reducing the sintering temperature; the copper-containing positive electrode material prepared by sintering the positive electrode material precursor for sodium ion batteries has good air stability, which is beneficial to improving the cycle life.
[0139] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them. Although the present disclosure has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present disclosure.
[0140] Furthermore, those skilled in the art will appreciate that although some embodiments herein include certain features included in other embodiments but not other features, the combination of features from different embodiments is intended to be within the scope of this disclosure and to form different embodiments. For example, in the claims above, any of the claimed embodiments may be used in any combination. The information disclosed in this background section is intended solely to enhance understanding of the overall background of this disclosure and should not be construed as an admission or any form of implication that such information constitutes prior art already known to those skilled in the art. Industrial Applicability
[0141] In summary, the primary particles in the inner core of the precursor of the positive electrode material for sodium ion batteries provided by the present invention are arranged in a disordered manner, which is beneficial to the diffusion of the Na element during the sintering process of the positive electrode material; the skeleton primary particles with thicker shells are staggered along the circumference of the secondary particles to form the outer skeleton structure of the secondary particles. The skeleton primary particles improve the particle strength of the secondary particles, so that the positive electrode material is not prone to structural collapse during the process of Na doping, batch mixing and sintering, and can maintain structural stability; the skeleton primary particles are filled with slender primary particles, which can increase the tap density of the precursor and the volume energy density of the material, so that the battery has a high discharge capacity and high charge and discharge efficiency; and the precursor has more overall pores and uniform element distribution, which is beneficial to the infiltration of Na and other doping elements during the sintering process to reduce the sintering temperature; the copper-containing positive electrode material prepared by sintering the positive electrode material precursor for sodium ion batteries has good air stability and is beneficial to improving the cycle life.
Claims
1. A positive electrode material precursor for a sodium ion battery, wherein: The secondary particles are formed by agglomerating a plurality of primary particles, wherein the secondary particles include a core and a shell covering the core; The primary particles of the inner core are arranged in a disordered manner, and the primary particles of the outer shell include skeleton primary particles arranged in a staggered manner along the circumference of the secondary particles and elongated primary particles filled between the skeleton primary particles.
2. The positive electrode material precursor for sodium ion battery according to claim 1, wherein Its chemical formula is (Ni x Cu y M 1-x-y )(OH)2, where 0 < x < 1, 0 < y < 1, and M is one or more of the elements Mn, Fe, Ti, Zn, Mg, Ca, Al, Ag, Co, Cr, La, Ce.
3. The positive electrode material precursor for sodium ion battery according to claim 1, wherein The positive electrode material precursor for sodium ion battery satisfies at least one of the following conditions (1) to (3): (1) The thickness of the skeleton primary particles in the shell is 30 to 600 nm and the length is 1.0 to 4.0 μm; (2) The thickness of the elongated primary particles in the shell is 5 to 80 nm and the length is 0.4 to 2.5 μm; (3) The thickness of the primary particles of the inner core is 10 to 50 nm, and the length is 0.2 to 1.0 μm.
4. The positive electrode material precursor for sodium ion battery according to claim 1, wherein The area ratio of the skeleton primary particles in the shell to the secondary particles is greater than or equal to 10%; Preferably, the area ratio of the skeleton primary particles to the secondary particles in the shell is greater than 40%.
5. The positive electrode material precursor for sodium ion battery according to claim 1, wherein The (D90-D10) / D50 of the positive electrode material precursor for sodium ion battery is 0.4 to 1.0; Preferably, the (D90-D10) / D50 is 0.6-0.
9.
6. The cathode material precursor for a sodium ion battery according to claim 1, wherein the cathode material precursor satisfies at least one of the following conditions (4) to (5): (4) The radius of the inner core is 1.0 to 2.0 μm; the thickness of the outer shell is 1.0 to 3.0 μm; (5) The porosity of the inner core is in the range of 5-30%, and the porosity of the outer shell is in the range of 20%-45%.
7. The positive electrode material precursor for sodium ion battery according to claim 1, wherein The positive electrode material precursor for sodium ion battery satisfies at least one of the following conditions (6) to (9): (6) The D50 of the cathode material precursor for sodium ion battery is 4 to 8 μm; (7) The TD of the positive electrode material precursor for sodium ion battery is 1.0 to 1.5 g / cm 3 ; (8) The BET of the positive electrode material precursor for sodium ion battery is 20 to 80 m 2 / g; (9) The BET of the positive electrode material precursor for sodium ion battery is 30 to 50 m 2 / g.
8. A method for preparing a positive electrode material precursor for a sodium ion battery, wherein: include: Adding water, a precipitant and a complexing agent into a reaction kettle and mixing them to obtain a reaction base liquid; Adding a metal salt solution, a precipitant, and a complexing agent to the reaction base liquid to perform a coprecipitation reaction, and controlling the pH value of the reaction system to gradually decrease; Wherein, the coprecipitation reaction further comprises adding an additive during the reaction, and the additive comprises at least one of ammonium sulfate and dilute sulfuric acid.
9. The method for preparing a cathode material precursor for a sodium ion battery according to claim 8, wherein: The method for preparing the positive electrode material precursor for a sodium ion battery satisfies at least one of the following conditions a to c: a. The complexing agent includes one or more of an aqueous ammonia solution, oxalic acid, sodium acetate, and EDTA-2Na; b. The metal salt solution comprises a metal salt solution containing Ni, Cu and at least one element selected from Fe, Mn, Ti, Zn, Mg, Ca, Al, Ag, Co, Cr, La, and Ce; c. The metal salt solution includes a metal salt solution containing Ni, Cu and at least one element selected from Fe, Mn and Mg.
10. The method for preparing a positive electrode material precursor for a sodium ion battery according to claim 8, wherein: The method for preparing the positive electrode material precursor for a sodium ion battery satisfies at least one of the following conditions d to g: d. The concentration of the additive is 0.01 to 0.5 mol / L; e. The mass concentration of each metal ion in the metal salt solution is independently 10 to 50 g / L; f. The mass concentration of the complexing agent is 60 to 100 g / L; g. The pH value of the reaction base liquid is 11-12, and the pH value of the reaction system is reduced to 10-11.
11. A sodium ion battery positive electrode material, wherein: The sodium ion battery positive electrode material comprises an inner layer and an outer layer, the outer layer is dense, the inner layer is a hollow structure, and the outer layer comprises a plurality of flaky primary particles.
12. The sodium ion battery positive electrode material according to claim 11, wherein The sodium ion battery positive electrode material meets at least one of the following conditions A to C: A. The diameter of the inner layer of the sodium ion battery positive electrode material is 0.5-2.0 μm, and the thickness of the outer layer of the sodium ion battery positive electrode material is 1.0-3.0 μm; B. The D50 of the sodium ion battery positive electrode material is 3.5 to 8 μm; C. The (D90-D10) / D50 of the sodium ion battery positive electrode material is 0.4-1.
13. A sodium ion battery, wherein: The raw material comprises the positive electrode material precursor for a sodium ion battery according to any one of claims 1 to 7 or the positive electrode material for a sodium ion battery according to any one of claims 11 to 12.
Citation Information
Patent Citations
Positive electrode active material precursor and preparation method thereof, and positive electrode active material
CN111370679A
Long-circulation and high-power lithium ion battery positive electrode material and preparation method thereof
CN112768685A
Hollow positive electrode material, precursor thereof, and preparation method of precursor
CN113247970A
High-power long-circulation nickel-cobalt-manganese ternary positive electrode material and preparation method thereof
CN114824196A
Positive electrode material precursor, preparation method thereof and positive electrode material
CN115520904A